Shot peening process, shot peening assessment process, and shot peening assessment setup structure

The method addresses inappropriate blasting conditions in shot peening by using a test peening and assessment process with a holding device and sealing unit to apply residual compressive stress effectively, improving mold fatigue strength and preventing stress corrosion cracking.

DE112013003216B4Active Publication Date: 2024-10-31SINTOKOGIO LTD
View PDF 23 Cites 0 Cited by

Patent Information

Application Number
DE112013003216
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2013-06-18
Publication Date
2024-10-31
Estimated Expiration
2033-06-18

AI Technical Summary

Technical Problem

Existing shot peening methods fail to effectively apply residual compressive stress to the surface of cooling water passages in molds due to inappropriate blasting conditions, which can lead to nitride layer formation and ineffective stress application.

Method used

A method involving a test peening step, assessment step, and jetting step to determine and apply appropriate blasting conditions, using a holding device and sealing unit to prevent air leakage and ensure precise shot peening of water cooling holes.

Benefits of technology

Enables the application of residual compressive stress under desired blasting conditions, preventing nitride layer removal and enhancing the fatigue strength of molds by reducing stress corrosion cracking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Shot peening process comprising: a test peening step in which a back surface (40B) of a mold (40) is shot peened in which an opening of a water cooling hole (42) with a closed end is formed; an evaluation step in which a compressive residual stress and / or a surface roughness of an area that has been shot peened in the test peening step is measured, and the extent of a shot peening treatment in the test peening step is evaluated based on measurement results, wherein the evaluation step is carried out after the test peening step;and a blasting step in which a surface of the water cooling hole (42) is shot-blasted under blasting conditions determined on the basis of blasting conditions for the test blasting step and evaluation results generated in the evaluation step, wherein the blasting step is carried out after the evaluation step; a holding device fastening step in which a holding device (46) in which a through-hole (50) is formed is fastened to the rear surface (40B) of the mold (40), wherein an open end (50A) of the through-hole (50) is turned towards the rear surface (40B) of the mold (40), wherein the through-hole (50) is determined to have the same diameter and depth as the water cooling hole (42);a test nozzle insertion step in which a shot peen nozzle (32) is inserted into the through-hole (50) after the holding device fastening step; and a nozzle insertion step in which the shot peen nozzle (32) is inserted into the water cooling hole (42) after the evaluation step, wherein the holding device fastening step and the test nozzle insertion step are preparatory steps before the test peening step is started, and the nozzle insertion step is a preparatory step before the peening step is started.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to a shot peening method, a shot peening evaluation method, and a Shot peening assessment setup structure. STATE OF THE ART

[0002] Conventionally, a shot blasting process has been used in various fields, whereby the Shot blasting is the process of hitting a surface of a workpiece with hard balls made of metal, ceramic or such as at high speeds to harden the surface of the metallic workpiece. The shot peening process involves subjecting the workpiece surface to hard balls at high speeds. a compressively stressed section on the workpiece surface to which a residual compressive stress has been imparted, and thereby hardens the workpiece surface and improves its wear resistance.

[0003] Patent Literature 1 describes a casting mold whose cooling water passage on a surface layer is was subjected to shot peening and thus provided with compressive residual stress. The shot peening process is applied to the surface layer of the cooling water passage in order to improve the operating and / or To increase fatigue strength against tensile stress generated on the surface layer of the cooling water passage, and thus prevent cracks.

[0004] WO 2005 / 068 666 A1 relates to a component with compressive residual stresses and a device for generating Compressive residual stresses. In a process for manufacturing the component, on a surface area of ​​the component locally different and non-zero residual compressive stresses are generated by a pressure generator. Residual compressive stresses are reduced by shot peening using at least two shot peening nozzles as pressure generators generated.

[0005] WO 2007 / 137 902 A1 and EP 2 032 310 B1 each relate to a blasting device for blasting a component with a part that is too radiant and a part that is not too radiant.

[0006] DE 10 2006 008 170 A1 relates to a method for treating castings, in which a casting is treated in dependence the residual stress profile is processed by means of steel blasting.

[0007] DE 26 05 988 B2 relates to a method for testing shot-peened surfaces of a workpiece to determine the degree of compaction of the surface layer achieved by shot peening.

[0008] DE 12 27 491 A relates to non-magnetic cap rings resistant to stress corrosion cracking. If the If cap rings have cooling holes, they should also have residual compressive stresses on the hole walls. Reference list Patent literature

[0009] Patent Literature 1: JP H07-290 222 A. SUMMARY OF THE INVENTION TECHNICAL PROBLEM

[0010] In order to give the surface of the cooling water passage a sufficient residual compressive stress, it is necessary to carry out the shot peening process under suitable blasting conditions. For example, molds are sometimes subjected to a nitriding process to improve their fatigue strength, if the shapes that undergo such Nitriding processes, but are shot peened excessively, a nitride layer on a mold surface could be removed, which makes it impossible to effectively impose residual compressive stress on the surface of the cooling water passage. However, the shot peening treatment method described in Patent Literature 1 does not take into account Blasting conditions to perform appropriate treatment on the surface of the cooling water hole and leaves room for improvement in terms of shot peening the surface of the water cooling hole under desired Blasting conditions.

[0011] An object of the present invention is to provide a shot peening method with which a Surface of a water cooling hole can be shot peened under desired blasting conditions, or a To create a shot peening assessment procedure or a shot peening assessment structure that can be used to define desired blasting conditions for the surface of the water cooling hole. SOLUTION TO THE PROBLEMS

[0012] A shot peening method according to one aspect of the present invention comprises: a test peening step in which a back surface of a mold is shot peened in which an opening of a water cooling hole with a closed end an assessment step in which at least one of compressive residual stress and surfaces roughness of an area shot peened in the test beam step is measured and in which a circumference or extent of the Shot peening treatment is assessed in the test blasting step on the basis of measurement results, whereby the assessment step after the test blasting step; and a blasting step in which a surface of the water cooling hole is blasting conditions based on blasting conditions for the test blasting step and Assessment results generated in the assessment step, wherein the beam step is determined according to the assessment step is carried out.

