Packaging material for energy storage device and energy storage device
The packaging material for energy storage devices, featuring a heat-resistant resin layer bonded with a UV-curable resin composition, addresses the challenge of heat resistance and moldability, ensuring no pinholes or cracks and maintaining adhesion under severe conditions.
Patent Information
- Application Number
- DE112017003136
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-06-24
- Filing Date
- 2017-04-28
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2037-04-28
AI Technical Summary
Existing packaging materials for energy storage devices face challenges in achieving both sufficient heat resistance and excellent moldability without causing pinholes, cracks, or delamination, especially under severe conditions like high temperature and high humidity.
A packaging material comprising a heat-resistant resin layer, a heat-fusable resin layer, and a metal foil layer bonded with an ultraviolet light-curable resin composition containing acrylate resin, silane coupling agent, acid anhydride, and phosphoric acid-containing (meth)acrylate, which ensures strong adhesion and prevents delamination.
The packaging material provides heat resistance, prevents pinholes and cracks during deep forming, and maintains adhesion under severe conditions, with improved production efficiency through rapid curing.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Field of invention
[0001] This invention relates to a packaging material (enclosing material) for an energy storage device, such as a capacitor or a battery, used in a mobile device like a smartphone or tablet computer, and to a battery or capacitor used for storing electricity for a hybrid vehicle, an electric vehicle, a wind energy generation system, a solar energy generation system, and a night-time electricity storage system. It also relates to an energy storage device.
[0002] In the claims and in this description, the term "phosphoric acid-containing (meth)acrylate" means "phosphoric acid-containing acrylate and / or phosphoric acid-containing methacrylate". background
[0003] A lithium-ion secondary battery is widely used as a power source for laptops, video cameras, mobile phones, electric vehicles, and similar devices. Such a lithium-ion secondary battery is configured in which a battery core (containing a positive electrode, a negative electrode, and an electrolyte) is enclosed in a casing. This casing is known to consist of an outer layer of a heat-resistant resin film, an aluminum foil layer, and an inner layer of a thermoplastic resin film, in that order.
[0004] For example, a laminate-type packaging material is known that comprises an inner layer of a resin film, a first adhesive layer, a metal layer, a second adhesive layer, and an outer layer of a resin film. In this packaging material, at least one of the first adhesive layer and the second adhesive layer is formed from an adhesive composition with a resin having an active hydrogen group in a side chain, multifunctional isocyanates, and a polyfunctional amine compound as essential components (see patent document 1).
[0005] A packaging material for a battery housing is also known, wherein a polyamide or polyester film with a thickness of 9 to 50 µm is laminated to at least one side of an aluminum foil, and a film of polypropylene, maleic acid-modified polypropylene, an ethylene acrylate copolymer, or an ionomer resin with a thickness of 9 to 50 µm is laminated to the outermost side, wherein the tensile strength to breakage in four directions (0°, 45°, 90°, and 135°) during the tensile strength test of the polyamide or polyester film is 150 N / mm². 2 or more and the elongation in four directions is 80% or more (see patent document 2). State of the art documents Patent document Patent document 1: Unexamined Japanese patent application publication 2008-287971 Patent document 2: Unexamined Japanese patent application publication 2000-123800 Summary of the invention Problems to be solved by the invention
[0006] However, with the techniques described in patent documents 1 and 2 above, it was impossible to achieve both sufficient heat resistance and excellent formability required as packaging material.
[0007] In the packaging material according to patent document 1, delamination (peeling) can occur between the metal foil layer and the outer resin layer when deep forming is carried out, and delamination can occur between the metal foil layer and the outer resin layer when the packaging material is used under harsh environments such as high temperature and high humidity.
[0008] In the packaging material according to patent document 2, there is a problem that when deep forming is carried out, stress is concentrated locally on the metal foil, so that fine holes and / or cracks may occur.
[0009] This invention was carried out with regard to the aforementioned technical background and is intended to provide a packaging material for an energy storage device that exhibits heat resistance and is capable of ensuring excellent formability without causing fine holes and / or cracks, even when deep forming is performed, and that is also capable of sufficiently preventing delamination (peeling), even when deep forming is performed, or even when used under harsh conditions such as high temperature and high humidity. This invention also aims to provide a packaging housing for an energy storage device. This invention also provides an energy storage device that is equipped with the packaging material and / or packaging housing described above. Means of solving the problems
[0010] To achieve the above-mentioned goal, this invention provides the following means: [1] Packaging material for an energy storage device, containing: a heat-resistant resin layer that serves as an outer layer, a heat-fusing resin layer that serves as an inner layer, and a metal foil layer that is positioned between the two layers, wherein the heat-resistant resin layer consists of a heat-resistant resin film with a hot water shrinkage percentage of 1.5 to 12%, wherein the heat-resistant resin layer and the metal foil layer are joined via an outer adhesive layer composed of a hardened film of an ultraviolet light-curable resin composition, wherein the ultraviolet light-curable resin composition comprises an acrylate resin, a photo-radical polymerization initiator, a silane coupling agent, acid anhydride, phosphoric acid-containing (meth)acrylate, one or more resins selected from the group consisting of an epoxy resin, an oxetane resin and a vinyl ether resin, and a photo-cationic polymerization initiator and wherein the ultraviolet light-curable resin composition contains an acrylate resin content of 70 to 98 wt%, a silane coupling agent content of 0.1 to 5 wt%, an acid anhydride content of 0.1 to 5 wt%, a phosphoric acid-containing (meth)acrylate content of 0.1 to 10 wt%, a photo-radical polymerization initiator content of 0.1 to 5 wt%, a content of one or more resins selected from the group consisting of an epoxy resin, oxetane resin and vinyl ether resin, 1 to 20 wt% and a photo-cationic polymerization initiator content of 0.5 to 5 wt%. [2] Packaging material for an energy storage device according to [1], wherein a Young module of the hardened film is 90 to 400 MPa. [3] Packaging material for an energy storage device according to [1] or [2], wherein a slightly adhesive layer is arranged between the heat-resistant resin layer and the outer adhesive layer. [4] Packaging housing for an energy storage device, wherein the packaging housing is produced from a molded product of the packaging material according to one of [1] to [3]. [5] Energy storage device, comprising: an energy storage device main body and a packaging part consisting of the packaging material according to [1] to [3] and / or the packaging housing according to [4], in which the energy storage device main body is packed with the packaging part. [6] Method for producing a packaging material for an energy storage device, the method comprising: a step towards the production of a first laminate in which a heat-resistant resin film with a hot water shrinkage percentage of 1.5 to 12% is bonded to a surface of a metal foil layer via an ultraviolet light-curable resin composition, a step towards shining an ultraviolet light onto the first laminate from the side of the heat-resistant resin film, a step in the manufacture of a second laminate, in which a heat-fusing resin film is bonded to the other surface of the metal foil layer of the first laminate after exposure to ultraviolet light via a thermosetting adhesive, and a step towards performing a heat treatment on the second laminate, wherein the ultraviolet light-curable resin composition comprises an acrylate resin, a photo-radical polymerization initiator, a silane coupling agent, acid anhydride, phosphoric acid-containing (meth)acrylate, one or more resins selected from the group consisting of an epoxy resin, an oxetane resin and a vinyl ether resin, and a photo-cationic polymerization initiator and wherein the ultraviolet light-curable resin composition contains an acrylate resin content of 70 to 98 wt%, a silane coupling agent content of 0.1 to 5 wt%, an acid anhydride content of 0.1 to 5 wt%, a phosphoric acid-containing (meth)acrylate content of 0.1 to 10 wt%, a photo-radical polymerization initiator content of 0.1 to 5 wt%, a content of one or more resins selected from the group consisting of an epoxy resin, oxetane resin and vinyl ether resin, 1 to 20 wt% and a photo-cationic polymerization initiator content of 0.5 to 5 wt%. Effects of the invention
[0011] In the invention according to aspect 1 above, the heat-resistant resin layer is composed of a heat-resistant resin film with a hot water shrinkage percentage of 1.5 to 12%, and the heat-resistant resin layer and the metal foil layer are bonded via an outer adhesive layer composed of a cured film of an ultraviolet-curable resin composition. Therefore, the packaging material for an energy storage device has heat resistance and can ensure excellent formability without causing fine holes and / or cracks, even when deep forming is performed by cold forming (at normal temperature), such as deep forming and stretch forming.Even when deep forming is performed or the material is used in harsh environments, such as high temperature and high humidity, delamination (peeling) between the outer layer (heat-resistant resin layer) and the metal foil layer can be sufficiently prevented. Because ultraviolet light curing (like light curing) of the ultraviolet light-curable resin composition can be carried out in a shorter time compared to curing a thermosetting resin, which requires several days for heat aging, there is also the advantage that the lead time (the time required from material input to product completion) can be drastically reduced. In the invention according to the above aspect [1], the ultraviolet light-curable resin composition comprises an acrylate resin and a photoradical polymerization initiator.Therefore, the time for ultraviolet light curing can be further reduced, which in turn can further shorten the throughput time.
[0012] According to the invention as described above [1], it is possible to sufficiently prevent the occurrence of delamination between the outer layer and the metal foil layer.
[0013] According to the invention as described above [2], because the Young's modulus of the hardened film is 90 to 400 MPa, it is possible to sufficiently prevent delamination between the outer layer and the metal foil layer and also to improve the lamination strength under high temperature environments.
