HOT-DIP GALVANIZING PLANT

DE502017016500D1Active Publication Date: 2024-10-31FONTAINE HLDG NV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502017016500
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2016-06-27
Filing Date
2017-03-13
Publication Date
2024-10-31
Estimated Expiration
2037-03-13

AI Technical Summary

Technical Problem

Conventional hot-dip galvanizing processes using aluminum-containing zinc melts face challenges with wettability issues, sensitivity to contaminants, and the need for heavy metal compounds, leading to defects and ecological concerns.

Method used

A system for hot-dip galvanizing that employs a flux composition with zinc chloride, ammonium chloride, and aluminum or silver salts in an alcohol-water mixture, eliminating lead chloride and nickel chloride, which improves wetting, reduces defects, and enhances ecological compatibility.

Benefits of technology

The system achieves defect-free, high-quality hot-dip galvanizing with improved corrosion protection and mechanical properties, while reducing environmental impact by avoiding heavy metal contaminants.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to the technical field of galvanizing iron-based or iron-containing components, in particular steel-based or steel-containing components (steel components), preferably for the automotive or motor vehicle industry, but also for other technical fields of application (e.g. for the construction industry, the field of general mechanical engineering, the electrical industry, etc.), by means of hot-dip galvanizing (hot-dip galvanizing).

[0002] In particular, the present invention relates to the inventive use of a plant for hot-dip galvanizing (hot-dip galvanizing) according to claims 1-14.

[0003] Metallic components of any kind made of ferrous material, especially steel components, often require effective corrosion protection due to their application. Steel components for motor vehicles (such as cars, trucks, commercial vehicles, etc.), but also for other technical sectors (e.g., the construction industry, mechanical engineering, the electrical industry, etc.), require effective corrosion protection that can withstand long-term stress.

[0004] In this context, it is known to protect steel-based components against corrosion by means of galvanizing (galvanizing). During galvanizing, the steel is coated with a generally thin layer of zinc to protect it from corrosion. Various galvanizing processes can be used to galvanize steel components, i.e., to coat them with a metallic zinc coating. These include, in particular, hot-dip galvanizing (also known as hot-dip galvanizing), spray galvanizing (flame spraying with zinc wire), diffusion galvanizing (Sherard galvanizing), electrolytic galvanizing, non-electrolytic galvanizing using zinc flake coatings, and mechanical galvanizing.There are major differences between the aforementioned galvanizing processes, particularly with regard to the process implementation, but also with regard to the nature and properties of the zinc layers or zinc coatings produced.

[0005] Arguably the most important method for corrosion protection of steel using metallic zinc coatings is hot-dip galvanizing (hot-dip galvanizing). This involves immersing steel continuously (e.g., strip and wire) or piece by piece (e.g., components) in a heated vat of molten zinc at temperatures of approximately 450 °C to 600 °C (melting point of zinc: 419.5 °C). This creates a resistant alloy layer of iron and zinc on the steel surface, with a very firmly adhering pure zinc layer forming on top.

[0006] Hot-dip galvanizing has been a recognized and proven method for protecting parts and components made of ferrous materials, especially steel, from corrosion for many years. As previously described, the typically pre-cleaned or pre-treated component is immersed in a hot, liquid zinc bath, where it reacts with the molten zinc and, as a result, forms a relatively thin zinc layer that is metallurgically bonded to the base material.

[0007] In hot-dip galvanizing, a distinction is made between discontinuous batch galvanizing (see, for example, DIN EN ISO 1461) and continuous strip and wire galvanizing (see, for example, DIN EN 10143 and DIN EN 10346). Both batch galvanizing and strip and wire galvanizing are standardized processes. Continuously galvanized steel strip and continuously galvanized wire are each a preliminary or intermediate product (semi-finished product) that is further processed after galvanizing, particularly by forming, punching, cutting, etc., whereas components to be protected by batch galvanizing are first completely manufactured and only then hot-dip galvanized (thereby providing all-round protection against corrosion). Batch galvanizing and strip / wire galvanizing also differ in terms of the thickness of the zinc layer, which results in different protection durations - also depending on the zinc layer.The zinc layer thickness of strip-galvanized sheets is usually a maximum of 20 to 25 micrometers, whereas the zinc layer thickness of batch-galvanized steel parts is usually in the range of 50 to 200 micrometers and even more.

[0008] Hot-dip galvanizing provides both active and passive corrosion protection. Passive protection is provided by the barrier effect of the zinc coating. Active corrosion protection is achieved through the cathodic effect of the zinc coating. Compared to more noble metals in the electrochemical series, such as iron, zinc acts as a sacrificial anode, protecting the underlying iron from corrosion until it is completely corroded.

[0009] In batch galvanizing according to DIN EN ISO 1461, the hot-dip galvanizing of mostly larger steel components and structures takes place. Steel-based blanks or finished workpieces (components) are pretreated and then immersed in the molten zinc bath. Immersion allows for easy access to interior surfaces, weld seams, and hard-to-reach areas of the workpieces or components to be galvanized.

[0010] Conventional hot-dip galvanizing, particularly dip galvanizing, is based primarily on dipping iron or steel components into a zinc bath, forming a zinc coating or coating on the surface of the components. To ensure the adhesion, integrity, and uniformity of the zinc coating, careful surface preparation of the components to be galvanized is generally required beforehand. This typically includes degreasing followed by rinsing, subsequent acid pickling followed by rinsing, and finally fluxing followed by drying.

[0011] For reasons of process economy and cost-effectiveness, during batch galvanizing of identical or similar components (e.g., series production of automotive components), these are typically brought together or grouped for the entire process (in particular by means of a common product carrier, e.g., designed as a crossbeam or frame, or a common holding or fastening device for a large number of these identical or similar components). For this purpose, a plurality of components are attached to the product carrier using holding devices, such as slings, tie wires, or the like. The components are then fed in a grouped state via the product carrier to the individual treatment steps or stages of the hot-dip galvanizing process.

[0012] The typical process sequence for conventional hot-dip galvanizing is usually as follows:

[0013] First, the surfaces of the components in question are degreased to remove grease and oil residues. Typically, aqueous alkaline or acidic degreasing agents can be used as degreasing agents. After cleaning in the degreasing bath, a rinsing process follows, typically by immersion in a water bath, to prevent degreasing agents from being carried over into the subsequent pickling process step with the galvanized material. This is particularly important when switching from alkaline degreasing to acidic pickling.

[0014] This is followed by a pickling treatment, which primarily serves to remove inherent contaminants, such as rust and scale, from the steel surface. Pickling is typically carried out in diluted hydrochloric acid, with the duration of the pickling process depending, among other things, on the contamination level (e.g., degree of rust) of the galvanized material and the acid concentration and temperature of the pickling bath. To prevent or minimize the carryover of acid and / or salt residues with the galvanized material, a rinsing process (rinsing step) usually follows the pickling treatment.

