SILICON DIOXIDE GRANULES FOR THE PRODUCTION OF QUARTZ GLASS BODY
Patent Information
- Application Number
- DE502016016764
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2015-12-18
- Filing Date
- 2016-12-16
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2036-12-16
AI Technical Summary
Current manufacturing processes for quartz glass struggle with producing high-purity glass bodies that are bubble-free, transparent, and cost-effective, often resulting in irregularities, contamination, and high production costs due to impurities and inefficient raw material usage.
The development of silicon dioxide granules with specific properties, such as a BET surface area of 20 to 50 m²/g and a bulk density of 0.5 to 1.2 g/cm³, which are used to produce quartz glass bodies through a method involving the formation of a glass melt without the need for pre-compression, allowing for efficient and bubble-free glass production.
This approach enables the production of quartz glass bodies with improved homogeneity, transparency, and reduced impurities, leading to longer service life, lower production costs, and increased efficiency in manufacturing, while also utilizing previously discarded materials as a cost-effective raw source.
Description
[0001] The invention relates to a silicon dioxide granulate, wherein the silicon dioxide granulate has the following features: A) a BET surface area in a range of 20 to 50 m 2 / g; B) a bulk density in a range of 0.5 to 1.2 g / cm 3 ; C) an average particle size in a range of 50 to 500 µm; D) a carbon content of less than 50 ppm; E) an aluminum content of less than 200 ppb, F) a tapped density in a range of 0.7 to 1.3 g / cm 3 ; H) a pore volume in a range of 0.1 to 2.5 mL / g; I) a particle size distribution D 10 in a range of 50 to 150 µm; J) a particle size distribution D 50 in a range of 150 to 300 µm; and K) a particle size distribution D 90 in a range of 250 to 620 µm; The particle size distribution of the silicon dioxide granules is determined according to DIN ISO 13322:2009; the ppm and ppb are each based on the total weight of the silicon dioxide granules. Background of the invention
[0002] Quartz glass, quartz glass products, and products containing quartz glass are well known. Various processes for producing quartz glass and quartz glass bodies are also already known. Nevertheless, considerable efforts are still being made to develop manufacturing processes that can produce quartz glass of even higher purity, meaning the absence of impurities. For example, some applications of quartz glass and its processed products place particularly high demands, for example, with regard to homogeneity and purity. This is the case, among other things, for quartz glass that is processed into light guides or in lighting devices. Impurities can cause absorption here. This is disadvantageous because it leads to color changes and the attenuation of the emitted light. Another example for the use of high-purity quartz glass is production steps in semiconductor manufacturing.Any contamination of the glass body potentially leads to defects in the semiconductors, and thus to scrap during production. The high-purity quartz glass grades used for these processes, especially high-purity synthetic quartz glass grades, are therefore very complex to produce and are expensive.
[0003] Furthermore, there is a market demand for the aforementioned high-purity quartz glass, especially high-purity synthetic quartz glass, and products made from it at a lower price. Therefore, there is an effort to offer high-purity quartz glass at a lower price than before. To this end, both more cost-effective manufacturing processes and cheaper raw material sources are being sought.
[0004] Known processes for producing quartz glass bodies involve melting silicon dioxide and forming it from the melt into quartz glass bodies. Examples include EP 3 000 790 A1, DE 10 2020 008 162 A1, and EP 1 148 035 A2. Irregularities in a glass body, for example, due to the inclusion of gases in the form of bubbles, can lead to failure of the glass body under load, particularly at high temperatures, or preclude its use for a specific purpose. For example, impurities in the raw material used to form quartz glass can lead to the formation of cracks, bubbles, streaks, and discoloration in the quartz glass. Furthermore, when used in processes for the production and treatment of semiconductor components, impurities in the glass body can be worked out and transferred to the treated semiconductor components. This is the case, for example, in etching processes and then leads to rejects in the semiconductor blanks.A frequently occurring problem with the known manufacturing processes is therefore the insufficient quality of the quartz glass bodies.
[0005] Another aspect concerns raw material efficiency. It appears advantageous to use quartz glass and its raw materials, which are generated as byproducts elsewhere, for industrial processing into quartz glass products, rather than using these byproducts as filler material, for example, in building construction, or disposing of them costlyly as waste. These byproducts are often captured as particulate matter in filters. This particulate matter poses further problems, particularly with regard to health, occupational safety, and handling. Tasks
[0006] An object of the present invention is to at least partially overcome one or more of the disadvantages resulting from the prior art.
[0007] A further object of the invention is to provide light guides, lamps, and components with a long service life. Components are understood, in particular, to be devices that can be used for or in reactors for chemical and / or physical treatment steps.
[0008] It is a further object of the invention to provide light guides, lamps and components made of glass which are bubble-free or have a low level of bubbles.
[0009] It is a further object of the invention to provide light guides, lighting means and components made of glass which have a high degree of transparency.
[0010] It is a further object of the invention to provide light guides, lighting means and components which have low opacity.
[0011] It is a further object of the invention to provide optical fibers with low attenuation.
[0012] A further object of the invention is to provide light guides, lighting devices, and components that exhibit high dimensional stability. In particular, it is an object of the invention to provide light guides, lighting devices, and components that do not deform at high temperatures. In particular, it is an object of the invention to provide light guides, lighting devices, and components that remain dimensionally stable even when formed with large dimensions.
[0013] It is a further object of the invention to provide light guides, lamps and components that are tear and break resistant.
[0014] It is a further object of the invention to provide light guides, lighting devices and components that can be manufactured efficiently.
[0015] It is a further object of the invention to provide light guides, lighting devices and components that can be manufactured cost-effectively.
[0016] It is a further object of the invention to provide light guides, lamps and components in the manufacture of which long post-treatment steps, for example tempering, can be dispensed with.
[0017] A further object of the invention is to provide light guides, lamps, and components that exhibit high thermal shock resistance. In particular, it is an object of the invention to provide light guides, lamps, and components that exhibit low thermal expansion under strong thermal fluctuations.
[0018] It is a further object of the invention to provide light guides, lighting devices and components which have a high degree of hardness.
[0019] A further object of the invention is to provide light guides, lamps, and components that exhibit high purity and low contamination with foreign atoms. Foreign atoms are understood to be components that have not been deliberately introduced.
[0020] It is a further object of the invention to provide light guides, illuminants and components that contain a small amount of dopants.
[0021] It is a further object of the invention to provide light guides, lamps, and components that exhibit high homogeneity. Homogeneity of a property or substance is a measure of the uniform distribution of that property or substance in a sample.
[0022] A particular object of the invention is to provide light guides, lamps, and components that exhibit high material homogeneity. Material homogeneity is a measure of the uniform distribution of elements and compounds contained in the light guide, lamp, or semiconductor device, in particular OH, chlorine, metals, especially aluminum, alkaline earth metals, refractory metals, and dopants.
[0023] It is a further object of the invention to provide a quartz glass body which is suitable for use in light guides, lighting devices and components made of quartz glass and which at least partially solves at least one, preferably several, of the objects already described.
[0024] It is a further object of the invention to provide a quartz glass body having a rectilinear shape. In particular, it is a further object to provide a quartz glass body having a high bending radius. In particular, it is a further object to provide a quartz glass body having a high curl parameter.
[0025] Another task is to provide a quartz glass body in which the migration of cations is as low as possible.
[0026] A further object is to provide a quartz glass body that has a high homogeneity over the entire length of the quartz glass body.
[0027] In particular, it is an object of the invention to provide a quartz glass body which has a high refractive index homogeneity over the entire length of the quartz glass body.
[0028] In particular, it is an object of the invention to provide a quartz glass body which has a high homogeneity of viscosity over the entire length of the quartz glass body.
[0029] In particular, it is an object of the invention to provide a quartz glass body which has a high material homogeneity over the entire length of the quartz glass body.
[0030] In particular, it is an object of the invention to provide a quartz glass body which has a high optical homogeneity over the entire length of the quartz glass body.
[0031] It is a further object of the invention to provide a silicon dioxide powder having a high sintering activity.
[0032] It is a further object of the invention to provide a silicon dioxide powder having a low sintering temperature.
[0033] It is a further object of the invention to provide a silicon dioxide powder from which stable granules can be obtained.
[0034] It is a further object of the invention to provide a silicon dioxide granulate that is easy to handle.
[0035] It is a further object of the invention to provide a silicon dioxide granulate which has a low particulate matter content.
[0036] Another task is to provide a silicon dioxide granulate that can be easily stored, transported and conveyed.
[0037] It is a further object of the invention to provide silicon dioxide granules capable of forming bubble-free quartz glass bodies. It is a further object of the invention to provide silicon dioxide granules that, as a bulk material, enclose as little gas volume as possible.
[0038] It is a further object of the invention to provide an open-pore silicon dioxide granulate.
[0039] It is a further object of the invention to provide a method by which quartz glass bodies can be produced, by means of which at least some of the objects already described are at least partially achieved.
[0040] It is a further object of the invention to provide a method by which quartz glass bodies can be manufactured more easily.
[0041] It is a further object of the invention to provide a method by which quartz glass bodies can be produced continuously.
[0042] It is a further object of the invention to provide a method by which quartz glass bodies can be produced by a continuous melting and forming process.
[0043] It is a further object of the invention to provide a method by which quartz glass bodies can be formed at a higher speed.
[0044] It is a further object of the invention to provide a method by which quartz glass bodies can be produced with low waste.
[0045] It is a further object of the invention to provide a method with which customizable quartz glass bodies can be produced.
[0046] It is a further object of the invention to provide a method for producing quartz glass bodies in which a silicon dioxide granulate can be processed in a melting furnace without having to be subjected beforehand to a targeted densification step, e.g. by a temperature treatment of more than 1000 °C.
[0047] In particular, it is an object of the invention to provide a method for producing quartz glass bodies in which a silicon dioxide granulate having a BET of 20 m 2 < / g or more can be introduced into a melting furnace, melted and processed into a quartz glass body.
[0048] It is a further object of the invention to provide an automated method by which quartz glass bodies can be produced.
[0049] Another task is to further improve the processability of quartz glass bodies.
[0050] Another task is to further improve the fabrication of quartz glass bodies. Subject of the invention
[0051] The independent claim contributes to at least partially fulfilling at least one of the aforementioned tasks. |1| A silicon dioxide granulate, the silicon dioxide granulate having the following features: A) a BET surface area in a range of 20 to 50 m 2 / g; B) a bulk density in a range of 0.5 to 1.2 g / cm 3 ; C) an average particle size in a range of 50 to 500 µm; D) a carbon content of less than 50 ppm; E) an aluminum content of less than 200 ppb; F) a tapped density in a range of 0.7 to 1.3 g / cm 3 ; H) a pore volume in a range of 0.1 to 2.5 mL / g; I) a particle size distribution D 10 in a range of 50 to 150 µm; J) a particle size distribution D 50 in a range of 150 to 300 µm; K) a particle size distribution D 90 in a range from 250 to 620 µm, the particle size distribution of the silicon dioxide granules being determined according to DIN ISO 13322:2009; the ppm and ppb are each based on the total weight of the silicon dioxide granules. General
[0052] In this description, range specifications also include the values referred to as limits. A specification such as "in the range from X to Y" with respect to a quantity A therefore means that A can assume the values X, Y, and values between X and Y. Unilaterally limited ranges such as "up to Y" for a quantity A correspondingly mean values Y and less than Y. Detailed description of the invention
[0053] A method for producing a quartz glass body comprising the following process steps is not claimed. The silicon dioxide granulate according to the invention can be used in this process: i.) Providing a silicon dioxide granulate; ii.) Forming a glass melt from the silicon dioxide granulate; and iii.) Forming a quartz glass body from at least a portion of the glass melt. Step i.)
[0054] This may include the provision of the silicon dioxide granules through the following process steps: I. Providing a silicon dioxide powder; and II. Processing the silicon dioxide powder into silicon dioxide granules, wherein the silicon dioxide granules have a larger particle diameter than the silicon dioxide powder.
[0055] Preferably, during processing, a silicon dioxide granulate comprising granules is formed, wherein the granules have a spherical morphology; more preferably, the processing includes spray granulation or roll granulation.
[0056] A powder is understood to mean particles of dry solid substances with a primary particle size in the range of 1 to less than 100 nm.
[0057] Silica granules can be obtained by granulating silica powder. Silica granules typically have a BET surface area of 3 m² / g or more and a density of less than 1.5 g / cm³. Granulation is the conversion of powder particles into granules. During granulation, several silica powder particles form aggregates, i.e., larger agglomerates called "silica granules." These are often also referred to as "silica granule particles" or "granulate particles." Together, the granules form a granulate, e.g., the silica granules form "silica granules." Silica granules have a larger particle diameter than silicon dioxide powder.
[0058] The process of granulation to convert a powder into granules will be explained in more detail later.
[0059] In the present context, silicon dioxide grains are understood to mean silicon dioxide particles obtainable by comminuting a silicon dioxide body, in particular a quartz glass body. A silicon dioxide grain generally has a density of more than 1.2 g / cm 3 , for example, in a range from 1.2 to 2.2 g / cm 3 , and particularly preferably of approximately 2.2 g / cm 3 . Further preferably, the BET surface area of a silicon dioxide grain is generally less than 1 m 2 / g, determined according to DIN ISO 9277:2014-01.
[0060] In principle, any silicon dioxide particles suitable for a person skilled in the art can be considered as silicon dioxide particles. Silicon dioxide granules and silicon dioxide grains are preferred.
[0061] A particle diameter or particle size is understood to be the diameter of a particle, which is defined as "area equivalent circular diameter x Ai " according to the formula x Ai = 4 A i π where Ai is the area of the particle being examined in an image analysis. Suitable methods for determination include ISO 13322-1:2014 or ISO 13322-2:2009. Comparative information such as "larger particle diameter" always means that the related values were determined using the same method. Silicon dioxide powder
[0062] Within the scope of the present invention, it is in principle possible to obtain silicon dioxide powder from naturally occurring or synthetically produced silicon dioxide. Synthetic silicon dioxide powder is preferably used. Pyrogenically produced silicon dioxide powder is particularly preferred.
[0063] The silicon dioxide powder can be any silicon dioxide powder containing at least two particles. Any method that is familiar to the person skilled in the art and appears suitable for the present purpose can be used as the manufacturing method.
[0064] Silicon dioxide powder can arise as a byproduct during the production of quartz glass, particularly in the manufacture of soot bodies. Silicon dioxide from this source is often referred to as "soot dust."
[0065] A preferred source for the silicon dioxide powder is silicon dioxide particles obtained during the synthetic production of soot bodies using flame hydrolysis burners. During the production of a soot body, a rotating support tube with a cylindrical surface is reversibly moved back and forth along a row of burners. Oxygen and hydrogen, as well as the starting materials for the formation of silicon dioxide primary particles, can be supplied to the flame hydrolysis burners as burner gases. The silicon dioxide primary particles preferably have a primary particle size of up to 100 nm. The silicon dioxide primary particles produced by flame hydrolysis aggregate or agglomerate to form silicon dioxide particles with particle sizes of approximately 9 µm (DIN ISO 13320:2009-1).The shape of the primary silicon dioxide particles in the silicon dioxide particles can be identified by scanning electron microscopy, and the primary particle size can be determined. A portion of the silicon dioxide particles is deposited on the cylindrical surface of the carrier tube rotating around its longitudinal axis. This builds up the soot body layer by layer. Another portion of the silicon dioxide particles is not deposited on the cylindrical surface of the carrier tube, but accumulates as dust, e.g., in a filter system. This other portion of silicon dioxide particles forms the silicon dioxide powder, often referred to as "soot dust." As a rule, the portion of silicon dioxide particles deposited on the carrier tube is larger than the portion of silicon dioxide particles accumulating as soot dust during soot body production, based on the total weight of the silicon dioxide particles.
[0066] Today, soot dust is usually disposed of as waste, which is a complex and costly process, or used as filler without added value, for example, in road construction, as aggregate in the dye industry, as a raw material for tile production, and for the production of hexafluorosilicic acid, which is used to rehabilitate building foundations. In the case of the present invention, it is suitable as a starting material and can be processed into a high-quality product.
[0067] Silica produced by flame hydrolysis is commonly referred to as fumed silica. Fumed silica is typically in the form of amorphous silica primary particles or silica particles.
[0068] Preferably, the silicon dioxide powder can be produced by flame hydrolysis from a gas mixture. In this case, the silicon dioxide particles are also formed in the flame hydrolysis and removed as silicon dioxide powder before agglomerates or aggregates form. Here, the silicon dioxide powder, previously referred to as soot dust, is the main product.
[0069] Siloxanes, silicon alkoxides, and inorganic silicon compounds are preferred starting materials for the formation of the silicon dioxide powder. Siloxanes are understood to mean linear and cyclic polyalkylsiloxanes. Polyalkylsiloxanes preferably have the general formula Si p O p R 2p , where p is an integer of at least 2, preferably from 2 to 10, particularly preferably from 3 to 5, and R is an alkyl group having 1 to 8 carbon atoms, preferably having 1 to 4 carbon atoms, particularly preferably a methyl group.
[0070] Particularly preferred siloxanes are those selected from the group consisting of hexamethyldisiloxane, hexamethylcyclotrisiloxane (D3), octamethylcyclotetrasiloxane (D4), and decamethylcyclopentasiloxane (D5), or a combination of two or more thereof. If the siloxane comprises D3, D4, and D5, D4 is preferably the main component. The main component is preferably present in a proportion of at least 70 wt. %, preferably at least 80 wt. %, for example at least 90 wt. % or at least 94 wt. %, particularly preferably at least 98 wt. %, in each case based on the total amount of silicon dioxide powder. Preferred silicon alkoxides are tetramethoxysilane and methyltrimethoxysilane. Preferred inorganic silicon compounds as starting materials for silicon dioxide powder are silicon halides, silicates, silicon carbide, and silicon nitride. Particularly preferred inorganic silicon compounds as starting materials for silicon dioxide powder are silicon tetrachloride and trichlorosilane.
[0071] The silicon dioxide powder can preferably be produced from a compound selected from the group consisting of siloxanes, silicon alkoxides and silicon halides.
[0072] Preferably, the silicon dioxide powder can be produced from a compound selected from the group consisting of hexamethyldisiloxane, hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane and decamethylcyclopentasiloxane, tetramethoxysilane and methyltrimethoxysilane, silicon tetrachloride and trichlorosilane or a combination of two or more thereof, for example from silicon tetrachloride and octamethylcyclotetrasiloxane, particularly preferably from octamethylcyclotetrasiloxane.
[0073] Various parameters are important for the formation of silicon dioxide from silicon tetrachloride by flame hydrolysis. A preferred composition of a suitable gas mixture includes an oxygen content in the flame hydrolysis in a range from 25 to 40 vol.%. The hydrogen content can be in a range from 45 to 60 vol.%. The silicon tetrachloride content is preferably 5 to 30 vol.%, all of the aforementioned vol.% based on the total volume of the gas stream. Further preferred is a combination of the aforementioned volume proportions for oxygen, hydrogen, and SiCl 4 . The flame in the flame hydrolysis preferably has a temperature in a range from 1500 to 2500 °C, for example in a range from 1600 to 2400 °C, particularly preferably in a range from 1700 to 2300 °C.Preferably, the silicon dioxide primary particles formed in flame hydrolysis are removed as silicon dioxide powder before agglomerates or aggregates form.
[0074] The silicon dioxide powder can have the following characteristics: a. a BET surface area in a range from 20 to 60 m 2 / g, for example from 25 to 55 m 2 / g, or from 30 to 50 m 2 / g, particularly preferably from 20 to 40 m 2 / g, and b. a bulk density of 0.01 to 0.3 g / cm 3 , for example in the range from 0.02 to 0.2 g / cm 3 , preferably in the range from 0.03 to 0.15 g / cm 3 , further preferably in the range from 0.1 to 0.2 g / cm 3 or in the range from 0.05 to 0.1 g / cm 3 .
[0075] The silicon dioxide powder preferably has at least one, for example at least two or at least three or at least four, particularly preferably at least five of the following features: c. a carbon content of less than 50 ppm, for example less than 40 ppm or less than 30 ppm, particularly preferably in a range from 1 ppb to 20 ppm; d. a chlorine content of less than 200 ppm, for example less than 150 ppm or less than 100 ppm, particularly preferably in a range from 1 ppb to 80 ppm; e. an aluminum content of less than 200 ppb, for example in the range from 1 to 100 ppb, particularly preferably in the range from 1 to 80 ppb; f. a total content of metals other than aluminum of less than 5 ppm, for example less than 2 ppm, particularly preferably in a range from 1 ppb to 1 ppm; g. at least 70 wt.% of the powder particles have a primary particle size in a range from 10 to less than 100 nm, for example in the range from 15 to less than 100 nm, particularly preferably in the range from 20 to less than 100 nm; h.a tamped density in a range from 0.001 to 0.3 g / cm 3 , for example in the range from 0.002 to 0.2 g / cm 3 or from 0.005 to 0.1 g / cm 3 , preferably in the range from 0.01 to 0.06 g / cm 3 , also preferably in the range from 0.1 to 0.2 g / cm 3 , or in the range from 0.15 to 0.2 g / cm 3 ; i. a residual moisture content of less than 5 wt.%, for example in the range from 0.25 to 3 wt.%, particularly preferably in the range from 0.5 to 2 wt.%; j. a particle size distribution D 10 in the range from 1 to 7 µm, for example in the range from 2 to 6 µm or in the range from 3 to 5 µm, particularly preferably in the range from 3.5 to 4.5 µm; k. a particle size distribution D 50 in the range from 6 to 15 µm, for example in the range from 7 to 13 µm or in the range from 8 to 11 µm, particularly preferably in the range from 8.5 to 10.5 µm; l. a particle size distribution D 90 in the range from 10 to 40 µm, for example in the range from 15 to 35 µm, particularly preferably in the range from 20 to 30 µm; where the wt.-%, ppm and ppb are each based on the total weight of the silicon dioxide powder.
[0076] The silicon dioxide powder contains silicon dioxide. Preferably, the silicon dioxide powder contains silicon dioxide in an amount of more than 95 wt.%, for example, in an amount of more than 98 wt.%, or more than 99 wt.%, or more than 99.9 wt.%, in each case based on the total weight of the silicon dioxide powder. Particularly preferably, the silicon dioxide powder contains silicon dioxide in an amount of more than 99.99 wt.%, based on the total weight of the silicon dioxide powder.
[0077] The silicon dioxide powder preferably has a metal content of metals other than aluminum of less than 5 ppm, for example less than 2 ppm, particularly preferably less than 1 ppm, in each case based on the total weight of the silicon dioxide powder. However, the silicon dioxide powder often has a content of metals other than aluminum in an amount of at least 1 ppb. Such metals include, for example, sodium, lithium, potassium, magnesium, calcium, strontium, germanium, copper, molybdenum, tungsten, titanium, iron, and chromium. These can be present, for example, as an element, as an ion, or as part of a molecule, an ion, or a complex.
[0078] The silicon dioxide powder preferably has a total proportion of other constituents of less than 30 ppm, for example less than 20 ppm, particularly preferably less than 15 ppm, the ppm in each case based on the total weight of the silicon dioxide powder. However, the silicon dioxide powder often contains other constituents in an amount of at least 1 ppb. Other constituents are understood to mean all constituents of the silicon dioxide powder that do not belong to the following group: silicon dioxide, chlorine, aluminum, OH groups.
[0079] In this context, the indication of a constituent, if the constituent is a chemical element, means that it can exist as an element or as an ion in a compound or salt. For example, the indication "aluminum" includes not only metallic aluminum but also aluminum salts, aluminum oxides, and aluminum metal complexes. For example, the indication "chlorine" includes not only elemental chlorine but also chlorides such as sodium chloride and hydrogen chloride. The other constituents are often in the same physical state as the substance in which they are contained.
[0080] In this context, the indication of a constituent, when the constituent is a chemical compound or a functional group, means that the constituent can exist in the stated form, as a charged chemical compound, or as a derivative of the chemical compound. For example, the indication of the chemical substance ethanol includes, in addition to ethanol, also ethanolate, for example, sodium ethanolate. The indication "OH group" also includes silanol, water, and metal hydroxides. For example, the indication "derivative" in the case of acetic acid also includes acetic acid ester and acetic anhydride.
[0081] Preferably, at least 70% of the powder particles of the silicon dioxide powder, based on the number of powder particles, have a primary particle size of less than 100 nm, for example in the range from 10 to 100 nm or from 15 to 100 nm, and particularly preferably in the range from 20 to 100 nm. The primary particle size is determined by dynamic light scattering according to ISO 13320:2009-10.
[0082] Preferably, at least 75% of the powder particles of the silicon dioxide powder, based on the number of powder particles, have a primary particle size of less than 100 nm, for example in the range from 10 to 100 nm or from 15 to 100 nm, and particularly preferably in the range from 20 to 100 nm.
[0083] Preferably, at least 80% of the powder particles of the silicon dioxide powder, based on the number of powder particles, have a primary particle size of less than 100 nm, for example in the range from 10 to 100 nm or from 15 to 100 nm, and particularly preferably in the range from 20 to 100 nm.
[0084] Preferably, at least 85% of the powder particles of the silicon dioxide powder, based on the number of powder particles, have a primary particle size of less than 100 nm, for example in the range from 10 to 100 nm or from 15 to 100 nm, and particularly preferably in the range from 20 to 100 nm.
[0085] Preferably, at least 90% of the powder particles of the silicon dioxide powder, based on the number of powder particles, have a primary particle size of less than 100 nm, for example in the range from 10 to 100 nm or from 15 to 100 nm, and particularly preferably in the range from 20 to 100 nm.
[0086] Preferably, at least 95% of the powder particles of the silicon dioxide powder, based on the number of powder particles, have a primary particle size of less than 100 nm, for example in the range from 10 to 100 nm or from 15 to 100 nm, and particularly preferably in the range from 20 to 100 nm.
[0087] The silicon dioxide powder preferably has a particle size D 10 in the range from 1 to 7 µm, for example in the range from 2 to 6 µm or in the range from 3 to 5 µm, particularly preferably in the range from 3.5 to 4.5 µm. The silicon dioxide powder preferably has a particle size D 50 in the range from 6 to 15 µm, for example in the range from 7 to 13 µm or in the range from 8 to 11 µm, particularly preferably in the range from 8.5 to 10.5 µm. The silicon dioxide powder preferably has a particle size D 90 in the range from 10 to 40 µm, for example in the range from 15 to 35 µm, particularly preferably in the range from 20 to 30 µm.
[0088] The silicon dioxide powder preferably has a specific surface area (BET surface area) in a range from 20 to 60 m² / g, for example from 25 to 55 m² / g, or from 30 to 50 m² / g, particularly preferably from 20 to 40 m² / g. The BET surface area is determined according to the Brunauer, Emmet, and Teller (BET) method based on DIN 66132 and is based on gas absorption at the surface to be measured.
[0089] Preferably, the silicon dioxide powder has a pH of less than 7, for example in the range from 3 to 6.5 or from 3.5 to 6 or from 4 to 5.5, particularly preferably in the range from 4.5 to 5. The pH can be determined by means of a single-rod measuring electrode (4% silicon dioxide powder in water).
[0090] The silicon dioxide powder preferably has the feature combination a. / b. / c. or a. / b. / f. or a. / b. / g., more preferably the feature combination a. / b. / c. / f. or a. / b. / c. / g. or a. / b. / f. / g., particularly preferably the feature combination a. / b. / c. / f. / g.
[0091] The silicon dioxide powder preferably has the feature combination a. / b. / c., wherein the BET surface area is in a range of 20 to 40 m 2 / g, the bulk density is in a range of 0.05 to 0.3 g / mL, and the carbon content is less than 40 ppm.
[0092] The silicon dioxide powder preferably has the feature combination a. / b. / f., wherein the BET surface area is in a range of 20 to 40 m 2 / g, the bulk density is in a range of 0.05 to 0.3 g / mL and the total content of metals other than aluminum is in a range of 1 ppb to 1 ppm.
[0093] The silicon dioxide powder preferably has the feature combination a. / b. / g., wherein the BET surface area is in a range of 20 to 40 m 2 / g, the bulk density is in a range of 0.05 to 0.3 g / mL and at least 70 wt.% of the powder particles have a primary particle size in a range of 20 to less than 100 nm.
[0094] The silicon dioxide powder further preferably has the feature combination a. / b. / c. / f., wherein the BET surface area is in a range of 20 to 40 m 2 / g, the bulk density is in a range of 0.05 to 0.3 g / mL, the carbon content is less than 40 ppm, and the total content of metals other than aluminum is in a range of 1 ppb to 1 ppm.
