POLYETHYLENE COEXTRUSION FILM
Patent Information
- Application Number
- DE502014016879
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2014-09-02
- Publication Date
- 2024-10-31
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Polyethylene coextrusion films with foamed core layers often exhibit surface waviness and roughness due to bubble-shaped cavities and pores, affecting the visual appearance and mechanical properties, which is undesirable for packaging applications.
The film is produced using the MuCell process with a core layer formed from particles and polyethylene, maintaining a high melt mass flow rate to create uniform, fine cavities, and the outer layers have lower melt mass flow rates to counteract core layer expansion, resulting in a smoother surface and improved mechanical properties.
The solution achieves a polyethylene coextrusion film with reduced surface waviness and roughness, enhanced mechanical properties, and a lower weight per unit area, suitable for packaging with improved stiffness and tear resistance.
Description
[0001] The invention relates to the technical field of multilayer plastic films with at least one foamed film layer.
[0002] Specifically, the invention relates to a polyethylene coextrusion film having a thickness between 20 µm and 250 µm comprising a foamed, particle-containing core layer between a first unfoamed heat-sealable outer layer and a second unfoamed outer layer.
[0003] The polyethylene coextrusion film is particularly suitable for the production of packaging, such packaging being able to be formed by heat sealing due to the first heat-sealable outer layer of the polyethylene coextrusion film, wherein either a film blank or a continuous web is formed into a packaging by folding or at least two film blanks or two film webs are joined by heat-sealed seams.
[0004] The polyethylene coextrusion film can be used both in a so-called FFS (Form Fill and Seal) process, in which a bag-shaped packaging is formed directly during the packaging of the contents, and in the production of prefabricated packaging that is then subsequently filled.
[0005] In addition, the polyethylene coextrusion film can also be used as a cover film for tray packaging, as a label or the like.
[0006] A film layer can be foamed for various reasons. Firstly, foaming results in a lower basis weight relative to the resulting thickness of the film and therefore a saving in material. Especially in combination with other unfoamed film layers, the greater thickness generally also results in an improvement in the mechanical properties relative to the amount of plastic used. If, for example, according to the preamble of patent claim 1, a foamed core layer is combined with unfoamed cover layers, a kind of plywood effect results, whereby the additional outer layers located apart are less likely to deform against one another due to the increase in volume of the core layer compared to an unfoamed design. In addition, foaming at least one film layer also influences the other physical properties of the resulting coextrusion film.
[0007] A polyethylene coextrusion film having the features of the preamble of patent claim 1 is known from JP 2004 009 522 A.
[0008] According to CA 1 145 724 A1, EP 0 512 740 B1, JP 2004-91024 A, EP 1 761 437 A1, JP 2007-230637 A and DE 10 2011 051 193 A1, a foamed film layer is used as a mechanical buffer in order to increase the puncture resistance or to compensate for mechanical deformations caused by the filling material to a certain extent.
[0009] At least one foamed foil layer can also be used for thermal insulation. Corresponding approaches are known from JP 2001-130586 A, US 6 913 389 B2, KR 2004-0005806, and KR 2004-0007381.
[0010] Furthermore, a foamed film layer in a film can also cause a weakening, which promotes tearing in a desired manner. Due to the lower density and the free spaces within the at least one foamed film layer, this can be torn relatively easily in the direction of its thickness. Depending on the specific design, foaming can also facilitate layer separation from an adjacent film layer, whereby these properties can be used for the production of tear-open packaging. Furthermore, if the film is torn perpendicular to its thickness, in particular if the tear propagates along the production direction, foaming also results in weakening.Depending on the manufacturing process, pronounced anisotropy can also be attributed to the fact that the pores or cavities formed during foaming are aligned in a production direction, so that tearing can occur particularly easily along the longitudinal direction of these cavities or pores (i.e., along the production direction). The use of foamed film layers to achieve defined tear properties is described, for example, in GB 2 110 215 B, US 4 762 230, US 4 781 294, EP 673 756 A1, JP 3823967, and DE 20 2005 002 615 U1.