[0015] This is followed by the so-called fluxing (synonymously known as flux treatment), whereby the previously degreased and pickled steel surface is treated with a so-called flux, which typically consists of an aqueous solution of inorganic chlorides, most commonly a mixture of zinc chloride (ZnCl 2 ) and ammonium chloride (NH 4 Cl). On the one hand, the task of the flux is to carry out a final intensive fine cleaning of the steel surface before the steel surface reacts with the molten zinc, to dissolve the oxide skin of the zinc surface and to prevent further oxidation of the steel surface until the galvanizing process. On the other hand, the flux is intended to increase the wettability between the steel surface and the molten zinc.After the flux treatment, drying usually takes place to create a solid flux film on the steel surface and to remove adhering water, so that subsequent undesirable reactions (especially the formation of water vapor) in the liquid zinc dip bath are avoided.

[0016] The components pretreated in the aforementioned manner are then hot-dip galvanized by immersion in the molten zinc bath. In hot-dip galvanizing with pure zinc, the zinc content of the melt is at least 98.0 wt.% according to DIN EN ISO 1461. After immersion of the galvanized part in the molten zinc bath, it remains in the molten zinc bath for a sufficient period of time, in particular until the part has assumed its temperature and is coated with a layer of zinc. Typically, the surface of the molten zinc bath is cleaned of oxides, zinc ash, flux residues, and the like, before the part is withdrawn from the molten zinc bath. The component hot-dip galvanized in this way is then subjected to a cooling process (e.g., in air or in a water bath). Finally, any holding devices for the component, such as lifting gear, tie wires, or the like, are removed.

[0017] Following the galvanizing process, a sometimes complex post-processing or post-treatment process can usually be carried out. This involves, for example, removing as much excess zinc bath residue as possible, particularly so-called drips from the zinc solidifying at the edges, as well as oxide or ash residues adhering to the component.

[0018] One criterion for the quality of hot-dip galvanizing is the thickness of the zinc coating in µm (micrometers). The DIN EN ISO 1461 standard specifies the minimum coating thicknesses required for batch galvanizing, depending on the material thickness. In practice, the coating thicknesses are significantly higher than the minimum coating thicknesses specified in DIN EN ISO 1461. Generally, zinc coatings produced by batch galvanizing have a thickness in the range of 50 to 200 micrometers and even more.

[0019] During the galvanizing process, a coating of iron / zinc alloy layers of varying composition forms on the steel part as a result of the mutual diffusion of the liquid zinc with the steel surface. When the hot-dip galvanized articles are removed, a layer of zinc – also known as the pure zinc layer – remains adhered to the uppermost alloy layer, which corresponds in composition to the molten zinc. Due to the high temperatures during hot-dip dipping, a relatively brittle layer based on an alloy (solid solution) between iron and zinc initially forms on the steel surface, followed by the pure zinc layer. While this relatively brittle iron / zinc alloy layer improves the adhesion to the base material, it makes the galvanized steel more difficult to form.Higher silicon contents in steel, such as those used to so-called "slaking" the steel during production, lead to increased reactivity between the zinc melt and the base material and, consequently, to strong growth of the iron / zinc alloy layer. This results in the formation of relatively thick overall layers. While this enables a very long corrosion protection period, the increasing zinc layer thickness also increases the risk of the layer flaking under mechanical stress, especially local impacts, thus compromising the corrosion protection effect.

[0020] To counteract the previously described problem of the rapidly growing, brittle, and thick iron / zinc alloy layer, and to enable thinner layer thicknesses while simultaneously providing high corrosion protection during galvanizing, it is known from the prior art to add additional aluminum to the zinc melt or liquid zinc bath. For example, adding 5 wt.% aluminum to a liquid zinc melt produces a zinc / aluminum alloy with a lower melting point than pure zinc. By using a zinc / aluminum melt (Zn / Al melt) orA liquid zinc / aluminium bath (Zn / Al bath) allows, on the one hand, significantly lower layer thicknesses for reliable corrosion protection to be achieved (generally below 50 micrometers); on the other hand, the formation of the brittle iron / tin alloy layer is avoided, since the aluminium - without being bound to a specific theory - first forms a barrier layer on the steel surface of the component in question, onto which the actual zinc layer is then deposited.

[0021] Components hot-dip galvanized with a zinc / aluminium melt can therefore be easily formed, but still have improved corrosion protection properties - despite the significantly lower layer thickness compared to conventional hot-dip galvanizing with a virtually aluminum-free zinc melt.

[0022] A zinc / aluminum alloy used in a hot-dip galvanizing bath exhibits improved fluidity properties compared to pure zinc. Furthermore, zinc coatings produced by hot-dip galvanizing using such zinc / aluminum alloys exhibit greater corrosion resistance (two to six times better than that of pure zinc), better aesthetics, improved formability, and better paintability than zinc coatings formed from pure zinc. Furthermore, this technology can also be used to produce lead-free zinc coatings.

[0023] Such a hot-dip galvanizing process using a zinc / aluminum melt or a zinc / aluminum hot-dip galvanizing bath is known, for example, from WO 2002 / 042512 A1 and the relevant publication equivalents to this patent family (e.g., EP 1 352 100 B1, DE 601 24 767 T2, and US 2003 / 0219543 A1). Suitable fluxes for hot-dip galvanizing using zinc / aluminum melt baths are also disclosed therein, since flux compositions for zinc / aluminum hot-dip galvanizing baths must be different from those for conventional hot-dip galvanizing with pure zinc.The process disclosed therein enables corrosion protection coatings to be produced with very low layer thicknesses (generally well below 50 micrometers and typically in the range of 2 to 20 micrometers) and with very low weight at a high cost-effectiveness, which is why the process described therein is used commercially under the name microZINQ ®< process.

[0024] However, prior art hot-dip galvanizing processes that utilize a zinc / aluminum melt or a zinc / aluminum hot-dip galvanizing bath (such as WO 2002 / 042512 A1) use fluxes containing significant amounts of lead chloride to enable good wettability with respect to the flux treatment, nickel chloride to ensure good temperature resistance of the flux, and optionally other transition or heavy metal chlorides to achieve other desired properties. Furthermore, the pH of the flux bath is generally adjusted in prior art hot-dip galvanizing processes using hydrochloric acid (hydrochloric acid), which can potentially promote undesirable hydrogen embrittlement of the metal substrate being treated.

[0025] With regard to the formation of the zinc layer and its properties, it has been shown that these can be significantly influenced by alloying elements in the zinc melt. Aluminum is one of the most important elements here: It has been shown that with an aluminum content of just 100 ppm (weight-based) in the zinc melt, the appearance of the resulting zinc layer can be improved, making it brighter and shinier. This effect increases steadily with increasing aluminum content in the zinc melt up to 1,000 ppm (weight-based). Furthermore, it has been shown that - as already described - from an aluminum content in the zinc melt of 0.12 wt.-%, an intermetallic Fe / Al phase forms between the iron material and the zinc layer, which inhibits the otherwise typical diffusion processes between iron and zinc melt, thus significantly reducing the growth of the Zn / Fe phases. As a result, significantly thinner zinc layers result from this aluminum content in the zinc melt. Finally, it has been shown that, in principle, the corrosion protection effect of the resulting zinc layer increases with increasing aluminum content in the zinc melt; this is based on the fact that the Al / Zn compounds form significantly more stable covering layers more quickly.