[0014] In the invention according to the above aspect [3], because a slightly adhesive layer is provided between the heat-resistant resin layer and the outer adhesive layer, even when used under harsh conditions such as high temperature and high humidity, delamination between the outer layer and the metal foil layer can be prevented more satisfactorily.
[0015] In the invention according to the aspect above [4], a well-shaped packaging housing can be provided. In this packaging housing, even when used under harsh conditions such as high temperature and high humidity, delamination between the outer layer and the metal foil layer can be prevented more satisfactorily, and productivity is excellent.
[0016] In the invention according to the above aspect [5] it is possible to specify an energy storage device which is packed with a packaging part which can sufficiently prevent delamination, even when deep forming is carried out or when it is used under harsh environments, such as high temperature and high humidity.
[0017] In the invention according to point [6] above, it is possible to provide a heat-resistant packaging material for an energy storage device that is capable of ensuring excellent formability without causing fine holes and / or cracks, even when deep forming is performed, and is also capable of sufficiently preventing delamination between the outer layer and the metal foil layer, even when used under harsh conditions such as high temperature and high humidity, or even when deep forming is performed. Because the curing of the outer adhesive (ultraviolet-curable resin composition) is carried out by ultraviolet light radiation, production efficiency can be considerably improved. Brief description of the drawings Fig.Figure 1 is a cross-sectional view showing an embodiment of a packaging material for an energy storage device of this invention. Fig. Figure 2 is a cross-sectional view showing another embodiment of a packaging material for an energy storage device of this invention. Fig. Figure 3 is a cross-sectional view showing an embodiment of a packaging material for an energy storage device of this invention. Fig. Figure 4 is a perspective view showing a packaging material (planar form), an energy storage device main body, and a packaging housing (three-dimensionally shaped product) that emerges from the energy storage device of Fig. 3 assembled in the extended state before thermal sealing. Exemplary embodiment for carrying out the invention
[0018] An embodiment of a packaging material for an energy storage device of this invention is shown in Fig. 1 shown. This packaging material 1 is shown as packaging material for a battery, such as a lithium-ion secondary battery. The packaging material 1 can be used as is, without any shaping (see Fig. 4) or as a shaped housing 10 by carrying out a shaping process such as deep forming and stretch forming (see Fig. 4) can be used.
[0019] The packaging material 1 for an energy storage device is configured such that a heat-resistant resin layer (outer layer) 2 is integrally laminated onto one surface (top surface) of a metal foil layer 4 over an outer adhesive layer (first adhesive layer) 5, and a heat-fusing resin layer (inner layer 3) is integrally laminated onto the other surface (bottom surface) of the metal foil layer 4 over an inner adhesive layer (second adhesive layer) 6.
[0020] Another embodiment of a packaging material for an energy storage device of this invention is shown in Fig.Figure 2 shows this packaging material for an energy storage device. It is configured such that a heat-resistant resin layer (outer layer) 2 is integrally laminated onto one surface (top surface) of a metal foil layer 4 over an outer adhesive layer (first adhesive layer) 5, and a heat-resistant resin layer (inner layer) 3 is integrally laminated onto the other surface (bottom surface) of the metal foil layer 4 over an inner adhesive layer (second adhesive layer) 6. Furthermore, a lightly adhesive layer 8 is laminated onto the bottom surface of the heat-resistant resin layer (outer layer) 2, and the outer resin layer (first adhesive layer) 5 is laminated onto the bottom surface of the lightly adhesive layer 8.This means it has a laminated structure of the heat-resistant resin layer (outer layer) 2 / slightly adhesive layer 8 / outer adhesive layer 5 / metal foil layer 4 / inner adhesive layer 6 / heat-fusing resin layer (inner layer) 3 (see . Fig. 2) In this embodiment, the slightly adhesive layer 8 is laminated onto the lower surface of the heat-resistant resin layer 2 by an engraving coating process.
[0021] According to the invention, the outer layer 2 is formed from a heat-resistant resin layer. The heat-resistant resin constituting the heat-resistant resin layer 2 is a heat-resistant resin that does not melt at the heat-sealing temperature when the packaging material is heat-sealed. Preferably, the heat-resistant resin should have a melting point 10°C or more higher than the melting point of the heat-melting resin that constitutes the heat-melting resin layer 3. In particular, it is preferred to use a heat-resistant resin with a melting point 20°C or more higher than the melting point of the heat-melting resin.
[0022] The heat-resistant resin layer (outer layer) 2 is a part that mainly plays a role in ensuring good formability as packaging material 1, that is, it mainly plays a role in preventing breakage due to the necking of the aluminum foil at the time of forming.
[0023] According to the invention, the heat-resistant resin layer 2 must consist of a heat-resistant film with a hot water shrinkage percentage of 1.5 to 12%. If the hot water shrinkage percentage is less than 1.5%, a problem arises in that breakage and / or cracking can easily occur during molding. On the other hand, if the hot water shrinkage percentage exceeds 12%, delamination (peeling) between the outer layer 2 and the metal foil layer 4 can occur. In particular, it is preferred to use a heat-resistant resin film with a hot water shrinkage percentage of 1.8 to 11% as the heat-resistant resin film. Furthermore, it is more preferred to use a heat-resistant resin film with a hot water shrinkage percentage of 1.8 to 6%. A stretched heat-resistant resin film is preferably used as the heat-resistant resin film.
[0024] The hot water shrinkage percentage is a dimensional rate of change of a test piece (10 cm x 10 cm) of a fair heat-resistant resin film 2 in the stretching direction before and after immersion of the test piece in 95°C hot water for 30 minutes and can be obtained by the following equation. Hot water shrinkage percentage (%) = {(X−Y) / X} × 100 wherein X: Dimension in the stretching direction before immersion treatment, and Y: Dimension in the stretching direction after immersion treatment.
[0025] The hot water shrinkage percentage when using a biaxially stretched film is an average value of the dimensional change rate in the two stretching directions.
[0026] The hot water shrinkage percentage of the heat-resistant resin film can be controlled, for example, by adjusting the heating temperature at the time of stretching.
[0027] The heat-resistant resin layer (outer layer) 2 is not particularly limited, and examples include a stretched polyamide film such as a stretched nylon film, a stretched polyester film, and the like. Among these, it is particularly preferred to use as the heat-resistant resin layer 2 a biaxially stretched polyamide film, a biaxially stretched polybutylene terephthalate (PBT) film, a biaxially stretched polyethylene terephthalate (PET) film, or a biaxially stretched polyethylene naphthalate (PEN) film such as a biaxially stretched nylon film, each having a hot water shrinkage percentage of 1.5 to 12%. Furthermore, it is preferred to use as the heat-resistant resin stretched film 2 a biaxially stretched heat-resistant resin film that has been stretched by a simultaneous biaxial stretching process. The nylon film is not particularly limited, but is illustrated by a nylon 6 film, a nylon 6.6 film, an MXD nylon film and the like.The heat-resistant resin layer 2 can be produced from a single layer (single stretched film) or from multiple layers (e.g. multiple layers composed of a stretched PET film / stretched nylon film) which are produced, for example, from a stretched polyester film / stretched polyamide film.
[0028] The thickness of the heat-resistant resin layer 2 is preferably 12 to 50 µm. By adjusting the thickness to a value equal to or greater than the preferred lower limit mentioned above, sufficient strength as a packaging material can be ensured. By adjusting the thickness to a value equal to or less than the preferred upper limit mentioned above, the stress at the time of stretching or drawing can be reduced, thereby improving formability.
[0029] A slightly adhesive layer 8 is preferably laminated onto the inner surface (surface on the side of the metal foil layer 4) of the heat-resistant resin layer 2. By coating the inner surface (surface on the side of the metal foil layer 4) of the heat-resistant resin layer 2 with a polar resin or the like, in order to laminate a slightly adhesive layer 8 onto it, it is possible to improve the adhesive and bonding properties of the outer adhesive layer 5. This allows the adhesive and bonding properties between the heat-resistant resin layer 2 and the metal foil layer 4 to be improved.It is preferred that the inner surface of the heat-resistant resin layer 2 (the surface on which the slightly adhesive layer 8 is laminated) is subjected to corona treatment or the like prior to laminating the slightly adhesive layer 8 in order to improve wettability.
[0030] The method for forming the slightly adhesive layer 8 is not particularly limited, but, for example, the slightly adhesive layer 8 can be formed by applying an aqueous emulsion (water-based emulsion) of one or two types of resins, selected from the group consisting of an epoxy resin, urethane resin, acrylic ester resin, methacrylic ester resin, and polyethyleneimine resin, to the surface of the heat-resistant resin film 2 and allowing the emulsion to dry. The coating method is not particularly limited, and, for example, a spray coating method, a roller coating method, a reverse roller coating method, and a lip coating method can be illustrated.
[0031] Thus, the slightly adhesive layer 8 is preferably configured to contain one or more resins selected from the group consisting of an epoxy resin, urethane resin, acrylic ester resin, methacrylic ester resin, and polyethyleneimine resin. By applying such a configuration, the adhesive strength between the heat-resistant resin layer 2 and the outer adhesive layer 5 can be further improved. If the packaging material is subjected to forming processes such as deep forming and stretch forming, and if the packaging material is heat-sealed, it is possible to adequately prevent delamination (peeling) between the outer layer (heat-resistant resin layer) 2 and the metal foil layer 4.Even when the packaging material 1 is used under strict conditions such as high temperature and high humidity, it is possible to prevent delamination (peeling) between the outer layer (heat-resistant resin layer) 2 and the metal foil layer 4.
