Oxide particles coated with amino groups

The composite coating of LLZO particles with a hydroxide ion, dopamine, and CTAB layers, along with carbon nanotubes and amorphous carbon, addresses moisture-induced deterioration and enhances lithium ion conductivity, improving battery electrode performance and reducing costs.

DE202024105972U1Active Publication Date: 2024-12-05SHENZHEN TXD TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE202024105972
Authority / Receiving Office
DE · DE
Patent Type
Utility models
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-12-05
Estimated Expiration
2034-10-31

AI Technical Summary

Technical Problem

LLZO particles in battery electrodes are prone to side reactions and deterioration due to moisture exposure, leading to uneven lithium ion distribution and material wear during the electrode slurry preparation process.

Method used

A composite structure is formed by coating LLZO particles with a hydroxide ion layer, followed by a dopamine layer and a CTAB layer, and further enhanced with carbon nanotubes and nanoscale amorphous carbon to create protective structures that prevent moisture ingress and enhance lithium ion conductivity.

Benefits of technology

The composite coating structure effectively prevents side reactions, maintains lithium ion distribution, and improves electrical conductivity, resulting in better battery electrode material quality and reduced production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

An oxide particle coated with amino groups, representing an LLZO composite particle; the LLZO composite particle is used in an electrode of a solid-state or semi-solid-state battery; and the electrode comprises a substrate and an electrode slurry layer coated onto the substrate; the LLZO composite particle comprises the following: a first LLZO particle, which serves to guide and distribute the paths of the lithium ions and to ensure that evenly distributed lithium ion channels are formed within the electrode; a hydroxide ion layer applied to an outer surface of the first LLZO particle; the hydroxide ion layer and the first LLZO particle form a second-order LLZO composite particle; the hydroxide ion layer is formed by a reaction of Tris molecules (tris(hydroxymethyl)aminomethane, ((HOCH2)3CNH2) and features a plurality of third OH ions; each of the Tris molecules comprises three OH ions, namely a first, a second, and the third OH ion; wherein the first and second OH ions of the Tris molecules are bound by hydrogen bonds to oxidizing functional groups on the first LLZO particle; and wherein the third OH ions of the Tris molecules extend outwards to an outer surface of the first LLZO particle to form the hydroxide ion layer; and a dopamine layer applied to an outer surface of the second-order LLZO composite particle; wherein the dopamine layer is formed from a plurality of copolymerized dopamine molecules; wherein a dehydration-induced polymerization is carried out between OH ions of the dopamine molecules and the third OH ions of the hydroxide ion layer of a corresponding second-order LLZO composite particle to cause the dopamine layer to remain connected to the second-order LLZO composite particle by means of the hydroxide ion layer; and wherein the dopamine molecules of the dopamine layer are hydrophobic to protect the first LLZO particle and prevent the first LLZO particle from becoming wet.
Need to check novelty before this filing date? Find Prior Art

Description

AREA OF INVENTION

[0001] The invention relates to a battery electrode material and in particular to an oxide particle coated with amino groups. BACKGROUND OF THE INVENTION

[0002] A typical battery consists of electrodes (positive and negative) placed in an electrolyte. In current technology, LLZO material (lithium lanthanum zirconium oxide) is added to the electrodes to increase their ionic conductivity. Since LLZO particles exhibit high ionic conductivity for lithium ions, the lithium ions are dispersed as they pass through the electrode, thanks to the guidance provided by the dispersed LLZO particles. This allows the lithium ions to be distributed evenly within the electrode, preventing abnormal accumulation of lithium ions in the electrode slurry and thus avoiding undesirable side reactions.