[0026] Well-known examples of the commercial use of aluminum-containing zinc melts are the so-called Galfan ® process and the aforementioned microZINQ ® process, with an aluminum content in the zinc melt typically ranging from 4.2 wt.% to 6.2 wt.%. One of the advantages of this alloy is that around the average value of 5 wt.%, a eutectic composition of the Al / Zn system with a melting point of 382 °C is present, which enables a reduction in the operating temperature in the galvanizing process.

[0027] However, the disadvantage of using aluminum-alloyed or aluminum-containing zinc melts (Zn / Al melts) is the significantly more difficult wettability of the iron or steel surface to be galvanized with the liquid-hot Zn / Al melt, and the significantly more sensitive and difficult-to-manage reaction between the Zn / Al melt and the iron or steel surface of the component to be treated due to the high affinity of aluminum to iron. This leads to the necessity of significantly higher cleanliness requirements for the steel surface after the cleaning steps and before immersion in the Zn / Al melt, compared to a process using a pure zinc melt.In addition, the use of a suitable flux and preheating of the galvanized material are necessary so that the reaction between the melt and the base material and, with it, the formation of a homogeneous, closed zinc coating can take place.

[0028] When using aluminum-alloyed or aluminum-containing zinc melts (Zn / Al melts), special fluxes are generally required for the flux treatment (flux treatment). These fluxes often contain heavy metal compounds (usually heavy metal chlorides) that are not always ecologically compatible or undesirable, in particular lead and / or nickel chloride, but possibly also cobalt, manganese, tin, antimony and / or bismuth chloride, which are necessary to ensure subsequent perfect hot-dip galvanizing, in particular without defects on the galvanized components. These fluxes are specifically designed for hot-dip galvanizing with aluminum-alloyed or aluminum-containing zinc melts.In fluxes designed for aluminium-containing zinc melts (Zn / Al melts), the lead chloride is intended in particular to reduce the surface tension and in this way to improve the wettability of the component surface to be treated with the liquid Zn / Al melt, while the nickel chloride is intended to improve the temperature resistance of the flux, particularly with regard to the drying process that usually follows the flux treatment.

[0029] Nevertheless, when using aluminum-alloyed or aluminum-containing zinc melts (Zn / Al melts) according to the state of the art, especially when using fluxes known from the state of the art, there remains a high sensitivity to foreign contaminants such as grease and oil, which are either not removed in the upstream cleaning stages or result from carryover through the cleaning stages despite rinsing processes. This is because in the pretreatment steps prior to the actual galvanizing process, the complete removal of all foreign and native contaminants (such as grease and oil, germs, oxidation residues, etc.) from the steel surface is required. This usually involves several alkaline degreasing baths and acidic pickling baths. In the usually multiple rinsing stages downstream of the respective degreasing and cleaning baths, the alkaline oracidic media to avoid carryover into the subsequent process step. In practice, however, it has been shown that under the conditions of the galvanizing process, in particular with large volumes of pretreatment baths, high throughputs of a wide variety of components to be galvanized, some of which have a very high variance in the existing surface conditions in the as-delivered state, etc., particularly when using aluminum-alloyed or aluminum-containing zinc melts (Zn / Al melts) according to the state of the art, defects on the galvanized material repeatedly occur. These are typically due to inadequate cleaning, possibly in conjunction with insufficiently effective flux treatment.

[0030] The internet excerpt according to Roeling: "Stahlbau Arbeitshilfe", 28 April 2010 (2010-04-28), XP055677329, (http: / / bauforumstahl.de / upload / documents / publikationen / arbeitshilfen / sta.01.4.pdf) concerns general statements and principles for hot-dip galvanizing in a liquid zinc melt.

[0031] Furthermore, EP 2 725 115 A1 relates to a flux composition for treating a metallic surface, wherein the flux composition comprises more than 40 and less than 70 wt% zinc chloride, 10 to 30 wt% ammonium chloride, more than 6 and less than 30 wt% of a combination of at least two alkali metal chlorides, including sodium chloride and potassium chloride, 0 to 2 wt% lead chloride and 0 to 15 wt% tin chloride.

[0032] Furthermore, WO 95 / 04607 A1 relates to a hot-dip galvanizing process for treating steel components. An aqueous flux is applied to the steel components, the components are then preheated and exposed to a non-reducing atmosphere to dry the flux. Additional energy in the form of heat is applied to the pretreated component, which exceeds the energy required to dry the flux, and the component is then placed in a molten zinc bath for hot-dip galvanizing.

[0033] DE 23 17 600 A1 relates to an aqueous flux solution for hot-dip galvanizing, which contains zinc chloride and optionally alkali chlorides. The flux solution also contains aluminum chloride and / or hydrogen chloride and optionally a maximum of 4 wt.% ammonium chloride, based on the zinc chloride and any alkali chlorides contained in the solution, as well as conventional corrosion inhibitors.

[0034] Furthermore, EP 1 694 880 A2 relates to an aqueous flux solution for hot-dip galvanizing steel components, wherein the flux solution comprises 200 to 600 g / l zinc chloride and ammonium chloride, wherein the molar ratio between ammonium chloride and zinc chloride is 1.7 to 3.3 and wherein the flux solution comprises 8 g / l to 80 g / l aluminum chloride (AlCl 3 ).

[0035] The problem underlying the present invention therefore consists in providing a method for hot-dip galvanizing (hot-dip galvanizing), in particular of iron-based or iron-containing components, preferably steel-based or steel-containing components (steel components), using an aluminum-containing or aluminum-alloyed zinc melt and a corresponding plant for carrying out this method and, moreover, a flux or flux bath that can be used in the method, wherein the previously described disadvantages of the prior art are to be at least largely avoided or at least mitigated.

[0036] In particular, such a process is to be provided which, compared to conventional hot-dip galvanizing processes using an aluminum-containing or aluminum-alloyed zinc melt, enables improved process economics and / or a more efficient, in particular more flexible and / or more reliable, in particular less error-prone process sequence and / or improved ecological compatibility.

[0037] In particular, such a process should not require the use of significant amounts of heavy metal compounds, in particular heavy metal chlorides, such as lead and / or nickel chloride, but possibly also other heavy metal chlorides, such as cobalt, manganese, tin, antimony and / or bismuth chloride, in the flux treatment and thus have improved ecological compatibility, but nevertheless reliably ensure that the treated components are galvanized efficiently and without defects.

[0038] To solve the problem described above, the present invention proposes the inventive use of a plant for hot-dip galvanizing iron or steel components according to claim 1; further, particularly special and / or advantageous embodiments of the inventive use are the subject of the relevant subclaims (claims 2 to 14).

[0039] It goes without saying that in the following explanations, configurations, embodiments, advantages and the like which are explained below only with regard to one aspect in order to avoid repetition, naturally also apply accordingly with regard to the other aspects without this requiring separate mention.