[0032] Among these, it is particularly preferred that the slightly adhesive layer 8 contains a urethane resin and an epoxy resin, or a (meth)acrylic acid ester resin and an epoxy resin. In this case, it is possible to more adequately suppress the occurrence of delamination between the outer layer (heat-resistant resin layer) 2 and the metal foil layer 4.
[0033] When using the first-mentioned configuration, the mass ratio of the urethane resin to the epoxy resin in the slightly adhesive layer 8 is preferably in the range of 98 / 2 to 40 / 60. In this case, the adhesive strength between the heat-resistant resin layer 2 and the outer adhesive layer 5 can be further improved. If the urethane resin ratio is greater than the mass ratio (98 / 2) of the urethane resin to the epoxy resin, the degree of crosslinking becomes insufficient, leading to inadequate solvent resistance and adhesive strength, which is not preferred. Conversely, if the urethane resin ratio is less than the mass ratio (40 / 60) of the urethane resin to the epoxy resin, it takes too long to complete the crosslinking, which is not preferred. Among these, the mass ratio of the urethane resin / epoxy resin in the light adhesive layer 8 is preferably in the range of 90 / 10 to 50 / 50.
[0034] When using the latter configuration, the mass ratio of the (meth)acrylic ester resin to the epoxy resin in the slightly adhesive layer 8 is preferably in the range of 98 / 2 to 40 / 60. In this case, the adhesive strength between the heat-resistant resin layer 2 and the outer adhesive layer 5 can be further improved. If the ratio of (meth)acrylic ester resin is greater than the (98 / 2) ratio of (meth)acrylic ester resin to epoxy resin, the degree of crosslinking becomes insufficient, leading to inadequate solvent resistance and adhesive strength, which is not preferred. Conversely, if the ratio of (meth)acrylic ester resin is less than the (40 / 60) mass ratio of (meth)acrylic ester resin to epoxy resin, the crosslinking takes too long to complete, which is not preferred.Among other things, the mass ratio of the (meth)acrylic acid ester resin / epoxy resin in the slightly adhesive layer 8 is preferably in the range of 90 / 10 to 50 / 50.
[0035] A surfactant, such as glycols and ethylene oxide adducts of glycol, can be added to the aqueous resin emulsion (resin-water-based emulsion) to form the lightly adhesive layer 8. In this case, sufficient defoaming effect can be achieved in the aqueous resin emulsion, allowing the formation of the lightly adhesive layer 8 with excellent surface smoothness. It is preferred that 0.01 to 2.0 wt% of the surfactant is present in the aqueous resin emulsion.
[0036] The aqueous resin emulsion (resin-aqueous emulsion) for forming the slightly adhesive layer 8 preferably contains fine inorganic particles such as silica and colloidal silica. In this case, an anti-blocking effect can be obtained. The fine inorganic particles are preferably added in an amount of 0.1 to 10 parts by mass relative to the resin content of 100 parts by mass.
[0037] The amount formed of the slightly adhesive layer 8 (solid content after drying) is preferably in the range of 0.01 to 0.5 g / m². 2 If they are 0.01 g / m³ 2 or more, the heat-resistant resin layer 2 and the outer adhesive layer 5 can be sufficiently bonded together, and if they are 0.5 g / m² 2 If the cost is lower or lower, a cost reduction can be implemented, which is economical.
[0038] The resin content in the slightly adhesive layer (after drying) 8 is preferably 88 to 99.9 wt%.
[0039] According to the invention, the outer adhesive layer (first adhesive layer) 5 is formed from an adhesive which consists of a hardened film of an ultraviolet light-curable resin composition.
[0040] The ultraviolet light-curable composition contains an acrylate resin and a photoradical polymerization initiator. In this case, the ultraviolet light curing time can be further reduced, which in turn can further shorten the throughput time.
[0041] The choice of acrylate resin is not particularly limited, but it is preferred, for example, to use at least one resin selected from the group consisting of a urethane acrylate resin, an epoxy acrylate resin and a polyester acrylate resin.
[0042] The photo-radical polymerization initiator is not particularly limited, but examples include benzophenone, benzoin alkyl ethers (benzoyl ethers, benzobutyl ethers, etc.), benzyldimethyl ketal, and the like.
[0043] The ultraviolet light-curable composition further contains a silane coupling agent, an acid anhydride and a phosphoric acid-containing (meth)acrylate in addition to the acrylate resin and the photo-radical polymerization initiator.
[0044] The silane coupling agent is not particularly limited, but examples include methyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, allyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, and the like. Among these, a silane coupling agent with a carbon-carbon double bond, such as vinyltriethoxysilane and allyltrimethoxysilane, is preferred. In this case, it is possible to strengthen the bond with the adhesive, particularly by utilizing the radical polymerization reaction (the adhesive strength of the outer adhesive layer 5 can be improved).
[0045] The acid anhydride is not particularly limited, and examples include maleic anhydride, methyl maleic anhydride, itaconic anhydride, himic anhydride, methylhiminic anhydride, and the like. Among these, an acid anhydride with a carbon-carbon double bond, such as maleic anhydride, is preferred, and the radical polymerization reaction can be further promoted by the acid anhydride with such a double bond.
[0046] The phosphoric acid-containing (meth)acrylate (monomer) is not particularly restricted, but examples include monomers such as acryloyloxyethyl acid phosphate and bis(2-(meth)acryloyloxyethyl) acid phosphate.
[0047] The ultraviolet light-curable resin composition further contains one or more resins selected from the group consisting of an epoxy resin, an oxyethane resin, and a vinyl ether resin. Using a composition with such a resin can adequately prevent delamination.
[0048] Additionally, a photocationic polymerization initiator is included. The simultaneous presence of a photocationic polymerization initiator adequately prevents delamination. The photocationic polymerization initiator is not particularly limited; for example, an onium salt can be used. The onium salt is not particularly limited, and examples include a sulfonium salt, iodonium salt, bromonium salt, diazonium salt, chloronium salt, and the like.
[0049] The sulfonium salt is not particularly restricted, but examples include triphenylsulfonium hexafluorophosphate, triphenylsulfonium hexafluoroantimonate, triphenylsulfonium tetrakis(pentafluorophenyl)borate, 4,4'-bis[diphenylsulfonio]diphenylsulfide bishexafluorophosphate, 4,4'-bis[di(β-hydroxyethoxy)phenylsulfonio]diphenylsulfide bishexafluoroantimonate, 4,4'-bis[di(β-hydroxyethoxy)phenylsulfonio]diphenylsulfide bishexafluorophosphate, 7-[di(p-toluyl)sulfonio]-2-isopropylthioxanthone hexafluoroantimonate, 7-[di(p-toluyl)sulfonio]-2-isopropylthioxanthone tetrakis-(pentafluorophenyl)borate, and 4-phenylcarbonyl-4'-diphenylsulfonio-diphenylsulfide hexafluorophosphate. 4-(p-ter-butylphenylcarbonyl)-4'-diphenylsulfonio-diphenyl sulfide hexafluoroantimonate, 4-(p-ter-butylphenylcarbonyl)-4'-di(p-toluyl)sulfonio-diphenyl sulfide tetrakis (pentafluorophenyl) borate, triphenylsulfonium bromide and the like.
[0050] The iodonium salt is not particularly restricted, but examples include diphenyliodonium tetrakis-(pentafluorophenyl)borate, diphenyliodonium hexafluorophosphate, diphenyliodonium hexafluoroantimonate, di(4-nonylphenyl)iodonium hexafluorophosphate and the like.
[0051] The ultraviolet light-curable resin composition contains: a) Acrylic resin, b) photo-radical polymerization initiator, c) Acid anhydride, d) Silane coupling agents e) Phosphoric acid-containing (meth)acrylate, f) one or more resins selected from the group consisting of an epoxy resin, an oxytan resin and a vinyl ether resin and g) Photocationic polymerization initiator.
[0052] In this ultraviolet light-curable resin composition, the content of the acrylate resin is 70 to 98 wt%, the content of the silane coupling agent is 0.1 to 5 wt%, the content of the acid anhydride is 0.1 to 5 wt%, the content of the phosphoric acid-containing (meth)acrylate is 0.1 to 10 wt%, the content of the photo-radical polymerization initiator is 0.1 to 5 wt%, the content of one or more resins selected from the group consisting of an epoxy resin, oxetane resin and vinyl ether resin is 1 to 20 wt% and the content of the photo-cationic polymerization initiator is 0.5 to 5 wt%.
[0053] It is preferred that the thickness (thickness after drying) of the outer adhesive layer (first adhesive layer) is adjusted to 1 to 6 µm.
[0054] The Young's modulus of the cured film of the ultraviolet-curable composition constituting the outer adhesive layer 5 is preferably in the range of 90 to 400 MPa. If the Young's modulus is 90 MPa or higher, it is possible to improve the thermal resistance of the outer adhesive layer 5 and also to sufficiently prevent delamination (peeling) between the outer layer 2 and the metal foil layer 4, even when deep forming is performed. If the Young's modulus is 400 MPa or lower, the adhesive strength of the cured film can be sufficiently improved, and the lamination strength under high-temperature environments can be sufficiently improved. In particular, the Young's modulus of the cured film of the ultraviolet-curable resin composition constituting the outer adhesive layer 5 is especially preferably in the range of 140 to 300 MPa.The Young module is a Young module, measured according to JIS K7127-1999.