[0013] With the shot peening method according to the aspect of the present invention, the test peening step includes Shot peening of the back surface of the mold where the opening of the closed water cooling hole is formed. In the assessment step after the test blasting step, at least one of compressive residual stress and surface roughness of the area that has been shot peened in the test peening step, and the extent of the shot peening treatment In the test beam step, the assessment is based on the measurement results. In the beam step following the assessment step, the surface of the water cooling hole in the mold is shot peened under the blasting conditions determined based on the Beam conditions for the test beam step and the assessment results are specified in the This allows the area of ​​the water cooling hole to be determined under desired Shot blasting conditions.

[0014] The shot peening method according to the aspect of the present invention further comprises: a Holder fixing step, in which a holder in which a through hole is formed is fixed to the back surface of the mold, with an open end of the through hole turned towards the back surface of the mold, where the through hole is fixed, identical diameter and identical depth as the water cooling hole a test nozzle insertion step in which a shot peening nozzle is inserted after the holder fixing step is inserted into the through hole; and a nozzle insertion step in which the shot peening nozzle is inserted after Assessment step is inserted into the water cooling hole, wherein the holder fixing step and the Test nozzle insertion step preparatory steps are before the test jet step is started, and the nozzle insertion step is a preparatory step before the blasting step is started.

[0015] With the shot peening method according to the aspect of the present invention, the Holder fixing step and test nozzle insertion step as preparatory steps before starting the In the fixture attachment step, a fixture in which a Through hole is formed which has the same diameter and depth as the water cooling hole fixed to the back surface of the mold, with the open end of the through hole facing the back surface of the In the test nozzle insertion step carried out after the fixture fixing step, a Shot peening nozzle is inserted into the through hole. In addition, the nozzle insertion step is considered a preparatory step before starting the blasting step. In the nozzle insertion step carried out before the assessment step The shot peening nozzle is inserted into the water cooling hole. This allows high-speed shot reach a bottom of the water cooling hole, even if the water cooling hole has a small diameter and is deep In the test nozzle insertion step, a practical test of the nozzle insertion step is also carried out in which Test blasting step, a practical test of the blasting step is carried out, and the extent of shot peening treatment in the test beam step is assessed in the assessment step, which makes it possible to prevent excessive use of the To prevent shot peening.

[0016] In the shot peening method according to the aspect of the present invention, the test peening step and the Assessment step can be performed alternately several times before the blasting step; and in the blasting step the area of ​​the water cooling hole under the conditions determined based on the blasting conditions of the repeatedly repeated test blasting step and the measurement results generated in the assessment step repeated several times blasting conditions are shot peened.

[0017] With the shot peening method according to the aspect of the present invention, the test blasting step and the Assessment step is performed alternately several times before the blasting step. Then the area of ​​the Water cooling hole in the mold in the blasting step under the blasting conditions determined based on the Beam conditions for the test beam step repeated several times and the measurement results obtained in the test beam step repeated several times In this way, since the beam conditions for the the beam step based on the beam conditions for the test beam step repeated several times and the Measurement results produced in the assessment step repeated several times are determined, the Area of ​​the water cooling hole can be shot peened under more desirable blasting conditions.

[0018] In the shot peening method according to the aspect of the present invention, in the Holding device fastening step Compressive forces directed in the direction where the holding device and the rear surface of the mold facing each other, are exerted on a sealing unit which is located between the holding device and the back surface of the mold to surround the open end of the through hole.

[0019] In the shot peening method according to the aspect of the present invention, the sealing unit prevents Air leakage from between the holding device and the back surface of the mold during the shot peening process in the Test blasting step, since pressure forces in the direction where the holding device and the back surface of the mold meet facing, aligned, are given to the sealing unit which is placed by surrounding the open End of the through hole in the opposite area between the holding device and the rear surface of the Form. This means that the test beam step can be performed in an environment configured to This allows for a more accurate definition of the beam conditions. improve.

[0020] A shot peening evaluation method for determining suitable peening conditions for shot peening according to another aspect of the present invention comprises: a test beam step in which a back surface of a mold in which an opening of a water cooling hole with a closed end is formed, wherein the A test blasting step is carried out before a surface of the water cooling hole in the mold is shot peened; and a Assessment step in which a residual compressive stress and / or a surface roughness of an area is measured, which has been shot peened in the test peening step, and a scope of shot peening treatment in the Test beam step is assessed on the basis of measurement results, whereby the assessment step is carried out after the test beam step, but is carried out before the shot irradiation of the surface of the water cooling hole.

[0021] With the shot peening evaluation method according to the aspect of the present invention, in the Test blasting step a shot peening process is applied to the back surface of the mold in which an opening of a water cooling hole with a closed end, wherein the test beam step is carried out before the shot irradiation of the surface of the water cooling hole in the mold. In addition, the assessment step is carried out after the test blasting step but before the shot peening of the water cooling hole. In the assessment step, at least one of the Compressive residual stress and surface roughness of the area shot peened in the test blasting step were measured, and the The extent of shot peening treatment in the test peening step is assessed based on the measurement results.

[0022] The beam conditions determined in the test beam step and one determined in the evaluation step The assessment made can be used to determine the desired surface area of ​​the water cooling hole. If blasting conditions for the water cooling hole area are to be determined based on the Beam conditions for the test beam step and the assessment results generated in the assessment step and the surface of the water cooling hole in the mold is shot peened under the specified blasting conditions, The surface of the water cooling hole in the mold can then be shot peened under the desired blasting conditions.

[0023] The shot peening evaluation method according to the aspect of the present invention further comprises: a Holder fixing step, in which a holder in which a through hole is formed is fixed to the back surface of the mold, with an open end of the through hole turned towards the back surface of the mold, wherein the through hole is defined so that it has the same diameter and depth as the water cooling hole; and a test nozzle insertion step in which a shot peening nozzle is inserted after the Holding device fastening step is inserted into the through hole, wherein the holding device fastening step and the test nozzle insertion step are preparatory steps before starting the test jet step.