[0040] With regard to all relative or percentage weight-related information mentioned below, in particular relative quantity or weight information, it should also be noted that, within the scope of the present invention, these must be selected by the person skilled in the art in such a way that, in total, including all components or ingredients, in particular as defined below, they always add up to 100% or 100% by weight; however, this is self-evident to the person skilled in the art.

[0041] Furthermore, the person skilled in the art may, depending on the application or the individual case, deviate from the range specifications given below if necessary, without departing from the scope of the present invention.

[0042] In addition, all values ​​or parameters or the like mentioned below can generally be determined using standardized or explicitly specified determination procedures or, if not, using determination or measurement methods that are familiar to a person skilled in the art.

[0043] Having said that, the present invention will now be explained in detail below.

[0044] The present invention therefore relates to the use of a plant for hot-dip galvanizing iron or steel components, the plant comprising the following treatment devices in the sequence listed below: (A) at least one degreasing device for the degreasing treatment of iron or steel components; downstream in the process direction or downstream of (A) (B) optionally at least one rinsing device for rinsing iron or steel components degreased in the degreasing device (A); downstream in the process direction or downstream of (B) (C) at least one pickling device for the pickling treatment of iron or steel components degreased in the degreasing device (A) and optionally rinsed in the rinsing device (B); downstream in the process direction or downstream of (C) (D) optionally at least one rinsing device for rinsing iron or steel components pickled in the pickling device (C); downstream in the process direction or downstream of (D) (E) at least one flux treatment device for the flux treatment of iron or steel components pickled in the pickling device (C) and optionally rinsed in the rinsing device (D).Steel components, wherein the flux treatment device contains at least one flux bath with a flux composition, wherein the flux bath comprises a liquid phase containing an alcohol / water mixture, wherein the liquid phase of the flux bath contains the flux composition, wherein the alcohol of the alcohol / water mixture of the flux bath is a water-miscible and / or water-soluble alcohol and is selected from the group of linear or branched, saturated or unsaturated, aliphatic, cycloaliphatic or aromatic, primary, secondary or tertiary monohydric C 1 -C 4 alcohols and mixtures thereof, and wherein the flux composition contains as ingredients (i) zinc chloride (ZnCl 2 ) in amounts in the range of 50 to 95 wt.%, (ii) ammonium chloride (NH 4 Cl) in amounts in the range of 5 to 45 wt.%, (iii) at least one alkali and / or alkaline earth salt in amounts in the range of 0.1 up to 25 wt.% and (iv)at least one aluminum salt and / or at least one silver salt in amounts in the range of 5 • 10 -5 < to 2 wt.%, wherein all the above-mentioned quantities are based on the composition and are to be selected such that a total of 100 wt.% results, and wherein the flux composition is completely free of lead chloride (PbCl 2 ) and nickel chloride (NiCl 2 ); downstream in the process direction or downstream of (E) (F) at least one drying device (F) for drying iron or steel components subjected to a flux treatment in the flux treatment device (E), wherein the drying device (F) is controlled by means of a control device such that the drying treatment is carried out such that the surface of the iron or steel component has a temperature in the range of 100 to 300 °C during drying, wherein the drying device (F) has at least one inlet for introducing and / or admittingof air and wherein the drying device (F) comprises at least one drying device; downstream of (F) (G) in the process direction or downstream of at least one hot-dip galvanizing device for hot-dip galvanizing iron or steel components which have been subjected to a flux treatment in the flux treatment device (E) and optionally dried in the drying device (F), wherein the hot-dip galvanizing device comprises at least one galvanizing bath containing an aluminum-containing zinc melt, designed for dipping iron or steel components.

[0045] As explained below, the present invention is associated with a multitude of completely unexpected advantages, special features and surprising technical effects, the following description of which makes no claim to completeness, but illustrates the inventive character of the present invention: Surprisingly, within the scope of the present invention it is possible to use a flux, ie a flux bath or a flux composition, which even in the difficult to carry out hot-dip galvanizing using aluminum-containing oraluminium-alloyed zinc melts without the presence of lead chloride (PbCl 2 ) and nickel chloride (NiCl 2 ) and preferably also without other transition metal chlorides in the flux, in particular in the flux bath or the flux composition, such as in particular cobalt chloride (CoCl 2 ), manganese chloride (MnCl 2 ), tin chloride (SnCl 2 ), bismuth chloride (BiCl 3 ) and antimony chloride (SbCl 3 ), without the quality of the resulting hot-dip galvanizing layer being impaired.

[0046] On the contrary, the present invention results in hot-dip galvanized layers that are completely free of defects and also have improved corrosion protection properties and generally also excellent, if not even improved, mechanical and other properties (e.g. optical properties such as gloss).

[0047] As explained below, a special feature of the present invention in this context is that the flux used according to the invention, in particular the flux composition used according to the invention or the flux bath used according to the invention, contains at least one aluminum salt and / or at least one silver salt, in particular aluminum chloride (AlCl 3 ) and / or silver chloride (AgCl), preferably aluminum chloride (AlCl 3 ), preferably in very small amounts, which means that organic and / or inorganic impurities (such as suspended matter), which are still present, for example, from the upstream treatment steps despite rinsing processes and generally lead to the formation of defects during hot-dip galvanizing, are discharged orcan be precipitated, so that additional transition metal chlorides to improve the wetting behavior or other properties in the context of the flux used according to the invention, in particular flux bath or flux composition, can be completely dispensed with.

[0048] In combination with a liquid phase of the flux bath based on a water / alcohol mixture, the efficiency of the process used according to the invention can be further improved: As explained in more detail below, the alcohol content in the flux bath can significantly shorten the times required to dry the flux film and / or significantly reduce the drying temperatures. Furthermore, the film formation and wetting with the flux are homogenized in this way.

[0049] In particular, the present invention, with regard to hot-dip galvanizing using aluminum-alloyed or aluminum-containing zinc melts, results in significantly improved process economics and a more efficient, in particular more flexible and / or more reliable, in particular less error-prone process sequence as well as improved ecological compatibility, in particular due to the omission of lead chloride and nickel chloride and possibly other transition or heavy metal chlorides in the flux used, but also the alcohol content in the flux bath.

[0050] Consequently, the present invention, particularly due to its improved ecological compatibility, can also be used in ecologically sensitive areas where transition and heavy metal compounds, in particular transition metal and heavy metal chlorides, are to be avoided.

[0051] In particular, the present invention does not require the use of significant amounts of transition and heavy metal compounds, in particular transition and heavy metal chlorides, such as lead and / or nickel chloride, but optionally also other heavy metal chlorides, such as cobalt, manganese, tin, antimony and / or bismuth chloride, in the flux treatment, but nevertheless reliably ensures that the treated components are galvanized efficiently and without defects.

