Electrode, electrolyte, capacitive element and capacitor
Surface modifications and passivating compounds improve the volumetric efficiency and lifespan of capacitors by enhancing adhesion and preventing gas formation, addressing issues in sintered anodes.
Patent Information
- Application Number
- DE202024103602
- Authority / Receiving Office
- DE · DE
- Patent Type
- Utility models
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2034-07-31
AI Technical Summary
Improving the volumetric efficiency of capacitors, particularly those using sintered anodes, while addressing issues such as reduced lifespan and adhesion problems, gas formation, and high energy consumption due to cracks and delamination.
Implementing surface modifications on the substrate to enhance adhesion, using passivating compounds to prevent delamination and gas formation, and optimizing electrolytes for improved wettability and reduced conductivity.
Enhances volumetric efficiency, reduces gas formation, and minimizes energy consumption by improving adhesion and passivation, thereby extending the lifespan and reducing manufacturing costs.
Smart Images

Figure 00000011_0000 
Figure 00000011_0001 
Figure 00000012_0000
Abstract
Description
[0001] The present application relates to an electrode, an electrolyte, a capacitive element, a capacitor and a method for manufacturing, modifying or impregnating an electrode.
[0002] Improving capacitors in general, and electrolytic capacitors in particular, can be challenging. Specifically, attempting to improve a capacitor's volumetric efficiency can introduce secondary problems.
[0003] The inventors of the present invention have found that at least some high-volume efficiency capacitors tend to have problems. In particular, one of these problems can be a reduced lifespan under the same operating conditions as capacitors with lower efficiency.
[0004] Further challenges may arise, in particular, when sintered anodes or similar materials are used for capacitors.
[0005] Accordingly, an objective of the present application is to provide electrodes or capacitors that at least partially solve one of the problems mentioned above or described below.
[0006] The electrodes, electrolytes, capacitors or capacitive elements or methods of the independent claims each solve at least a part of a problem addressed above or below. Advantageous embodiments are specified in the dependent claims.
[0007] The following section reveals several features that, individually, offer advantages such as those described above, or other benefits described below. However, synergistic effects and additional benefits can be achieved, particularly when combined.
[0008] A sintered electrode is described according to a first embodiment, which may apply to all other embodiments below, but does not necessarily have to apply to all other embodiments.
[0009] In the most general sense, a sintered electrode is an electrode that has a sintered body. A sintered electrode can be used in a capacitor, preferably an electrolytic capacitor. Preferably, the sintered electrode includes a valve element. This can mean that it includes one or more valve elements.
[0010] In a sintered body, one or more different types of particles containing or consisting of a valve metal are bonded or sintered together. "Bond" here means that the particles in the sintered body are not loose, but rather embedded in a solid and preferably porous structure of particles, some of which are intergrown with other particles. Such a sintered body of bonded particles can generally be produced in any way. In particular, it can be achieved by sintering valve metal particles, i.e., by a heating or annealing step that causes the particles to bond or fuse. This means that the term "sintered body" is not limited to a body made of particles that have actually been sintered. Any other process that results in a similar bonding of particles can form a sintered body, even if, for example, no heat treatment is carried out.However, sintering is the preferred method.
[0011] The inventors of the present invention have discovered that sintered electrodes, particularly when used as anodes, can contribute to increasing the volume efficiency of a capacitor. In particular, improved volume efficiency can be found compared to etched electrodes. Electrodes, especially those used as anodes, are preferably passivated by an oxide layer.
[0012] Here and in the following, "valve metals" are understood in a general technical sense and are not otherwise limited. Valve metals include, for example, at least aluminum, titanium, tantalum, niobium, tungsten, chromium, zirconium, hafnium, zinc, vanadium, bismuth, or antimony. Of these metals, aluminum, tantalum, and vanadium are particularly preferred. The preferred valve metal used for electrodes in the embodiments described herein is aluminum.
[0013] According to one embodiment, the electrode can be a sintered bulk anode, which in this case means that most of the anode's volume can consist of the sintered body or the sintered material. Within this housing, a sintered material block can be contacted via a contact terminal or similar feature.
