Corrosion-resistant and wear-resistant nickel-based alloy
A Ni-based alloy with optimized Mo/B ratio and Cu addition improves corrosion resistance and wear resistance in fluoro resin molding components, addressing premature wear and cost issues in existing cermet materials.
Patent Information
- Application Number
- DE112012004408
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2011-10-19
- Filing Date
- 2012-09-26
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2032-09-26
AI Technical Summary
Existing Ni-based cermet materials used in fluoro resin molding machines suffer from premature wear due to corrosive gases, leading to high production costs and insufficient wear resistance, despite having high corrosion resistance.
A Ni-based alloy with optimized Mo/B ratio and added Cu forms a solid solution in the metallic binder phase, enhancing corrosion resistance while maintaining wear resistance by incorporating spherical hard aggregates and borides like Mo2NiB2 and Ni3B.
The alloy achieves improved corrosion resistance against fluorine-containing gases with minimal deterioration in wear resistance, maintaining comparable production costs and manufacturing efficiency.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to a corrosion-resistant and wear-resistant Ni-based alloy. TECHNICAL BACKGROUND
[0002] Demand for molded fluororesin products, such as protective layers for solar cell modules and water treatment filters, has increased year after year. Fluororesin components are molded into predetermined shapes using a molding machine, such as an extrusion molding machine or an injection molding machine.
[0003] For components intended to be placed in a molten resin environment in the resin molding machine, such as a channel, etc., of the extrusion molding machine, high wear resistance may be required. For such components, a Ni-based sintered cermet is used, as described in Japanese Patent No. JP 4121694 B2 (hereinafter referred to as Patent Document 1), whose patentee is the same as the applicant of the present patent application.
[0004] However, during the casting of the fluororesin, the fluororesin is sometimes decomposed to form a corrosive gas (fluorine-containing gas), in which even the Ni-based cermet, which inherently has high corrosion resistance and wear resistance, may be worn out prematurely.
[0005] To prevent or suppress corrosion loss, consideration is given to using Hastelloy C (trademark), a highly corrosion-resistant Ni-based alloy, or CH-501 supplied by Kubota Co. Hastelloy C is a Ni-Mo-Cr-based corrosion-resistant alloy available from Haynes International, Inc. (USA). It exhibits excellent corrosion resistance, but it has low hardness and is inferior in wear (abrasion) resistance. CH-501 is a Ni-based cermet characterized by a fine structure, but it requires HIP sintering, so high production costs are a problem.This means that when the above-mentioned known materials are used, although the loss of material due to corrosion can be reduced, there are problems that the wear resistance is insufficient and the service life is short, and that the component production costs (for example, the cost of manufacturing the channel) are increased. SUMMARY OF THE INVENTION
[0006] The object of the present invention is to provide a corrosion-resistant and wear-resistant Ni-based alloy which has sufficient corrosion and wear resistance even under circumstances where a corrosive gas such as fluorine gas is present.
[0007] The present invention is based on the alloy of Patent Document 1 (JP 4121694 B2) and improves corrosion resistance without sacrificing wear resistance, mainly by adding Cu and optimizing the Mo / B ratio. BRIEF DESCRIPTION OF THE DRAWINGS Fig. 1 is a schematic view for explaining an alloy structure of an alloy according to the present invention. Fig. 2 is a copy of an electron microscopic photograph (secondary electron beam image) showing the alloy structure of the alloy of the invention. Fig. 3 is a schematic view for illustrating a method for integrating the alloy of the present invention with a substrate material during sintering. EMBODIMENTS OF THE INVENTION
[0008] The alloy of the present invention follows the characteristics of the alloy structure of Patent Document 1 (JP 4121694 B2), which improves toughness without deteriorating wear resistance by binding aggregates of hard microparticles in a spherical or lumpy shape with a metallic binder phase of excellent toughness. In the present invention alloy, the amount of Mo forming a solid solution in the metallic binder phase is increased compared to the alloy of Patent Document 1, and further, added Cu forms a solid solution in the metallic binder phase, thereby improving the corrosion resistance of the metallic binder phase and thus the entire alloy. The improvement in corrosion resistance is achieved with less sacrifice in wear resistance than Hastelloy C.
[0009] Specifically, in the alloy of the invention, the entire alloy structure comprises a binder phase (a) in which Si, Mo and Cu form a solid solution in Ni (metallic binder phase), and spherical or lump-shaped aggregates of hard material (b) dispersed in the binder phase (a), and the metal structure of the hard material aggregate (b) contains a binder phase (c) in which Si, Mo and Cu form a solid solution and a dispersion phase (d) comprising borides such as Mo2NiB2 and Ni3B, which are dispersed in the binder phase (c) in Ni in the same manner as in the binder phase (a) (see Fig. 1 and Fig. 2). In the alloy of the present invention, the size of the hard material aggregate (b) is preferably about 30 to 300 µm, as in the alloy of Patent Document 1, which is a basis for the present invention.