[0052] The special features of the inventive use or the system used according to the invention described below are also directly reflected in the obtainable process products, i.e., the hot-dip galvanized or hot-dip galvanized iron and steel components: These not only exhibit improved mechanical and optical properties and improved corrosion protection properties, but are also completely free of defects, even with relatively thin layers compared to the hot-dip galvanized layer. Furthermore, no undesirable transition metals or heavy metals can be introduced from the flux into the ultimately resulting hot-dip galvanized layer, since transition metals or heavy metals are completely avoided during the flux treatment according to the present invention.

[0053] Transition metals or heavy metals are at most deliberately added or alloyed to the zinc melt or the hot-dip galvanizing bath in order to specifically adjust certain properties of the hot-dip galvanizing layer, but then in an ecologically compatible manner, since they are an integral part of the hot-dip galvanizing layer and are embedded or incorporated therein as a solid alloy component.

[0054] The individual ingredients or components of the flux composition and flux bath used according to the invention work together synergistically: The zinc chloride ensures very good coverage of the iron or steel surface, particularly due to the flat formation of the dried ZnCl 2 crystals. However, since 100% coverage is practically impossible and smaller oxidation sites or a thin oxidation layer can always be present, a sufficient amount of ammonium chloride is added to the flux composition. This ammonium chloride is deposited on the component surface and thermally decomposes into NH 3 and HCl when immersed in the zinc melt, thus removing any remaining oxide residues from the component surface. Since an excessively high NH 4 Cl content causes the melting point of the ZnCl 2 / NH 4 Cl mixture to drop significantly compared to pure zinc chloride (approx.300 °C), alkali and / or alkaline earth salts, in particular NaCl and / or KCl, are added, which raise the melting point of the flux composition and thus enable high and effective drying.

[0055] In addition, it has now surprisingly been shown that the use of silver or aluminum salt, in particular AgCl and / or AlCl 3 , in the flux or flux composition leads to an increase in the purity of the flux or flux composition, since silver or aluminum salt, in particular AgCl and / or AlCl 3 , namely organic and / or inorganic impurities, such as suspended matter, which, for example, can be introduced from the upstream pretreatment steps despite repeated rinsing processes, are removed or precipitated in quantities that are only small, but in the case of Zn / Al melts, in quantities that are sufficient to form defects. Examples of such impurities are germs or bacteria (e.g. carryover from degreasing) as well as phosphates and sulfates (e.g. carryover from pickling).By precipitating these substances, transfer to the component surface is avoided and the source of incorrect galvanizing is thus eliminated.

[0056] Furthermore, it has been shown that the use of alcohol in the flux bath as at least a partial replacement for the otherwise commonly used pure water base has a positive effect on the process control and the galvanizing result in several respects.

[0057] Due to the alcohol content, even the smallest impurities can be dissolved in the flux (which, in the case of organic substances, are then precipitated by the aluminum or silver salt used, especially AlCl 3 and / or AgCl), so that an improved cleaning effect is achieved.

[0058] The alcohol content can shorten the time required to dry the flux film, particularly due to the lower evaporation point of alcohol compared to water. This represents a significant improvement over the previous state of the art, where the maximum drying time was defined by the galvanizing cycle, meaning that drying time was often insufficient to sufficiently dry the flux film, particularly in the case of massive components. A completely dried flux film enables a clean reaction with the molten zinc without splashing due to evaporating residual water. Better drying also results in less zinc ash being produced, reducing the risk of zinc ash adhering to the galvanized material (i.e., better galvanizing quality and less rework).In addition, faster drying means that the drying time and / or drying temperature can be reduced, which in turn means energy savings and / or increased productivity. The flux in the zinc bath also burns off more quickly (also due to the lower vaporization point), meaning the energy from the molten zinc can flow directly into heating the component, which in turn leads to a faster and more effective galvanizing process.

[0059] The proportion of alcohol used depends in particular on the aluminum content of the zinc melt used, on the required drying or preheating (which in turn depends on the component geometry, in particular the material thickness, with thicker components requiring longer drying times), on the zinc alloy used and on the thickness of the applied flux film, with thicker flux layers requiring longer drying times depending on the salt concentration, withdrawal speed, roughness of the steel surface, etc.), on the existing degree of contamination of the material to be galvanized and on the plant-technical requirements (e.g. performance of the drying furnace, timing of the galvanizing process, extraction performance of the flux bath, etc.).

[0060] As a result, under identical drying conditions (i.e., identical drying times and temperatures), the use of alcohol in the flux bath, even in small quantities and up to large quantities, leads to faster drying of the flux film and improved galvanizing quality. This means that better drying leads to better galvanizing quality. Furthermore, in corrosion tests (e.g., salt spray test or salt spray test according to DIN EN ISO 9227:2012), hot-dip galvanized components pretreated with an alcohol-containing flux demonstrate significantly longer service life (up to 20% service life improvement or even more) compared to hot-dip galvanized components pretreated with an otherwise identical flux (but without any alcohol content, i.e., purely aqueous).

[0061] Within the scope of the present invention, an efficient and ecologically compatible hot-dip galvanizing process can thus be provided, whereby the disadvantages of the prior art described above can be at least largely avoided or at least mitigated.

[0062] Preferred embodiments of the use according to the invention or of the process sequence used according to the invention are described and explained in more detail below: According to the present invention, the flux bath is adjusted to a defined and / or predetermined, in particular acidic pH, in particular in the pH range from 0 to 6.9, preferably in the pH range from 0.5 to 6.5, preferably in the pH range from 1 to 5.5, particularly preferably in the pH range from 1.5 to 5, very particularly preferably in the pH range from 2 to 4.5, even more preferably in the pH range from 2 to 4.

[0063] According to a particularly preferred embodiment, the flux bath is adjusted to a defined and / or predetermined, in particular acidic, pH value, wherein the pH value is adjusted by means of a preferably inorganic acid in combination with a preferably inorganic basic compound, in particular ammonia (NH 3 ). This embodiment, i.e., the fine adjustment of the pH value by means of a preferably inorganic basic compound, in particular ammonia (NH 3 ), is particularly advantageous because it counteracts undesirable hydrogen embrittlement of the component to be treated.

[0064] With regard to the flux bath used according to the invention, in particular the alcohol / water mixture of the liquid phase of the flux bath, the weight-based alcohol / water ratio can vary within wide ranges. Generally, the flux bath contains the alcohol / water mixture in a weight-based alcohol / water ratio in the range from 0.5:99.5 to 99:1, in particular in the range from 2:98 to 95:5, preferably in the range from 5:95 to 90:10, more preferably in the range from 5:95 to 50:50, particularly preferably in the range from 5:95 to 45:55, very particularly preferably in the range from 5:95 to 50:50, even more preferably in the range from 10:90 to 30:70, based on the alcohol / water mixture.

[0065] According to a particular embodiment, the flux bath contains the alcohol, based on the alcohol / water mixture, in an amount of at least 0.5 wt.%, in particular in an amount of at least 1 wt.%, preferably in an amount of at least 2 wt.%, particularly preferably in an amount of at least 3 wt.%, even more preferably in an amount of at least 4 wt.%.