[0014] According to one embodiment, which is particularly preferred among the other embodiments described herein, the sintered anode can comprise a substrate. In principle, the substrate can comprise or consist of any conductive material, such as a metal or an alloy. Preferably, the substrate also comprises or consists of a valve metal, which can be referred to here as the first valve metal. The valve metal of the particles of the sintered body can, in this case, be referred to as the second valve metal. In both cases, the first valve metal and the second valve metal can be individually selected from the valve metals listed above. It is particularly preferred that both are the same. Even more preferably, both are aluminum.
[0015] The sintered body can be arranged on a major surface of the substrate. For example, and preferably, the substrate can be a plate or a film, and the sintered body can be a sintered layer arranged on the major surface of the film. Even more preferably, two opposing major surfaces of the substrate film are covered with a sintered layer. Such a configuration can enable a higher specific capacity than can be achieved, for example, with an etched anode.
[0016] The inventors of the present invention have observed that, in the case of an electrode with a substrate and sintered body, as described above, adhesion between the sintered body and the surface may be lacking in some cases. In such a case, the sintered body can detach from the substrate. This can occur, for example, during the processing of the electrode foil, such as cutting, winding, and cold welding, as well as during the operation of the capacitor. Besides impairing the quality of the electrode and any capacitor constructed with it, the detached parts can also lead to gas formation during storage or operation of a capacitor. Delamination can create exposed metal, which is then oxidized, for example, by an electrolyte, producing gas. Such gas can lead to a pressure buildup in a capacitor, which can destroy it.
[0017] To at least partially overcome this challenge, the inventors surprisingly discovered that by modifying the surface of the substrate's primary surface, the sintered body positioned on this surface can exhibit improved adhesion. This helps to better prevent delamination.
[0018] According to one embodiment, the surface modification can increase the surface area or roughness of the first main surface of the substrate. The unmodified surface of the substrate can be used as a reference point. The inventors assume that an increased surface area can contribute to improved adhesion.
[0019] According to one embodiment, the surface modification can include protruding parts. The protruding parts can be any part produced by the surface modification that projects above an average level of the modified surface. According to a preferred variant of this embodiment, some protruding parts can be pointed and / or angular. In general, the protruding parts can have a thinner thickness at least along one direction at the point furthest from the substrate than at a point closer to the substrate.
[0020] According to one embodiment, the surface modification can include depressions in the substrate. These depressions can, for example, have a concave shape. In particular, it may be preferred that these recessed sections in the substrate have a crater-like shape.
[0021] According to a modification of the embodiment described above and the embodiment in which the surface has depressions, the protruding parts can be edge sections or pointed sections of the crater-like depressions.
[0022] The inventors have found that adhesion can be improved by some or all of the surface morphological properties described above. For example, the depressions can help to trap the particles. The protruding parts can form sections of the modified substrate surface that heat up to the sintering temperature more quickly during a sintering process, which can simplify the sintering of the sintered body on the main surface.
[0023] Accordingly, in a more generalized form, it is also an embodiment of the present description that parts of the surface modification are designed to improve adhesion during sintering.
[0024] The formation of the aforementioned surface modification is not, in the most general sense, limited to any specific type of structure. Nor is it limited to any particular method for producing this structure. In particular, the technique can, for example, include lithographic steps.
[0025] According to a preferred embodiment, the surface modification is achieved by, or is achieved through, chemical or electrochemical surface etching. In particular, depressions can be easily etched chemically or electrochemically into surfaces containing valve metal, and especially preferably into surfaces containing aluminum. The edges of the depressions can form protruding parts. This provides a simple method for surface modification.
[0026] Surface modification in general, and etching in particular, can be advantageous because they can at least partially remove a natural oxide that has formed on the substrate surface, or impurities.
[0027] In one embodiment, the surface roughness R can be a The surface-modified main substrate particles are of the same order of magnitude as the particles of the sintered body. They can also be smaller. The term "same order of magnitude" is to be understood in a general technical sense. This can mean, for example, that the average size of the structures on the surface determines the surface roughness R. a The surface roughness can be 0.1 to 10 times the average particle size used. Alternatively or additionally, the surface roughness can be in the range of 0.01 to 50 µm. Even more preferably, it can be 0.1 to 50 µm, 0.5 to 10 µm, or even 0.7 to 7 µm or 0.5 to 5 µm.
[0028] The inventors of the present invention have found that adhesion can be advantageous if the size of the structures on the surface corresponds to the size of the particles used for the sintered body.
