Method for producing a fine catalyst particle and fuel cell comprising a fine catalyst particle produced by the manufacturing process

The production of fine catalyst particles with a palladium core and platinum shell, using Cu-UPD and platinum substitution, addresses the low initial activity and durability issues of conventional core-shell catalysts, achieving high and stable catalytic performance without preconditioning.

DE112013007069B4Active Publication Date: 2024-11-21TOYOTA JIDOSHA KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
DE112013007069
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2013-05-13
Publication Date
2024-11-21
Estimated Expiration
2033-05-13

AI Technical Summary

Technical Problem

Conventional core-shell catalysts for fuel cells exhibit low initial catalytic activity and require a long preconditioning interim operation to achieve high activity, due to incomplete core coverage with platinum and environmental differences between liquid cells and fuel cells.

Method used

A method for producing fine catalyst particles by forming a palladium-containing particle with a platinum layer, followed by copper underpotential deposition (Cu-UPD) and subsequent substitution with platinum, ensuring complete core-shell structure and high initial activity without the need for preconditioning.

Benefits of technology

The method results in catalyst particles with high initial activity and durability, maintaining mass activity and specific activity levels even after potential cycles, reducing the need for interim operations and minimizing copper discharge.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Method for producing a fine catalyst particle comprising a palladium-containing particle and an outermost platinum layer covering the palladium-containing particle, wherein a first composite body containing palladium and platinum is formed by mixing the palladium-containing particle with a first solution in which a platinum compound is dissolved, and as a result of directly contacting the palladium-containing particle with the first solution, then covering at least a part of a surface of the palladium-containing particle with platinum; wherein a second composite body containing palladium, platinum and copper is formed by mixing the first composite body with a second solution in which a copper compound is dissolved, and then covering at least part of a surface of the first composite body with copper using copper sub-potential deposition; wherein the copper in the second composite body is substituted by platinum obtained from a third solution in which a platinum compound is dissolved, by mixing the second composite body with the third solution; and wherein the amount of platinum atoms contained in the first solution is 70 at.% or less, where the minimum amount of platinum atoms required to cover the palladium-containing particle with a monatomic platinum layer is 100 at.%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field

[0001] The present invention relates to a method for producing a fine catalyst particle designed to exhibit high activity from the beginning of its manufacture, and to a fuel cell comprising a fine catalyst particle produced by the manufacturing method. Current state of the art

[0002] Fuel cells convert chemical energy directly into electrical energy by supplying a fuel and an oxidant to two electrically connected electrodes and electrochemically oxidizing the fuel. Unlike thermal energy generation, fuel cells are not limited by the Carnot cycle; therefore, they exhibit high energy conversion efficiency. Fuel cells generally consist of a stack of individual cells, each with a membrane electrode array as its basic structure, in which an electrolyte membrane is positioned between a pair of electrodes.

[0003] Supported platinum and platinum alloy materials are used as the catalyst for the anode and cathode electrodes of a fuel cell. However, platinum remains too expensive to be used in the quantities required by current electrode catalysts for the commercial mass production of fuel cells. Accordingly, investigations have been conducted to reduce the amount of platinum contained in the cathode and anode of a fuel cell by combining platinum with a less expensive metal.

[0004] In recent years, fine core-shell catalyst particles have gained attention as a catalyst for fuel cell electrodes (hereinafter also referred to as core-shell catalysts). From the perspective of increasing the coverage of a core with a shell, a generally known method for producing core-shell catalysts involves first forming a monatomic layer on a core surface using a sub-potential deposition process, such as copper sub-potential deposition (hereinafter also referred to as Cu-UPD), and then replacing this monatomic layer with a shell.

[0005] As a technique utilizing Cu-UPD, patent literature 1 discloses a method for forming a catalyst material in which a catalyst material containing a platinum atom layer is produced by substituting a copper atom layer with a platinum atom layer in the presence of a surfactant. Patent literature 2, patent literature 3, patent literature 4, and scientific literature 1 disclose further technologies relating to a catalyst material and / or fuel cells. List of objections Patent literature 1: International publication WO 2012 / 115624 A1 Patent literature 2: DE 11 2010 005 260 T5 Patent literature 4: US 2010 / 0 197 490 A1 Patent literature 5: DE 11 2010 005 593 T5

[0006] Scientific literature 1: Zhang J, Lima FH, Shao MH, Sasaki K, Wang JX, Hanson J, Adzic RR. Platinum monolayer on nonnoble metal-noble metal coreshell nanoparticle electrocatalysts for O2 reduction. J Phys Chem B. 2005 Dec 8;109(48):22701-4. doi: 10.1021 / jp055634c. PMID: 16853957. Summary of the invention: Technical problem

[0007] However, as a result of research, the inventors of the present invention discovered that the method disclosed in patent literature 1, i.e., the method of covering a core with a copper atom layer using Cu-UPD and subsequently substituting the copper atom layer with a platinum atom layer, does not sufficiently cover or coat the core with a platinum atom layer. Consequently, the core-shell catalyst obtained in this way does not exhibit high activity from the start of its production, and a problem arises such that achieving high activity requires a long preconditioning interim operation, i.e., prior operation to increase the activity of the core-shell catalyst by changing the state of the core-shell catalyst surface through the application of a potential cycle, etc., is necessary.

[0008] The present invention was made in view of the foregoing circumstances. One object of the present invention is to provide a method for producing a fine catalyst particle designed to exhibit high activity from the start of its production, and a fuel cell comprising a fine catalyst particle produced by the manufacturing process. Solution to the problem

[0009] The aforementioned problem is solved by the subject matter of independent claims 1 and 5. Advantageous embodiments of the present invention are the subject matter of dependent claims 2 to 4.

[0010] The first method for producing a fine catalyst particle of the present invention is a method for producing a fine catalyst particle comprising a palladium-containing particle and an outermost platinum layer covering the palladium-containing particle, wherein a first composite body containing palladium and platinum is formed by mixing the palladium-containing particle with a first solution in which a platinum compound is dissolved, and as a result of directly contacting the palladium-containing particle with the first solution, then covering at least a part of a surface of the palladium-containing particle with platinum;wherein a second composite body containing palladium, platinum, and copper is formed by mixing the first composite body with a second solution in which a copper compound is dissolved, and then covering at least a portion of a surface of the first composite body with copper using copper sub-potential deposition; wherein the copper in the second composite body is substituted by platinum derived from a third solution in which a platinum compound is dissolved, by mixing the second composite body with the third solution; and wherein an amount of platinum atoms contained in the first solution is 70 at.% or less, where a minimum amount of platinum atoms required to cover the palladium-containing particle with a monatomic platinum layer is 100 at.%.

[0011] A second, non-inventive method for producing a fine catalyst particle is a method for producing a fine catalyst particle comprising a palladium-containing particle and an outermost platinum layer covering the palladium-containing particle, wherein a composite body A containing palladium and copper is formed by mixing the palladium-containing particle with a second solution in which a copper compound is dissolved, and then covering at least a part of a surface of the palladium-containing particle with copper using copper sub-potential deposition; wherein a composite body B containing palladium and platinum is formed by mixing the composite body A with a third solution in which a platinum compound is dissolved, and then substituting the copper in the composite body A with the platinum originating from the third solution;and wherein at least a part of a surface of the composite body B is covered with platinum by mixing the composite body B with a first solution in which a platinum compound is dissolved.

[0012] In the present invention, the palladium-containing particle is preferably carried on a carrier.

[0013] In the present invention, the palladium-containing particle is preferably subjected to an acid treatment beforehand, before the first composite body (or, according to a non-inventive method, the composite body A) is formed.

[0014] In the present invention, the amount of platinum atoms contained in the first solution is 70 at.% or less, if a minimum amount of platinum atoms required to cover the palladium-containing particle with a monatomic platinum layer is 100 at.%.

[0015] The fuel cell of the present invention is a fuel cell with unit cells, each comprising a membrane electrode arrangement in which an anode electrode with at least one anode catalyst layer is arranged on one side of a polyelectrolyte membrane and a cathode electrode with at least one cathode catalyst layer is arranged on another side of the polyelectrolyte membrane, wherein a fine catalyst particle produced by the first or second manufacturing process is contained in the anode catalyst layer and / or the cathode catalyst layer. Advantageous effects of the invention

[0016] According to the present invention, a fine catalyst particle with a very high coverage can be produced by mixing the palladium-containing particle with the first solution, covering at least a portion of the surface of the palladium-containing particle with platinum, and then covering the remaining surface of the palladium-containing particle with platinum using Cu-UPD. Furthermore, according to the present invention, the fine catalyst particle obtained in this way exhibits high activity from the start of its production, so that a preconditioning intermediate operation is not required and, consequently, the fine catalyst particle can be used for a catalytic reaction immediately after its production. Brief description of the drawings Fig. Figure 1 is a schematic sectional view of a typical example of the first composite body of the present invention. Fig. Figure 2 is a schematic view showing a transition of a section into a covered state in the process for producing a fine catalyst particle of the present invention. Fig. Figure 3 is a view showing an example of the unit cell of the fuel cell of the present invention, and is also a view schematically showing a section through the unit cell along a layer arrangement direction. Fig. Figure 4 is a graph showing a transition which is determined by observing the formation of the first composite body in Example 1. Fig. Figure 5 is a graph showing a transition that is determined by observing the substitution of the copper atom layer by the outermost platinum layer in Example 1. Fig. Figure 6 is a graph showing a transition which is determined by observing the coverage with platinum in reference example 1. Fig. Figure 7 is a graph showing the proportion of platinum on the surface of the palladium particle (core) in relation to the average particle diameter of the palladium particles. Fig. Figure 8 is a schematic view showing a transition of a section into a covered state, as would be expected from a conventional method for producing a core-shell catalyst using Cu-UPD. Fig. Figure 9 is a graph showing a transition which is determined by observing the substitution of the copper atom layer by the outermost platinum layer in comparative example 1. Fig. Figure 10 is a graph showing a transition which is determined by observing the substitution of the copper atom layer by the outermost platinum layer in comparative example 2. Fig. Figure 11 is a schematic cross-sectional view of the composite body in which the surface of the palladium particle is completely covered with copper atoms. Description of embodiments 1. First method for producing a fine catalyst particle

[0017] The first method for producing a fine catalyst particle of the present invention is a method for producing a fine catalyst particle comprising a palladium-containing particle and an outermost platinum layer covering the palladium-containing particle, wherein a first composite body containing palladium and platinum is formed by mixing the palladium-containing particle with a first solution in which a platinum compound is dissolved, and as a result of directly contacting the palladium-containing particle with the first solution, then covering at least a part of a surface of the palladium-containing particle with platinum;wherein a second composite body containing palladium, platinum, and copper is formed by mixing the first composite body with a second solution in which a copper compound is dissolved, and then covering at least a portion of a surface of the first composite body with copper using copper sub-potential deposition; wherein the copper in the second composite body is substituted by platinum derived from a third solution in which a platinum compound is dissolved, by mixing the second composite body with the third solution; and wherein an amount of platinum atoms contained in the first solution is 70 at.% or less, where a minimum amount of platinum atoms required to cover the palladium-containing particle with a monatomic platinum layer is 100 at.%.

