Coated steel sheet for hot pressing with excellent impact properties after hot pressing, hot-pressed part
A coated steel sheet with controlled alloy compositions and a zinc or aluminum plating layer improves impact strength and flexibility, overcoming the limitations of high-strength steel sheets in automotive applications.
Patent Information
- Application Number
- DE202019006085
- Authority / Receiving Office
- DE · DE
- Patent Type
- Utility models
- Current Assignee / Owner
- Priority Date
- 2018-12-19
- Filing Date
- 2019-12-19
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2029-12-31
AI Technical Summary
Existing high-strength steel sheets used in automotive parts face challenges with low impact strength properties and poor processability due to high tensile strength, which complicates the production of lightweight vehicles with improved safety.
A coated steel sheet with specific alloy compositions and controlled C, Mn, and Cr ratios in the surface layer, combined with a plating layer of zinc or aluminum, is produced through a controlled heating and rolling process to enhance impact strength and flexibility.
The coated steel sheet achieves excellent impact strength and bending properties, ensuring a bending angle of 60° or more with a tensile strength of 1500 MPa, addressing the limitations of previous technologies.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a coated steel sheet for hot press forming which has excellent impact properties after hot press forming and can be preferably used for automobile parts requiring impact resistance, and to a hot press formed part. [State of the art]
[0002] In recent years, due to the depletion of petroleum resources and strong concern for the environment, regulations for improving the fuel efficiency of automobiles have been tightened. Reducing the thickness of steel sheets used in automobiles can be a method to improve the fuel efficiency of automobiles, but reducing the thickness of steel sheets may cause problems with vehicle safety. Therefore, in this case, improving the strength of steel sheets should be facilitated.
[0003] Therefore, there is a constant demand for high-strength steel sheets, and various types of steel sheets have been developed. However, because these steel sheets have high strength in themselves, their workability is poor. Since the product of strength and elongation tends to be constant for each steel grade, increasing the strength of the steel sheet may result in a decrease in elongation, an index of workability.
[0004] To solve this problem, a hot press forming process was proposed. Hot press forming is a process in which a low-temperature structure, such as martensite, is formed in a steel sheet by forming at a high temperature suitable for forming, followed by quenching the steel sheet at a low temperature to produce the final product. This approach has the advantage of minimizing the processability problem when manufacturing a high-strength component.
[0005] A typical technology for such a hot-press-formed part is Patent Document 1. In Patent Document 1, an Al-Si-coated steel sheet is heated to 850°C or more, hot-rolled, press-formed, and then quenched to form a martensite element structure, thereby achieving ultra-high tensile strength exceeding 1600 MPa. Ensuring such ultra-high tensile strength facilitates the production of lightweight vehicles. However, according to Patent Document 1, the impact resistance properties in the event of an impact are relatively low due to the high strength, and a phenomenon occurs in some cases where abnormally low impact resistance properties occur depending on the hot-press forming conditions, etc.
[0006] Accordingly, Patent Document 2 proposes a technique for improving impact resistance properties after hot press forming by spheroidizing inclusions by adjusting the Ca / S ratio and refining grains by adding an alloying element such as niobium (Nb) to a steel for hot press forming. However, Patent Document 2 refers to the control of inclusions and grain size to improve the impact toughness of general steel materials and is evaluated as difficult to apply as a means for improving the low impact strength that occurs during actual hot press forming in the hot press forming field.
[0007] Therefore, there is a need to develop a clad or coated steel sheet for hot press forming which has excellent impact properties after hot press forming and a hot press formed part. (Patent Document 1) US Patent Publication No. 6296805 (Patent Document 2) Korean Publication No. 10-2010-0047011 [Technical problem]
[0008] One aspect of the present disclosure may provide a plated steel sheet for hot press forming having excellent impact resistance properties after hot press forming and a hot press formed part thereof.
[0009] The technical problem of the present disclosure is not limited to the above points. Additional problems of the present disclosure are described in the overall content of the disclosure, and those with ordinary skill in the art to which the present disclosure relates will have no difficulty understanding the additional problems of the present disclosure from the contents described in the disclosure of the present disclosure. [Technical solution]
[0010] According to one aspect of the present disclosure, a clad or coated steel sheet for hot press forming having excellent impact resistance properties after hot press forming comprises: a base steel sheet having in wt%: 0.15% to 0.4% carbon (C), 0.1% to 1% silicon (Si), 0.6% to 8% manganese (Mn), 0.001% to 0.05% phosphorus (P), 0.0001% to 0.02% sulfur (S), 0.01% to 0.1% aluminum (Al), 0.001% to 0.02% nitrogen (N), 0.01% to 0.5% chromium (Cr), and the balance Fe and other impurities; and an alloy plating layer formed of zinc, aluminum or alloys thereof on a surface of the base steel sheet, wherein a ratio (C S / C B ) of a C content (C S ) of a surface layer part to a C content (C B ) of the base steel sheet is 0.6 or less, and a ratio ((Mn S +Cr S) / (Mn B +Cr B )) of the sum (Mn S +Cr S ) of the contents of Mn and Cr of the surface layer part to the sum (Mn S +Cr S ) of the contents of Mn and Cr of the base steel sheet is 0.8 or more, wherein the surface layer part refers to an area up to a depth of 15 µm from the surface of the base steel sheet excluding the plating layer.
[0011] The base steel sheet may also contain 0.0005 to 0.01 wt% boron (B) and 0.01 to 0.05 wt% titanium (Ti) or more.