[0029] In one embodiment, the particles of the sintered body have an average size between 0.5 µm and 10 µm, e.g. 1 µm to 5 µm.
[0030] The inventors have discovered that this particle size contributes to increasing the volumetric efficiency of the electrode. Furthermore, the inventors have found that particles of this size can adhere well with the measures defined above. In particular, the structures created by etching and / or the surface roughness described above provide good adhesion for particles of this size.
[0031] According to a further embodiment, the content of the valve metal in the substrate can be 98 wt.% or more, for example 99 wt.% or more, or even more preferably 99.7 wt.% or more, or even more preferably 99.9 wt.% or more. These values are particularly relevant for the valve metal aluminum. Previously, high-purity valve metal substrates often had to be used for the production of sintered electrodes. These are more expensive to produce than the substrates described above, which have a lower degree of purity. Furthermore, the inventors have found that the lower purity of the substrates can facilitate the modification of the substrate surface.
[0032] According to one embodiment, the purity of the valve metal in the substrate can be below 99.99 wt.% and preferably below 99.9 wt.% for the reasons mentioned above. Accordingly, for example, a range of 98 wt.% to 99.90 or 99.99 wt.% can be used. Alternatively, the values mentioned above can replace "98%" within this range. In particular, with a range of 99.7 wt.% to 99.99 wt.% or, more specifically, 99.7 wt.% to 99.90 wt.%, the inventors have found that the levels of impurities are suitable for surface modification but not excessively high, and other disadvantages of impurities are reduced.
[0033] The next embodiment is also preferably used for an electrode with a sintered body as described above. However, this approach can also be applied to any other type of electrode that can be used in an electrolytic capacitor. An electrode may have defects or cracks for various reasons. At these defects or cracks, the oxide layer, which is preferably formed on the surface of an electrode, may be partially absent.
[0034] The inventors discovered that the sintered bodies described above are particularly susceptible to the formation of the cracks described above. Cracks can arise, for example, during the electrode manufacturing process. In a foil electrode with a foil-like substrate and sintered body, cracks or partial delaminations of the sintered body can occur during process steps such as cutting, winding, and cold welding, as well as during subsequent capacitor operation.
[0035] According to the present embodiment, such cracks or any area which at least partially lacks an oxide layer can be at least partially passivated with a passivating compound.
[0036] If these areas are not passivated quickly, gases can form at these points during operation or even during passive storage due to chemical reactions with the exposed metal. This can lead to an undesirable excess of gas in a condenser, which can destroy it. Venting systems can be used to counteract this gas formation. Accordingly, passivating these areas helps reduce gas formation and can also help avoid costly gas compensation measures.
[0037] Previously, the high energy density or capacitive density of a sintered anode foil, combined with the large number of surface cracks, led to high energy consumption or leakage current until the damaged electrode had sufficient passivating oxide. Typically, several repairs are required for a state-of-the-art electrode during the lifetime of a capacitor, which limits the applicability of this technology due to the resulting high hydrogen gas formation. These disadvantages can be reduced by using a passivating compound.
[0038] As described in more detail below, these substances can either be applied separately directly to the anode or to a capacitive element such as a winding element before the assembly of a capacitor, or they can be introduced as a component of the electrolyte itself.
[0039] The inventors have found that the passivating compounds can reduce gas formation before and during oxide formation, which can occur from the liquid electrolyte. This means that, in addition to the passivating effect of the compounds themselves, they can also facilitate the sealing of sites through a combination of the passivating compound and the oxides that form.
[0040] The passivating compound is generally not limited and can be applied in the form of a molecular or particle-containing compound or a composite.
[0041] According to one embodiment, phosphorus-containing compounds or silicon-containing compounds can be used as the partially passivating compound described above.
[0042] In one embodiment, the silicon-containing compound can, for example, be provided in a form that includes particles. Such particles can, for example, contain silicon oxide.
[0043] According to one embodiment, the application of a passivating compound can also reduce the requirements for a high degree of purity of the valve metals in the electrodes. In the case of a sintered electrode with a substrate and a sintered body, this can apply to the substrate and / or the sintered body. For example, a passivating compound can be helpful when a purity of 99.7 or 99.8 wt.% or higher is used for the valve metal, such as 99.7 to 99.99 wt.% or 99.7 to 99.0 wt.%. The inventors have found that the passivation of components can help to reduce leakage current in combination with reduced purity. This applies to both the substrate and the sintered body. In both housings, the effect is particularly pronounced with aluminum.