[0018] Patent literature 1 discloses a conventional synthesis method using Cu-UPD as a method for the synthesis of a core-shell catalyst, which aims to regulate a monatomic platinum layer, which will be a shell.

[0019] However, as a result of research, the inventors of the present invention identified the following problem: In particular, a conventional core-shell catalyst produced on a milligram or gram scale, in which the core contains palladium and the shell contains platinum, exhibits low mass activity immediately after preparation, and the mass activity is at most slightly more than twice that of a platinum-supported carbon. Accordingly, the conventional core-shell catalyst has a problem such that, without potential treatment, such as a rotating disk electrode (RDE) method, it cannot achieve the mass activity obtained by synthesis on a microgram scale (corresponding to a mass activity three times or more that of the platinum-supported carbon).

[0020] Furthermore, the inventors of the present invention identified the following problem: Although the catalytic activity immediately after manufacture (initial activity) is important from the perspective of its application to fuel cells, the conventional core-shell catalyst inherently possesses low catalytic activity and, moreover, requires preconditioning interim operation for a very long period to maintain the catalytic activity at or above a certain level. This is because, due to a difference in the operating environment between the interior of a fuel cell and that of a liquid cell, potential treatment inside the fuel cell is less effective than potential treatment inside the liquid cell using RDE.The operating environment inside the fuel cell differs from the operating environment inside the liquid cell, for example, in the following ways: The core-shell catalyst is covered with an ionomer; the catalyst layer is very thin; and the convection effect of mass transport is generated by rotation.

[0021] The inventors of the present invention predicted the following: Conventional core-shell catalysts produced using Cu-UPD on a milligram scale or larger exhibit an incomplete core-shell structure immediately after production, in which the shell is not uniform; therefore, when potential treatment is performed on the conventional core-shell catalyst, the shell coverage is altered, and consequently, the core-shell structure is eventually completed. The inventors of the present invention have pursued research and development with the aim of producing a fine catalyst particle that possesses a complete core-shell structure immediately after production.

[0022] However, a known method for producing a core-shell catalyst involves the direct deposition of platinum onto a gold particle by contacting a gold particle (core) with a platinum complex solution. This method can directly coat a gold particle with platinum, not via Cu-UPD.

[0023] However, in the case of a gold core, the resulting catalyst is more expensive than a conventional platinum-supported carbon catalyst and offers no cost advantage. A well-known document (M. Inaba et al., ECS Transaction, 33(1) 231-238 (2010)) describes on page 237 how, in a core-shell catalyst using a gold core, a platinum shell dissolves to form an alloy with the gold core, and that such dissolution of the platinum shell leads to a reduction in activity when a potential cycle is applied. This is attributed to gold's high mechanical flexibility, such as malleability and ductility.

[0024] Since gold also has very low oxygen reduction activity, a possible disadvantage is that a loss of the platinum shell leads to a significant reduction in activity.

[0025] It was conventionally assumed that when a palladium-containing particle is brought into direct contact with a solution containing a platinum compound, the palladium on the surface of the palladium-containing particle is substituted by the platinum due to an ionization tendency. However, the inventors of the present invention were the first to discover, as shown in the examples described below, that in this case the palladium is not substituted by the platinum and the platinum is deposited on the surface of the palladium-containing particle in a system using chloroplatinate.The inventors of the present invention have also found that the core-shell catalyst obtained by direct contact of the palladium-containing particle with the solution containing the platinum compound exhibits higher activity and better stability than the conventional core-shell catalyst produced using Cu-UPD.

[0026] Furthermore, the inventors of the present invention have found that a core-shell catalyst, which exhibits high catalytic activity and excellent stability immediately after synthesis, can be obtained by directly contacting the palladium-containing particle with the solution containing the platinum compound, so that a platinum layer is formed, and then further deposition of platinum using Cu-UPD on a part where the platinum layer has not yet formed. Based on these findings, the present invention was further developed.

[0027] The present invention comprises the steps of: (1) forming the first composite body, (2) forming the second composite body, and (3) substituting copper in the second composite body with platinum. The present invention is not limited to these three steps. In addition to these three steps, the present invention may, for example, include an acid treatment step, a filtration step, a rinsing step, and a drying step, as described below.

[0028] The following describes steps (1) to (3) and further steps in sequence. 1-1. Step of forming the first composite body

[0029] This is a step in forming the first composite body containing palladium and platinum by mixing the palladium-containing particle with the first solution in which the platinum compound is dissolved, and as a result of immediately bringing the palladium-containing particle into contact with the first solution, then covering at least part of the palladium-containing particle surface with the platinum.

[0030] In the present invention, the term “palladium-containing particle” is used as a generic term for palladium particles and palladium alloy particles.

[0031] As described below, the outermost layer covering the palladium-containing particle contains platinum. Platinum possesses excellent catalytic activity, particularly excellent oxygen reduction reaction (ORR) activity. While the lattice constant of platinum is 3.92 Å, the lattice constant of palladium is 3.89 Å, a value that lies within 5% of either side of the lattice constant of platinum. Accordingly, no lattice mismatch occurs between platinum and palladium, and the palladium is sufficiently covered by platinum.

[0032] In the present invention, from the point of view of cost reduction, it is preferred that the palladium-containing particle contains a metal material that is less expensive than platinum, which is used for the outermost layer. It is also preferred that the palladium-containing particle contains a metal material that contributes to electrical continuity.

[0033] From the aforementioned perspectives, in the present invention the palladium-containing particle is preferably a palladium particle or a particle made of an alloy of palladium with a metal such as iridium, rhodium, or gold. In the case of using a palladium alloy particle, the palladium alloy particle may contain only one type of metal or two or more types of metals in combination with palladium.

[0034] The mean particle diameter of the palladium-containing particles is not subject to any particular restrictions, provided it is less than or equal to the mean particle diameter of the fine catalyst particles described below. Considering that the surface area to cost ratio per palladium-containing particle is high, the mean particle diameter of the palladium-containing particles is preferably 30 nm or less, more preferably 3 to 10 nm.

[0035] In the present invention, the mean particle diameter of the palladium-containing particles and the fine catalyst particles is calculated using a conventional method. An example of the method for calculating the mean particle diameter of the palladium-containing particles and the fine catalyst particles is as follows. First, the particle diameter of a particle shown in a TEM image at a magnification of 400,000x to 1,000,000x is calculated, assuming that the particle is spherical. Such a calculation of the particle diameter based on TEM observation is performed on 200 to 300 particles of the same type, and the mean of these particles is considered the mean particle diameter.

[0036] The palladium-containing particle can be mounted on a support. Particularly from the perspective of imparting electrical conductivity to the electrocatalyst layer of a fuel cell when the fine catalyst particle produced by the present invention is used for the electrocatalyst layer, the support is preferably an electrically conductive material.

[0037] Specific examples of electrically conductive materials that can be used as the substrate include, for example, electrically conductive carbon-containing materials, including carbon particles and carbon fibers, such as Ketjen Black (product name; manufactured by: Ketjen Black International Company), Vulcan (product name; manufactured by: Cabot), Norit (product name; manufactured by: Norit), Black Pearls (product name; manufactured by: Cabot) and Acetylene Black (product name; manufactured by: Chevron), and metallic materials such as metal particles and metal fibers.

[0038] The support on which the palladium-containing particle is mounted can be a previously manufactured support or a commercially available support.

[0039] Any conventional application method can be used to deposit the palladium-containing particle onto the substrate. If a palladium alloy particle is used, the production of the palladium alloy can be carried out simultaneously with the application of the palladium alloy particle.

[0040] In this step, the palladium-containing particle is mixed with the first solution in which the platinum compound is dissolved. There are no particular restrictions on how the palladium-containing particle is mixed with the first solution. For example, a powder of the palladium-containing particle itself can be mixed with the first solution; a powder on the support to which the palladium-containing particle is attached can be mixed with the first solution; a dispersion of the palladium-containing particle can be mixed with the first solution; or a dispersion of the support to which the palladium-containing particle is attached can be mixed with the first solution. That is to say, the palladium-containing particles can be in a solid state or in a state dispersed in solution. It also makes no difference whether the palladium-containing particle is attached to the support or not.

[0041] In the present invention, the platinum compound as such can be present in "the first solution in which the platinum compound is dissolved," or platinum ions can be present therein. That is to say, the platinum element originating from the platinum compound must be contained in the first solution. The platinum compound used here comprises platinum salts and platinum complexes.

[0042] As described above, the inventors of the present invention first discovered that when the palladium-containing particle is brought into direct contact with the solution in which the platinum compound is dissolved (hereinafter also referred to as the platinum compound solution), the platinum is deposited on the surface of the palladium-containing particle without the palladium being substituted by the platinum.

[0043] The platinum compound solution specifically concerns a system that uses chloroplatinate. This finding is based on the following verification (see Reference Example 1). First, the palladium content in the palladium-supported carbon used in Reference Example 1 is 15.9%. Next, if the palladium is eluted from the palladium particle surface (corresponding to approximately 33% of the particle) and platinum is deposited on it (calculated as Pt: 9.47% and Pd: 10.1%), the ratio of palladium (10.1%) to the palladium-supported carbon (90.5%) is calculated as follows: 10.1 / 90.5 = 11.2%. However, in the catalyst for fuel cells of reference example 1, the ratio of palladium (13.9%) to palladium-supported carbon (93.4%) is 13.9 / 93.4=14.9%.The palladium content in reference example 1 (14.9%) is closer to the palladium content in the raw material (palladium-supported carbon) (15.9%) than the value when the palladium is eluted (11.2%). This result clearly shows that when the palladium-containing particle is immersed in the platinum compound solution, the platinum is deposited directly onto the surface of the palladium-containing particle without damaging its surface.

