Self-aligning gate insulation with asymmetrical cut arrangement

The described process flow for self-aligned gate isolation with symmetrical and asymmetrical cuts addresses alignment and uniformity challenges, improving semiconductor structure performance and scalability by reducing short-channel effects and parasitic resistance in multi-gate FETs.

DE112020002838B4Active Publication Date: 2024-10-02INTERNATIONAL BUSINESS MACHINE CORPORATION

Patent Information

Application Number
DE112020002838
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-15
Filing Date
2020-06-15
Publication Date
2024-10-02
Estimated Expiration
2040-06-15

AI Technical Summary

Technical Problem

Existing techniques for self-aligned gate cuts in semiconductor structures, particularly for asymmetrical gate cuts required in SRAM units, face challenges in achieving precise alignment and uniformity below 5 nm, leading to issues like short-channel effects and increased parasitic resistance in multi-gate FETs.

Method used

A process flow involving self-aligned gate isolation with both symmetrical and asymmetrical notch arrangements, including forming a channel protection coating, dummy gates, and using selective epitaxial growth and etching to create precise gate cuts, followed by filling with dielectric material, addresses the alignment and uniformity issues.

Benefits of technology

Enables the formation of semiconductor structures with both symmetrical and asymmetrical gate isolations, allowing for precise gate cuts and improved control over channel characteristics, reducing short-channel effects and parasitic resistance in multi-gate FETs, thereby enhancing performance and scalability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A method for forming a semiconductor structure comprising: forming a plurality of fins (120; 304) over an upper surface of a substrate (302); forming a region (306) for shallow trench insulation over the upper surface of the substrate surrounding the plurality of fins; forming a plurality of nanosheet stacks of a channel material over the plurality of fins, wherein the plurality of nanosheet stacks provide channels (310) for one or more nanosheet field-effect transistors;Forming a channel protection coating (312) over at least a portion of the side walls and upper surface of a first of the plurality of nanosheet stacks formed over a first of the plurality of fins, wherein the channel protection coating is further formed over a portion of the shallow trench insulation area extending from the portion of the side walls of the first nanosheet stack towards a second of the plurality of nanosheet stacks formed over a second of the plurality of fins; forming a plurality of gate stacks (334) surrounding portions of the plurality of nanosheet stacks exposed by the channel protection coating; forming at least one asymmetric self-aligned gate insulation structure over the channel protection coating;and forming at least one symmetrical self-aligned gate isolation structure over a sub-region of the area for shallow trench isolation between and at equal distances from a third of the plurality of fins and a fourth of the plurality of fins, wherein the asymmetrical self-aligned gate isolation structure formed over the channel protection coating comprises: a first sub-region formed adjacent to the channel protection coating surrounding side walls of the first nanosheet stack; and a second sub-region formed over an upper surface of the channel protection coating surrounding the sub-region of the upper surface of the first nanosheet stack.
Need to check novelty before this filing date? Find Prior Art

Description

BACKGROUND

[0001] The present invention relates to semiconductors and more specifically to techniques for forming Semiconductor structures. Semiconductors and integrated circuit chips have become omnipresent in many products as particularly a reduction in their costs and dimensions. There is a continuing desire to reduce the size of structural features and / or to use a larger set of structural features for a given chip dimensions. Miniaturization generally allows for increased Performance at lower power levels and lower costs. This technology achieves a Scaling of certain micro-units, such as logic gates, field-effect transistors (FETs) and Capacitors, at the atomic level or approaching it.

[0002] The document US 2017 / 0 330 801 A1 relates to semiconductor devices, a gate structure for a Semiconductor device and a method for its manufacture. A method for forming a gate structure comprises Forming a first set of one or more semiconductor features and a second set of one or more several semiconductor features. The method additionally includes forming a sacrificial gate extending over the semiconductor features of the first set and the semiconductor features of the second set. The method comprises further forming a hole by etching the sacrificial gate, wherein the sacrificial gate is divided into a first sacrificial gate section and a second sacrificial gate section, forming a barrier in the hole by depositing a Barrier material in the hole, removing the first sacrificial gate section and the second sacrificial gate section by Etching, wherein a first trench section is formed and a second trench section is formed, forming a first gate conductor in the first trench section and the second trench section, forming a mask over the second trench section, wherein the mask exposes the first trench section, the etching of the first gate conductor in the first trench section, wherein the mask and the barrier are used for etching the first gate conductor in the second trench section, and forming a second gate conductor in the first trench section.

[0003] The publication ´´Stacked nanosheet fork architecture for SRAM design and device co-optimization toward 3nm´´ deals with SRAM scaling beyond the 5nm technology node and shows the basic Scaling limits due to FinFET and Gate All-Around (GAA) technology. The paper discusses that, to compensate for the expected slowdown in gate pitch scaling below 42 nm, several Scaling amplifiers are required to reduce the cell height. With FinFET and GAA technology, However, only limited scaling benefits can be achieved. Therefore, a vertically stacked lateral nanosheet architecture with a bifurcated gate structure, which offers superior performance compared to FinFET and GAA devices. performance and area scaling. In addition, limited additional processing complexity The fork architecture enables scaling of the SRAM area by 20% at iso-performance and a 30% performance improvement in iso-area compared to FinFET beyond the 5 nm technology node (WECKX, P. [et al.]: Stacked nanosheet fork architecture for SRAM design and device co-optimization toward 3nm. In: IEEE International Electron Devices Meeting (IEDM)), 2017, pp. 20.5.1-20.5.4. doi: 10.1109 / IEDM.2017.8268430).

[0004] The document US 2014 / 0 284 667 A1 relates to a FinFET structure and method for its manufacture, with a A plurality of fins etched from a semiconductor substrate, a plurality of gates above and perpendicular to the plurality of ribs, each comprising a pair of spacers on opposite sides of the gates, and a Gap filling material above the semiconductor substrate, below the gate and between the plurality of fins, wherein the Gate that separates the gap filler material from each of the plurality of ribs. SUMMARY

[0005] The invention relates to a semiconductor structure, a method for its production and an integrated circuit, whose features are specified in the corresponding independent claims. Embodiments are described in the dependent claims. In particular, the method comprises forming self-aligned gate Isolation structures with both symmetric and asymmetric notch arrangements are available.

[0006] In particular, the method for forming a semiconductor structure comprises: forming a plurality of fins over a upper surface of a substrate, forming a region surrounding the plurality of fins for shallow trench isolation over the upper surface of the substrate and forming a plurality of nanosheet stacks of a channel material over the plurality of fins, wherein the plurality of nanosheet stacks form channels for one or more nanosheet field effect transistors. The method further comprises: forming a channel protection coating over at least a portion of side walls and an upper surface of a first of the plurality of nanosheet stacks, the formed over a first of the plurality of fins, wherein the channel protection coating is further formed over a Part of the shallow trench isolation area is formed, which is different from the part of the side walls of the first nanosheet stack towards a second one of the plurality of nanosheet stacks, which is arranged above a second of the plurality of fins. The method further comprises: forming a plurality of gate Stacks surrounding portions of the plurality of nanosheet stacks exposed by the channel protection coating, Forming at least one asymmetric self-aligned gate insulation structure over the channel protection overcoat and forming at least one symmetrical self-aligned gate insulation structure over a portion of the Area for shallow trench isolation between a third of the plurality of fins and a fourth of the plurality of Fins.