[0055] According to the invention, the metal foil layer 4 plays a role in providing a gas barrier property that prevents the invasion of oxygen and moisture into the packaging material 1. The metal foil layer 4 is not particularly limited, but examples include aluminum foil and copper foil, and aluminum foil is generally used. The thickness of the metal foil layer 4 is preferably 9 to 120 µm. If the thickness is 9 µm or more, it is possible to prevent the formation of fine holes during the rolling process when producing a metal foil, and if the thickness is 120 µm or less, it is possible to reduce the stress during forming processes such as stretching and drawing, thereby improving formability. In particular, the thickness of the metal foil layer 4 is especially preferably 20 to 100 µm.
[0056] It is preferred that the metal foil layer 4 be subjected to a chemical conversion treatment, at least on its inner surface (the surface adjacent to the inner adhesive layer 6). Because such a chemical conversion treatment is carried out, corrosion of the metal foil surface due to its contents (electrolyte, etc., of a battery) can be sufficiently prevented. For example, a chemical conversion treatment is performed on the metal foil by carrying out the following procedure. That is, for example, on the surface of a metal foil that has undergone a degreasing treatment, after application of the aqueous solution according to one of 1) to 3) as described below, it is dried and subjected to a chemical conversion treatment. 1) Aqueous solution of a mixture containing: a phosphoric acid a chromic acid and at least one compound selected from the group consisting of a metal salt of a fluoride and a non-metal salt of a fluoride. 2) Aqueous solution of a mixture containing: a phosphoric acid at least one resin selected from the group consisting of an acrylic-based resin, a chitosan derivative resin, and a phenol-based resin; and at least one compound selected from the group consisting of a chromic acid and a chromium(III) salt. 3) Aqueous solution from a mixture containing: a phosphoric acid at least one resin selected from the group consisting of an acrylic-based resin, a chitosan derivative resin and a phenol-based resin; at least one compound selected from the group consisting of a chromic acid and a chromium(III) salt; and at least one compound selected from the group consisting of a metal salt of a fluoride and a non-metal salt of a fluoride.
[0057] The chemical conversion coating is preferably 0.1 to 50 mg / m² 2 as chromium adhesion quantity (per side), in particular preferably 2 to 20 mg / m² 2 .
[0058] The heat-melting resin layer (inner layer) 3 plays a role in that it exhibits excellent chemical resistance even against a highly corrosive electrolyte used in a lithium-ion secondary battery, and the like, and also provides a heat-sealing property to the packaging material.
[0059] The resin constituting the heat-fusing resin layer 3 is not particularly limited, but examples include polyethylene, polypropylene, ionomer, ethylene ethyl acrylate (EEA), ethylene methacrylate (EAA), ethylene methyl methacrylate resin (EMMA), ethylene vinyl acetate copolymer resin (EVA), maleic anhydride-modified polypropylene, maleic anhydride-modified polyethylene, and the like.
[0060] The thickness of the heat-fusing resin layer 3 is preferably set to 15 to 30 µm. Setting the thickness to 15 µm or more ensures sufficient heat-sealing strength, while setting the thickness to 30 µm or less contributes to thinning and weight reduction. The heat-fusing resin layer 3 is preferably formed from an unstretched film layer of a heat-fusing resin, and the heat-fusing resin layer 3 can be a single layer or multiple layers.
[0061] The inner adhesive layer (second adhesive layer) 6 is not particularly restricted, but it is preferred to use, for example, a heat-curing type adhesive. Examples of heat-curing type adhesives include a heat-curing acrylic adhesive, an acid-modified polypropylene heat-curing adhesive, a heat-curing polyurethane-based adhesive, and the like. Among these, a heat-curing acrylic adhesive is preferred. In this case, there is an advantage that the heat-aging processing temperature for curing can be lowered (for example, to 40°C), and it is possible to obtain a beneficial effect, sufficiently preventing the formation of white powder in the heat-fusing resin layer 3 during heat-aging processing. The thickness (thickness after drying) of the inner adhesive layer 6 is preferably 1 to 4 µm.
[0062] By shaping (deep forming, stretching, etc.) the packaging material 1 for an energy storage device of this invention, a packaging housing 10 for an energy storage device can be obtained (see Fig. 4) The packaging material 1 of this invention can be used as is, without any shaping (see Fig. 4).
[0063] Fig. Figure 3 shows an embodiment of an energy storage device 30 configured using the packaging material 1 of this invention. This energy storage device 30 is a lithium-ion secondary battery. In this embodiment, as shown in the Fig. 3 and Fig.Figure 4 shows a packaging part 15 constituted by a housing 10, obtained by shaping the packaging material 1 and a planar packaging material 1 with which no shaping is carried out. The energy storage device 30 of this invention is constituted (see Figure 4). Fig. 3 and Fig.4) by accommodating a substantially rectangular parallelepiped energy storage device main body (electrochemical element or the like) 31 in a housing recess of a packaging housing 10, obtained by shaping the packaging material 1 of this invention, arranging a packaging material 1 of this invention on the energy storage device main body 31 without shaping, whereby the side of the inner layer 3 faces inwards (bottom side), and thermally sealing the peripheral area of the inner layer 3 of the planar packaging material 1 and the inner layer 3 of the flange area (peripheral sealing area) 29 of the packaging housing 10, which is to be thermally sealed. The inner side surface of the housing recess of the packaging housing 10 is an inner layer (heat-fusing layer) 3, and the outer surface of the housing recess is an outer layer (heat-resistant layer) 2 (see Fig. 4).
[0064] In Fig. Reference numeral 39 denotes a heat-sealing area in which the peripheral area of the packaging material 1 and the flange area (peripheral sealing area) 29 of the packaging housing 10 are connected (fused). In the energy storage device 30, an end section of a tab line, which is connected to the energy storage device main body area 31, is brought outwards from the packaging part 15, but the explanation is omitted.
[0065] Although the energy storage device main body 31 is not particularly restricted, it is illustrated, for example, by a battery main body, a capacitor main body, and an electrical capacitor main body.
[0066] It is preferred that the width of the thermal sealing area 39 is set to 0.5 mm or more. If it is set to 0.5 mm or more, sealing can be carried out reliably. In particular, it is preferred that the width of the thermal sealing area 39 is set to 3 to 15 mm.
[0067] In the embodiment described above, the packaging part 15 is configured by the packaging housing 10, which is obtained by shaping the packaging material 1 and the planar packaging material 1 (see Fig. 3 and Fig. 4) However, this invention is not particularly limited to such a combination. For example, the packaging part 1 can be constituted by a pair of packaging materials 1 or a pair of packaging housings 10.
[0068] A preferred example of a method for producing a packaging material for an energy storage device according to this invention is described below. First, a first laminate is produced in which a heat-resistant resin film 2 with a hot water shrinkage percentage of 1.5 to 12% is bonded to a surface of a metal foil layer 4 via the ultraviolet-curable resin composition (first manufacturing step).
[0069] Then, ultraviolet light is shone onto the first laminate from the side of the heat-resistant resin film to cure the ultraviolet-curable composition (curing step). The amount of ultraviolet light applied is not particularly limited, but is preferably set at 50 to 1000 mJ / cm². 2 set.
[0070] Then, a second laminate is produced in which a thermosetting resin film 3 is bonded to the other surface of the metal foil layer 4 of the first laminate, which has undergone curing via a thermosetting adhesive (second manufacturing step). The thermosetting adhesive is not particularly limited, and examples include a thermosetting acrylic resin, a thermosetting polypropylene adhesive, a thermosetting polyurethane adhesive, and the like. A heat treatment is then performed on the second laminate to cure the thermosetting adhesive (aging treatment step). The packaging material 1 for an energy storage device of this invention can be obtained through the aging treatment step. The heat treatment is preferably carried out at 35 to 40°C.Although the time of heat treatment (heat aging processing) is not particularly limited, for example when using a thermosetting acrylic adhesive as the heat-curing adhesive, the heat treatment is preferably 3 to 15 days.
[0071] The production process described above is merely an example, and the packaging material 1 for an energy storage device of this invention is not limited to the one produced by the production process described above. Examples
[0072] Specific examples of this invention are described below, but this invention is not particularly limited to these examples. <Referenzbeispiel 1>
[0073] A chemical conversion coating was formed by applying a chemical conversion treatment solution containing phosphoric acid, polyacrylic acid (acrylic-based resin), a chromium(III) salt compound, water, and alcohol to both sides of a 35 µm thick aluminum foil (aluminum foil A8079, specified in JIS H4160) and subsequently drying at 180°C. The chromium adhesion of this chemical conversion coating was 10 mg / m². 2 per page.
[0074] Then a light-curing resin composition (external adhesive) with 95 wt% of a urethane acrylate resin with two acryloyl groups, 5 wt% of a benzophenone was applied to a surface of the aluminum conversion-treated aluminum foil 4, so that the mass after drying was 4 g / m² 2 became.