[0095] The silicon dioxide powder further preferably has the feature combination a. / b. / c. / g., wherein the BET surface area is in a range of 20 to 40 m 2 / g, the bulk density is in a range of 0.05 to 0.3 g / mL, the carbon content is less than 40 ppm and at least 70 wt.% of the powder particles have a primary particle size in a range of 20 to less than 100 nm.
[0096] The silicon dioxide powder further preferably has the feature combination a. / b. / f. / g., wherein the BET surface area is in a range of 20 to 40 m 2 / g, the bulk density is in a range of 0.05 to 0.3 g / mL, the total content of metals other than aluminum is in a range of 1 ppb to 1 ppm, and at least 70 wt.% of the powder particles have a primary particle size in a range of 20 to less than 100 nm.
[0097] The silicon dioxide powder particularly preferably has the feature combination a. / b. / c. / f. / g., wherein the BET surface area is in a range from 20 to 40 m 2 / g, the bulk density is in a range from 0.05 to 0.3 g / mL, the carbon content is less than 40 ppm, the total content of metals other than aluminum is in a range from 1 ppb to 1 ppm and at least 70 wt.% of the powder particles have a primary particle size in a range from 20 to less than 100 nm. Step II.
[0098] In step II, the silicon dioxide powder can be processed into silicon dioxide granules, with the silicon dioxide granules having a larger particle diameter than the silicon dioxide powder. In principle, any process known to the person skilled in the art that leads to an increase in particle diameter is suitable for this purpose.
[0099] The silicon dioxide granules have a particle diameter that is larger than the particle diameter of the silicon dioxide powder. The particle diameter of the silicon dioxide granules is preferably in a range of 500 to 50,000 times larger than the particle diameter of the silicon dioxide powder, for example, 1,000 to 10,000 times larger, particularly preferably 2,000 to 8,000 times larger.
[0100] Preferably, at least 90% of the silicon dioxide granules provided in step i.) are formed from pyrogenically produced silicon dioxide powder, for example at least 95% by weight or at least 98% by weight, particularly preferably at least 99% by weight or more, in each case based on the total weight of the silicon dioxide granules.
[0101] According to the invention, the silicon dioxide granulate used has the following features: A) a BET surface area in the range of 20 m 2 / g to 50 m 2 / g; B) a bulk density in the range of 0.5 to 1.2 g / cm 3 < ; C) an average particle size in the range of 50 to 500 µm D) a carbon content of less than 50 ppm; E) an aluminum content of less than 200 ppb; F) a tapped density in the range of 0.7 to 1.2 g / cm 3 < ; G) a pore volume in the range of 0.1 to 2.5 mL / g; H) a particle size distribution D 10 in the range of 50 to 150 µm; J) a particle size distribution D 50 in the range of 150 to 300 µm; K) a particle size distribution D 90 in the range of 250 to 620 µm, where ppm and ppb are each based on the total weight of the silicon dioxide granules.
[0102] The granules of the silicon dioxide granulate preferably have a spherical morphology. Spherical morphology refers to a round to oval shape of the particles. The granules of the silicon dioxide granulate preferably have an average sphericity in a range from 0.7 to 1.3 SPHT3, for example, an average sphericity in a range from 0.8 to 1.2 SPHT3, particularly preferably an average sphericity in a range from 0.85 to 1.1 SPHT3. The SPHT3 characteristic is described in the test methods.
[0103] Furthermore, the granules of the silicon dioxide granulate preferably have an average symmetry in a range of 0.7 to 1.3 Symm3, for example an average symmetry in a range of 0.8 to 1.2 Symm3, particularly preferably an average symmetry in a range of 0.85 to 1.1 Symm3. The characteristic of average symmetry Symm3 is described in the test methods.
[0104] The silicon dioxide granules preferably have a metal content of metals other than aluminum of less than 1000 ppb, for example less than 500 ppb, particularly preferably less than 100 ppb, in each case based on the total weight of the silicon dioxide granules. However, the silicon dioxide granules often have a content of metals other than aluminum in an amount of at least 1 ppb. The silicon dioxide granules often have a metal content of metals other than aluminum of less than 1 ppm, preferably in a range from 40 to 900 ppb, for example in a range from 50 to 700 ppb, particularly preferably in a range from 60 to 500 ppb, in each case based on the total weight of the silicon dioxide granules. Such metals include, for example, sodium, lithium, potassium, magnesium, calcium, strontium, germanium, copper, molybdenum, titanium, iron, and chromium.These can exist, for example, as an element, as an ion, or as part of a molecule or an ion or a complex.
[0105] The silicon dioxide granules may contain additional components, for example in the form of molecules, ions, or elements. The silicon dioxide granules preferably contain less than 500 ppm, for example less than 300 ppm, particularly preferably less than 100 ppm, of additional components, based in each case on the total weight of the silicon dioxide granules. Additional components are often present in an amount of at least 1 ppb. The additional components can, in particular, be selected from the group consisting of carbon, fluoride, iodide, bromide, phosphorus, or a mixture of at least two thereof.
[0106] The silicon dioxide granules preferably contain less than 10 ppm of carbon, for example less than 8 ppm or less than 5 ppm, particularly preferably less than 4 ppm, each based on the total weight of the silicon dioxide granules. Carbon is often present in the silicon dioxide granules in an amount of at least 1 ppb.
[0107] The silicon dioxide granules preferably contain less than 100 ppm, for example less than 80 ppm, particularly preferably less than 70 ppm, of other components, based in each case on the total weight of the silicon dioxide granules. However, the other components are often present in an amount of at least 1 ppb.
[0108] Preferably, step II includes the following steps: II-1. Providing a liquid; II-2. Mixing the silicon dioxide powder with the liquid to obtain a slurry; II-3. Granulating, preferably spray-drying, the slurry.
[0109] For the purposes of the present invention, a liquid is understood as a substance or a mixture of substances that is liquid at a pressure of 1013 hPa and a temperature of 20 °C.
[0110] A "slurry" in the sense of the present invention means a mixture of at least two substances, wherein the mixture comprises at least one liquid and at least one solid under the conditions under consideration.
[0111] In principle, all substances and mixtures of substances known to the person skilled in the art and deemed suitable for the intended use are suitable as the liquid. The liquid is preferably selected from the group consisting of organic liquids and water. The silicon dioxide powder is preferably soluble in the liquid in an amount of less than 0.5 g / L, preferably in an amount of less than 0.25 g / L, and particularly preferably in an amount of less than 0.1 g / L. The g / L is expressed as g of silicon dioxide powder per liter of liquid.
[0112] Polar solvents are preferably suitable as the liquid. These can be organic liquids or water. The liquid is preferably selected from the group consisting of water, methanol, ethanol, n-propanol, isopropanol, n-butanol, tert-butanol, and mixtures of more than one thereof. The liquid is particularly preferably water. The liquid particularly preferably comprises distilled or deionized water.
[0113] Preferably, the silicon dioxide powder is processed into a slurry. The silicon dioxide powder is virtually insoluble in the liquid at room temperature, but can be incorporated into the liquid in high weight proportions to obtain a slurry.
[0114] The silicon dioxide powder and the liquid can be mixed in any manner. For example, the silicon dioxide powder can be added to the liquid, or the liquid can be added to the silicon dioxide powder. The mixture can be agitated during or after addition. More preferably, the mixture is agitated during and after addition. Examples of agitation include shaking and stirring, or a combination of both. Preferably, the silicon dioxide powder can be added to the liquid while stirring. More preferably, a portion of the silicon dioxide powder can be added to the liquid, the resulting mixture being agitated, and the mixture can then be mixed with the remaining portion of the silicon dioxide powder. Likewise, a portion of the liquid can be added to the silicon dioxide powder, the resulting mixture being agitated, and the mixture can then be mixed with the remaining portion of the liquid.
[0115] By mixing the silicon dioxide powder and the liquid, a slurry is obtained. The slurry is preferably a suspension in which the silicon dioxide powder is evenly distributed throughout the liquid. "Uniform" means that the density and composition of the slurry at any point deviate by no more than 10% from the average density and composition, each based on the total amount of slurry. A uniform distribution of the silicon dioxide powder in the liquid can be produced or maintained by agitation as previously described, or both.
[0116] The slurry preferably has a liter weight in the range of 1000 to 2000 g / L, for example in the range of 1200 to 1900 g / L or 1300 to 1800 g / L, particularly preferably in the range of 1400 to 1700 g / L. The liter weight is determined by weighing a volume-calibrated container.
[0117] More preferably, the slurry has at least one, for example at least two or at least three or at least four, particularly preferably at least five of the following features: a.) the slurry is transported in contact with a plastic surface; b.) the slurry is sheared; c.) the slurry has a temperature of more than 0°C, preferably in a range of 5 to 35°C; d.) the slurry has a zeta potential at a pH of 7 in a range of 0 to -100 mA, for example from -20 to -60 mA, more preferably from -30 to -45 mA; e.) the slurry has a pH in a range of 7 or more, for example more than 7 or a pH in the range of 7.5 to 13 or from 8 to 11, more preferably from 8.5 to 10; f.) the slurry has an isoelectric point of less than 7, for example in a range of 1 to 5 or in a range of 2 to 4, more preferably in a range of 3 to 3.5; g.) the slurry has a solids content of at least 40 wt.%, for example in a range of 50 to 80 wt.%, or in a range of 55 to 75 wt.-%, particularly preferably in a range of 60 to 70 wt.%, in each case based on the total weight of the slurry; h.) the slurry has a viscosity according to DIN 53019-1 (5 rpm, 30 wt.%) in a range of 500 to 2000 mPas, for example in the range of 600 to 1700 mPas, particularly preferably in the range of 1000 to 1600 mPas; i.) the slurry has a thixotropy according to DIN SPEC 91143-2 (30 wt.% in water, 23 °C, 5 rpm / 50 rpm) in the range of 3 to 6, for example in the range of 3.5 to 5, particularly preferably in the range of 4.0 to 4.5; j.) the silicon dioxide particles in the slurry have, in a 4 wt.% slurry, a mean particle size in suspension according to DIN ISO 13320-1 in the range of 100 to 500 nm, for example in a range of 200 to 300 nm.
[0118] Preferably, the silicon dioxide particles in a 4 wt.% aqueous slurry have a particle size D 10 in a range from 50 to 250 nm, particularly preferably in the range from 100 to 150 nm. Preferably, the silicon dioxide particles in a 4 wt.% aqueous slurry have a particle size D 50 in a range from 100 to 400 nm, particularly preferably in the range from 200 to 250 nm. Preferably, the silicon dioxide particles in a 4 wt.% aqueous slurry have a particle size D 90 in a range from 200 to 600 nm, particularly preferably in a range from 350 to 400 nm. The particle size is determined using DIN ISO 13320-1.
[0119] The "isoelectric point" is the pH value at which the zeta potential assumes the value 0. The zeta potential is determined according to ISO 13099-2:2012.
[0120] Preferably, the pH of the slurry is adjusted to a value within the above-mentioned range. To adjust the pH, substances such as NaOH or NH3 can be added to the slurry, for example as an aqueous solution. The slurry is often agitated. granulation
[0121] Silicon dioxide granules can be obtained by granulating silicon dioxide powder. Granulation is the conversion of powder particles into granules. During granulation, larger agglomerates called "silicon dioxide granules" form due to the agglomeration of several silicon dioxide powder particles. These are often also referred to as "silicon dioxide particles," "silicon dioxide granulate particles," or "granulate particles." Together, the granules form a granulate, for example, silicon dioxide granules form "silicon dioxide granules."
[0122] In this case, in principle, any granulation process known to the person skilled in the art and suitable for granulating silicon dioxide powder can be selected. Granulation processes can be divided into built-up granulation and press granulation, and further into wet and dry granulation processes. Known methods include roller granulation in a granulating disc, spray granulation, centrifugal atomization, fluidized bed granulation, granulation using a granulating mill, compaction, roller pressing, briquetting, slurry production, or extrusion.
[0123] During processing, silicon dioxide granules are preferably formed with granules having a spherical morphology; further preferably, the processing is carried out by spray granulation or roller granulation. Further preferably, silicon dioxide granules with granules having a spherical morphology contain at most 50% granules, preferably at most 40% granules, further preferably at most 20% granules, more preferably between 0 and 50%, between 0 and 40%, or between 0 and 20%, or between 10 and 50%, between 10 and 40%, or between 10 and 20% granules that do not have a spherical morphology, the percentage being based in each case on the total number of granules in the granule. The granules with a spherical morphology have the SPHT3 values already mentioned in this description. Spray drying
[0124] Silica granules can be obtained by spray granulating the slurry. Spray granulation is also known as spray drying.
[0125] Spray drying is preferably carried out in a spray tower. For spray drying, the slurry is pressurized at elevated temperature. The pressurized slurry is then released through a nozzle and sprayed into the spray tower. This results in droplets forming, which dry instantly and initially form dry microparticles ("nuclei"). These microparticles, together with a gas stream acting on them, form a fluidized bed. They are thus kept suspended, providing a surface for drying additional droplets.
[0126] The nozzle through which the slurry is sprayed into the spray tower preferably forms an inlet into the interior of the spray tower.
[0127] The nozzle preferably has a contact surface with the slurry during spraying. The "contact surface" refers to the area of the nozzle that comes into contact with the slurry during spraying. Often, at least part of the nozzle is shaped like a tube through which the slurry is passed during spraying, so that the inside of the hollow tube comes into contact with the slurry.
[0128] The contact surface preferably comprises a glass, a plastic, or a combination thereof. The contact surface preferably comprises a glass, particularly preferably quartz glass. The contact surface preferably comprises a plastic. In principle, all plastics known to those skilled in the art that are stable at the process temperatures and do not release foreign atoms into the slurry are suitable. Preferred plastics are polyolefins, for example homo- or copolymers containing at least one olefin, particularly preferably homo- or copolymers containing polypropylene, polyethylene, polybutadiene, or combinations of two or more thereof.The contact surface preferably consists of a glass, a plastic, or a combination thereof, for example, selected from the group consisting of quartz glass and polyolefins, particularly preferably selected from the group consisting of quartz glass and homopolymers or copolymers including polypropylene, polyethylene, polybutadiene, or combinations of two or more thereof. The contact surface preferably contains no metals, in particular no tungsten, titanium, tantalum, chromium, cobalt, nickel, iron, vanadium, zirconium, and manganese.
[0129] In principle, it is possible for the contact surface and the other parts of the nozzle to be made of the same or different materials. Preferably, the other parts of the nozzle contain the same material as the contact surface. It is also possible for the other parts of the nozzle to contain a different material than the contact surface. For example, the contact surface can be coated with a suitable material, such as glass or plastic.
[0130] Preferably, the nozzle is formed to more than 70 wt.%, based on the total weight of the nozzle, from an element selected from the group consisting of glass, plastic or a combination of glass and plastic, for example to more than 75 wt.% or to more than 80 wt.% or to more than 85 wt.% or to more than 90 wt.% or to more than 95 wt.%, particularly preferably to more than 99 wt.%.
[0131] The nozzle preferably comprises a nozzle plate. The nozzle plate is preferably made of glass, plastic, or a combination of glass and plastic. The nozzle plate is preferably made of glass, particularly preferably quartz glass. The nozzle plate is preferably made of plastic. Preferred plastics are polyolefins, for example homo- or copolymers containing at least one olefin, particularly preferably homo- or copolymers containing polypropylene, polyethylene, polybutadiene, or combinations of two or more thereof. The nozzle plate preferably contains no metals, in particular no tungsten, titanium, tantalum, chromium, cobalt, nickel, iron, vanadium, zirconium, and manganese.
[0132] The nozzle preferably comprises a swirl screw. The swirl screw is preferably made of glass, plastic, or a combination of glass and plastic. The swirl screw is preferably made of glass, particularly preferably quartz glass. The swirl screw is preferably made of plastic. Preferred plastics are polyolefins, for example homo- or copolymers containing at least one olefin, particularly preferably homo- or copolymers containing polypropylene, polyethylene, polybutadiene, or combinations of two or more thereof. The swirl screw preferably contains no metals, in particular no tungsten, titanium, tantalum, chromium, cobalt, nickel, iron, vanadium, zirconium, and manganese.
[0133] The nozzle can also comprise further components. Preferred further components are a nozzle body, particularly preferred is a nozzle body surrounding the swirl screw and the nozzle plate, a crosspiece, and an impact plate. A nozzle preferably comprises one or more, particularly preferably all, of the further components. The further components can, independently of one another, in principle consist of any material known to the person skilled in the art and suitable for this purpose, for example a metal-containing material, glass, or a plastic. The nozzle body is preferably made of glass, particularly preferably quartz glass. The further components are preferably made of plastic. Preferred plastics are polyolefins, for example homo- or copolymers containing at least one olefin, particularly preferably homo- or copolymers containing polypropylene, polyethylene, polybutadiene, or combinations of two or more thereof.Preferably, the other components do not contain any metals, in particular no tungsten, titanium, tantalum, chromium, cobalt, nickel, iron, vanadium, zirconium and manganese.
[0134] The spray tower preferably has a gas inlet and a gas outlet. Gas can be introduced into the interior of the spray tower through the gas inlet, and discharged through the gas outlet. It is also possible to introduce gas into the spray tower via the nozzle. Gas can also be discharged via the spray tower outlet. Furthermore, gas can preferably be supplied via the nozzle and a gas inlet of the spray tower, and discharged via the spray tower outlet and a gas outlet of the spray tower.
[0135] Preferably, the interior of the spray tower contains an atmosphere selected from air, an inert gas, at least two inert gases, or a combination of air with at least one inert gas, preferably at least two inert gases. Inert gases are preferably selected from the list consisting of nitrogen, helium, neon, argon, krypton, and xenon. For example, air, nitrogen, or argon is present in the interior of the spray tower, particularly preferably air.
[0136] More preferably, the atmosphere present in the spray tower is part of a gas stream. The gas stream is preferably introduced into the spray tower via a gas inlet and discharged via a gas outlet. It is also possible to introduce portions of the gas stream via the nozzle and discharge portions of the gas stream via a solids outlet. The gas stream can absorb additional components in the spray tower. These can originate from the slurry during spray drying and pass into the gas stream.
[0137] Preferably, a dry gas stream is fed to the spray tower. A dry gas stream is understood to be a gas or gas mixture whose relative humidity is below the condensation point at the temperature set in the spray tower. A relative humidity of 100% corresponds to a water content of 17.5 g / m³ at 20°C. The gas is preferably preheated to a temperature in the range from 150 to 450°C, for example from 200 to 420°C or from 300 to 400°C, particularly preferably from 350 to 400°C.
[0138] The interior of the spray tower is preferably temperature-controlled. The temperature in the interior of the spray tower is preferably up to 550°C, for example 300 to 500°C, particularly preferably 350 to 450°C.
[0139] The gas stream at the gas inlet preferably has a temperature in a range from 150 to 450°C, for example from 200 to 420°C or from 300 to 400°C, particularly preferably from 350 to 400°C.
[0140] At the solids outlet, the gas outlet or at both locations, the discharged gas stream preferably has a temperature of less than 170°C, for example from 50 to 150°C, particularly preferably from 100 to 130°C.
[0141] More preferably, the difference between the temperature of the gas stream upon introduction and the gas stream upon discharge is in a range from 100 to 330°C, for example from 150 to 300°C.
[0142] The resulting silicon dioxide granules are present as an agglomerate of individual silicon dioxide powder particles. The individual silicon dioxide powder particles are still recognizable in the agglomerate. The average particle size of the silicon dioxide powder particles is preferably in the range of 10 to 1000 nm, for example in the range of 20 to 500 nm, or 30 to 250 nm, or 35 to 200 nm, or 40 to 150 nm, or particularly preferably in the range of 50 to 100 nm. The average particle size of these particles is determined according to DIN ISO 13320-1.
[0143] Spray drying can be carried out in the presence of excipients. In principle, any substances known to the person skilled in the art and deemed suitable for the intended purpose can be used as excipients. Examples of excipients include so-called binders. Examples of suitable binders include metal oxides such as calcium oxide, metal carbonates such as calcium carbonate, and polysaccharides such as cellulose, cellulose ethers, starch, and starch derivatives.
[0144] Particularly preferably, spray drying in the context of the present invention is carried out without auxiliaries.
[0145] Preferably, a portion of the silicon dioxide granules is separated before, after, or before and after removal from the spray tower. Any method known to the person skilled in the art and deemed suitable may be used for the separation. Separation is preferably carried out by sifting or sieving.
[0146] Preferably, before removing the silicon dioxide granules formed by spray drying from the spray tower, particles with a particle size of less than 50 µm, for example with a particle size of less than 70 µm, particularly preferably with a particle size of less than 90 µm, are separated by screening. The screening is preferably carried out by a cyclone, which is preferably arranged in the lower region of the spray tower, particularly preferably above the spray tower outlet.
[0147] After removing the silicon dioxide granules from the spray tower, particles with a particle size of more than 1000 µm, for example, with a particle size of more than 700 µm, particularly preferably with a particle size of more than 500 µm, are preferably separated by sieving. Sieving the particles can, in principle, be carried out using any method known to the person skilled in the art and suitable for this purpose. Sieving is preferably carried out using a vibrating chute.
[0148] According to a preferred embodiment, the spray drying of the slurry through a nozzle into a spray tower is characterized by at least one, for example two or three, particularly preferably all of the following features: a] spray granulation in a spray tower; b] presence of a pressure of the slurry at the nozzle of not more than 40 bar, for example in a range from 1.3 to 20 bar, from 1.5 to 18 bar or from 2 to 15 bar or from 4 to 13 bar, or particularly preferably in the range from 5 to 12 bar, the pressure being given in absolute terms (relative to p = 0 hPa); c] a temperature of the droplets on entry into the spray tower in a range from 10 to 50°C, preferably in a range from 15 to 30°C, particularly preferably in a range from 18 to 25°C.d] a temperature on the side of the nozzle facing the spray tower in a range from 100 to 450°C, for example in a range from 250 to 440°C, particularly preferably from 350 to 430°C; e] a throughput of slurry through the nozzle in a range from 0.05 to 1 m 3 / h, for example in a range from 0.1 to 0.7 m 3 / h or from 0.2 to 0.5 m 3 / h, particularly preferably in a range from 0.25 to 0.4 m 3 / h; f] a solids content of the slurry of at least 40 wt.%, for example in a range from 50 to 80 wt.%, or in a range from 55 to 75 wt.%, particularly preferably in a range from 60 to 70 wt.-%, in each case based on the total weight of the slurry; g] a gas inflow into the spray tower in a range from 10 to 100 kg / min, for example in a range from 20 to 80 kg / min or from 30 to 70 kg / min, particularly preferably in a range from 40 to 60 kg / min; h] a temperature of the gas stream on entry into the spray tower in a range from 100 to 450°C, for example in a range from 250 to 440°C, particularly preferably from 350 to 430°C; i] a temperature of the gas stream on exit from the spray tower of less than 170°C; j] the gas is selected from the group consisting of air, nitrogen and helium, or a combination of two or more thereof; preferably air; k] a residual moisture content of the granules upon removal from the spray tower of less than 5 wt.%, for example less than 3 wt.% or less than 1 wt.% or in a range from 0.01 to 0.5 wt.%, particularly preferably in a range from 0.1 to 0.3 wt.-%, in each case based on the total weight of the silicon dioxide granules produced during spray drying; l] at least 50 wt.% of the spray granules, based on the total weight of the silicon dioxide granules produced during spray drying, have a flight time in a range from 1 to 100 s, for example over a period of 10 to 80 s, particularly preferably over a period of 25 to 70 s; m] at least 50% by weight of the spray granules, based on the total weight of the silicon dioxide granules produced during spray drying, travel a distance of more than 20 m, for example more than 30 or more than 50 or more than 70 or more than 100 or more than 150 or more than 200 or in a range from 20 to 200 m or from 10 to 150 or from 20 to 100, particularly preferably a range from 30 to 80 m.n] the spray tower has a cylindrical geometry, o] a height of the spray tower of more than 10 m, for example of more than 15 m or of more than 20 m or of more than 25 m or of more than 30 m or in a range from 10 to 25 m, particularly preferably in a range from 15 to 20 m; p] screening out particles with a size of less than 90 µm before removing the granules from the spray tower; q] sieving out particles with a size of more than 500 µm after removing the granules from the spray tower, preferably on a vibrating chute; r] the droplets of the slurry emerge from the nozzle at an angle of 30 to 60 degrees counter to the vertical direction, particularly preferably at an angle of 45 degrees counter to the vertical direction.
[0149] The plumb line is the direction of the gravity vector.
[0150] The flight path refers to the distance traveled by a droplet of slurry from exiting the nozzle in the gas space of the spray tower, forming a granule, until the completion of the flight and fall process. The flight and fall process usually ends with the granule hitting the bottom of the spray tower or with the granule hitting other granules already on the bottom of the spray tower, whichever occurs first.
[0151] The flight time is the time it takes a granule to travel the distance in the spray tower. Granules in the spray tower preferably follow a helical trajectory.
[0152] Preferably, at least 60% by weight of the spray granules, based on the total weight of the silicon dioxide granules produced during spray drying, cover an average flight distance of more than 20 m, for example of more than 30 or of more than 50 or of more than 70 or of more than 100 or of more than 150 or of more than 200 or in a range from 20 to 200 m or from 10 to 150 or from 20 to 100, particularly preferably a range from 30 to 80 m.
[0153] Preferably, at least 70% by weight of the spray granules, based on the total weight of the silicon dioxide granules produced during spray drying, cover an average flight distance of more than 20 m, for example of more than 30 or of more than 50 or of more than 70 or of more than 100 or of more than 150 or of more than 200 or in a range from 20 to 200 m or from 10 to 150 or from 20 to 100, particularly preferably a range from 30 to 80 m.
[0154] Preferably, at least 80% by weight of the spray granules, based on the total weight of the silicon dioxide granules produced during spray drying, cover an average flight distance of more than 20 m, for example of more than 30 or of more than 50 or of more than 70 or of more than 100 or of more than 150 or of more than 200 or in a range from 20 to 200 m or from 10 to 150 or from 20 to 100, particularly preferably a range from 30 to 80 m.
[0155] Preferably, at least 90% by weight of the spray granules, based on the total weight of the silicon dioxide granules produced during spray drying, cover an average flight distance of more than 20 m, for example of more than 30 or of more than 50 or of more than 70 or of more than 100 or of more than 150 or of more than 200 or in a range from 20 to 200 m or from 10 to 150 or from 20 to 100, particularly preferably a range from 30 to 80 m. Roll granulation
[0156] Silica granules can also be obtained by roll granulating the slurry.
[0157] Roll granulation is carried out by stirring the slurry in the presence of a gas at elevated temperature. Roll granulation is preferably carried out in a stirred vessel equipped with a stirring tool. The stirred vessel preferably rotates counterclockwise to the stirring tool. The stirred vessel preferably also has an inlet through which silicon dioxide powder can be introduced into the stirred vessel, an outlet through which silicon dioxide granules can be removed, a gas inlet, and a gas outlet.
[0158] A pin agitator is preferably used to stir the slurry. A pin agitator is a stirring tool equipped with several elongated pins, each of whose longitudinal axes runs coaxially with the rotational axis of the stirring tool. The movement of the pins preferably describes coaxial circles around the rotational axis.
[0159] Preferably, the slurry is adjusted to a pH of less than 7, for example to a pH in the range from 2 to 6.5, more preferably to a pH in a range from 4 to 6. To adjust the pH, an inorganic acid is preferably used, for example an acid selected from the group consisting of hydrochloric acid, sulfuric acid, nitric acid and phosphoric acid, more preferably hydrochloric acid.
[0160] Preferably, the atmosphere present in the stirred tank is selected from air, an inert gas, at least two inert gases, or a combination of air with at least one inert gas, preferably at least two inert gases. Inert gases are preferably selected from the list consisting of nitrogen, helium, neon, argon, krypton, and xenon. For example, the atmosphere present in the stirred tank is air, nitrogen, or argon, particularly preferably air.
[0161] More preferably, the atmosphere present in the stirred tank is part of a gas stream. The gas stream is preferably introduced into the stirred tank via the gas inlet and discharged via the gas outlet. The gas stream can absorb additional components in the stirred tank. These can originate from the slurry during roller granulation and pass into the gas stream.
[0162] Preferably, a dry gas stream is fed to the stirred vessel. A "dry gas stream" is understood to mean a gas or gas mixture whose relative humidity is below the condensation point at the temperature set in the stirred vessel. The gas is preferably preheated to a temperature in the range from 50 to 300°C, for example from 80 to 250°C, particularly preferably from 100 to 200°C.