[0044] In one embodiment, it may be preferred to combine surface modification and passivation, since both can help to reduce the exposed metal surface area in a complementary manner. Furthermore, both measures can contribute to the use of less pure metal.
[0045] Furthermore, the inventors have discovered that the thickness of a separator can be reduced through improved passivation by using a passivating compound in a capacitor assembly. This can increase the volumetric efficiency. For example, this can help reduce the thickness of a separator to 44 µm or less, or to 40 µm or less, or even to 35 µm or less. These values can refer to the total thickness of the separator between the anode and cathode foils. Here and in this description, the term "separator" can refer to the functional unit that separates the cathode and anode. It is not limited to a single-layer separator but can also include separator designs with two or more layers.
[0046] According to a further embodiment, an electrode is described which has an impregnation on at least part of its surface. Here, too, the electrode is preferably an electrode with a sintered part that is impregnated. However, it is not limited to such sintered electrodes. The impregnation is designed to increase the wettability of the electrode or the impregnated part by an electrolyte. The inventors have found that, for example, increasing the surface area of the electrode, particularly by means of a sintered body, makes the wettability of the electrode by the electrolyte increasingly important.
[0047] The inventors discovered that the high compactness and density of the sintered electrodes and the oxide grown on them can hinder wetting by an electrolyte, especially with electrolytes of higher viscosity. This is improved by the impregnating compound.
[0048] According to one embodiment, silanes can act as wetting-enhancing impregnating agents. The same applies to polyethylene oxides, sulfonates, or anionic surfactants. Silanes, polyethylene oxides, sulfonates, or anionic surfactants can be used individually or in a mixture of one or two of these substances.
[0049] The approach described above for increasing wettability can preferably also be applied to the surface modification described above and additionally to reducing the non-passivated areas.
[0050] Furthermore, electrolytes for electrolytic capacitors are described as additional embodiments.
[0051] According to a first embodiment, an electrolyte is described which comprises a compound designed to adsorb at cracks in an electrode or at areas of an electrode that are at least partially lacking an oxide layer. The compound is designed to at least partially passivate these areas. The electrolyte, which can be used in an electrolytic capacitor, can comprise the at least partially passivating compounds described above.
[0052] The advantages described above also apply here.
[0053] According to one embodiment, the passivating compound, as described above, can be a phosphorus- or silicon-containing compound, either in molecular or particulate form. In the latter case, the electrolyte can be an emulsion containing these particles. For example, particles containing silicon dioxide at a concentration of 0.1 to 5 wt%, such as 0.5 to 1.5 wt%, can be used.
[0054] For example, the electrolyte in a capacitor can be combined with an electrode as described above, preferably a sintered electrode. Accordingly, the partially passivated electrode described above can be formed in situ by the electrolyte. In many packages, some of the passivating compound may remain in the electrolyte even after adsorption onto the electrode.
[0055] According to a further embodiment, an electrolyte for an electrolytic capacitor is described, comprising an impregnating compound configured to impregnate a portion of the electrode surface. The impregnating compound is designed to enhance the wettability of the electrode surface by the electrolyte. It is further designed to adsorb onto the electrode surface. For example, it may be a silane, polyethylene oxide, sulfonate, and / or anionic surfactant as described above, added to the electrolyte.
[0056] According to one embodiment, the concentration of the impregnating compound in the electrolyte can be 10 to 200 ppm by weight, for example 15 to 50 ppm. In general, but especially for the listed examples of an impregnating compound, the inventors have found that for this concentration range, the wettability by the electrolyte could be significantly improved.
[0057] For example, the electrolyte in a capacitor can be combined with an electrode as described above, preferably a sintered electrode. Accordingly, the impregnated electrode described above can be formed in situ by the electrolyte. In many housings, some of the impregnating compound may also remain in the electrolyte after adsorption onto the electrode.
[0058] The impregnating compound and the passivating compound can be added together to an electrolyte.
[0059] According to a further embodiment, which can exist independently of the other embodiments above but can also be advantageously combined with them, an electrolyte for an electrolytic capacitor is described which, in a state prior to wetting a separator or a winding element, has a conductivity of 660 µS / cm or less at a temperature of 30°C. The inventors of the present invention have found that a conductivity of 660 µS / cm or less can be advantageous for sintered electrodes and can help to reduce the thickness of a separator impregnated with the electrolyte.