[0024] In the shot peening evaluation method according to the aspect of the present invention, the Holder fixing step and test nozzle insertion step before starting the test jet step as preparatory steps are carried out. In the holding device fastening step, a holding device in which a through hole is formed, which is set with identical diameter and depth as the water cooling hole, at the back surface of the mold, with the open end of the through hole turned towards the back surface of the mold. In the test nozzle insertion step carried out after the fixture fixing step, a shot peening nozzle is inserted into the through hole. If the shot peening process is carried out with the nozzle inserted into the water cooling hole is carried out, since practical tests in the test nozzle insertion step and test jet step can be carried out and the extent of shot peening treatment in the test blasting step and the assessment step is assessed against an excessive sive application of the shot peening process on the cooling water hole surface.

[0025] In the shot peening evaluation method according to the aspect of the present invention, the Test blasting step and the assessment step are carried out alternately several times, before shot peening the Area of ​​the water cooling hole.

[0026] Since the test beam step and the assessment step are alternately performed several times before the Surface of the water cooling hole is shot peened, can be assessed with the shot peening assessment method according to one aspect the present invention, more desirable beam conditions can be found.

[0027] In the shot peening method according to the aspect of the present invention, in the Holding device fastening step Compressive forces directed in the direction where the holding device and the rear surface of the mold facing each other, are exerted on a sealing unit which is located between the holding device and the back surface of the mold to surround the open end of the through hole.

[0028] Since in the holder fixing step, compressive forces directed in the direction where the Holding device and the back surface of the mold are facing each other, are transferred to the sealing unit, the by surrounding the open end of the through hole in the opposite area between the holding device and the back surface of the mold, in the shot peening evaluation method according to a Aspect of the present invention, the sealing unit against air leakage from between the holding device and the back surface of the mold during the shot peening process in the test peening step. This means that a Process environment of the test beam step can be configured to more closely approximate a process environment, in which the surface of the closed water cooling hole of the mold is shot peened, which accordingly enables to improve the accuracy of the beam conditions to be defined.

[0029] A shot peening evaluation structure for determining suitable peening conditions for the Shot peening according to one aspect of the present invention comprises: a mold having a water cooling hole with closed end, wherein the water cooling hole is formed on the back surface of the mold, which is a parting surface side opposite; and a holding device in which a through hole of identical diameter and identical depth as the water cooling hole, and which is attached to a rear surface of the mold, wherein a open end of the through hole is turned towards the back surface of the mold.

[0030] In the shot peening evaluation structure according to one aspect of the present invention, the mold has a closed cooling water hole formed on the rear side, opposite to the parting surface side, while a through hole which is designed to be identical in diameter and depth to the water cooling hole, in the holding device. In addition, the holding device is attached to a rear surface of the mold with an open end of the through hole turned toward the back surface of the mold.

[0031] Therefore, the shot peening process can be used, for example, in the case of shot peening a floor surface of the Water cooling hole with the shot peening nozzle inserted into the water cooling hole of the mold as a practical test for the back surface of the mold, with the nozzle inserted into the through hole of the holding device. Then When setting the desired jet conditions for the area of ​​the water cooling hole, it is useful to have at least one of To measure the residual compressive stress and surface roughness of the shot peened area on the back surface of the mold and to assess the extent of shot peening treatment based on the measurement results.

[0032] The shot peening evaluation structure according to one aspect of the present invention may further include a Sealing unit arranged between the holding device and the rear surface of the mold to seal the open end of the through-hole and by providing it with compressive forces directed in the direction where the holding device and the back surface of the mold face each other.

[0033] Since the sealing unit in the shot peening evaluation assembly structure according to one aspect of the present Invention is placed in the opposite area of ​​the holding device and the back surface of the mold so that it open end of the through hole and is provided with compressive forces directed in the direction where the holding device and the back surface of the mold are facing each other, the sealing unit bends when the The back surface of the mold is shot peened with the shot peening nozzle inserted into the through hole of the holding device against air leakage between the holding device and the back surface of the mold. This means that the Process environment in which the back surface of the mold is shot peened, can be configured to Procedural environment closer, in which the surface of the water cooling hole in the mold is shot peened. ADVANTAGEOUS EFFECTS OF THE INVENTION

[0034] As described above, the shot peening method according to one aspect of the present invention has the Advantage that the surface of the water cooling hole can be shot peened under desired blasting conditions.

[0035] In addition, the shot peening evaluation method according to one aspect of the present invention has the advantage of Setting desired blasting conditions for the water cooling hole area may be useful.

[0036] In addition, the shot peening evaluation structure according to one aspect of the present invention has the advantage that to be useful in determining desired blasting conditions for the area of ​​the water cooling hole. BRIEF DESCRIPTION OF THE DRAWINGS [Fig. 1] Fig. 1 is a schematic diagram showing a blasting device applied to a Shot peening method and a shot peening evaluation method according to an embodiment of the present Invention. [Fig. 2] Fig. 2 is a sectional view illustrating the shot peening process, Shot peening evaluation method, and the shot peening evaluation structure according to the embodiment of the present invention. [Fig. 3] Fig. 3 is a flow chart showing the shot peening process and shot peening evaluation process according to the embodiment of the present invention. [Fig. 4] Fig. 4 is a graph showing distributions of compressive residual stress under conditions where a shot blasting process is used optimally, used excessively and not used at all. DESCRIPTION OF EMBODIMENTS

[0037] A shot peening method, shot peening evaluation method and shot peening evaluation structure according to An embodiment of the present invention will be described with reference to Figs. 1 to 4. (Construction of a blasting device, mold and the like)

[0038] Fig. 1 is a schematic diagram showing a blasting device 10 and the like mounted on or at the Shot peening methods and shot peening evaluation methods according to the present invention are applied. Fig. 2 is a sectional view to illustrate the shot peening process, shot peening evaluation process and the Shot peening evaluation structure 38 according to the present invention. The peening device 10 as well as a irradiating form 40 are described first.