[0012] A microstructure of the base steel sheet may contain, based on the area ratio, 40% to 100% ferrite and a residue of 0% to 60% pearlite, bainite or martensite in the surface layer part and 30% to 90% ferrite and a residue of 10% to 70% pearlite, bainite or martensite in a central part thereof.
[0013] According to another aspect of the present disclosure, a hot-press formed member having excellent impact resistance properties comprises: a base steel sheet containing, by weight, 0.15% to 0.4% carbon (C), 0.1% to 1% silicon (Si), 0.6% to 8% manganese (Mn), 0.001% to 0.05% phosphorus (P), 0.0001% to 0.02% sulfur (S), 0.01% to 0.1% aluminum (Al), 0.001% to 0.02% nitrogen (N), 0.01% to 0.5% chromium (Cr), the balance Fe and other impurities; and an alloyed plating layer formed from a zinc- or aluminum-containing alloy on a surface of the base steel sheet, wherein the ratio (C PS / C B ) of the C content (C PS ) of a component surface layer to the C content (C B ) of the base steel sheet is 1.2 or less, and a ratio ((Mn PS +Cr PS ) / (Mn B +Cr B )) of the sum (Mn PS +Cr PS) of the Mn and Cr contents of the component surface layer section to the sum (Mn S +Cr S ) the contents of Mn and Cr of the base steel sheet is 0.8 or more, wherein the component surface layer refers to an area up to a depth of 25 µm from the surface of the base steel sheet excluding the alloy coating layer.
[0014] The coverage of ferrite at a martensitic grain boundary of the surface layer part of the component may be 30% or less.
[0015] According to another aspect of the present disclosure, a method for producing a clad steel sheet for hot press forming having excellent impact resistance properties after hot press forming comprises: preparing a slab having a weight of-% 0.15% to 0.4% carbon (C), 0.1% to 1% silicon (Si), 0.6% to 8% manganese (Mn), 0.001% to 0.05% phosphorus (P), 0.0001% to 0.02% sulfur (S), 0.01% to 0.1% aluminum (Al), 0.001% to 0.02% nitrogen (N), 0.01% to 0.5% chromium (Cr), and the balance Fe and other impurities, and heating the slab to a temperature of 1050°C to 1300°C; hot rolling the heated slab in a hot finishing rolling temperature range of 800°C to 950°C to obtain a hot-rolled steel sheet; Annealing the hot-rolled steel sheet at 450°C to 750°C after the hot finish rolling is completed; annealing the coiled hot-rolled steel sheet by heating at 740°C to 860°C under an atmosphere in which the dew point temperature is -10°C to 30°C for 10 to 600 seconds; and immersing the hot-rolled steel sheet after annealing in a plating bath formed of zinc, aluminum, or their alloys to perform plating.
[0016] The method may further comprise: cold rolling the hot-rolled steel sheet before coiling it after hot rolling to obtain cold-rolled steel sheet.
[0017] The slab may also contain 0.00005 to 0.01 wt% boron (B) and 0.01 to 0.05 wt% titanium (Ti) or more.
[0018] According to another aspect of the present disclosure, a method for producing a hot-press-formed part having excellent impact resistance properties comprises the steps of: heat-treating the clad steel sheet for hot press-forming produced by the above-described method for producing a clad steel sheet for hot press-forming having excellent impact resistance properties after hot press-forming in a temperature range of Ac3 to 950°C for 1 to 15 minutes; and then performing hot press-forming. [Beneficial effects]
[0019] According to the present disclosure, a clad steel sheet for hot press forming which has excellent impact resistance properties after hot press forming can be provided.
[0020] The hot-press-formed part produced by hot-press-forming a clad steel sheet for hot-press forming according to the present disclosure has a bending angle of 60° or more as measured by a VDA238-100 bending test at a tensile strength of 1500 MPa, thereby ensuring excellent impact resistance properties.
[0021] Various and advantageous advantages and effects of the present disclosure are not limited to the above disclosure and will become more readily understood as specific embodiments of the present disclosure progress. [Description of the drawings] Fig.1 is the result of analysis of the concentration of carbon (C), manganese (Mn), and chromium (Cr) in a depth direction of a surface layer part using a GDS before hot press forming for the clad steel sheet for hot press forming of Invention Example 1. Fig. 2 is an optical microscope photograph showing the structure of a surface layer part of a member after hot press molding of Inventive Example 1. Fig. 3 is the result of analysis of the concentration of carbon (C), manganese (Mn), and chromium (Cr) in a depth direction of a surface layer part using a GDS before hot press forming for the clad steel sheet for hot press forming of Comparative Example 1. Fig. 4 is an optical microscope photograph showing the structure of the surface layer part of the element after hot press molding of Comparative Example 3. [Preferred embodiments]
[0022] Embodiments of the present disclosure will be described below. However, the embodiments of the present disclosure may be modified in various other forms, and the scope of the present disclosure is not limited to the embodiments described below. Furthermore, embodiments of the present disclosure are provided to more fully explain the present disclosure to those having ordinary skill in the art.
[0023] The present inventors found that the bending angle of an uncoated material after hot press forming was significantly better than that of a coated material. Further investigations confirmed that decarburization occurred in a surface layer portion of a steel sheet during heating for hot press forming in uncoated materials, resulting in the formation of a soft ferrite layer on the surface layer portion, resulting in excellent bending performance.