[0075] On the other side, a biaxially stretched polyamide film 2 with a slightly adhesive layer 8 was obtained by applying a resin. This resin was obtained by mixing 70 parts by mass of a urethane resin and 30 parts by mass of an epoxy resin onto one side of a biaxially stretched polyamide film 2 with a hot water shrinkage percentage of 2.0% and a thickness of 15 µm by a spray coating process. The film was then dried, forming a slightly adhesive layer 8 with a thickness of 0.05 µm. The biaxially stretched polyamide film 2 with the hot water shrinkage percentage of 2.0% was obtained by setting the heat saturation temperature to 214°C during the biaxial stretching of the polyamide film.
[0076] The slightly adhesive layer side of the polyamide film 2 with the slightly adhesive layer 8 was placed onto the outer adhesive-coated side of one side of the aluminum foil 4 and laminated, resulting in a first laminate. Ultraviolet rays with 300 mJ / m 2 were irradiated onto the first laminate from the polyamide film 2 side, to light-cure the light-curing resin coating, to form a hardened film (outer adhesive layer 5).
[0077] Then an internal adhesive, consisting of an acid-modified, heat-curing polypropylene adhesive, was applied to the other surface of the aluminum foil 4 of the first laminate, so that the mass after drying was 2.5 g / m². 2 was, and then an unstretched polypropylene film 3 with a thickness of 30 µm was laminated onto the side coated with the inner agent, obtaining a second laminate.
[0078] The second laminate was subjected to heat aging by being placed in an environment of 40°C for 9 days to harden the internal heat-curing adhesive, forming an internal adhesive layer 6, while retaining a packaging material 1 for an energy storage device. <Referenzbeispiel 2>
[0079] A packaging material 1 for an energy storage device 1 with the configuration according to Fig. Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 90 parts by mass of a urethane acrylate resin having two acryloyl groups, 0.2 parts by mass of benzophenone, 5 parts by mass of maleic anhydride and 5 parts by mass of methyltrimethoxysilane was used as the light-curing resin composition (external adhesive). <Referenzbeispiel 3>
[0080] A packaging material 1 for an energy storage device 1 with the configuration according to Fig. Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 94 parts by mass of a urethane acrylate resin having two acryloyl groups, 5 parts by mass of benzophenone, 0.2 parts by mass of maleic anhydride and 0.2 parts by mass of methyltrimethoxysilane was used as the light-curing resin composition (external adhesive). <Referenzbeispiel 4>
[0081] A packaging material 1 for an energy storage device 1 with the configuration according to Fig.Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 91 parts by mass of a urethane acrylate resin having two acryloyl groups, 3 parts by mass of benzophenone, 3 parts by mass of maleic anhydride and 3 parts by mass of methyltrimethoxysilane and 0.3 parts by mass of acryloyloxyethyl acid phosphate was used as the light-curing resin composition (external adhesive). <Referenzbeispiel 5>
[0082] A packaging material 1 for an energy storage device 1 with the configuration according to Fig.Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 90 parts by mass of a urethane acrylate resin having two acryloyl groups, 0.2 parts by mass of benzophenone, 0.2 parts by mass of maleic anhydride, 0.2 parts by mass of methyltrimethoxysilane and 10 parts by mass of acryloyloxyethyl acid phosphate was used as the light-curing resin composition (external adhesive). <Beispiel 6>
[0083] A packaging material 1 for an energy storage device 1 with the configuration according to Fig.Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 90 parts by mass of a urethane acrylate resin having two acryloyl groups, 2 parts by mass of benzophenone, 2 parts by mass of maleic anhydride, 2 parts by mass of methyltrimethoxysilane, 2 parts by mass of acryloyloxyethyl acid phosphate, 3 parts by mass of epoxy resin and 0.5 parts by mass of triphenylsulfonium hexafluorophosphate (sulfonium salt) was used as the light-curing resin composition (external adhesive). <Beispiel 7>
[0084] A packaging material 1 for an energy storage device 1 with the configuration according to Fig.Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 82 parts by mass of a urethane acrylate resin having two acryloyl groups, 2 parts by mass of benzophenone, 2 parts by mass of maleic anhydride, 2 parts by mass of methyltrimethoxysilane, 2 parts by mass of acryloyloxyethyl phosphate and 2 parts by mass of triphenylsulfonium hexafluorophosphate was used as the light-curing resin composition (external adhesive). <Beispiel 8>
[0085] A packaging material 1 for an energy storage device 1 with the configuration according to Fig.Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 70 parts by mass of a urethane acrylate resin with two acryloyl groups, 1 part by mass of benzophenone, 1 part by mass of maleic anhydride, 1 part by mass of methyltrimethoxysilane, 2 parts by mass of acryloyloxyethyl phosphate, 20 parts by mass of an epoxy resin and 5 parts by mass of triphenylsulfonium hexafluorophosphate was used as the light-curing resin composition (external adhesive). <Beispiel 9>
[0086] Packaging material 1 for an energy storage device with the configuration according to Fig.Example 2 was obtained in the same way as in Example 7, except that a biaxially stretched polyamide film with a hot water shrinkage percentage of 5.0% was used as biaxially stretched polyamide film 2. The biaxially stretched polyamide film 2 with the hot water shrinkage percentage of 5.0% was obtained by setting the heat-curing temperature to 191°C during the biaxial stretching of the polyamide film. <Beispiel 10>
[0087] Packaging material 1 for an energy storage device with the configuration according to Fig.Example 2 was obtained in the same way as in Example 7, except that a biaxially stretched polyamide film with a hot water shrinkage percentage of 10.0% was used as biaxially stretched polyamide film 2. The biaxially stretched polyamide film with the hot water shrinkage percentage of 10.0% was obtained by setting the heat-curing temperature to 160°C during the biaxial stretching of the polyamide film. <Beispiel 11>
[0088] Packaging material 1 for an energy storage device with the configuration according to Fig.Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 82 parts by mass of a urethane acrylate resin having two acryloyl groups, 2 parts by mass of benzophenone, 2 parts by mass of maleic anhydride, 2 parts by mass of methyltrimethoxysilane, 2 parts by mass of acryloyloxyethyl phosphate, 8 parts by mass of an epoxy resin and 2 parts by mass of triphenylsulfonium hexafluorophosphate was used as the light-curing resin composition (external adhesive). <Beispiel 12>
[0089] Packaging material 1 for an energy storage device with the configuration according to Fig.Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 82 parts by mass of a polyester acrylate resin having two acryloyl groups, 2 parts by mass of benzophenone, 2 parts by mass of maleic anhydride, 2 parts by mass of methyltrimethoxysilane, 2 parts by mass of acryloyloxyethyl phosphate, 8 parts by mass of an epoxy resin and 2 parts by mass of triphenylsulfonium hexafluorophosphate was used as the light-curing resin composition (external adhesive). <Beispiel 13>
[0090] Packaging material 1 for an energy storage device with the configuration according to Fig.Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 82 parts by mass of a urethane acrylate resin having two acryloyl groups, 2 parts by mass of benzoin ethyl ether, 2 parts by mass of maleic anhydride, 2 parts by mass of methyltrimethoxysilane, 2 parts by mass of acryloyloxyethyl phosphate, 8 parts by mass of an epoxy resin and 2 parts by mass of triphenylsulfonium hexafluorophosphate was used as the light-curing resin composition (external adhesive). <Beispiel 14>
[0091] Packaging material 1 for an energy storage device with the configuration according to Fig.Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 82 parts by mass of a urethane acrylate resin having two acryloyl groups, 2 parts by mass of benzyl dimethyl ketal, 2 parts by mass of maleic anhydride, 2 parts by mass of methyl trimethoxysilane, 2 parts by mass of acryloyloxyethyl phosphate, 8 parts by mass of an epoxy resin and 2 parts by mass of triphenylsulfonium hexafluorophosphate was used as the light-curing resin composition (external adhesive). <Beispiel 15>
[0092] Packaging material 1 for an energy storage device with the configuration according to Fig.Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 82 parts by mass of a urethane acrylate resin having two acryloyl groups, 2 parts by mass of benzophenone, 2 parts by mass of maleic anhydride, 2 parts by mass of methyltrimethoxysilane, 2 parts by mass of acryloyloxyethyl phosphate, 8 parts by mass of an oxetane resin and 2 parts by mass of triphenylsulfonium hexafluorophosphate was used as the light-curing resin composition (external adhesive). <Beispiel 16>
[0093] Packaging material 1 for an energy storage device with the configuration according to Fig.Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 82 parts by mass of a urethane acrylate resin having two acryloyl groups, 2 parts by mass of benzophenone, 2 parts by mass of maleic anhydride, 2 parts by mass of methyltrimethoxysilane, 2 parts by mass of acryloyloxyethyl phosphate, 8 parts by mass of a vinyl ether resin and 2 parts by mass of triphenylsulfonium hexafluorophosphate was used as the light-curing resin composition (external adhesive). <Beispiel 17>