[0007] In particular, the semiconductor structure comprises: a substrate, a plurality of fins arranged above an upper surface of the substrate, an area arranged above the upper surface of the substrate for a flat Trench isolation surrounding the plurality of fins, and a plurality of nanosheet stacks made of a channel material, arranged above the plurality of fins, wherein the plurality of nanosheet stacks form channels for one or more Nanosheet field-effect transistors. The semiconductor structure also has a channel protection coating that over at least a portion of side walls and an upper surface of a first of the plurality of nanosheet stacks arranged over a first of the plurality of fins, wherein the channel protection coating of the Furthermore, it is arranged over a portion of the shallow trench isolation area which is different from the portion the side walls of the first nanosheet stack towards a second of the plurality of nanosheet stacks which is arranged over a second of the plurality of fins. The semiconductor structure further comprises: a A plurality of gate stacks surrounding portions of the plurality of nanosheet stacks formed by the Channel protection coating exposed, at least one asymmetric self-aligned gate insulation structure formed over the channel protection coating is arranged, and at least one symmetrical self-aligned gate insulation structure, the over a portion of the shallow trench isolation region between a third of the plurality of fins and a fourth of the plurality of fins.

[0008] In particular, the integrated circuit comprises a nanosheet field effect transistor structure comprising: a Substrate, a plurality of fins arranged over an upper surface of the substrate, a fin arranged over the upper Surface of the substrate arranged area for a shallow trench isolation surrounding the plurality of fins, and a plurality of nanosheet stacks of a channel material arranged over the plurality of fins, wherein the A plurality of nanosheet stacks provides channels for one or more nanosheet field-effect transistors. Nanosheet field effect transistor structure further comprises a channel protection coating disposed over at least one Partial region of side walls and an upper surface of a first of the plurality of nanosheet stacks disposed over a first of the plurality of fins, wherein the channel protection coating is further disposed over a Part of the area for shallow trench isolation is arranged, which is different from the part of the side walls of the first nanosheet stack towards a second one of the plurality of nanosheet stacks, which is arranged above a second of the plurality of fins. The nanosheet field-effect transistor structure further comprises: a A plurality of gate stacks surrounding portions of the plurality of nanosheet stacks formed by the Channel protection coating exposed, at least one asymmetric self-aligned gate insulation structure formed over the channel protection coating is arranged, and at least one symmetrical self-aligned gate insulation structure, the over a portion of the shallow trench isolation region between a third of the plurality of fins and a fourth of the plurality of fins. BRIEF DESCRIPTION OF THE DRAWINGS Fig. 1A shows a top-down view of an aligned gate notch between two fins according to an embodiment of the invention. Fig. 1B shows a top-down view of an incorrectly aligned and enlarged gate incision between two fins. Fig. 2 shows a top-down view of asymmetric gate cuts in a topology of a Structure of a static random access memory according to an embodiment of the invention. Fig. 3A shows a side cross-sectional view of a semiconductor structure after patterning of nanosheet Stacking according to an embodiment of the invention. Fig. 3B is a top-down view of a portion of the structure shown in Fig. 3A according to an embodiment of the invention. Fig. 4 shows a side cross-sectional view of the structure of Fig. 3A following formation of a Channel protection overlay, a dummy gate and a gate hard mask according to an embodiment of the invention represents. Fig. 5A represents a first lateral cross-sectional view of the structure of Fig. 4 following formation of Source / drain regions and planarization according to an embodiment of the invention. Fig. 5B represents a second lateral cross-sectional view of the structure of Fig. 4 following the formation of Source / drain regions and planarization according to an embodiment of the invention. Fig. 6 is a lateral cross-sectional view of the structure of Fig. 5A following removal of the Dummy gates according to an embodiment of the invention. Fig. 7 shows a side cross-sectional view of the structure of Fig. 6 following structuring of the Channel protection cover according to an embodiment of the invention. Fig. 8 shows a side cross-sectional view of the structure of Fig. 7 following selective growth of the nanosheet sacrificial material according to an embodiment of the invention. Fig. 9 shows a side cross-sectional view of the structure of Fig. 8 following formation of a self-aligned insulation layer according to an embodiment of the invention. Fig. 10 represents a side cross-sectional view of the structure of Fig. 9 following formation of a organic planarization layer according to an embodiment of the invention. Fig. 11 shows a side cross-sectional view of the structure of Fig. 10 following structuring of a symmetric and an asymmetric gate notch according to an embodiment of the invention. Fig. 12 shows a side cross-sectional view of the structure of Fig. 11 following filling of the symmetrical and asymmetrical gate cut with a dielectric material according to a embodiment of the invention. Fig. 13 is a lateral cross-sectional view of the structure of Fig. 12 following removal of the organic planarization layer and the nanosheet sacrificial material according to an embodiment of the invention. Fig. 14 shows a side cross-sectional view of the structure of Fig. 13 following formation of gate Structures according to an embodiment of the invention. DETAILED DESCRIPTION

[0009] Herein, illustrative embodiments of the invention may be described in connection with illustrative methods for a Performing self-aligned gate isolation with both symmetric and asymmetric notch Arrangements are described.

[0010] A FET is a transistor that has a source, a gate and a drain and the has an effect that depends on the flow of majority charge carriers along a channel located at the Gate passes between the source and the drain. A current through the channel between the source and the drain can be controlled by a transverse electric field under the gate. The length of the gate determines how how fast the FET switches, and can be about the same length as the length of the channel (such as the Distance between the source and drain).

[0011] For some FETs, arrangements with more than one gate or multi-gate arrangements can be used to control the channel. Multi-gate FETs are promising candidates for downscaling in complementary metal oxide semiconductor (CMOS) FET technology. The smaller dimensions that are possible with multi-gate FETs (compared to single gate FETs) require better control over aspects of performance, such as short-channel effects, punch-through, leakage currents of metal-oxide semiconductors (MOS) and the parasitic resistance present in a multi-gate FET.

[0012] Various techniques can be used to reduce the dimensions of FETs. One technique is by using fin-shaped channels in FinFET devices. Before the introduction of FinFET devices, CMOS devices are typically substantially planar along the surface of the semiconductor substrate except for the FET gates, which were arranged above the top of the channel. FinFETs use a vertical channel structure, with the surface area of ​​the channel exposed towards the gate Thus, the gate in FinFET structures can control the channel more effectively, since the gate extends over more than the one side or surface of the channel. In some FinFET devices, the gate encloses three surfaces of the three-dimensional channel, rather than just being located above the upper surface of a conventional planar channel.

[0013] Another technique useful for reducing the size of FETs is through the use of stacked nanosheet channels formed over a semiconductor substrate. In the case of stacked nanosheets, These are two-dimensional nanostructures, such as sheets with a thickness range in the Size range from 1 nanometer to 100 nanometers (nm). Nanosheets and nanowires are viable options for scaling to 7 nm and beyond. A general process flow for the formation of a nanosheet stack is associated with the removal of sacrificial layers, which may be formed from silicon germanium (SiGe), between Sheets made of a channel material that can be made of silicon (Si).