[0003] However, during the production of the electrode slurry, the LLZO material can easily undergo a side reaction with other materials in the electrode, leading to a deterioration of the material within an electrode slurry. SUMMARY OF THE INVENTION

[0004] To overcome the aforementioned shortcomings of the prior art, the object of the invention is accordingly to provide an oxide particle coated with amino groups, wherein a first LLZO particle is coated with a hydroxide ion layer to form a second-order LLZO composite particle. The second-order LLZO composite particle is coated with a dopamine layer and a CTAB layer to form a LLZO composite particle. The dopamine layer is hydrophobic and serves to prevent the external penetration of water into the first LLZO particle. The LLZO composite particle is also coated with carbon nanotubes and nanoscale amorphous carbon to increase lithium ion conductivity, the nanoscale amorphous carbon being filled into the voids of the carbon nanotubes to improve electrical conductivity.The dopamine layer, the CTAB layer, the carbon nanotubes and the nanoscale amorphous carbons form several protective structures for the first LLZO particle, which further increases the lithium conductivity of the first LLZO particle, prevents side reactions of the first LLZO particle as well as material wear of the electrode slurry and results in better quality in the production of battery electrode material. BRIEF DESCRIPTION OF THE IMAGES Fig. shows a schematic view illustrating the structure of the invention. Fig. shows an application of the structure according to the invention. Fig. shows a schematic view illustrating the complete structure and a partial structure of the hydroxide ion layer of the invention. Fig. shows a schematic view illustrating the structure of the third-order LLZO composite particle according to the invention. Fig. shows a schematic view depicting the overall structure and substructure of the LLZO composite particle, where the polymerization triggered by dehydration takes place between the OH- ion of dopamine in the dopamine layer and the third OH- ion of the hydroxide ion layer. Fig. Figure 1 shows a schematic view which shows a partial structure of the LLZO composite particle of the invention, wherein the attractive forces are formed between the OH- ion of the CTAB and dopamine and the third OH- ion of the hydroxide ion layer. Fig. shows a cross-sectional view which shows the structure of the LLZO composite particle according to the invention. DETAILED DESCRIPTION OF THE INVENTION

[0005] With regard to the Fig. The invention provides an oxide particle coated with amino groups. The oxide particle is an LLZO composite particle 100. The LLZO composite particle 100 is used in an electrode 10 of a solid-state or semi-solid-state battery. In the application, several LLZO composite particles 100 can be incorporated into the electrode 10, which is particularly a positive electrode of the solid-state or semi-solid-state battery. The size of the LLZO composite particle 100 ranges from 50 nm to 200 nm. The electrode 10 comprises a substrate 11 as a support for the electrode material 10 and an electrode slurry layer 13, which is applied to the substrate 11. The electrode slurry layer 13 comprises the LLZO composite particles 100 and an electrode slurry 12, which serves as a binder.The weight fraction of the LLZO composite particles 100 in an electrode sludge layer 13 (especially a positive electrode sludge layer) is 0.5 wt.% to 5 wt.%.

[0006] The LLZO composite particle 100 comprises the following elements: A first LLZO particle 15. Since LLZO material has a high ionic conductivity, the first LLZO particle 15 serves to guide and distribute the paths of the lithium ions as they flow through the electrode. It causes uniformly distributed lithium ion channels to form within the electrode, thereby preventing an abnormal accumulation of lithium ions in the electrode sludge and thus undesirable side reactions.

[0007] The first LLZO particle 15 consists of LLZO (lithium lanthanum zirconium oxide, Li7La3Zr2O). 12 ) or from LLZO doped with at least one metal (such as gallium (Ga) doped LLZO (Li 6.2 Ga 0.8 La3Zr2O 12), made of aluminum (Al) doped LLZO or barium (Ba) doped LLZO.

[0008] Since moisture is present in the electrode during the manufacturing process, the LLZO particles are hydrophilic and can easily become damp, resulting in the formation of an alkaline solution. Therefore, in the invention, an outer surface of the first LLZO particle 15 is coated with a protective layer (the following dopamine layer 35) to prevent the first LLZO particle 15 from becoming damp during the electrode manufacturing process.