[0094] Packaging material 1 for an energy storage device with the configuration according to Fig.Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 82 parts by mass of a urethane acrylate resin having two acryloyl groups, 2 parts by mass of benzophenone, 2 parts by mass of maleic anhydride, 2 parts by mass of methyltrimethoxysilane, 2 parts by mass of acryloyloxyethyl phosphate, 8 parts by mass of an epoxy resin and 2 parts by mass of diphenyliodonium hexafluorophosphate was used as the light-curing resin composition (external adhesive). <Beispiel 18>
[0095] Packaging material 1 for an energy storage device with the configuration according to Fig.Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 82 parts by mass of a urethane acrylate resin having two acryloyl groups, 2 parts by mass of benzophenone, 2 parts by mass of itaconic anhydride, 2 parts by mass of methyltrimethoxysilane, 2 parts by mass of acryloyloxyethyl phosphate, 8 parts by mass of an oxetane resin and 2 parts by mass of triphenylsulfonium hexafluorophosphate was used as the light-curing resin composition (external adhesive). <Beispiel 19>
[0096] Packaging material 1 for an energy storage device with the configuration according to Fig.Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 82 parts by mass of a urethane acrylate resin having two acryloyl groups, 2 parts by mass of benzophenone, 2 parts by mass of anhydrous himic acid, 2 parts by mass of methyltrimethoxysilane, 2 parts by mass of acryloyloxyethyl acid phosphate, 8 parts by mass of an epoxy resin and 2 parts by mass of triphenylsulfonium hexafluorophosphate was used as the light-curing resin composition (external adhesive). <Beispiel 20>
[0097] Packaging material 1 for an energy storage device with the configuration according to Fig.Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 82 parts by mass of a urethane acrylate resin having two acryloyl groups, 2 parts by mass of benzophenone, 2 parts by mass of maleic anhydride, 2 parts by mass of vinyl triethoxysilane, 2 parts by mass of acryloyloxyethyl phosphate, 8 parts by mass of an oxetane resin and 2 parts by mass of triphenylsulfonium hexafluorophosphate was used as the light-curing resin composition (external adhesive). <Beispiel 21>
[0098] Packaging material 1 for an energy storage device with the configuration according to Fig.Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 82 parts by mass of a urethane acrylate resin having two acryloyl groups, 2 parts by mass of benzophenone, 2 parts by mass of maleic anhydride, 2 parts by mass of allyl trimethoxysilane, 2 parts by mass of acryloyloxyethyl phosphate, 8 parts by mass of an epoxy resin and 2 parts by mass of triphenylsulfonium hexafluorophosphate was used as the light-curing resin composition (external adhesive). <Beispiel 22>
[0099] Packaging material 1 for an energy storage device with the configuration according to Fig.Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 82 parts by mass of a urethane acrylate resin with two acryloyl groups, 2 parts by mass of benzophenone, 2 parts by mass of maleic anhydride, 2 parts by mass of methyltrimethoxysilane, 2 parts by mass of bis(2-methacryloyloxyethyl) phosphate, 8 parts by mass of an epoxy resin and 2 parts by mass of triphenylsulfonium hexafluorophosphate was used as the light-curing resin composition (external adhesive). <Referenzbeispiel 23>
[0100] Packaging material 1 for an energy storage device with the configuration according to Fig. 2 was obtained in the same manner as in reference example 1, except that a light-curing resin composition comprising 99 parts by mass of a urethane acrylate resin having two acryloyl groups and 1 part by mass of a benzophenone was used as the light-curing resin composition (external adhesive). <Referenzbeispiel 24>
[0101] Packaging material 1 for an energy storage device with the configuration according to Fig. Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 45 parts by mass of a urethane acrylate resin having two acryloyl groups, 5 parts by mass of benzophenone, 3 parts by mass of maleic anhydride, 2 parts by mass of methyltrimethoxysilane, 20 parts by mass of acryloyloxyethyl phosphate, 20 parts by mass of an epoxy resin and 5 parts by mass of triphenylsulfonium hexafluorophosphate was used as the light-curing resin composition (external adhesive). <Referenzbeispiel 25>
[0102] Packaging material 1 for an energy storage device with the configuration according to Fig.Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 54 parts by mass of a urethane acrylate resin having two acryloyl groups, 1 part by mass of benzophenone, 1 part by mass of maleic anhydride, 2 parts by mass of methyltrimethoxysilane, 2 parts by mass of acryloyloxyethyl phosphate, 30 parts by mass of an epoxy resin and 8 parts by mass of triphenylsulfonium hexafluorophosphate was used as the light-curing resin composition (external adhesive). <Referenzbeispiel 26>
[0103] Packaging material 1 for an energy storage device with the configuration according to Fig.Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 82 parts by mass of a urethane acrylate resin having two acryloyl groups, 2 parts by mass of benzophenone and 8 parts by mass of methyltrimethoxysilane was used as the light-curing resin composition (external adhesive). <Referenzbeispiel 27>
[0104] Packaging material 1 for an energy storage device with the configuration according to Fig. Example 2 was obtained in the same manner as in Reference Example 1, except that a light-curing resin composition comprising 79 parts by mass of a urethane acrylate resin having two acryloyl groups, 2 parts by mass of benzophenone, 2 parts by mass of maleic anhydride, 2 parts by mass of methyltrimethoxysilane, and 15 parts by mass of acryloxyethyl acid phosphate was used as the light-curing resin composition (external adhesive). <Beispiel 28>
[0105] A packaging material 1 for an energy storage device with the structure according to Fig. 1 was obtained in the same way as in Example 7, except that the slightly adhesive layer 8 was not provided. <Vergleichsbeispiel 1>
[0106] A packaging material 1 for an energy storage device was obtained in the same way as in Example 7, except that a biaxially stretched polyamide film with a hot water shrinkage percentage of 1.0% was used as the biaxially stretched polyamide film 2. The biaxially stretched polyamide film with the hot water shrinkage percentage of 1.0% was obtained by setting the heat set temperature to 221°C during the biaxial stretching of the polyamide film. <Vergleichsbeispiel 2>
[0107] A packaging material 1 for an energy storage device was obtained in the same way as in Example 7, except that a biaxially stretched polyamide film with a hot water shrinkage percentage of 15.0% was used as the biaxially stretched polyamide film 2. The biaxially stretched polyamide film with the hot water shrinkage percentage of 15.0% was obtained by setting the heat set temperature to 135°C during the biaxial stretching of the polyamide film. <Vergleichsbeispiel 3>
[0108] A chemical conversion coating was formed by applying a chemical conversion treatment solution containing phosphoric acid, polyacrylic acid (acrylic-based resin), a chromium(III) salt compound, water, and alcohol to both sides of 35 µm thick aluminum foil (aluminum foil A8079, specified in JIS H4160) and subsequent drying at 180°C. The chromium adhesion of this chemical conversion coating was 10 mg / m². 2 per page.
[0109] Then, a heat-curing type adhesive (external adhesive) containing 80 parts by mass of an acid-modified polyolefin resin and 20 parts by mass of polyisocyanate was sprayed onto a surface of the aluminum conversion-treated aluminum foil 4, so that the mass after drying was 4 g / m² 2 became.
[0110] On the other hand, a biaxially stretched polyamide film 2 with a slightly adhesive layer 8 was obtained by applying a resin, obtained by mixing 70 parts by mass of a urethane resin and 30 parts by mass of an epoxy resin, to a surface of a biaxially stretched polyamide film 2 with a hot water shrinkage percentage of 2.0% and a thickness of 15 µm by a spray coating process and subsequent drying, forming a slightly adhesive layer 8 with a thickness of 0.05 µm. The biaxially stretched polyamide film 2 with the hot water shrinkage percentage of 2.0% was obtained by setting the heat set temperature to 214°C during the biaxial stretching of the polyamide film.
[0111] The slightly adhesive side of the polyamide film 2 with the slightly adhesive layer 8 was placed onto the outer adhesive-coated side of one side of the aluminum foil 4 and laminated, resulting in a first laminate. The first laminate was placed in an environment of 60°C for 9 days and subjected to heat aging to cure the outer adhesive.
[0112] Then, an internal adhesive, consisting of an acid-modified, heat-curing polypropylene adhesive, was applied to the other surface of the aluminum foil 4 of the first laminate after the heat aging process, so that the mass after drying was 2.5 g / m². 2 was, and then a non-stretched polypropylene film 3 with a thickness of 30 µm was laminated onto the inner side coated with medium, obtaining a second laminate.