[0014] When the cell height is scaled, techniques for performing gate cuts do not meet the Requirements when the distance between active areas is too small. A process referred to as a self-aligned gate notch or self-aligned gate insulation is referred to, this can used to scale the active-active distance to 5 nm and beyond. SAGE-induced gate cuts However, they are not ideal in certain situations that require the use of asymmetric gate notches For example, in static random access memory (SRAM) units, asymmetric Gate cuts are used.

[0015] Fig. 1A shows a top-down view 100 of an aligned gate notch 101 formed between two of a set of fins 102 on one of two gate structures 104. The aligned gate notch 101 represents an ideal case in which the gate notch 101 between the adjacent fins 104 is perfectly aligned and has a small critical dimension 103 (e.g., in a range of 6 nm to 15 nm). Fig. 1b represents a top-down view 150 of a misaligned gate notch 110 located between two of a set of fins 102 is implemented on one of two gate structures 104. As shown, the gate Notch 110 is not perfectly aligned in that it is closer to one of the two adjacent fins 102 than the other. The incorrectly aligned gate notch 110 also has a larger critical Dimension 130 (e.g. in a range of 15 nm to 40 nm).

[0016] For scaling to 5 nm and beyond, the cell height is 105, which is twice the pitch of the gate notch 101 to the fin 104 plus the critical dimension 103 of the gate notch 101 with tolerances for fluctuations, is approximately equal to 40 nm. The distance from the gate notch 101 to the fin 104 should not pinched off, with the required distance being equal to twice the thickness of the gate stack, which is a gate Dielectric with a high k and a gate conductor made of a work function metal (WFM) (e.g. 2 × (2 + 5) = 14 nm). Furthermore, parameters relating to the uniformity of the critical Dimension of the fin (CDU, Critical Dimension Uniformity), a walking of the distance (PW, Pitch Walking) of the fins, a CDU of the gate notch as well as an overlay of gate notches that are believed to be closely monitored a total variation of only 5 nm. The CD of the gate cut 101 should therefore be approximately 40 nm - (2 × 14 nm) - 5 nm = 7 nm, although this cannot be achieved using a conventional lithography process flow can be.

[0017] As noted above, for future scaling of cell height, techniques for a self-aligned gate cut or self-aligned gate insulation. A process flow for a self-aligned gate notch may have a structuring of the fins (e.g. fins and other Layers that include a passivation layer, a polysilicon layer, and a hard mask layer). Next A dielectric for a coating can be formed, followed by the formation of an area for a flat Trench isolation (STI, Shallow Trench Isolation). The STI area can then be deepened (e.g. exposing fins followed by the formation of a dummy gate dielectric. After that, a spacer (e.g. made of Polysilicon) which, depending on the distance between the fins, either merges into one another or is independent. An insulation plug is then formed. After that, the dummy gate is created using a gate hard mask and structured by techniques such as self-aligned double structuring (SADP, Self-Aligned Double Patterning). Then an anisotropic etching is carried out, whereby the anisotropic etching is selective with respect to the Insulation plug, dummy gate dielectric and gate hard mask. In this way, symmetrical gate incisions are made.

[0018] However, a process flow for a self-aligned gate cut is suitable for forming asymmetric gate cuts that are necessary in some application scenarios. As noted above, it is For example, it is possible that SRAM structures use asymmetric gate notches. An SRAM is a type of storage unit that offers high speed, low power consumption and easy operation Unlike dynamic random access memory (DRAM), SRAM does not require regular Updating stored data and has a simple design. SRAM cells can be updated using a varying number of transistors.

[0019] The six-transistor (6T) SRAM cell is often used as a primary memory in microprocessor circuits used. A 6T SRAM cell may include a first n-type FET (nFET) device connected to a first bit line node (BL) connected to the transistor, have a first output node (Q) and a word line node (WL). A second nFET unit the 6T SRAM cell is connected to the Q node, a ground node (e.g. VSS) and a second output node (Q') A first p-type FET unit (pFET) is connected to the Q node, the Q' node and a voltage source or a supply node (e.g. VDD). A second pFET unit is connected to the VDD node, the Q node and the Q' node. A third nFET unit is connected to the VSS node, the Q node and the Q' node A fourth nFET unit is connected to a second bit line node (BLB), the WL node and the Q' node The first and fourth nFET units are pass-gate (PG) transistors of the 6T SRAM cell, The second and third nFET units are the pull-down (PD) transistors of the 6T SRAM cell, and The first and second pFET units are the pull-up (PU) transistors of the 6T SRAM cell.

[0020] Fig. 2 shows a top-down view 200 of asymmetric gate cuts 209-1 and 209-2 for a SRAM cell. In the view 200 from top to bottom, an element 201 shows VSS connections (e.g., a 0-volt (V) connection or a ´´ground´´ voltage connection), while an element 203 shows VDD connections (e.g. a connection to a positive supply voltage). Elements 205-1 and 205-2 show WL connections of the SRAM cell, and elements 207-1 and 207-2 show bit line connections (e.g. BL and BLB, respectively) of the SRAM cell. Elements 209-1 and 209-2 represent the asymmetric gate notches located closer to one of two adjacent Fins are arranged instead of being formed symmetrically between two adjacent fins.

[0021] The following is an illustrative process for performing self-aligned gate isolation with both symmetrical and asymmetrical incision arrangements with reference to Figures 3 to 14 in more detail described.

[0022] Fig. 3A shows a side cross-sectional view 300 of a semiconductor structure after patterning of Nanosheet stacking over a substrate 302. A set of fins 304-1 to 304-5 (together fins 304) is stacked over the Substrate 302. The set of fins 304 is surrounded by an STI region 306. The nanosheet stacks, which alternating layers 308 and 310 of a sacrificial material and a channel material are disposed over each of the Fins 304 are formed. While Fig. 3A shows an example in which each nanosheet stack contains three sacrificial layers 308 and three channel layers 310, it should be noted that this is only an example and that the nanosheet stacks comprise more or less than three sets of alternating layers of the sacrificial material and the channel material.

[0023] The substrate 302 may be a semiconductor structure formed from bulk silicon (Si), although other suitable materials may be used, such as various silicon-containing Materials. Illustrative examples of silicon-containing materials suitable for the substrate 302 include but not limited to, Si, silicon germanium (SiGe), silicon germanium carbide (SiGeC), silicon carbide (SiC), Polysilicon, epitaxial silicon, amorphous silicon and multi-layers of the same. Although the wafer Manufacturing silicon is the predominantly used semiconductor material, alternative semiconductor materials can be used such as, but not limited to, germanium (Ge), gallium arsenide (GaAs), gallium nitride (GaN), Cadmium telluride (CdTe) and zinc selenide (ZnSe). In an alternative embodiment, the substrate 302 may be be a silicon-on-insulator (SOI) wafer. As is known in the art, an SOI wafer has an SOI layer separated from a substrate by a buried insulator. Suitable substrate materials include but are not limited to, Si, strained Si, silicon carbide (SiC), Ge, SiGe, SiGeC, Si alloys, Ge alloys, GaAs, indium arsenide (InAs), indium phosphide (InP), or any combination thereof. Suitable dielectric Materials for the buried insulator include, but are not limited to, an oxide material such as Silicon dioxide (SiO ). If the engraved 2 Since the buried insulator is an oxide, the buried insulator is also referred to as a buried oxide or BOX taken.