[0010] The raw material powder used for producing the alloy of the present invention is produced, for example, by an atomization method (molten metal spraying method) using a molten metal formed by melting NiB, Si, Mo, Ni, and Cu, and has a composition containing, in wt%, B: 2.2 to 3.0%; Si: 3.0 to 5.0%; Mo: 18 to 25%; Cu: 1 to 15%, the balance of Ni and unavoidable impurities, wherein the weight ratio of the Mo content and the B content is from 7 to 9. An atomized powder having a particle diameter of 30 to 300 μm obtained by sieving the atomized powder through a sieve having a predetermined mesh size is used as the raw material powder.A powder having a metal structure in which hard particles comprising borides such as Mo2NiB2 and Ni3B are dispersed in a binder phase in which Si, Mo, and Cu form a solid solution in Ni can be obtained by preparing the raw material powder of the inventive alloy by the atomization method, and a sintered alloy having a binder phase in which Si, Mo, and Cu form a solid solution is obtained by sintering the powder (binder phases (a), (c)), and the sintered alloy (inventive alloy) has excellent corrosion resistance. On the other hand, it has been confirmed that when the raw material powder is prepared by a grinding method, a NiSiMo compound is formed, and the corrosion resistance of the sintered alloy is deteriorated if the NiSiMo compound is present. When sintering the raw material powder, the shaping is preferably carried out, for example, by sintering the powder.by a vacuum sintering process or an isostatic hot pressing process.
[0011] The composition of the alloy according to the invention is, in wt%, B: 2.2 to 3.0%; Si: 3.0 to 5.0%; Mo: 18 to 25%; Cu: 1 to 15%; the balance being Ni and unavoidable impurities. Furthermore, the weight ratio of the Mo content to the B content is 7 to 9. From the viewpoint of improving sinterability, the powder before sintering preferably contains 0.01 to 0.5 wt% of C, but the addition of C is not always essential. In the present specification, all percentages expressing composition or content mean "wt%" unless otherwise stated.
[0012] The reasons for defining the ingredients described above will be described individually.
[0013] Mo forms a solid solution in the binder phase (binder phases (a), (c)) to improve the corrosion resistance of the alloy. When the Mo content is less than 18%, the amount of Mo forming a solid solution in the binder phase decreases, and a sufficient effect of improving corrosion resistance cannot be achieved. Furthermore, when the Mo content exceeds 25%, the sintering temperature must be higher to obtain satisfactory sintered products, which increases production costs.
[0014] B forms a boride (Mo2NiB2) as a hard particle together with Ni and Mo to increase the wear resistance of the alloy. When the B content is less than 2.2%, the amount of Mo2NiB2 formed decreases, resulting in a deterioration in wear resistance (however, since the amount of Mo forming a solid solution in the binder phase increases, corrosion resistance is slightly improved at the same time). When the B content exceeds 3.0%, the amount of Mo forming a solid solution in the binder phase decreases, and corrosion resistance deteriorates unless the Mo content is increased by the amount of resulting Mo2NiB2. However, increasing the Mo content requires a higher sintering temperature, which increases production costs (sintering costs). Accordingly, the B content is defined as 2.2 to 3.0%.
[0015] As described above, in the alloy of the present invention, the added Cu forms a solid solution in the binder phase, in addition to the amount of Mo forming a solid solution in the binder phase, thereby increasing the corrosion resistance of the binder phase and, furthermore, of the entire alloy. As can be seen from the above-described explanation regarding the B content, the Mo contained in the alloy is partially consumed in proportion to the B content to form Mo2NiB2, and the remaining Mo exists while forming a solid solution in the binder phase. Considering this, the weight ratio of the Mo content to the B content (Mo / B weight ratio) must be 7 or more to improve the corrosion resistance to such an extent that an improvement is observed.On the other hand, as described above, the raw material powder produced by the atomization process has a metal structure in which hard particles, including borides such as Mo2NiB2 and Ni3B, are dispersed in the binder phase, where Si, Mo, and Cu form a solid solution in Ni. When a large amount of Mo forms a solid solution in the binder phase of the powder, this leads to the problem that the sintering temperature required to obtain a proper structure becomes higher.
[0016] Accordingly, the Mo / B weight ratio is defined as 9 or less.