[0113] The second laminate was subjected to a heat aging process by being placed in an environment of 40°C for 9 days to harden the internal heat-curing type adhesive, to form an internal adhesive layer 6, while retaining a packaging material 1 for an energy storage device. [Table 1] Ref.-Example 1 Ref.-Example 2 Ref.-Example 3 Ref.-Example 4 Ref.-Example 5 Example 6 Example 7 Example 8 Example 9 Example 10 Light-curing resin composition / bulk parts A Urethane acrylate resin 95 90 94 91 90 90 82 70 82 82 Epoxy acrylate resin - - - - - - - - - - Polyester acrylate resin - - - - - - - - - - B Benzophenone 5 0,2 5 3 0,2 2 2 1 2 2 Benzoin ethyl ether - - - - - - - - - - Benzyldimethylketal - - - - - - - - - - C Maleic anhydride - 5 0,2 3 0,2 2 2 1 2 2 Itaconic anhydride - - - - - - - - - - Anhydrous Himic Acid - - - - - - - - - - D Methyltrimethoxysilane - 5 0,2 3 0,2 2 2 1 2 2 Vinyltriethoxysilane - - - - - - - - - - Allyl trimethoxysilane - - - - - - - - - - E Phosphoric acid acrylate X - - - 0,3 10 2 2 2 2 2 Phosphoric acid acrylate Y - - - - - - - - - - F Epoxy resin - - - - - 2 8 20 8 8 Oxetan resin - - - - - - - - - - Vinyl ether resin - - - - - - - - - G Sulfonium salt V - - - - - 0,5 2 5 2 2 Iodonium salt W - - - - - - - - - - Ref.-Example 1 Ref.-Example 2 Ref.-Example 3 Ref.-Example 4 Ref.-Example 5 Example 6 Example 7 Example 8 Example 9 Example 10 Outer layer hydrothermal shrinkage (%) 2,0 2,0 2,0 2,0 2,0 2,0 2,0 2,0 5,0 10,0 Presence or absence of the slightly adhesive layer Yes Yes Yes Yes Yes Yes Yes Yes Yes Yes Evaluation Hardened Film Young Module (MPa) 500 460 420 420 420 400 250 90 250 250 malleability ◯ ◯ ◯ ◯ ◯ ◯ ◯ ◯ ◯ ◯ Sealing properties (presence / absence of peeling) Δ ◯ ◯ ◯ ◯ ◯ ◯ ◯ ◯ ◯ Hot water resistance (presence or absence of peeling) Δ Δ ◯ ◯ ◯ ◯ ◯ ◯ ◯ ◯ Curing temperature lamination strength Δ Δ Δ Δ Δ ◯ ◯ ◯ ◯ ◯ [Table 2] Example 11 Example 12 Example 13 Example 14 Example 15 Example 16 Example 17 Example 18 Example 19 Example 20 Light-curing resin composition / bulk parts A Urethane acrylate resin - - 82 82 82 82 82 82 82 82 Epoxy acrylate resin 82 - - - - - - - - - Polyester acrylate resin - 82 - - - - - - - - B Benzophenone 2 2 - - 2 2 2 2 2 2 Benzoin ethyl ether - - 2 - - - - - - - Benzyldimethylketal - - - 2 - - - - - - C Maleic anhydride 2 2 2 2 2 2 2 - - 2 Itaconic anhydride - - - - - - - 2 - - Anhydrous Himic Acid - - - - - - - - 2 - D Methyltrimethoxysilane 2 2 2 2 2 2 2 2 2 - Vinyltriethoxysilane - - - - - - - - - 2 Allyl trimethoxysilane - - - - - - - - - - E Phosphoric acid acrylate X 2 2 2 2 2 2 2 2 2 2 Phosphoric acid acrylate Y - - - - - - - - - - F Epoxy resin 8 8 8 8 - - 8 - 8 - Oxetan resin - - - - 8 - - 8 - 8 Vinyl ether resin - - - - - 8 - - - - G Sulfonium salt V 2 2 2 2 2 2 - 2 2 2 Iodonium salt W - - - - - - 2 - - - Example 11 Example 12 Example 13 Example 14 Example 15 Example 16 Example 17 Example 18 Example 19 Example 20 Outer layer hydrothermal shrinkage (%) 2,0 2,0 2,0 2,0 2,0 2,0 2,0 2,0 2,0 2,0 Presence or absence of the slightly adhesive layer Yes Yes Yes Yes Yes Yes Yes Yes Yes Yes Evaluation Hardened Film Young Module (MPa) 260 280 240 250 250 250 250 250 250 250 malleability ◯ ◯ ◯ ◯ ◯ ◯ ◯ ◯ ◯ ◯ Sealing properties (presence / absence of peeling) ◯ ◯ ◯ ◯ ◯ ◯ ◯ ◯ ◯ ◯ Hot water resistance (presence or absence of peeling) ◯ ◯ ◯ ◯ ◯ ◯ ◯ ◯ ◯ ◯ Curing temperature-lamination strength) ◯ ◯ ◯ ◯ ◯ ◯ ◯ ◯ ◯ ◯ [Table 3] Example 21 Example 22 Ref.-Example 23 Ref.-Example 24 Ref. - Example 25 Ref.-Example 26 Ref. - Example 27 Example 28 Light-curing resin composition / bulk parts A Urethane acrylate resin 82 82 99 45 54 82 79 82 Epoxy acrylate resin - - - - - - - - Polyester acrylate resin - - - - - - - - B Benzophenone 2 2 1 5 1 2 2 2 Benzoin ethyl ether - - - - - - - - Benzyldimethylketal - - - - - - - - C Maleic anhydride 2 2 - 3 1 8 2 2 Itaconic anhydride - - - - - - - - Anhydrous Himic Acid - - - - - - - - D Methyltrimethoxysilane - 2 - 2 2 8 2 2 Vinyltriethoxysilane - - - - - - - - Allyl trimethoxysilane 2 - - - - - - - E Phosphoric acid acrylate X 2 - - 20 2 - 15 2 Phosphoric acid acrylate Y - 2 - - - - - - F Epoxy resin 8 8 - 20 30 - - 8 Oxetan resin - - - - - - - - Vinyl ether resin - - - - - - - - G Sulfonium salt V 2 2 - 5 8 - - 2 Iodonium salt W - - - - - - - - Example 21 Example 22 Ref.-Example 23 Ref.-Example 24 Ref. - Example 25 Ref.-Example 26 Ref. - Example 27 Example 28 Outer layer hydrothermal shrinkage (%) 2,0 2,0 2,0 2,0 2,0 2,0 2,0 2,0 Presence or absence of the slightly adhesive layer Yes Yes Yes Yes Yes Yes Yes no Evaluation Hardened Film Young Module (MPa) 250 250 520 60 40 530 510 250 malleability ◯ ◯ ◯ ◯ ◯ ◯ ◯ ◯ Sealing properties (presence / absence of peeling) ◯ ◯ ◯ Δ Δ ◯ ◯ ◯ Hot water resistance (presence or absence of peeling) ◯ ◯ ◯ ◯ Δ Δ Δ ◯ Curing temperature lamination strength ◯ ◯ Δ ◯ ◯ Δ Δ Δ [Table 4] See example 1 See example 2 See example 3 Light-curing resin composition / bulk parts A Urethane acrylate resin 82 82 (Heat-curing resin composition) 80 parts by mass acid-modified polyolefin resin + 20 parts by mass polyisocyanate Epoxy acrylate resin - - Polyester acrylate resin - - B Benzophenone 2 2 Benzoin ethyl ether - - Benzyldimethylketal - - C Maleic anhydride 2 2 Itaconic anhydride - - Anhydrous Himic Acid - - D Methyltrimethoxysilane 2 2 Vinyltriethoxysilane - - Allyl trimethoxysilane - - E Phosphoric acid acrylate X 2 2 Phosphoric acid acrylate Y - - F Epoxy resin 8 8 Oxetan resin - - Vinyl ether resin - - G Sulfonium salt V 2 2 Iodonium salt W - - See example 1 See example 2 See example 3 Outer layer hydrothermal shrinkage ( ) 1,0 15,0 2,0 Presence or absence of the slightly adhesive layer Yes Yes Yes Evaluation Hardened Film Young Module (MPa) 250 250 250 malleability × ◯ ◯ Sealing properties (presence / absence of peeling) ◯ × ◯ Hot water resistance (presence or absence of peeling) ◯ × ◯ Curing temperature lamination strength ◯ ◯ ×
[0114] In Tables 1 to 4, acryloyloxyethyl acid phosphate is expressed as "phosphoric acid acrylate X", bis(2-methacryloyloxyethyl) acid phosphate is expressed as "phosphoric acid acrylate Y", triphenylsulfonium hexafluorophosphate is given as "sulfonium salt V", diphenyliodonium hexafluorophosphate is given as "iodonium salt W".
[0115] In Tables 1 to 4, for the light-curing composition, “A” means an acrylate resin, “B” means a photo-radical polymerization initiator, “C” means an acid anhydride, “D” means a silane coupling agent, “E” means phosphoric acid-containing (meth)acrylate, “F” means an epoxy resin, oxetane resin or vinyl ether resin, and “G” means a photo-cationic polymerization initiator.