[0024] The substrate 302 may have a width or horizontal thickness (in the X-X' direction) as desired varies (e.g. based on the number of fins 304 or other structures of units to be formed). The substrate 302 may have a height or vertical thickness (in the Y-Y' direction) in a range of 300 micrometers (µm) to 1000 µm have.

[0025] The fins 304 may be formed from the same material as the underlying substrate 302. In some In some embodiments, the fins 304 are formed, for example, from a bulk substrate using lithography and Etching (e.g. using reactive ion etching (RIE)). Other suitable techniques, such as Sidewall image transfer (SIT), self-aligned double patterning (SADP), self-aligned multiple Structuring (SAMP), self-aligned quadruple structuring (SAQP), etc., can be used to form the fins 304 In such cases, the fins 304 may be formed from the same material as the substrate 302 (e.g., Si). Alternatively, the fins 304 may be formed from a different material than that of the substrate 302 by first, another material is grown epitaxially on the substrate 302 and then structured to form the fins 304. The fins can be, for example, silicon germanium (SiGe), while the substrate 302 is made of Si can be formed.

[0026] Each of the fins 304 may have a vertical thickness or height (in the Y-Y' direction) in a range of 20 nm to 35 nm and have a horizontal thickness or width (in the X-X' direction) varying in a range from 6 nm to 100 nm. As shown in Fig. 3A, different fins of the fins 304 have different widths (e.g., the fins 304-1, 304- 2 and 304-3 in the direction XX' wider than the fins 304-4 and 304-5). The distance between the fins 304 can also vary, as described in more detail below.

[0027] The STI layer 306 may be formed from a dielectric material, such as silicon oxide (SiO ), silicon nitride (SiN), silicon oxycarbide (SiOC), silicon oxynitride (SiON) or any other suitable x dielectric material. The vertical thickness or height (in the Y-Y' direction) of the STI layer 306 is determined by a fin- Disclosure process flow defined and approximately matches the level of the bottom surface of the nanosheet stack The horizontal thickness or width (in the X-X' direction) of the STI layer 306 is determined by the distance between the Fins 304 defined as shown.

[0028] As noted above, the nanosheet stack comprises alternating layers of a sacrificial material 308 and a channel material 310. The sacrificial layers 308 may be formed from any suitable material that can be etched selectively with respect to the channel material 310. If the channel material 310 is Si, the sacrificial layers 308 may be formed of SiGe. If the channel material 310 is indium gallium arsenide (InGaAs), the sacrificial layers 308 may be formed from indium aluminum arsenide (InAlAs). Various other combinations of III-V materials can be used. The material of the sacrificial layers 308 is one that can be selectively removed with respect to the material of the channel layers 310. The Sacrificial layers 308 and the channel layers 310 may each have a thickness in a range of 4 nm to 15 nm. The nanosheet stack of the sacrificial layers 308 and the channel layers 310 can be epitaxially grown over the fins 304 be raised.

[0029] Fig. 3A shows two regions of nanosheet stacks, designated 301 and 303, which are arranged over a common Substrate 302. Region 301 is referred to herein as a ´´logical´´ region, and the fins 304-1 and 304-2 can provide nFET or pFET devices, as for logic devices of a resulting structure desired. The area 303 is referred to herein as an ´´SRAM´´ area in which the fins 304-3, 304-4 and 304-5 provide nFET and pFET devices to form SRAM cells (such as those shown in view 200 of top to bottom of Fig. 2). In some embodiments, the fin 304-3 provides nFET devices, while Fins 304-4 and 304-5 provide pFET devices. The distance between the fins, designated as element 305 in Fig. 3A, Fin 304-3, which provides the nFET unit, and Fin 304-4, which provides the pFET unit, can be equal to about 40 nm The width of fin 304-4, designated as element 307 in Fig. 3A, may be approximately 15 nm. The width of fin 304-4, designated as element 307 in Fig. 3A, The distance between the fins 304-4 and 304-5, which provide the pFET units, referred to as element 309, can be approximately 30 nm.

[0030] Fig. 3B shows a top-down view 350 of the region 303 of a resulting SRAM cell consisting of the structure shown in the side cross-sectional view 300 of Fig. 3A. The side cross-sectional view 300 of Fig. 3A (as well as the side cross-sectional views of Figs. 4, 5A and 6 to 14) is transverse or perpendicular to the Fins 304 shown.

[0031] Fig. 4 shows a side cross-sectional view 400 of the structure of Fig. 3A following a formation of a channel protection coating, a dummy gate 314 and a gate hard mask 316. The channel protection coating 312 is formed, as shown, over the STI region 306 and surrounds the nanosheet stacks. The channel protection coating 312, which may also be referred to as a dummy gate oxide layer 312, may have a uniform thickness in a range of 2 nm to 5 nm. The channel protection coating 312 can be formed using atomic layer deposition (ALD) or using other suitable techniques. Channel protection layer 312 may be formed from an oxide, such as silicon dioxide (SiO). 2

[0032] The dummy gate 314 is formed over the channel protection coating 312, filling the spaces between the nanosheet stacks and overfills the structure. The dummy gate 314 may have a height or vertical thickness (in the direction Y-Y'), as measured from the channel protection coating 312 formed over the STI region 306, in a range of 60 nm to 200 nm. The dummy gate 314 can be made of amorphous silicon (a-Si) or a other suitable material, such as amorphous silicon germanium (a-SiGe), polysilicon (Poly-Si), Poly-Silicon Germanium (Poly-SiGe), etc. The dummy gate 314 can be fabricated using ALD, chemical Chemical vapor deposition (CVD), physical vapor deposition (PVD) or using another appropriate process flow.

[0033] The gate hard mask 316 is patterned over the top of the dummy gate 314 (e.g., in areas where Gates for the resulting structures are formed). The gate hard mask 316 can be formed using CVD, PVD or using another suitable process flow. The gate hard mask 316 may be made of SiO , 2 SiN, combinations thereof, etc. The gate hard mask 316 may have a height or vertical thickness (in the direction Y-Y') in a range of 20 nm to 120 nm.

[0034] Fig. 5A shows a first side cross-sectional view 500 of the structure of Fig. 4 following formation of Source / drain regions 318 and planarization. Fig. 5B shows a second side cross-sectional view 550 of the Structure of Fig. 4 following formation of the source / drain regions 318. Fig. 5B also shows a first Spacer 320 formed between the sacrificial layers 308 and the source / drain regions 318, and a second spacer 322 disposed between the dummy gate 314 and an interlayer dielectric (ILD) 316 As noted above, the side cross-sectional view 500 of Fig. 5A is transverse or perpendicular to the fins 304. The side cross-sectional view 550 of Fig. 5B is along or parallel to one of the fins 304 shown.