[0044] Furthermore, the inventors of the present invention have found that the fine catalyst particle obtained by such direct contact of the palladium particle with the platinum compound solution exhibits better bulk activity, specific activity and stability compared to the conventional core-shell catalyst synthesized by Cu-UPD.This means that, as can be clearly seen from the comparison between Reference Example 1 and Comparison Example 1 described below, although the platinum was deposited in an amount approximately identical to the surface area of ​​the palladium particle, the fine catalyst particle obtained by direct contact of the palladium particle with the platinum compound solution (Reference Example 1) exhibits better bulk activity and specific activity than the conventional core-shell catalyst synthesized by Cu-UPD (Comparison Example 1), and the retention rate of the electrochemical surface area after one potential cycle is higher.

[0045] The reason for the difference in the retention rate of the electrochemical surface area is attributed to the following: Due to the difference in the platinum deposition method, the platinum-covered area on the surface of the palladium-containing particle varies, resulting in varying integrity of the resulting fine catalyst particle. Specifically, the method of directly contacting the palladium-containing particle with the platinum compound solution is considered a method that can preferentially deposit the platinum on the relatively unstable surface of the palladium-containing particle.

[0046] The fuel cell catalysts of Reference Examples 1 and 2 differ only in the amount of platinum compound used, and both contain the fine catalyst particle obtained through direct contact of the palladium particle with the platinum compound solution. As shown in Table 1 below, a comparison of the ICP measurement results of Reference Examples 1 and 2 reveals virtually no difference in the proportion of platinum and palladium on the surface of the palladium particle and in terms of coverage.This result illustrates the following facts: Even if the amount of platinum compound is changed in the process of directly contacting the palladium-containing particle with the platinum compound solution, the composition of the surface of the palladium-containing particle is not significantly affected and is not very sensitive to the amount of platinum added; and the amount of platinum that can be directly deposited on the surface of the palladium-containing particle has already been determined. From this result, it is inferred that in the process of directly contacting the palladium-containing particle with the platinum compound solution, platinum atoms are deposited only on the palladium surface where the platinum is relatively unstable, and that no platinum atoms are deposited on the palladium surface where the platinum is relatively stable.

[0047] Accordingly, it is assumed that the fine catalyst particle with excellent stability can be obtained by depositing the platinum on the relatively unstable surface of the palladium-containing particle and then depositing the platinum on another surface of the palladium-containing particle.

[0048] Fig. Figure 1 is a schematic sectional view of a typical example of the first composite body obtained by this step. Fig. Figure 1 is a view intended to explain how the palladium-containing particle is coated with the platinum, and the first composite body of the present invention is not related to the one shown in Figure 1. Fig. 1. The embodiment shown is limited.

[0049] As in Fig. As shown in Figure 1, a typical example 100a of the first composite body is a composite body in which platinum atoms 2 are deposited on a portion of the surface of a palladium-containing particle 1. The typical example 100a of the first composite body exhibits better mass activity and specific activity and shows a higher retention rate of the electrochemical surface area (which provides information about the catalyst stability) than the conventional core-shell catalyst synthesized by Cu-UPD. Therefore, it is assumed that in the case of direct contact of the palladium-containing particle with the platinum compound solution, the platinum is deposited on a portion of the Pd{110} surface, which consists of more easily elutible edges and corners, and on a portion of the Pd{111} surface, which has a higher oxygen reduction activity of platinum.

[0050] However, it is assumed that platinum obtained by Cu-UPD in such a quantity that the geometric coverage is about 60% cannot cover the easily elutable Pd{110} surface.

[0051] In this specification, a combination of the chemical formula representing the crystal's chemical composition (the element symbol if the crystal is a single crystal) and the crystal surface is used to designate a particular crystal surface of a metal crystal. For example, "Pd{110}" means the {110} surface of a palladium metal crystal. This specification also shows a group of equivalent surfaces in parentheses to designate a crystal surface. For example, the (110) surface, (101) surface, (011) surface, (-1-10) surface, (-10-1) surface, (0-1-1) surface, and the like are all referred to as the (110) surface.

[0052] In this step, the platinum, which covers at least part of the surface of the palladium-containing particle, exhibits high activity as a catalyst for a fuel cell, in particular high oxygen reduction reaction (ORR) activity. The platinum serves as a raw material for forming the outermost platinum layer of the fine catalyst particle.

[0053] The first solution used in this step preferably contains an acid. Examples of acids contained in the first solution include sulfuric acid, nitric acid, perchloric acid, hydrochloric acid, and hypochlorous acid. Of these, sulfuric acid is preferred.

[0054] It is preferred to remove oxygen and so forth from the first solution as much as possible by pre-injecting an inert gas such as nitrogen gas or argon gas into the first solution.

[0055] The amount of platinum compound in the first solution is preferably determined from the area (or volume) of the outermost platinum layer to be formed, which is calculated from the mean particle diameter of the palladium-containing particles. The mean particle diameter of the palladium-containing particles can be calculated using the method described above.

[0056] The amount of platinum atoms contained in the first solution is 70 at.% or less if the minimum amount of platinum atoms required to cover the palladium-containing particle with a monatomic platinum layer (hereinafter also referred to as the "minimum platinum atom amount") is 100 at.%. As just described, adjusting the amount of platinum atoms contained in the first solution to a predetermined amount or less allows for a greater increase in the catalytic activity of the resulting first composite body itself compared to using the platinum atoms directly at an amount of 100 at.% or more.

[0057] If the minimum platinum atom quantity is 100 at.%, then the quantity of platinum atoms contained in the first solution is preferably 65 at.% or less, more preferably 60 at.% or less.

[0058] The time required for the formation of the first composite body is not subject to any particular limitations, provided that it is a time during which the platinum contained in the first solution can be sufficiently deposited on the surface of the palladium-containing particle, and that the time can be appropriately controlled by a reaction scale. For example, the point at which the formation of the first composite body ceases to form is indicated when the rise in the open-circuit potential, which is increased by mixing the palladium-containing particle with the first solution, stops.

[0059] For example, the time required to form the first composite body is approximately 1 to 24 hours based on 1 to 100 g of the palladium-containing particles.

[0060] A concrete example of the first composite formation step is as follows. First, the already deoxidized first solution is gradually added dropwise to a reaction vessel containing the palladium-containing particle. The amount of first solution added to the vessel is 70 at.% or less, provided the minimum amount of platinum atoms required to cover the palladium-containing particle with a monatomic platinum layer is 100 at.%. While simultaneously monitoring the internal potential of the reaction vessel, the mixture is stirred until the potential reaches a plateau (i.e., until the platinum covering reaction ends), at which point at least a portion of the surface of the palladium-containing particle is covered with platinum.

[0061] Preferably, the palladium-containing particle is subjected to an acid treatment before the first composite body is formed. More preferably, the support on which the palladium-containing particle is mounted is subjected to an acid treatment. As used herein, "acid treatment" comprises a treatment such that the support on which the palladium-containing particle is mounted is simply added to an acid solution, and a treatment such that the support on which the palladium-containing particle is mounted is added to an acid solution and then a potential is applied to it.

[0062] The acid solution preferably used in the present invention is an acid solution with an oxidizing power sufficient to remove oxides from the surface of the palladium-containing particle. Specific examples include nitric acid, sulfuric acid, perchloric acid, hydrochloric acid, and hypochlorous acid. Sulfuric acid is particularly preferred with regard to its oxidizing power, especially for dissolving palladium. The concentration of the acid solution and the control of the acid solution atmosphere by bubble generation can be adjusted appropriately depending on the type of acid solution.

[0063] From the perspective that the potential treatment is carried out uniformly and quickly on all palladium-containing particles, it is preferred that the palladium-containing particles do not aggregate with each other in the acid solution in which the palladium-containing particles are dispersed and are uniformly distributed in the acid solution.

[0064] When a potential is applied to the dispersion during acid treatment, the applied potential is not subject to any particular restrictions. For example, a rectangular wave pattern of 0.1 to 1.1 V can be applied.

[0065] In particular, a potential range of 0.4 to 0.6 V (vs. RHE) is preferred, as this is a potential range that allows the removal of oxides (oxide film or layer) from the surface of the palladium-containing particle. A potential of less than 0.4 V (vs. RHE) can cause the palladium to trap hydrogen. Conversely, a potential of more than 0.6 V (vs. RHE) can cause metals in the palladium-containing particle, such as palladium, to elute. Even if the applied potential is approximately 0.2 V below the lower limit of 0.4 V (vs. RHE), the cleaning effect of removing the oxides from the surface of the palladium-containing particle is comparable to the effect of a sweep in a potential range of 0.4 to 0.6 V (vs. RHE). The range of the potential applied during acid treatment is preferably a range of 0.4 to 0.45 V (vs. RHE).

[0066] During acid treatment, the potential treatment can be carried out by setting the potential to a predetermined value, or a sweep can be performed once or repeatedly within a predetermined potential range, provided the potential is in the range of 0.4 to 0.6 V (vs. RHE). Considering that desorption of materials adsorbed on the surface of the palladium-containing particle can be repeated, and that oxides present on the surface can be efficiently removed, the potential treatment performed during acid treatment is preferably such that the potential is swept between any two potentials in the range of 0.4 to 0.6 V (vs. RHE).

[0067] When the potential is swept between any two potentials, the number of sweeps can be appropriately controlled depending on the reaction scale. For example, the number of sweeps is approximately 1 to 1,000 cycles based on 1 to 100 g of the palladium-containing particles.

[0068] During acid treatment, the potential application time is not subject to any particular restrictions, provided it is sufficient to remove the oxides from the surface of the palladium-containing particle. The time can be appropriately controlled depending on the synthesis scale. For example, in the case of a potential treatment where the potential is swept between any two potentials in a range of 0.4 to 0.6 V (vs. RHE), a state in which the contour of the potential treatment waveform almost coincides with the contour of the waveform of the last sweep, and even after multiple sweeps the potential, the contours of the potential sweep waveforms become almost identical, can serve as an indication to terminate the potential application.In this case, the current fluctuation with respect to the potential treatment is constant, and it can be assumed that almost all oxides on the surface of the palladium-containing particle have disappeared.

[0069] The potential application time is, for example, approximately 1 to 24 hours based on 1 to 100 g of the palladium-containing particles.

[0070] A concrete example of acid treatment is as follows. First, the palladium-containing particles are added to water and dispersed in it in a suitable manner. An acid solution is then added. Next, a potential in the range of 0.4 to 0.6 V (vs. RHE) is traversed back and forth. It is preferred that oxygen and other elements be removed from the acid solution as much as possible at this point by first introducing an inert gas such as nitrogen or argon into the acid solution.