[0011] The foaming of at least one film layer also leads to increased roughness or waviness of the film surface, whereby this effect is used to advantage according to DE 2 038 557 A1, DE 37 22 139 C2, DE 196 53 608 B4, JP 2001-055242 A, and EP 1 237 751 B1 B1. However, the waviness or roughness of the surface resulting from foaming is also undesirable in many cases, for example, when a surface as uniform, smooth, and as high-quality as possible is desired in packaging.
[0012] Another effect of a foamed film layer known from practice is that the corresponding film exhibits increased haze and opacity. For example, foaming can also reduce the use of color particles to create a non-transparent or merely translucent film. The increase in opacity and the use of this effect are described in EP 83 167 B1.
[0013] Various processes are known for producing films with at least one foamed film layer. Foaming can occur, in particular, through a chemical reaction or a physical process. For example, during extrusion, substances contained in the polymer melt can evaporate or react to form a gas. In this context, it is also possible to introduce microspheres into the polymer melt, which have a blowing medium within a meltable shell.
[0014] In physical foaming, a blowing agent is added to the molten plastic mass in the extruder under high pressure. Suitable blowing agents include water, nitrogen, or carbon dioxide.
[0015] Particularly uniform, good mechanical properties are achieved when the foamed layer has a particularly fine-cell foam structure, which can be achieved, for example, using the so-called MuCell process. Devices for carrying out this process or for retrofitting conventional extruders are sold by Drexel Inc., USA. The MuCell process is described in particular in US 5,866,053, US 6,051,174, EP 923,443 B1, EP 1,275,485, EP 377,650 A1, EP 580,777 B1, US 6,231,942, EP 996,536 A2, EP 1,040,158 B2, EP 1,131,387 B1, EP 1,283,767 B1, EP 1,337,387 A1, EP 1,539,868 B1, EP 1,337,387 A1, and EP 1,575,763 B1. The present invention relates in particular to polyethylene coextrusion films in which the foamed core layer is formed according to the described MuCell process.
[0016] During extrusion, a blowing agent is added to the melt for the core layer to be foamed, which causes it to foam during extrusion or immediately after it exits the extrusion gap. The blowing agent, previously added to the melt under pressure, experiences a sudden expansion upon exiting the die gap of the coextrusion die. Within the extruder, the blowing agent is usually present as a supercritical fluid, which combines the incompressibility of a liquid with the solvency properties of a gas. The blowing agent dissolves in the polymer melt and forms a distributed single-phase system with the plastic melt. Due to a rapid pressure drop upon exiting the extrusion die, nucleation nuclei form in the polymer melt. The gas dissolves from the melt, forming a very fine, uniform foam structure.The particles in the core layer can promote the formation of a particularly large number of small nucleation nuclei. Therefore, within the scope of the invention, the particles do not serve, or at least not exclusively, as a cheap bulk material, but are also used as a functional component to improve the film properties, namely for the formation of a particularly large number of small cavities or cells. Nevertheless, the particles can also be referred to as nucleating agents.
[0017] To enable the most uniform, fine formation of cavities or pores, it has proven advantageous to keep the solubility pressure in the melt at a high level for as long as possible, only then achieving a sudden pressure drop immediately upon the melt exiting an extrusion die. While extrusion dies for blown film extrusion or slot die extrusion often flare out conically or are straight, for foaming in a MuCell process, narrowing the die gap directly at the end of the gap can be advantageous in order to keep the melt pressure at a high level for as long as possible and achieve the steepest possible pressure drop.However, if the gap is too narrow, excessive resistance occurs during extrusion, and even in multilayer coextrusion with a foamed core layer and unfoamed outer layers, structural irregularities can occur if the melt flow is partially interrupted. Corresponding technical solutions are known from US 2012 / 228793 A and WO 2013 / 148841 A.