[0060] Lower conductivity can reduce the generation of local heat during self-healing or decrease the need for passivation processes of damaged sintered bodies, as described above. Prior to the present invention, highly conductive electrolytes were frequently used, in which surface repair processes generated a high density of local heat, resulting in a very high leakage current.
[0061] According to one variant of the above embodiment, the electrolyte can have a water content of 1% to 10%. The inventors of the present invention have found that such a high water content of the electrolyte can help to reduce the thickness of the separator paper.
[0062] According to a further embodiment, a capacitive element is described. The capacitive element can be configured to store electrical charges during the operation of a capacitor. For example, the capacitive element can be configured to be charged and discharged during the operation of a capacitor. The capacitive element can, for example, have a cathode and an anode. The cathode and the anode can be electrically contacted by electrically conductive elements, such as wires or conductors. The cathode and the anode are generally not restricted. Preferably, the anode can have the properties of the electrode described above.
[0063] According to one embodiment, which may be preferred for the other embodiments, the capacitive element can be a winding element in which the anode and the cathode are wound. The winding element can, for example, be a cylindrical winding element or a flattened winding element.
[0064] According to one embodiment, which may also be preferred in the other embodiments, the winding element can be designed for an electrolytic capacitor. In this housing, an electrolyte is arranged between the anode and the cathode. For example, a separator, which is impregnated or saturated with the electrolyte, can be arranged between the anode and the cathode. The separator is not restricted; it should simply be designed to be impregnated or saturated with an electrolyte and should not be electrically conductive. The separator can be made of or consist of a cellulose-based material, such as paper. In an electrolytic capacitor, it may be preferred that the anode has an oxide on its surface, which provides at least partial chemical and electrical separation between the anode and the electrolyte.
[0065] The electrolyte is generally not restricted. However, the electrolytes mentioned above can exhibit the properties of the electrolytes described above, leading to the described advantages.
[0066] According to one embodiment, a capacitive element can be described in which a separator is impregnated with an electrolyte having a maximum conductivity of 660 µS / cm and preferably additionally containing 1 to 10% water. In this case, the thickness of the separator can be 44 µm or less. For example, the thickness of the separator can even be 40 µm or less, and even 35 µm or less.
[0067] According to a further embodiment, a capacitor is provided with a capacitive element. The capacitive element can be one of the capacitive elements described above or have a combination of their properties. Alternatively or additionally, the capacitor can have any of the electrodes described above as the anode. Alternatively or additionally, the capacitor can have any electrolyte, but preferably one of the electrolytes described above.
[0068] According to further embodiments, methods for manufacturing or treating electrodes are described below. Where applicable, the methods may have the features described above, which are explained for the electrodes or the electrolytes.
[0069] According to one embodiment, a method for manufacturing an electrode is described. First, a substrate is provided. The substrate used here has or consists of a first valve metal. It can, for example, have or consist mainly of aluminum. It can, for example, have the substrate purity grades described above. In a further step, the main surface of the substrate is modified to obtain a surface-modified main surface of the substrate. As described above, the surface modification can, for example, involve the formation of protrusions and / or depressions, and it can increase the surface roughness and preferably the adhesion to the sintered body. In a subsequent process step, a sintered body is formed on the surface-modified main surface.The sintered body comprises or consists of interconnected particles that include or are composed of a second valve metal. The subprocess for forming the sintered body is not restricted and can be any suitable method. For example, the formation of the sintered body can involve sintering particles at a temperature of 400 to 660°C. The particles can, for example, contain aluminum as the main component. The formation of the sintered body can also, for example, involve applying a slurry containing the particles. The slurry can then be sintered. The particles generally include a second valve metal, preferably aluminum.
[0070] As described above, surface modification can be achieved by any suitable means such as lithography or any type of etching. Chemical or electrochemical etching is preferably used.
[0071] According to a further embodiment, a method is described in which at least a portion of a sintered body is modified by adsorption of a compound at crack locations or at least at locations where an oxide layer is at least partially lacking. The compound is such that it at least partially passivates these locations. The properties described above for such a compound can apply here. This method can be carried out either on the electrode in its original state, or the at least partially passivating compound can be introduced into the electrolyte, or a combination of both.