[0163] Preferably, per 1 kg of the slurry used, 10 to 150 m 3< gas per hour are introduced into the stirred vessel, for example 20 to 100 m 3< gas per hour, particularly preferably 30 to 70 m 3< gas per hour.
[0164] The gas stream dries the slurry during stirring, forming silicon dioxide granules. The resulting granules are removed from the stirring chamber.
[0165] Preferably, the removed granules are further dried. Drying is preferably carried out continuously, for example, in a rotary kiln. Preferred drying temperatures are in the range of 80 to 250°C, for example, in the range of 100 to 200°C, particularly preferably in the range of 120 to 180°C.
[0166] In the context of the present invention, "continuous" means that a process can be operated continuously. This means that the addition and removal of substances and materials involved in the process can occur continuously while the process is being carried out. It is not necessary to interrupt the process for this purpose.
[0167] Continuous as an attribute of an object, e.g. in relation to a "continuous furnace", means that this object is designed in such a way that a process or process step taking place in it can be carried out continuously.
[0168] The granules obtained by roller granulation can be sieved. Sieving can take place before or after drying. Sieving is preferably carried out before drying. Granules with a particle size of less than 50 µm, for example with a particle size of less than 80 µm, particularly preferably with a particle size of less than 100 µm, are preferably sieved out. Granules with a particle size of more than 900 µm, for example with a particle size of more than 700 µm, particularly preferably with a particle size of more than 500 µm, are further preferably sieved out. Larger particles can in principle be sieved out using any method known to the person skilled in the art and suitable for this purpose. Larger particles are preferably sieved out using a vibrating trough.
[0169] Roll granulation can be characterized by at least one, for example two or three, particularly preferably all of the following features: [a] granulation is carried out in a rotating stirred vessel; [b] granulation is carried out under a gas stream of 10 to 150 kg of gas per hour and per 1 kg of slurry; [c] the gas temperature on introduction is 40 to 200°C; [d] granules with a particle size of less than 100 µm and more than 500 µm are sieved off; [e] the granules formed have a residual moisture content of 15 to 30% by weight; [f] the granules formed are dried at 80 to 250°C, preferably in a continuous drying tube, particularly preferably to a residual moisture content of less than 1% by weight.
[0170] Preferably, the silicon dioxide granules obtained by granulation, preferably by spray or roller granulation, also referred to as silicon dioxide granules I, are treated before being processed into quartz glass bodies. This pretreatment can serve various purposes, either facilitating processing into quartz glass bodies or influencing the properties of the resulting quartz glass bodies. For example, the silicon dioxide granules I can be compacted, cleaned, surface modified, or dried.
[0171] Preferably, the silicon dioxide granulate I can be subjected to a thermal, mechanical or chemical treatment or a combination of two or more treatments to obtain a silicon dioxide granulate II. chemical
[0172] The silicon dioxide granules I may have a carbon content w C(1). The carbon content w C(1) is preferably less than 50 ppm, for example in the range from 5 to 45 ppm or from 15 to 40 ppm, particularly preferably in the range from 25 to 35 ppm, in each case based on the total weight of the silicon dioxide granules I.
[0173] The silicon dioxide granulate I preferably contains at least two particles. The at least two particles can preferably move relative to one another. Measures for generating the relative movement can, in principle, be any measures known to the person skilled in the art and deemed suitable. Mixing is particularly preferred. Mixing can, in principle, be carried out in any desired manner. A continuous furnace is preferably selected for this purpose. Accordingly, the at least two particles can preferably move relative to one another by being moved in a continuous furnace, for example, a rotary kiln.
[0174] Continuous furnaces are furnaces in which loading and unloading, known as charging, takes place continuously. Examples of continuous furnaces include rotary kilns, roller kilns, conveyor belt kilns, continuous kilns, and pusher kilns. Rotary kilns are preferred for the treatment of silicon dioxide granulate I.
[0175] Preferably, the silicon dioxide granulate I is treated with a reactant to obtain a silicon dioxide granulate II. The treatment is carried out to change the concentration of certain substances in the silicon dioxide granulate. The silicon dioxide granulate I may contain impurities or certain functionalities whose content is to be reduced, such as: OH groups, carbon-containing compounds, transition metals, alkali metals, and alkaline earth metals. The impurities and functionalities can be
[0176] They can originate from the starting material or be introduced during the process. The treatment of silicon dioxide granules I can serve various purposes. For example, the use of treated silicon dioxide granules I, i.e., silicon dioxide granules II, can simplify the processing of the silicon dioxide granules into quartz glass bodies. Furthermore, this selection can adjust the properties of the resulting quartz glass bodies. For example, the silicon dioxide granules I can be purified or surface-modified. The treatment of silicon dioxide granules I can therefore be used to improve the properties of the resulting quartz glass bodies.
[0177] A gas or a combination of several gases is preferably suitable as reactant. This is also referred to as a gas mixture. In principle, all gases known to the person skilled in the art which are known and appear suitable for the treatment mentioned can be used. Preference is given to using a gas selected from the group consisting of HCl, Cl 2 , F 2 , O 2 , O 3 , H 2 , C 2 F 4 , C 2 F 6 , HClO 4 , air, inert gas, e.g. N 2 , He, Ne, Ar, Kr, or combinations of two or more thereof. The treatment is preferably carried out in the presence of a gas or a combination of two or more gases. The treatment is preferably carried out in a countercurrent gas flow or in a cocurrent gas flow.
[0178] The reactant is preferably selected from the group consisting of HCl, Cl 2 , F 2 , O 2 , O 3 or combinations of two or more thereof. Mixtures of two or more of the aforementioned gases are preferably used to treat silicon dioxide granules I. The presence of F, Cl or both makes it possible to remove metals present as impurities in the silicon dioxide granules I, such as, for example, transition metals, alkali metals and alkaline earth metals. The aforementioned metals can form gaseous compounds with constituents of the gas mixture under the process conditions, which compounds are subsequently discharged and are thus no longer present in the granules. More preferably, the OH content in the silicon dioxide granules I can be reduced by treating the silicon dioxide granules I with these gases.
[0179] A gas mixture of HCl and Cl 2 is preferably used as the reactant. The gas mixture preferably has an HCl content in a range from 1 to 30 vol.%, for example in a range from 2 to 15 vol.%, particularly preferably in a range from 3 to 10 vol.%. The gas mixture also preferably has a Cl 2 content in a range from 20 to 70 vol.%, for example in a range from 25 to 65 vol.%, particularly preferably in a range from 30 to 60 vol.% The remainder to 100 vol.% can be supplemented by one or more inert gases, e.g. N 2 , He, Ne, Ar, Kr, or by air. Preferably, the proportion of inert gas in reactants is in a range from 0 to less than 50 vol.%, for example in a range from 1 to 40 vol.% or from 5 to 30 vol.%, particularly preferably in a range from 10 to 20 vol.%, in each case based on the total volume of the reactant.
[0180] O 2 , C 2 F 2 , or mixtures thereof with Cl 2 are preferably used for the purification of silicon dioxide granules I which were prepared from a siloxane or a mixture of several siloxanes.
[0181] The reactant in the form of a gas or gas mixture is preferably contacted with the silicon dioxide granules as a gas stream or as part of a gas stream with a throughput in a range of 50 to 2000 L / h, for example in a range of 100 to 1000 L / h, particularly preferably in a range of 200 to 500 L / h. A preferred embodiment of the contacting is contact of the gas stream and the silicon dioxide granules in a continuous furnace, for example, a rotary kiln. Another preferred embodiment of the contacting is a fluidized bed process.
[0182] Treating the silicon dioxide granules I with the reactant produces silicon dioxide granules II having a carbon content w C(2). The carbon content w C(2) of the silicon dioxide granules II is less than the carbon content w C(1) of the silicon dioxide granules I, based on the total weight of the respective silicon dioxide granules. Preferably, w C(2) is 0.5 to 99%, for example, 0.5 to 50% or 1 to 45%, particularly preferably 1.5 to 40% less than w C(1). thermal
[0183] Preferably, the silicon dioxide granulate I is additionally subjected to a thermal or mechanical treatment or a combination of these treatments. One or more of these additional treatments can be carried out before or during the treatment with the reactant. Alternatively or additionally, the additional treatment can also be carried out on the silicon dioxide granulate II. The general term "silicon dioxide granulate" used below includes the alternatives "silicon dioxide granulate I" and "silicon dioxide granulate II." It is also possible to carry out the treatments described below on both the "silicon dioxide granulate I" and the treated silicon dioxide granulate I, the "silicon dioxide granulate II."
[0184] The treatment of silica granules can serve various purposes. For example, this treatment facilitates the processing of the silica granules into quartz glass bodies. The treatment can also influence the properties of the resulting quartz glass bodies. For example, the silica granules can be compacted, cleaned, surface modified, or dried. This can reduce the specific surface area (BET). Likewise, the bulk density and average particle size can increase due to agglomeration of silica particles. The thermal treatment can be carried out dynamically or statically.
[0185] In principle, any furnace in which the silicon dioxide granules can be thermally treated and agitated is suitable for dynamic thermal treatment. Continuous furnaces are preferred for dynamic thermal treatment.
[0186] A preferred average residence time of the silicon dioxide granules during the dynamic thermal treatment depends on the quantity. The average residence time of the silicon dioxide granules during the dynamic thermal treatment is preferably in the range of 10 to 180 minutes, for example in the range of 20 to 120 minutes or 30 to 90 minutes. The average residence time of the silicon dioxide granules during the dynamic thermal treatment is particularly preferably in the range of 30 to 90 minutes.
[0187] In the case of a continuous process, a batch is considered to be a defined portion of a flow of silicon dioxide granules, e.g., one gram, one kilogram, or one ton, for the purpose of determining the residence time. The start and end of the residence time are determined by the inlet and outlet from the continuous furnace operation.
[0188] In a continuous process for dynamic thermal treatment, the throughput of the silicon dioxide granules is preferably in the range of 1 to 50 kg / h, for example in the range of 5 to 40 kg / h or 8 to 30 kg / h. The throughput is particularly preferably in the range of 10 to 20 kg / h.
[0189] In the case of a discontinuous dynamic thermal treatment process, the treatment time results from the period between loading and subsequent unloading of the furnace.
[0190] In the case of a batch-based dynamic thermal treatment process, the throughput is in a range from 1 to 50 kg / h, for example in the range from 5 to 40 kg / h or from 8 to 30 kg / h. Particularly preferably, the throughput is in the range from 10 to 20 kg / h. The throughput can be achieved by a batch of a certain quantity being treated for one hour. According to another embodiment, the throughput can be achieved by a number of batches per hour, for example, the quantity of a batch corresponding to the throughput per hour divided by the number of batches. The treatment time then corresponds to the fraction of an hour resulting from 60 minutes divided by the number of batches per hour.
[0191] Preferably, the dynamic thermal treatment of the silicon dioxide granules is carried out at a furnace temperature of at least 500°C, for example in the range from 510 to 1700°C or from 550 to 1500°C or from 580 to 1300°C, particularly preferably in the range from 600 to 1200°C.
[0192] As a rule, the furnace chamber maintains the specified temperature. This temperature preferably deviates by less than 10% above or below the specified temperature, based on the total treatment time and the entire length of the furnace, both at any point during the treatment and at any location within the furnace.
[0193] Alternatively, in particular the continuous process of dynamic thermal treatment of the silicon dioxide granules can be carried out at different furnace temperatures. For example, the furnace can have a constant temperature over the treatment time, wherein the temperature varies in sections over the length of the furnace. Such sections can be of equal or different lengths. In this case, a temperature that increases from the furnace inlet to the furnace outlet is preferred. Preferably, the temperature at the inlet is at least 100°C lower than at the outlet, for example 150°C lower, or 200°C lower, or 300°C lower, or 400°C lower. More preferably, the temperature at the outlet is preferably at least 500°C, for example in the range from 510 to 1700°C, or from 550 to 1500°C, or from 580 to 1300°C, particularly preferably in the range from 600 to 1200°C.More preferably, the temperature at the inlet is preferably at least 300°C, for example from 400 to 1000°C or from 450 to 900°C or from 500 to 800°C or from 550 to 750°C, particularly preferably from 600 to 700°C. Furthermore, each of the mentioned temperature ranges at the furnace inlet can be combined with each of the mentioned temperature ranges at the furnace outlet. Preferred combinations of furnace inlet and furnace outlet temperature ranges are: Furnace inlet temperature range [°C] Furnace outlet temperature range [°C] 400 - 1000 510 - 1300 450 - 900 550 - 1260 480 - 850 580 - 1200 500 - 800 600 - 1100 530 - 750 630 - 1050
[0194] For the static thermal treatment of the silicon dioxide granules, crucibles arranged in a furnace are preferably used. Suitable crucibles are sintered crucibles or sheet metal crucibles. Rolled sheet metal crucibles made of several riveted plates are preferred. Examples of crucible materials include refractory metals, particularly tungsten, molybdenum, and tantalum. The crucibles can also be made of graphite or, in the case of refractory metal crucibles, lined with graphite foil. More preferably, the crucibles can be made of silicon dioxide. Silicon dioxide crucibles are particularly preferred.
[0195] The average residence time of the silicon dioxide granules during the static thermal treatment depends on the quantity. For a quantity of 20 kg of silicon dioxide granules, the average residence time of the silicon dioxide granules during the static thermal treatment is preferably in the range of 10 to 180 minutes, for example in the range of 20 to 120 minutes, particularly preferably in the range of 30 to 90 minutes.
[0196] The static thermal treatment of the silicon dioxide granules is preferably carried out at a furnace temperature of at least 800°C, for example in the range from 900 to 1700°C or from 950 to 1600°C or from 1000 to 1500°C or from 1050 to 1400°C, particularly preferably in the range from 1100 to 1300°C.
[0197] The static thermal treatment of the silicon dioxide granules I preferably takes place at a constant furnace temperature. The static thermal treatment can also take place at a varying furnace temperature. In this case, the temperature preferably increases over the course of the treatment, wherein the temperature at the beginning of the treatment is at least 50°C lower than at the end, for example 70°C lower or 80°C lower or 100°C lower or 110°C lower, and wherein the temperature at the end is preferably at least 800°C, for example in the range from 900 to 1700°C or from 950 to 1600°C or from 1000 to 1500°C or from 1050 to 1400°C, particularly preferably in the range from 1100 to 1300°C. mechanically
[0198] The silicon dioxide granules I can also be mechanically treated. The mechanical treatment can be carried out to increase the bulk density. The mechanical treatment can be combined with the previously described thermal treatment. Mechanical treatment can prevent the agglomerates in the silicon dioxide granules, and thus the average particle size of the individual, treated silicon dioxide granules, from becoming too large. An increase in the size of the agglomerates can complicate further processing or have adverse effects on the properties of the quartz glass bodies produced using the process according to the invention, or can result in a combination of both effects. Mechanical treatment of the silicon dioxide granules also promotes uniform contact of the surfaces of the individual silicon dioxide granules with the gas or gases.This is particularly achieved by combining simultaneous mechanical and chemical treatment with one or more gases. This can enhance the effectiveness of the chemical treatment.
[0199] The mechanical treatment of the silicon dioxide granules can be carried out by moving two or more silicon dioxide granules in a relative motion to each other, for example by rotating the tube of a rotary kiln.
[0200] Preferably, the silicon dioxide granulate I is treated chemically, thermally, and mechanically. In particular, the silicon dioxide granulate I is treated simultaneously chemically, thermally, and mechanically.
[0201] Chemical treatment reduces the impurity content in silicon dioxide granules I. For this purpose, the silicon dioxide granules I can be treated in a rotary kiln at elevated temperatures in a chlorine- and oxygen-containing atmosphere. Water present in the silicon dioxide granules I evaporates, and organic materials react to form CO and CO2. Metal impurities can be converted into volatile, chlorine-containing compounds.
[0202] Preferably, the silicon dioxide granulate I is treated in a chlorine- and oxygen-containing atmosphere in a rotary kiln at a temperature of at least 500°C, preferably in a temperature range of 550 to 1300°C or 600 to 1260°C or 650 to 1200°C or 700 to 1000°C, particularly preferably in a temperature range of 700 to 900°C. The chlorine-containing atmosphere contains, for example, HCl or Cl 2 or a combination of both. This treatment reduces the carbon content.
[0203] Furthermore, alkali and iron impurities are preferably reduced. A reduction in the number of OH groups is also preferred. At temperatures below 700°C, long treatment times can result; at temperatures above 1100°C, there is a risk that the pores of the granulate will close, trapping chlorine or gaseous chlorine compounds.
[0204] Preferably, it is also possible to carry out several chemical treatment steps consecutively, each with simultaneous thermal and mechanical treatment. For example, the silicon dioxide granulate I can be treated first in a chlorine-containing atmosphere and then in an oxygen-containing atmosphere.
[0205] The resulting low concentrations of carbon, hydroxyl groups and chlorine facilitate the melting of the silicon dioxide granules II.
[0206] Preferably, step II.2) can be characterized by at least one, for example by at least two or at least three, particularly preferably by a combination of all of the following features: N1) the reactant comprises HCl, Cl 2 or a combination thereof; N2) the treatment is carried out in a rotary kiln; N3) the treatment is carried out at a temperature in a range of 600 to 900°C; N4) the reactant forms a countercurrent; N5) the reactant has a gas flow in a range of 50 to 2000 L / h, preferably 100 to 1000 L / h, particularly preferably 200 to 500 L / h; N6) the reactant has a volume fraction of inert gas in a range of 0 to less than 50 vol%.
[0207] The silicon dioxide granules I can have a particle diameter that is larger than the particle diameter of the silicon dioxide powder. Preferably, the particle diameter of the silicon dioxide granules I is up to 300 times larger than the particle diameter of the silicon dioxide powder, for example, up to 250 times larger, or up to 200 times larger, or up to 150 times larger, or up to 100 times larger, or up to 50 times larger, or up to 20 times larger, or up to 10 times larger, particularly preferably 2 to 5 times larger.
[0208] The resulting silicon dioxide granulate is also referred to as silicon dioxide granulate II. Particularly preferably, silicon dioxide granulate II is obtained from silicon dioxide granulate I in a rotary kiln using a combination of thermal, mechanical, and chemical treatment.
[0209] The silicon dioxide granules provided in step i.) are preferably selected from the group consisting of silicon dioxide granules I, silicon dioxide granules II and a combination thereof.
[0210] "Silicon dioxide granulate I" refers to silicon dioxide granules produced by granulating silicon dioxide powder obtained during the pyrolysis of silicon compounds in a fuel gas flame. The preferred fuel gases are oxyhydrogen gas, natural gas, or methane gas, with oxyhydrogen gas being particularly preferred.
[0211] "Silicon dioxide granulate II" refers to granules of silicon dioxide produced by post-treatment of silicon dioxide granulate I. Chemical, thermal, and / or mechanical treatments are possible post-treatments. This will be explained in detail in the description of the preparation of the silicon dioxide granulate (process step II of the first aspect of the invention).
[0212] Particularly preferably, the silicon dioxide granulate provided in step i.) is silicon dioxide granulate I. The silicon dioxide granulate I has the following features: [A] a BET surface area in the range from 20 to 50 m 2 / g, for example in a range from 20 to 40 m 2 / g; particularly preferably in a range from 25 to 35 m 2 / g; the micropore content preferably amounts to a BET surface area in a range from 4 to 5 m 2 / g; for example in a range from 4.1 to 4.9 m 2 / g; particularly preferably in a range from 4.2 to 4.8 m 2 / g; and [B] an average particle size in a range from 180 to 300 µm.
[0213] Preferably, the silicon dioxide granulate I is characterized by at least one, for example by at least two or at least three or at least four, particularly preferably by at least five of the following features: [C] a bulk density in a range of 0.5 to 1.2 g / cm 3 , for example in a range of 0.6 to 1.1 g / cm 3 , more preferably in a range of 0.7 to 1.0 g / cm 3 ; [D] a carbon content of less than 50 ppm, for example less than 40 ppm or less than 30 ppm or less than 20 ppm or less than 10 ppm, more preferably in a range of 1 ppb to 5 ppm; [E] an aluminum content of less than 200 ppb, preferably less than 100 ppb, for example less than 50 ppb or from 1 to 200 ppb or from 15 to 100 ppb, more preferably in a range of 1 to 50 ppb. [F] a tapped density in a range of 0.5 to 1.2 g / cm 3 , for example in a range of 0.6 to 1.1 g / cm 3 , particularly preferably in a range of 0.75 to 1.0 g / cm 3 ; [G] a pore volume in a range of 0.1 to 1.5 mL / g, for example in a range of 0.15 to 1.1 mL / g;particularly preferably in a range from 0.2 to 0.8 mL / g, [H] a chlorine content of less than 200 ppm, preferably less than 150 ppm, for example less than 100 ppm, or less than 50 ppm, or less than 1 ppm, or less than 500 ppb, or less than 200 ppb, or in a range from 1 ppb to less than 200 ppm, or from 1 ppb to 100 ppm, or from 1 ppb to 1 ppm, or from 10 ppb to 500 ppb, or from 10 ppb to 200 ppb, particularly preferably from 1 ppb to 80 ppb; [I] metal content of metals other than aluminum of less than 1000 ppb, preferably in a range of 1 to 900 ppb, for example in a range of 1 to 700 ppb, particularly preferably in a range of 1 to 500 ppb; [J] a residual moisture content of less than 10 wt%, preferably in a range of 0.01 wt% to 5 wt%, for example from 0.02 to 1 wt%, particularly preferably from 0.03 to 0.5 wt%; ; where the wt%, ppm and ppb are each based on the total weight of the silicon dioxide granules I.
[0214] The OH content, also known as the hydroxyl group content, refers to the amount of OH groups in a material, for example, silicon dioxide powder, silicon dioxide granules, or a quartz glass body. The OH group content is determined spectroscopically in the infrared by comparing the first and third OH bands.
[0215] The chlorine content refers to the content of elemental chlorine or chloride ions in the silicon dioxide granules, the silicon dioxide powder or the quartz glass body.
[0216] The aluminum content refers to the content of elemental aluminum or aluminum ions in the silicon dioxide granules, the silicon dioxide powder or the quartz glass body.
[0217] The silicon dioxide granulate I preferably has a micropore content in a range of 4 to 5 m 2 / g, for example in a range of 4.1 to 4.9 m 2 / g; particularly preferably in a range of 4.2 to 4.8 m 2 / g.
[0218] The silicon dioxide granulate I preferably has a density in a range of 2.1 to 2.3 g / cm 3< , particularly preferably in a range of 2.18 to 2.22 g / cm 3<.
[0219] The silicon dioxide granulate I preferably has an average particle size in a range of 180 to 300 µm, for example in a range of 220 to 280 µm, particularly preferably in a range of 230 to 270 µm.
[0220] The silicon dioxide granules I preferably have a particle size D 50 in a range from 150 to 300 µm, for example in a range from 200 to 280 µm, particularly preferably in a range from 230 to 270 µm. Further preferably, the silicon dioxide granules I have a particle size D 10 in a range from 50 to 150 µm, for example in a range from 100 to 150 µm, particularly preferably in a range from 120 to 150 µm. Further preferably, the silicon dioxide granules I have a particle size D 90 in a range from 250 to 620 µm, for example in a range from 300 to 550 µm, particularly preferably in a range from 300 to 450 µm.
[0221] The silicon dioxide granulate I preferably has the feature combination [A] / [B] / [C] or [A] / [B] / [E] or [A] / [B] / [G], more preferably the feature combination [A] / [B] / [C] / [E] or [A] / [B] / [C] / [G] or [A] / [B] / [E] / [G], particularly preferably the feature combination [A] / [B] / [C] / [E] / [G].
[0222] The silicon dioxide granulate I preferably has the feature combination [A] / [B] / [C], wherein the BET surface area is in a range of 20 to 40 m 2 < / g, the average particle size is in a range of 180 to 300 µm and the bulk density is in a range of 0.6 to 1.1 g / mL.
[0223] The silicon dioxide granulate I preferably has the feature combination [A] / [B] / [E], wherein the BET surface area is in a range of 20 to 40 m 2 < / g, the average particle size is in a range of 180 to 300 µm and the aluminum content is in a range of 1 to 50 ppb.
[0224] The silicon dioxide granulate I preferably has the feature combination [A] / [B] / [G], wherein the BET surface area is in a range of 20 to 40 m 2 < / g, the average particle size is in a range of 180 to 300 µm and the pore volume is in a range of 0.2 to 0.8 mL / g.
[0225] The silicon dioxide granulate I preferably has the feature combination [A] / [B] / [C] / [E], wherein the BET surface area is in a range of 20 to 40 m 2 < / g, the average particle size is in a range of 180 to 300 µm, the bulk density is in a range of 0.6 to 1.1 g / mL and the aluminum content is in a range of 1 to 50 ppb.
[0226] The silicon dioxide granulate I preferably has the feature combination [A] / [B] / [C] / [G], wherein the BET surface area is in a range of 20 to 40 m 2 < / g, the average particle size is in a range of 180 to 300 µm, the bulk density is in a range of 0.6 to 1.1 g / mL and the pore volume is in a range of 0.2 to 0.8 mL / g.
[0227] The silicon dioxide granulate I preferably has the feature combination [A] / [B] / [E] / [G], wherein the BET surface area is in a range of 20 to 40 m 2 / g, the average particle size is in a range of 180 to 300 µm, the aluminum content is in a range of 1 to 50 ppb and the pore volume is in a range of 0.2 to 0.8 mL / g.
[0228] The silicon dioxide granulate I preferably has the feature combination [A] / [B] / [C] / [E] / [G], wherein the BET surface area is in a range of 20 to 40 m 2 < / g, the average particle size is in a range of 180 to 300 µm, the bulk density is in a range of 0.6 to 1.1 g / mL, the aluminum content is in a range of 1 to 50 ppb and the pore volume is in a range of 0.2 to 0.8 mL / g.
[0229] Particle size is the size of the aggregated primary particles present in a silica powder, slurry, or silica granules. Mean particle size is the arithmetic mean of all particle sizes of the specified substance. The D 50 value indicates that 50% of the particles, based on the total number of particles, are smaller than the specified value. The D 10 value indicates that 10% of the particles, based on the total number of particles, are smaller than the specified value. The D 90 value indicates that 90% of the particles, based on the total number of particles, are smaller than the specified value. The particle size is determined using the dynamic image analysis method according to ISO 13322-2:2006-11.
[0230] More particularly preferably, the silicon dioxide granulate provided in step i.) may be the silicon dioxide granulate II. The silicon dioxide granulate II has the following features: (A) a BET surface area in the range of 10 to 35 m 2 / g, for example in a range of 10 to 30 m 2 / g, particularly preferably in a range of 20 to 30 m 2 / g; and (B) an average particle size in a range of 100 to 300 µm, for example in a range of 150 to 280 µm or 200 to 270 µm, particularly preferably in a range of 230 to 260 µm.
[0231] Preferably, the silicon dioxide granulate II has at least one, for example at least two or at least three or at least four, particularly preferably at least five of the following features: (C) a bulk density in a range of 0.7 to 1.2 g / cm 3 , for example in a range of 0.75 to 1.1 g / cm 3 , more preferably in a range of 0.8 to 1.0 g / cm 3 ; (D) a carbon content of less than 5 ppm, for example less than 4.5 ppm or in a range of 1 ppb to 4 ppm, more preferably less than 4 ppm; (E) an aluminum content of less than 200 ppb, for example less than 150 ppb or less than 100 ppb or from 1 to 150 ppb or from 1 to 100 ppb, more preferably in a range of 1 to 80 ppb; (F) tapped density in a range of 0.7 to 1.2 g / cm 3 , for example in a range of 0.75 to 1.1 g / cm 3 , particularly preferably in a range of 0.8 to 1.0 g / cm 3 ; (G) a pore volume in a range of 0.1 to 2.5 mL / g, for example in a range of 0.2 to 1.5 mL / g; particularly preferably in a range of 0.4 to 1 mL / g;(H) a chlorine content of less than 500 ppm, preferably less than 400 ppm, for example less than 350 ppm or preferably less than 330 ppm or in a range from 1 ppb to 500 ppm or from 10 ppb to 450 ppm, particularly preferably from 50 ppb to 300 ppm; (I) a metal content of metals other than aluminum of less than 1000 ppb, for example in a range from 1 to 400 ppb, particularly preferably in a range from 1 to 200 ppb; (I) a residual moisture content of less than 3 wt.%, for example in a range from 0.001 wt.% to 2 wt.%, particularly preferably from 0.01 to 1 wt.%, wherein the wt.%, ppm and ppb are each based on the total weight of the silicon dioxide granules II. ;
[0232] Preferably, the silicon dioxide granulate II has a micropore content in a range of 1 to 2 m 2 < / g, for example in a range of 1.2 to 1.9 m 2 < / g, particularly preferably in a range of 1.3 to 1.8 m 2 < / g.