[0071] As just described, by performing the potential treatment on the palladium-containing particle prior to its platinum coating, oxides that accumulate on the surface of the palladium-containing particle, such as palladium oxide, can be removed, thus cleaning the surface of the palladium-containing particle. By setting the applied potential in the range of 0.4 to 0.6 V (vs. RHE), preferably in the range of 0.4 to 0.45 V (vs. RHE), there is no possibility of metals such as palladium being eluted from the palladium-containing particle and no possibility of hydrogen being trapped by the palladium. Therefore, there is no possibility of new oxides appearing on the surface of the palladium-containing particle. Steps 1-2 of forming the second composite body

[0072] This is a step in forming the second composite body containing palladium, platinum, and copper by mixing the first composite body with a second solution in which a copper compound is dissolved, and then covering at least part of the surface of the first composite body with copper using copper underpotential deposition (Cu-UPD). Cu-UPD allows the amount of copper deposited between the first composite bodies to be standardized when the first composite bodies are covered with copper.

[0073] In this step, the first composite body is mixed with the second solution in which the copper compound is dissolved. The embodiment of mixing the first composite body with the second solution is not subject to any particular restrictions. For example, a powder of the first composite body itself can be mixed with the second solution; a powder of the support on which the first composite body is mounted can be mixed with the second solution; a dispersion of the first composite body can be mixed with the second solution; or a dispersion of the support on which the first composite body is mounted can be mixed with the second solution. That is to say, the first composite body can be in a solid state or in a state dispersed in solution. It is also irrelevant whether the first composite body is mounted on the support or not.Furthermore, the first composite body can be mixed with the second solution while the first composite body is in a state where it is dispersed in the first solution described above.

[0074] In the present invention, the copper compound as such can be present "in the second solution in which the copper compound is dissolved," or copper ions can be present therein. That is to say, the copper element originating from the copper compound must be contained in the second solution. The copper compound used here comprises copper salts and copper complexes.

[0075] Further conditions for the Cu-UPD used in this step can be generally known conditions.

[0076] A concrete example of this step is as follows. First, a copper compound such as copper sulfate is added to a reaction vessel containing the first composite body. Next, a potential approximately equal to the underpotential deposition (UPD) potential is applied to the reaction mixture, so that only one layer of copper atoms is deposited on the first composite body. This process forms the second composite body, in which at least part of the surface of the first composite body is covered with copper. Steps 1-3 of substituting the copper in the second composite body with platinum

[0077] This is a step of substituting the copper in the second composite body with platinum, which comes from a third solution in which a platinum compound is dissolved, by mixing the second composite body with the third solution.

[0078] In this step, the copper in the second composite body is preferably substituted by the platinum from the third solution by mixing the second composite body with the third solution and then maintaining a potential until it becomes uniform.

[0079] The platinum compound dissolved in the third solution and the acid preferably contained in the third solution are identical to those in the first solution.

[0080] The amount of platinum compound contained in the first and third solutions can be appropriately controlled depending on the reaction conditions. From the perspective of minimizing the amount of platinum used, it is preferred to keep the total amount of platinum atoms contained in the first and third solutions approximately equal to the minimum amount of platinum atoms described above.

[0081] It is assumed that in the conventional manufacturing process using Cu-UPD, the edges and so on of the surface of the palladium-containing particle are less likely to be substituted by the platinum, resulting in an incomplete core-shell structure. Fig. Figure 11 is a schematic cross-sectional view of the composite body, in which the surface of the palladium particle is completely covered with copper atoms. As in Fig. As shown in Figure 11, a composite body 300 is a particle in which copper atoms 3 are deposited on the surface of the palladium-containing particle 1. The copper atoms 3 include copper atoms 3a, which are deposited on the edges or corners of the surface of the palladium-containing particle, and copper atoms 3b, which are deposited on the terraces or projections of the surface of the palladium-containing particle. Adsorption of oxygen atoms at the edges and corners of the surface of the palladium-containing particle is known to be probable, while their detachment from these edges is less probable. Due to the same principle, the copper atoms 3a have a higher adsorbability to the surface of the palladium-containing particle than the copper atoms 3b. Accordingly, the copper atoms 3a are less likely to be substituted by platinum.The platinum atoms that are not substituted by the copper atoms 3a are inevitably deposited on other platinum atoms or on the support. Consequently, although the platinum itself can be deposited, the contribution of the deposited platinum to the ORR activity is small, thus reducing the overall mass activity of the fine catalyst particle.

[0082] In the manufacturing process of the present invention, the in Fig. The first composite body shown, using Cu-UPD, is further coated with platinum. When the platinum-coated state is reached, two [units] are shown. Fig. 2 and Fig. Eight models are expected, as shown below.

[0083] Fig. Figure 8 is a schematic view showing a transition of a section into a covered state, as would be expected from a conventional method for producing a core-shell catalyst using Cu-UPD. Fig. Figure 8 above is a schematic sectional view of the first composite body 100a and is equipped with Fig. 1 identical. Fig. Figure 8 in the middle is a schematic sectional view of a second composite body 100b, in which the surface of the first composite body is further covered with a monatomic layer consisting of the copper atoms 3. Fig. Figure 8 below is a schematic sectional view of the second composite body 100b in a state such that the copper atoms 3 on the platinum atoms 2 have preferably been substituted by the platinum atoms 2. Arrows between the views indicate the transition to the covered state.

[0084] In the Fig. In the model shown below, if, for example, the platinum and palladium exposed on the surface of the core-shell catalyst correspond to 60% and 40% respectively, the specific activity of the core-shell catalyst is 2.40 (A / m²). 2) calculated. This specific activity does not differ from the specific activity of the first composite body 100a. However, as shown in Table 1 below, the specific activity of the fine catalyst particle obtained by the manufacturing process of the present invention (Example 1) is 4.73 (A / m³). 2 ), so this model cannot be used.

[0085] Fig. Figure 2 is a schematic view showing the transition of a section to a covered state when copper atoms on a palladium atom are preferentially substituted by platinum atoms. The figures shown in Fig. The two images shown above and in the middle are the same as those in Fig. 8 top and middle. Fig. Figure 8 below is a schematic sectional view showing the second composite body 100b in a state such that the copper atoms 3 on the surface of the palladium-containing particle 1 have preferably been replaced by the platinum atoms 2. Arrows between the views indicate the transition to the covered state.

[0086] As is known, the specific activity of platinum atoms on palladium atoms is 1.3 times higher than that of pure platinum. Since the specific activity of platinum is 3.2 (A / m³), 2 ) the specific activity of the platinum atoms on the palladium atoms is calculated to be more than 4.2 (A / m²). 2 Accordingly, the above value of 4.73 (A / m²) 2 ) (the specific activity of Example 1) is almost identical to the value calculated assuming that 100% of the palladium particle surface is covered with platinum. That is to say, it can be stated that a in Fig. 2 Model 100c shown below is the fine catalyst particle produced by the present invention.

[0087] In a generally known document ( Fig. 2. In J. Greeley et al., Electrochimica Acta, 52 (2007) 5829-5836), a first-principle energy calculation describes how the energy required to detach a copper particle from the surface of a palladium host is lower than that required to detach a copper particle from a platinum host. The calculation results described in this well-known document are helpful in understanding the phenomenon caused by the in Fig. 2. The model shown below illustrates that the copper atoms on the surface of the palladium-containing particle are more likely to be preferentially substituted by the platinum atoms than the copper atoms on the platinum atoms.

[0088] Furthermore, the fine catalyst particle produced by the present invention, as shown in Table 1 below, exhibits a very small difference between the mass activity before its use and the mass activity after the application of a potential cycle (see Example 1). This fact indicates that a complete core-shell structure is formed immediately after production, in which the surface of the palladium-containing particle is almost completely covered with the outermost platinum layer, which is responsible for the ORR activity.

[0089] A concrete example of this step is as follows. First, the third solution, in which the platinum compound is dissolved, is gradually added dropwise to a reaction vessel containing the second composite body. While simultaneously monitoring the intrinsic potential inside the reaction vessel, the mixture is stirred until the potential reaches a plateau (i.e., until the platinum covering reaction ends), whereby the monatomic copper layer on the surface of the palladium-containing particle is replaced by a monatomic platinum layer, and the fine catalyst particle is obtained. 1-4. Further steps

[0090] After the production of the fine catalyst particle, filtering, rinsing, drying, and so on can be carried out on the fine catalyst particle.

[0091] The filtering and rinsing of the fine catalyst particle is not subject to any particular restrictions, provided it is carried out by methods that can remove impurities without damaging the coated structure of the fine catalyst particle thus produced. An example of filtering and rinsing is suction filtration using water, perchloric acid, dilute sulfuric acid, dilute nitric acid, etc.

[0092] Drying the fine catalyst particle is not subject to any particular restrictions, provided it is carried out by a process capable of removing solvents, etc. One example of such a drying process is to vacuum-dry the fine catalyst particle for 0.5 to 2 hours at room temperature and then dry it for 1 to 12 hours at a temperature of 60 to 80°C in an inert gas atmosphere.

[0093] As described above, in the manufacturing process of the present invention, platinum is deposited on at least a portion of the surface of the palladium-containing particle without the use of Cu-UPD, and then platinum is further deposited on the remaining surface of the palladium-containing particle using Cu-UPD. Therefore, compared to conventional manufacturing processes using only Cu-UPD, a fine catalyst particle can be obtained that exhibits higher mass activity and specific activity from the early stage (immediately after production) and has excellent stability. This result indicates that, compared to conventional Cu-UPD, the manufacturing process of the present invention has been able to create a core-shell structure that closely resembles the structure of a final product (i.e., a fine catalyst particle with the highest activity).Due to its high degree of perfection, the mass activity, specific activity and electrochemical surface area can be maintained at exactly the same level as in the early stage, even after the application of a potential cycle.

[0094] Furthermore, the present invention offers the advantage that, in contrast to conventional synthesis methods that use only Cu-UPD, the amount of copper used is small, resulting in little copper-containing effluent that is removed after synthesis. Also, when the fine catalyst particle produced by the present invention is used in a membrane electrode arrangement, the influence of copper remaining in the fine catalyst particle on the membrane electrode arrangement is minimal, a feature that has long been of interest.

[0095] As just described, compared to conventional synthesis methods, the manufacturing process of the present invention can provide the fine catalyst particle with a higher coverage in a simpler and more cost-effective manner. 2. Second method for producing a fine catalyst particle

[0096] The second, non-inventive method for producing a fine catalyst particle is a method for producing a fine catalyst particle comprising a palladium-containing particle and an outermost platinum layer covering the palladium-containing particle, wherein a composite body A containing palladium and copper is formed by mixing the palladium-containing particle with a second solution in which a copper compound is dissolved, and then covering at least a part of a surface of the palladium-containing particle with copper using copper sub-potential deposition; wherein a composite body B containing palladium and platinum is formed by mixing the composite body A with a third solution in which a platinum compound is dissolved, and substituting the copper in the composite body A with the platinum from the third solution;and wherein at least a part of a surface of the composite body B is covered with platinum by mixing the composite body B with a first solution in which a platinum compound is dissolved.