[0072] According to a further embodiment, a method for impregnating at least a portion of an electrode, preferably a sintered electrode, is described. This impregnation can be carried out by applying an impregnating compound, which may be the impregnating compound described above. The impregnating compound is designed to increase the wettability of the electrode surface by an electrolyte. This method can also be carried out either before the electrode is installed in a capacitor, by introducing the impregnating compound into the electrolyte, or by a combination of both.
[0073] Further advantageous embodiments and further embodiments of the electrode or the capacitor, as well as a method for manufacturing such electrodes or the capacitor, can be seen from the following exemplary embodiments, which are described in conjunction with the figures. It should be noted, however, that the invention is not limited to these exemplary embodiments. Furthermore, the exemplary embodiments are at least partially illustrated in figures with schematic drawings. These schematic drawings are not to scale, and absolute and relative dimensions may be distorted. In fact, individual elements may be exaggerated to improve clarity or understanding. Accordingly, no absolute or relative dimensions can be derived from the schematic representations unless otherwise indicated.Identical, similar, or similarly effective elements are marked with the same reference symbols in the figures. Fig. Figure 1 shows a schematic sketch of a surface modification process; Fig. Figure 2 shows a schematic cross-section of a first embodiment of an electrode; Fig. Figure 3 shows a cracked embodiment of an electrode; Fig. Figure 4 shows an intermediate stage of at least partial passivation of an electrode; Fig. Figure 5 shows an embodiment of an electrode that is at least partially passivated; Fig. Figure 6 schematically shows the wetting behavior of an unimpregnated electrode; Fig. Figure 7 shows the wetting behavior of an impregnated electrode; Fig. Figure 8 shows an exemplary embodiment of a capacitor.
[0074] In Fig. Figure 1 shows a schematic cross-section of a process for producing a surface-modified substrate. On the left side of the diagram is a substrate 1 with a first main surface 2 and a second main surface 3. The substrate 1 consists of a material containing 99.7 wt.% or more aluminum. It is then etched either chemically or electrochemically. In particular, electrochemical etching can be carried out using a process similar to the formation of cathodes in the manufacture of an electrolytic capacitor. In this process, a modified first main surface 2' is formed from the first main surface 2. A modified second main surface 3' is formed from the second main surface 3. The resulting structure includes projections that are pointed or angular, as well as depressions in the substrate that are concave or shell-shaped.
[0075] Chemical etching can be carried out in an HCl or NaOH solution. The concentration can range from 0.5 mol / L to 4 mol / L, preferably 1 mol / L. Etching can be performed at temperatures of, for example, 60°C, but also at other temperatures. Electrochemical etching can be carried out under essentially the same conditions and at current densities of 100 mA / cm². 2 up to 3 A / cm 2 This can be carried out. The conditions can be chosen or adapted to create the described structures.
[0076] In a further step, the result of which in Fig. As shown in Figure 2, a first sintered body 4 and a second sintered body 5 can be formed on the first and second modified main surfaces 2' and 3'. The sintered bodies 4 and 5 are formed from aluminum particles provided in a slurry. The slurry is applied to the modified substrate surfaces 2' and 3'. Subsequently, the slurry can be debound and sintered. Sintering takes place at a temperature between 400 and 660°C. The particles in the sintered bodies 4 and 5 are bonded together by sintering. The particles are aluminum-based with an aluminum content of 99 wt% or more. It is not explicitly shown here that the aluminum sintered bodies can be passivated by oxidation. This process forms an insulating surface oxide.
[0077] The surface modification described above improves the adhesion of the sintered body to the surface. The inventors attribute this to increased surface roughness and possibly also to the removal of natural oxide from the substrate and any impurities. Furthermore, the inventors have found that the comparatively low purity of the substrate, as described above, simplifies the formation of the surface modification.
[0078] In the Fig. Figures 3 to 5 illustrate a method for passivating cracks. Fig. Figure 3 shows a substrate 1 with a surface-modified main surface 2', as above for the Fig. 1 and Fig. Figure 2 explains. A sintered body 4 is formed on the substrate 1. The sintered body is composed of bonded particles 6. The surface oxide 7 is shown explicitly here. The sintered body can be damaged during the manufacturing steps for producing a capacitor, such as cutting, winding, and cold welding.