[0066] Typically, the flux bath contains the alcohol, based on the alcohol / water mixture, in an amount of up to 90 wt.%, in particular in an amount of up to 70 wt.%, preferably in an amount of up to 50 wt.%, particularly preferably in an amount of up to 30 wt.%, even more preferably in an amount of up to 25 wt.%.

[0067] According to the invention, the alcohol of the alcohol / water mixture of the flux bath is a water-miscible and / or water-soluble alcohol.

[0068] Advantageously, the alcohol of the alcohol / water mixture of the flux bath is an alcohol that forms an azeotropic mixture with water.

[0069] According to the invention, the alcohol of the alcohol / water mixture of the flux bath is selected from the group of C 1 -C 4 alcohols and mixtures thereof.

[0070] According to the invention, the alcohol of the alcohol / water mixture of the flux bath is selected from the group of linear or branched, saturated or unsaturated, aliphatic, cycloaliphatic or aromatic, primary, secondary or tertiary monohydric C 1 -C 4 alcohols.

[0071] According to a particularly preferred embodiment, the alcohol of the alcohol / water mixture of the flux bath is selected from the group of methanol, ethanol, propan-1-ol, propan-2-ol, butan-1-ol, butan-2-ol and mixtures thereof.

[0072] As regards the flux bath used according to the invention, the flux bath may - in addition to the above-mentioned ingredients or components - also contain at least one wetting agent and / or surfactant, in particular at least one ionic or non-ionic wetting agent and / or surfactant, preferably at least one non-ionic wetting agent and / or surfactant.

[0073] The amounts of the wetting agent and / or surfactant in question can vary within wide ranges: In particular, the flux bath can contain the at least one wetting agent and / or surfactant in amounts of 0.0001 to 15 wt.%, preferably in amounts of 0.001 to 10 wt.%, preferably in amounts of 0.01 to 8 wt.%, even more preferably in amounts of 0.01 to 6 wt.%, very particularly preferably in amounts of 0.05 to 3 wt.%, even more preferably in amounts of 0.1 to 2 wt.%, based on the flux bath.

[0074] Furthermore, the flux can contain the at least one wetting agent and / or surfactant in particular in amounts of 0.0001 to 10 vol.%, preferably in amounts of 0.001 to 8 vol.%, preferably in amounts of 0.01 to 5 vol.%, even more preferably in amounts of 0.01 to 5 vol.%, very particularly preferably in amounts of 0.05 to 3 vol.%, even more preferably in amounts of 0.1 to 2 vol.%, based on the flux bath.

[0075] The amount or concentration of the flux composition used according to the invention in the flux bath used according to the invention can likewise vary within wide ranges: Typically, the flux bath can contain the flux composition in an amount of at least 150 g / l, in particular in an amount of at least 200 g / l, preferably in an amount of at least 250 g / l, preferably in an amount of at least 300 g / l, particularly preferably in an amount of at least 400 g / l, very particularly preferably in an amount of at least 450 g / l, even more preferably in an amount of at least 500 g / l, in particular calculated as the total salt content of the flux composition.

[0076] Preferably, the flux bath can contain the flux composition in an amount of 150 g / l to 750 g / l, in particular in an amount of 200 g / l to 700 g / l, preferably in an amount of 250 g / l to 650 g / l, preferably in an amount of 300 g / l to 625 g / l, particularly preferably in an amount of 400 g / l to 600 g / l, very particularly preferably in an amount of 450 g / l to 580 g / l, even more preferably in an amount of 500 g / l to 575 g / l, in particular calculated as the total salt content of the flux composition.

[0077] As regards the flux composition used according to the invention as such, the flux composition contains as ingredients (i) zinc chloride (ZnCl 2 ) in amounts in the range of 50 to 95 wt.%, preferably in the range of 55 to 90 wt.%, preferably in the range of 60 to 85 wt.%, particularly preferably in the range of 65 to 82.5 wt.%, even more preferably in the range of 70 to 82 wt.%, (ii) ammonium chloride (NH 4 Cl) in amounts in the range of 5 to 45 wt.%, preferably in the range of 7.5 to 40 wt.%, preferably in the range of 10 to 35 wt.%, particularly preferably in the range of 11 to 25 wt.%, even more preferably in the range of 12 to 20 wt.%, (iii) at least one alkali and / or alkaline earth metal salt in amounts in the range of 0.1 to 25 wt.%, preferably in the range of 0.5 to 20 wt.%, preferably in the range of 1 to 15 wt.%, particularly preferably in the range of 2 to 12.5 wt.%, more preferably in the range of 4 to 10 wt.%, and(iv) at least one aluminum salt and / or at least one silver salt, in particular aluminum chloride (AlCl 3 ) and / or silver chloride (AgCl), preferably aluminum chloride (AlCl 3 ), in amounts in the range of 5 • 10 -5< to 2 wt.%, even more preferably in the range of 5 • 10 -5< to 5 • 10 -3< wt.%, wherein all the above-mentioned quantities are based on the composition and are to be selected such that a total of 100 wt.% results, and wherein the flux composition is at least substantially free, preferably completely free, of lead chloride (PbCl 2 ) and Nickel chloride (NiCl 2 ) is trained.

[0078] As regards component (iii), ie the alkaline earth metal and / or alkaline earth metal salt, of the flux composition used according to the invention, there are also various possible variations: In particular, the flux composition used according to the invention can contain an alkali metal and / or alkaline earth metal chloride as the alkali metal and / or alkaline earth metal salt of component (iii).

[0079] Furthermore, the flux composition used according to the invention can contain as alkali and / or alkaline earth salt of component (iii) at least one alkali and / or alkaline earth salt of an alkali and / or alkaline earth metal from the group of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr) and barium (Ba) and combinations thereof.

[0080] According to the invention, it is preferred if the flux composition used according to the invention contains, as alkali and / or alkaline earth salt of component (iii), at least two different alkali and / or alkaline earth salts, in particular at least two alkali and / or alkaline earth salts of an alkali and / or alkaline earth metal from the group of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr) and barium (Ba) and combinations thereof.

[0081] Furthermore, it is particularly preferred if the flux composition used according to the invention contains, as alkali and / or alkaline earth salt of component (iii), at least two different alkali salts, in particular two different alkali chlorides, preferably sodium chloride andPotassium chloride, in particular with a sodium / potassium weight ratio in the range of 50:1 to 1:50, in particular in the range of 25:1 to 1:25, preferably in the range of 10:1 to 1:10.

[0082] According to the invention, it is particularly preferred if the flux composition used according to the invention is completely free of cobalt chloride (CoCl 2 ), manganese chloride (MnCl 2 ), tin chloride (SnCl 2 ), bismuth chloride (BiCl 3 ) and Antimony chloride (SbCl 3 ) is formed.