[0039] As shown in Fig. 1, the blasting device 10 has an ejection unit 12. The ejection unit 12 is used for Ejection (spinning) of weft material 14 onto an object to be processed (the mold 40 according to the present embodiment) and is equipped with a tank 16 for use in supplying the firing means 14. In the present invention embodiment, metal balls are used as the shot means 14 (also called shots or The Vickers hardness of the metal balls is approximately the same as or higher than the object(s) to be processed.

[0040] An air inlet port 16A is formed in an upper part of the tank 16 and connected to one end of a connecting line 18. Another end of the connecting line 18 is connected to a connecting section 20B which is arranged in a central part of a connecting line 20 along a flow path, while a End of the connecting line 20 on an upstream side (right side in Fig. 1) along the flow path with a compressor 22 (compressed air supply device) for use in supplying compressed air. That is, the Tank 16 is connected to the compressor 22 via the connecting lines 18 and 20. In addition, a Air flow control valve 24 (electro-pneumatic proportional valve) in a middle section of the connecting line 18 installed along the flow path, and when the air flow control valve 24 is opened, compressed air is supplied from the Compressor 22 feeds the compressed air into the tank 16. This allows the interior of the tank 16 to be pressurized.

[0041] In addition, a shot exit port 16B is formed in a lower part of the tank 16, with a provided (not shown) cut opening, and this is connected to one end of a connecting line 26. A Another end of the connecting line 26 is connected to a middle part of the connecting line 20 along the flow path on a downstream side of the connecting portion 20B and a shot flow control valve 28 is in a middle part of the connecting line 26 along the flow path. As the shot flow control valve 28 For example, a Magna valve, mixing valve, or the like can be used. A connection point of the Connecting line 20 with connecting line 26 is configured to serve as a mixing unit 20A. On the upstream side (right side in Fig. 1) of the Mixing unit 20A along the flow path, but on the downstream side (left side in Fig. 1) of the Connecting section 20B along the flow path, an air flow control valve 30 is provided in the connecting line 20 (electro-pneumatic proportional valve) installed.

[0042] That is, when the cutting opening and the shot flow control valve 28 are opened while the interior of the tank 16 is pressurized and the air flow control valve 30 is opened, it is provided that the Tank 16 supplied shot 14 and the compressed air supplied by the compressor 22 through the mixing unit 20A mixed and fed to the downstream side (left side in Fig. 1) of the connecting line 20 along the flow path.

[0043] One end of the connecting line 20 on the downstream side of the flow path is provided with an ejection (shot peening) valve 32. Accordingly, the shot 14 flowing to the mixing unit 20A is one end of a nozzle 32 by mixing it with compressed air. The nozzle 32 has a cylindrical shape and a diameter that allows insertion of the nozzle 32 into a water cooling hole 42 of the mold 40.

[0044] Incidentally, the blasting device 10 may be designed to have a robot arm (not shown), which is suitable for gripping the nozzle 32, and the rotor arm may be suitable for moving the nozzle 32 forward and to move backward (moving the nozzle 32 back and forth) with respect to the water cooling hole 42.

[0045] The blasting device 10 is equipped with an operating unit 34. The operating unit 34 is suitable for Accept inputs of process conditions for the shot peening process (some of the peening conditions include for example, a pressure of the compressed air supplied by the compressor 22 and an amount of firing means 14), and is suitable for sending a signal to a control unit 36 ​​according to an input actuation The control unit 36 ​​comprises, for example, a memory device, a processing unit and the like and is used to control the compressor 22, air flow valves 34, shot flow control valve 28 of the above described (not shown) cutting opening and the like, based on the control unit 35 output signal. That is, the control unit 36 ​​stores a program required to execute the shot peening process under blasting conditions corresponding to the signal received from the control unit 34 is issued.

[0046] On the other hand, an aesthetic surface 40A of the mold 40 on the parting surface side was formed into a mold for Use in molding. In contrast, several water cooling holes 42 with closed ends are formed with small diameter (see Fig. 2) on the side of a rear surface 40B (towards the aesthetic surface 40A opposite surface) of the mold 40, which extend in a thickness direction of the mold 40. Although a Bottom 42A of each water cooling hole 42 is shown as flat in Fig. 1 and Fig. 2, the bottom 42A of each Water cooling hole 42 may be conical or hemispherically concave inwards.

[0047] The mold 40 according to the present embodiment is a die-casting mold made of an alloy which has been subjected to a nitriding process (according to the present embodiment, for example, a Nitrocarburized SKD-61 material). Die casting is a type of metal casting and is a casting process that converts the Form 40 involves the injection of molten metal under pressure to produce large quantities of high dimensional accuracy in a short time. Such molds are exposed to high temperatures when molten metal is injected under pressure and are cooled during water cooling using the Water cooling holes 42. A distance d between the bottom 42A of the water cooling hole 42 and the aesthetic Surface 40A is set short to quickly cool the mold 40.

[0048] The nitriding process applied to the form 40 is a heat treatment that involves heating alloyed steel comprising, for example, at least one of Al, Cr, Mo, Ti and V, in an NH gas at low 3 Temperatures close to approximately 500°C to form an extremely hard nitrided layer on the surface of the The nitrided layer basically has a diffusion layer on an alloyed steel side made of base material and a bonding layer on one surface side. The diffusion layer is a layer of alloyed steel in which Nitrogen is diffused. The compound layer also has nitrides, carbides and carbonitrides or the like as main components and has the properties of being very hard and brittle. The nitrided layer can only have a diffusion layer rather than a solid layer. Here, the ´´solid layer´´ according to the present Invention a layer thick enough to be recognized as falling under normal layer conditions.