[0024] The inventors focused on the idea that the bendability of a hot-press-formed (structural) part can be improved if it is possible to form a soft layer on the surface layer portion of the base steel sheet by reducing the C content of the surface layer portion in clad materials. However, it was found that it is difficult to form a soft ferrite layer like that in uncoated materials in clad materials because decarburization during heating for hot press forming does not occur to a sufficient extent as in uncoated materials. If the ferrite layer is not continuously formed to a sufficient extent, the bendability is likely to be impaired.
[0025] The present inventors further investigated to overcome the problem and completed the present disclosure after confirming that a clad steel sheet for hot press forming having excellent impact-resistant properties after hot press forming and a hot press formed part can be provided by setting a C content in a surface layer part of the base steel sheet to a value below a predetermined level compared to a C content in a center part of the base steel sheet and controlling the sum of the contents of Mn and Cr in the surface layer part of the base steel sheet to a level above a predetermined level compared to the sum of the contents of Mn and Cr in the center part by controlling annealing conditions.
[0026] Hereinafter, a clad steel sheet for hot press forming and a hot press formed (structural) part having excellent impact resistance properties after hot press forming according to one aspect of the present disclosure will first be described in detail.
[0027] Coated steel sheet for hot press forming with excellent impact resistance properties after hot press forming
[0028] A clad steel sheet for hot press forming having excellent impact resistance properties after hot press forming according to one aspect of the present disclosure comprises: a base steel sheet having, by weight, 0.15% to 0.4% carbon (C), 0.1% to 1% silicon (Si), 0.6% to 8% manganese (Mn), 0.001% to 0.05% phosphorus (P), 0.0001% to 0.02% sulfur (S), 0.01% to 0.1% aluminum (Al), 0.001% to 0.02% nitrogen (N), 0.01% to 0.5% chromium (Cr), and the balance Fe and other impurities; and a plating layer formed of zinc, aluminum, or alloys thereof on a surface of the base steel sheet, wherein a ratio (C S / C B ) of a C content (C S ) of a surface layer part to a C content (C B ) of the base steel sheet is 0.6 or less, and a ratio ((Mn S +Cr S ) / (Mn B +Cr B )) of the sum (Mn S +Cr S) of the contents of Mn and Cr of the surface layer part to the sum (Mn B +Cr B ) the contents of Mn and Cr of the base steel sheet is 0.8 or more.
[0029] First, the alloy composition of a base steel sheet according to the present disclosure will be described in detail. In this disclosure, it should be noted that the content of each element refers to weight percentages (wt%) unless otherwise stated. C : 0.15% to 0.4%
[0030] C is an essential element for increasing the strength of a hot-press-formed part. If the C content is less than 0.15%, it may be difficult to achieve sufficient strength. Conversely, if the C content is more than 0.4%, the strength of the hot-rolled material is too high when the hot-rolled material is cold-rolled, so the cold-rolling properties may be significantly worse and weldability may be significantly impaired. Therefore, in the present disclosure, the C content may be limited to 0.15 to 0.4%. Si: 0.1% to 1%
[0031] Si, added as a deoxidizer during steelmaking, is an element for strengthening solid solutions and preventing the occurrence of carbide. Furthermore, Si contributes to increasing the strength of the hot-press-formed part and is an element that ensures material uniformity. If the Si content is less than 0.1%, the above-mentioned effect is insufficient. If the Si content exceeds 1%, the Al coating properties may be significantly deteriorated by a Si oxide formed on the surface of the steel sheet during annealing. Therefore, in the present disclosure, the Si content may be limited to 0.1% to 1%. Mn: 0.6% to 8%
[0032] Mn is an element added to ensure a solid solution strengthening effect and to reduce the critical cooling rate for securing martensite in the hot-press-formed part. To achieve the above-mentioned effect, Mn must be added in an amount of 0.6% or more. However, if the Mn content exceeds 8%, cold rolling properties may be reduced due to increased strength of the steel sheet before hot-press forming, the cost of the ferroalloy may increase, and weldability may be poorer. Therefore, in the present disclosure, the Mn content may be limited to 0.6 to 8%. P: 0.001% to 0.05%
[0033] Phosphorus (P) is present as an impurity in steel, and a lower content is advantageous. Accordingly, in the present disclosure, the P content can be limited to 0.05% or less, and preferably to 0.03% or less. Since a lower P content is advantageous, it is not necessary to set a specific lower limit for the content. However, an excessive reduction in the P content may lead to an increase in manufacturing costs, so the lower limit of the P content can be set to 0.001%. S: 0.0001% to 0.02%
[0034] Sulfur (S) is an impurity in steel and an element that impairs the ductility, impact strength, and weldability of the component, which is why the maximum S content is limited to 0.02% and preferably to 0.01% or less. Furthermore, manufacturing costs may increase if the minimum S content is less than 0.0001%, so a lower limit for the S content can be set at 0.0001%. Al: 0.01% to 0.1%
[0035] Al can increase the purity of the steel by deoxidizing the steel together with Si. 0.01% or more of Al can be added to achieve the above-mentioned effect. However, if the Al content exceeds 0.1%, high-temperature ductility may deteriorate due to excessive AlN formed during the casting process and lead to cracks in the slab, so an upper limit for the content may be set at 0.1% or less. Therefore, in the present disclosure, the Al content is preferably 0.01% to 0.1%. N: 0.001% to 0.02%
[0036] N is an element contained as an impurity in steel. When the N content exceeds 0.02%, high-temperature ductility may deteriorate due to excessive AlN formation during the casting process, leading to slab cracking. Therefore, to reduce the susceptibility to cracking during continuous slab casting and to ensure impact toughness, the N content may be 0.02% or less. A lower limit cannot be explicitly specified, but considering an increase in manufacturing costs, the lower limit of the N content may be set to 0.001% or more. Therefore, within the scope of the present disclosure, the N content is preferably 0.001% to 0.02%. Cr: 0.01% to 0.5%
[0037] Cr is an element added to enhance the solid solution strengthening and hardenability during hot press forming, similar to Mn, and can be added in an amount of 0.01% or more to achieve the above-mentioned effect. However, if the Mn content exceeds 0.5%, hardenability may be sufficiently secured, but the properties may be saturated, and the cost of producing the steel sheet may increase. Therefore, in the present disclosure, the Cr content is preferably 0.01% to 0.5%.