[0018] Further processes for producing a film or a plastic body with at least one foamed layer are also known from US 4 473 665, US 4 522 675, EP 580 777 B1, EP 843 246 B1, TW 384271, US 6 403 663 B1, EP 1 189 978 B1, US 7 341 683 B2, EP 1 857 501 A1 and EP 1 888 676 A2.
[0019] Various extrusion devices are the subject of EP 1 075 921 B1 and EP 1 719 600 A2.
[0020] The publications US 4,533,578, US 4,657,811, EP 237,977 B1, US 5,000,992, EP 5,553,522 A1, JP 11079192, US 6,096,793, EP 1,088,022 B1, JP 2002-154555, EP 1 297 067 B1, EP 1 646 677 B1, JP 2006-027185 A, JP 2007-045047 A, JP 2007-045046 A, EP 1 857 501 A1, EP 1 973 733 B1, EP 2 043 857 A2, WO 2008 / 100501 A2, WO 2009 / 155326 A1, EP 2 258 545 A1, JP 2013-111811 A, EP 2 668 036 A1, KR 2013-0100597 A and WO 2013 / 179947 A1 and DE 102012108705 A1 relate to further films or other plastic articles with a foamed layer or to the production thereof.
[0021] As explained above, the present invention specifically relates to a polyethylene coextrusion film, in particular for packaging, with a thickness between 20 µm and 250 µm, comprising a foamed, filler-containing core layer between a first unfoamed, heat-sealable outer layer and a second unfoamed outer layer. The polyethylene coextrusion film can be produced in particular using the MuCell process described above, with blown film coextrusion being preferred.
[0022] Due to the foamed core layer, known polyethylene coextrusion films with the features described above have the disadvantage that the outer layers are uneven due to the underlying core layer with bubble-shaped cavities and pores, which impairs the optical appearance.
[0023] Against this background, the object of the present invention is to provide a polyethylene coextrusion film which is easy to produce and has a lower waviness or roughness on the surface.
[0024] The subject of the invention and the solution to the problem is a polyethylene coextrusion film according to patent claim 1.
[0025] The melt mass-flow rate (MFR) is used to characterize the flow behavior of a thermoplastic under specified pressure and temperature conditions. The melt mass-flow rate is often used as a comparative value to characterize the flow properties of different plastics. According to DIN ISO EN 1133, it is defined as the mass of plastic that flows through a capillary of a specified size in 10 minutes at a specified temperature and pressure. Typically, the viscosity of a thermoplastic increases with the chain length of the polymer and the degree of branching, which correspondingly decreases the melt mass-flow rate.
[0026] According to the present invention, the core layer is formed from particles and the polymer component based on polyethylene and optionally also further processing aids, usually in a proportion of less than 10 wt. %. The entire polymer component based on polyethylene has, according to the invention, a melt mass flow rate (MFR) of more than 6 g / 10 min at 190 °C and 2.16 kg and is thus comparatively thin-flowing. Particularly in connection with the particles provided according to the invention, at the stated melt mass flow rate during production, small, very evenly distributed cavities can form in the core layer after exiting the gap of a coextrusion die, wherein the core layer, which is relatively thin-flowing during the extrusion process after exiting the extrusion die, is arranged between the two outer layers, thereby enclosing the core layer towards the outside.However, due to the high melt mass flow rate of more than 5 g / 10 min, preferably more than 6 g / 10 min, more preferably more than 8 g / 10 min and particularly preferably more than 10 g / 10 min at 190 °C and 2.16 kg, relatively uniform conditions prevail in the entire core layer immediately after extrusion, which promote particularly uniform foaming.
[0027] In particular, the invention also achieves that the outer layers have a low waviness and roughness on the surfaces of the outer layers compared to known polyethylene coextrusion films with a foamed core layer.
[0028] According to the invention, the melt mass flow rate is determined based on the entire polymer component of the core layer. For example, if the core layer contains different types of polyethylene, the melt mass flow rate is to be determined for the corresponding polymer mixture.
[0029] The proportion of particles in the core layer is between 5 and 50 wt.%, preferably between 10 and 30 wt.%.