[0009] A hydroxide ion layer (OH-) 24 is applied to an outer surface of the first LLZO particle 15. The hydroxide ion layer 24 and the first LLZO particle 15 form a second-order LLZO composite particle 30 (as shown in Fig. (shown). The thickness of the hydroxide ion layer 24 is 0.5 nm to 2 nm. The hydroxide ion layer 24 is formed by a reaction of Tris molecules (tris(hydroxymethyl)aminomethane, (HOCH2)3CNH2) and features a multitude of third OH ions. The Tris molecules are added during the fabrication process of the composite LLZO particle 100. Each of the Tris molecules has three OH ions, namely a first, a second, and a third OH ion. The first and second OH ions of the Tris molecules are bound by hydrogen bonds to oxidizing functional groups on the first LLZO particle 15. The third OH ions of the Tris molecules extend outwards to an outer surface of the first LLZO particle 15 to form the hydroxide ion layer 24. Fig. This shows an example of only two Tris molecules and is not intended to limit the scope of the invention.

[0010] A dopamine layer 35 is applied to an outer surface of the second-order LLZO composite particle 30. The dopamine layer 35 is formed by a multitude of copolymerized dopamine molecules. Dehydration-induced polymerization takes place between the OH ions of the dopamine molecules and the third OH ions of the hydroxide ion layer 24 of a corresponding second-order LLZO composite particle 30 to cause the dopamine layer 35 to be encapsulated by the hydroxide ion layer 24 (as in Fig. (shown) is connected to the second-order LLZO composite particle 30. The thickness of the dopamine layer 35 is 1 nm to 10 nm.

[0011] Since moisture is present during the manufacturing process of the electrode slurry and the LLZO particles are hydrophilic, they can easily become damp and form an alkaline solution that destroys the lithium conductivity of the LLZO particles. Therefore, dopamine is used in the invention. Because the dopamine molecules of the dopamine layer 35 are hydrophobic, this protects the first LLZO particle 15 and prevents it from becoming damp.

[0012] The hydroxide ion layer 24 is used to connect the first LLZO particle 15 and the dopamine layer 35. Since the OH ion of the hydroxide ion layer 24 has a polarity, the dopamine layer 35 can react with the hydroxide ion layer 24 when the hydroxide ion layer 24 is applied to the outer surface of the first LLZO particle 15 and is more stably attached to the second-order LLZO composite particle 30.

[0013] The LLZO composite particle 100 also comprises a CTAB (cetyltrimethylammonium bromide) layer 61, which is applied to the outer surface of the dopamine layer 35. The CTAB layer 61 is formed by a large number of CTAB (cetyltrimethylammonium bromide) molecules 60. The CTAB molecules 60 are used as a surfactant. Some of the CTAB molecules 60 are mixed into the dopamine layer 35 and the hydroxide ion layer 24. An excess of the CTAB molecules 60 surrounds the outer surface of the dopamine layer 35.

[0014] The ratio of the total weight of the CTAB molecules 60 of CTAB layer 61 to the total weight of the dopamine molecules of dopamine layer 35 is 0.1% to 0.3%.

[0015] The structure of the CTAB molecules 60 on the outer surface of the dopamine layer 35 and the CTAB molecules 60 within the dopamine layer 35 and the hydroxide ion layer 24 is a naturally occurring result of the manufacturing process. In CTAB layer 61, some of the CTAB molecules 60 with a specific polarity attract molecules of opposite polarity in the dopamine layer 35 and the hydroxide ion layer 24, causing the portion of the CTAB molecules 60 within the dopamine layer 35 and the hydroxide ion layer 24 to mix. An excess of CTAB molecules 60 from CTAB layer 61 surrounds the outer surface of the dopamine layer 35 through attractive forces arising from the polarities of the excess CTAB molecules.