[0097] In the first manufacturing process, the step of coating with platinum using Cu-UPD (the preceding “1-2 step of forming the second composite body”) and „ 1-3. Step of substituting the copper in the second composite body with platinum") after the step of covering with platinum without using Cu-UPD (the preceding "1-1. Step of forming the first composite body").

[0098] As a general principle, there is no problem with platinum coating even if, contrary to the above sequence, the step of coating with platinum without using Cu-UPD is carried out after the step of coating with platinum using Cu-UPD, and the same effects can be obtained as with the manufacturing process described above.

[0099] Step (A) is a step involving the application of Cu-UPD and corresponds to the preceding “Steps 1-2 of forming the second composite body”. Step (A) and the preceding “Steps 1-2 of forming the second composite body” differ in that, while in the preceding “Steps 1-2 of forming the second composite body” the first composite body containing palladium and platinum is the subject of Cu-UPD, in step (A) the palladium-containing particle (raw material) is the subject. However, in step (A), the composite body A containing palladium and copper can be formed by applying Cu-UPD under almost the same conditions as in the preceding “Steps 1-2 of forming the second composite body”. Preferably, the palladium-containing particle is pre-treated with acid before the composite body A is formed.Preferably, the carrier on which the palladium-containing particle is mounted is subjected to acid treatment.

[0100] Step (B) corresponds to the preceding “steps 1-3 of substituting the copper in the second composite body with platinum”. Step (B) and the preceding “steps 1-3 of substituting the copper in the second composite body with platinum” differ in that, while in the preceding “steps 1-3 of substituting the copper in the second composite body with platinum” the second composite body containing palladium, platinum, and copper is the object of the platinum coating, in step (B) the composite body A containing palladium and copper is the object. However, in step (B), composite body B containing palladium and platinum can be formed by substituting the copper with platinum under almost the same conditions as in the preceding “steps 1-3 of substituting the copper in the second composite body with platinum”.

[0101] Excess copper remaining on the surface of the composite body B can be removed by rinsing the composite body B thus obtained after step (B) and before step (C).

[0102] Step (C) corresponds to the preceding “Step 1-1 of forming the first composite body”. Step (C) and the preceding “Step 1-1 of forming the first composite body” differ in that, while in the preceding “Step 1-1 of forming the first composite body” the palladium-containing particle (raw material) is coated with platinum, in step (C) the composite body B containing palladium and platinum is the subject. However, in step (C), the fine target catalyst particle can be obtained by coating it with platinum under almost the same conditions as in the preceding “Step 1-1 of forming the first composite body”. 3. Fine catalyst particle

[0103] In the fine catalyst particle produced by the present invention, the coverage of the palladium-containing particle with the outermost platinum layer is preferably 88 to 100%. If the coverage is less than 88%, the palladium-containing particle is eluted in electrochemical reactions and can lead to a deterioration of the fine catalyst particle.

[0104] In the fine catalyst particle produced by the present invention, the coverage of the palladium-containing particle with the outermost platinum layer is preferably 89 to 100%, more preferably 97 to 100%.

[0105] The outermost platinum layer formed in this step is preferably a monatomic layer. This is because the catalytic performance of the outermost platinum layer of such a fine catalyst particle is significantly higher than that of fine catalyst particles where the outermost platinum layer consists of two or more atomic layers, and the amount of covering outermost platinum layer is small, resulting in lower material costs.

[0106] The lower limit of the mean particle diameter of the fine catalyst particles is preferably 3 nm or more, more preferably 4 nm or more, and the upper limit is preferably 40 nm or less, more preferably 10 nm or less.

[0107] The fine catalyst particles produced by the manufacturing process of the present invention are preferably supported on a support. The support is as described above. 4. Fuel cell

[0108] The fuel cell of the present invention is a fuel cell with unit cells, each comprising a membrane electrode arrangement in which an anode electrode with at least one anode catalyst layer is arranged on one side of a polyelectrolyte membrane and a cathode electrode with at least one cathode catalyst layer is arranged on another side of the polyelectrolyte membrane, wherein a fine catalyst particle produced by the first or second manufacturing process is contained in the anode catalyst layer and / or the cathode catalyst layer.

[0109] Fig. Figure 3 shows an example of the unit cell of the fuel cell of the present invention and also schematically shows a section through the unit cell along a layer arrangement direction. A membrane electrode assembly 18 comprises a hydrogen ion-conducting polyelectrolyte membrane (hereinafter also referred to simply as the electrolyte membrane) 11 and a pair of a cathode electrode 16 and an anode electrode 17, which enclose the electrolyte membrane 11 between them. A unit cell 200 comprises the membrane electrode assembly 18 and a pair of separators 19 and 20, which enclose the membrane electrode assembly 18 from the outside of the electrodes. Gas channels 21 and 22 are arranged at the boundaries of the separators and the electrodes.In general, a layered composite consisting of a catalyst layer and a gas diffusion layer, stacked in that order starting from the closest to the electrolyte membrane side, is used as the electrodes. That is, the cathode electrode 16 comprises a layered composite consisting of a cathode catalyst layer 12 and a gas diffusion layer 14, and the anode electrode 17 comprises an anode catalyst layer 13 and a gas diffusion layer 15. The catalyst for fuel cells according to the present invention is used in the anode catalyst layer and / or the cathode catalyst layer.

[0110] A polyelectrolyte membrane is a polyelectrolyte membrane used in fuel cells. Examples include fluorine-based polyelectrolyte membranes containing fluorine-based polyelectrolytes, such as perfluorocarbon sulfonic acid resin, as represented by Nafion (trademark), and hydrocarbon-based polyelectrolyte membranes containing hydrocarbon-based polyelectrolytes obtained by incorporating a proton-conducting group, such as a sulfonic acid group, carboxylic acid group, phosphoric acid group, or boric acid group, into an engineering plastic, such as polyetheretherketone, polyetherketone, polyethersulfone, polyphenylene sulfide, polyphenylene ether, or polyparaphenylene, or into a commodity plastic, such as polyethylene, polypropylene, or polystyrene.

[0111] Each of the electrodes contains the catalyst layer and the gas diffusion layer.

[0112] Both the anode catalyst layer and the cathode catalyst layer can be formed using a catalyst ink containing a catalyst, an electrically conductive material, and a polyelectrolyte. The same material used for the polyelectrolyte membrane mentioned above can be used as the polyelectrolyte. The fine catalyst particle according to the present invention is used as the catalyst.

[0113] The fine catalyst particle according to the present invention can be used only for the anode catalyst layer, only for the cathode catalyst layer, or for both the anode catalyst layer and the cathode catalyst layer. If the fine catalyst particle according to the present invention is used only for the anode catalyst layer, a different catalyst is used for the cathode catalyst layer. Conversely, if the fine catalyst particle according to the present invention is used only for the cathode catalyst layer, a different catalyst is used for the anode catalyst layer.

[0114] The other catalyst is generally one in which a catalytic component is carried on an electrically conductive particle. The catalytic component is not subject to any particular restrictions, provided it exhibits catalytic activity with respect to the oxidation reaction of a fuel supplied to the anode electrode or with respect to the reduction reaction of an oxidant supplied to the cathode electrode. A catalyst generally used for solid polymer fuel cells can be employed. For example, platinum or an alloy of platinum and a metal, such as ruthenium, iron, nickel, manganese, cobalt, or copper, can be used. The electrically conductive particle serving as the catalyst support can be an electrically conductive carbon-containing material, such as a carbon particle or carbon fiber (e.g., carbon fiber).Carbon black), or a metallic material, such as a metal particle or a metal fiber, can be used. The electrically conductive material also plays a role in imparting electrical conductivity to the catalyst layer.

[0115] The method for forming the catalyst layer is not subject to any particular restrictions. For example, the catalyst layer can be formed on a gas diffusion layer by applying the catalyst ink to a surface of the gas diffusion layer and drying the applied ink, or the catalyst layer can be formed on the polyelectrolyte membrane by applying the catalyst ink to a surface of the polyelectrolyte membrane and drying the applied ink.Alternatively, the catalyst layer can be formed on the polyelectrolyte membrane or the gas diffusion layer by the following procedure: a transfer layer is produced by applying the catalyst ink to a surface of a transfer substrate and drying the applied ink; the transfer layer is applied to the polyelectrolyte membrane or the gas diffusion layer by hot pressing or the like; and the substrate film of the transfer layer is removed, thereby forming the catalyst layer on the polyelectrolyte membrane or the gas diffusion layer.

[0116] The catalyst ink can be obtained by dispersing the aforementioned catalyst, an electrolyte for electrodes, and so on, in a solvent. The solvent for the catalyst ink can be selected appropriately. For example, an organic solvent such as alcohol (e.g., methanol, ethanol, propanol), N-methyl-2-pyrrolidone (NMP), or dimethyl sulfoxide (DMSO), a mixture of organic solvents, or a mixture of water and one of the organic solvents can be used. In addition to the catalyst and the electrolyte, the catalyst ink may optionally contain other components, such as a binder and a water-repellent resin.

[0117] The method for applying the catalyst ink, the method for drying the catalyst ink, etc., can be selected appropriately. Examples of methods for applying the catalyst ink include spraying, screen printing, doctor blade or scraper application, gravure printing, and die coating. Examples of methods for drying the catalyst ink include reduced-pressure drying, heat drying, and reduced-pressure heat drying. The specific conditions for reduced-pressure drying or heat drying are not subject to any particular restrictions and can be determined appropriately. The thickness of the catalyst layer is not subject to any particular restrictions and can range from approximately 1 to 50 µm.

[0118] The gas diffusion layer used to form the gas diffusion layer must possess the required gas diffusion capacity to ensure efficient fuel supply to the catalyst layer, as well as electrical conductivity and strength. Examples include carbon-containing porous materials such as carbon paper, carbon cloth, and carbon felt, and electrically conductive porous materials such as metallic lattices and metallic porous materials made from metals like titanium, aluminum and alloys thereof, nickel, nickel-chromium alloy, copper and alloys thereof, silver, zinc alloy, lead alloy, niobium, tantalum, iron, stainless steel, gold, platinum, etc. The thickness of the electrically conductive porous material is preferably about 50 to 500 µm.