[0049] A plurality of bolt holes 44 formed with closed ends are formed at locations that are free of water cooling holes 42 in the rear surface 40B of the mold 40, which extend in a thickness direction of the mold 40. The bolt holes 44 are used to attach a holding device 46 described later. An internal thread 44A is provided on a inner surface of each bolt hole 44.

[0050] The holding device 46 is used for assessing a shot peening. Several bolt insertion holes 48 for Use for fastening the holding device 46 to the mold 40 are by penetrating or penetrating the Holding device 46 is formed. Formation locations of the plurality of bolt insertion holes 48 are determined, with the Bolt holes 44 at the fastening points of the holding device 46 on the form 40. In addition, in each Bolt insertion hole 48 is formed with a countersink 48A to provide a seat for a head 54B of a bolt shown in Fig. 2 bolt 54.

[0051] As shown in Fig. 2, the bolts 54 clamp the holding device 46 between the heads 54B and the mold 40 firmly, since external threads 54A, which penetrate the bolt insertion holes 48 in the holding device 46, are inserted into the Internal thread 44A in the form 40. This means that the holding device 46 is connected to the bolts on the form 40 attached.

[0052] A through-bore 50 is formed in the holding device 46. A penetration direction of the Through hole 50 is set parallel to the penetration direction of the bolt insertion holes 48. The through hole 50 in the holding device 46 is determined to be identical in diameter with the Water cooling holes 42 in the mold. In addition, the through hole 50 in the holding device 46 is Dimension in depth is set to be identical (length in the left-to-right direction in Fig. 2) with the Water cooling holes 42 in the mold 40.

[0053] The holding device 46 is attached to the rear surface 40B of the mold 40, with an open end 50A of the Through hole 50 is rotated to the rear surface 40B. The mold 40, holding device 46 and bolt 54 form the Shot peening assessment structure 38.

[0054] A mounting recess 46B used for mounting an annular sealing element 52A is provided on a seat surface 46A of the holding device 46, wherein the seat surface 46A is formed as an opposite area between the holding device 46 and the rear surface 46B of the mold 40. When viewed from a direction perpendicular to the Viewed from the seat surface 46A, the mounting recess 46B is formed in a ring shape which surrounds the open end 50A of the through-hole 50. The sealing element 52A, which is attached by being inserted into the mounting recess 46B serves as a sealing unit 52. The sealing unit 52 is placed so that it covers the open end 50A of the Through hole 50 and is provided with compressive forces that are aligned in the direction where the Holding device 46 and the rear surface 40B of the mold 40 face each other when the bolts 54 are tightened. From the standpoint of easy handling, the sealing element 52A forming the sealing unit 52 is desirably mounted in such a way that it is prevented from falling off by its own tension even if an open side of the mounting recess 46B is turned downward.

[0055] Therefore, the through hole 50 in the holding device 46 and a test-machined area 40B1, which facing the open end 50A of the through hole 50 on the rear surface 40B of the mold 40, in a structural section which is patterned according to the water cooling holes 42 of the mold 40.

[0056] As shown in Fig. 1, the blasting device 10 is also provided with a residual stress or Residual stress measuring device 56 (for example an X-ray diffraction residual stress measuring device) which is intended to measure compressive residual stress in a given area of ​​the mold 40. In addition, the Blasting device 10 is equipped with a surface roughness measuring device 58, which is intended to To measure surface roughness at a given area of ​​Form 40.

[0057] Although in the present embodiment, the residual stress measuring device 56 and the Surface roughness measuring device 58 is installed as part of the blasting device 10, the Residual stress measuring device 56 and the surface roughness measuring device 58 are independent of the Blasting device 10 may be installed. In addition, an equipment configuration may be used in which the Residual stress measuring device 56 and the surface roughness measuring device 58 each with the control unit 36 (see the chain double-dotted lines A and B in Fig. 1) to obtain measurement results obtained by the residual stress measuring device 56 are produced, and measurement results which are determined by the surface roughness measuring device 58 to the control unit 36. (Shot peening process and shot peening assessment process)

[0058] Next, a shot peening method and a shot peening evaluation method as well as an operation and Effects of the same are described with reference to Fig. 3. Fig. 3 is a flow chart showing the Shows shot peening process and shot peening assessment process.

[0059] In the shot peening process and shot peening assessment process, first a Holding device fastening step (step S1) is carried out. In the holding device fastening step, the Holding device 46, in which the through hole 50 shown in Fig. 2 is formed, using bolts attached to the rear surface 40B of the mold 40, wherein the open end 50A of the through hole 50 to the rear surface 40B the form 40. In the span direction fixing step, compressive forces in the direction are aligned where the holding device 46 and the rear surface 40B of the mold 40 face each other, to the Sealing unit 52 which is placed by inserting the open end 50A of the through hole 50 in the opposite area between the holding device 46 and the rear surface 40B of the surface 40. As Next, a test nozzle insertion step is carried out (step S2). In the test nozzle insertion step, the shot peening nozzle 32 is inserted into the through hole 50 in the holding device 46. The holding device fastening step and Test nozzle insertion steps are carried out as preparatory steps before a test jet step is started, which is called described next.

[0060] Next, the test blasting step is carried out (step S3). In the test blasting step, a shot peening process applied to the back surface 40B of the mold 40, in which the openings of the closed water cooling holes 42 During the shot peening process in the test peening step, the sealing unit 52 prevents Air leakage from between the holding device 46 and the rear surface 40B of the mold 40. Accordingly, a Process environment of the test beam step very closely approximates a process environment in which the surfaces of the closed water cooling holes 42 in the mold 40 are shot peened (peening step to be described later).