[0038] The base steel sheet of the clad steel sheet for hot press forming according to one aspect of the present disclosure may contain, in addition to the above-mentioned components, one or more of 0.0005% to 0.01% boron (B) and 0.01% to 0.05% titanium (Ti). B: 0.0005% to 0.01%
[0039] B is an element that improves hardenability even with a small addition amount and segregates along the grain boundaries of pre-tenite to suppress embrittlement of the hot-press-formed part due to grain boundary segregation of P and / or S. It can be added in an amount of 0.0005% or more to achieve the above-mentioned effect. However, if the B content exceeds 0.01%, the effect is saturated and embrittlement occurs during hot rolling, so an upper limit of the B content can be set to 0.01%, and preferably the B content can be set to 0.005% or less. Therefore, in the present disclosure, the B content is preferably 0.0005% to 0.01%. Ti: 0.01% to 0.05%
[0040] Ti is added to combine with the nitrogen remaining as an impurity in the steel to produce TiN, thereby maintaining the solid solution B, which is essential for ensuring hardenability. If the Ti content is less than 0.01%, it may be difficult to sufficiently achieve the above-mentioned effect, and if the Ti content is more than 0.05%, the properties may be saturated and the cost of producing the steel sheet may increase. Therefore, in the present disclosure, the Ti content is preferably 0.01% to 0.05%.
[0041] The remainder other than the above-mentioned components is iron (Fe), and the addition of any component is not limited as long as the component can be contained in the hot-press forming steel sheet. Furthermore, in a general manufacturing process, unintentional impurities derived from raw materials or the environment may inevitably be mixed in, which cannot be ruled out. Since these impurities are known to those skilled in the art in the manufacturing process, they are not explicitly mentioned in the present disclosure.
[0042] The clad steel sheet for hot press forming with excellent impact resistance properties after hot press forming according to one aspect of the present disclosure includes a plating layer of zinc, aluminum, or their alloys formed on a surface of the base steel sheet. The plating layer imparts corrosion resistance to the component in a final part and serves to prevent decarburization and scaling of the base steel sheet during heating for hot press forming.
[0043] In the present disclosure, the type of plating layer is not particularly limited, and any plating layer applied to a steel sheet for hot press forming in the related art can be used in the present disclosure without limitation. In one non-limiting embodiment, the plating layer may be made of zinc, aluminum, or their alloys, and specifically, the plating layer may be a hot-dip galvanizing layer, an electrogalvanizing layer, a zinc alloy plating layer, an aluminum plating layer, or an aluminum alloy plating layer.
[0044] According to one aspect of the present disclosure, the plating layer may contain components that may be contained during the manufacturing process within a range that does not impair the purpose of the present disclosure, and in particular, may contain other unavoidable impurities.
[0045] In addition, the coating thickness can range from 5µm to 100µm. If the coating thickness is less than 5µm, it may be difficult to achieve sufficient corrosion resistance in the hot-press-formed part. If the thickness is more than 100µm, the heating time for hot-press forming may be excessively prolonged and the manufacturing cost may increase excessively for the effect of improving corrosion resistance.
[0046] Meanwhile, in the clad steel sheet for hot press forming according to the present disclosure, the ratio (C S / C B) of the C content (C S ) of a surface layer section to a C content (C B ) of the base steel sheet (hereinafter referred to as “ratio (C S / C B )") 0.6 or less. The surface layer area refers to an area from the surface of the base steel sheet without the plating layer to a depth of 15 µm.
[0047] Furthermore, according to one aspect of the present disclosure, in the clad steel sheet for hot press forming, the ratio (C B / C S ) of the C content (C S ) of the surface layer part to the C content (C B ) of the base steel sheet is preferably 0.5 or less, more preferably 0.4 or less, and most preferably 0.35 or less.
[0048] If the ratio (C S / C B) is set to less than 0.6, a relatively soft martensite phase with a low C content can form in the surface layer part, in contrast to a hard martensite phase that forms in the center of the base steel sheet after hot press forming. Since the soft martensite phase forms on the surface layer part of the coated steel sheet, the hardness of the surface layer part decreases, thus ensuring excellent bending properties. When the ratio (C S / C B ) exceeds 0.6, it may be difficult to achieve the effect of improving bendability by softening the surface layer after hot press forming. A lower limit of the ratio (C S / C B) cannot be particularly limited. However, if the C content in the surface layer part is too low, the strength of the element may decrease or the fatigue properties may be worse after hot press forming, so the lower limit of the ratio (C S / C B ) can be set to 0.05 or more, but is not limited to that.