[0233] The silicon dioxide granulate II preferably has a density in a range from 0.5 to 2.0 g / cm 3 , for example from 0.6 to 1.5 g / cm 3 , particularly preferably from 0.8 to 1.2 g / cm 3 . The density is determined according to the method described in the test methods.
[0234] The silicon dioxide granulate II preferably has a particle size D 50 in a range from 150 to 300 µm, for example in a range from 200 to 280 µm, particularly preferably in a range from 230 to 270 µm. Further preferably, the silicon dioxide granulate II has a particle size D 10 in a range from 50 to 150 µm, for example in a range from 100 to 150 µm, particularly preferably in a range from 120 to 150 µm. Further preferably, the silicon dioxide granulate II has a particle size D 90 in a range from 250 to 620 µm, for example in a range from 300 to 550 µm, particularly preferably in a range from 300 to 450 µm.
[0235] The silicon dioxide granulate II preferably has the feature combination (A) / (B) / (D) or (A) / (B) / (F) or (A) / (B) / (I), more preferably the feature combination (A) / (B) / (D) / (F) or (A) / (B) / (D) / (I) or (A) / (B) / (F) / (I), particularly preferably the feature combination (A) / (B) / (D) / (F) / (I).
[0236] The silicon dioxide granulate II preferably has the feature combination (A) / (B) / (D), wherein the BET surface area is in a range of 10 to 30 m 2 / g, the average particle size is in a range of 150 to 280 µm and the carbon content is less than 4 ppm.
[0237] The silicon dioxide granulate II preferably has the feature combination (A) / (B) / (F), wherein the BET surface area is in a range of 10 to 30 m 2 / g, the average particle size is in a range of 150 to 280 µm and the tamped density is in a range of 0.8 to 1.0 g / mL.
[0238] The silicon dioxide granulate II preferably has the feature combination (A) / (B) / (I), wherein the BET surface area is in a range of 10 to 30 m 2 < / g, the average particle size is in a range of 150 to 280 µm and the metal content of metals other than aluminum is in a range of 1 to 400 ppb.
[0239] The silicon dioxide granulate II preferably has the feature combination (A) / (B) / (D) / (F), wherein the BET surface area is in a range of 10 to 30 m 2 < / g, the average particle size is in a range of 150 to 280 µm, the carbon content is less than 4 ppm and the tamped density is in a range of 0.8 to 1.0 g / mL.
[0240] The silicon dioxide granulate II preferably has the feature combination (A) / (B) / (D) / (I), wherein the BET surface area is in a range of 10 to 30 m 2 < / g, the average particle size is in a range of 150 to 280 µm, the carbon content is less than 4 ppm and the metal content of metals other than aluminum is in a range of 1 to 400 ppb.
[0241] The silicon dioxide granulate II preferably has the feature combination (A) / (B) / (F) / (I), wherein the BET surface area is in a range of 10 to 30 m 2 < / g, the average particle size is in a range of 150 to 280 µm, the tamped density is in a range of 0.8 to 1.0 g / mL and the metal content of metals other than aluminum is in a range of 1 to 400 ppb.
[0242] The silicon dioxide granulate II preferably has the feature combination (A) / (B) / (D) / (F) / (I), wherein the BET surface area is in a range of 10 to 30 m 2 < / g, the average particle size is in a range of 150 to 280 µm, the carbon content is less than 4 ppm, the tamped density is in a range of 0.8 to 1.0 g / mL and the metal content of metals other than aluminum is in a range of 1 to 400 ppb. Step ii.)
[0243] According to step ii.), a glass melt can be formed from the silicon dioxide granules. Typically, the silicon dioxide granules are heated until a glass melt is obtained. Heating the silicon dioxide granules to a glass melt can, in principle, be carried out by any method known to the person skilled in the art for this purpose. V-Zug for producing a glass melt
[0244] The formation of a glass melt from the silicon dioxide granules, for example, by heating, can be carried out using a continuous process. In the process according to the invention for producing a quartz glass body, the silicon dioxide granules can preferably be continuously introduced into a furnace, or the glass melt can be continuously removed from the furnace, or both. Particularly preferably, the silicon dioxide granules are continuously introduced into the furnace and the glass melt is continuously removed from the furnace.
[0245] In principle, a furnace having at least one inlet and at least one outlet is suitable for this purpose. An inlet is understood to be an opening through which silicon dioxide and, if appropriate, other substances can be introduced into the furnace. An outlet is understood to be an opening through which at least a portion of the silicon dioxide can be removed from the furnace. The furnace can, for example, be oriented vertically and horizontally. The furnace is preferably oriented vertically. Preferably, at least one inlet is located above at least one outlet. In the context of internals and features of a furnace, in particular an inlet and outlet, "above" means that the internal or feature arranged "above" another is at a higher position above sea level. "Vertical" is understood to mean that the direct connection between the inlet and outlet of the furnace has a deviation of no more than 30° from the vertical direction.
[0246] The furnace may include a suspended metal crucible. The silicon dioxide granules are placed into the suspended metal crucible and heated to form a glass melt. A metal crucible is understood to be a crucible containing at least one rolled sheet. A metal crucible preferably comprises several rolled sheets. A suspended metal crucible is understood to be a metal crucible of the type described above that is suspended in a furnace.
[0247] The suspended metal crucible can, in principle, be made of any material known to those skilled in the art and suitable for melting silicon dioxide. Preferably, the sheet metal of the suspended metal crucible contains a sintered material, for example, a sintered metal. Sintered metals are metals or alloys obtained by sintering metal powders.
[0248] The sheet metal of the sheet metal crucible preferably contains at least one element selected from the group consisting of refractory metals. Refractory metals are understood to be the metals of subgroup 4 (Ti, Zr, H1), subgroup 5 (V, Nb, Ta), and subgroup 6 (Cr, Mo, W).
[0249] The sheet of the sheet metal crucible preferably contains a sintered metal selected from the group consisting of molybdenum, tungsten, or a combination thereof. Further preferably, the sheet of the sheet metal crucible contains at least one further refractory metal, particularly preferably rhenium, osmium, iridium, ruthenium, or a combination of two or more thereof.
[0250] Preferably, the sheet of the sheet metal crucible comprises an alloy of molybdenum with a refractory metal, or tungsten with a refractory metal. Particularly preferred alloying metals are rhenium, osmium, iridium, ruthenium, or a combination of two or more thereof. According to another example, the sheet of the sheet metal crucible is an alloy of molybdenum with tungsten, rhenium, osmium, iridium, ruthenium, or a combination of two or more thereof. For example, the sheet of the sheet metal crucible is an alloy of tungsten with molybdenum, rhenium, osmium, iridium, ruthenium, or a combination of two or more thereof.
[0251] Preferably, the above-described sheet of the sheet metal crucible can be coated with a refractory metal. According to a preferred example, the sheet of the sheet metal crucible is coated with rhenium, osmium, iridium, ruthenium, molybdenum, and tungsten, or a combination of two or more thereof.
[0252] Preferably, the sheet and the coating have different compositions. For example, a molybdenum sheet is coated with one or more layers of rhenium, osmium, iridium, ruthenium, tungsten, or a combination of two or more thereof. According to another example, a tungsten sheet is coated with one or more layers of rhenium, osmium, iridium, ruthenium, molybdenum, or a combination of two or more thereof. According to a further example, the sheet of the sheet crucible can consist of molybdenum alloyed with rhenium or of tungsten alloyed with rhenium, and can be coated on the inside of the crucible with one or more layers comprising rhenium, osmium, iridium, ruthenium, or a combination of two or more thereof.
[0253] The sheet of the suspended sheet metal crucible preferably has a density of 95% or more of the theoretical density, for example a density of 95% to 98% or of 96% to 98%. Higher theoretical densities are further preferred, in particular in the range of 98 to 99.95%. The theoretical density of a material corresponds to the density of a pore-free and 100% dense material. A density of the sheet of the sheet metal crucible of more than 95% of the theoretical density can be obtained, for example, by sintering a sintered metal and subsequently compacting the sintered material. A sheet metal crucible is particularly preferably obtainable by sintering a sintered metal, rolling to obtain a sheet, and processing the sheet metal into a crucible.
[0254] The metal crucible preferably has at least one lid, one wall, and one base plate. The suspended metal crucible preferably has at least one, for example at least two or at least three or at least four, particularly preferably at least five or all of the following features: (a) at least one, e.g. more than one or at least two or at least three or at least five, particularly preferably three or four layers of sheet metal; (b) at least one sheet, e.g. at least three or at least four or at least six or at least eight or at least twelve or at least 15 or at least 16 or at least 20 sheets, particularly preferably twelve or 16 sheets; (c) at least one connection of two sheet metal pieces, e.g. at least two or at least five or at least ten or at least 18 or at least 24 or at least 36 or at least 48 or at least 60 or at least 72 or at least 48 or at least 96 or at least 120 or at least 160, particularly preferably 36 or 48 connections of two identical or more different sheet metal pieces of the hanging sheet metal crucible; (d) the sheet metal pieces of the hanging sheet metal crucible are riveted, e.g. at at least one connection, by deep drawing, e.g.by a combination of deep drawing with sheet metal attachment, or connected by countersinking, screwed or welded, e.g. by electron beam welding and sintering of the welds, particularly preferably riveted; (e) the sheet metal of the suspended sheet metal crucible is obtainable by a forming step associated with an increase in the physical density, preferably by forming a sintered metal or a sintered alloy; more preferably, the forming is rolling; (f) a suspension made of copper, aluminum, steel, iron, nickel or a refractory metal, e.g. from the crucible material, preferably a water-cooled suspension made of copper or steel; (g) a nozzle, preferably a nozzle firmly connected to the crucible; (h) a mandrel, for example a mandrel attached to the nozzle by webs or a mandrel attached to the lid by a holding rod or a mandrel connected to a holding rod from below the crucible; (i) at least one gas inlet, e.g.in the form of a filling tube or as a separate inlet; (j) at least one gas outlet, e.g. as a separate outlet on the lid or in the wall of the crucible; (k) a cooled jacket, preferably a water-cooled jacket; (l) external insulation, preferably external insulation made of zirconium oxide.
[0255] The hanging sheet metal crucible can, in principle, be heated by any method familiar to a person skilled in the art and deemed suitable for this purpose. The hanging sheet metal crucible can be heated, for example, using electrical heating elements (resistive) or by induction. With resistive heating, the solid surface of the sheet metal crucible is heated from the outside and transfers the energy from there to its interior. With inductive heating, the energy is coupled directly into the side wall of the crucible via coils and from there transferred to the interior of the crucible. With resistive heating, the energy is coupled in by radiation, whereby the solid surface is heated from the outside and the energy is transferred from there to its interior. The crucible is preferably heated inductively.
[0256] Preferably, the energy input into the melting crucible, in particular for melting a melting material, is not carried out by heating the melting crucible, or a melting material present therein, or both, by means of a flame, such as a burner flame directed into the melting crucible or onto the melting crucible.
[0257] The suspended arrangement allows the suspended sheet metal crucible to be moved within the furnace. Preferably, the crucible can be moved at least partially into and out of the furnace. If the furnace contains different heating zones, their temperature profiles are transferred to the crucible located within the furnace. By changing the position of the crucible within the furnace, multiple heating zones, varying heating zones, or multiple varying heating zones within the crucible can be realized.
[0258] The sheet metal crucible has a nozzle. The nozzle is formed from a nozzle material. The nozzle material preferably contains a pre-compacted material, for example with a density in a range of more than 95%, for example from 98 to 100%, particularly preferably from 99 to 99.999%, in each case based on the theoretical density of the nozzle material. The nozzle material preferably contains a refractory metal, for example molybdenum, tungsten, or a combination thereof with another refractory metal. Molybdenum is particularly preferred as the nozzle material. A nozzle containing molybdenum can preferably have a density of 100% of the theoretical density.
[0259] Preferably, the base plate contained in a sheet metal crucible is thicker than the sides of the sheet metal crucible. Preferably, the base plate is made of the same material as the sides of the sheet metal crucible. Preferably, the base plate of the sheet metal crucible is not a rolled sheet. The base plate is, for example, 1.1 to 5000 times thicker, or 2 to 1000 times thicker, or 4 to 500 times thicker, particularly preferably 5 to 50 times thicker, in each case with respect to a wall of the sheet metal crucible.
[0260] The furnace preferably includes a hanging or standing sintering crucible. The silicon dioxide granules are placed into the hanging or standing sintering crucible and heated to form a glass melt.
[0261] A sintered crucible is a crucible made of a sintered material containing at least one sintered metal and having a density of no more than 96% of the theoretical density of the metal. Sintered metals are metals or alloys obtained by sintering metal powders. The sintered material and the sintered metal in a sintered crucible are not rolled.
[0262] Preferably, the sintered material of the sintering crucible has a density of 85% or more of the theoretical density of the sintered material, for example a density of 85% to 95% or of 90% to 94%, particularly preferably of 91% to 93%.
[0263] The sintered material can, in principle, consist of any material known to the person skilled in the art and suitable for melting silicon dioxide. Preferably, the sintered material is made of at least one element selected from the group consisting of refractory metals, graphite, or materials coated with graphite foil.
[0264] The sintered material preferably contains a first sintered metal selected from the group consisting of molybdenum, tungsten, and a combination thereof. More preferably, the sintered material also contains at least one further refractory metal that is different from the first sintered metal, particularly preferably selected from the group consisting of molybdenum, tungsten, rhenium, osmium, iridium, ruthenium, or a combination of two or more thereof.
[0265] The sintered material preferably comprises an alloy of molybdenum with a refractory metal, or tungsten with a refractory metal. Particularly preferred alloying metals are rhenium, osmium, iridium, ruthenium, or a combination of two or more thereof. According to another example, the sintered material comprises an alloy of molybdenum with tungsten, rhenium, osmium, iridium, ruthenium, or a combination of two or more thereof. For example, the sintered material comprises an alloy of tungsten with molybdenum, rhenium, osmium, iridium, ruthenium, or a combination of two or more thereof.
[0266] Preferably, the sintered material described above can include a coating containing a refractory metal, in particular rhenium, osmium, iridium, ruthenium, or a combination of two or more thereof. According to a preferred example, the coating contains rhenium, osmium, iridium, ruthenium, molybdenum, and tungsten, or a combination of two or more thereof.
[0267] The sintered material and its coating preferably have different compositions. For example, a sintered material comprising molybdenum is coated with one or more layers of rhenium, osmium, iridium, ruthenium, tungsten, or a combination of two or more thereof. According to another example, a sintered material comprising tungsten is coated with one or more layers of rhenium, osmium, iridium, ruthenium, molybdenum, or a combination of two or more thereof. According to a further example, the sintered material can consist of molybdenum alloyed with rhenium or of tungsten alloyed with rhenium, and can be coated towards the inside of the crucible with one or more layers comprising rhenium, osmium, iridium, ruthenium, or a combination of two or more thereof.
[0268] A sintered crucible is preferably manufactured by sintering the sintered material in a mold. The sintered crucible can be manufactured as a whole in a mold. It is also possible for individual parts of the sintered crucible to be manufactured in a mold and then processed to form the sintered crucible. The crucible is preferably manufactured from more than one part, for example from a base plate and one or more side parts. The side parts are preferably manufactured in one piece relative to the circumference of the crucible. The sintered crucible can preferably be manufactured from several side parts arranged one above the other. The side parts of the sintered crucible are preferably sealed by screwing or by a tongue and groove connection. Screwing is preferably carried out by manufacturing side parts that have a thread on the edges.In a tongue-and-groove joint, two side parts to be connected each have a groove at the edges, into which a tongue is inserted as a connecting third part, thus forming a positive connection perpendicular to the crucible wall plane. A sintered crucible is particularly preferably manufactured from more than one side part, for example, from two or more side parts, particularly preferably from three or more side parts. The parts of the suspended sintered crucible are particularly preferably screwed together. The parts of the upright sintered crucible are particularly preferably connected by means of a tongue-and-groove joint.
[0269] The base plate can in principle be connected to the crucible wall by any means known to those skilled in the art and suitable for this purpose. According to a preferred embodiment, the base plate is provided with an external thread and is connected to the crucible wall by screwing the base plate into the crucible wall. According to a further preferred embodiment, the base plate is connected to the crucible wall by means of screws. According to a further preferred embodiment, the base plate is suspended in the sintering crucible, for example by placing the base plate on an inner collar of the crucible wall. According to a further preferred embodiment, at least part of the crucible wall and a thickened base plate are sintered in one piece. The base plate and the crucible wall of the suspended sintering crucible are particularly preferably screwed together.Particularly preferably, the base plate and the crucible wall of the standing sintering crucible are connected by means of a tongue and groove connection.
[0270] Preferably, the base plate contained in a sintered crucible is thicker than the sides, for example, 1.1 to 20 times thicker, or 1.2 to 10 times thicker, or 1.5 to 7 times thicker, particularly preferably 2 to 5 times thicker. The sides preferably have a constant wall thickness across the circumference and height of the sintered crucible.
[0271] The sintered crucible can have a nozzle. The nozzle is formed from a nozzle material. The nozzle material preferably contains a pre-compacted material, for example with a density in a range of more than 95%, for example from 98 to 100%, particularly preferably from 99 to 99.999%, in each case based on the theoretical density of the nozzle material. The nozzle material preferably contains a refractory metal, for example molybdenum, tungsten, or a combination thereof with a refractory metal. Molybdenum is particularly preferred as the nozzle material. A nozzle containing molybdenum can preferably have a density of 100% of the theoretical density.
[0272] The hanging sintering crucible can in principle be heated in any way that is familiar to a person skilled in the art and appears suitable for this purpose. The hanging sintering crucible can, for example, be heated inductively or resistively. With inductive heating, the energy is coupled directly into the side wall of the sintering crucible through coils and from there transferred to the inside of the crucible. With resistive heating, the energy is coupled in by radiation, whereby the solid surface is heated from the outside and the energy is transferred from there to its inside. The sintering crucible is preferably heated inductively. With resistive heating, the energy is coupled in by radiation, whereby the solid surface is heated from the outside and the energy is transferred from there to its inside. The crucible is preferably heated inductively.
[0273] Preferably, the energy input into the melting crucible, in particular for melting a melting material, is not carried out by heating the melting crucible, or a melting material present therein, or both, by means of a flame, such as a burner flame directed into the melting crucible or onto the melting crucible.
[0274] The sintering crucible preferably has one or more than one heating zone, for example one or two or three or more than three heating zones, preferably one or two or three heating zones, particularly preferably one heating zone. The heating zones of the sintering crucible can be brought to the same or different temperatures. For example, all heating zones can be brought to one temperature, all heating zones to different temperatures, or two or more heating zones can be brought to one temperature and one or more heating zones can be brought to different temperatures independently of one another. Preferably, all heating zones are brought to different temperatures; for example, the temperature of the heating zones increases in the direction of material transport of the silicon dioxide granules.
[0275] A hanging sintering crucible is a sintering crucible of the type described above which is arranged in a hanging manner in a furnace.
[0276] Preferably, the suspended sintering crucible has at least one, for example at least two or at least three or at least four, particularly preferably all of the following features: {a} a suspension, preferably a height-adjustable suspension; {b} at least two sealed rings as side parts, preferably at least two rings screwed together as side parts; {c} a nozzle, preferably a nozzle firmly connected to the crucible; {d} a mandrel, for example a mandrel attached to the nozzle by webs or a mandrel attached to the lid by a holding rod or a mandrel connected to a holding rod from below the crucible; {e} at least one gas inlet, e.g. in the form of a filler tube or as a separate inlet, particularly preferably in the form of a filler tube; {f} at least one gas outlet, e.g. on the lid or in the wall of the crucible. {g} a cooled jacket, particularly preferably a water-cooled jacket; {h} insulation on the outside of the crucible, for example on the outside of the cooled jacket, preferably an insulation layer made of zirconium oxide.
[0277] A preferred suspension is one attached during the manufacture of the suspended sintering crucible, for example, a suspension provided as an integral component of the crucible, particularly preferably a suspension made of the sintering material provided as an integral component of the crucible. A further preferred suspension is a suspension attached to the sintering crucible made of a material different from the sintering material, for example, aluminum, steel, iron, nickel, or copper, preferably copper, particularly preferably a cooled suspension, for example, a water-cooled suspension made of copper, attached to the sintering crucible.
[0278] The suspended arrangement allows the suspended sintering crucible to be moved within the furnace. Preferably, the crucible can be moved at least partially into and out of the furnace. If the furnace contains different heating zones, their temperature profiles are transferred to the crucible located within the furnace. By changing the position of the crucible in the furnace, multiple heating zones, varying heating zones, or multiple varying heating zones within the crucible can be realized.
[0279] A standing sintering crucible is understood to be a sintering crucible of the type described above, which is arranged upright in a furnace.
[0280] Preferably, the standing sintering crucible has at least one, for example at least two or at least three or at least four, particularly preferably all of the following features: / a / a region shaped as a standing surface, preferably a region shaped as a standing surface at the bottom of the crucible, more preferably a region shaped as a standing surface in the bottom plate of the crucible, particularly preferably a region shaped as a standing surface at the outer edge of the bottom of the crucible; / b / at least two sealed rings as side parts, preferably at least two rings sealed by a tongue and groove connection as side parts; / c / a nozzle, preferably a nozzle firmly connected to the crucible, particularly preferably one in the region of the bottom of the crucible not shaped as a standing surface; / d / a mandrel, for example a mandrel attached to the nozzle by webs or a mandrel attached to the lid by webs or a mandrel connected to a support rod from below the crucible; / e / at least one gas inlet, e.g. in the form of a filling tube or as a separate inlet; / f / at least one gas outlet, e.g.as a separate outlet on the lid or in the wall of the crucible; / g / a lid. .
[0281] The upright sintering crucible preferably has a separation of the gas spaces in the furnace and in the area below the furnace. The area below the furnace is understood to be the area below the nozzle in which the removed glass melt is located. The gas spaces are preferably separated by the surface on which the crucible stands. Gas located in the gas space of the furnace between the inner and outer walls of the furnace cannot escape downwards into the area below the furnace. The removed glass melt has no contact with the gases from the gas space of the furnace. Glass melts removed from a furnace with an upright sintering crucible and quartz glass bodies formed therefrom preferably have a higher surface purity than glass melts and quartz glass bodies formed therefrom from a furnace with a hanging sintering crucible.
[0282] Preferably, the crucible is connected to the inlet and the outlet of the furnace in such a way that silicon dioxide granules can enter the crucible through the inlet of the furnace via the inlet of the crucible and glass melt can be removed through the outlet of the crucible and the outlet of the furnace.
[0283] In addition to the at least one inlet, the crucible preferably includes at least one opening, preferably a plurality of openings, through which gas can be introduced and discharged. The crucible preferably comprises at least two openings, at least one of which can be used as a gas inlet and at least one as a gas outlet. The use of at least one opening as a gas inlet and at least one opening as a gas outlet preferably results in a gas flow within the crucible.
[0284] The silicon dioxide granules are introduced into the crucible through the inlet and then heated within the crucible. Heating can occur in the presence of a gas or a mixture of two or more gases. During heating, water bound to the silicon dioxide granules can also enter the gas phase, forming another gas. The gas or mixture of two or more gases is located in the gas space of the crucible. The gas space of the crucible is the area inside the crucible that is not occupied by a solid or liquid phase. Suitable gases include hydrogen, inert gases, and two or more of these. Inert gases are those gases that do not react with the materials contained in the crucible up to a temperature of 2400°C. Preferred inert gases are nitrogen, helium, neon, argon, krypton, and xenon, particularly preferably argon and helium.Preferably, the heating is carried out in a reducing atmosphere. This can preferably be provided by hydrogen or a combination of hydrogen and an inert gas, for example, by a combination of hydrogen and helium, or hydrogen and nitrogen, or hydrogen and argon, particularly preferably by a combination of hydrogen and helium.
[0285] Preferably, an at least partial gas exchange of air, oxygen, and water for hydrogen, at least one inert gas, or for a combination of hydrogen and at least one inert gas is carried out on the silicon dioxide granules. The at least partial gas exchange is carried out on the silicon dioxide granules during introduction of the silicon dioxide granules, or before heating, or during heating, or during at least two of the aforementioned activities. Preferably, the silicon dioxide granules are heated to melting in a gas stream of hydrogen and at least one inert gas, for example, argon or helium.
[0286] Preferably, the dew point of the gas exiting through the gas outlet is below 0°C. The dew point is the temperature below which, at unchanged pressure, a component of the gas or gas mixture under investigation condenses. Generally, this refers to the condensation of water. The dew point is determined using a mirror dew point hygrometer according to the measurement method described in the methods section.
[0287] The furnace, and preferably also a melting crucible located therein, preferably has at least one gas outlet through which gas supplied to the furnace and generated during operation of the furnace is removed. The furnace may also have at least one dedicated gas inlet. Alternatively or additionally, gas can be introduced through the solids feed, also referred to as the solids inlet, for example, together with the silicon dioxide particles, or before, after, or through a combination of two or more of the aforementioned possibilities.
[0288] Preferably, the gas withdrawn from the furnace through the gas outlet has a dew point of less than 0°C upon exiting the furnace through the gas outlet, for example, less than -10°C or less than -20°C. The dew point is determined according to the measurement method described in the methods section at a slight overpressure of 5 to 20 mbar. A suitable measuring device, for example, is an "Optidew" device from Michell Instruments GmbH, D-61381 Friedrichsdorf.
[0289] The dew point of the gas is preferably determined at a measuring point at a distance of 10 cm or more from the furnace's gas outlet. This distance is often between 10 cm and 5 m. Within this distance range—here described as "at the outlet"—the distance of the measuring point from the furnace's gas outlet is irrelevant for the dew point measurement result. The gas is conveyed from the outlet to the measuring point by a fluid, for example, in a hose or pipe. The temperature of the gas at the measuring point is often between 10 and 60°C, for example, 20 to 50°C, especially 20 to 30°C.
[0290] Suitable gases and gas mixtures have already been described. Our own tests have shown that the above information applies to each of the gases and gas mixtures mentioned.
[0291] Preferably, the gas or gas mixture before entering the furnace, in particular the melting pot, has a dew point of less than -50°C, for example, less than -60°C, or less than -70°C, or less than -80°C. A dew point of -60°C is generally not exceeded. The following ranges for the dew point upon entering the furnace are also preferred: from -50 to -100°C; from -60 to -100°C; and from -70 to -100°C.
[0292] Preferably, the dew point of the gas before entering the furnace is at least 50°C lower than when exiting the melting pot, for example, at least 60°C or even 80°C. The above specifications apply to measuring the dew point upon exiting the melting pot. The same applies to measuring the dew point before entering the furnace. Since there is no source of moisture and no possibility of condensation between the measurement location and the furnace, the distance of the measuring point from the furnace's gas inlet is irrelevant.
[0293] Preferably, the furnace, in particular the melting pot, is operated with a gas exchange rate in a range of 200 to 3000 L / h.
[0294] The dew point is preferably determined in a measuring cell, wherein the measuring cell is separated from the gas exiting the gas outlet by a membrane. The membrane is preferably permeable to moisture. This measure can protect the measuring cell from a quantity of dust and other particles present in the gas stream, which are carried along with the gas flow from the melting furnace, especially a melting pot. This measure can significantly extend the service life of a measuring probe. The service life refers to the period of furnace operation during which neither replacement of the measuring probe nor cleaning of the measuring probe is necessary.
[0295] A dew point mirror measuring device is preferably used to determine the dew point.
[0296] The dew point at the gas outlet of the furnace can be adjusted. Preferably, a method for adjusting the dew point at the furnace outlet includes the following steps: I) providing an input material in a furnace, wherein the input material has a residual moisture content; II) operating the furnace with a gas stream being passed through the furnace; and III) varying the residual moisture content of the input material or the gas exchange rate of the gas stream.
[0297] Preferably, this method allows the dew point to be adjusted to a range of less than 0°C, for example, less than -10°C, particularly preferably less than -20°C. Further preferably, the dew point can be adjusted to a range of less than 0°C to -100°C, for example, less than -10°C to -80°C, particularly preferably less than -20°C to -60°C.
[0298] "Input material" refers to silicon dioxide particles provided for the production of a quartz glass body, preferably silicon dioxide granules, silicon dioxide grains, or combinations thereof. The silicon dioxide particles, the granules, and the grains are preferably characterized by the features described in the context of the first subject matter.