[0017] Like Mo, Cu forms a solid solution in the binder phase to enhance the corrosion resistance of the alloy. When the Cu content is less than 2%, the amount of Cu forming a solid solution in the binder phase is small, and no effect of improving corrosion resistance is apparent. On the other hand, when the Cu content exceeds 15%, Cu-type compounds are formed, and the corrosion resistance of the alloy deteriorates. Furthermore, when the Cu content exceeds 15%, the toughness decreases, which tends to cause fine chipping, and as a result, the low wear resistance is worsened. Accordingly, the Cu content is defined as 1 to 15%. When wear resistance is important, the amount of Cu added is preferably 10% or less.
[0018] Si has the function of reducing the sintering temperature. If the Si content is less than 3.0%, a sufficient effect of reducing the sintering temperature cannot be achieved. On the other hand, if the Si content exceeds 5.0%, this is not preferable because there is a tendency to form a NiSi compound, which degrades the toughness of the alloy, and a NiSiMo compound, which degrades the corrosion resistance of the alloy. Accordingly, the Si content is defined as 3.0 to 5.0%.
[0019] C has the effect of reducing the oxide film on the powder surface and lowering the sintering temperature of the atomized powder. When the C content (amount added) is 0.01% or less, the effect of reducing the oxide film on the powder surface is small, and a sufficient effect of reducing the sintering temperature cannot be obtained. When the C content is 0.5% or more, more carbides are precipitated, and the strength and high-temperature corrosion resistance deteriorate. Accordingly, the amount of C added is defined as 0.01 to 0.5%. C is preferably added, but the extent of oxidation on the powder surface is sometimes small, depending on the manufacturing conditions of the atomized powder, etc. In such a case, the amount of C added is reduced as much as possible.Two methods can be considered as the addition method of C: one is a method that adds C when the raw material of the atomized powder is melted, followed by spraying; the other is a method that melts a raw material containing no C to prepare the atomized powder and then adds C (graphite) to the atomized powder, in the usual case. By either method, the oxides on the powder surface are sufficiently reduced by the addition of C, and the sinterability of the atomized powder can be improved. When C is added when the raw material is melted as in the first method, C can be added alone, or C can be added by adding carbides of Mo, Si, B, or the like, and in both cases, a similar effect can be achieved.
[0020] The alloy according to the invention can be suitably used for components, e.g., a channel or a screw, of a plastic molding machine that are in contact with molten plastic (especially plastics containing fluorine). Since the alloy according to the invention is relatively expensive, it is preferable to provide only the portion that is in contact with the molten resin by lining a substrate material (which usually comprises iron and steel material or cast iron), rather than forming the entire component from the alloy according to the invention. The manufacturing process will be briefly described with reference to Fig. 3 are described. Fig.3 shows a cylindrical body 1, a rod-shaped body 2, lower and upper lids 3, and a raw material powder 4 filled between the cylindrical body 1 and the rod-shaped body 2. In this state, a mold-releasing agent is applied to the surface of the cylindrical body 1 or the surface of the rod-shaped body 2 and the surface of the lid 3, and sintering is performed at a predetermined temperature to obtain a structure in which the cylindrical body 1 (or the rod-shaped body 2) and the raw material powder 4 (a sintered product made of the raw material powder 4) are integrated. The cylindrical body 1 may be, for example, a substrate material of a channel (including a steel material or cast iron). Furthermore, the rod-shaped body 2 may be, for example, a substrate material of a screw (including a steel material).For the design of a sintering mold or sintering template for forming a sintered body (sintered layer) on the surface of the substrate material, those disclosed, for example, in Japanese Patent Application Laid-Open No. JP-A No. JP-4-202705A, the patent application filed by the applicant of the present applicant (and the corresponding U.S. Patent No. US 5,336,527 and the corresponding German Patent Laid-Open No. DE 4 139 421 A), can be used. US 5,336,527 is incorporated herein by reference.
[0021] The content of expensive Mo is increased in the inventive alloy compared to the alloy of Patent Document 1. However, since Cu, which is cheaper than Ni, is added, the content of expensive Ni is reduced in proportion to the amount of Cu added. Therefore, the material cost is substantially identical to that of the alloy of Patent Document 1. Furthermore, the processing cost for sputtering the inventive alloy is identical to that of the alloy described in Patent Document 1. Furthermore, since the inventive alloy can be produced at a sintering temperature not so different from that of the alloy of Patent Document 1 (although slightly higher) and the shrinkage during sintering is no different from that of the alloy of Patent Document 1, the components can be manufactured using identical manufacturing equipment.This means that when using the alloy of the invention, the components can be manufactured at the same total cost as those for the alloy of Patent Document 1. EXAMPLES
[0022] The present invention will be described in more detail by means of specific examples.