[0016] The CTAB layer 61 serves to impart higher dispersivity to the first LLZO particle 15 without agglomeration and to reduce the probability of fluorination induced by interaction with lithium between the first LLZO particle 15 and PVDF (polyvinylidene fluoride) in a positive electrode slurry. For a large number of first LLZO particles 15, concentrated electrical charges are required if agglomeration is to be avoided. In the modification of the first LLZO particle 15, an outer surface of the first LLZO particle 15 may exhibit exposed OH ions (including the third OH ion of the hydroxide ion layer 24 and the OH ion of dopamine molecules of the dopamine layer 35). By using the CTAB molecule 60, two ends of the CTAB molecule 60 each exhibit a positive and a negative electrical charge (as shown in Fig. (shown). The end of the CTAB molecule 60 with the positive electrical charge can attract the exposed OH ion and its entire electrical properties. Therefore, the completeness of the surface coating of the LLZO composite particle 100 can be increased accordingly, and agglomeration is prevented. The ions are also not exposed on the outer surface of the LLZO composite particle 100, thus preventing alkalization.

[0017] Since not all third OH ions of the hydroxide ion layer 24 and not all OH ions of the dopamine molecules of the dopamine layer 35 undergo the polymerization triggered by dehydration, exposed OH ions are formed. The CTAB molecule 60 can establish an attractive force with the exposed OH ions and thus form a layered protective structure, which makes the overall coating more complete.

[0018] A multitude of carbon nanotubes 42 and a multitude of nanoscale amorphous carbons 45 are deposited on an outer surface of the LLZO composite particle 100. The carbon nanotubes 42, the nanoscale amorphous carbons 45, and the LLZO composite particle 100 form a third-order LLZO composite particle 50 (as shown in Fig. (shown). The size of each of the carbon nanotubes 42 is 200 nm to 500 nm. The size of each of the nanoscale amorphous carbons 45 is 10 nm to 40 nm. Preferably, the nanoscale amorphous carbons 45 are amorphous carbons of a Super P auxiliary.

[0019] The ratio of the total weight of the carbon nanotubes 42 and the nanoscale amorphous carbons 45 to the weight of the first LLZO particle 15 is 0.2 to 2: 99.8 to 98.

[0020] Carbon nanotubes 42 and nanoscale amorphous carbons 45 are used as auxiliary materials. Since the nanoscale amorphous carbons 45 are in particle form and the carbon nanotubes 42 are in the form of long strips, several gaps form in the intermediate structure created by the carbon nanotubes 42, which cannot conduct electricity. Therefore, the nanoscale amorphous carbons 45 are filled into these gaps to transfer the electrical charge between the carbon nanotubes 42 by bridging the nanoscale amorphous carbons 35, thereby further increasing the electrical current transfer efficiency.

[0021] The advantages of carbon nanotubes 42 lie in the fact that lithium ions can be easily stabilized between them, thereby increasing lithium-ion conductivity. This very high lithium-ion conductivity helps the entire battery to charge and discharge quickly. Furthermore, the use of cobalt can also be reduced, thus lowering overall production costs.

[0022] The invention thus relates to an oxide particle coated with amino groups, which represents an LLZO composite particle; the LLZO composite particle comprises a first LLZO particle. A hydroxide ion layer is applied to an outer surface of the first LLZO particle. The hydroxide ion layer and the first LLZO particle form a second-order LLZO composite particle. A dopamine layer is applied to an outer surface of the second-order LLZO composite particle. Dopamine molecules of the dopamine layer are hydrophobic to protect the first LLZO particle and prevent it from becoming wet. A CTAB (cetyltrimethylammonium bromide) layer is applied to an outer surface of the dopamine layer. Some of the CTAB molecules are mixed in the dopamine layer and the hydroxide ion layer.

[0023] In describing the invention, it is obvious that it can be varied in many ways. Such variations are not to be considered a departure from the spirit and scope of the invention, and all modifications that would be obvious to a person skilled in the art are to fall within the scope of the following claims.