[0299] The furnace and the gas flow are preferably characterized by the features described in the first aspect. The gas flow is preferably formed by introducing a gas into the furnace through an inlet and discharging a gas from the furnace through an outlet. The "gas exchange rate" refers to the volume of gas that is discharged from the furnace through the outlet per unit of time. The gas exchange rate is also referred to as the gas flow rate or volumetric flow rate.
[0300] The dew point can be adjusted, in particular, by varying the residual moisture content of the input material or the gas exchange rate of the gas stream. For example, increasing the residual moisture content of the input material can raise the dew point. Reducing the residual moisture content of the input material can lower the dew point. An increased gas exchange rate can lead to a lower dew point. Conversely, a reduced gas exchange rate can result in an increased dew point.
[0301] Preferably, the gas exchange rate of the gas stream is in a range from 200 to 3000 L / h, for example from 200 to 2000 L / h, particularly preferably from 200 to 1000 L / h.
[0302] The residual moisture content of the input material is preferably in a range from 0.001 wt.% to 5 wt.%, for example from 0.01 to 1 wt.%, particularly preferably from 0.03 to 0.5 wt.%, in each case based on the total weight of the input material.
[0303] Preferably, the dew point can also be influenced by other measures. Examples of such measures are the dew point of the gas stream entering the furnace, the furnace temperature, and the composition of the gas stream. A reduction in the dew point of the gas stream entering the furnace, a reduction in the furnace temperature, or a reduction in the temperature of the gas stream at the furnace outlet can lead to a reduction in the dew point of the gas stream at the outlet. The temperature of the gas stream at the furnace outlet has no influence on the dew point as long as it is above the dew point.
[0304] Particularly preferably, the gas exchange rate of the gas stream is varied to adjust the dew point at the outlet of the furnace.
[0305] Preferably, the method is characterized by at least one, for example at least two or at least three, particularly preferably at least four of the following features: I} a residual moisture content of the input material in a range from 0.001 to 5 wt.%, for example from 0.01 to 1 wt.%, particularly preferably from 0.03 to 0.5 wt.-%, in each case based on the total weight of the input material; II} a gas exchange rate of the gas stream in a range from 200 to 3000 L / h, for example from 200 to 2000 L / h, particularly preferably from 200 to 1000 L / h; III} a furnace temperature in a range from 1700 to 2500°C, for example in a range from 1900 to 2400°C, particularly preferably in a range from 2100 to 2300°C; IV} a dew point of the gas stream on entry into the furnace in a range from -50°C to -100°C, for example from -60°C to -100°C, particularly preferably from -70°C to -100°C; V} the gas stream comprises helium, hydrogen or a combination thereof, preferably helium and hydrogen in a ratio of 20:80 to 95:5; VI} a temperature of the gas at the outlet in a range from 10 to 60°C, for example from 20 to 50°C, particularly preferably from 20 to 30°C.
[0306] For example, when using silicon dioxide granules with high residual moisture, it is preferable to use a gas stream with a high gas exchange rate and a low dew point at the furnace inlet. When using silicon dioxide granules with low residual moisture, however, a gas stream with a low gas exchange rate and a higher dew point at the furnace inlet can be used.
[0307] When using silicon dioxide granules with a residual moisture content of less than 3 wt.%, the gas exchange rate of a gas stream containing helium and hydrogen is particularly preferably in a range of 200 to 3000 L / h.
[0308] If silicon dioxide granules with a residual moisture content of 0.1% are fed into the furnace at a rate of 30 kg / h, a gas exchange rate of the gas stream is preferably selected, in the case of He / H 2 = 50:50 in a range of 2800 to 3000 l / h, and in the case of He / H 2 = 30:70 in a range of 2700 to 2900 l / h, and a dew point of the gas stream before entering the furnace of -90 °C. This results in a dew point of less than 0 °C at the gas outlet.
[0309] If silicon dioxide granules with a residual moisture content of 0.05% are fed into the furnace at a rate of 30 kg / h, a gas exchange rate of the gas stream is preferably selected, in the case of He / H 2 = 50:50, in a range of 1900 to 2100 l / h, and in the case of He / H 2 = 30:70, in a range of 1800 to 2000 l / h, and a dew point of the gas stream before entering the furnace of -90 °C. This results in a dew point of less than 0 °C at the gas outlet.
[0310] If silicon dioxide granules with a residual moisture content of 0.03% are fed into the furnace at a rate of 30 kg / h, a gas exchange rate of the gas stream is preferably selected, in the case of He / H 2 = 50:50, in a range of 1400 to 1600 l / h, and in the case of He / H 2 = 30:70, in a range of 1200 to 1400 l / h, and a dew point of the gas stream before entering the furnace of -90 °C. This results in a dew point of less than 0 °C at the gas outlet.
[0311] The furnace temperature for melting the silicon dioxide granules is preferably in the range of 1700 to 2500°C, for example in the range of 1900 to 2400°C, particularly preferably in the range of 2100 to 2300°C.
[0312] The residence time in the furnace is preferably in a range from 1 hour to 50 hours, for example, 1 to 30 hours, particularly preferably 5 to 20 hours. In the context of the present invention, the residence time means the time required to remove a filling quantity from the melting furnace in which the glass melt is formed during the process according to the invention. The filling quantity is the total mass of silicon dioxide present in the melting furnace. The silicon dioxide can be present as a solid or as a glass melt.
[0313] The furnace temperature preferably increases along the length in the direction of material transport. The furnace temperature preferably increases along the length in the direction of material transport by at least 100°C, for example by at least 300°C or by at least 500°C or by at least 700°C, particularly preferably by at least 1000°C. The highest temperature in the furnace is preferably 1700 to 2500°C, for example 1900 to 2400°C, particularly preferably 2100 to 2300°C. The furnace temperature can increase uniformly or according to a temperature profile.
[0314] The furnace temperature preferably decreases before the glass melt is removed from the furnace. The furnace temperature preferably decreases by 50 to 500°C, for example by 100°C or 400°C, particularly preferably by 150 to 300°C, before the glass melt is removed from the furnace. The temperature of the glass melt during removal is preferably 1750 to 2100°C, for example 1850 to 2050°C, particularly preferably 1900 to 2000°C.
[0315] The furnace temperature preferably increases along the length in the direction of material transport and decreases before the glass melt is removed from the furnace. The furnace temperature preferably increases along the length in the direction of material transport by at least 100°C, for example by at least 300°C or by at least 500°C or by at least 700°C, particularly preferably by at least 1000°C. The highest temperature in the furnace is preferably 1700 to 2500°C, for example 1900 to 2400°C, particularly preferably 2100 to 2300°C. The furnace temperature preferably decreases by 50 to 500°C before the glass melt is removed from the furnace, for example by 100°C or by 400°C, particularly preferably by 150 to 300°C. Preheating section
[0316] The furnace preferably has at least a first and one further chamber connected to one another by a passage, wherein the first and the further chamber have different temperatures, the temperature of the first chamber being lower than the temperature of the further chamber. In the further chamber, a glass melt is formed from the silicon dioxide granules. This chamber is referred to below as the melting chamber. A chamber connected to the melting chamber via a material guide but located upstream is also referred to as a preheating section. For example, it is one in which at least one outlet is directly connected to an inlet of the melting chamber. The aforementioned arrangement can also be implemented in stand-alone furnaces. In this case, the melting chamber is a melting furnace. For the purposes of the further description, however, the melting furnace can be understood as a synonym for the melting chamber.Accordingly, the statements regarding the melting furnace also apply to the melting chamber, and vice versa. The term "preheating section" is the same in both perspectives.
[0317] Preferably, the silicon dioxide granules have a temperature in the range of 20 to 1300°C when entering the furnace.
[0318] Preferably, the silicon dioxide granules can be omitted before entering the melting chamber. For example, the silicon dioxide granules have a temperature in the range of 20 to 40°C, particularly preferably 20 to 30°C, upon entering the furnace. If silicon dioxide granules II are provided according to step i.), they preferably have a temperature in the range of 20 to 40°C, particularly preferably 20 to 30°C, upon entering the furnace.
[0319] Alternatively, the silicon dioxide granules can be tempered to a temperature in the range of 40 to 1300°C before entering the furnace. Tempering means setting the temperature to a selected value. Tempering can, in principle, be carried out using any method known to those skilled in the art and known for tempering silicon dioxide granules. For example, tempering can take place in a furnace located separately from the melting chamber or in a furnace connected to the melting chamber.
[0320] Preferably, tempering takes place in a chamber connected to the melting chamber. The furnace preferably comprises a preheating section in which the silicon dioxide can be tempered. The preheating section itself is preferably a continuous furnace, particularly preferably a rotary kiln. A continuous furnace is understood to be a heated chamber that, during operation, causes the silicon dioxide to move from an inlet of the continuous furnace to an outlet of the continuous furnace. The outlet is preferably directly connected to the inlet of the melting furnace. This allows the silicon dioxide granules to flow from the preheating section into the melting furnace without any further intermediate steps or measures.
[0321] It is further preferred that the preheating section comprises at least one gas inlet and at least one gas outlet. Gas can enter the interior, the gas space of the preheating section, through the gas inlet, and can be discharged through the gas outlet. It is also possible to introduce gas into the preheating section via the inlet for the silicon dioxide granules of the preheating section. Gas can also be discharged via the outlet of the preheating section and subsequently separated from the silicon dioxide granules. Further preferably, gas can be supplied to the preheating section via the inlet for the silicon dioxide granules and a gas inlet, and discharged via the outlet of the preheating section and a gas outlet of the preheating section.
[0322] Preferably, a gas flow is formed in the preheating section by using the gas inlet and the gas outlet. Suitable gases are, for example, hydrogen, inert gases, and two or more thereof. Preferred inert gases are nitrogen, helium, neon, argon, krypton, and xenon, particularly preferably nitrogen and helium. Preferably, a reducing atmosphere is present in the preheating section. This can preferably be provided by hydrogen or a combination of hydrogen and an inert gas, for example by a combination of hydrogen and helium or of hydrogen and nitrogen, particularly preferably by a combination of hydrogen and helium. More preferably, an oxidizing atmosphere is present in the preheating section. This can preferably be provided by oxygen or a combination of oxygen and one or more other gases, particularly preferably air.It is further preferably possible to temper the silicon dioxide at reduced pressure in the preheating section.
[0323] For example, the silicon dioxide granules have a temperature in a range of 100 to 1100°C, or 300 to 1000°C, or 600 to 900°C upon entering the furnace. If silicon dioxide granules II are provided according to step i.), they preferably have a temperature in a range of 100 to 1100°C, or 300 to 1000°C, or 600 to 900°C upon entering the furnace.
[0324] The furnace preferably comprises at least two chambers. The furnace preferably comprises a first and at least one further chamber. The first and further chambers are connected to each other by a passage.
[0325] The at least two chambers can, in principle, be arranged in any desired manner in the furnace, preferably vertically or horizontally, particularly preferably vertically. Preferably, the chambers in the furnace are arranged such that, when carrying out the method according to the first aspect of the invention, silicon dioxide granules pass through the first chamber and are subsequently heated in the further chamber to obtain a glass melt. The further chamber preferably has the previously described features of the melting furnace and the crucible arranged therein.
[0326] Preferably, each of the chambers contains an inlet and an outlet. Preferably, the inlet of the furnace is connected to the inlet of the first chamber by a passage. Preferably, the outlet of the furnace is connected to the outlet of the further chamber by a passage. Preferably, the outlet of the first chamber is connected to the inlet of the further chamber by a passage.
[0327] Preferably, the chambers are arranged in the furnace such that the silicon dioxide granules can enter the first chamber through the furnace inlet. Preferably, the chambers are arranged in the furnace such that a silicon dioxide glass melt can be removed from the further chamber through the furnace outlet. Particularly preferably, the silicon dioxide granules can enter the first chamber through the furnace inlet, and a silicon dioxide glass melt can be removed from a further chamber through the furnace outlet.
[0328] The silicon dioxide can pass through the passage as granules or powder from a first chamber into a further chamber in the direction of material transport specified by the process. Chambers connected by a passage include arrangements in which further intermediate elements are arranged between a first and a further chamber in the direction of material transport. In principle, gases, liquids and solids can pass through the passage. Silicon dioxide powder, slurries of silicon dioxide powder and silicon dioxide granules can preferably pass through the transition between a first and a further chamber. During implementation of the process according to the invention, all substances introduced into the first chamber can pass into the further chamber via the passage between the first and the further chamber.Preferably, only silicon dioxide in the form of granules or powder enters the further chamber via the passage between the first and further chambers. Preferably, the passage between the first and further chambers is sealed by the silicon dioxide, so that the gas spaces of the first and further chambers are separated from each other, preferably such that different gases or gas mixtures, different pressures, or both can be present in the gas spaces. According to another preferred embodiment, the passage is formed by a lock, preferably a rotary valve.
[0329] The first chamber of the furnace preferably has at least one gas inlet and at least one gas outlet. The gas inlet can, in principle, have any shape known to those skilled in the art and suitable for introducing a gas, for example, a nozzle, a valve, or a pipe. The gas outlet can, in principle, have any shape known to those skilled in the art and suitable for discharging a gas, for example, a nozzle, a valve, or a pipe.
[0330] Preferably, silicon dioxide granules are introduced into the first chamber through the inlet of the furnace and heated. The heating can be carried out in the presence of a gas or a combination of two or more gases. For this purpose, the gas or the combination of two or more gases is present in the gas space of the first chamber. The gas space of the first chamber is understood to be the area of the first chamber that is not occupied by a solid or liquid phase. Suitable gases include, for example, hydrogen, oxygen, inert gases, and two or more thereof. Preferred inert gases are nitrogen, helium, neon, argon, krypton, and xenon; more preferably, nitrogen, helium, and a combination thereof. Heating is preferably carried out in a reducing atmosphere. This can preferably be provided by hydrogen or a combination of hydrogen and helium.Preferably, the silicon dioxide granules are heated in the first chamber in a stream of the gas or the combination of two or more gases.
[0331] It is further preferred that the silicon dioxide granules in the first chamber are heated at reduced pressure, for example at a pressure of less than 500 mbar or less than 300 mbar, for example 200 mbar or less.
[0332] Preferably, the first chamber is provided with at least one device for moving the silicon dioxide granules. In principle, any device known to the person skilled in the art and deemed suitable for this purpose can be selected. Stirring, shaking, or swiveling devices are preferred.
[0333] The temperatures in the first and further chambers are preferably different. The temperature in the first chamber is preferably lower than the temperature in the further chamber. The temperature difference between the first and further chambers is preferably in a range from 600 to 2400°C, for example in a range from 1000 to 2000°C or from 1200 to 1800°C, particularly preferably in a range from 1500 to 1700°C. Further preferably, the temperature in the first chamber is 600 to 2400°C, for example 1000 to 2000°C or 1200 to 1800°C, particularly preferably 1500 to 1700°C lower than the temperature in the further chamber.
[0334] Preferably, the first chamber of the furnace is a preheating section, particularly preferably a preheating section as described above, which has the features described above. Preferably, the preheating section is connected to the further chamber by a passage. Silicon dioxide preferably passes from the preheating section into the further chamber via a passage. The passage between the preheating section and the further chamber can be closed so that no gases introduced into the preheating section pass through the passage into the further chamber. Preferably, the passage between the preheating section and the further chamber is closed so that the silicon dioxide does not come into contact with water.The passage between the preheating section and the further chamber can be closed, so that the gas space of the preheating section and the first chamber are separated from each other in such a way that different gases or gas mixtures, different pressures, or both can be present in the gas spaces. The previously described configurations are preferably suitable as the passage.
[0335] Preferably, the first chamber of the furnace is not a preheating section. For example, the first chamber is an equalization chamber. A compensation chamber is understood to be a chamber of the furnace in which throughput variations in an upstream preheating section or throughput differences between a preheating section and the further chamber are compensated. For example, a rotary kiln can be arranged upstream of the first chamber as described above. This typically has a throughput that can vary by up to 6% of the average throughput. Preferably, silicon dioxide is kept in an equalization chamber at the temperature at which it enters the equalization chamber.
[0336] It is also possible for the furnace to have a first chamber and more than one further chamber, for example, two further chambers, three further chambers, four further chambers, five further chambers, or more than five further chambers, particularly preferably two further chambers. If the furnace has two further chambers, the first chamber is preferably a preheating section, the first of the further chambers is an equalization chamber, and the second of the further chambers is the melting chamber, based on the direction of material transport.
[0337] Preferably, an additive is present in the first chamber. The additive is preferably selected from the group consisting of halogens, inert gases, bases, oxygen, or a combination of two or more thereof.
[0338] In principle, suitable additives are halogens in elemental form and halogen compounds. Preferred halogens are selected from the group consisting of chlorine, fluorine, chlorine-containing compounds, and fluorine-containing compounds. Elemental chlorine and hydrogen chloride are particularly preferred.
[0339] In principle, all inert gases and mixtures of two or more of them are suitable as additives. Preferred inert gases are nitrogen, helium, or a combination thereof.
[0340] In principle, bases are also suitable as additives. Preferred bases are inorganic and organic bases.
[0341] Oxygen is also suitable as an additive. The oxygen is preferably present as an oxygen-containing atmosphere, for example in combination with an inert gas or a mixture of two or more inert gases, particularly preferably in combination with nitrogen, helium, or nitrogen and helium.
[0342] The first chamber can, in principle, contain any material known to those skilled in the art and suitable for heating silicon dioxide. Preferably, the first chamber contains at least one element selected from the group consisting of quartz glass, a refractory metal, aluminum, and a combination of two or more thereof. Particularly preferably, the first chamber contains quartz glass or aluminum.
[0343] Preferably, the temperature in the first chamber does not exceed 600°C if the first chamber contains a polymer or aluminum. Preferably, the temperature in the first chamber is 100 to 1100°C if the first chamber contains quartz glass. Preferably, the first chamber essentially contains quartz glass.
[0344] During transport of the silicon dioxide from the first chamber to the second chamber through the passage between the first and second chambers, the silicon dioxide can, in principle, be in any desired state. Preferably, the silicon dioxide is present as a solid, for example, as particles, powder, or granules. According to a preferred embodiment of the first aspect of the invention, the silicon dioxide is transported from the first to the second chamber as granules.
[0345] Preferably, the further chamber is a crucible made of a sheet or a sintered material containing a sintered metal, wherein the sheet or the sintered metal is selected from the group consisting of molybdenum, tungsten and a combination thereof.
[0346] The glass melt is removed from the furnace through the outlet, preferably via a nozzle. Step iii.)
[0347] A quartz glass body can be formed from at least a portion of the glass melt. Preferably, at least a portion of the glass melt produced in step ii) is removed and the quartz glass body is formed from it.
[0348] The removal of a portion of the glass melt produced in step ii) can, in principle, take place continuously from the melting furnace or the melting chamber, or after the glass melt has been produced. Preferably, a portion of the glass melt is removed continuously. The glass melt is removed through the outlet from the furnace or the outlet of the melting chamber, in each case preferably via a nozzle.
[0349] The glass melt can be cooled before, during, or after removal to a temperature that allows it to be shaped. Cooling of the glass melt is associated with an increase in its viscosity. The glass melt is preferably cooled to such an extent that the formed shape is retained during molding and, at the same time, molding can be carried out as quickly, reliably, and with minimal effort as possible. A person skilled in the art can easily determine the viscosity of the glass melt for molding by varying the temperature of the glass melt at the molding tool. The glass melt preferably has a temperature in the range of 1750 to 2100°C during removal, for example 1850 to 2050°C, particularly preferably 1900 to 2000°C.Preferably, after removal, the glass melt is cooled to a temperature of less than 500°C, for example less than 200°C or less than 100°C or less than 50°C, particularly preferably to a temperature in the range of 20 to 30°C.
[0350] The quartz glass body formed can be a solid body or a hollow body. A solid body is understood to be a body which essentially consists of a single material. However, a solid body can have one or more inclusions, e.g. gas bubbles. Such inclusions in a solid body often have a size of 65 mm 3< or less, for example less than 40 mm 3< , or less than 20 mm 3< , or less than 5 mm 3< , or less than 2 mm 3< , particularly preferably less than 0.5 mm 3< . A solid body preferably contains less than 0.02 vol.% of its volume, for example less than 0.01 vol.% or less than 0.001 vol.% of inclusions, in each case based on the total volume of the solid body.
[0351] The quartz glass body has an external shape. The external shape refers to the shape of the outer edge of the cross-section of the quartz glass body. The external shape of the quartz glass body is preferably round, elliptical, or polygonal in cross-section with three or more corners, for example, 4, 5, 6, 7, or 8 corners. The quartz glass body is particularly preferably round.
[0352] The quartz glass body preferably has a length in the range from 100 to 10,000 mm, for example from 1,000 to 4,000 mm, particularly preferably from 1,200 to 3,000 mm.
[0353] The quartz glass body preferably has an outer diameter in the range of 1 to 500 mm, for example in a range of 2 to 400 mm, particularly preferably in a range of 5 to 300 mm.
[0354] The quartz glass body is formed using a nozzle. The molten glass is guided through the nozzle. The external shape of a quartz glass body formed by the nozzle is determined by the shape of the nozzle opening. If the nozzle opening is round, a cylinder is formed during the formation of the quartz glass body. If the nozzle opening has a structure, this structure is transferred to the external shape of the quartz glass body. A quartz glass body formed using a nozzle with structures at the opening has an image of the structures in the longitudinal direction on the glass strand.
[0355] The nozzle is integrated into the melting furnace. It is preferably integrated into the melting furnace as part of the crucible, particularly preferably as part of the crucible outlet.
[0356] Preferably, at least a portion of the glass melt is removed through the nozzle. The outer shape of the quartz glass body is formed by removing at least a portion of the glass melt through the nozzle.
[0357] Preferably, the quartz glass body is cooled after forming to retain its shape. Preferably, the quartz glass body is cooled after forming to a temperature that is at least 1000°C below the temperature of the glass melt during forming, for example, at least 1500°C or at least 1800°C, particularly preferably 1900 to 1950°C. Preferably, the quartz glass body is cooled to a temperature of less than 500°C, for example, less than 200°C, less than 100°C, or less than 50°C, particularly preferably to a temperature in the range of 20 to 30°C.
[0358] Preferably, the resulting quartz glass body can be treated with at least one measure selected from the group consisting of chemical, thermal or mechanical treatment.
[0359] Preferably, the quartz glass body is chemically post-treated. Post-treatment refers to the treatment of an already formed quartz glass body. Chemical post-treatment of the quartz glass body is understood to mean, in principle, any measure known to the person skilled in the art and deemed suitable for changing the chemical structure or composition of the surface of the quartz glass body, or both, through the use of substances. The chemical post-treatment preferably comprises at least one measure selected from the group consisting of treatment with fluorine compounds and ultrasonic cleaning.
[0360] Particularly suitable fluorine compounds are hydrogen fluoride and fluorine-containing acids, for example, hydrofluoric acid. The liquid preferably has a fluorine compound content in a range of 35 to 55 wt.%, preferably in a range of 35 to 45 wt.%, the wt.% in each case based on the total amount of liquid. The remainder to 100 wt.% is usually water. Demineralized or deionized water is preferably selected as the water.
[0361] Ultrasonic cleaning is preferably carried out in a liquid bath, particularly preferably in the presence of detergents. In ultrasonic cleaning, fluorine compounds, such as hydrofluoric acid and hydrogen fluoride, are generally not used.
[0362] The ultrasonic cleaning of the quartz glass body is preferably carried out under at least one, for example at least two or at least three or at least four or at least five, particularly preferably all of the following conditions: Ultrasonic cleaning is carried out in a continuous process. The ultrasonic cleaning system has six chambers connected to one another by pipes. The residence time of the quartz glass bodies in each chamber can be adjusted. Preferably, the residence time of the quartz glass bodies in each chamber is the same. The residence time in each chamber is preferably in a range of 1 to 120 minutes, for example from less than 5 minutes, or from 1 to 5 minutes, or from 2 to 4 minutes, or from less than 60 minutes, or from 10 to 60 minutes, or from 20 to 50 minutes, particularly preferably in a range of 5 to 60 minutes. The first chamber comprises a basic medium, preferably containing water and a base, and an ultrasonic cleaner. The third chamber comprises an acidic medium, preferably containing water and an acid, and an ultrasonic cleaner. In the second chamber and in the fourth to sixth chambers, the quartz glass body is cleaned with water, preferably demineralized water.The fourth to sixth chambers are operated as a cascade with water, preferably demineralized water. Preferably, the water is introduced only into the sixth chamber and flows from the sixth to the fifth and from the fifth to the fourth chamber.
[0363] Preferably, the quartz glass body is thermally post-treated. Thermal post-treatment of the quartz glass body is understood to mean, in principle, any measure known to the person skilled in the art and deemed suitable for changing the shape or structure of the quartz glass body, or both, through the action of temperature. The thermal post-treatment preferably comprises at least one measure selected from the group consisting of annealing, compressing, blowing, drawing, welding, and a combination of two or more thereof. The thermal post-treatment is preferably carried out without the aim of removing material.
[0364] Annealing is preferably carried out by heating the quartz glass body in a furnace, preferably to a temperature in a range from 900 to 1300°C, for example in a range from 900 to 1250°C or from 1040 to 1300°C, particularly preferably in a range from 1000 to 1050°C or from 1200 to 1300°C. During the thermal treatment, a temperature of 1300°C is preferably not exceeded for a continuous period of more than 1 hour, and a temperature of 1300°C is particularly preferably not exceeded during the entire thermal treatment period. In principle, annealing can be carried out under reduced pressure, at atmospheric pressure, or at elevated pressure, preferably under reduced pressure, particularly preferably in a vacuum.
[0365] Upsetting is preferably carried out by heating the quartz glass body, preferably to a temperature of approximately 2100°C, and then forming it during a rotating motion, preferably at a rotational speed of approximately 60 rpm. For example, a quartz glass body in the form of a rod can be formed into a cylinder by upsetting.
[0366] Preferably, a quartz glass body can be inflated by blowing a gas into it. For example, a quartz glass body can be formed into a large tube by inflating it. For this purpose, the quartz glass body is preferably heated, preferably to a temperature of approximately 2100°C, while rotating, preferably at a speed of approximately 60 rpm, and the interior is flushed with a gas, preferably at a defined and controlled internal pressure of up to approximately 100 mbar. A large tube is understood to be a tube with an outer diameter of at least 500 mm.
[0367] A quartz glass body can preferably be drawn. Drawing is preferably carried out by heating the quartz glass body, preferably to a temperature of approximately 2100°C, and then drawing it at a controlled drawing speed to the desired outer diameter of the quartz glass body. For example, lamp tubes can be formed from quartz glass bodies by drawing.
[0368] Preferably, the quartz glass body is mechanically post-treated. Mechanical post-treatment of the quartz glass body is understood to mean, in principle, any measure known to the person skilled in the art and deemed suitable for changing the shape of the quartz glass body or dividing the quartz glass body into several pieces through an abrasive measure. In particular, mechanical post-treatment includes at least one measure selected from the group consisting of grinding, drilling, honing, sawing, waterjet cutting, laser cutting, roughening by sandblasting, milling, and a combination of two or more thereof.
[0369] Preferably, the quartz glass body is treated with a combination of these measures, for example, with a combination of chemical and thermal post-treatment, or chemical and mechanical post-treatment, or thermal and mechanical post-treatment, particularly preferably with a combination of chemical, thermal, and mechanical post-treatment. Furthermore, the quartz glass body can be subjected to several of the aforementioned measures independently of one another.
[0370] Preferably, the method may also include the following method step: iv.) Forming a hollow body with at least one opening from the quartz glass body.
[0371] The resulting hollow body has an inner and an outer shape. The inner shape refers to the shape of the inner edge of the hollow body in cross-section. The inner and outer shapes of the hollow body's cross-section can be the same or different. The inner and outer shapes of the hollow body can be round, elliptical, or polygonal in cross-section with three or more corners, for example, 4, 5, 6, 7, or 8 corners.
[0372] Preferably, the outer shape of the cross section corresponds to the inner shape of the cross section of the hollow body. Particularly preferably, the hollow body has a round inner and a round outer cross section.
[0373] In another embodiment, the hollow body can differ in its inner and outer shape. Preferably, the hollow body has a round outer shape and a polygonal inner shape in cross-section. Particularly preferably, the hollow body has a round outer shape and a hexagonal inner shape in cross-section.
[0374] The hollow body preferably has a length in the range from 100 to 10,000 mm, for example from 1,000 to 4,000 mm, particularly preferably from 1,200 to 2,000 mm.