[0049] Furthermore, in the clad steel sheet for hot press forming according to one aspect of the present disclosure, a ratio ((Mn S +Cr S ) / (Mn B +Cr B )) of the sum (Mn S +Cr S ) of the contents of Mn and Cr of the surface layer part to the sum (Mn B +Cr B ) of the Mn and Cr contents of the base steel sheet (hereinafter referred to as “(Ratio (Mn S +Cr S ) / (Mn B +Cr B))") be 0.8 or more. Here, the surface layer proportion refers to a range from the surface of the base steel sheet excluding the plating layer to a depth of 15 µm.
[0050] According to one aspect of the present disclosure, the ratio ((Mn S +Cr S ) / (Mn B +Cr B )) of the sum (Mn S +Cr S ) of the Mn and Cr contents of the surface layer part to the sum (Mn B +Cr B ) of the Mn and Cr contents of the base steel sheet is preferably 0.85 or more, and more preferably 0.87 or more.
[0051] If the ratio ((Mn S +Cr S ) / (Mn B +Cr B)) is less than 0.8, the hardenability of the surface layer part may be insufficient during hot press forming, so that ferrite may be partially formed on a surface of the member. Since ferrite partially formed at the hard martensitic grain boundary significantly deteriorates the bending ability, the ratio ((Mn S +Cr S ) / (Mn B +Cr B )) preferably 0.8 or more. The upper limit of the ratio ((Mn S +Cr S ) / (Mn B +Cr B )) does not need to be limited, but if the contents of Mn and Cr in the surface layer part are too high, the hardness of the surface layer part may increase after hot press forming and tend to deteriorate the flexibility. Therefore, the upper limit of the ratio ((Mn S +Cr S ) / (Mn B +Cr B )) 2 or less, but not limited to.
[0052] The microstructure of the base steel sheet does not need to be particularly limited. However, the microstructure of the surface layer portion of the base steel sheet may contain 40% to 100% ferrite and a remainder of 0% to 60% pearlite, bainite, or martensite. Furthermore, the microstructure of a central portion of the base steel may contain 30% to 90% ferrite and a remainder of 10% to 70% pearlite, bainite, or martensite.
[0053] Hot-press-formed component with excellent impact resistance properties.
[0054] Meanwhile, a hot press formed (structural) part with excellent impact resistance properties can be manufactured by heat treating the coated steel sheet for hot press forming with the above configuration in a temperature range of Ac3 to 950°C for 1 to 15 minutes and then performing hot press forming on it.
[0055] A hot-press formed part having excellent impact resistance properties according to one aspect of the present disclosure comprises a base steel sheet having the same alloy composition as that of the base steel sheet of the coated or clad steel sheet and an alloy plating layer formed of an alloy including zinc or aluminum on a surface of the base steel sheet, wherein a ratio (C PS / C B ) of a C content (C PS ) of a component surface layer part to a C content (C B ) of the base steel sheet is 1.2 or less, and a ratio ((Mn PS +Cr PS ) / (Mn B +Cr B )) of the sum (Mn PS +Cr PS ) of the Mn and Cr contents of the component surface layer portion or the surface layer portion of the component (member surface layer portion) to the sum (Mn B +Cr B) of the Mn and Cr contents of the base steel sheet (hereinafter referred to as “ratio ((Mn-+Cr PS ) / (Mn B +Cr B ))") is 0.8 or more. Here, the part of the surface layer refers to an area from the surface of the base steel sheet excluding the alloy layer to a depth of 25 μm.
[0056] Meanwhile, according to one aspect of the present disclosure, in the hot-press molded part, the ratio (C PS / C B ) of the C content (C PS ) of the surface layer part of the (structural) part to the C content (C B ) of the base steel sheet is preferably 1.1 or less, and more preferably 1.05 or less.
[0057] Furthermore, according to one aspect of the present disclosure, in the hot press-formed part, the ratio ((Mn PS +Cr PS ) / (Mn B +Cr B )) of the sum (Mn PS +Cr PS) of the Mn and Cr content of the component surface layer part to the sum (Mn S +Cr S ) of the Mn and Cr content of the base steel sheet is preferably 0.9 or more, and more preferably 0.93 or more.
[0058] When the clad steel sheet is heated for hot press forming, the thickness of the clad layer generally increases because the clad layer and the base iron are alloyed, and because the clad layer has very low solubility of C, C which has not been dissolved during the alloying process is concentrated in the surface layer part, which increases the C content of the surface layer part, and the high C content of the surface layer part increases the hardness of the surface layer part and deteriorates the bendability.
[0059] In producing a hot-press-formed part by hot-press-forming the coated steel sheet for hot-press-forming according to one aspect of the present disclosure, the ratio (C PS / C B ) of the C content (C PS ) of the surface layer part of the component to the C content (C B ) of the base steel sheet is 1.2 or less, so that an excessive increase in the hardness of the surface layer part of the molded part can be prevented even if C is concentrated in the surface area of the molded part. In addition, since the ratio ((Mn PS +Cr PS ) / (Mn B +Cr B )) of the sum (Mn PS +Cr PS ) of the Mn and Cr contents of the component surface layer part to the sum (Mn B +Cr B) of the contents of Mn and Cr of the base steel sheet is 0.8 or more, the hardenability is sufficient and thus the formation of ferrite can be prevented, so that the coverage rate of ferrite at the martensitic grain boundary in the surface layer part of the component (area occupied by ferrite in the martensitic grain boundary when a cross section is observed) can be 30% or less, and as a result, excellent bendability with sufficient strength can be ensured.