[0116] The evaluation was carried out with each packaging material for an energy storage device, obtained as described above, based on the following measurement and evaluation procedure. <Messverfahren für Young-Modul>
[0117] The Young's modulus (MPa) of the cured film, where each outer adhesive (light-curing resin composition) used in the examples, reference examples, and comparison examples was subjected to light curing and measured according to JIS K7127-1999. Specifically, after coating each outer adhesive (light-curing resin composition) onto a 50 µm thick glass plate, the light-curing resin composition was irradiated with ultraviolet rays at 300 mJ / cm². 2 Light-cured to obtain a hardened film with a thickness of 46 µm. After removing the hardened film from the glass plate, it was cut to a size of 15 mm wide x 100 mm long to produce a test piece. The test piece was subjected to a tensile test using Strograph (AGS-5kNX), manufactured by Shimadzu Corporation, at a draw rate of 200 mm / minute to measure the Young's modulus (MPa). <Formfähigkeit-Auswertungsverfahren>
[0118] Deep forming was performed on a packaging material in a substantially rectangular parallelepiped shape (55 mm length x 35 mm width x any depth) (a substantially rectangular parallelepiped shape with an open surface) using a deep-drawing tool manufactured by Amada Co., Ltd. That is, the deep forming was carried out by changing the mold depth. The presence or absence of fine holes and / or cracks on the edge of the resulting formed product was then examined. The maximum mold depth (mm) at which no fine holes and / or cracks appeared was tested and evaluated based on the following criteria. The presence or absence of fine holes and / or cracks was examined using a light transmission method in a darkened room. (Evaluation criteria) °◯°: Maximum mold depth at which no fine holes and / or cracks appeared was 5 mm or more (successful) “Δ”: Maximum mold depth at which no fine holes and / or cracks appeared was 4 mm or more but less than 5 mm (successful) “X” Maximum mold depth at which no fine holes and / or cracks appeared was less than 4 (not successful) <Auswertungsverfahren der Abdichteigenschaft> (Evaluation of the presence or absence of delamination when deep forming was performed)
[0119] Deep forming was performed on a packaging material using the deep-drawing tool described above, with a substantially parallelepiped shape (essentially a rectangular parallelepiped shape with an open surface) measuring 5 mm in length × 35 mm in width × 5 mm. At this stage, the forming was carried out such that the heat-resistant resin layer 2 was located outside the formed product. Two formed products were produced for each example, each reference example, and each comparison example. The side parts (peripheral sealing areas: see Fig.4) 29 of the two molded product parts 10 were brought into contact and overlapped and heat-sealed for 6 seconds at 170°C. Afterwards, the presence or absence of delamination (peeling) in the heat-sealed area 39 and the presence or absence of floatation were checked by visual observation and evaluated based on the following assessment criteria. (Evaluation criteria) “◯” No delamination (peeling) was observed and no change in appearance was observed (successful) “Δ” Although some delamination (peeling) sometimes occurred, there was actually no delamination (peeling) and no change in appearance (successful) “X” Delamination (peeling) occurred and there was also a change in appearance (not successful). <Heißwasserresistenz-Bewertungsverfahren>(Assessment of the presence or absence of delamination when used under harsh conditions such as high temperature and high humidity)
[0120] A deep-drawing was performed using a substantially rectangular parallelepiped shape (essentially a rectangular parallelepiped shape with one open face) measuring 55 mm in length × 35 mm in width × 5 mm, with respect to a packaging material, using the deep-drawing tool described above. At this stage, the forming process was carried out such that the heat-resistant resin layer 2 was located outside the formed product. Two formed products were produced for each example, each reference example, and each comparison example. The flanks (peripheral sealing area: see Fig.4) 29 of the two molded products 10 were brought into contact and overlapped and heat-sealed for 6 seconds at 170°C. The heat-sealed object was then immersed in hot water at 85°C for 240 hours, removed, and visually inspected for the presence or absence of delamination (peeling) in the heat-sealed area 39 and the presence or absence of appearance float. (Evaluation criteria) “◯” No delamination (peeling) was observed and no change in appearance was observed (successful) “Δ” Although some delamination (peeling) sometimes occurred, there was actually no delamination (peeling) and no change in appearance (successful) “X” Delamination (peeling) occurred and there was also a change in appearance (not successful). <Laminationsfestigkeits-Messverfahren bei hoher Temperatur>
[0121] A sample measuring 15 mm in width and 150 mm in length was cut from the received packaging material and peeled off between the aluminum foil and the heat-resistant resin layer in the area from one end in the longitudinal direction to the position 10 mm inwards.
[0122] Using a Strograph (AGS-5kNX) manufactured by Shimadzu Corporation, conforming to JIS K6854-3(1999), one laminate was clamped with the aluminum foil and fixed with a chuck, and the peeled-off heat-resistant resin layer was clamped and fixed with the other chuck and held for 1 minute at a temperature of 120°C. The peel strength was then measured when T-peeling was performed at a temperature of 120°C and a pulling rate of 100 mm / min. The value at which the measurement stabilized was termed "lamination strength (N / 15 mm width) at high temperature." The measurement results were evaluated based on the following criteria. “O”: The lamination strength was equal to or greater than “2.0 N / 15 mm width” (successful) “Δ”: The lamination strength was equal to or greater than “1.5 N / 15 mm width” and less than 2.0 N / 15 mm width” (successful) “X”: The lamination strength was less than “1.5 N / 15 mm width” (not successful).
[0123] As can be seen from the tables, the packaging materials for an energy storage device of reference examples 1 to 5 and 23 to 27 and examples 6 to 22 and 28 of this invention exhibited excellent formability without the appearance of fine holes and / or cracks, even after deep forming. Furthermore, even after deep forming, it was possible to suppress delamination (peeling). Lamination strength was high even at high temperatures, and hot water resistance was good, preventing delamination (peeling) even under harsh environments such as high temperature and high humidity.
[0124] On the other hand, in comparison examples 1 to 3, which deviated from the area according to the claims of this invention, at least one of the assessments was rated with “X” (not sufficient). Industrial applicability
[0125] As a specific example of the packaging material for an energy storage device of this invention, this packaging material can be used as packaging material for various energy storage devices, such as... * Energy storage device such as lithium-ion secondary battery (lithium-ion battery), lithium polymer battery, etc.), * Lithium-ion capacitor and * Electrical double-layer capacitor.
[0126] Furthermore, the energy storage device of this invention includes not only the energy storage devices illustrated above, but also a battery with a total solid state.
[0127] This application claims priority over Japanese patent application 2016-125294, filed on June 24, 2016, the full disclosure of which is incorporated herein by reference.
[0128] It is understood that the terms and expressions used herein are for illustrative purposes only and are not intended to limit this invention. They do not eliminate equivalents of features shown and mentioned herein and permit various modifications that fall within the scope of this invention. This invention permits any design changes, provided they do not deviate from the scope defined in these claims. Description of reference symbols 1 Packaging material for an energy storage device 2. Heat-resistant resin layer (outer layer) 3. Heat-fusing resin layer (inner layer) 4 layers of metal foil 5 First adhesive layer (outer adhesive layer) 6 Second adhesive layer (inner adhesive layer) 8 Light adhesive layer 10 Housings (molded housings) 15 Packaging part 30 Energy storage device 31 Energy storage device main body
Claims
[1] Packaging material for an energy storage device, comprising: a heat-resistant resin layer that serves as the outer layer, a heat-fusible resin layer serving as the inner layer, and a metal foil layer arranged between the two layers, wherein the heat-resistant resin layer is composed of a heat-resistant resin film having a hot water shrinkage percentage of 1.5 to 12%, wherein the heat-resistant resin layer and the metal foil layer are bonded via an outer adhesive layer composed of an ultraviolet light-curable resin composition, wherein the ultraviolet light-curable resin composition contains an acrylate resin, a photo-radical polymerization initiator, a silane coupling agent, acid anhydride, phosphoric acid-containing (meth)acrylate, one or more resins selected from the group consisting of an epoxy resin, oxetane resin and a vinyl ether resin, and a photo-cationic polymerization initiator and wherein in the ultraviolet light-curable resin composition, a content of the acrylate resin is 70 to 98 mass%, a content of the silane coupling agent is 0.1 to 5 mass%, a content of the acid anhydride is 0.1 to 5 mass%, a content of the phosphoric acid-containing (meth)acrylate is 0.1 to 10 mass%, a content of the photo-radical polymerization initiator is 0.1 to 5 mass%, a content of one or more resins selected from the group consisting of an epoxy resin, oxetane resin and vinyl ether resin is 1 to 20 mass%, and a content of the photo-cationic polymerization initiator is 0.5 to 5 mass%. [2] The packaging material for an energy storage device according to claim 1, wherein a Young's modulus of the cured film is 90 to 400 MPa. [3] The packaging material for an energy storage device according to claim 1 or 2, wherein a slightly adhesive layer is disposed between the heat-resistant resin layer and the outer adhesive layer. [4] A packaging case for an energy storage device, wherein the packaging case is made from a molded product of the packaging material according to any one of claims 1 to 3. [5] Energy storage device comprising: an energy storage device main body and a packaging part composed of the packaging material according to one of claims 1 to 3 and / or the packaging housing according to claim 4, wherein the energy storage device main body is packaged with the packaging part. [6] A method for producing a packaging material for an energy storage device, the method comprising: a step of producing a first laminate in which a heat-resistant resin film having a hot water shrinkage percentage of 1.5 to 12% is bonded to a surface of a metal foil layer via an ultraviolet light-curable resin composition, a step of irradiating an ultraviolet light onto the first laminate from the side of the heat-resistant resin film, a step of producing a second laminate, wherein a heat-fusible resin film is bonded to the other surface of the metal foil layer of the first laminate after irradiation of ultraviolet light via a thermosetting adhesive, and a step of performing a heat treatment on the second laminate, wherein the ultraviolet light-curable resin composition contains an acrylate resin, a photo-radical polymerization initiator, a silane coupling agent, acid anhydride, phosphoric acid-containing (meth)acrylate, one or more resins selected from the group consisting of an epoxy resin, oxetane resin and a vinyl ether resin, and a photo-cationic polymerization initiator and wherein in the ultraviolet light-curable resin composition, a content of the acrylate resin is 70 to 98 mass%, a content of the silane coupling agent is 0.1 to 5 mass%, a content of the acid anhydride is 0.1 to 5 mass%, a content of the phosphoric acid-containing (meth)acrylate is 0.1 to 10 mass%, a content of the photo-radical polymerization initiator is 0.1 to 5 mass%, a content of one or more resins selected from the group consisting of an epoxy resin, oxetane resin and vinyl ether resin is 1 to 20 mass%, and a content of the photo-cationic polymerization initiator is 0.5 to 5 mass%.
Citation Information
Patent Citations
Flying object protection facility
JP2016125294A
MOLDING PACKAGING MATERIAL AND MOLDING CASES
DE102014211477A1
Packaging material and molded body housings
DE102014214675A1
Resin composition
EP3015523A1
Packaging material for battery case and battery case
US20090130407A1