[0375] Preferably, the hollow body has a wall thickness in a range of 0.8 to 50 mm, for example in a range of 1 to 40 mm or 2 to 30 mm or 3 to 20 mm, particularly preferably in a range of 4 to 10 mm.
[0376] The hollow body preferably has an outer diameter of 2.6 to 400 mm, for example in a range of 3.5 to 450 mm, particularly preferably in a range of 5 to 300 mm.
[0377] The hollow body preferably has an inner diameter of 1 to 300 mm, for example in a range of 5 to 280 mm or 10 to 200 mm, particularly preferably in a range of 20 to 100 mm.
[0378] The hollow body contains one or more openings. Preferably, the hollow body contains one opening. Preferably, the hollow body contains an even number of openings, for example 2, 4, 6, 8, 10, 12, 14, 16, 18, or 20 openings. Preferably, the hollow body contains two openings. Preferably, the hollow body is a tube. This shape of the hollow body is particularly preferred when the light guide contains only one core. The hollow body can contain more than two openings. The openings are preferably located in pairs opposite one another in the ends of the quartz glass body. For example, each end of the quartz glass body has 2, 3, 4, 5, 6, 7, or more than 7 openings, particularly preferably 5, 6, or 7 openings. Preferred shapes are, for example, tubes, twin tubes, i.e. tubes with two parallel channels, and multi-channel rods, i.e. tubes with more than two parallel channels.
[0379] In principle, the hollow body can be formed by any method known to those skilled in the art. The hollow body is preferably formed using a nozzle. The nozzle preferably contains a device in the center of its opening that diverts the molten glass during molding. This allows a hollow body to be formed from molten glass.
[0380] A hollow body can be formed using a nozzle followed by post-treatment. In principle, any method known to those skilled in the art for producing a hollow body from a solid body is suitable for post-treatment, for example, upsetting channels, drilling, honing, or grinding. A preferred post-treatment is passing the solid body over one or more mandrels, thereby forming a hollow body. Likewise, the mandrel can be inserted into the solid body to form a hollow body. The hollow body is preferably cooled after forming.
[0381] Preferably, after forming, the hollow body is cooled to a temperature of less than 500°C, for example less than 200°C or less than 100°C or less than 50°C, particularly preferably to a temperature in the range of 20 to 30°C. Pre-compaction
[0382] In principle, it is possible to subject the silicon dioxide granules prepared in step i.) to one or more pretreatment steps before heating them in step ii.) until a glass melt is obtained. Pretreatment steps can include thermal or mechanical treatment steps. For example, the silicon dioxide granules are compacted before heating in step ii.). "Compaction" refers to a reduction in the BET surface area and a reduction in the pore volume.
[0383] The silicon dioxide granules are preferably densified thermally by heating the silicon dioxide granules or mechanically by applying pressure to the silicon dioxide granules, for example, by rolling or pressing the silicon dioxide granules. The silicon dioxide granules are preferably densified by heating. Particularly preferably, the densification of the silicon dioxide granules takes place by heating using a preheating section connected to the melting furnace.
[0384] Preferably, the silicon dioxide is densified by heating at a temperature in a range of 800 to 1400°C, for example at a temperature in a range of 850 to 1300°C, particularly preferably at a temperature in a range of 900 to 1200°C.
[0385] The BET surface area of the silicon dioxide granules cannot be reduced to less than 5 m 2 / g before heating in step ii.), preferably not to less than 7 m 2 / g or not to less than 10 m 2 / g, particularly preferably not to less than 15 m 2 / g. It is further preferred that the BET surface area of the silicon dioxide granules before heating in step ii.) is not reduced compared to the silicon dioxide granules provided in step i.).
[0386] Preferably, the BET surface area of the silicon dioxide granules is reduced to less than 20 m 2 / g, for example to less than 15 m 2 / g, or to less than 10 m 2 / g, or to a range from more than 5 to less than 20 m 2 / g or from 7 to 15 m 2 / g, particularly preferably to a range from 9 to 12 m 2 / g. Preferably, the BET surface area of the silicon dioxide granules before heating in step ii.) is reduced by less than 40 m 2 / g compared to the silicon dioxide granules provided in step i.), for example by 1 to 20 m 2 / g or by 2 to 10 m 2 / g, particularly preferably by 3 to 8 m 2 / g, the BET surface area after compaction being more than 5 m 2 / g.
[0387] The compacted silicon dioxide granulate is referred to below as silicon dioxide granulate III. Preferably, silicon dioxide granulate III has at least one, for example at least two or at least three or at least four, particularly preferably at least five of the following features: A. a BET surface area in a range from more than 5 to less than 40 m 2 / g, for example from 10 to 30 m 2 / g, particularly preferably in a range from 15 to 25 m 2 / g; B. a particle size D 10 in a range from 100 to 300 µm, particularly preferably in a range from 120 to 200 µm; C. a particle size D 50 in a range from 150 to 550 µm, particularly preferably in a range from 200 to 350 µm; D. a particle size D 90 in a range from 300 to 650 µm, particularly preferably in a range from 400 to 500 µm; E. a bulk density in a range of 0.8 to 1.6 g / cm 3 , particularly preferably from 1.0 to 1.4 g / cm 3 ; F. a tapped density in a range of 1.0 to 1.4 g / cm 3 , particularly preferably from 1.15 to 1.35 g / cm 3 ; G. an amount of carbon of less than 5 ppm, for example less than 4.5 ppm, particularly preferably less than 4 ppm; H. a Cl content of less than 500 ppm, particularly preferably from 1 ppb to 200 ppm, where the ppm and ppb are each based on the total weight of the silicon dioxide granules III.
[0388] The silicon dioxide granulate III preferably has the feature combination A. / F. / G. or A. / F. / H. or A. / G. / H., particularly preferably the feature combination A. / F. / G. / H.
[0389] The silicon dioxide granulate III preferably has the feature combination A. / F. / G., wherein the BET surface area is in a range of 10 to 30 m 2 / g, the tamped density is in a range of 1.15 to 1.35 g / mL and the carbon content is less than 4 ppm.
[0390] The silicon dioxide granulate III preferably has the feature combination A. / F. / H., wherein the BET surface area is in a range of 10 to 30 m 2 / g, the tamped density is in a range of 1.15 to 1.35 g / mL and the chlorine content is in a range of 1 ppb to 200 ppm.
[0391] The silicon dioxide granulate III preferably has the feature combination A. / G. / H., wherein the BET surface area is in a range of 10 to 30 m 2 / g, the carbon content is less than 4 ppm and the chlorine content is in a range of 1 ppb to 200 ppm.
[0392] The silicon dioxide granulate III preferably has the feature combination A. / F. / G. / H., wherein the BET surface area is in a range of 10 to 30 m 2 / g, the tamped density is in a range of 1.15 to 1.35 g / mL, the carbon content is less than 4 ppm and the chlorine content is in a range of 1 ppb to 200 ppm.
[0393] In at least one process step, a silicon component other than silicon dioxide can be added. The addition of a silicon component other than silicon dioxide is also referred to below as Si doping. In principle, Si doping can occur in any process step. Si doping preferably occurs in step i.) or step ii.).
[0394] The silicon component other than silicon dioxide can, in principle, be added in any form, for example, as a solid, as a liquid, as a gas, in solution, or as a dispersion. Preferably, the silicon component other than silicon dioxide is added as a powder. Likewise, the silicon component other than silicon dioxide is added as a liquid or as a gas.
[0395] The silicon component other than silicon dioxide is preferably added in an amount in a range of 1 to 100,000 ppm, for example in a range of 10 to 10,000 ppm or 30 to 1,000 ppm or in a range of 50 to 500 ppm, particularly preferably in a range of 80 to 200 ppm, further particularly preferably in a range of 200 to 300 ppm, in each case based on the total weight of silicon dioxide.
[0396] The silicon component other than silicon dioxide can be solid, liquid, or gaseous. If solid, it preferably has an average particle size of up to 10 mm, for example up to 1000 µm, up to 400 µm, or in a range from 1 to 400 µm, for example 2 to 200 µm or 3 to 100 µm, particularly preferably in a range from 5 to 50 µm. The particle size specifications are based on the state of the silicon component other than silicon dioxide at room temperature.
[0397] The silicon component preferably has a purity of at least 99.5 wt.%, for example, at least 99.8 wt.% or at least 99.9 wt.%, or at least 99.99 wt.%, particularly preferably at least 99.999 wt.%, in each case based on the total weight of the silicon component. The silicon component preferably has a carbon content of no more than 10 ppm, for example, no more than 50 ppm, particularly preferably no more than 1 ppm, in each case based on the total weight of the silicon component. This particularly preferably applies to silicon used as a silicon component. Preferably, the silicon component has an amount of impurities selected from the group consisting of Al, Ca, Co, Cr, Cu, Fe, Ge, Hf, K, Li, Mg, Mn, Mo, Na, Nb, Ni, Ti, V, W, Zn, Zr of not more than 250 ppm, for example not more than 150 ppm, particularly preferably not more than 100 ppm, in each case based on the total weight of the silicon component.This particularly applies to silicon used as a silicon component.
[0398] Preferably, a silicon component other than silicon dioxide is added in process step i.). The silicon component other than silicon dioxide is preferably added during the processing of the silicon dioxide powder into silicon dioxide granules (step II.). For example, the silicon component other than silicon dioxide can be added to the silicon dioxide before, during, or after granulation.
[0399] Preferably, the silicon dioxide can be Si-doped by adding the silicon component other than silicon dioxide to the slurry containing silicon dioxide powder. For example, the silicon component other than silicon dioxide is mixed with silicon dioxide powder and then slurried in a liquid, or the silicon component other than silicon dioxide is added to a slurry of silicon dioxide powder in a liquid and slurried, or the silicon dioxide powder is added to a slurry or solution of the silicon component other than silicon dioxide in a liquid and slurried.
[0400] Preferably, the silicon dioxide can be Si-doped by adding the silicon component other than silicon dioxide during granulation. In principle, it is possible to add the silicon component other than silicon dioxide at any time during granulation. In the case of spray granulation, the silicon component other than silicon dioxide can, for example, be sprayed through the nozzle together with the slurry into the spray tower. In the case of roller granulation, the silicon component other than silicon dioxide can preferably be added in solid form or as a slurry, for example, after the slurry has been introduced into the stirred tank.
[0401] Further preferably, the silicon dioxide can be Si-doped by adding the silicon component other than silicon dioxide after granulation. For example, the silicon dioxide can be doped during the treatment of silicon dioxide granules I to form silicon dioxide granules II, preferably by adding the silicon component other than silicon dioxide during the thermal or mechanical treatment of silicon dioxide granules I.
[0402] Preferably, the silicon dioxide granulate II is doped with the silicon component other than silicon dioxide.
[0403] More preferably, the silicon component other than silicon dioxide can also be added during several of the aforementioned stages, in particular during and after the thermal or mechanical treatment of the silicon dioxide granulate I to form the silicon dioxide granulate II.
[0404] The silicon component other than silicon dioxide can, in principle, be silicon or any reducing silicon-containing compound known to those skilled in the art. Preferably, the silicon component other than silicon dioxide is silicon, a silicon-hydrogen compound, for example, a silane, a silicon-oxygen compound, for example, silicon monoxide, or a silicon-hydrogen-oxygen compound, for example, disiloxane. Examples of preferred silanes are monosilane, disilane, trisilane, tetrasilane, pentasilane, hexasilane, heptasilane, higher homologues and isomers of the aforementioned, as well as cyclic silanes such as isotrisilane or cyclopentasilane.
[0405] Preferably, in process step ii.) a silicon component other than silicon dioxide is added.
[0406] Preferably, the silicon component other than silicon dioxide can be added directly to the melting crucible together with the silicon dioxide granules. Preferably, silicon as the silicon component other than silicon dioxide can be added to the melting crucible together with the silicon dioxide granules. The silicon is preferably added as a powder, in particular in the particle size already mentioned for the silicon component other than silicon dioxide.
[0407] Preferably, the silicon component other than silicon dioxide is added to the silicon dioxide granules before they are introduced into the melting crucible. In principle, the addition can take place at any time after the granules have been formed, for example, in the preheating section, before or during the pre-compaction of silicon dioxide granules II, or to silicon dioxide granules III.
[0408] A silicon dioxide granulate obtained by adding a silicon component other than silicon dioxide is referred to below as "Si-doped granulate." The Si-doped granulate preferably has at least one, for example at least two or at least three or at least four, particularly preferably at least five, of the following features: [1] a BET surface area in a range from more than 5 to less than 40 m 2 < / g, for example from 10 to 30 m 2 < / g, particularly preferably in a range from 15 to 25 m 2 < / g; [2] a particle size D 10 in a range from 100 to 300 µm, particularly preferably in a range from 120 to 200 µm; [3] a particle size D 50 in a range from 150 to 550 µm, particularly preferably in a range from 200 to 350 µm; [4] a particle size D 90 in a range from 300 to 650 µm, particularly preferably in a range from 400 to 500 µm; [5] a bulk density in a range from 0.8 to 1.6 g / cm 3< , particularly preferably from 1.0 to 1.4 g / cm 3< ; [6] a tapped density in a range from 1.0 to 1.4 g / cm 3< , particularly preferably from 1.15 to 1.35 g / cm 3< ; [7] an amount of carbon of less than 5 ppm, for example less than 4.5 ppm, particularly preferably less than 4 ppm; [8] a Cl content of less than 500 ppm, particularly preferably from 1 ppb to 200 ppm;[9] an Al content of less than 200 ppb, particularly preferably from 1 ppb to 100 ppb;
[10] a metal content of metals other than aluminum of less than 1000 ppb, for example in a range from 1 to 400 ppb, particularly preferably in a range from 1 to 200 ppb;
[11] a residual moisture content of less than 3 wt.%, for example in a range from 0.001 wt.% to 2 wt.%, particularly preferably from 0.01 to 1 wt.%; ; where the wt%, ppm and ppb are each based on the total weight of the Si-doped granules.
[0409] The present invention relates to a silicon dioxide granulate, wherein the silicon dioxide granulate has the following features: A) a BET surface area in a range of 20 to 50 m 2 / g; B) a bulk density in a range of 0.5 to 1.2 g / cm 3 ; C) an average particle size in a range of 50 to 500 µm; D) a carbon content of less than 50 ppm; E) an aluminum content of less than 200 ppb; F) a tapped density in a range of 0.7 to 1.3 g / cm 3 ; G) a pore volume in a range of 0.1 to 2.5 mL / g; I) a particle size distribution D 10 in a range of 50 to 150 µm; J) a particle size distribution D 50 in a range of 150 to 300 µm; K) a particle size distribution D 90 in a range of 250 to 620 µm, where ppm and ppb are each based on the total weight of the silicon dioxide granules.
[0410] According to a preferred embodiment of the invention, the silicon dioxide granulate has the features described above in the general part. Features and properties considered preferred in this context are also preferred.
[0411] According to a preferred embodiment of the invention, the silicon dioxide granulate has the features of the previously described silicon dioxide granulate II. Embodiments described as preferred in this context are also preferred. Figures
[0412] Fig. 1 Flowchart (method for producing a quartz glass body) Fig. 2 Flowchart (Process for producing silicon dioxide granules I) Fig. 3 Flowchart (Process for producing silicon dioxide granules II) Fig. 4 Flowchart (method for manufacturing a light guide) Fig. 5 Flowchart (method for manufacturing a light source) Fig. 6schematic representation of a hanging crucible in a furnace Fig. 7 schematic representation of a standing crucible in a furnace Fig. 8 schematic representation of a crucible with a rinsing ring Fig. 9 schematic representation of a spray tower Fig. 10 schematic representation of a cross-section of a light guide Fig. 11 schematic representation of a top view of a light guide Fig. 12 schematic representation of a crucible with a dew point measuring device Fig. 13 schematic representation of a gas pressure sintering furnace (GDS furnace) Fig. 14 Flowchart (process for producing a molded body) Description of the characters
[0413] Figure 1shows a flowchart containing steps 101 to 104 of a method 100 for producing a quartz glass body according to the present invention. In a first step 101, silicon dioxide granules are provided. In a second step 102, a glass melt is formed from the silicon dioxide granules.
[0414] Preferably, molds that can be placed in and removed from a furnace are used for melting. Such molds are often made of graphite. They produce a negative mold of the casting. The silicon dioxide granules are poured into the mold and, in the third step 103, initially melted in the mold. Subsequently, the quartz glass body forms in the same mold as the melt cools. This is then removed from the mold and further processed, for example, in an optional step 104. This procedure is discontinuous. The melt is preferably formed under reduced pressure, particularly under vacuum. It is also possible to temporarily expose the furnace to a reducing, hydrogen-containing atmosphere during step 103.
[0415] In another procedure, hanging or standing crucibles are preferably used as melting crucibles. Melting preferably takes place in a reducing, hydrogen-containing atmosphere. In a third step 103, a quartz glass body is formed. The formation of the quartz glass body preferably takes place here by removing at least a portion of the molten glass from the crucible and cooling it. The removal preferably takes place through a nozzle at the lower end of the crucible. In this case, the shape of the quartz glass body can be determined by the design of the nozzle. For example, solid bodies can be obtained. Hollow bodies are obtained, for example, if a mandrel is additionally provided in the nozzle. This exemplary method for producing quartz glass bodies, and in particular step 103, preferably takes place continuously. A hollow body can be formed from a solid quartz glass body in an optional step 104.
[0416] Figure 2shows a flow diagram containing steps 201, 202, and 203 of a method 200 for producing silicon dioxide granules I. In a first step 201, a silicon dioxide powder is provided. A silicon dioxide powder is preferably obtained from a synthetic process in which a silicon-containing material, for example a siloxane, a silicon alkoxide, or a silicon halide, is converted to silicon dioxide in a pyrogenic process. In a second step 202, the silicon dioxide powder is mixed with a liquid, preferably with water, to obtain a slurry. In a third step 203, the silicon dioxide contained in the slurry is converted into silicon dioxide granules. Granulation is carried out by spray granulation.For this purpose, the slurry is sprayed through a nozzle into a spray tower and dried to form granules, whereby the contact surface between the nozzle and the slurry contains a glass or a plastic.
[0417] Figure 3 shows a flow chart containing the steps 301, 302, 303 and 304 of a method 300 for producing a silicon dioxide granulate II. The steps 301, 302 and 303 run according to the steps 201, 202 and 203 according to Figure 2 In step 304, the silicon dioxide granulate 1 obtained in step 303 is processed into silicon dioxide granulate II. This is preferably done by heating the silicon dioxide granulate I in a chlorine-containing atmosphere.
[0418] Figure 4shows a flowchart containing steps 401, 403, and 404, as well as the optional step 402, of a method for producing a light guide. In the first step 401, a quartz glass body is provided, preferably a quartz glass body produced according to method 100. Such a quartz glass body can be a solid or a hollow quartz glass body. In a second step 402, a hollow quartz glass body is formed from a solid quartz glass body provided in step 401, in accordance with step 104. In a third step 403, one or more core rods are introduced into the hollow quartz glass body. In a fourth step 404, the quartz glass body provided with one or more core rods is processed into a light guide. For this purpose, the quartz glass body provided with one or more core rods is preferably heated to soften it and elongated until the desired light guide thickness is achieved.
[0419] Figure 5shows a flowchart containing steps 501, 503, and 504, as well as optional step 502, of a method for producing a luminous means. In the first step 501, a quartz glass body is provided, preferably a quartz glass body produced according to method 100. Such a quartz glass body can be a solid or a hollow quartz glass body. If the quartz glass body provided in step 501 is solid, it is optionally formed into a hollow quartz glass body in a second step 502, corresponding to step 104. In an optional third step, the hollow quartz glass body is equipped with electrodes. In a fourth step 504, the hollow quartz glass body is filled with a gas, preferably with argon, krypton, xenon, or a combination thereof. Preferably, a solid quartz glass body is first provided (501), formed into a hollow body (502), equipped with electrodes (503), and filled with a gas (504).
[0420] In Figure 6A preferred embodiment of a furnace 800 with a suspended crucible is shown. The crucible 801 is arranged suspended in the furnace 800. The crucible 801 has a suspension 802 in its upper region, as well as a solids inlet 803 and a nozzle 804 as an outlet. The crucible 801 is filled with silicon dioxide granules 805 via the solids inlet 803. During operation, silicon dioxide granules 805 are present in the upper region of the crucible 801, while a glass melt 806 is present in the lower region of the crucible 801. The crucible 801 can be heated by heating elements 807 arranged on the outside of the crucible wall 810. The furnace also has an insulation layer 809 between the heating elements 807 and the furnace outer wall 808. The space between the insulation layer 809 and the crucible wall 810 can be filled with a gas and has a gas inlet 811 and a gas outlet 812 for this purpose. A quartz glass body 813 can be removed from the furnace through the nozzle 804.
[0421] In Figure 7 A preferred embodiment of a furnace 900 with a vertical crucible is shown. The crucible 901 is arranged vertically in the furnace 900. The crucible 901 has a base 902, a solids inlet 903, and a nozzle 904 as an outlet. The crucible 901 is filled with silicon dioxide granules 905 via the inlet 903. During operation, silicon dioxide granules 905 are present in the upper region of the crucible, while a glass melt 906 is present in the lower region of the crucible. The crucible can be heated by heating elements 907 arranged on the outside of the crucible wall 910. The furnace also has an insulating layer 909 between the heating elements 907 and the furnace outer wall 908. The space between the insulation layer 909 and the crucible wall 910 can be filled with a gas and has a gas inlet 911 and a gas outlet 912 for this purpose. A quartz glass body 913 can be removed from the crucible 901 through the nozzle 904.
[0422] In Figure 8A preferred embodiment of a crucible 1000 is shown. The crucible 1000 has a solids inlet 1001 and a nozzle 1002 as an outlet. The crucible 1000 is filled with silicon dioxide granules 1003 via the solids inlet 1001. During operation, silicon dioxide granules 1003 are present in the upper region of the crucible 1000 as a cone of material 1004, while a glass melt 1005 is present in the lower region of the crucible. The crucible 1000 can be filled with a gas. It has a gas inlet 1006 and a gas outlet 1007. The gas inlet is a purge ring attached to the crucible wall above the silicon dioxide granules. Through the purge ring (with a gas supply not shown here), the gas is released in the interior of the crucible just above the melt level and / or the cone of material near the crucible wall and flows towards the gas outlet 1007, which is arranged in a ring shape in the lid 1008 of the crucible 1000.The resulting gas stream 1010 moves along the crucible wall and floods it. A quartz glass body 1009 can be removed from the crucible 1000 through the nozzle 1002.
[0423] In Figure 9A preferred embodiment of a spray tower 1100 for spray granulating silicon dioxide is shown. The spray tower 1100 comprises a feed line 1101 through which a pressurized slurry containing silicon dioxide powder and a liquid is fed to the spray tower. At the end of the line is a nozzle 1102 through which the slurry is introduced into the spray tower in finely distributed form. The nozzle is preferably oriented obliquely upwards so that the slurry is sprayed into the spray tower as fine droplets in the direction of the nozzle alignment and then falls downwards in an arc driven by gravity. At the upper end of the spray tower is a gas inlet 1103. By introducing a gas through the gas inlet 1103, a gas flow is generated that is directed opposite to the exit direction of the slurry from the nozzle 1102. The spray tower 1100 also includes a viewing device 1104 and a screening device 1105.Particles below a defined particle size are suctioned off by the screening device 1104 and removed through the discharge 1106. The suction strength of the screening device 1104 can be adjusted according to the particle size of the particles to be suctioned off. Particles above a defined particle size are screened off by the screening device 1105 and removed through the discharge 1107. The permeability of the screening device 1105 can be selected according to the particle size of the particles to be screened off. The remaining particles, a silicon dioxide granulate of the desired particle size, are removed through the outlet 1108.
[0424] In Figure 10 is shown schematically a cross section through an optical fiber 1200 according to the invention, which has a core 1201 and a sheath M1 1202 surrounding the core 1201.
[0425] Figure 11shows a schematic plan view of a light guide 1300 having a cable-like structure. To illustrate the arrangement of the core 1301 and the sheath M1 1302 around the core 1301, a portion of the core 1301 was shown without the sheath M1 1302. However, it is typical for the core 1301 to be encased over its entire length with the sheath M1 1302.
[0426] Figure 12shows a preferred embodiment of a crucible 1400. The crucible has a solid inlet 1401 and an outlet 1402. During operation, silicon dioxide granules 1403 are present in a cone 1404 in the upper region of the crucible 1400, while a glass melt 1405 is present in the lower region of the crucible. The crucible 1400 has a gas inlet 1406 and a gas outlet 1407. The gas inlet 1406 and the gas outlet 1407 are arranged above the cone 1404 of the silicon dioxide granules 1403. The gas outlet 1406 comprises a line for gas guidance 1408 and a device 1409 for measuring the dew point of the escaping gas. The device 1409 comprises a dew point mirror hygrometer (not shown here). The distance between the crucible and the dew point measuring device 1409 can vary. A quartz glass body 1410 can be removed through the outlet 1402 of the crucible 1400.
[0427] Figure 13shows a preferred embodiment of a furnace 1500 suitable for a vacuum sintering process, a gas pressure sintering process, and in particular a combination thereof. The furnace comprises, from the outside to the inside, a pressure-resistant shell 1501 and a thermal insulation layer 1502. The space enclosed thereby, referred to as the furnace interior, can be supplied with a gas or gas mixture via a gas inlet 1504. Furthermore, the furnace interior is provided with a gas outlet 1505 through which gas can be removed. Depending on the balance of gas transport between the gas inlet 1504 and the gas outlet at 1505, an overpressure, a vacuum, or even a gas flow can be generated inside the furnace 1500. Furthermore, heating elements 1506 are provided inside the furnace 1500. These are often attached to the insulation layer 1502 (not shown here).To protect the melt from contamination, the interior of the furnace is provided with a so-called "liner" 1507, which separates the furnace chamber 1503 from the heating elements 1506. Melting molds 1508 containing melt 1509 can be placed into the furnace chamber 1503. The melting mold 1508 can be open on one side (shown here) or completely surround the melt 1509 (not shown).
[0428] Figure 14 shows a flowchart containing steps 1601 and 1602 of a method for producing a shaped body. In the first step 1601, a quartz glass body is provided, preferably a quartz glass body produced according to method 100. Such a quartz glass body can be a solid or a hollow quartz glass body. In a second step 1602, a shaped body is formed from a solid quartz glass body provided in step 1601. Test methods a. Fictitious temperature
[0429] The fictive temperature is determined by Raman spectroscopy based on the Raman scattering intensity at approximately 606 cm -1 . The procedure and analysis are described in the article by Pfleiderer et al., "The UV-induced 210 nm absorption band in fused silica with different thermal history and stoichiometry"; Journal of Non-Crystalline Solids, Volume 159 (1993), pages 145-153. b. OH content
[0430] The OH content of the glass is determined by infrared spectroscopy. The method described in "Optical Determinations of OH in Fused Silica" by DM Dodd & DM Fraser (JAP 37, 3991 (1966)) is used. Instead of the instrument specified therein, an FTIR spectrometer (Fourier transform infrared spectrometer, currently a System 2000 from Perkin Elmer) is used. The spectra can, in principle, be analyzed using either the absorption band at approximately 3670 cm -1 or the absorption band at approximately 7200 cm -1 . The band used is selected according to the rule that the transmission loss due to OH absorption is between 10 and 90%. c. Oxygen Deficiency Centers (ODCs)
[0431] For quantitative detection, the ODC(I) absorption at 165 nm is determined by means of a transmission measurement on a sample between 1-2 mm thick using a vacuum UV spectrometer, model VUVAS 2000, from McPherson, Inc. (USA).
[0432] Then the following applies: N = α / σ . with N = defect concentration [1 / cm 3< ] α = optical absorption [1 / cm, base e] of the ODC(I) band σ = cross section [cm 2< ] where the cross section is σ=7.5·10 -17 cm 2 is used (from L. Skuja, "Color Centers and Their Transformations in Glassy SiO2", Lectures of the summer school "Photosensitivity in optical Waveguides and glasses", July 13-18 1998, Vitznau, Switzerl and). d. Elemental analysis
[0433] d-1) Solid samples are crushed. For cleaning, approximately 20 g of the sample is placed in an HF-resistant vessel, completely covered with HF, and thermally treated at 100°C for one hour. After cooling, the acid is discarded and the sample is rinsed several times with ultrapure water. The vessel containing the sample is then dried in a drying cabinet.