[0060] Since, as described above, the hot press-formed part according to one aspect of the present disclosure has a ratio (C S / C B ) of 1.2 or less and the ratio ((Mn PS +Cr PS ) / (Mn B +Cr B)) of 0.8 or more, the bending angle measured in a VDA238-100 bending test at a tensile strength of 1500 MPa is 60° or more, so excellent impact resistance properties can be ensured. However, as the tensile strength increases, such as when the tensile strength of the hot-press-formed part is 1800 MPa or more, the bending angle criterion for determining excellent impact resistance properties can be lowered.
[0061] Next, an illustrative, unclaimed method for producing a clad steel sheet for hot press forming and a hot press formed part having excellent impact resistance properties after hot press forming will be described in detail.
[0062] Process for producing a clad steel sheet for hot press forming having excellent impact resistance properties after hot press forming
[0063] A method for producing a clad steel sheet for hot press forming having excellent impact resistance properties after hot press forming according to another aspect of the present disclosure comprises heating a slab satisfying the above-mentioned alloy composition to 1050°C to 1300°C; hot finish rolling the heated slab in a temperature range of 800°C to 950°C to obtain a hot-rolled steel sheet; annealing the hot-rolled steel sheet at 450°C to 750°C after completion of the hot finish rolling; annealing the coiled hot-rolled steel sheet by heating to 740°C to 860°C under an atmosphere where the dew point temperature is -10°C to 30°C for 10 to 600 seconds; and immersing the annealed hot-rolled steel sheet in a plating bath formed of zinc, aluminum or their alloys to perform the plating. Step of slab heating
[0064] First, the slab corresponding to the above-mentioned alloy composition is heated to 1050°C to 1300°C (1050-1300°C). If the slab heating temperature is below 1050°C, it may be difficult to homogenize the slab structure, and if the temperature exceeds 1300°C, an excessive oxide layer may form. Hot rolling step
[0065] The heated slab is subjected to final hot rolling at a temperature range of 800°C to 950°C (800~950) to obtain hot-rolled steel sheet. If the final hot rolling temperature is below 800°C, it may be difficult to control the sheet shape because a duplex grain structure occurs in the surface layer of the steel sheet due to rolling in two-phase regions. When the temperature exceeds 950°C, the grains become coarse. Cooling and coiling step
[0066] After the final hot rolling, the hot-rolled steel sheet is coiled at 450°C to 750°C. At a coiling temperature below 450°C, material fluctuations in the width direction increase, leading to strip breakage and shape defects during cold rolling. However, if the coiling temperature exceeds 750°C, the carbides become coarse, resulting in poor bendability. Cold rolling step
[0067] If necessary, an additional step can be performed before annealing to produce cold-rolled steel sheet by cold rolling the coiled hot-rolled steel sheet. Cold rolling allows for more precise control of the thickness of the steel sheet, and annealing and plating can be performed directly without cold rolling. In this case, cold rolling can be performed at a reduction rate of 30% to 80%. Annealing step
[0068] Annealing is performed for 10 to 600 seconds in an atmosphere with a dew point temperature of -10 to 30°C by heating the coiled hot-rolled steel sheet to 740°C to 860°C. At an annealing temperature of less than 740°C or an annealing time of less than 10 seconds, the microstructure may not be sufficiently recrystallized, resulting in a poor sheet shape, or the strength after coating may be too high, which may lead to tool wear during the stamping process. In addition, the diffusion of C during annealing is insufficient, making it difficult to determine the ratio (C S / C B ) of the C content (C S ) of the surface layer part to the C content (C B) of the base steel sheet to 0.6 or less. If the annealing temperature exceeds 860°C or the annealing time exceeds 600 seconds, a large amount of annealing oxide may form on the surface of the steel sheet during annealing, resulting in coating peeling or deterioration of coating adhesion. In addition, Mn, Cr, etc., form in the base steel sheet at an interface between the coating layer and the base steel sheet or at a grain boundary of the base steel sheet, making it difficult to achieve a ratio of 0.8 or more as the ratio ((Mn S +Cr S ) / (Mn B +Cr B )) of the sum (Mn S +Cr S ) of the Mn and Cr contents of the surface layer part to the sum (Mn B +Cr B) of the contents of Mn and Cr of the base steel sheet, resulting in a lack of hardenability of the surface layer part, and accordingly, ferrite may partially form in the surface layer part after hot press forming, which impairs the flexibility.
[0069] In the present disclosure, it is very important to control the dew point temperature of the annealing atmosphere to control the ratio of the C, Mn, and Cr contents in the surface layer portion to the base material component of the base steel sheet. If the dew point temperature of the annealing atmosphere is less than -10°C, the decarburization reaction may be insufficient, and the effect of improving flexibility may be insignificant. Conversely, if the dew point temperature exceeds 30°C, the hardenability of the surface layer portion may decrease due to excessive internal oxidation, leading to partial ferrite formation and deteriorating bendability.
[0070] Furthermore, according to one aspect of the present disclosure, annealing may be performed for 10 to 100 seconds under an atmosphere in which the dew point temperature is 10 to 30°C by heating the coiled hot-rolled steel sheet to 800 to 840°C (800-840°C). Coating step
[0071] After annealing, the annealed hot-rolled steel sheet is immersed in a plating bath of zinc, aluminum, or their alloys to coat it. In the present disclosure, the components of the plating bath used in forming the coating layer are not particularly limited. However, as a non-limiting example, the plating bath used in the present disclosure may be made of zinc, a zinc alloy, aluminum, or an aluminum alloy. Furthermore, the plating conditions can be applied without limitation to the present disclosure, as long as the plating conditions are commonly applied to a hot-pressed steel sheet and are therefore not specifically mentioned in the present disclosure.Furthermore, according to one aspect of the present disclosure, the plating bath may contain other unavoidable impurities, and the zinc alloy and the aluminum alloy may also contain components that are usually contained within a range that does not affect the subject matter of the present disclosure, and in particular, contain other unavoidable impurities.