[0030] As already described above, the first outer layer and the second outer layer serve as a type of boundary during coextrusion and foaming of the core layer, which also build up a certain counterpressure with regard to the expansion of the core layer. Preferably, the first outer layers have a significantly higher viscosity and thus a significantly lower melt mass flow rate according to DIN ISO EN 1133 at 190 °C and 2.16 kg. If the first and second outer layers each have a polyethylene or a polyethylene-based mixture as a polymer component, the melt mass flow rate (MFR) of the two polymer components is preferably below 3 g / 10 min, more preferably below 2 g / 10 min, and particularly preferably below 1 g / 10 min.
[0031] In other words, the ratio of the melt mass flow rate of the polymer component of the core layer to the melt mass flow rate of the polymer components of the two outer layers is preferably about 2, more preferably at least 3, and particularly preferably at least 6. Ratios of more than 10 can also be readily achieved within the scope of the invention. The ratio thus formed clearly shows that the two outer layers are significantly more viscous than the core layer. Taking these specifications into account, films with a relatively uniform, flat surface could be formed in preliminary tests.It is assumed that this is partly due to the fact that the two outer layers, with their low melt mass flow rate, exert increased backpressure upon expansion of the core layer immediately upon extrusion. On the other hand, the comparatively viscous outer layers are less susceptible to deformation due to the formation of individual cavities and bubbles in the core layer. The outer layers are therefore too viscous to be subjected to significant deformation from a substantially flat orientation.
[0032] The first heat-sealable outer layer and the second outer layer may comprise polymer blends having an equal or approximately equal melt mass flow rate to provide approximately equal back pressure upon expansion of the core layer, as previously described.
[0033] According to an alternative embodiment of the invention, the first, heat-sealable outer layer has a higher melt mass flow rate than the second outer layer. The first outer layer, intended as the sealing layer, is often arranged on the inside so that a certain slight waviness can be tolerated there, while the second, usually outer layer, should be as smooth as possible. The first outer layer can, for example, have a melt mass flow rate of 2 to 3 g / 10 min, while the second outer layer has a melt mass flow rate of 1 g / 10 min. With such an asymmetric setting of the melt mass flow rate, the surface of the second outer layer can ultimately be made even smoother, since during foaming of the core layer the individual cells spread more towards the first outer layer and are more likely to lead to unevenness there.
[0034] As described above, within the scope of the invention, the MuCell process described at the outset is preferably used for foaming the core layer, whereby a microcell structure is created in the core layer. The microcell structure is characterized by a pore structure with an average pore size of less than 100 µm, whereby the pore size can also be in the range between 0.1 µm and 10 µm. Since the individual pores or cavities can be aligned to a certain extent in the production direction due to the coextrusion process, the volume of the closed cavities in the core layer is a suitable characteristic feature, whereby the volume is preferably less than 50,000 µm 3< , preferably less than 20,000 µm 3< and, for example, less than 5,000 µm 3<.
[0035] If, according to a preferred embodiment of the invention, nitrogen is used as a blowing agent for the physical foaming, the core layer has correspondingly closed cavities filled with nitrogen.
[0036] The degree of foaming can be adjusted by the amount of blowing agent added, the viscosity of the polymer components of the core layer and outer layers, and the extrusion conditions. The core layer preferably has a density between 0.2 g / cm 3 and 0.8 g / cm 3 . The increase in thickness of the core layer compared to an unfoamed layer with the same amount of polymer is therefore typically between about 20% and 500%, more preferably between about 40% and 200%, and most preferably between 50% and 120%.
[0037] The polyethylene coextrusion film according to the invention is characterized by a low basis weight and thus a lower material usage compared to a completely unfoamed film. Adequate mechanical properties with regard to stiffness and tear resistance can be achieved by appropriately matching the layer thicknesses of the polyethylene coextrusion film. The thickness of the foamed core layer is preferably between 30% and 70% of the total thickness of the entire polyethylene coextrusion film. Accordingly, the two outer layers each have a thickness between approximately 15% and 30% of the total thickness of the polyethylene coextrusion film.