[0035] The source / drain regions 318 may be formed using an epitaxial growth process In some embodiments, the epitaxial growth process includes in-situ doping (Dopants are incorporated into the epitaxial material during epitaxy.) Epitaxial materials are made from gaseous or liquid precursors. Epitaxial materials can be grown using Gas phase epitaxy (VPE), molecular beam epitaxy (MBE), liquid phase epitaxy (LPE), using a fast thermal chemical vapor deposition (RTCVD), a metal-organic chemical vapor deposition (MOCVD), ultra-high vacuum chemical vapor deposition (UHVCVD), chemical Low pressure chemical vapor deposition (LPCVD), a limited reaction CVD process (LRPCVD) or grown using other suitable processes. Epitaxial silicon, silicon germanium (SiGe), germanium (Ge) and / or carbon-doped silicon (Si:C) can be deposited during deposition (in-situ Doping) depending on the type of transistor by adding dopants, such as for example, n-type dopants (e.g. phosphorus (P), arsenic (As), antimony (Sb) etc.) or p-type dopants Type (e.g. boron (B), boron fluoride (BF ), gallium (Ga), indium (In), thallium (TI) etc.). The dopant concentration in the source 2 19 - 3 21 -3 20 -3 / the drain can be in a range of 1 × 10 cm to 3 × 10 cm or preferably between 2 × 10 cm and 3 × 10 21 - 3 cm.

[0036] The spacer 322 may be formed by depositing a conformal spacer coating followed by a anisotropic RIE of the spacer. The spacer 320 can be formed by deepening the nanosheet stack followed by forming a selective notch in the sacrificial layers 308 of the nanosheet stack (where, for example, the sacrificial layers 308 may be formed from SiGe and the channel layers 310 may be formed from Si, as noted above). The spacer material for the spacer 320 can then be inserted into the notches with a conformal spacer coating, the spacer coating being applied elsewhere using an isotropic etching process. The spacer 320 and the spacer 322 can each be made of SiN, Silicon oxycarbonitride (SiOCN), silicon oxycarbide (SiOC), SiC, silicon boron carbide nitride (SiBCN), etc.

[0037] Fig. 6 shows a side cross-sectional view 600 of the structure of Fig. 5A following removal of the dummy Gates 314. The dummy gate 314 can be removed using a selective wet or dry etching process such as cleaning with hot ammonia. The removal of the dummy gate 314 sets the Sewer protection cover 312 free.

[0038] Fig. 7 shows a side cross-sectional view 700 of the structure of Fig. 6 following structuring of the Channel protection coating 312 using a dummy oxide mask layer 324. The dummy oxide mask layer 324 is structured over a portion of the fin 304-4 that is opposite to the fin 304-3 (e.g., the dummy oxide protects Mask layer 324 in an SRAM device, the side of the SRAM pFET opposite the nFET formed using of the fin 304-3). The dummy oxide mask layer 324 may be formed using lithography and etching or using other suitable techniques.

[0039] The dummy oxide mask layer 324 may be made of an organic planarization layer (OPL) material such as polyacrylate resin, epoxy resin, phenol resin, polyamide resin, polyimide resin, not saturated polyester resin, polyphenylene ether resin, polyphenylene sulfide resin, benzocyclobutene (BCB) etc. The dummy oxide Mask layer 324 may be deposited using spin-on coating or other suitable process The dummy oxide mask layer 324 may have a height or vertical thickness (in the Y-Y' direction) as measured from a top side of the channel protection coating 312 formed over the STI region 306, in a range of 60 nm to 200 nm. The width or horizontal thickness (in the X-X' direction) of the EG- Mask layer 324 may vary, such as based on the width of the fin 304-4 and the distance between the fins 304-3 and 304-4. As shown in Fig. 7, the dummy oxide mask layer 324 extends from a center of a Top of the nanosheet stack above the fin 304-4 to a center of the STI region 306 between the fins 304-3 and 304-4.

[0040] After structuring the dummy oxide mask layer 324, the channel protection coating 312, which is formed by the structured dummy oxide mask layer 324 is exposed, for example using an isotropic oxide dry etching process.

[0041] Fig. 8 shows a side cross-sectional view 800 of the structure of Fig. 7 following removal of the structured dummy oxide mask layer 324 (e.g. using ashing) and following a selective epitaxial growth of the material 326 (e.g., SiGe) of the sacrificial layers 308 of the nanosheet stacks. As shown, the material 326 is grown over exposed surfaces of the nanosheet stacks that are not in contact with the remaining channel protection coating 312. The epitaxial growth of the material 326 can have a uniform thickness in a range from 5 nm to 30 nm.

[0042] Fig. 9 shows a side cross-sectional view 900 of the structure of Fig. 8 following formation of a self-aligned insulation layer 328. The self-aligned insulation layer 320 may be made of a dielectric material such as SiO , SiN, SiOCN, SiOC, SiC, SiBCN etc. The self-aligned 2 Insulation layer 328 can be formed by depositing the dielectric material into the gaps followed by a Etching back the level of the upper surface of the material 326 disclosed as above The insulation layer 328 is self-aligned when it fills the gaps between the material 326 over the STI area 306 and the remaining channel protection coating 312.

[0043] Fig. 10 shows a side cross-sectional view 1000 of the structure of Fig. 9 following formation of an OPL 330 over the top of the self-aligned insulation layer 328 and the material 326. The OPL 330 can be Using a spin-on coating, using materials similar to those used described above with respect to the dummy oxide mask layer 324. The OPL 330 may have a height or vertical thickness (in the Y-Y' direction) in a range of 20 nm to 100 nm.

[0044] Fig. 11 shows a side cross-sectional view 1100 of the structure of Fig. 10 following structuring of gate notches in the OPL 330. More specifically, Fig. 11 shows a symmetrical gate notch 1101 formed in the OPL 330 in the logic area 301, and an asymmetric gate notch 1103 formed in the OPL 330 in the SRAM region 303. The symmetrical gate notch 1101 and the asymmetrical gate notch 1103 can be formed by patterning a mask over the OPL 330 and etching the exposed portion of the OPL 330 formed so that portions of the underlying self-aligned insulation layer 328 are exposed. The symmetrical gate notch 1101 and the asymmetrical gate notch 1103 can be formed using lithography. The asymmetric gate cut 1103 defines parts of the self-aligned insulation layer 328. The insulation layer 328 is self-aligned, and thus the asymmetric gate notch 1103 can therefore be considered self-aligned. As noted elsewhere herein, In some embodiments, the asymmetric gate cutout 1103 may be located between the fin 304-3, which is an SRAM nFET unit, and the fin 304-4, which provides an SRAM pFET unit. The sub-area of ​​the self-aligned insulation layer 328, which is exposed through the asymmetric gate cut 1103, is located near in the nanosheet stack above the fin 304-4, and thus the asymmetric gate cut 1103 can be considered as a self-aligned asymmetric gate notch.

[0045] The symmetrical gate cut 1101 exposes the self-aligned insulation layer 328, which is located between the fins 304-1 and 304-2 in the logic area 301. The symmetrical gate notch 1101 may have a width or horizontal thickness (in the X-X' direction) in a range of 15 nm to 35 nm.