[0072] Process for producing a hot-press-molded part with excellent impact resistance properties
[0073] A hot-press-formed part with excellent impact resistance properties can be manufactured by hot-press forming the clad steel sheet for hot-press forming produced by the above-described manufacturing method of the present disclosure. The hot-press forming can be performed by a method generally used in the art. However, as a non-limiting example, the clad steel sheet for hot-press forming can be heat-treated in a temperature range of Ac3 to 950°C for 1 to 15 minutes and then pressed to perform the hot-press forming. [Examples of implementation]
[0074] The present disclosure is described in more detail below using examples. However, it should be noted that the following examples are for illustrative purposes only and are not intended to limit the scope of the present disclosure. This is because the scope of the present disclosure is determined by the subject matter described in the claims and the subject matter derived therefrom. (Example)
[0075] First, a slab with the alloy composition shown in Table 1 was prepared, heated, hot-rolled, and coiled under the manufacturing conditions shown in Table 2 to produce a hot-rolled steel sheet. The produced steel sheet was then subjected to Fig. 2 and then immersed in a galvanizing bath, and then the coating was carried out so that the coating amount per side was 70 g / m 2to produce a coated steel sheet. [Table 1] Classification C Si Mn P S Al N Cr Ti B Steel A 0,21 0,25 1,3 0,01 0,002 0,035 0,005 0,22 0,03 0,0022 Steel B 0,2 0,1 2,5 0,009 0,001 0,03 0,004 0,1 - - [Table 2] Classification Steel grade Slab heating temperature (°C) Final temperature during hot rolling (°C) Annealing temperature (°C) Annealing condition Heating temperature (°C) Hold time (sec.) Dew point temperature (°C) IE 1 A 1250 900 560 820 42 15 IE2 B 1200 880 500 800 65 10 CE 1 A 1250 900 560 820 42 -15 CE 2 A 1250 900 560 700 45 10 CE3 B 1200 880 500 800 65 40 CE4 B 1200 880 500 870 620 15 IE*: Invention example CE*: Comparison example
[0076] For the clad steel sheets of the Invention Examples and Comparative Examples produced according to the above-mentioned production conditions, the concentrations of carbon (C), manganese (Mn), and chromium (Cr) were analyzed to a sufficient depth from a surface layer in the depth direction using a glow discharge spectrometer (GDS) (GDS 850A from USA LECO), which is capable of quantitatively analyzing various components. An average content of an area corresponding to a surface layer portion was calculated from the GDS analysis results by integration, and the results are shown in Table 3 below.Generally, in GDS analysis, the analysis is performed in the depth direction on a circular area of 2 mm to 6 mm, so it may be difficult to determine an accurate interface between the coating and the base steel sheet in the form of a concentration profile for the depth direction, but in the present disclosure, a point where the Zn content was 1% was determined as the interface between the coating and the base steel sheet based on various optical and SEM analysis results, etc. [Table 3] Classification Steel grade C B C S Ratio (C S / C B ) Mn B +Cr B Mn S +Cr S Ratio((Mn S +Cr S ) / (Mn S +Cr S ) IE1 A 0,21 0,03 0,14 1,52 1,32 0,87 IE 2 B 0,2 0,07 0,35 2,6 2,43 0,93 CE 1 A 0,21 0,2 0,95 1,52 1,49 0,98 CE 2 A 0,21 0,19 0,90 1,52 1,5 0,99 CE3 B 0,2 0,02 0,10 2,6 1,74 0,67 CE4 B 0,2 0,01 0,05 2,6 1,52 0,58 IE*: Invention example CE*: Comparison example
[0077] In addition, a hot-press-formed part was manufactured by hot-press forming on the coated steel sheets of the inventive examples and the comparative examples under the conditions described in Table 4. Tensile and flexural tests (VDA238-100) were conducted by taking a sample from a flat portion of the manufactured hot-press-formed part. The concentration analysis of C, Mn, and Cr was performed by GDS analysis in the depth direction, and the coverage degree of ferrite at a martensitic grain boundary of a portion of the surface layer of a component was evaluated by observing a cross-section with an optical microscope. The results are summarized in Table 4. [Table 4] Classification Condition of hot press forming Ratio (C PS / C B ) Ratio (Mn PS +Cr PS ) / (Mn B +Cr B )) Detection range Ferrite content (%) Tensile strength (MPa) Bending angle (degrees) Heating temperature (°C) Heating time (min.) IE 1 900 6 0,95 0,93 0,5 1502 72 IE 2 930 5 1,05 0,97 2,7 1527 67 CE 1 930 5 1,52 0,98 0,2 1508 53 CE 2 900 6 1,29 0,99 1,3 1511 51 CE3 900 6 0,9 0,76 36 1478 42 CE4 930 5 0,88 0,65 48 1427 47 IE*: Invention example CE*: Comparison example
[0078] The clad steel sheets of Invention Examples 1 and 2, which were produced according to the conditions of the present disclosure, satisfied a ratio (C S / C B) of 0.6 or less and a ratio ((Mn S +Cr S ) / (Mn S +Cr S ) ) of 0.8 or more. Accordingly, the hot-press-formed part produced by hot-press-forming the clad steel sheets of Invention Examples 1 and 2 satisfies a ratio (C PS / C B ) of 1.2 or less and a ratio ((Mn PS +Cr PS ) / (Mn B +Cr B )) of 0.8 or more, and accordingly, the coverage ratio of ferrite at the martensitic grain boundary of the surface layer part was 30% or less, and the bending angle was 60° or more at a tensile strength of 1500 MPa, indicating good bending properties.