[0119] The gas diffusion layer can be made from a single layer of electrically conductive, porous material, or a water-repellent layer can be provided on one side of the layer facing the catalyst layer. Generally, the water-repellent layer has a porous structure containing an electrically conductive powder and granular material, such as carbon particles or carbon fibers, a water-repellent resin, such as polytetrafluoroethylene (PTFE), etc. The water-repellent layer is not always necessary; however, it offers the advantage of enhancing the conductivity of the gas diffusion layer, maintaining the water content in the catalyst layer and the polyelectrolyte membrane appropriately, and improving the electrical contact between the catalyst layer and the gas diffusion layer.

[0120] The polyelectrolyte membrane with the catalyst layer formed on it by the aforementioned method and the gas diffusion layer can be stacked in a suitable manner and attached to one another by hot pressing or the like, thereby obtaining a membrane electrode arrangement.

[0121] The membrane electrode assembly thus produced is preferably arranged between a pair of separators that have a reaction gas channel, thereby forming a unit cell. The separators can be those that possess electrical conductivity and gas sealing properties and can serve as a current collector and gas sealant, such as carbon separators containing a high concentration of carbon fibers and made from a resin composite, or metal separators made from a metallic material. Examples of metal separators include those made from a metal material with excellent corrosion resistance and separators coated with carbon or a metal material with excellent corrosion resistance, thus providing a coating for enhanced corrosion resistance.The reaction gas channel described above can be formed, for example, by suitable cutting or compression molding of the separators. Examples

[0122] The present invention is described in more detail below with reference to examples and comparative examples. However, the scope of the present invention is not limited to these examples. 1. Production of a catalyst for fuel cells containing fine catalyst particles. Example 11-1. Pretreatment of carbon-supported palladium particles.

[0123] First, 5 g of carbon-supported palladium particles were added to 1 L of pure water and dispersed using an ultrasonic homogenizer. The resulting dispersion was added to an electrochemical reactor and mixed with sulfuric acid to achieve a sulfuric acid concentration of 0.05 mol / L. The electrochemical reactor was placed in a glove box. The dispersion was deoxidized by bubbling a sufficient amount of an inert gas (N₂ gas) into it. A potential window of 0.4 to 0.45 V (vs. RHE) was then applied to the working electrode of the electrochemical reactor for 360 cycles to adequately reduce the palladium particle surface area. 1-2. Formation of the first composite body

[0124] A deoxidized K₂PtCl₄ sulfuric acid solution was gradually added dropwise to the electrochemical reactor. The amount of K₂PtCl₄ sulfuric acid solution added was 55 at.%, given that the minimum amount of platinum atoms required to cover the palladium particle with a monatomic platinum layer is 100 at.%. While simultaneously monitoring the intrinsic potential within the electrochemical reactor, the mixture was stirred until the potential reached a plateau (i.e., until the platinum covering reaction ended), at which point a portion of the palladium particle's surface was covered with platinum.

[0125] Fig. Figure 4 is a graph showing a transition observed by monitoring the formation of the first composite body in Example 1. Fig. 4. The K2PtCl4-sulfuric acid solution was added dropwise at a time two minutes after the start of the measurement. As from Fig. As can be clearly seen in Figure 4, the intrinsic potential began to rise quite rapidly immediately after the addition of K₂PtCl₄ sulfuric acid; however, the rise of the intrinsic potential slowed down due to the consumption of the K₂PtCl₄. After 20 minutes had elapsed since the start of the measurement, the intrinsic potential reached a plateau at 0.86 V (vs. RHE) and the reaction ended. 1-3. Formation of the second composite body

[0126] A deoxidized 0.05 mol / l copper sulfate (CuSO4)-sulfuric acid solution was added to the electrochemical reactor containing the first composite body, and the copper ions (Cu 2+The concentration of the mixture was adjusted to 0.05 mol / l. Then, 0.37 V (vs. RHE) was applied to the working electrode of the electrochemical reactor, and the potential was maintained unchanged until the current reached 0 A (Cu-UPD). This process formed the second composite body, in which at least part of the surface of the first composite body was covered with copper. 1-4. Substitution of the copper atom layer by the outermost platinum layer

[0127] Deoxidized K₂PtCl₄ sulfuric acid was gradually added dropwise to the electrochemical reactor containing the second composite body. While simultaneously monitoring the intrinsic potential within the electrochemical reactor, the mixture was stirred until the intrinsic potential reached a plateau (i.e., until no change in the intrinsic potential was observed). This resulted in the replacement of the monatomic copper layer on the surface of the palladium particle with a platinum layer and the synthesis of fine catalyst particles. The amount of K₂PtCl₄ sulfuric acid solution added was the remainder of the amount used to form the first composite body, i.e., 45 at.%, given that the minimum amount of platinum atoms required to cover the palladium particle with a monatomic platinum layer is 100 at.%.

[0128] Fig. Figure 5 is a graph showing a transition that is identified by observing the substitution of the copper atom layer by the outermost platinum layer in Example 1. As shown from Fig. As can be clearly seen in Figure 5, the intrinsic potential began to rise immediately after the addition of the K₂PtCl₄-sulfuric acid solution (minute 0); however, the intrinsic potential reached a plateau at 0.58 V (vs. RHE) when the K₂PtCl₄ was consumed (80 minutes after the start) and the reaction ended. The reason why the potential only rose to 0.58 V (vs. RHE) is explained as follows: The platinum was deposited on the surface of the palladium particle during the formation of the first composite body, and then the copper was deposited onto the platinum by the Cu-UPD; however, the copper remained on the platinum. 1-5. Follow-up treatment

[0129] Impurities (such as excess ions and the copper deposited on the platinum) were removed by filtering the mixture contained in the electrochemical vessel and rinsing the resultant with 4 L of pure water. After rinsing, the resultant was vacuum-dried at 60°C for 10 hours, producing the catalyst for fuel cells of Example 1, containing the fine catalyst particles. Reference example 1

[0130] First, a pretreatment was carried out in the same manner as the above “1-1. Pretreatment of carbon-supported palladium particle” in Example 1.

[0131] Next, a deoxidized K₂PtCl₄ sulfuric acid solution was gradually added dropwise to an electrochemical reactor. The amount of K₂PtCl₄ sulfuric acid solution added was 120 at.% (St = 1.2), given that the minimum amount of platinum atoms required to cover the palladium particle with a monatomic platinum layer is 100 at.%. While simultaneously monitoring the self-potential within the electrochemical reactor, the mixture was stirred until the potential reached a plateau (i.e., until the platinum covering reaction ended), thus coating the surface of the palladium particle with platinum.

[0132] Fig. Figure 6 is a graph showing a transition that was determined by observing the platinum coverage in Reference Example 1. As shown from Fig. As can be clearly seen in Figure 6, the intrinsic potential began to rise rapidly immediately after the addition of the K2PtCl4-sulfuric acid solution; however, the rise of the intrinsic potential slowed down due to the consumption of the K2PtCl4. After 40 minutes from the start of the measurement, the intrinsic potential reached a plateau at 0.88 V (vs. RHE) and the reaction ended.

[0133] Subsequently, a post-treatment was carried out in the same manner as the preceding “1-5. Post-treatment” in Example 1, thereby producing the fuel cell catalyst of Reference Example 1 containing the fine catalyst particles. Reference example 2

[0134] The fuel cell catalyst from Reference Example 2, containing the fine catalyst particles, was produced by performing a pretreatment, platinum coating, and posttreatment in the same manner as in Reference Example 1, except that when adding the K2PtCl4 sulfuric acid solution, the amount of K2PtCl4 sulfuric acid solution added was 100 at.% (St=1.0) if the minimum amount of platinum atoms required to cover the palladium particle with a monatomic platinum layer is 100 at.%. Comparative example 1

[0135] First, a pretreatment was carried out in the same manner as the preceding “1-1. Pretreatment of carbon-supported palladium particle” in Example 1.

[0136] Next, a deoxidized 0.05 mol / l copper sulfate (CuSO4)-sulfuric acid solution was added to the electrochemical reactor containing the carbon-supported palladium particles, and the copper ions (Cu 2+ The concentration of the mixture was adjusted to 0.05 mol / L. Then, 0.37 V (vs. RHE) was applied to the working electrode of the electrochemical reactor, and the potential was maintained unchanged until the current reached 0 A (Cu-UPD). This process coated the surface of the palladium particle with a layer of copper atoms. This step corresponds to the preceding „ 1-3. Formation of the second composite body" in Example 1.

[0137] A deoxidized K₂PtCl₄ sulfuric acid solution was then gradually added dropwise to the electrochemical reactor containing the palladium-copper composite. While simultaneously monitoring the self-potential within the electrochemical reactor, the solution was added dropwise until the self-potential reached 0.65 V (vs. RHE). The addition of the K₂PtCl₄ sulfuric acid solution was then stopped. This process substituted the copper atom layer on the surface of the palladium particle with an outermost platinum layer. This step corresponds to the preceding “1-4. Substitution of the copper atom layer by the outermost platinum layer” in Example 1.

[0138] Fig. Figure 9 is a graph showing a transition that is observed by noting the substitution of the copper atom layer by the outermost platinum layer in comparative example 1. Fig. 9. The K2PtCl4-sulfuric acid solution was added dropwise at the moment 4 minutes had elapsed since the start of the measurement. As from Fig. As can be clearly seen in Figure 9, the intrinsic potential within the reactor increased immediately after the addition of the K2PtCl4 sulfuric acid solution until it reached 0.65 V (vs. RHE) (50 minutes after the start of the measurement).

[0139] Subsequently, a post-treatment was carried out in the same manner as the preceding “1-5. Post-treatment” in Example 1, thereby producing the fuel cell catalyst of Comparative Example 1 containing the fine catalyst particles. Comparative example 2

[0140] First, a pretreatment was carried out in the same manner as the preceding “1-1. Pretreatment of carbon-supported palladium particle” in Example 1.

[0141] Next, a deoxidized 0.05 mol / l copper sulfate (CuSO4)-sulfuric acid solution was added to the electrochemical reactor containing the carbon-supported palladium particles, and the copper ions (Cu 2+ The concentration of the mixture was adjusted to 0.05 mol / L. Then, 0.37 V (vs. RHE) was applied to the working electrode of the electrochemical reactor, and the potential was maintained unchanged until the current reached 0 A (Cu-UPD). This process coated the surface of the palladium particle with a layer of copper atoms. This step corresponds to the preceding " 1-3. Formation of the second composite body" in Example 1.