[0061] After the test blasting step, the holding device 46 is removed from the rear surface 40B of the mold 40, and then an assessment step is carried out (step S4). In the assessment step, the compressive residual stress and Surface roughness of the area shot peened in the test blasting step was measured (condition of the processed area is checked in a broader sense) and the extent of shot peening treatment in the test peening step is The test beam step can be assessed, for example, by a Memory unit 36 ​​pre-stored program (see Fig. 1). The beam conditions in the Test beam step and the assessment in the assessment step are used to determine desired beam conditions for to define the surfaces (inner surfaces) of the water cooling hole 42. According to the present embodiment The blasting conditions include conditions for the type of shot 14, pressure of the compressor 22 supplied compressed air (see Fig. 1) and quantity of shot 14 to be ejected.

[0062] Although in the evaluation step according to the present embodiment, the compressive residual stress and Surface roughness of the area shot peened in the test blasting step is measured and the extent of a Shot peening treatment in the test blasting step is assessed on the basis of the measurement results, can be considered as a Variation of the present embodiment of a compressive residual stress and surface roughness of the Test beam step shot irradiated area in the assessment step and the extent of Shot peening treatment in the test peening step can be assessed based on the measurement results. This means that sufficient if at least one of the compressive residual stress and surface roughness of the sample in the test blasting step shot blasted area is used as a parameter to be assessed in the assessment step.

[0063] As described above, since the sealing unit 52 is installed on the holding device 46, the Test beam step must be carried out in an environment that closely approximates that of the beam step, which Improved accuracy of beam conditions to be defined.

[0064] The fixture fixing step, test nozzle insertion step, test jet step and evaluation step, the As described above, some of the steps of the shot peening process and all the steps of the Shot peening assessment procedure.

[0065] Next, according to the present embodiment, it is determined whether the test-processed area 40B1 has a desired residual compressive stress or surface roughness (desired shot peening treatment) has been imparted or not (step S5). If it is determined in step S5 that the desired shot peening treatment is not carried out the beam conditions are changed (step S6) and the test beam step and the assessment step can be repeated until the desired shot peening treatment is achieved. The blasting conditions created by the Repeating steps S3 to S6 are desired beam conditions, which are determined on the basis of Measurement results generated in the assessment step can be determined. During implementation, either the same area or different areas on the back surface 40B of the mold 40 are shot peened in the test peening step If different areas on the back surface 40B of the mold 40 are formed in several repetitions of the test blasting step, this means that the back surface 40B of the mold 40 is shot peened under blasting conditions shot peened, which differ among the multiple repetitions of the test beam step.

[0066] If it is determined in step S5 that the desired shot peening treatment has been carried out, the Nozzle insertion step is carried out (step S7). In the nozzle insertion step, the shot peening nozzle 32 is inserted into each water cooling hole 42 (see the chain double-dotted lines). Even if the water cooling hole 42 small diameter and and is deep, the high-speed weapons can be made to penetrate the ground of the water cooling hole 42 or to pressurize it. According to the present embodiment, a Insertion depth of the nozzle 32 into each water cooling hole 42 in the nozzle insertion step is identical to that of the nozzle 32 into the Through hole 50 in the test nozzle insertion step. The nozzle insertion step is carried out as a preparatory step, before a beam step is started, which is described next.

[0067] Next, the blasting step is carried out (step S8). In the blasting step, the surface (inner surface) of the water cooling hole 42 in the mold 40 under the blasting conditions determined on the basis of the blasting conditions for the test beam step and the assessment results generated in the assessment step. This allows shot peening on the surface of the water cooling hole 42 under desired blasting conditions to carry out.

[0068] In other words, a practical test of the nozzle insertion step is carried out in the test nozzle insertion step, A practical test of the beam step is carried out in the test beam step, and the extent of Shot peening treatment in the test peening step is assessed in the assessment step, which allows, for example, to prevent excessive use of the shot peening process.

[0069] According to the present embodiment, furthermore, since the blasting conditions for the blasting step are based on the beam conditions for the test beam step, which is repeated several times, and the Assessment results generated in the assessment step, which is repeated several times, the surfaces the water cooling holes 42 under more desirable (close to ideal) blasting conditions. If the same area on the back surface 40B of the mold 40 is shot peened several times in the test peening step, the Beam conditions for the test beam step, which serve as decision-making information when setting the Beam conditions are used for the beam step, incidentally cumulative beam conditions for the Test beam step.

[0070] As described above, the shot peening method according to the present invention enables Shot blasting the surface of the water cooling holes 42 under desirable blasting conditions. Shot peening evaluation method and the shot peening evaluation structure 38 according to the present invention can also be used to achieve desired blasting conditions for the surfaces of the water cooling holes 42 to be determined.

[0071] If the surfaces of the water cooling holes 42 are subjected to shot irradiation of the surfaces of the water cooling holes 42 under desired blasting conditions, a compressive residual stress can be effectively imparted, Stress corrosion cracking (SCC) around the water cooling holes 42 of the mold 40 is accordingly prevented or effectively be reduced.

[0072] Now, an additional explanation of stress corrosion cracking is given. The aesthetic surface 40A of the Form 40 is exposed to high temperatures when molten metal is injected under pressure, and then the mold 40 is cooled during water cooling, which is carried out by causing cooling water to enter the Water cooling holes 42. Since this cycle is repeated successively, heat gaps could possibly or thermal cracks may occur, which could cause mold failure. If the distance between the water cooling holes is 42 and the aesthetic surface 40A is small, a steep thermal gradient prevails, which reduces the thermal load (tensile stress f), which is absorbed by the surfaces of the water cooling holes 42, and thereby the Probability of stress corrosion cracking increased.

[0073] In general, there are three contributing factors for stress corrosion cracking, namely a material factor, an environmental factor, and train stress f; and stress corrosion cracking occurs when the three factors overlap. The present invention transfers However, residual compressive stress can be reduced by performing the shot peening process under desired blasting conditions, whereby the influence of the tensile stress f is inhibited, which is one of the factors contributing to stress corrosion cracking, and ultimately inhibits the formation of stress corrosion cracking.