[0079] Comparative Example 1 is a case where the dew point temperature during annealing was less than -10°C, and Comparative Example 2 is a case where the heating temperature was not reached during annealing. In both Comparative Examples 1 and 2, the ratio (C S / C B ) of the coated steel sheet was above 0.6, and accordingly the ratio (C PS / C B ) in the hot-pressed part was also above 1.2, resulting in poor bending properties.
[0080] Comparative Example 3 is a case where the dew point temperature during annealing exceeded 30°C, and Comparative Example 4 is a case where annealing was carried out excessively. In both Comparative Examples 3 and 4, a ratio (C S / C B ) of the coated steel sheets meet the conditions of the present disclosure, but the ratio ((Mn S +Cr S ) / (Mn B Cr B)) was less than 0.8 and the ratio ((Mn PS +Cr PS ) / (Mn S +Cr S )) of the hot-press-formed part was less than 0.8. As a result, the ferrite content at the martensitic grain boundary of the surface layer of the component exceeded 30%, and the tensile strength was relatively low compared to the other samples, and the flexibility was also severely impaired.
[0081] Although embodiments of the present disclosure have been shown and described, it will be apparent to those skilled in the art that modifications and variations may be made without departing from the scope of the present invention. Therefore, the scope of the present invention should not be limited to the embodiments, but should be defined by the appended claims and their equivalents. QUOTES CONTAINED IN THE DESCRIPTION
[0000] This list of documents submitted by the applicant was generated automatically and is included solely for the convenience of the reader. This list is not part of the German patent or utility model application. The DPMA assumes no liability for any errors or omissions. Cited patent literature
[0000] US 6296805
[0007] KR 1020100047011
[0007]
Claims
[1] Coated steel sheet for hot press forming having excellent impact resistance properties after hot press forming, the coated steel sheet comprising: a base steel sheet containing, by weight, 0.15% to 0.4% carbon (C), 0.1% to 1% silicon (Si), 0.6% to 8% manganese (Mn), 0.001% to 0.05% phosphorus (P), 0.0001% to 0.02% sulfur (S), 0.01% to 0.1% aluminum (Al), 0.001% to 0.02% nitrogen (N), 0.01% to 0.5% chromium (Cr), and the balance Fe and other impurities; and a plating layer of zinc, aluminum or their alloys on a surface of the base steel sheet, where a ratio (C S / C B ) of a C content (C S ) of a surface layer part to a C content (C B ) of the base steel sheet is 0.6 or less, and a ratio ((Mn S +Cr S ) / (Mn B +Cr B )) of the sum (Mn S +Cr S) of the contents of Mn and Cr of the surface layer part to the sum (Mn B +Cr B ) the Mn and Cr contents of the base steel sheet is 0.8 or more, where the part of the surface layer refers to an area up to a depth of 15 µm from the surface of the base steel sheet excluding the cladding layer. [2] Coated steel sheet according to claim 1, wherein the base steel sheet further contains in wt% one or more of the following elements: 0.0005% to 0.01% boron (B) and 0.01% to 0.05% titanium (Ti). [3] The coated steel sheet according to claim 1, wherein the microstructure of the surface layer part in the base steel sheet contains, in terms of area fraction, 40% to 100% ferrite and a balance of 0% to 60% pearlite, bainite or martensite, and the microstructure of a middle part in the base steel contains, in terms of area fraction, 30% to 90% ferrite and a balance of 10% to 70% pearlite, bainite or martensite. [4] A hot-press formed part having excellent impact resistance properties, the hot-press formed part comprising: a base steel sheet containing, by weight, 0.15% to 0.4% carbon (C), 0.1% to 1% silicon (Si), 0.6% to 8% manganese (Mn), 0.001% to 0.05% phosphorus (P), 0.0001% to 0.02% sulfur (S), 0.01% to 0.1% aluminum (Al), 0.001% to 0.02% nitrogen (N), 0.01% to 0.5% chromium (Cr), and the balance Fe and other impurities; and an alloy layer of a zinc or aluminum-containing alloy on a surface of the base steel sheet, where a ratio (C PS / C B ) of a C content (C PS ) of a component surface layer part to a C content (C B ) of the base steel sheet is 1.2 or less, and a ratio ((Mn PS +Cr PS ) / (Mn B +Cr B )) of the sum (Mn PS +Cr PS )of the Mn and Cr contents of the component surface layer part to the sum (Mn S +Cr S ) the Mn and Cr contents of the base steel sheet is 0.8 or more, wherein the component surface layer part refers to an area up to a depth of 25 µm from the surface of the base steel sheet excluding the alloy layer. [5] A hot press formed part according to claim 4, wherein the base steel sheet further contains, in weight percent, one or more of the following elements: 0.0005% to 0.01% boron (B) and 0.01% to 0.05% titanium (Ti). [6] The hot press-formed part according to claim 4, wherein the coverage ratio of the ferrite at a martensitic grain boundary of the surface layer part of the part is 30% or less.
Citation Information
Patent Citations
Hot-rolled press steel sheet having excellentplating weld and impact property and process for producing the same
KR1020100047011A
Coated hot- and cold-rolled steel sheet comprising a very high resistance after thermal treatment