[0046] The asymmetric gate notch 1103 defines at least a portion of the self-aligned insulation layer 328, which is formed over the remaining channel protection coating 312, as shown. The asymmetric gate Notch 1103 may have a width or horizontal thickness (in the direction X-X') in a range of 15 nm to 35 nm have.

[0047] Fig. 12 shows a side cross-sectional view 1200 of the structure of Fig. 11 following filling of the symmetrical gate cut 1101 and the asymmetrical gate cut 1103 with a dielectric material 332. The dielectric material 332 may comprise SiN, SiCO, SiC, or another suitable material.

[0048] Fig. 13 shows a side cross-sectional view 1300 of the structure of Fig. 12 following removal of the OPL 330 and the sacrificial material (e.g., the sacrificial nanosheets 308 and the material 326). The OPL 330 can be The sacrificial material (e.g. 308 and 326) is removed using an ashing process. selective etching process.

[0049] Fig. 14 shows a side cross-sectional view 1400 of the structure of Fig. 13 following formation of Gate structures 334 (e.g., using a replacement metal gate (RMG) process). The gate structures 334 may have a gate dielectric layer that is conformally deposited, followed by formation of a gate Conductor layer.

[0050] The gate dielectric layer may be formed from a high-k dielectric material. Examples for high k materials include, but are not limited to, metal oxides such as hafnium oxide (HfO ), hafnium silicon oxide (Hf-Si-O), hafnium silicon oxynitride (HfSiON), lanthanum oxide (La O ), lanthanum aluminum oxide 2 2 3 (LaAlO), zirconium oxide (ZrO), zirconium silicon oxide, zirconium silicon oxynitride, tantalum oxide (TaO), titanium oxide (TiO), 3 2 2 5 2 Barium strontium titanium oxide, barium titanium oxide, strontium titanium oxide, yttrium oxide (YO), aluminum oxide (AlO), 2 3 2 3 Lead scandium tantalum oxide and lead zinc niobate. The high-k material can also contain dopants such as for example, lanthanum (La), aluminum (Al), and magnesium (Mg). The gate dielectric layer can have a uniform Thickness in a range of 1 nm to 4 nm.

[0051] The gate conductor layer may comprise a metal gate or a work function metal (WFM). In some Embodiments, the gate conductor layer is formed using atomic layer deposition (ALD) or using another suitable process. For nFET devices, the WFM for the gate Conductor layer around titanium (Ti), aluminum (Al), titanium aluminum (TiAl), titanium aluminum carbon (TiAlC), a combination of Ti and Al alloys, a stack containing a barrier layer (e.g. made of titanium nitride (TiN) or another suitable material) followed by one or more of the aforementioned WFM materials, etc. In the case of pFET Units, the WFM for the gate conductor can be TiN, tantalum nitride (TaN) or another suitable material In some embodiments, the pFET WFM may include a metal stack in which a thicker Barrier layer (e.g. TiN, TaN etc.) is formed, followed by a WFM, such as Ti, Al, TiAl, TiAlC or any combination of Ti and Al alloys. It should be noted that for the gate conductor layer Various other materials can be used if desired.

[0052] The process sequence described above with reference to Figures 3 to 14 advantageously enables the formation of a structure (e.g. an integrated circuit) with both symmetric and asymmetric self-aligned gate insulations. For the gate cut area, an additional gate cut structure is the self-aligned gate insulations. For asymmetric self-aligned gate insulations, a part of the upper portion of the insulation structure over the top of a nanosheet stack.

[0053] The process for forming the self-aligned gate insulation comprises: forming a channel protection coating (e.g., the Dummy oxide layer 312) and using a mask (e.g., dummy oxide mask 322) to cover at least a portion of the channel protective coating, and removing the unprotected coating to protect the channel of the nanosheet stack A sacrificial coating (e.g., material 326) is formed over the exposed channel of the nanosheet stacks, followed by the formation of a self-aligned gate insulation (e.g. the self-aligned gate insulation layer 328). A sacrificial material (e.g. OPL 330) is deposited over the self-aligned gate insulation and the sacrificial coating formed, followed by the formation of gate notches (e.g. the symmetrical gate notch 1101 and the asymmetric gate cut 1103) in the sacrificial material. The sacrificial material and the sacrificial coating are then removed, followed by an RMG process flow to form the gate structures.

[0054] In some embodiments, a method of forming a semiconductor structure comprises: forming a plurality of fins over an upper surface of a substrate, forming an STI region over the upper surface of the substrate, surrounding the plurality of fins, and forming a plurality of nanosheet stacks of a channel material over the A plurality of fins, wherein the plurality of nanosheet stacks provide channels for one or more nanosheet FETs. The method further comprises: forming a channel protection coating over at least a portion of side walls and a top surface of a first of the plurality of nanosheet stacks disposed over a first of the plurality of Fins, wherein the channel protection coating is further formed over a portion of the STI region which extending from the portion of the side walls of the first nanosheet stack toward a second of the plurality of nanosheet stacks formed over a second of the plurality of fins. The method comprises Further comprising: forming a plurality of gate stacks surrounding portions of the plurality of nanosheet stacks, the exposed through the channel protection coating, forming at least one asymmetric self-aligned gate insulation Structure over the channel protection coating and forming at least one symmetrical self-aligned gate insulation Structure over a portion of the STI area between a third of the plurality of fins and a fourth of the Plural of fins.

[0055] The asymmetric self-aligned gate insulation structure formed over the channel protection overcoat may have a channel protection coating formed adjacent to the channel protection coating surrounding side walls of the first nanosheet stack first portion and one over an upper surface of the channel protection coating, which covers the portion of the upper surface of the first nanosheet stack, formed second partial region.

[0056] The first nanosheet stack and the second nanosheet stack represent nanosheet channels for nanosheet FETs of at least one structure of an SRAM device. The first nanosheet stack can form nanosheet channels for a pFET and the second nanosheet stack provides nanosheet channels for an nFET. A third of the plurality of Nanosheet stacks formed over the third fin, and a fourth of the plurality of nanosheet stacks formed over the fourth fin, nanosheet channels for nanosheet FETs can be formed by one or more structures logical units.

[0057] Forming the channel protection coating may comprise: forming the channel protection coating, the plurality of nanosheet Stacking surrounding and over the STI region between the plurality of fins, forming a dummy gate structure over the Channel protection overlay, patterning a gate hard mask over the dummy gate structure and removing partial areas of the dummy gate structure exposed through the patterned gate hard mask. Forming the channel protection overcoat can further comprising: forming source / drain regions in spaces created by the removal of the dummy Gate structure were formed, and removing remaining areas of the dummy gate structure. Forming the Channel protection coating may further comprise: structuring a mask layer over portions of the Channel protection coating surrounding the portion of the side walls and the upper surface of the first nanosheet stack and the portion of the STI region that is separated from the portion of the side walls of the first nanosheet in direction to the second nanosheet stack, and removing portions of the channel protection coating that are the structured mask layer is exposed.