[0038] Preliminary tests have shown that the quality of the surfaces of the outer layers increases with an increasing melt mass flow rate of the polymer component of the core layer, although this may result to a certain extent in an impairment of the mechanical properties of the polyethylene coextrusion film.
[0039] The polymer component of the core layer can contain a linear polyethylene as its main component, including types obtained with metallocene catalysts. Linear polyethylenes of high (LHDPE), medium (LMDPE), and low (LLDPE) density are suitable. In principle, all known linear types of polyethylene, i.e., alpha-olefin copolymers based on polyethylene, are suitable. Copolymers with hexene (C6) and octene (C8) are preferred.
[0040] The various types of linear polyethylene described above allow for a wide range of mechanical properties. Especially with regard to packaging, a low-density linear polyethylene is often advantageous to avoid packaging that is too stiff and brittle.
[0041] However, a mixture containing at least one other low-density polyethylene in addition to the linear polyethylene, in particular a linear low-density polyethylene (LLDPE), is also preferred for the polymer component of the core layer. This mixture can be, without limitation, a non-linear low-density polyethylene (LDPE) or a linear low-density polyethylene (mLLDPE) obtained using metallocene catalysts. Within the scope of these embodiments, linear polyethylene is also provided as the main constituent of the polymer component of the core layer. The core layer can, for example, be formed from 10 to 30% by weight of particles including processing aids, 10 to 30% by weight of LDPE or mLLDPE, and the remainder LLDPE.
[0042] The present invention relates to a polyethylene coextrusion film which has at least three layers, comprising the two outer layers and the core layer. Although additional layers may be present in principle, a three-layer design is preferred, in which the outer layers directly adjoin the core layer on opposite sides.
[0043] The first non-foamed, heat-sealable outer layer enables the formation of a package by heat sealing. Therefore, the first outer layer is usually placed on the inside of the package.
[0044] The second outer layer, in contrast, is arranged toward the outer side of the packaging, whereby the second outer layer can either form an exposed surface or be laminated with another cover film. The second outer layer can, for example, be laminated with an adhesive to a cover film, which can contain, without limitation, polyethylene terephthalate (PET), biaxially oriented polypropylene (BO-PP), or even polyethylene. Within the scope of the latter variant, a packaging film that is essentially single-material can also be provided.
[0045] Within the scope of the invention, it can be provided that at least one of the two outer layers contains color particles in order to obtain an overall opaque film. This can also take advantage of the fact that the core layer is clouded at least to a certain extent by the foaming process, so that the proportion of color particles can then possibly be reduced compared to an unfoamed coextrusion film.
[0046] Even if, within the scope of the invention, less waviness and surface roughness can be achieved, particularly on the surface of the second outer layer, the residual waviness due to the foamed core layer, which cannot be avoided even within the scope of the invention, can lead to impairments in a glossy surface. In particular, with a glossy surface, surface roughness visible due to light refraction cannot be avoided in all cases; to a certain extent, this roughness is reminiscent of the texture of orange peel.
[0047] Surprisingly, this impression can be completely avoided if the second outer layer is matte, laminated with a matte film, or coated with a matte coating. Even if these measures do not reduce the actual unevenness at all, or at least not significantly, the waviness is no longer visible due to diffuse light refraction. Surprisingly, this is especially true for the structure resulting from foaming, which, on a glossy surface, creates the impression of uneven waves or dents for the user.
[0048] When matte raw materials are used for the second unfoamed outer layer or when the second unfoamed outer layer is coated with a matte varnish, the polyethylene coextrusion film preferably has a matte surface with a reflectometer value according to DIN 67530 at a measuring angle of 85° of less than 40, preferably less than 30, in particular between 10 and 25. Accordingly, the reflectometer value according to DIN 67530 at a measuring angle of 60° is usually less than 30, preferably less than 20, and in particular between 5 and 15. At a measuring angle of 20°, the reflectometer value is usually less than 10, preferably less than 5, and in particular between 1 and 3.