[0074] When deep aperture water cooling holes with small diameter 42 (closed end, narrow, deep holes) shot peened, the compressed air injected from the nozzle 32 into the water cooling holes 42 does not escape easily. In such a case, the speed of the shot 14 mixed with the compressed air does not increase as easily as When a shot peening process is carried out in an open space, if the speed of the compressed air mixed firing agent 14 falls short of the required speed, it is conceivable that the Shot peening at the bottom 42A (end portion) of the water cooling hole 42 does not have a sufficient effect Since the surface of each water cooling hole 42 is ejected together with the compressed air by the shot 14 is shot peened by the nozzle 32, which is inserted into the water cooling hole 43, can be Embodiment, however, even if the aperture water cooling holes 42 are small in diameter and deep, the high-speed shot means 14 is caused to reach the bottom 42A of the water cooling hole 42. Therefore, a compressive residual stress can be effectively transferred to the bottom 42A of the water cooling hole 42.

[0075] Depending on whether a nitrided layer is present on the surfaces of the water cooling hole 42 or not, on the other hand, it is conceivable that a residual compressive stress cannot be effectively imparted, and therefore it is important to carry out the shot peening process under the desired blasting conditions. To clarify this point, it Hot-work tool steel SKT-61 is often used as a material for the die-casting mold 40 and it is considered a Heat treatment often involves applying a nitriding process to the Form 40. In addition, one of the factors to be considered is Points during shot peening of the form 40 which has been subjected to the nitriding processes, the removal (removal or Grinding) of the nitrided layers (a compound layer and diffusion layer). If the shot peening process is carried out under a strong blasting condition, the nitrided layer is also scraped off, but the nitrided layer and a layer directly below it (base material or substrate) have different mechanical properties and differ significantly in terms of the residual or internal stress imparted, as a result of the shot peening process.

[0076] Fig. 4 shows results of measuring distributions of compressive residual stress under conditions where a Shot blasting is optimally applied, excessively applied and not applied. The abscissa represents the Distance from the surface of the water cooling hole 42 (depth from the surface in a direction perpendicular to the Base material of the form 40). As can be seen from Fig. 4, if an area has a nitrided surface before the shot peening process, layer and the nitrided layer has been removed from the area as a result of excessive application of the shot peening process has been removed, the target area cannot be effectively given a compressive residual stress. Under a condition which assumes that the shot peening process is applied to the base material as a result of scraping or Scraping off the nitrided layer during shot peening is the residual or internal stress that is imparted less than the residual stress imparted during nitriding. This means that the state of the Compressive residual stress on the surface of the water cooling hole 42 is consequently worse than before the application of the Shot blasting process.

[0077] At this point, it should be noted that the surfaces of the water cooling holes 42 are effectively subjected to compressive residual stress is given, since the surfaces of the water cooling holes 42 in the form 20 shown in Fig. 2 in the present Embodiment shall be shot peened under the blasting conditions determined on the basis of the blasting conditions for the test beam step and the assessment results generated in the assessment step.

[0078] To make a supplementary statement from another point of view: general conditions of a Heat treatment (nitriding process) applied to workpieces (molds) according to the present embodiment vary from workpiece to workpiece, and this also applies to the extent of the applied Nitriding. This makes it necessary to specify blasting conditions (shot peening conditions) for each shape to be processed. to determine, within the limits or framework conditions, not to remove the nitrided layer. In principle, a prolonged duration of the shot peening process may lead to the removal of the nitrided layer, and therefore the The processing time can be set correctly. In addition, the effects of sphere irradiation can be influenced by differences regarding the material and a heat treatment (nitriding process) or the like of the workpiece (shape, according to of the present embodiment). Therefore, it is important to have desirable beam conditions for each form to be processed 40.

[0079] However, according to the present embodiment, since the test beam step and judgment step are performed for each to be processed form 40 and the extent of shot peening is assessed before the Shot peening is carried out, the surfaces of the water cooling holes 42 under more reliable blasting conditions be shot irradiated (treated). (Supplementary explanation of an embodiment)

[0080] With the shot peening method and shot peening evaluation method according to the above embodiment the test beam step and assessment step are carried out alternately several times before the beam step, and This is desirable, but the shot peening process and the shot peening assessment process can be configured to perform the test beam step and the assessment step once.

[0081] Although the fixture fixing step and test nozzle insertion step in the shot peening method and Shot peening assessment methods according to the above embodiment can also be carried out, For example, when the surfaces of shallow or shallow water cooling holes with a large diameter be shot peened and the blasting step is carried out without inserting the nozzle into the water cooling holes, the fixture attachment step and test nozzle insertion step are omitted.

[0082] In the holding device fastening step according to the above embodiment, compressive forces, which is aligned in the direction where the holding device 46 and the rear surface 40B of the mold 40 face each other are transferred to the sealing unit 52, which is placed by the open end 50A of the through hole 50 in the opposite area between the holding device 46 and the rear surface 40B of the mold 40, and this configuration is desirable, but if a seal between the holding device 46 and the Rear surface 40B of the mold 40 is secured even if such a sealing unit 52 is not provided, a Configuration without a sealing unit.

[0083] In addition, although the holding device 46 in the above embodiment is fixed to the mold 40 with bolts is attached, the holding device may be attached to the mold using a different fastening structure: For example, the holding device and form can be mounted in a screw clamp or clamping jaw or vice be clamped.

[0084] Furthermore, the concept of ´´having identical diameter and depth´´ defined in the appended claims described, not only cases where diameter and depth are identical in the narrow sense, as in the above embodiment, but also cases where it is recognized that diameter and depth are essentially identical are, even if the diameter and depth are not identical in the strict sense, and which are essentially the same Actuation and effects as when diameter and depth are identical in the narrow sense. If the floor of the water cooling hole is, for example, curved inwards or hemispherically concave, if the depth the through hole of the holding device is identical to the depth of the water cooling hole, with the exception of the inward curved or concave section, the water cooling hole and the through hole sometimes as essentially be considered identical in terms of depth.