[0058] Forming the plurality of nanosheet stacks may comprise: forming alternating layers of a sacrificial material and the channel material, and the method may further comprise: selectively growing a additional sacrificial material over portions of the majority of nanosheet stacks formed by the channel protection coating The formation of the asymmetric self-aligned gate insulation structure and the symmetric self-aligned gate structure may comprise: forming an insulating material over the structure that contains the additional sacrificial material. Forming the asymmetric self-aligned gate insulation structure and The symmetrical self-aligned gate structure may further comprise: forming an OPL over the Insulation material and the additional sacrificial material. Forming the asymmetric self-aligned gate Isolation structure and the symmetrical self-aligned gate structure may further comprise: Structuring the OPL to (i) protect at least a portion of the insulation material formed over the duct protection coating for the asymmetric self-aligned gate insulation structure and (ii) at least a portion of the above the STI region insulation material formed between the third and fourth nanosheet stack for the symmetric self-aligned gate insulation structure. Forming the asymmetric self-aligned gate Isolation structure and the symmetrical self-aligned gate structure may further comprise: filling a additional insulation material in areas exposed by structuring the OPL.

[0059] Forming the plurality of gate stacks comprises: removing the OPL, the sacrificial material of the nanosheet stacks and the additional sacrificial material. Forming the plurality of gate stacks may further comprise: forming a Gate dielectric and a gate conductor in the spaces created by the removal of the OPL, the sacrificial material the nanosheet channel stack and the additional sacrificial material.

[0060] In some embodiments, a semiconductor structure comprises: a substrate, a plurality of fins disposed over a upper surface of the substrate, an STI region which is arranged above the upper surface of the substrate a plurality of fins, and a plurality of nanosheet stacks made of a channel material, which are arranged above the plurality of fins, wherein the plurality of nanosheet stacks form channels for one or more Nanosheet FETs. The semiconductor structure also comprises: a channel protection coating which extends over at least a portion of sidewalls and an upper surface of a first of the plurality of nanosheet stacks disposed over a first of the plurality of fins, wherein the channel protection coating further comprises is arranged over a portion of the STI area which is different from the portion of the side walls of the first nanosheet stack toward a second of the plurality of nanosheet stacks that extends over a second of the A plurality of fins is arranged. The semiconductor structure further comprises: a plurality of gate stacks, the Partial regions of the plurality of nanosheet stacks exposed by the channel protection coating, at least one asymmetric self-aligned gate insulation structure arranged over the channel protection overlay, and at least one symmetrical self-aligned gate insulation structure formed over a portion of the STI region arranged between a third of the plurality of fins and a fourth of the plurality of fins.

[0061] The asymmetric self-aligned gate insulation structure disposed over the channel protection overcoat may include a channel protection coating arranged adjacent to the channel protection coating surrounding side walls of the first nanosheet stack. first portion, and one over an upper surface of the channel protection coating, which covers the portion of the upper surface of the first nanosheet stack, arranged second subregion.

[0062] The first nanosheet stack and the second nanosheet stack can form nanosheet channels for nanosheet FETs of at least one structure of an SRAM device. The first nanobody surface stack can provide nanosheet channels for provide a pFET, and the second nanosheet stack provides nanosheet channels for an nFET. A third of the A plurality of nanosheet stacks arranged above the third fin, and a fourth of the plurality of sheet stacks, which is arranged above the fourth fin, nanosheet channels for nanosheet FETs of one or more structures logical units.

[0063] In some embodiments, integrated circuits include nanosheet FET structures that semiconductor structures described above.

[0064] It is understood that the various layers, structures and regions shown in the figures are schematic representations that are not drawn to scale. In addition, one or more several layers, structures and regions of a material commonly used to form semiconductor devices or Semiconductor structures used type may be shown in a given figure for the sake of simplicity of explanation not explicitly shown. This does not imply that any layers, structures and areas not explicitly shown are omitted from the actual semiconductor structures. Especially with regard to semiconductor process steps, It should be emphasized that the descriptions provided herein are not intended to cover all of the process steps that may be required to form a functional integrated semiconductor circuit unit. Rather, are certain process steps that are commonly used in the formation of semiconductor devices, such as Example wet cleaning steps and tempering steps, intentionally not described here for the sake of economy of description.

[0065] Furthermore, the same or similar reference numerals are used throughout the figures to indicate the same or similar features, elements or structures, and thus a detailed explanation of the same or similar features, elements or structures are not repeated for each of the figures. It is understood that the Terms ´´about´´ or ´´substantially´´ as used herein with reference to thicknesses, widths, percentages, areas, etc. used, it is meant that they describe them almost or approximately, but not exactly. The term ´´approximately´´ or ´´substantially´´ as used herein implies, for example, that a small margin of error is present, such as 15%, preferably less than 2% or 1% or less, than the stated amount.

[0066] In the above description, different materials and dimensions are used for different elements are provided. Unless otherwise noted, such materials are provided for illustrative purposes only. Similarly, unless otherwise stated, all dimensions are given as examples.

[0067] Semiconductor devices and methods of forming the same according to the techniques described above may used in different applications, different hardware and / or different electronic systems Suitable hardware and systems for implementing embodiments of the invention may include, but are not limited to, personal computers, communication networks, commercial electronic Systems, portable communication devices (e.g. mobile phones and smartphones), storage devices with solid-state Media, functional circuit structures, etc. For systems and hardware in which the semiconductor units are installed are contemplated embodiments of the invention.

[0068] In some embodiments, the techniques described above are used in conjunction with Semiconductor devices such as complementary metal oxide semiconductors (CMOSs), metal oxide semiconductors Field-effect transistors (MOSFETs) and / or fin field-effect transistors (FinFETs) require or otherwise utilize The semiconductor devices may include CMOS, MOSFET and FinFET devices and / or semiconductor devices, which use CMOS, MOSFET and / or FinFET technology.

[0069] Various structures described above can be implemented in integrated circuits. The resulting integrated circuit chips can be supplied by the manufacturer in raw wafer form (i.e., as a single Wafer containing multiple unpackaged chips) may be sold as a single bare chip or in a packaged form. In the latter case, the chip is in a single-chip package (such as a plastic carrier with leads connected to a motherboard or other higher-level carrier) or mounted in a multi-chip package (such as for example, a ceramic carrier containing either surface interconnections or buried interconnections or both). In any case, the chip is then combined with other chips, discrete Circuit elements and / or other signal processing units as part of either (a) an intermediate product, such as such as a motherboard, or (b) a final product. The final product may be any Product that has integrated circuit chips, in a range of toys and other low-end applications to sophisticated computer products that include a display, keyboard or other input device and a central processor.