[0142] A deoxidized K₂PtCl₄ sulfuric acid solution was then gradually added dropwise to the electrochemical reactor containing the palladium-copper composite. While simultaneously monitoring the self-potential within the electrochemical reactor, the solution was added dropwise until the self-potential reached a plateau (i.e., until no change in the self-potential was observed). The addition of the K₂PtCl₄ sulfuric acid solution was then stopped. The amount of K₂PtCl₄ sulfuric acid solution added was 120 at.% (St = 1.2), where the minimum amount of platinum atoms required to cover the palladium particle with a monatomic platinum layer is 100 at.%. This process substituted the copper atom layer on the surface of the palladium particle with an outermost platinum layer. This step corresponds to the preceding “1-4. Substitution of the copper atom layer by outermost platinum layer” in Example 1.

[0143] Fig. Figure 10 is a graph showing a transition that is observed by noting the substitution of the copper atom layer by the outermost platinum layer in comparative example 2. Fig. The infusion of the K2PtCl4-sulfuric acid solution was started at the moment two minutes had elapsed since the start of the measurement. As from Fig. As can be clearly seen in Figure 10, the intrinsic potential began to rise immediately after the addition of the K2PtCl4-sulfuric acid solution; however, the rise of the intrinsic potential slowed down due to the consumption of the K2PtCl4. After 80 minutes had elapsed since the start of the measurement, the intrinsic potential reached a plateau at 0.85 V (vs. RHE), and the reaction ended.

[0144] Subsequently, a post-treatment was carried out in the same manner as the preceding “1-5. Post-treatment” in Example 1, thereby producing the fuel cell catalyst of Comparative Example 2, which contained the fine catalyst particles. Comparative example 3

[0145] The catalyst for fuel cells of Comparative Example 3, which contained the fine catalyst particles, was produced by carrying out a pretreatment, platinum coating and posttreatment in the same manner as in Comparative Example 2, except that in the dropwise addition of the K2PtCl4 sulfuric acid solution, the amount of K2PtCl4 sulfuric acid solution added was 100 at.% (St=1.0) if the minimum amount of platinum atoms required to cover the palladium particle with a monatomic platinum layer is 100 at.%. 2. Evaluation of catalysts for fuel cells 2-1. Analysis of platinum and palladium compositions and calculation of coverage

[0146] For the fuel cell catalysts from Example 1, Reference Examples 1 and 2, and Comparison Examples 1 to 3, the amounts of platinum and palladium on the surface of the fine catalyst particle were quantified by ICP-MS and the coverage was calculated. The results are shown in Table 1. 2-2. Measurement of mass activity and electrochemical surface area of ​​catalysts for fuel cells

[0147] For the fuel cell catalysts from Example 1, Reference Example 1, and Comparison Examples 1 to 3, the mass activity (ORR activity at 0.9 V vs. RHE) and the electrochemical surface area (ECSA) were calculated using the rotating disk electrode (RDE) method. These fuel cell catalysts were also subjected to 100 potential cycles in a range of 1.05 to 0.1 V (vs. RHE) and back again; subsequently, the mass activity (ORR activity at 0.9 V vs. RHE) and the electrochemical surface area (ECSA) were measured using the RDE method. 2-3. Experimental Results

[0148] Table 1 below shows the amount of platinum added, ICP measurement results, mass activity, electrochemical surface area, and specific activity of the fuel cell catalysts from Example 1, Reference Examples 1 and 2, and Comparison Examples 1 to 3. The specific activity was calculated from the mass activity and electrochemical surface area results. In Table 1 below, "initial" refers to the result of a new fuel cell catalyst that was not used for charging and discharging.

[0149] Fig. Figure 7 is a graph showing the proportion of platinum on the surface of the palladium particle (core) in relation to the mean particle diameter of the palladium particles. The platinum fraction x on the palladium particle surface (%, the vertical axis of the graph) is calculated from the Pt fraction x using the following formula (1). Pt (%) and the Pd share x Pd(%) of the ICP measurement results shown in Table 1 were obtained. x=xPt / (xPt+xPd)

[0150] In Fig. 7. White square areas represent the data from reference example 1; black triangular areas represent the data from comparison example 1; and black circular areas represent the data from comparison example 2. White diamond areas represent the data that represent the calculation results in the case where the palladium particle surface is covered with only one platinum layer. Also, the in Fig. The curve shown in Figure 7 represents an approximation that applies to all the surfaces. The approximation (the theoretically obtained approximation of the monatomic platinum layer) is as follows: y=−25.924ln(x)+88.944

[0151] Based on the data in Table 1 and Fig. The results shown in section 7 will first be discussed in comparison example 1.

[0152] The ICP measurement results shown in Table 1 clearly show that, with regard to the fuel cell catalyst from comparative example 1, the platinum content on the catalyst surface is 7.69% and the palladium content is 14.6%. From this result, the platinum content x on the palladium particle surface is calculated as follows: x = 7.69 / (7.69 + 14.6) = 34%. Therefore, as also shown in the table, Fig. As is clearly shown in section 7, the amount of platinum in comparative example 1 (the black triangular areas) is insufficient to cover the palladium particle surface with a platinum layer. Furthermore, the coverage calculated from the ICP measurement results is 67%.

[0153] Referring to Table 1, the initial mass activity of the fuel cell catalyst from Comparative Example 1 is 394 (A / g-Pt); the mass activity after the potential cycles is 493 (A / g-Pt); and the rate of change is 25.1%. Also, the initial electrochemical surface area of ​​the fuel cell catalyst from Comparative Example 1 is 202 (m²). 2 / g-Pt); the electrochemical surface area after the potential cycles is 162 (m²) 2 / g-Pt); and the rate of change (decrease rate) is -19.8%. The absolute value of the decrease rate is the highest of the fuel cell catalysts from Example 1, Reference Example 1, and Comparison Examples 1 to 3. Furthermore, with respect to the fuel cell catalyst from Comparison Example 1, the initial specific activity is 1.95 (A / m³). 2 ); the specific activity after the potential cycles is 3.04 (A / m²). 2); and the rate of change is 55.9%.

[0154] Accordingly, with regard to the fuel cell catalyst from Comparative Example 1, which was obtained by forming half of the outermost platinum layer using conventional Cu-UPD, it becomes clear that the state of coverage with the outermost platinum layer was not yet complete even when the catalyst was new. With regard to the fuel cell catalyst from Comparative Example 1, it also becomes clear that the electrochemical surface area is very easily reduced by a preconditioning interim operation.

[0155] Next, comparative example 2 will be discussed. From the ICP measurement results shown in Table 1, it is clear with regard to the fuel cell catalyst from comparative example 2 that the platinum present on the catalyst surface is 13.2% and the palladium present on it is 13.0%. From this result, the platinum fraction x on the palladium particle surface is calculated as follows: x = 13.2 / (13.2 + 13.0) = 50%. Therefore, as shown from Fig. As can be clearly seen in comparison example 2 (the black circles), the amount of platinum is sufficient to almost completely cover the palladium particle surface with a platinum layer. The coverage calculated from the ICP measurement results is also 97%.

[0156] Referring to Table 1, the initial mass activity of the fuel cell catalyst from Comparative Example 2 is 470 (A / g-Pt); the mass activity after the potential cycles is 730 (A / g-Pt); and the rate of change is 55.3%. Also, the initial electrochemical surface area of ​​the fuel cell catalyst from Comparative Example 2 is 124 (m²). 2 / g-Pt); the electrochemical surface area after the potential cycles is 115 (m²). 2 / g-Pt); and the rate of change (decrease rate) is -7.26%. Furthermore, with respect to the fuel cell catalyst from comparative example 2, the initial specific activity is 3.79 (A / m³). 2 ); the specific activity after the potential cycles is 6.35 (A / m²) 2 ); and the rate of change is 67.5%.

[0157] Accordingly, with regard to the fuel cell catalyst from Comparative Example 2, which was obtained by forming the outermost platinum layer until the intrinsic potential reached a plateau with conventional Cu-UPD, it becomes clear that the mass activity of the catalyst in its new state is less than two-thirds of its mass activity after the potential cycles, and that the state of coverage with the outermost platinum layer was far from complete. With regard to the fuel cell catalyst from Comparative Example 2, it also becomes clear that the electrochemical surface area is very easily reduced by a preconditioning interim operation.

[0158] Next, we will discuss comparative example 3. The ICP measurement results shown in Table 1 clearly indicate that, with regard to the fuel cell catalyst from comparative example 3, the platinum content on the catalyst surface is 12.4% and the palladium content is 14.4%. From this result, the platinum content x on the palladium particle surface is calculated as follows: x = 12.4 / (12.4 + 14.4) = 46%. Therefore, the amount of platinum in comparative example 2 is sufficient to almost completely cover the palladium particle surface with a platinum layer. The coverage calculated from the ICP measurement results is also 89%.

[0159] Referring to Table 1, the initial mass activity of the fuel cell catalyst from Comparative Example 3 is 503 (A / g-Pt); the mass activity after the potential cycles is 785 (A / g-Pt); and the rate of change is 56.1%. This rate of change is the highest of the fuel cell catalysts from Example 1, Reference Example 1, and Comparative Examples 1 to 3. Also, the initial electrochemical surface area of ​​the fuel cell catalyst from Comparative Example 3 is 140 (m²). 2 / g-Pt); the electrochemical surface area after the potential cycles is 123 (m²). 2 / g-Pt); and the rate of change (decrease rate) is -12.1%. Furthermore, with respect to the fuel cell catalyst from comparative example 3, the initial specific activity is 3.59 (A / m³). 2 ); the specific activity after the potential cycles is 6.38 (A / m²) 2); and the rate of change is 77.7%.

[0160] Accordingly, with regard to the fuel cell catalyst from Comparative Example 3, which was obtained by forming the outermost platinum layer until the intrinsic potential reached a plateau with conventional Cu-UPD, it becomes clear that the mass activity of the catalyst in its new state is less than two-thirds of its mass activity after the potential cycles, and that the state of coverage with the outermost platinum layer was far from complete. With regard to the fuel cell catalyst from Comparative Example 3, it also becomes clear that the electrochemical surface area is very easily reduced by a preconditioning interim operation.

[0161] A comparison between examples 2 and 3, where the amount of platinum added in example 2 (St=1.2) is greater than in example 3 (St=1.0), reveals that the platinum content on the palladium particle surface is slightly higher in example 2 than in example 3; the rate of change of the mass activity is slightly lower in example 2 than in example 3; and the absolute value of the rate of change (decrease rate) of the electrochemical surface area is lower in example 2 than in example 3.