[0049] If, according to an alternative embodiment of the invention, the polyethylene coextrusion film is bonded to a matte film on the second outer layer as a lamination layer, the indicated reflectometer values are preferably obtained on the surface of the additionally laminated cover film.
[0050] The invention is explained below using exemplary embodiments.
[0051] In the course of exploratory tests, three formulations were considered for the first unfoamed, heat-sealable outer layer as the sealing layer, the core layer and the second unfoamed outer layer.
[0052] To provide a sealing layer with conventional sealing properties, the first outer layer can be formed from a material composition A1 comprising polyethylene with a density between 0.92 and 0.94 g / cm 3 , with particular consideration given to blends of linear and non-linear polyethylene types. To provide a low-sealing first outer layer as a sealing layer, a polyethylene with a density of 0.905 to 0.917 g / cm 3 (ULDPE) can be used as material A2. For a very low-sealing sealing layer, however, a polymer material A3 based on polyethylene with a density of less than 0.905 g / cm 3 can be used.
[0053] The composition of the core layer can be based on the desired properties of the polyethylene coextrusion film.
[0054] In particular, for the formation of comparatively thick films where a slightly higher surface roughness can be accepted and where a high seal seam strength is desired, a material B1 with 20 wt.% talc as filler and the remainder LLDPE C8 with a melt mass flow rate of 6 to 8 can be used for the core layer.
[0055] For thinner films with improved, lower surface roughness and low seal seam strength, however, a material B2 with 20 wt.% talc, 20% LDPE and the remainder LLDPE is preferably used, whereby the two polyethylene types mentioned have a melt mass flow rate between 6 and 8, so that, as expected, the melt mass flow rate of the polymer component formed from LLDPE and LDPE also has corresponding values.
[0056] The third material, B3, is a composition of 20% talc, 20% mLLDPE with an MFI of 15 to 20, and the remainder LLDPE with an MFI of 6 to 8. Formulation B3 is suitable for both thin and thick films and results in good seal strength and good surface properties with low surface roughness. However, compared to materials B1 and B2, it results in somewhat more difficult coextrusion processes and increased material costs.
[0057] The second unfoamed outer layer, together with the first unfoamed outer layer, contributes to the stiffness and strength of the polyethylene coextrusion film. Consequently, the mechanical properties of the entire polyethylene coextrusion film can be significantly influenced by the material of the second outer layer. The first material C1 for the second outer layer is a polyethylene blend of LDPE and LLDPE with a density of approximately 0.92 g / cm³.
[0058] To achieve increased rigidity, a blend of LDPE and LMDPE with a density between 0.925 and 0.935 g / cm 3 can be used as material C2. Finally, a comparatively high rigidity can be achieved if a third material C3 for the second unfoamed outer layer is blended with LDPE and linear high-density polyethylene (LHDPE), with the resulting total density of the blend C3 being between 0.935 and 0.95 g / cm 3.
[0059] Depending on the specific requirements, the different formulations for the individual layers can be freely combined. For example, if a comparatively thin film with low surface roughness is desired, which offers low sealing strength with low seal seam strength and high rigidity, a layer structure A2 / B2 / C3 is preferred. Of course, all other combinations are also possible, depending on the specific requirements.