[0083] According to the invention, it is also preferred if the flux composition used according to the invention is completely free of lead chloride (PbCl 2 ), nickel chloride (NiCl 2 ), cobalt chloride (CoCl 2 ), manganese chloride (MnCl 2 ), tin chloride (SnCl 2 ), bismuth chloride (BiCl 3 ) andAntimony chloride (SbCl 3 ) and / or if the flux composition is at least completely free of chlorides from the group of lead chloride (PbCl 2 ), nickel chloride (NiCl 2 ), cobalt chloride (CoCl 2 ), manganese chloride (MnCl 2 ), tin chloride (SnCl 2 ), bismuth chloride (BiCl 3 ) and Antimony chloride (SbCl 3 ) is formed.

[0084] It is furthermore advantageous according to the invention if the flux composition used according to the invention is completely free of salts and compounds of metals from the group of lead (Pb), nickel (Ni), cobalt (Co), manganese (Mn), tin (Sn), bismuth (Bi) and Antimony (Sb) is formed.

[0085] Finally, it is also advantageous according to the invention if the flux composition used according to the invention, apart from zinc chloride (ZnCl 2 ) and aluminum and / or silver salt, in particular silver chloride (AgCl) and / or aluminum chloride (AlCl 3 ), is completely free of salts and compounds of transition and heavy metals.

[0086] As far as flux treatment is concerned, the procedure is generally such that the flux treatment is carried out by bringing the iron or steel component into contact with the flux bath and / or the flux composition, in particular by dipping or spraying, preferably dipping. It is particularly advantageous if the iron or steel component is brought into contact with the flux bath and / or the flux composition, in particular by immersing it in the flux bath, for a period of 0.001 to 30 minutes, in particular 0.01 to 20 minutes, preferably 0.1 to 15 minutes, preferably 0.5 to 10 minutes, particularly preferably 1 to 5 minutes.In particular, the iron or steel component can be brought into contact with the flux bath and / or the flux composition, in particular immersed in the flux bath, for a period of up to 30 minutes, in particular up to 20 minutes, preferably up to 15 minutes, preferably up to 10 minutes, particularly preferably up to 5 minutes.

[0087] As far as the drying treatment is concerned, it is preferred according to the invention if the drying treatment is carried out at a temperature in the range from 50 to 400 °C, in particular in the range from 75 to 350 °C, preferably in the range from 100 to 300 °C, preferably in the range from 125 to 275 °C, particularly preferably in the range from 150 to 250 °C, and / or if the drying treatment is carried out at a temperature up to 400 °C, in particular up to 350 °C, preferably up to 300 °C, preferably up to 275 °C, particularly preferably up to 250 °C.

[0088] The drying treatment is usually carried out in such a way that the surface of the iron or steel component has a temperature in the range of 100 to 300 °C, in particular in the range of 125 to 275 °C, preferably in the range of 150 to 250 °C, more preferably in the range of 160 to 225 °C, particularly preferably in the range of 170 to 200 °C, during drying.

[0089] Typically, the drying treatment can be carried out in the presence of and / or by means of air.

[0090] In particular, the drying treatment can be carried out in at least one drying device, in particular in at least one oven.

[0091] As regards the aluminum-containing, in particular aluminum-alloyed, zinc melt ("Zn / Al melt") and / or the galvanizing bath used according to the invention, the following should be stated in this regard.

[0092] According to a typical embodiment of the present invention, it is advantageous if the aluminum-containing, in particular aluminum-alloyed zinc melt ("Zn / Al melt") and / or the galvanizing bath has an amount of aluminum in the range from 0.0001 to 25 wt.%, in particular in the range from 0.001 to 20 wt.%, preferably in the range from 0.005 to 17.5 wt.%, more preferably in the range from 0.01 to 15 wt.%, particularly preferably in the range from 0.02 to 12.5 wt.%, very particularly preferably in the range from 0.05 to 10 wt.%, even more preferably in the range from 0.1 to 8 wt.%, based on the aluminum-containing, in particular aluminum-alloyed zinc melt ("Zn / Al melt") and / or the galvanizing bath.In particular, the aluminum-containing, in particular aluminum-alloyed, zinc melt ("Zn / Al melt") and / or the galvanizing bath can contain, based on the aluminum-containing, in particular aluminum-alloyed zinc melt ("Zn / Al melt") and / or the galvanizing bath, an amount of zinc of at least 75 wt. %, in particular at least 80 wt. %, preferably at least 85 wt. %, preferably at least 90 wt. %, and optionally at least one further metal, in particular in amounts of up to 5 wt. % and / or in particular selected from the group consisting of bismuth (Bi), lead (Pb), tin (Sn), nickel (Ni), silicon (Si), magnesium (Mg), and combinations thereof. All of the above-mentioned quantities must be selected such that a total of 100 wt. % results.

[0093] Furthermore, it is preferred according to the invention if the aluminum-containing, in particular aluminum-alloyed zinc melt ("Zn / Al melt") and / or the galvanizing bath has the following composition, wherein all quantities mentioned below are based on the aluminum-containing, in particular aluminum-alloyed zinc melt ("Zn / Al melt") and / or the galvanizing bath and are to be selected such that a total of 100 wt.% results: (i) zinc (Zn), in particular in amounts in the range from 75 to 99.9999 wt.%, in particular in the range from 80 to 99.999 wt.%, preferably in the range from 82.5 to 99.995 wt.%, preferably in the range from 85 to 99.99 wt.%, particularly preferably in the range from 87.5 to 99.98 wt.%, very particularly preferably in the range from 90 to 99.95 wt.%, even more preferably in the range from 92 to 99.9 wt.%, (ii) aluminum (Al), in particular in amounts in the range from 0.0001 to 25 wt.%, in particular in the range from 0.001 to 20 wt.%, preferably in the range from 0.005 to 17.5 wt.%, preferably in the range from 0.01 to 15 wt.%, particularly preferably in the range from 0.02 to 12.5 wt.%, very particularly preferably in the Range of 0.05 to 10 wt.%, more preferably in the range of 0.1 to 8 wt.%, (iii) optionally bismuth (Bi), in particular in amounts of up to 0.5 wt.%, preferably in amounts of up to 0.3 wt.%, preferably in amounts of up to 0.1 wt.-%, (iv) optionally lead (Pb), in particular in amounts of up to 0.5 wt.%, preferably in amounts of up to 0.2 wt.%, preferably in amounts of up to 0.1 wt.%, (v) optionally tin (Sn), in particular in amounts of up to 0.9 wt.%, preferably in amounts of up to 0.6 wt.%, preferably in amounts of up to 0.3 wt.%, (vi) optionally nickel (Ni), in particular in amounts of up to 0.1 wt.%, preferably in amounts of up to 0.08 wt.%, preferably in amounts of up to 0.06 wt.%, (vii) optionally silicon (Si), in particular in amounts of up to 0.1 wt.%, preferably in amounts of up to 0.05 wt.%, preferably in amounts of up to 0.01 wt.%, (viii) optionally magnesium (Mg), in particular in amounts of up to 5 wt.%, preferably in amounts of up to 2.5 wt.%, preferably in amounts of up to 0.8 % by weight. .