[0079] This can lead to the formation of cracks (8). As in Fig. As shown in Figure 4, components 8 can be adsorbed at these crack locations, designed to at least partially passivate them. This can occur either in an electrolyte within the capacitor or additionally or instead before the electrolyte is added. The passivating compound 9 is formed from silicon oxide particles. These can be present in an emulsion-like electrolyte or applied by a separate emulsion before the capacitor is potted. Such silicon oxides, or alternatively phosphorus-containing compounds or particles, adhere to the crack locations and form modified crack locations 8', as shown in Figure 4. Fig. Figure 4 shows that this partially passivates these cracks. This can reduce the formation of gases from the electrolyte reaction in the assembled capacitor.
[0080] As in Fig. As shown in Figure 5, when a suitable solution, or in particular an aqueous electrolyte, is used, a partial oxide 10 can form in addition to the silicon particles 9. This oxide is indicated by the dashed lines. This oxide can at least partially and additionally passivate the cracks. The inventors have found that by using a compound that is at least partially passivating, such as silicon oxide, the passivation of the cracks can be improved by the oxide newly formed in the electrolyte or by another separate technique. The cracks are marked here with reference numeral 8'', which indicates enhanced passivation.
[0081] In Fig. Figure 6 shows a sintered electrode immersed in an electrolyte. In this housing, the electrolyte 11 has difficulty fully wetting the entire sintered body.
[0082] To solve this problem, the inventors, as in Fig. As shown in Figure 7, it was found that an impregnating compound 12 can be adsorbed onto the particles 6 of the sintered body. This can be done either before potting the capacitor or by adding such a compound to the electrolyte. In the case of an electrolyte, the concentration of the impregnating compound can be 10 to 200 ppm by weight. As shown, the wetting by the electrolyte is improved, thereby allowing a larger portion of the capacitor to be used for capacitive interactions.
[0083] In Fig.Figure 8 shows a schematic cross-section of a capacitor 13. The capacitor 13 has a housing 14, which is closed by a cover 15. Inside this housing, formed by the housing 14 and the cover 15, a winding element 16 is arranged. Although the winding element is not explicitly shown, it includes a cathode, which is not limited. It also includes an anode, which can be one of the anodes described above. In addition, two terminal contacts 17 are provided, which connect the anode and cathode. Furthermore, the anode and cathode are separated within the winding element by a separator paper. The separator paper is impregnated with the electrolyte. Optionally, the electrolyte can contain the substances described above for passivating cracks and increasing wettability.Furthermore, the electrolyte used here preferably has a conductivity of 660 µS / cm or less and a water content of 1 to 10%. This allows the thickness of the separator paper to be reduced to 40 µm or even less. Reference character list 1 substrate 2 first main surface 2' modified first main surface 3 second main surface 3' modified second main surface 4 first sintered body 5 second sintered body 6 particles 7 Oxide 8 Crack location 9 passivating connection 10 partial oxide 11 Electrolyte 12 impregnating compound 13 Capacitor 14 cases 15 lids 16 winding element 17 Connection contact
Claims
[1] Electrode comprising a substrate and a sintered body on a first main surface of the substrate, wherein the substrate comprises or consists of a first valve metal, the sintered body comprises or consists of bonded or sintered particles containing or consisting of a second valve metal, the first main surface is surface modified. [2] Electrode according to claim 1, wherein the surface modification represents an increase in the surface area and / or the surface roughness compared to an unmodified substrate surface. [3] Electrode according to claim 1 or 2, wherein the surface modification is designed to increase the adhesion of the sintered body or particles of the sintered body to the surface compared to an unmodified substrate surface. [4] The electrode according to any one of claims 1 to 3, wherein the surface modification has protruding parts. [5] Electrode according to one of claims 1 to 4, wherein the surface modification is a chemical or electrochemical surface etching. [6] Electrode according to one of claims 1 to 5, wherein the surface modification comprises depressions in the substrate. [7] Electrode according to one of claims 1 to 6, wherein the surface roughness R produced by the surface modification a is of the same order of magnitude or smaller than the average particle size of the particles of the sintered body. [8] Electrode according to one of claims 1 to 7, wherein the particles of the sintered body have an average size between 0.5 µm and 20 µm. [9] An electrode according to any one of claims 1 to 8, wherein the content of the valve metal in the substrate is 98 wt% or more, preferably 99.7 wt% or more. [10] The electrode according to