[0060] Another exemplary layer structure is described in Table 1. The thickness ratios are given relative to an unfoamed core layer. Thus, when the core layer is foamed, the thickness ratio changes accordingly. Table 1 Layer: first outer layer core layer second outer layer Layer thickness unfoamed: 29% 42% 29% Components: 57% mLLDPE-C8 Density: 0.925 g / cm 3 < / MFI 0.85 77% LLDPE-C8 Density: 0.919 g / cm 3 < / MFI 6 71% mLLDPE-C8 Density: 0.925 g / cm 3 < / MFI 0.85 28% LDPE Density: 0.929 g / cm 3 < / MFI 0.55 20% talc batch (with 60% talc) 26% LDPE Density: 0.923 g / cm 3 < / MFI 2 14% white batch (with 60% TiO2) 2% lubricant antiblock batch 2% lubricant antiblock batch 1% fluoropolymer batch (processing aid) 1% thermal stabilizer batch 1% fluoropolymer batch (processing aid) specified thickness measured thickness (DIN 53370) Basis weight Force at break (DIN EN ISO 527-1) Elongation at break (DIN EN ISO 527-1) Bending stiffness 30° / 10 mm (DIN 53121) Tensile strength according to Elemdorf (ISO 6383 / 2) Opacity (DIN 53146) Coefficient of friction COF (DIN EN ISO 8295) Seal strength Water vapor transmission rate WVTR (DIN 53122-1) unfoamed / foamed - - Production direction MD Transverse direction CD MD CD MD CD MD CD - first outer layer against first outer layer first outer layer against metal 150 °C / 1.5s / 3 bar x°C / x% RH µm / µm µm g / m 2 N / Inch N / Inch % % mN mN mN mN % 1 1 N / Inch g / (m 2 < *day) Comparison example 100 / 100 98,9 94,7 73,9 69,1 692 919 25,4 36,6 6954 34519 78 0,15 0,20 44,5 2,8 Slide 1 90 / 100 98,9 86,3 59,5 38,5 639 607 26,4 34,4 7168 28352 80 0,18 0,19 40,3 3,2 Slide 2 80 / 100 103,3 75,5 41,4 27,0 451 500 25,6 35,5 1961 22267 77 0,16 0,23 35,2 4,9 Slide 3 70 / 100 104,6 65,6 36,7 23,1 432 497 22,4 28,7 1398 13802 75 0,16 0,25 28,9 3,2 Slide 4 60 / 100 105,1 59,0 27,1 13,2 293 125 19,7 17,7 999 10632 77 0,21 0,30 29,3 7,2 Slide 5 100 / 110 107,7 97,4 65,9 41,8 672 643 34,3 44,4 6669 32578 81 0,16 0,21 42,3 2,9 Slide 6 100 / 120 117,6 97,3 54,6 34,3 554 513 47,1 58,5 4286 31272 82 0,18 0,22 39,7 3,5 Slide 7 100 / 130 127,7 97,1 55,0 30,3 497 486 54, 6 68,9 2321 29224 85 0,14 0,21 37,8 3,9 Slide 8 100 / 140 138,0 98,3 48,3 28,1 465 419 65, 7 74,3 2067 23923 84 0,17 0,23 35,7 4,7
[0061] Based on the material composition shown in Table 1, the total thickness relative to the unfoamed state (i.e., the basis weight) and the degree of foaming of the core layer were varied in tests. The results show that foaming increases the flexural rigidity of the polyethylene coextrusion film in both the production direction (MD) and the transverse direction (CD).
[0062] To achieve a specified stiffness value compared to an unfoamed film, less material is required. Foaming reduces the seal strength, but the foaming of the core layer also makes the polyethylene coextrusion film more easily stretchable, with relatively little impact on its mechanical properties. In addition, the water vapor transmission rate increases to a certain extent due to foaming.
[0063] The properties of the material composition according to Table 1 are shown in Table 2.
[0064] The first column of Table 2 compares the thickness in the foamed state with the thickness that would result from using the same material (without a foaming agent). The first column refers to standard values. The comparison example therefore concerns a film that is not foamed. The thicknesses given for an unfoamed and a foamed configuration determine the degree to which the core layer is foamed.
[0065] The second column concerns the actual thickness determined for a film specifically formed according to the specifications.
[0066] The other columns reveal various characteristic parameters.