[0434] Subsequently, approximately 2 g of the solid sample (broken material, cleaned as above; dust, etc., directly without pretreatment) is weighed into an HF-resistant digestion vessel and mixed with 15 ml of HF (50 wt.%). The digestion vessel is sealed and thermally treated at 100°C until the solid sample is completely dissolved. The digestion vessel is then opened and thermally treated further at 100°C until the solution has completely evaporated. During this time, the digestion vessel is filled three times with 15 ml of ultrapure water. 1 ml of HNO3 is added to the digestion vessel to dissolve any separated impurities and filled to 15 ml with ultrapure water. The measurement solution is then ready. d-2) Measurement ICP-MS / ICP-OES
[0435] Whether OES or MS is used depends on the expected element concentration. Typical limits of quantification for MS are 1 ppb, and for OES 10 ppb (each based on the weighed sample volume). The element concentration is determined using the measuring instruments according to the manufacturer's specifications (ICP-MS: Agilent 7500ce; ICP-OES: Perkin Elmer 7300 DV) and certified reference fluids for calibration. The element concentration in the solution (15 ml) determined by the instruments is then converted to the original sample weight (2 g).
[0436] Note: It is important to ensure that the acid, vessels, water, and equipment are of sufficient purity to determine the element concentrations to be detected. This is verified by digesting a blank sample without quartz glass.
[0437] The following elements are determined in this way: Li, Na, Mg, K, Ca, Fe, Ni, Cr, Hf, Zr, Ti, (Ta), V, Nb, W, Mo, Al. d-3) The determination of liquid samples is carried out as described above, but the sample preparation according to step d-1) is omitted. 15 ml of the liquid sample is added to the decomposition vessel. Conversion to the original weight is not necessary. e. Determination of the density of a liquid
[0438] To determine the density of a liquid, a precisely defined volume of the liquid is weighed into a measuring vessel that is inert to the liquid and its components, and the empty weight and the weight of the filled vessel are measured. The density is calculated by dividing the difference between the two weight measurements by the added volume of liquid. f. Detection of fluoride
[0439] 15g of a quartz glass sample is crushed and treated with nitric acid at a temperature of 70°C to clean it. The sample is then rinsed several times with ultrapure water and dried. 2g of the sample is weighed into a nickel crucible and covered with 10g Na2CO3 and 0.5g ZnO. The crucible is sealed with a nickel lid and annealed at 1000°C for one hour. The nickel crucible is then filled with water and boiled until the melt cake has completely dissolved. The solution is transferred to a 200ml volumetric flask and made up to 200ml with ultrapure water. After the undissolved components have settled, 30ml is removed and transferred to a 100ml volumetric flask, 0.75ml glacial acetic acid and 60ml TISAB are added and made up to the mark with ultrapure water. The measuring solution is transferred to a 150ml beaker.
[0440] The fluoride content of the sample solution is determined using an ion-sensitive (fluoride) electrode suitable for the expected concentration range and a display device according to the manufacturer's specifications. In this case, a fluoride ion-selective electrode and reference electrode F-500 with R503 / D on a pMX 3000 / pH / ION from Wissenschaftlich-Technische Werkstätten GmbH. The fluoride concentration in the quartz glass is calculated using the fluoride concentration in the solution, the dilution factor, and the sample weight. G. Detection of chlorine (>= 50 ppm)
[0441] A 15g sample of quartz glass is crushed and treated with nitric acid at approximately 70°C for cleaning. The sample is then rinsed several times with ultrapure water and dried. 2g of the sample is placed into a PTFE insert of a pressure vessel, mixed with 15mL of NaOH (c=10 mol / L), sealed with a PTFE lid, and placed in the pressure vessel. The vessel is sealed and thermally treated at approximately 155°C for 24 hours. After cooling, the PTFE insert is removed, and the solution is transferred completely into a 100mL volumetric flask. 10mL of HNO3 (65 wt%) and 15mL of acetate buffer are added, the flask is allowed to cool, and the volume is made up to 100mL with ultrapure water. The measurement solution is transferred to a 150mL beaker. The measurement solution has a pH value between 5 and 7.
[0442] The chloride content of the measuring solution is determined using an ion-sensitive (chloride) electrode, suitable for the expected concentration range, and a display device according to the manufacturer's specifications, here an electrode type Cl-500 and reference electrode type R-503 / D on a pMX 3000 / pH / ION from Wissenschaftlich-Technische Werkstätten GmbH. h. Chlorine content (< 50 ppm)
[0443] Chlorine levels < 50 ppm down to 0.1 ppm in quartz glass are determined using neutron activation analysis (NAA). For this purpose, three drill bits, each 3 mm in diameter and 1 cm long, are taken from the quartz glass body to be examined. These are then submitted to a research institute for analysis, in this case the Institute of Nuclear Chemistry at Johannes Gutenberg University in Mainz. To rule out chlorine contamination of the samples, an agreement is reached with the research institute to thoroughly clean the samples in an HF bath on site, but only immediately before measurement. Each drill bit is measured several times. The results and the drill bits are then returned by the research institute. i. Optical properties
[0444] The transmittance of fused silica samples is determined using commercial grating or FTIR spectrometers from Perkin Elmer (Lambda 900 [190-3000 nm] or System 2000 [1000-5000 nm]). The choice depends on the required measurement range.
[0445] To determine absolute transmittance, the specimens are polished to a plane-parallel plane (surface roughness RMS < 0.5 nm). After polishing, the surface is cleaned of all residues using ultrasonic treatment. The specimen thickness is 1 cm. If significant transmission loss due to contamination, doping, etc., is expected, a thicker or thinner specimen can be selected to remain within the measuring range of the device. A specimen thickness (gauge length) is selected at which only minimal artifacts occur due to the beam passing through the specimen, while still allowing a sufficiently detectable effect to be measured.
[0446] To measure opacity, the sample is placed in front of an Ulbrich sphere in the beam path. The opacity is calculated from the measured transmission value T according to the formula: O = 1 / T = I 0 / I. j. Refractive index and refractive index distribution on a tube or rod
[0447] The refractive index distribution of tubes / rods can be characterized using a York Technology Ltd. Preform Profiler P102 or P104. The rod is placed horizontally in the measuring chamber, which is then tightly sealed. The measuring chamber is then filled with an immersion oil that has a refractive index at the test wavelength of 633 nm that is very similar to the outermost glass layer at 633 nm. The laser beam then passes through the measuring chamber. A detector is mounted behind the measuring chamber (in the beam direction) to determine the deflection angle (beam entry into versus beam exit from the measuring chamber). Assuming radial symmetry of the refractive index distribution of the rod, the diametrical refractive index profile can be reconstructed using an inverse Abel transformation. These calculations are performed by software from the device manufacturer York.
[0448] The refractive index of a sample is determined using the York Technology Ltd. Preform Profiler P104, as described above. For isotropic samples, even measuring the refractive index distribution yields only one value: the refractive index. k. Carbon content
[0449] The quantitative determination of the surface carbon content of silicon dioxide granules and silicon dioxide powder is carried out using an RC612 carbon analyzer from Leco Corporation, USA, by completely oxidizing all surface carbon contamination (except SiC) with oxygen to carbon dioxide. For this purpose, 4.0 g of a sample is weighed and placed in a quartz glass boat in the carbon analyzer. The sample is flushed with pure oxygen and heated to 900 °C for 180 seconds. The CO2 formed is detected by the carbon analyzer's infrared detector. Under these measurement conditions, the detection limit is ≤ 1 ppm (ppm by weight) of carbon.
[0450] A quartz glass boat suitable for this analysis on the above-mentioned carbon analyzer is available as consumables for LECO analyzers with the LECO number 781-335 from laboratory supply stores, in this case from Deslis Laborhandel, Flurstraße 21, D-40235 Düsseldorf (Germany), Deslis No. LQ-130XL. Such a boat has the dimensions (width / length / height) of approximately 25 mm / 60 mm / 15 mm. The quartz glass boat is filled halfway with sample material. For silicon dioxide powder, a sample weight of 1.0 g can be achieved. The lower detection limit is then <1 ppm by weight of carbon. A sample weight of 4 g of silicon dioxide granules (average particle size in the range of 100 to 500 µm) is achieved in the same quartz glass boat at the same filling level. The lower detection limit is then about 0.1 ppm by weight of carbon.The lower detection limit is reached when the measuring area integral of the sample is not greater than three times the measuring area integral of a blank sample (blank sample = procedure as above, but with an empty quartz glass boat). 1. Curl parameters
[0451] The curl parameter (also called "fibre curl") is determined according to DIN EN 60793-1-34:2007-01 (German version of the IEC 60793-1-34:2006 standard). Measurements are carried out using the method described in Annex A, sections A.2.1, A.3.2, and A.4.1 ("extrema technique"). m. damping
[0452] Attenuation is determined according to DIN EN 60793-1-40:2001 (German version of IEC 60793-1-40:2001). Measurements are performed using the cut-back method described in the Annex at a wavelength of λ=1550 nm. n. Viscosity of the slurry
[0453] The slurry is adjusted to a concentration of 30 wt% solids with demineralized water (Direct-Q 3UV, Millipore, water quality: 18.2 MΩcm). The viscosity is then measured using an Anton-Paar MCR102. The viscosity is measured at 5 revolutions per minute (rpm). The measurement is carried out at a temperature of 23 °C and an air pressure of 1013 hPa. O. Thixotropy
[0454] The slurry is adjusted to a concentration of 30 wt% solids with demineralized water (Direct-Q 3UV, Millipore, water quality: 18.2 MΩcm). Thixotropy is then determined using an Anton-Paar MCR102 cone-and-plate tester. For this purpose, the viscosity is measured at 5 and 50 revolutions per minute (rpm). The quotient of the first and second values yields the thixotropy index. The measurement is performed at a temperature of 23 °C. p. Zeta potential of the slurry
[0455] A zeta potential flow cell (Beckman Coulter) is used for zeta potential measurements. The sample is dissolved in demineralized water (Direct-Q 3UV, Millipore, water quality: 18.2 MΩcm) to obtain a 20 mL solution with a concentration of 1 g / L. The pH is adjusted to 7 by adding HNO3 solutions with concentrations of 0.1 mol / L and 1 mol / L and a NaOH solution with a concentration of 0.1 mol / L. The measurement is carried out at a temperature of 23 °C. q. Isoelectric point of the slurry
[0456] A zeta potential cell (Flow Cell, Beckman Coulter) and an autotitrator (DelsaNano AT, Beckman Coulter) are used to determine the isoelectric point. The sample is dissolved in demineralized water (Direct-Q 3UV, Millipore, water quality: 18.2 MΩcm) to obtain a 20 mL solution with a concentration of 1 g / L. The pH is varied by adding HNO 3 solutions with concentrations of 0.1 mol / L and 1 mol / L and a NaOH solution with a concentration of 0.1 mol / L. The isoelectric point is the pH value at which the zeta potential is equal to 0. It is measured at a temperature of 23 °C. r. pH value of the slurry
[0457] The pH value of the slurry is measured using a WTW 3210 from Wissenschaftlich-Technische-Werkstätten GmbH. A pH 3210 Set 3 from WTW is used as the electrode. Measurements are taken at a temperature of 23 °C. see Solids content
[0458] A sample weight m 1 is heated to 500 °C for 4 hours and then reweighed (m 2 ) after cooling. The solids content w is determined from m 2 / m 1 * 100 [wt. %]. t. Bulk density
[0459] The bulk density is determined according to DIN ISO 697:1984-01 using an SMG 697 from Powtec. The bulk material (silicon dioxide powder or granules) does not form lumps. and Tapped density (granules)
[0460] The tamped density is measured according to DIN ISO 787:1995-10. v. Determination of pore size distribution
[0461] The pore size distribution is determined according to DIN 66133 (with a surface tension of 480 mN / m and a contact angle of 140°). The Pascal 400 from Porotec is used to measure pore sizes smaller than 3.7 nm. The Pascal 140 from Porotec is used to measure pore sizes from 3.7 nm to 100 µm. The sample is subjected to a pressure treatment prior to measurement. A manual hydraulic press (order no. 15011 from Specac Ltd., River House, 97 Cray Avenue, Orpington, Kent BR5 4HE, UK) is used for this purpose. 250 mg of sample material is weighed into a 13 mm inner diameter pellet die from Specac Ltd. and subjected to a load of 1 t according to the display. This load is held for 5 s and adjusted if necessary. The sample is then released and dried for 4 h at 105 ± 2°C in a circulating air drying cabinet.
[0462] The sample is weighed into the Type 10 penetrometer to the nearest 0.001 g. To ensure good measurement reproducibility, the "stem volume used"—the percentage of mercury volume used to fill the penetrometer—is between 20% and 40% of the total mercury volume. The penetrometer is then slowly evacuated to 50 µm Hg and held at this pressure for 5 minutes. The following parameters are directly displayed by the measuring instrument's software: total pore volume, total pore surface area (assuming cylindrical pores), average pore radius, modal pore radius (most common pore radius), and peak n. 2 pore radius (µm). w. Primary particle size
[0463] The primary particle size is measured using a Zeiss Ultra 55 scanning electron microscope (SEM). The sample is suspended in demineralized water (Direct-Q 3UV, Millipore, water quality: 18.2 MQcm) to obtain an extremely dilute suspension. The suspension is treated with an ultrasonic probe (UW 2070, Bandelin electronic, 70 W, 20 kHz) for 1 min and then applied to a carbon adhesive pad. x. Average particle size in suspension
[0464] The mean particle size in suspension is measured using a Mastersizer 2000, available from Malvern Instruments Ltd., UK, according to their operating instructions, using the laser diffraction method. The sample is suspended in demineralized water (Direct-Q 3UV, Millipore, water quality: 18.2 MΩcm) to obtain a 20 mL suspension with a concentration of 1 g / L. The suspension is treated with an ultrasonic probe (UW 2070, Bandelin electronic, 70 W, 20 kHz) for 1 min. y. Particle size and grain size of the solid
[0465] The particle size and grain size of the solid are measured using a Camsizer XT, available from Retsch Technology GmbH, Germany, according to the manufacturer's manual. The software outputs the D10, D50, and D90 values for a sample. e.g. BET measurement
[0466] The static volumetric BET method according to DIN ISO 9277:2010 is used to measure the specific surface area. A "NOVA 3000" or a "Quadrasorb" (available from Quantachrome), which operates according to the SMART method ("Sorption Method with Adaptive Dosing Rate"), is used for the BET measurement. Micropore analysis is performed using the t-plot method (p / p0 = 0.1-0.3), and mesopore analysis is performed using the MBET method (p / p0 = 0.0-0.3). Alumina standards SARM-13 and SARM-214, available from Quantachrome, are used as reference materials. The tare weight of the measuring cells used (clean and dry) is weighed. The measuring cell type is selected so that the sample material and the filler rod fill the measuring cell as much as possible, reducing dead space to a minimum. The sample material is placed in the measuring cell. The amount of sample material is selected so that the expected measured value corresponds to 10-20 m 2 / g.The measuring cells are fixed in the bake-out stations of the BET measuring device (without filler rod) and evacuated to <200 mbar. The evacuation rate is adjusted so that no material escapes from the measuring cell. In this state, it is baked out at 200°C for 1 hour. After cooling, the measuring cell filled with sample is weighed (gross). The tare weight is then subtracted from the gross weight = net weight = weight of the sample. The filler rod is then inserted into the measuring cell, which in turn is fixed in the measuring station of the BET measuring device. Before starting the measurement, the sample designation and sample weight are entered into the software. The measurement is started. The saturation pressure of the nitrogen gas (N2 4.0) is measured. The measuring cell is evacuated and cooled to 77 K using a nitrogen bath. The dead space is measured using helium gas (He 4.6). It is evacuated again. A multi-point analysis with at least 5 measuring points is carried out.N2 4.0 is used as an adsorptive. The specific surface area is given in m2 / g. za. Viscosity of vitreous bodies
[0467] The viscosity of the glass is measured using a Type 401 beam bending viscometer from TA Instruments with the manufacturer's software WinTA (current version 9.0) under Windows 10 in accordance with DIN ISO 7884-4:1998-02. The span between the supports is 45 mm. Sample bars with a rectangular cross-section are cut from areas of homogeneous material (the top and bottom of the sample are finely ground to a grain size of at least 1000). The sample surfaces after processing have a grain size of 9 µm and a grain size of 0.15 µm. The sample bars have the following dimensions: length = 50 mm, width = 5 mm, and height = 3 mm (length, width, and height are assigned as per the standard). Three samples are measured, and the average value is calculated. The sample temperature is measured using a thermocouple placed close to the sample surface. The following parameters are used: heating rate = 25 K to maximum 1500 °C, load weight = 100 g, maximum deflection = 3000 µm (deviating from the standard). e.g. Dew point measurement
[0468] The dew point is determined using a mirror dew point hygrometer called "Optidew" from Michell Instruments GmbH, D-61381 Friedrichsdorf. The measuring cell of the mirror dew point hygrometer is positioned 100 cm from the furnace's gas outlet. The measuring device and the measuring cell are connected to the furnace's gas outlet via a T-piece and a hose (Swagelok PFA, outer diameter: 6 mm). The measuring cell is subjected to an overpressure of 10±2 mbar. The gas flow through the measuring cell is 1-2 standard liters / min. The measuring cell is located in a room with a temperature of 25°C, 30% relative humidity, and an average air pressure of 1013 hPa. e.g. residual moisture
[0469] The residual moisture content of a sample of silicon dioxide granules is determined using a Mettler Toledo HX204 moisture analyzer. The instrument operates according to the principle of thermogravimetry. The HX204 is equipped with a halogen lamp as the heating element. The drying temperature is 220°C. The starting weight of the sample is 10 g ± 10%. The "Standard" measurement method is selected. Drying is continued until the weight change does not exceed 1 mg / 140 s. The residual moisture content is calculated as the difference between the starting weight of the sample and the final weight of the sample, divided by the starting weight of the sample.
[0470] The determination of the residual moisture content of silicon dioxide powder is carried out according to DIN EN ISO 787-2:1995 (2h, 105°C). Examples
[0471] The invention is further illustrated by examples below. The invention is not limited to the examples. A. 1. Production of silicon dioxide powder (OMCTS route)
[0472] The aerosol formed from the atomization of a siloxane with air (A) is introduced under pressure into a flame formed by igniting a mixture of oxygen-enriched air (B) and hydrogen. Furthermore, an air stream (C) surrounding the flame is introduced, and the process mixture is subsequently cooled with process gas. The product is separated on a filter. The process parameters are given in Table 1, and the characteristics of the resulting products are given in Table 2. Experimental data for this example are provided with A1-x marked. 2. Modification 1: Increased carbon content
[0473] The procedure was as described under A.1., but the combustion of the siloxane was carried out in such a way that a large amount of carbon was also formed. Experimental data for this example are provided with A2- x marked. Table 1 Example A1-1 A2-1 A2-2 Aerosol formation Siloxane OMCTS* OMCTS* OMCTS* supply kg / h (kmol / h) 10 (0,0337) 10 (0,0337) 10 (0,0337) Air supply (A) Nm3 / h 14 10 12 Pressure barÜ 1,2 1,2 1,2 Burner supply Oxygen-enriched air (B) Nm3 / h 69 65 68 O 2 content Vol.% 32 30 32 Total O 2 supply Nm 3 < / h 25,3 21,6 24,3 kmol / h 1,130 0,964 1,083 Hydrogen supply Nm3 / h 27 27 12 kmol / h 1,205 1,205 0,536 supply -- -- Carbon compound Material methane Crowd Nm 3 < / h 5,5 Air flow (C) Nm 3 < / h 60 60 60 Stoichiometric ratios V 2,099 1,789 2,011 X 0,938 0,80 2,023 Y 0,991 0,845 0,835 V = molar ratio of O 2 used / O 2 required for complete oxidation of the siloxane; X = molar ratio of O 2 / H 2 ; Y = (molar ratio of O 2 used / O 2 required for stoichiometric conversion of OMCTS + fuel gases); barg = overpressure; * OMCTS = octamethylcyclotetrasiloxane. Table 2 Example A1-1 A2-1 A2-2 BET m 2 < / g 30 33 34 Bulk density g / ml 0,114 +- 0,011 0,105 +- 0,011 0,103 +- 0,011 Tapped density g / ml 0,192 +- 0,015 0,178 +- 0,015 0,175 +- 0,015 Primary particle size nm 94 82 78 Particle size distribution D10 µm 3,978±0,380 5,137±0,520 4,973±0,455 Particle size distribution D50 µm 9,383±0,686 9,561±0,690 9,423±0,662 Particle size distribution D90 µm 25,622±1,387 17,362±0,921 18,722±1,218 C content ppm 34±4 73±6 80±6 Cl content ppm < 60 < 60 < 60 Al content ppb 20 20 20 Total content of metals except Al ppb < 700 < 700 < 700 residual moisture % by weight 0,02-1,0 0,02-1,0 0,02-1,0 pH value in water 4% (IEP) - 4,8 4,6 4,5 Viscosity at 5 rpm, aqueous suspension 30 wt%, 23 °C mPas 753 1262 1380 Alkaline earth metal content ppb 538 487 472 B. 1. Production of silicon dioxide powder (silicon source: SiCl 4 )
[0474] A quantity of silicon tetrachloride (SiCl 4 ) is vaporized at a temperature T and introduced at a pressure P into a burner flame formed by igniting a mixture of oxygen-enriched air and hydrogen. The mean normalized gas flow at the burner orifice is recorded. The process mixture is subsequently cooled with process gas. The product is separated on a filter. The process parameters are given in Table 3 and the characteristics of the resulting products in Table 4. They are B1-x marked. 2. Modification 1: Increased carbon content
[0475] The procedure was as described under B.1., but the combustion of the silicon tetrachloride was carried out in such a way that a large amount of carbon was also formed. Experimental data for this example are provided with B2-x marked. Table 3 Example B1-1 B2-1 Aerosol formation Supply of silicon tetrachloride kg / h (kmol) 50 (0,294) 50 (0,294) Temperature T °C 90 90 Pressure p barÜ 1,2 1,2 Burner supply Oxygen-enriched air, containing O 2 Nm 3 < / h 145 115 Vol.% 45 30 supply -- Carbon compound Material methane Crowd Nm 3 < / h 2,0 Hydrogen supply Nm 3 < / h 115 60 kmol / h 5,13 2,678 Stoichiometric ratios X 0,567 0,575 Y 0,946 0,85 X = molar ratio of O 2 / H 2 ; Y = mol. ratio of O 2 used / O 2 required for stoichiometric reaction with SiCl 4 + H 2 + CH 4 ); barg = overpressure. Table 4 Example B1-1 B2-1 BET m 2 < / g 49 47 Bulk density g / ml 0,07 ± 0,01 0,06±0,01 Tapped density g / ml 0,11 ± 0,01 0,10 ± 0,01 Primary particle size nm 48 43 Particle size distribution D10 µm 5,0±0,5 4,5±0,5 Particle size distribution D50 µm 9,3±0,6 8,7±0,6 Particle size distribution D90 µm 16,4±0,5 15,8±0,7 C content ppm <4 76 Cl content ppm 280 330 Al content ppb 20 20 Sum of the concentrations of Ca, Co, Cr, Cu, Fe, Ge, Hf, K, Li, Mg, Mn, Mo, Na, Nb, Ni, Ti, V, W, Zn, Zr ppb < 1300 < 1300 residual moisture % by weight 0,02-1,0 0,02-1,0 pH value in water 4% (IEP) pH 3,8 3,8 Viscosity at 5 rpm, aqueous suspension 30 wt%, 23 °C mPas 5653 6012 Alkaline earth metal content ppb 550 342 C. Steam treatment
[0476] A particle stream of silicon dioxide powder is introduced via the top of a vertical column. Steam at a temperature (A) and air are introduced via the base of the column. The column is maintained by an internal heater at a temperature (B) at the column head and a second temperature (C) at the column base. After leaving the column (residence time (D)), the silicon dioxide powder exhibits the properties shown in Table 6. The process parameters are given in Table 5. Table 5 Example C-1 C-2 Educt: Product of B1-1 B2-1 Feed reactant kg / h 100 100 Supply of steam kg / h 5 5 Water vapor temperature (A) °C 120 120 Air supply Nm 3 < / h 4,5 4,5 column Height m 2 2 inner diameter mm 600 600 T (B) °C 260 260 T (C) °C 425 425 Residence time (D) s 10 10 Silicon dioxide powder Table 6 Example C-1 C-2 pH value in water 4% (IEP) - 4,6 4,6 Cl content ppm < 60 < 60 C content ppm <4 36 Viscosity at 5 rpm, aqueous suspension 30 wt%, 23 °C mPas 1523 1478
[0477] The silicon dioxide powders obtained in Examples C-1 and C-2 each have a low chlorine content and a moderate pH in suspension. The carbon content of Example C-2 is higher than that of Example C-1. D. Treatment with neutralizing agent
[0478] A particle stream of silicon dioxide powder is introduced via the top of a vertical column. A neutralizing agent and air are introduced via the base of the column. The column is maintained by an internal heater at a temperature (B) at the column top and a second temperature (C) at the column base. After leaving the column (residence time (D)), the silicon dioxide powder exhibits the properties shown in Table 8. The process parameters are given in Table 7. Table 7 Example D-1 Educt: Product of B 1-1 Feed reactant kg / h 100 Neutralizing agent ammonia Supply of neutralizing agent kg / h 1,5 Characteristics of neutralizing agents Available from Air Liquide: Ammonia N38, purity ≥ 99.98 vol.% Air supply Nm 3 < / h 4,5 column Height m 2 inner diameter mm 600 T (B) °C 200 T (C) °C 250 Residence time (D) s 10 Silicon dioxide powder Table 8 Example D-1 pH value in water 4% (IEP) - 4,8 Cl content ppm 210 C content ppm < 4 Viscosity at 5 rpm, aqueous suspension 30 wt%, 23 °C mPas 821 E. 1. Production of silicon dioxide granules from silicon dioxide powder
[0479] A silicon dioxide powder is dispersed in demineralized water. A Type R intensive mixer from Maschinenfabrik Gustav Eirich is used. The resulting suspension is conveyed by a diaphragm pump, pressurized, and formed into droplets through a nozzle. These droplets are dried in a spray tower and collect at the bottom. The process parameters are listed in Table 9, and the properties of the resulting granules are listed in Table 10. Experimental data for this example are provided with E1-x Furthermore, Table 10 (continued) shows the properties of Examples E14-2 to E14-4. These are samples that are not derived from an Example A or B. These samples were also not granulated as in Example E. 2. Modification 1: Increased carbon content
[0480] The procedure is analogous to description E.1. In addition, carbon powder is dispersed into the suspension. Experimental data for this example are provided with E2-x marked. 3. Modification 2: Addition of silicon
[0481] The procedure is analogous to description E.1. In addition, a silicon component is dispersed into the suspension. Experimental data for this example are provided with E3-1 marked. Table 9 Example E 1-1 E 1-2 E 1-3 E1-4 E1-5 E2-1 E3-1 E3-2 Educt = product of A1-1 A2-1 B1-1 C-1 C-2 A1-1 A1-1 A2-1 Amount of reactant kg 10 10 10 10 10 10 10 10 Carbon powder -- -- -- -- -- -- -- material C** Max. particle size 75 µm Crowd 1 g Silicon component -- -- -- -- -- -- Siliziu mpulv er*** -- Material Grain size (d50) 8 µm Crowd 1000 ppm Carbon content 0.5 ppm Sum of the concentrations of Ca, Co, Cr, Cu, Fe, Ge, Hf, K, Li, Mg, Mn, Mo, Na, Nb, Ni, Ti, V, W, Zn, Zr 5 ppm Water Quality* VE VE VE VE VE VE VE VE liter 5,4 5,4 5,4 5,4 5,4 5,4 5,4 5,4 Dispersion Solids content % by weight 65 65 65 65 65 65 65 65 nozzle diameter mm 2,2 2,2 2,2 2,2 2,2 2,2 2,2 2,2 temperature °C 25 25 25 25 25 25 25 25 Pressure Bear 16 16 16 16 16 16 16 16 Installation height m 6,5 6,5 6,5 6,5 6,5 6,5 6,5 6,5 Spray tower Height m 18,20 18,20 18,20 18,20 18,20 18,20 18,20 18,20 inner diameter m 6,30 6,30 6,30 6,30 6,30 6,30 6,30 6,30 T (supplied gas) °C 380 380 380 380 380 380 380 380 T (exhaust air) °C 110 110 110 110 110 110 110 110 Airflow m 3 < / h 6500 6500 6500 6500 6500 6500 6500 6500 Installation height = distance between the nozzle and the lowest point of the spray tower interior in the direction of the gravity vector. * VE = fully demineralized, conductivity ≤ 0.1 µS; ** C 006011: Graphite powder, max. particle size: 75 µm, high purity (available from Goodfellow GmbH, Bad Nauheim (Germany); *** available from Wacker Chemie AG (Munich, Germany). Table 9 (continued) Example E14-1 reactant Analogous to B1-1, but with BET=60 m 2< / g Amount of reactant kg 10 Carbon powder -- Silicon component -- Water Quality* VE liter 5,4 Dispersion Solids content % by weight 65% nozzle diameter mm 2,2 temperature °C 25 Pressure Bear 16 Installation height m 6,5 Spray tower Height m 18,2 inner diameter m 6,3 T (supplied gas) °C 380 T (exhaust air) °C 110 Airflow m 3 < / h 6500 Installation height = distance between the nozzle and the lowest point of the spray tower interior in the direction of the gravity vector. * VE = fully demineralized, conductivity ≤ 0.1 µS; ** C 006011: Graphite powder, max. particle size: 75 µm, high purity (available from Goodfellow GmbH, Bad Nauheim (Germany); *** available from Wacker Chemie AG (Munich, Germany). Table 10 Example E1-1 E 1-2 E1-3 E1-4 E1-5 E2-1 E3-1 E3-2 BET m 2 < / g 30 33 49 49 47 28 31 35 Bulk density g / ml 0,8±0,1 0,8±0,1 0,8±0,1 0,8±0,1 0,8±0,1 0,8±0,1 0,8±0,1 0,8±0, 1 Tapped density g / ml 0,9±0,1 0,9±0,1 0,9±0,1 0,9±0,1 0,9±0,1 0,9±0,1 0,9±0,1 0,9±0, 1 average particle size µm 255 255 255 255 255 255 255 255 Particle size distribution D10 µm 110 110 110 110 110 110 110 110 Particle size distribution D50 µm 222 222 222 222 222 222 222 222 Particle size distribution D90 µm 390 390 390 390 390 390 390 390 SPHT3 Dimlos 0,64-0,98 0,64-0,98 0,64-0,98 0,64-0,98 0,64-0,98 0,64-0,98 0,64-0,98 0,64-0,98 Aspect ratio W / L (width to length) Dimlos 0,64-0,94 0,64-0,94 0,64-0,94 0,64-0,94 0,64-0,94 0,64-0,94 0,64-0,94 0,64-0,94 C content ppm <4 39 <4 <4 32 100 <4 39 Cl content ppm < 60 < 60 280 <60 <60 <60 <60 < 60 Al content ppb 20 20 20 20 20 20 20 20 Sum of the concentrations of Ca, Co, Cr, Cu, Fe, Ge, Hf, K, Li, Mg, Mn, Mo, Na, Nb, Ni, Ti, V, W, Zn, Zr ppb < 700 < 700 < 1300 < 1300 < 1300 < 700 < 700 < 700 residual moisture % by weight < 3 < 3 < 3 < 3 < 3 < 3 < 3 <3 Alkaline earth metal content ppb 538 487 550 550 342 538 538 487 Pore volume ml / g 0,33 0,33 0,45 0,45 0,45 0,33 0,33 0,33 Angle of repose ° 26 26 26 26 26 26 26 26 Table 10 (continued) Example E14-1 E14-2 +< E14-3 ++< E14-4 +++< BET m 2 < / g 60 2,2 32 33 Bulk density m 2 < / g 0,8 0,76 0,79 0,82 Tapped density m 2 < / g 0,9 0,88 0,89 0,92 average particle size µm 255 8 Particle size distribution D10 µm 110 1,6 93 160 Particle size distribution D50 µm 222 7,5 235 295 Particle size distribution D90 µm 390 24 434 1120 SPHT3 Dimlos 0,64-0,98 n / a n / a n / a Aspect ratio W / L (width to length) Dimlos 0,64-0,94 n / a n / a n / a C content ppm < 4 n / a <4 < 4 Cl content ppm 280 <60 < 60 < 60 Al content ppb 20 70 34 29 Sum of the concentrations of Ca, Co, Cr, Cu, Fe, Ge, Hf, K, Li, Mg, Mn, Mo, Na, Nb, Ni, Ti, V, W, Zn, Zr ppb < 1300 <1000 < 700 < 700 residual moisture % by weight <3 <1 <3 < 3 Alkaline earth metal content ppb 550 90 562 546 Pore volume ml / g 0,45 n / a n / a n / a Angle of repose ° 26 n / a 31 36 + Commercial product "Excelica SE-5" from Tokuyama Corp. (Japan) with BET = 2.2±0.6 m² / g; ++ Granules produced from rolled granules using an Eirich mixer as described in the example in EP 0 890 555 B1, followed by a roller crusher (gap = 1 mm, two Telekom quartz glass cylinders with a diameter of 150 mm as rollers, 30 revolutions / minute), fraction with particle size < 500 µm (sieve). +++ As for ++, but fraction with particle size > 500 µm (sieve).