[0023] As shown in the upper section of Table 1 below, eight types of samples, Sample Nos. 1 to 8, were manufactured. In Table 1 below, "existing material" refers to an alloy having the alloy composition of Patent Document 1 (JP 4121694 B2), and "Mo / B" refers to a value of Mo content / B content as a weight ratio. Furthermore, in each of Sample Nos. 1 to 4, 7, and 8, C (carbon) was added at 0.1%. "Sintering temperature" in the table refers to the lowest temperature at which a proper sintered structure free of voids can be obtained, which was determined experimentally. A corrosion test and a wear test were conducted on each of the samples described above. In the corrosion test, a rectangular test piece measuring 4 x 7 x 25 mm was immersed in 10% hydrofluoric acid at 50°C for 24 hours, and the corrosion loss was measured.In the wear test, the abrasion loss for a test specimen comprising an 8 mm diameter needle was measured using a needle-on-disk wear tester from Takachihoseiki Co. Ltd. under the conditions of a load of 1,000 N, a friction speed of 0.2 m / s, and a friction distance of 400 m. The results are shown in the lower section of Table 1 below.
[0024] As can be seen from the lower section of Table 1, the alloys of the invention (Sample Nos. 7, 8) exhibit significantly improved hydrofluoric acid corrosion resistance (fluorine gas corrosion resistance index) compared to the existing alloys (Sample Nos. 1, 3), and also exhibit equivalent corrosion resistance to the alloys (Sample Nos. 5, 6) previously used for the corrosion loss problem. The wear resistance of the alloys of the invention (Sample Nos. 7, 8) tends to be somewhat lower than that of the existing alloys (Sample Nos. 1, 3), but the wear resistance is significantly improved compared to the alloys previously used for the corrosion loss problem (Sample Nos. 5, 6).That is, it is apparent that in the alloy of the present invention, improvement in corrosion resistance to hydrofluoric acid can be enhanced while suppressing deterioration in wear resistance to a minimum level.
[0025] When comparing the alloys according to the invention (samples Nos. 7, 8) with each other, sample No. 7 with high Cu content is slightly more outstanding in corrosion resistance, but slightly inferior in wear resistance.
[0026] In the lower section of Table 1, "Channel Manufacturing Ratio" shows the manufacturing cost for manufacturing a duct of a resin extrusion molding machine, expressed as a ratio using the case of the alloy of Patent Document 1 (existing material) as a reference (= 1). Sample Nos. 7 and 8, as the alloy of the invention, can be manufactured at a cost equivalent to that of the existing material. The alloy of Sample No. 4, which has an identical composition to the alloy of the invention but is manufactured by a different powder manufacturing method, cannot be bonded to the iron and steel substrate material simultaneously with sintering, or bonding is very difficult due to severe shrinkage during sintering (i.e., not practical as an industrial manufacturing method).The alloy of the present invention uses a raw material powder (atomized powder) produced by the molten metal spraying method in the same way as the alloy of Patent Document 1 (existing material). Such a raw material powder causes less shrinkage during sintering and can be easily bonded to the iron and steel substrate simultaneously with sintering. Therefore, a channel coated with the corrosion-resistant and wear-resistant Ni-based alloy can be manufactured at low cost. Furthermore, the alloys of Sample Nos. 5 and 6 are difficult to bond to the iron and steel substrate material simultaneously with sintering, or they require high manufacturing costs because a special sintering method (HIP) is required.
Claims
[1] A corrosion-resistant and wear-resistant Ni-based alloy obtained by preparing, using a molten metal spraying method, a raw material powder having a composition containing, by weight, B: 2.2 to 3.0%; Si: 3.0 to 5.0%; Mo: 18 to 25%; Cu: 1 to 15%, the balance Ni and unavoidable impurities, with a weight ratio of the Mo content to the B content of 7 to 9, and then sintering the raw material powder. [2] A corrosion-resistant and wear-resistant Ni-based alloy according to claim 1, wherein the powder still contains 0.01 to 0.50% C, in wt.%, before sintering. [3] A component of a resin molding machine, in which at least a portion in contact with a resin is formed of the corrosion-resistant and wear-resistant Ni-based alloy according to claim 1 or 2.
Citation Information
Patent Citations
Sinter coating of ferrous substrate - using powder material contg. one liq. and one solid element at sintering temp.
DE4139421A1
Sintered ni-based cermet and parts for plastic molding machines and die casting machines using the same
JP4121694B2
How to remove noise from laser data
JP4202705B2
Method of covering substrate surface with sintered layer and powdery raw material used for the method
US5336527A
JP000004121694B2