[0067] The polyethylene coextrusion film according to the invention is intended for use in particular for packaging, although other applications are also conceivable. For example, the polyethylene coextrusion film can be used as a label film, in which case a particularly smooth surface is also desired. The same applies to the use of the polyethylene coextrusion film as a surface protection film, in which case the foamed core layer can also provide mechanical damping and, through such a buffer effect, offer increased protection. Finally, the polyethylene coextrusion film according to the invention also has a more pleasant, softer feel than an unfoamed film, resulting in a more textile-like feel.The foamed film can therefore also be used to a certain extent as a substitute for a textile or at least suggest textile properties that are desirable, for example, in clothing, disposable hygiene products or the like.
[0068] It can also be used for adhesive tape, whereby the foamed core layer can then compensate for mechanical stresses to a certain extent.
[0069] Due to its relatively high thickness and low basis weight, the polyethylene coextrusion film can also be used as a type of seal in the form of a closure label, for example to indicate an original closure on screw caps or other containers, whereby such a closure label is torn when opened for the first time.
[0070] Finally, due to its softer nature compared to film, polyethylene coextrusion film can also be used as a kind of water-resistant substitute for paper. Fillers and additives can optionally be added to at least one of the outer layers to improve writable properties. Suitable additives for this purpose include kaolin and chalk.
[0071] Finally, it is also possible to introduce active substances into the cavities and cells during the foaming process, which then remain effective over a long period of time. In the case of packaging, these could be, for example, special fragrances, absorbers, or the like. Such substances are preferably introduced with the foaming agent during extrusion.
Claims
1. A coextruded polyethylene film, particularly for packaging, with a thickness between 20 µm and 250 µm comprising a foamed core layer between a first unfoamed heat-sealable outer layer and a second unfoamed outer layer, wherein the core layer comprises a polyethylene or a polyethylene-based mixture as a polymer component having a melt mass-flow rate (MFR) according to DIN ISO EN 1133 of greater than 5 g / 10 min at 190 °C and 2.16 kg, characterised in that the core layer and the unfoamed outer layers are formed jointly by blown film coextrusion, and in that the core layer contains particles, wherein the proportion of the particles is between 5 and 50 wt.%.
2. The coextruded polyethylene film according to claim 1, characterised in that the first and the second outer layer each have a polyethylene or a polyethylene-based mixture as a polymer component, wherein the polymer components of the first outer layer and of the second outer layer each have a melt mass-flow rate (MFR) according to DIN ISO EN 1133 of less than 3 g / 10 min, in particular less than 1 g / 10 min at 190 °C and 2.16 kg.
3. The coextruded polyethylene film according to claim 1 or 2, characterised in that the first outer layer has a higher melt mass-flow rate (MFR) than the second outer layer.
4. The coextruded polyethylene film according to any one of claims 1 to 3, characterised in that the foamed core layer has closed cells filled with nitrogen or carbon dioxide.
5. The coextruded polyethylene film according to any one of claims 1 to 4, characterised in that the foamed core layer has closed cells with a volume of less than 50000 µm3.
6. The coextruded polyethylene film according to any one of claims 1 to 5, characterised in that the core layer has a density between 0.2 g / cm3 and 0.8 g / cm3.
7. The coextruded polyethylene film according to any one of claims 1 to 6, characterised in that the thickness of the foamed core layer is between 40 % and 70 % of the total thickness.
8. The coextruded polyethylene film according to any one of claims 1 to 6, characterised in that the polymer component of the core layer contains a linear polyethylene as the main component, including types obtained with metallocene catalysts.
9. The coextruded polyethylene film according to claim 8, characterised in that the polymer component of the core layer contains at least one other low-density polyethylene besides the linear polyethylene.
10. The coextruded polyethylene film according to any one of claims 1 to 9, characterised in that the outer layers are immediately adjacent to the core layer on opposite sides.
11. The coextruded polyethylene film according to any one of claims 1 to 10, characterised in that at least one of the outer layers contains coloured particles.
12. The coextruded polyethylene film according to any one of claims 1 to 11, characterised in that the second outer layer has a matte surface with a reflectometer value according to DIN 67530 of less than 40 at an angle of measurement of 85°.