[0085] It should be noted that the embodiment and a variety of variations described above can be implemented in combination as required. List of reference symbols

[0086] 10: Blasting device; 12: Ejection unit; 14: Shot; 16: Tank; 18: Connecting line; 20: Connecting line; 20A: Mixing unit; 20B: Connecting section; 22: Compressor; 24: Air flow control valve; 26: Connecting line; 28: Shot flow control valve; 30: Air flow control valve; 32: Nozzle; 34: Actuator; 36: Control unit; 38: Shot peening assessment assembly structure; 40: Mold; 40A: Aesthetic surface (parting surface); 40B: Back surface (back surface of the mold); 40B1: Test-machined area; 42: Water cooling hole; 42A: Bottom; 44: Bolt hole; 46: Holding device; 48: Bolt insertion hole; 50: Through hole; 50A: Open end; 52: Sealing unit; 54: Bolt; 56: Residual stress measuring unit; 58: Surface roughness measuring device.

Claims

1. Shot blasting process, which includes: a test blasting step in which a back surface (40B) of a mold (40) in which an opening of a Water cooling hole (42) is formed with a closed end; an assessment step in which a residual compressive stress and / or a surface roughness of an area is measured which has been shot peened in the test peening step, and an amount of shot peening treatment in the test peen step is assessed on the basis of measurement results, whereby the assessment step is carried out after the test beam step will; and a blasting step in which a surface of the water cooling hole (42) is shot peened under blasting conditions that are Based on beam conditions for the test beam step and on assessment results obtained in the assessment step generated, wherein the beam step is carried out after the assessment step; a holding device fastening step in which a holding device (46) in which a through hole (50) is formed, is attached to the rear surface (40B) of the mold (40), wherein an open end (50A) of the through hole (50) is rotated to the rear surface (40B) of the mold (40), wherein the through hole (50) is fixed, identical diameter and depth identical to the water cooling hole (42); a test nozzle insertion step in which a shot peening nozzle (32) is inserted into the through hole (50), after which Holding device fastening step; and a nozzle insertion step in which the shot peening nozzle (32) is inserted into the water cooling hole (42), after which Assessment step, where the fixture attachment step and the test nozzle insertion step are preparatory steps before the Test jet step is started, and the nozzle insertion step is a preparatory step before the jet step is started becomes.

2. Shot blasting process according to claim 1, wherein: the test beam step and the assessment step are carried out alternately several times before the beam step; and the surface of the water cooling hole (42) is shot peened in the blasting step under the blasting conditions which are Based on the blasting conditions for the test blasting step repeated several times and the evaluation results, which are which are generated by the assessment step repeated several times.

3. A shot peening method according to claim 1 or 2, wherein in the holder fixing step, compressive forces which are aligned where the holding device (46) and the rear surface (40B) of the mold (40) face each other, on a sealing unit (52) arranged between the holding device (46) and the rear surface (40B) of the mold (40) is arranged to surround the open end (50A) of the through hole (50).

4. Shot peening evaluation method for determining suitable blasting conditions for shot peening, wherein the Shot peening assessment procedure includes: a test blasting step in which a back surface (40B) of a mold (40) in which an opening of a water cooling hole (42) with a closed end, wherein the test blasting step is carried out before shot peening a surface of the water cooling hole (42) in the mold (40); and an assessment step in which a residual compressive stress and / or a surface roughness of a material in the Test blasting step shot peened area is measured and a scope of shot peening treatment in the Test beam step is assessed on the basis of measurement results, whereby the assessment step is carried out after the test beam step, but is carried out before shot peening the surface of the water cooling hole (42); a holding device fastening step in which a holding device (46) in which a through hole (50) is formed, is attached to the rear surface (40B) of the mold (40), wherein an open end (50A) of the through hole (50) is rotated to the rear surface (40B) of the mold (40), wherein the through hole (50) is fixed, identical diameter and depth identical to the water cooling hole (42); and a test nozzle insertion step in which a shot peening nozzle (32) is inserted into the through hole (50), after which Holding device fastening step; wherein The fixture fixing step and test nozzle insertion step are preparatory steps before the Test beam step is started.

5. A shot peening evaluation method according to claim 4, wherein the test peening step and the evaluation step alternately several times before the surface of the water cooling hole (42) is shot peened.

6. A shot peening evaluation method according to claim 4 or 5, wherein in the holder fixing step Pressure forces directed to where the holding device (46) and the back surface (40B) of the mold (40) meet facing, are exerted on a sealing unit (52) which is arranged between the holding device (46) and the Rear surface (40B) of the mold (40) is arranged to surround the open end (50A) of the through hole (50).

7. Shot peening evaluation structure for determining suitable blasting conditions for shot peening, wherein the shot peening assessment structure has: a mold (40) having a closed-end water cooling hole (42), the water cooling hole being formed on the back surface of the shape which is opposite to a parting surface side; and a holding device (46) in which a through hole (50) is formed, which is fixed, iden diameter and identical depth as the water cooling hole (42), and which is arranged on a rear surface (40B) of the mold (40), wherein an open end (50A) of the through hole (50) is directed to the rear surface (40B) of the mold (40) is rotated.

8. A shot peening evaluation assembly structure according to claim 7, further comprising a sealing unit (52) arranged between the holding device (46) and the rear surface (40B) of the mold (40) is arranged to form the open end (50A) of the through-hole (50) and by providing it with compressive forces directed to where the Holding device (46) and the rear surface (40B) of the mold (40) face each other.

Citation Information

Patent Citations

  • Steel shot blasting process to modify the tensile characteristics of a cast metal crankcase produced by e.g. lamellar cast or vermicular cast iron

    DE102006008170A1

  • Method for work-hardening surfaces of vehicle engine and transmission components comprises ultrasonic shot peening using component as part of sonotrode, its vibrating surfaces being hardened by contact with shot

    DE102006048712A1

  • Process to increase the strength of a component

    DE102007028888A1

  • Method and device for shot peening of blisk blades

    DE102008010847A1

  • non-magnetic cap rings resistant to stress corrosion cracking

    DE1227491A