[0162] However, the ICP measurement results shown in Table 1 for the fuel cell catalyst from Example 1 clearly show that the platinum present on the catalyst surface is 12.1% and the palladium present on it is 14.4%. From these results, the platinum fraction x on the palladium particle surface is calculated as follows: x = 12.1 / (12.1 + 14.4) = 46%. Therefore, the amount of platinum in comparative example 2 is an amount that can almost cover the palladium particle surface with a platinum layer (see Table 1). Fig. 7) The coverage calculated from the ICP measurement results is also 88%.

[0163] Referring to Table 1, the initial mass activity of the fuel cell catalyst from Example 1 is 624 (A / g-Pt); the mass activity after the potential cycles is 629 (A / g-Pt); and the rate of change is 0.801%. This rate of change is the lowest of the fuel cell catalysts from Example 1, Reference Example 1, and Comparison Examples 1 to 3. Also, the initial electrochemical surface area of ​​the fuel cell catalyst from Example 1 is 132 (m²). 2 / g-Pt); the electrochemical surface area after the potential cycles is 123 (m²). 2 / g-Pt); and the rate of change (decrease rate) is -6.82%. The absolute value of the decrease rate is the lowest of the fuel cell catalysts from Example 1, Reference Example 1, and Comparison Examples 1 to 3. Furthermore, with respect to the fuel cell catalyst from Example 1, the initial specific activity is 4.73 (A / m³). 2 ); the specific activity after the potential cycles is 5.11 (A / m²). 2 ); and the rate of change is 8.03%. The initial specific activity of Example 1 is the highest of the fuel cell catalysts from Example 1, Reference Example 1, and Comparison Examples 1 to 3. Likewise, the rate of change of the specific activity of Example 1 is the lowest of the fuel cell catalysts from Example 1, Reference Example 1, and Comparison Examples 1 to 3.

[0164] From the foregoing, with regard to the fuel cell catalyst from Example 1, which was obtained by immersing the palladium particles in the platinum compound solution and then Cu-UPD, it is clear that the outermost platinum layer was already almost complete in the new state of the catalyst, and the catalyst can be used for a catalytic reaction as is, without any preconditioning. It is also clear with regard to the fuel cell catalyst from Example 1 that the electrochemical surface area is not easily reduced and the stability is excellent.

[0165] Next, Reference Example 1 will be discussed. From the ICP measurement results shown in Table 1, it is clear that, with regard to the fuel cell catalyst from Reference Example 1, the platinum content on the catalyst surface is 6.58% and the palladium content is 13.9%. From this result, the platinum content x on the palladium particle surface is calculated as follows: x = 6.58 / (6.58 + 13.9) = 32%. Therefore, as also shown from Fig. As is clearly shown in Figure 7, the amount of platinum in reference example 1 (the white square areas) is insufficient to cover the palladium particle surface with a platinum layer. Furthermore, the coverage calculated from the ICP measurement results is 62%.

[0166] Referring to Table 1, the initial mass activity of the fuel cell catalyst from Reference Example 1 is 525 (A / g-Pt); the mass activity after potential cycles is 654 (A / g-Pt); and the rate of change is 24.6%. Also, the initial electrochemical surface area of ​​the fuel cell catalyst from Reference Example 1 is 219 (m²). 2 / g-Pt); the electrochemical surface area after the potential cycles is 202 (m²) 2 / g-Pt); and the rate of change (decrease rate) is -7.76%. Furthermore, with respect to the fuel cell catalyst from reference example 1, the initial specific activity is 2.40 (A / m³). 2 ); the specific activity after the potential cycles is 3.24 (A / m²). 2 ); and the rate of change is 35.0%.

[0167] The IPC measurement results from reference example 1 will now be discussed further. According to the ICP measurement results of the carbon-supported palladium particles (raw material) from reference example 1, the palladium content on the surface of the catalyst for fuel cells is 15.9%.

[0168] It is assumed that the palladium on the palladium particle surface, corresponding to a palladium layer, is eluted and the platinum is deposited (hereinafter referred to as the "palladium-eluted model"). The number of palladium atoms on the palladium particle surface is calculated for a palladium particle of 4.2 nm. The composition is then calculated when all the palladium atoms on the surface, corresponding to a palladium layer, are substituted by platinum atoms. In this case, the platinum present on the surface of the fuel cell catalyst is 9.47%, and the palladium present is 10.1%. The amount of palladium that constitutes the remainder (excluding the platinum (90.5%)) is as follows: 10.1 / 90.5 = 11.2%.

[0169] In reality, however, as shown in Table 1, the platinum present on the surface of the fuel cell catalyst from Reference Example 1 is 6.58%, and the palladium present on it is 13.9%. In Reference Example 1, the amount of palladium relating to the remainder (excluding the platinum (93.4%)) is as follows: 13.9 / 93.4 = 14.9%. This value is closer to the value relating to the carbon-supported palladium particles (raw material) (15.9%) than the value in the preceding palladium-eluted model (11.2%). That is to say, it becomes clear that in the manufacturing process of Reference Example 1, the amount of palladium contained in the raw material is almost entirely retained.

[0170] Accordingly, it becomes clear that in the process of immersing the palladium particles in the platinum compound solution, no substitution reaction takes place between the palladium and the platinum, and that the platinum is deposited on the palladium surface.

[0171] Next, Reference Example 2 is discussed. The ICP measurement results shown in Table 1 for the fuel cell catalyst in Reference Example 2 clearly show that the platinum content on the palladium particle surface is 6.40% and the palladium content is 13.8%. From this result, the platinum content x on the palladium particle surface is calculated as follows: x = 6.40 / (6.40 + 13.8) = 32%. Therefore, it is clear that the amount of platinum in Reference Example 2 is insufficient to cover the palladium particle surface with a platinum layer. Furthermore, the coverage calculated from the ICP measurement results is 61%.

[0172] According to a comparison of the ICP measurement results of reference examples 1 and 2, there is virtually no difference in the platinum and palladium content on the palladium particle surface, nor in the coverage. This result clearly demonstrates that the method for obtaining palladium particles by immersing them in the platinum compound solution does not result in a significant change in the composition of the palladium particle surface, even when the amount of platinum added is increased from St=1.0 (reference example 2) to St=1.2 (reference example 1); the composition of the palladium particle surface is insensitive to the amount of platinum added; and the amount of platinum that can be directly deposited on the palladium particle surface has already been determined.

[0173] Finally, the results of Reference Example 1 and Comparison Example 1 are compared. According to Table 1, the initial mass activity of Reference Example 1 is 1.3 times higher than that of Comparison Example 1, and the initial specific activity of Reference Example 1 is 1.2 times higher than that of Comparison Example 1. Similarly, after the potential cycles, the mass activity of Reference Example 1 is 1.3 times higher than that of Comparison Example 1, and the specific activity of Reference Example 1 is 1.1 times higher than that of Comparison Example 1. As in Fig.As shown in Figure 7, there is virtually no difference in the platinum content on the palladium particle surface between Comparison Example 1 and Reference Example 1; however, the mass activity and specific activity are higher in Reference Example 1. This fact indicates that Reference Example 1 is superior to Comparison Example 1 in the platinum-coated state, meaning that while in Reference Example 1 the palladium particle surface is covered with the monatomic platinum layer, in Comparison Example 1 two or more platinum atom layers are deposited on the palladium particle surface.

[0174] Furthermore, according to Table 1, the rate of change (decline rate) of the electrochemical surface area in Reference Example 1 is only 39% of the rate of change (decline rate) of the electrochemical surface area in Comparison Example 1. Given that Reference Example 1 and Comparison Example 1 have substantially the same platinum content, this result indicates that the platinum in Reference Example 1 is more widely distributed on the palladium particle surface than in Comparison Example 1, and the portion where the palladium particle surface is exposed is smaller in Reference Example 1 than in Comparison Example 1, thus giving Reference Example 1 greater durability. Reference symbol list 1 Palladium-containing particle 2 platinum atoms 3 copper atoms 3a Copper atoms deposited on edges or corners of the palladium-containing particle surface 3b Copper atoms deposited on terraces of the palladium-containing particle surface 11 Polyelectrolyte membrane 12 Cathode catalyst layer 13 Anode catalyst layer 14, 15 Gas diffusion layer 16 Cathode electrode 17 Anode electrode 18 Membrane electrode arrangement 19, 20 Separator 21, 22 Gas channel 100a Typical example of a first composite body 100b Typical example of a second composite body 100c Typical example of a fine catalyst particle 200 unit cells of a fuel cell 300 composite bodies in which copper atoms are deposited on the surface of a palladium particle

Claims

[1] A method for producing a fine catalyst particle comprising a palladium-containing particle and an outermost platinum layer covering the palladium-containing particle, wherein a first composite body containing palladium and platinum is formed by mixing the palladium-containing particle with a first solution in which a platinum compound is dissolved, and as a result of directly contacting the palladium-containing particle with the first solution, then covering at least a portion of a surface of the palladium-containing particle with platinum; wherein a second composite body containing palladium, platinum and copper is formed by mixing the first composite body with a second solution in which a copper compound is dissolved, and then covering at least a portion of a surface of the first composite body with copper using copper underpotential deposition; wherein the copper in the second composite body is substituted by platinum derived from a third solution in which a platinum compound is dissolved, by mixing the second composite body with the third solution; and wherein an amount of platinum atoms contained in the first solution is 70 at.% or less when a minimum amount of platinum atoms required to cover the palladium-containing particle with a monoatomic platinum layer is 100 at.%. [2] A method for producing the fine catalyst particle according to claim 1, wherein the palladium-containing particle is supported on a carrier. [3] A method for producing the fine catalyst particle according to claim 1 or 2, wherein the palladium-containing particle is subjected to an acid treatment in advance before the first composite body is formed. [4] A fuel cell comprising unit cells each comprising a membrane electrode assembly in which an anode electrode having at least one anode catalyst layer is arranged on one side of a polyelectrolyte membrane and a cathode electrode having at least one cathode catalyst layer is arranged on another side of the polyelectrolyte membrane, wherein a fine catalyst particle produced by the production method defined in any one of claims 1 to 3 is contained in the anode catalyst layer and / or the cathode catalyst layer.

Citation Information

Patent Citations

  • Method of forming a catalyst with an atomic layer of platinum atoms

    WO2012115624A1

  • Platinum monolayer on alloy nanoparticles with high surface area and manufacturing process

    DE112010005260T5

  • FUEL CELL SYSTEM

    DE112010005593T5

  • Method for manufacturing catalyst fine particle

    JP2012192334A

  • Platinum-Coated Non-Noble Metal-Noble Metal Core-Shell Electrocatalysts

    US20100197490A1