any one of claims 1 to 9, wherein the content of the valve metal in the substrate is 99.99 wt% or less. [11] Electrode comprising a sintered body, wherein the sintered body comprises or consists of bonded or sintered particles comprising or consisting of a valve metal, a compound is adsorbed at cracks in the sintered body or at locations on the sintered body where an oxide layer is at least partially missing, and the compound is such that it at least partially passivates these locations. [12] Electrode with a sintered body, wherein the sintered body comprises or consists of bonded or sintered particles comprising or consisting of a valve metal, a phosphorus-containing compound or a silicon-containing compound is adsorbed at cracks in the sintered body or at locations on the sintered body where an oxide layer is at least partially missing. [13] An electrode according to claim 11 or 12, wherein the compound adsorbed at crack sites comprises molecular and / or particulate compounds and / or composites. [14] An electrode having the combined features of at least one of claims 11 to 13 and of at least one of claims 1 to 10. [15] An electrode having an impregnation on at least part of its surface, the impregnation being designed to increase wettability by an electrolyte. [16] The electrode of claim 15, wherein the impregnation comprises a silane, a polyethylene oxide, a sulfonate and / or an anionic surfactant. [17] An electrode having the combined features of claim 15 or 16 and at least one of claims 1 to 10. [18] An electrode having the combined features of claim 15 or 16 and at least one of claims 11 to 14. [19] An electrolyte for an electrolytic capacitor comprising a compound designed to adsorb at cracked sites of an electrode or at sites on the electrode that at least partially lack an oxide layer, and the compound is designed to at least partially passivate these sites. [20] Electrolyte for an electrolytic capacitor comprising a phosphorus-containing compound or a silicon-containing compound. [21] An electrolyte for an electrolytic capacitor comprising an impregnating compound adapted to impregnate a portion of the surface of an electrode and adapted to increase the wettability of the surface of the electrode by the electrolyte when adsorbed on the surface of the electrode. [22] The electrolyte of claim 21, wherein the concentration of the impregnating compound is 10 to 200 ppm by weight. [23] An electrolyte for an electrolytic capacitor, wherein the electrolyte, in a state before wetting a separator or a winding element, has a conductivity of 660 µS / cm or less at a temperature of 30°C. [24] An electrolyte for an electrolytic capacitor according to claim 23, which has a water content of 1% to 10%. [25] Capacitive element having an electrode according to at least one of claims 1 to 18 as an anode. [26] A capacitive element comprising an anode, a cathode and an electrolyte according to any one of claims 19 to 24. [27] A capacitive element according to claim 26, wherein a separator impregnated with the electrolyte is arranged between the cathode and the anode, and wherein the total thickness of the separator is 44 µm or less. [28] Capacitive element according to one of claims 25 to 27, comprising an electrode according to at least one of claims 1 to 18 as an anode. [29] Capacitor comprising an electrode according to at least one of claims 1 to 18 and / or an electrolyte according to at least one of claims 20 to 24 or a capacitive element according to at least one of claims 25 to 28, arranged in a housing. [30] An electrode produced by a method comprising providing a substrate containing or consisting of a first valve metal, Surface modifying a main surface of the substrate to obtain a surface-modified main surface of the substrate, Forming a sintered body on the surface-modified main surface, the sintered body comprising or consisting of bonded or sintered particles comprising or consisting of a second valve metal. [31] The electrode of claim 30, wherein the main surface is chemically or electrochemically etched to form the surface modification. [32] An electrode according to claim 30 or 31, wherein the formation of the sintered body includes applying a slurry containing particles with a second valve metal to the surface-modified major surface. [33] An electrode according to any one of claims 30 to 32, wherein the formation of the sintered body includes sintering at a temperature of 400 to 660°C. [34] An electrode modified by a method for modifying at least a portion of a sintered body of an electrode by adsorbing a compound at crack sites or sites at least partially lacking an oxide layer, the compound being such that it at least partially passivates these sites. [35] An electrode modified by a process for modifying at least part of a sintered body of an electrode by adsorbing a phosphorus-containing compound or a silicon-containing compound at crack sites or sites which at least partially do not have an oxide layer. [36] An electrode modified by a process for impregnating at least a portion of an electrode by applying an impregnating compound adapted to increase the wettability of the surface of the electrode by an electrolyte.