Claims

1. A method for forming a semiconductor structure, comprising: Forming a plurality of fins (120; 304) over a top surface of a substrate (302); Forming a shallow trench isolation region (306) over the upper surface of the substrate, the plurality of fins surrounding; Forming a plurality of nanosheet stacks of a channel material over the plurality of fins, wherein the plurality of Nanosheet stacks provide channels (310) for one or more nanosheet field effect transistors; Forming a channel protection coating (312) over at least a portion of side walls and a top surface a first of the plurality of nanosheet stacks formed over a first of the plurality of fins, wherein the Channel protection coating is further formed over a portion of the shallow trench isolation area which extending from the portion of the side walls of the first nanosheet stack toward a second of the plurality of nanosheet stacks formed over a second of the plurality of fins; Forming a plurality of gate stacks (334) surrounding portions of the plurality of nanosheet stacks formed by the channel protection coating is exposed; Forming at least one asymmetric self-aligned gate insulation structure over the Sewer protection cover; and Forming at least one symmetrical self-aligned gate insulation structure over a portion of the Area for shallow trench isolation between and equidistant from a third of the plurality of fins and a fourth of the majority of Fins, wherein the asymmetric self-aligned gate insulation structure formed over the channel protection overcoat has: a channel protection coating formed adjacent to the channel protection coating surrounding side walls of the first nanosheet stack first sub-area; and one over an upper surface of the channel protection coating, which covers the portion of the upper surface of the first Nanosheet stack surrounds, formed second sub-area.

2. The method according to claim 1, wherein the first nanosheet stack and the second nanosheet stack comprise nanosheet channels for Nanosheet field-effect transistors of at least one structure of a static random access memory device provide.

3. The method of claim 2, wherein the first nanosheet stack comprises nanosheet channels for a nanosheet p-type field effect transistor and the second nanosheet stack provides nanosheet channels for a nanosheet n-type field effect transistor.

4. The method of claim 2, wherein a third of the plurality of nanosheet stacks formed over the third fin and a fourth of the plurality of nanosheet stacks formed over the fourth fin has nanosheet channels for Provide nanosheet field-effect transistors from one or more logic unit structures.

5. The method of claim 1, wherein forming the channel protective coating comprises: Forming the channel protection coating surrounding the plurality of nanosheet stacks and over the area for a flat Trench isolation between the majority of fins; forming a dummy gate structure (314) over the channel protection overlay; Patterning a gate hard mask (316) over the dummy gate structure; and Removing portions of the dummy gate structure exposed by the patterned gate hardmask.

6. The method of claim 5, wherein forming the channel protective coating further comprises: Forming source / drain regions (318) in spaces formed by the removal of the dummy gate structure were; and Removing remaining parts of the dummy gate structure.

7. The method of claim 6, wherein forming the channel protective coating further comprises: Structuring a mask layer (234) over portions of the channel protection coating, which mask the portion of the side walls and the upper surface of the first nanosheet stack and the sub-region of the shallow trench isolation region which extends from the partial area of the side walls of the first nanosheet towards the second nanosheet stack extends; and Removing portions of the channel protection coating exposed by the patterned mask layer.

8. The method of claim 7, wherein forming the plurality of nanosheet stacks comprises forming alternating Layers of a sacrificial material (308) and the channel material (310) and further comprising a selective Growing an additional sacrificial material (326) over portions of the plurality of nanosheet stacks, which exposed through the channel protection cover.

9. The method of claim 8, wherein forming the asymmetric self-aligned gate insulation structure and the symmetrical self-aligned gate structure comprising forming an insulating material (328) over the structure, which surrounds the additional sacrificial material.

10. The method of claim 9, wherein forming the asymmetric self-aligned gate insulation structure and the symmetrical self-aligned gate structure further comprising forming an organic planarization layer (330) over the insulation material and the additional sacrificial material.

11. The method of claim 10, wherein forming the asymmetric self-aligned gate insulation structure and the symmetrical self-aligned gate structure furthermore a structuring of the organic planarization layer to (i) at least a portion (1103) of the channel protection coating formed over Insulation material for the asymmetric self-aligned gate insulation structure and (ii) at least a portion (1101) of the insulation material formed over the shallow trench isolation region between the third and the fourth nanosheet stack for the symmetric self-aligned gate insulation structure.

12. The method of claim 11, wherein forming the asymmetric self-aligned gate insulation structure and the symmetrical self-aligned gate structure further comprises filling an additional insulating material (332) in areas that are defined by the structuring of the organic planarization layer was exposed.

13. The method of claim 12, wherein forming the plurality of gate stacks comprises removing the organic Planarization layer, the sacrificial material of the nanosheet channel stacks and the additional sacrificial material.

14. The method of claim 12, wherein forming the plurality of gate stacks further comprises forming a gate dielectric and a gate conductor in the spaces created by the removal of the organic Planarization layer, the sacrificial material of the nanosheet channel stacks and the additional sacrificial material became.

15. Semiconductor structure comprising: a substrate (302); a plurality of fins (120; 304) disposed over a top surface of the substrate; a shallow trench isolation region (306) having a plurality of fins disposed above the upper surface of the substrate is arranged surrounding; a plurality of nanosheet stacks of a channel material arranged over the plurality of fins, wherein the A plurality of nanosheet stacks provide channels (310) for one or more nanosheet field effect transistors; a channel protection cover (312) disposed over at least a portion of side walls and an upper surface a first of the plurality of nanosheet stacks arranged over a first of the plurality of fins wherein the channel protection coating is further provided over a portion of the area for shallow trench isolation which extends from the partial area of the side walls of the first nanosheet stack towards a second the plurality of nanosheet stacks, which is arranged over a second of the plurality of fins; a plurality of gate stacks (334) surrounding portions of the plurality of nanosheet stacks formed by the Channel protection cover exposed; at least one asymmetric self-aligned gate insulation structure arranged over the channel protection coating, and at least one symmetrical self-aligned gate insulation structure arranged over a portion of the region for a shallow trench isolation between and equidistant from a third of the plurality of fins and a fourth of the A plurality of fins is arranged, wherein the asymmetric self-aligned gate insulation structure disposed over the channel protection overcoat comprises: a channel protection coating arranged adjacent to the channel protection coating surrounding side walls of the first nanosheet stack first sub-area; and one over an upper surface of the channel protection coating, which covers the portion of the upper surface of the first Nanosheet stack surrounds, arranged second sub-area.

16. A semiconductor structure according to claim 15, wherein the first nanosheet stack and the second nanosheet stack comprise nanosheet Channels for nanosheet field-effect transistors of at least one structure of a static memory unit with random Provide access.

17. A semiconductor structure according to claim 16, wherein the first nanosheet stack comprises nanosheet channels for a nanosheet p-type field effect transistor and the second nanosheet stack provides nanosheet channels for a nanosheet n-type field effect transistor.

18. The semiconductor structure of claim 17, wherein a third of the plurality of nanosheet stacks disposed over the third fin and a fourth of the plurality of nanosheet stacks, which is arranged above the fourth fin, nanosheet Provide channels for nanosheet field-effect transistors from one or more logic unit structures.

19. Integrated circuit comprising: a nanosheet field-effect transistor structure comprising a semiconductor structure as defined in any one of claims 15 to 18 is claimed.

Citation Information

Patent Citations

  • Finfet with reduced capacitance

    US20140284667A1

  • Method of forming gate of semiconductor device and semiconductor device having same

    US20170330801A1

  • Stacked nanosheets by aspect ratio trapping

    US9425291B1

Cited By

  • Semiconductor device having mixed CMOS architecture and method of manufacturing same

    US12563831B2

  • Semiconductor device having mixed CMOS architecture and method of manufacturing same

    US20240055430A1