Claims

[1] An oxide particle coated with amino groups, which is an LLZO composite particle; the LLZO composite particle is used in an electrode of a solid-state or semi-solid-state battery; and the electrode comprises a substrate and an electrode slurry layer coated on the substrate; the LLZO composite particle comprises the following: a first LLZO particle, which serves to guide and distribute the paths of the lithium ions and to ensure that evenly distributed lithium ion channels are formed within the electrode; a hydroxide ion layer coated on an outer surface of the first LLZO particle; the hydroxide ion layer and the first LLZO particle form a second-order LLZO composite particle; the hydroxide ion layer is formed by a reaction of Tris molecules (tris(hydroxymethyl)aminomethane, ((HOCH2)3CNH2)) and has a plurality of third OH ions; each of the Tris molecules comprises three OH ions, namely a first, a second, and the third OH ion; wherein the first OH ions and the second OH ions of the Tris molecules are bonded by hydrogen bonds to oxidizing functional groups on the first LLZO particle; and wherein the third OH ions of the Tris molecules extend outward to an outer side of the first LLZO particle to form the hydroxide ion layer; and a dopamine layer coated on an outer surface of the second-order LLZO composite particle; wherein the dopamine layer is formed from a plurality of copolymerized dopamine molecules; wherein dehydration-induced polymerization is performed between OH ions of the dopamine molecules and the third OH ions of the hydroxide ion layer of a corresponding second-order LLZO composite particle to cause the dopamine layer to remain bonded to the second-order LLZO composite particle through the hydroxide ion layer; and wherein the dopamine molecules of the dopamine layer are hydrophobic to protect the first LLZO particle and prevent the first LLZO particle from becoming wet. [2] An oxide particle according to claim 1, wherein the LLZO composite particle further comprises a CTAB (cetyltrimethylammonium bromide) layer coated on an outer side of the dopamine layer; and wherein the CTAB layer consists of a plurality of CTAB (cetyltrimethylammonium bromide) molecules used as a surfactant. [3] An oxide particle according to claim 2, wherein in the CTAB layer, a part of the CTAB molecules having a certain polarity attracts molecules having an opposite polarity in the dopamine layer and the hydroxide ion layer to cause the part of the CTAB molecules within the dopamine layer and the hydroxide ion layer to be mixed; and wherein an excess of the CTAB molecules in the CTAB layer surrounds the outside of the dopamine layer by attractions formed between the polarities of the excess CTAB molecules. [4] An oxide particle according to claim 3, wherein a ratio of the total weight of the CTAB molecules in the CTAB layer and the total weight of the dopamine molecules of the dopamine layer is 0.1% to 0.3%; and wherein the CTAB layer serves to impart higher dispersivity to the first LLZO particle without agglomeration and to reduce the likelihood of fluorination induced by interaction with lithium between the first LLZO particle and a positive electrode slurry. [5] An oxide particle according to claim 1, wherein the electrode is a positive electrode. [6] An oxide particle according to claim 1, wherein the size of the LLZO composite particle is 50 nm to 200 nm. [7] An oxide particle according to claim 1, wherein the thickness of the hydroxide ion layer is 0.5 nm to 2 nm. [8] An oxide particle according to claim 1, wherein the thickness of the dopamine layer is 1 nm to 10 nm. [9] An oxide particle according to claim 1 or 2 or 3, wherein a plurality of carbon nanotubes and a plurality of amorphous carbons in nanoscale are coated on an outer surface of the LLZO composite particle. [10] An oxide particle according to claim 9, wherein the size of each of the carbon nanotubes is 200 nm to 500 nm; and the size of each of the amorphous carbon nanotubes is 10 nm to 40 nm. [11] An oxide particle according to claim 9, wherein a ratio of a total weight of the carbon nanotubes and the nano-sized amorphous carbons and a weight of the first LLZO particle is 0.2 to 2: 99.8 to 98.