[0482] The granules are all open-pored and exhibit a uniform, spherical shape (all as determined by microscopic examination). They do not tend to caking or sticking together. F. Cleaning of silica granules
[0483] Silicon dioxide granules are first treated in a rotary kiln, optionally at a temperature T1, with oxygen or nitrogen (see Table 11). The silicon dioxide granules are then treated in cocurrent with a chlorine-containing component, increasing the temperature to a temperature T2. The process parameters are given in Table 11, and the properties of the resulting treated granules are given in Table 12. Table 11 Example F1-1 F1-2 F1-3 F1-4 F1-5 F2-1 F3-1 F3-2 Educt = product of E1-1 E1-2 E1-3 E1-4 E1-5 E2-1 E3-1 E3-2 rotary kiln length cm 200 200 200 200 200 200 inner diameter cm 10 10 10 10 10 10 Throughput 1)< kg / h 2 2 2 2 2 2 Rotational speed rpm 2 2 2 2 2 2 it T1 °C 1100 not applicable 1100 1100 1100 not applicable 1100 1100 atmosphere Pure O 2 not applicable Pure O 2 Pure O 2 Pure O 2 not applicable N 2 N 2 reactant O 2 not applicable O 2 O 2 O 2 not applicable No No Feeding 300l / h not applicable 300l / h 300l / h 300l / h not applicable residual moisture % by weight <1 <3 <1 <1 <1 <3 <1 <1 T2 °C 1100 1100 1100 1100 1100 1100 not applicable not applicable direct current Component 1: HCl l / h 50 50 50 50 50 50 not applicable not applicable Component 2: Cl 2 l / h 0 15 0 0 0 15 not applicable not applicable Component 3: N 2 l / h 50 35 50 50 50 35 not applicable not applicable Total direct current l / h 100 100 100 100 100 100 not applicable not applicable 1)< For the rotary kilns, throughput was chosen as the control variable. This means that the mass flow leaving the rotary kiln is continuously weighed during operation, and the rotation speed and / or inclination of the rotary kiln are then adjusted accordingly. For example, an increase in throughput can be achieved by a) increasing the rotation speed, or b) increasing the inclination of the rotary kiln from the horizontal, or a combination of a) and b). Table 11 (continued) Example F14-1 F14-2 F14-3 F14-4 Educt = product of E14-1 E14-2 E14-3 E14-4 rotary kiln 1)< length cm 200 Not applicable 200 200 inner diameter cm 10 10 10 Throughput kg / h 2 2 2 Rotation speed rpm 2 2 2 T1 °C 1100 1100 1100 atmosphere Pure O 2 Pure O 2 Pure O 2 reactant O 2 O 2 O 2 Feeding 300l / h none 300l / h none 300l / h none residual moisture % by weight <1 <1 <1 T2 °C 1100 1100 1100 direct current Component 1: HCl l / h 50 50 50 Component 2: Cl2 l / h 0 0 0 Component 3: N2 l / h 50 50 50 Total direct current l / h 100 100 100 1)< For the rotary kilns, throughput was chosen as the control variable. This means that the mass flow leaving the rotary kiln is continuously weighed during operation, and the rotation speed and / or inclination of the rotary kiln are then adjusted accordingly. For example, an increase in throughput can be achieved by a) increasing the rotation speed, or b) increasing the inclination of the rotary kiln from the horizontal, or a combination of a) and b). Table 12 Example F1-1 F1-2 F1-3 F1-4 F1-5 F2-1 F3-1 F3-2 BET m 2 < / g 25 27 43 45 40 23 25 26 C content ppm <4 <4 <4 <4 <4 <4 <4 <4 Cl content ppm 100-200 100-200 300-400 100-200 100-200 100-200 <60 <60 Al content ppb 20 20 20 20 20 20 20 20 Pore volume mm 3< / g 650 650 650 650 650 650 650 650 Sum of the concentrations of Ca, Co, Cr, Cu, Fe, Ge, Hf, K, Li, Mg, Mn, Mo, Na, Nb, Ni, Ti, V, W, Zn, Zr ppb <200 <200 <200 <200 <200 <200 <700 <700 Alkaline earth metal content ppb 115 55 95 115 40 35 136 33 Tapped density g / cm 3< 0,95 ± 0,05 0,95 ± 0,05 0,95 ± 0,05 0,95 ± 0,05 0,95 ± 0,05 0,95 ± 0,05 0,95 ± 0,05 0,95 ± 0,05 Table 12 (continued) Example F14-1 F14-2 F14-3 F14-4 BET m 2 < / g 55 2,2 26 28 C content ppm <4 n / a <4 <4 Cl content ppm 350-450 <60 100-200 100-200 Al content ppb 20 70 35 30 Pore volume mm 3< / g n / a n / a n / a n / a Sum of the concentrations of Ca, Co, Cr, Cu, Fe, Ge, Hf, K, Li, Mg, Mn, Mo, Na, Nb, Ni, Ti, V, W, Zn, Zr ppb < 200 <1000 < 200 < 200 Alkaline earth metal content ppb 105 90 119 135 Tapped density g / cm 3< 0,95 0,88 0,95 1,00
[0484] The granules after the purification step show a significantly reduced carbon content in the case of F1-2, F2-1, and F3-2 (like low-carbon granules, e.g., F1-1). In particular, F1-2, F1-5, F2-1, and F3-2 show a significantly lower alkaline earth metal content. SiC formation was not observed. G. Heat treatment of silicon dioxide granules
[0485] Silicon dioxide granules are subjected to a heat treatment in a pre-chamber in the form of a rotary kiln, which is located upstream of the melting furnace and connected to it via an intermediate chamber. The rotary kiln is characterized by a temperature profile that increases in the conveying direction. Further treated silicon dioxide granules were obtained. In Example G-4-2, heat treatment was omitted during mixing in the rotary kiln. The process parameters are listed in Table 13, and the properties of the resulting treated granules are listed in Table 14. Table 13 Example G1-1 G1-2 G1-3 G1-4 G1-5 G2-1 G3-1 G3-2 G4-1 G4-2 Educt = product of F1-1 F1-2 F1-3 F1-4 F1-5 F2-1 F3-1 F3-2 F1-1 F1-1 Silicon components -- -- -- -- -- -- -- --- Silicon powder** * Silicon powder** * Material Crowd 0,01% 0,1% Rotary kiln 1)< not applicable length cm 200 200 200 200 200 200 200 200 200 inner diameter cm 10 10 10 10 10 10 10 10 10 Throughput kg / h 8 5 5 5 5 5 5 5 5 Rotation speed rpm 30 30 30 30 30 30 30 30 30 T1 (rotary kiln inlet) °C RT RT RT RT RT RT RT RT RT T2 (rotary kiln outlet) °C 500 500 500 500 500 500 500 500 500 atmosphere Gas, flow direction Air, free convection O 2 , countercurrent O 2 , countercurrent O 2 , countercurrent O 2 , countercurrent O 2 , countercurrent O 2 , countercurrent O 2 , countercurrent O 2 , countercurrent Total gas flow throughput Nm 3 < / h 0,6 0,6 0,6 0,6 0,6 0,6 0,6 0,6 *** Grain size D 50 = 8 µm; carbon content ≤ 5 ppm; total foreign metals ≤ 5 ppm; 0.5 ppm; available from Wacker Chemie AG (Munich, Germany); RT = room temperature. 1)< For the rotary kilns, the throughput was chosen as the control variable. This means that during operation the mass flow leaving the rotary kiln is continuously weighed and then the rotation speed and / or the inclination of the rotary kiln are adjusted accordingly. For example, an increase in throughput can be achieved by a) increasing the rotation speed, or b) increasing the inclination of the rotary kiln from the horizontal, or a combination of a) and b). Table 13 (continued) Example G14-1 G14-2 G14-3 G14-4 Educt = product of F14-1 F14-2 F14-3 F14-4 Silicon components Material -- -- -- -- Crowd rotary kiln 1) < length cm 200 200 200 200 inner diameter cm 10 10 10 10 Throughput kg / h 8 8 8 8 Rotation speed rpm 30 30 30 30 T1 (rotary kiln inlet) °C RT RT RT RT T2 (rotary kiln outlet) °C 500 500 500 500 atmosphere Gas, flow direction Air, free convection Air, free convection Air, free convection Air, free convection Total gas flow throughput Nm 3 < / h 0,6 0,6 0,6 0,6 *** Grain size D 50 = 8 µm; carbon content ≤ 5 ppm; total foreign metals ≤ 5 ppm; 0.5 ppm; available from Wacker Chemie AG (Munich, Germany); RT = room temperature. 1)< For the rotary kilns, the throughput was chosen as the control variable. This means that during operation the mass flow leaving the rotary kiln is continuously weighed and then the rotation speed and / or the inclination of the rotary kiln are adjusted accordingly. For example, an increase in throughput can be achieved by a) increasing the rotation speed, or b) increasing the inclination of the rotary kiln from the horizontal, or a combination of a) and b). Table 14 Example G1-1 G1-2 G1-3 G1-4 G1-5 G2-1 G3-1 G3-2 G4-1 G4-2 BET m 2 < / g 22 23 38 42 37 22 22 21 22 24 Water content (residual moisture) ppm 500 100 100 100 100 100 500 100 500 <10000 C content ppm < 4 < 4 <4 <4 <4 <4 <4 <4 <4 <4 Cl content ppm 100-200 100-200 300-400 100-200 100-200 100-200 <60 <60 100-200 100-200 Al content ppb 20 20 20 20 20 20 20 20 20 20 Sum of the concentrations of Ca, Co, Cr, Cu, Fe, Ge, Hf, K, Li, Mg, Mn, Mo, Na, Nb, Ni, Ti, V, W, Zn, Zr ppb ≤ 200 ≤ 200 ≤ 200 ≤ 200 ≤ 200 ≤ 200 ≤ 200 ≤ 200 ≤ 200 ≤ 200 Alkaline earth metal content ppb 115 55 95 115 40 35 136 33 115 115 Angle of repose ° 26 26 26 26 26 26 26 26 26 26 Table 14 (continued) Example G14-1 G14-2 G14-3 G14-4 BET m 2 < / g 55 2,2 26 28 Water content ppm 600 <50 150 150 C content ppm < 4 n / a < 4 < 4 Cl content ppm 350-450 <60 100-200 100-200 Al content ppb 20 70 35 30 Sum of the concentrations of Ca, Co, Cr, Cu, Fe, Ge, Hf, K, Li, Mg, Mn, Mo, Na, Nb, Ni, Ti, V, W, Zn, Zr ppb ≤ 200 ≤ 1000 ≤ 200 ≤ 200 Alkaline earth metal content ppb 105 90 119 135 Angle of repose ° 26 n / a 31 36 As a result of this treatment, G3-1 and G3-2 have a significantly reduced alkaline earth metal content compared to before (F3-1 and F3-2 respectively). H. Melting granules to quartz glass
[0486] Silicon dioxide granules according to row 2 of Table 15 are used to produce a quartz glass tube in a vertical crucible drawing process. The structure of the vertical furnace for example H5-1 containing a standing melting pot is in Figure 7 shown schematically, for all other examples with a hanging melting pot Figure 6as a schematic illustration. The silicon dioxide granules are added via the solids feed, and the interior of the crucible is flushed with a gas mixture. A glass melt forms in the crucible, on which a cone of silicon dioxide granules sits. In the lower area of the crucible, molten glass is withdrawn from the glass melt via a drawing nozzle (if necessary with a mandrel) and drawn vertically downwards as a tube strand. The system's throughput is determined by the weight and viscosity of the glass melt above the nozzle and the hole size specified by the nozzle. By varying the added amount of silicon dioxide granules and the temperature, the throughput can be adjusted to the desired level. The process parameters are given in Table 15 and Table 17 and, where applicable, Table 19; the properties of the resulting quartz glass bodies are given in Table 16 and Table 18.
[0487] In Example H7-1A gas distribution ring is arranged in the crucible, through which the purge gas is supplied close to the surface of the molten glass. An example of such an arrangement is shown in the Figure 8 .
[0488] In Example H8-x The dew point was determined at the gas outlet. The measuring principle is Figure 12 shown. Between the outlet of the crucible and the dew point measurement point, the gas flow travels a distance of 100 cm. Table 15 Example H1-1 H1-2 H1-3 H1-4 H1-5 H3-1 H3-2 H4-1 H4-2 Educt = product of G1-1 G1-2 G1-3 G1-4 G1-5 G3-1 G3-2 G4-1 G4-2 melting pot type Hanging Hanging Hanging Hanging Hanging Hanging Hanging Hanging Hanging Tin crucible Tin crucible Tin crucible Tin crucible Tin crucible Tin crucible Tin crucible Tin crucible Tin crucible Metal type tungsten tungsten tungsten tungsten tungsten tungsten tungsten tungsten tungsten length cm 200 150 150 150 150 200 150 200 200 inner diameter cm 40 25 25 25 25 40 25 40 40 Throughput kg / h 30 20 20 20 20 30 20 30 30 T1 (gas chamber melting pot) °C 300 300 300 300 300 300 300 300 300 T2 (glass melt) °C 2100 2100 2100 2100 2100 2100 2100 2100 2100 T3 (nozzle) °C 1900 1900 1900 1900 1900 1900 1900 1900 1900 Atmosphere / purge gas Hey concentration Vol.-% 50 50 50 50 50 50 50 50 50 H 2 concentration Vol.-% 50 50 50 50 50 50 50 50 50 Total gas flow throughput Nm3 / h 4 4 4 4 4 2 4 2 2 O 2 ppm ≤100 ≤100 ≤100 ≤100 ≤100 ≤100 ≤100 ≤100 ≤100 Table 15 (continued) Example H14-1 H14-2 H14-3 H14-4 Educt = product of G14-1 G14-2 G14-3 G14-4 melting pot type Hanging Hanging Hanging Hanging Tin crucible Tin crucible Tin crucible Tin crucible Metal type tungsten tungsten tungsten tungsten length cm 200 200 200 200 inner diameter cm 40 40 40 40 Throughput kg / h 30 30 30 30 T1 (gas chamber melting pot) °C 300 300 300 300 T2 (glass melt) °C 2100 2100 2100 2100 T3 (nozzle) °C 1900 1900 1900 1900 Atmosphere / purge gas Hey concentration Vol.-% 50 50 50 50 H 2 concentration Vol.-% 50 50 50 50 Total gas flow throughput Nm 3 < / h 4 4 4 4 O 2 ppm ≤100 ≤100 ≤100 ≤100 Table 16 Example H1-1 H1-2 H1-3 H1-4 H1-5 H3-1 H3-2 H4-1 H4-2 C content ppm < 4 < 4 < 4 < 4 < 4 < 4 < 4 < 4 < 4 Cl content ppm 100-200 100-200 300-400 100-200 100-200 <60 <60 100-200 100-200 Al content ppb 20 20 20 20 20 20 20 20 20 Sum of the concentrations of Ca, Co, Cr, Cu, Fe, Ge, Hf, K, Li, Mg, Mn, Mo, Na, Nb, Ni, Ti, V, W, Zn, Zr ppb <400 <400 <400 <400 <400 <400 <400 <400 <400 OH content ppm 400 400 400 400 400 80 400 80 80 Alkaline earth metal content ppb 115 55 95 115 40 136 33 115 115 ODC content 1 / cm 3< 4*10 15< 2*10 16< 4*10 15< 4*10 15< 4*10 15< 5*10 18< 2*10 16< 5*10 18< 8*10 18< Pore volume mL / g 0,1 0,1 0,1 0,1 0,1 0,1 0,1 0,1 0,1 Outer diameter of tubing / quartz glass body cm 19,7 3,0 19,7 19,7 19,7 19,7 3,0 19,7 19,7 viscosity Lg(η / dPas) @1250°C 11,69 ± 0,13 11,69 ± 0,13 11,69 ± 0,13 11,69 ± 0,13 11,69 ± 0,13 12,16 ± 0,2 11,69 ± 0,13 12,16 ± 0,2 12,16 ± 0,2 @1300°C 11,49 ± 0,15 11,49 ± 0,15 11,49 ± 0,15 @1350°C 11,26 ± 0,1 11,26 ± 0,1 11,26 ± 0,1 11,26 ± 0,1 11,26 ± 0,1 11,26 ± 0,1 10,69 ± 0,07 10,69 ± 0,07 10,69 ± 0,07 10,69 ± 0,07 10,69 ± 0,07 10,88 ± 0,1 10,69 ± 0,07 10,88 ± 0,1 10,88 ± 0,1 " ± " values are the standard deviation. Table 16 (continued) Example H14-1 H14-2 H14-3 H14-4 C content < 4 n / a < 4 < 4 Cl content 350-450 <60 100-200 100-200 Al content 20 70 35 30 Sum of the concentrations of Ca, Co, Cr, Cu, Fe, Ge, Hf, K, Li, Mg, Mn, Mo, Na, Nb, Ni, Ti, V, W, Zn, Zr ≤ 1000 ≤ 100 ≤ 200 ≤ 200 OH content 800 250 400 400 Alkaline earth metal content 105 90 119 135 ODC content 4,00*10 15< 3,00*10 16< 4,00*10 15< 4,00*10 15< Pore volume 0,1 0,4 0,6 0,7 Outer diameter of tubing / quartz glass body 19,7 19,7 19,7 19,7 viscosity @1250°C 11,62±0,12 11,86±0,15 11,69±0,13 11,69±0,13 @1300°C 11,24±0,1 11,3±0,11 11,26±0,1 11,26±0,1 @1350°C 10,67±0,05 10,74±0,1 10,69±0,07 10,69±0,07 Fine bubbles* >50 / kg n / a >10 / kg >10 / kg Large bubbles** <1 / kg n / a >2 / kg >4 / kg *Fine bubbles: bubble diameter of < 200 mµ. ** Large bubbles: bubble diameter of > 500 mµ. Table 17 Example H5-1 H6-1 H7-1 H8-1 H8-2 H8-3 H8-4 Educt = product of G1-1 G1-1 G1-1 G1-1 G1-1 G1-1 G1-1 melting pot type Standing Hanging Hanging Hanging Hanging Hanging Hanging sintered crucible sintered crucible Tin crucible Tin crucible Tin crucible Tin crucible Tin crucible Metal type tungsten tungsten tungsten tungsten tungsten tungsten tungsten Additional installations or attachments Gas distribution ring Dew point measurement Dew point measurement Dew point measurement Dew point measurement length cm 250 250 200 200 200 200 200 inner diameter cm 40 36 40 40 40 40 40 Throughput kg / h 40 35 30 30 30 30 30 T1 (gas chamber melting pot) °C 300 400 300 300 300 300 300 T2 (glass melt) °C 2100 2150 2100 2100 2100 2100 2100 T3 (nozzle) °C 1900 1900 1900 1900 1900 1900 1900 atmosphere Hey concentration Vol.-% 30 50 50 50 50 50 50 H 2 concentration Vol.-% 70 50 50 50 50 50 50 Total gas flow throughput Nm 3 < / h 4 4 8 8 4 3 2 O 2 ppm <100 <100 ≤10 ≤100 ≤100 ≤100 ≤100 Table 18 Example H5-1 H6-1 H7-1 H8-1 H8-2 H8-3 H8-4 C content ppm < 4 < 4 < 4 < 4 < 4 < 4 < 4 Cl content ppm 100-200 100-200 100-200 100-200 100-200 100-200 100-200 Al content ppb 20 20 20 20 20 20 20 Sum of the concentrations of Ca, Co, Cr, Cu, Fe, Ge, Hf, K, Li, Mg, Mn, Mo, Na, Nb, Ni, Ti, V, W, Zn, Zr ppb <400 <400 <400 <400 <400 <400 <400 OH content ppm 400 400 400 250 400 500 800 Alkaline earth metal content ppb 115 115 115 115 115 115 115 ODC content 1 / cm 3< <4*10 15< <4*10 15< <4*10 15< <4*10 15< <4*10 15< <4*10 15< <4*10 15< Content of W, Mo, Re, Ir, Os ppb <300ppb <300ppb <100 ppb <50 ppb <100 ppb <5 ppm 100 ppm Outer diameter of tubing / quartz glass body cm 26,0 19,7 19,7 19,7 19,7 19,7 19,7 viscosity Lg(η / dPas) @1250°C 11,69 ± 0,13 11,69 ± 0,13 11,69 ± 0,13 12,06 ± 0,15 11,69 ± 0,13 11,69 ± 0,13 11,63 ± 0,13 @1300°C @1350°C 11,26 ± 0,1 11,26 ± 0,1 11,26 ± 0,1 11,38 ± 0,1 11,26 ± 0,1 11,26 ± 0,1 11,22 ± 0,1 10,69 ± 0,07 10,69 ± 0,07 10,69 ± 0,07 10,75 ± 0,08 10,69 ± 0,07 10,69 ± 0,07 10,65 ± 0,07 Table 19 Example H-7-1 H8-1 H8-2 H8-3 H8-4 Distribution ring (gas inlet in the crucible), height above molten glass cm 2 -- -- -- -- Location of gas outlet In melting crucible lid In melting pot lid In melting crucible lid In Schme lztiege ldecke l In melting pot blanket l Dew point of the gas stream -90 -90 -90 -90 -90 Before feeding to the melting pot After removal from the melting pot -10 -30 -10 0 +10 I. Reworking a quartz glass body
[0489] A previously drawn quartz glass body obtained in Example H1-1 (1000 kg, surface area = 110 m²; diameter = 1.65 cm, total length 2120 m²) was cut into 200 cm long pieces by scoring and chipping. The end faces were reworked by sawing to obtain a straight end face. The resulting batch of quartz glass body (N-1) was cleaned by immersion in an HF bath (V = 2 m³) for 30 minutes and then rinsed with deionized water (yielding quartz glass body (N-1')). J. "Old acid" (HF bath after use)
[0490] The liquid present in the immersion bath in Example I (V= 2m 3< ) is determined directly after treatment of the quartz glass body (I-1') without further processing. The liquid used for the aforementioned treatment is characterized by the properties listed in Table 20 before and after treatment. K. Conveyability of granules (angle of repose)
[0491] Beds with an angle of repose of 23 to 26° (silicon dioxide granules) and those with a larger angle of repose, e.g., quartz glass granules with an angle of repose of 33 to 37°, were investigated. Beds with an angle of repose of 23 to 26° exhibited good flow properties when transporting material through a conveyor pipe inclined at 30° from the horizontal. Beds with a larger angle of repose, with the same arrangement, exhibited uneven transport characterized by intermittent settling. Table 1 element Unit Before treating a quartz glass body After treatment of a quartz glass body with mass m= 1000kg and surface area of 110m 2< Al ppm 0,04 0,8 Refractory metal (W, Mo, ...) ppm 0 0,15 Other metals according to list* total, of which ppm 0,15 1 Ca ppm 0,01 0,3 Mg ppm 0,04 0,09 N / a ppm 0,04 0,1 Cr ppm 0,01 0,01 Ni ppm 0,001 0,01 Fe ppm 0,01 0,05 Zr ppm 0,01 0,05 Ti ppm 0,01 0,05 HF % by weight 40 35 Content of Si-F compounds % by weight 4 6 density g / cm 3< 1,14 1,123
Claims
1. A silicon dioxide granulate, wherein the silicon dioxide granulate comprises the following features: A) a BET surface area in a range of from 20 to 50 m2 / g; B) a bulk density in a range of from 0.5 to 1.2 g / cm3; C) an average particle size in a range of from 50 to 500 µm; D) a carbon content of less than 50 ppm; E) an aluminum content of less than 200 ppb; F) a tapped density in a range of from 0.7 to 1.3 g / cm3; I) a pore volume in a range of from 0.1 to 2.5 mL / g; J) a particle size distribution D10 in a range of from 50 to 150 µm; K) a particle size distribution D50 in a range of from 150 to 300 µm; and L) a particle size distribution D90 in a range of from 250 to 620 µm; wherein the particle size distribution of the silicon dioxide granulate is determined according to DIN ISO 13322:2009; wherein the ppm and ppb are each based on the total weight of the silicon dioxide granulate.