[0094] If the zinc melt used contains other alloying components or alloying metals in addition to aluminum, the process can be controlled in a targeted manner: The presence of lead and bismuth in particular can reduce the surface tension and thus improve the wettability of the surface to be galvanized, while the presence of tin can improve the optical properties, in particular the gloss, of the resulting galvanizing layer, the presence of nickel can further reduce the layer thickness, the presence of silicon can extend the service life of the zinc bath container (e.g. steel kettle) and the presence of magnesium can improve the corrosion properties, in particular the corrosion resistance, of the resulting galvanizing layer.

[0095] According to a particular embodiment, the aluminum-containing, in particular aluminum-alloyed zinc melt ("Zn / Al melt") and / or the galvanizing bath can have a temperature in the range of 375 °C to 750 °C, in particular a temperature in the range of 380 °C to 700 °C, preferably a temperature in the range of 390 °C to 680 °C, even more preferably in the range of 395 °C to 675 °C.

[0096] Typically, the hot-dip galvanizing step is carried out in such a way that the iron or steel component is immersed, in particular immersed and moved, in the aluminum-containing, in particular aluminum-alloyed zinc melt ("Zn / Al melt") and / or in the galvanizing bath, in particular for a period of time sufficient to ensure effective hot-dip galvanizing (hot-dip galvanizing), in particular for a period of time in the range of 0.0001 to 60 minutes, preferably in the range of 0.001 to 45 minutes, more preferably in the range of 0.01 to 30 minutes, even more preferably in the range of 0.1 to 15 minutes.

[0097] In particular, the aluminum-containing, in particular aluminum-alloyed zinc melt ("Zn / Al melt") and / or the galvanizing bath can be contacted with and / or flushed or passed through at least one inert gas, in particular nitrogen.

[0098] In principle, the process used in the context of the invention can be operated continuously or discontinuously.

[0099] The iron or steel component to be treated may be a single product or a multitude of individual products. In this case, a batch process is preferred, although a continuous process is not excluded in principle.

[0100] Furthermore, the iron or steel component can also be a long product, in particular a wire, tube, sheet, coil, or the like. In this case, a continuous process is preferred, although a discontinuous process is not excluded.

[0101] According to a particular embodiment of the present invention, the hot-dip galvanizing (hot-dip galvanizing) carried out can be followed by a cooling step, i.e. the hot-dip galvanized (hot-dip galvanized) iron or steel component can be subjected to a cooling treatment, optionally followed by a further post-processing and / or post-treatment step.

[0102] The optional cooling step and / or the optional cooling treatment can be carried out in particular by means of air and / or in the presence of air, preferably down to ambient temperature.

[0103] As stated above, the subject of the present invention is therefore the inventive use of a plant for hot-dip galvanizing iron or steel components, wherein the plant comprises the following treatment devices in the sequence listed below: (A) at least one degreasing device for the degreasing treatment of iron or steel components; downstream in the process direction or downstream of (A) (B) optionally at least one rinsing device for rinsing iron or steel components degreased in the degreasing device (A); downstream in the process direction or downstream of (B) (C) at least one pickling device for the pickling treatment of iron or steel components degreased in the degreasing device (A) and optionally rinsed in the rinsing device (B); downstream in the process direction or downstream of (C) (D) optionally at least one rinsing device for rinsing iron or steel components pickled in the pickling device (C); downstream in the process direction or downstream of (D) (E) at least one flux treatment device for the flux treatment of iron or steel components pickled in the pickling device (C) and optionally rinsed in the rinsing device (D).Steel components, wherein the flux treatment device contains at least one flux bath with a flux composition, wherein the flux bath comprises a liquid phase containing an alcohol / water mixture, wherein the liquid phase of the flux bath contains the flux composition, wherein the alcohol of the alcohol / water mixture of the flux bath is a water-miscible and / or water-soluble alcohol and is selected from the group of linear or branched, saturated or unsaturated, aliphatic, cycloaliphatic or aromatic, primary, secondary or tertiary monohydric C 1 -C 4 alcohols and mixtures thereof, and wherein the flux composition contains as ingredients (i) zinc chloride (ZnCl 2 ) in amounts in the range of 50 to 95 wt.%, (ii) ammonium chloride (NH 4 Cl) in amounts in the range of 5 to 45 wt.%, (iii) at least one alkali and / or alkaline earth salt in amounts in the range of 0.1 up to 25 wt.% and(iv) contains at least one aluminum salt and / or at least one silver salt in amounts in the range of 5 • 10 -5< to 2 wt.%, wherein all the above-mentioned amounts are based on the composition and are to be selected such that a total of 100 wt.% results, and wherein the flux composition is completely free of lead chloride (PbCl 2 ) and nickel chloride (NiCl 2 );downstream of (E) (F) in the process direction, at least one drying device (F) for drying iron or steel components subjected to a flux treatment in the flux treatment device (E), wherein the drying device (F) is controlled by means of a control device such that the drying treatment is carried out such that the surface of the iron or steel component has a temperature in the range of 100 to 300 °C during drying, wherein the drying device (F) has at least one inlet for introducing and / or admitting air and wherein the drying device (F) comprises at least one drying device;downstream of (F) (G) in the process direction, at least one hot-dip galvanizing device for hot-dip galvanizing iron or steel components which have been subjected to a flux treatment in the flux treatment device (E) and optionally dried in the drying device (F), wherein the hot-dip galvanizing device comprises at least one galvanizing bath containing an aluminum-containing zinc melt, designed for dipping iron or steel components. ;

[0104] As previously described, the flux bath of the flux treatment device (E) is usually acidic.

[0105] In particular, the flux bath is adjusted to a defined and / or predetermined, in particular acidic pH, in particular in the pH range from 0 to 6.9, preferably in the pH range from 0.5 to 6.5, preferably in the pH range from 1 to 5.5, particularly preferably in the pH range from 1.5 to 5, very particularly preferably in the pH range from 2 to 4.5, even more preferably in the pH range from 2 to 4.

[0106] According to a particularly preferred embodiment, the flux bath is adjusted to a defined and / or predetermined, in particular acidic, pH value, wherein the pH value is adjusted using a preferably inorganic acid in combination with a preferably inorganic basic compound, in particular ammonia (NH 3 ). The associated advantages have already been explained in connection with the method used according to the invention.

[0107] As far as the flux bath used in the flux treatment device (E) is concerned, its composition can vary within wide ranges: Typically, the system is designed such that the flux bath contains the alcohol / water mixture in a weight-related alcohol / water ratio in the range from 0.5:99.5 to 99:1, in particular in the range from 2:98 to 95:5, preferably in the range from 5:95 to 90:10, more preferably in the range from 5:95 to 50:50, particularly preferably in the range from 5:95 to 45:55, very particularly preferably in the range from 5:95 to 50:50, even more preferably in the range from 10:90 to 30:70, based on the alcohol / water mixture.

[0108] Typically, the system used according to the invention is designed such that the flux bath contains the alcohol, based on the alcohol / water mixture, in an amount of at least 0.5 wt.%, in particular in an amount of at least 1 wt.%, preferably in an amount of at least 2 wt.%, particularly preferably in an amount of at least 3 wt.%, even more preferably in an amount of at least 4 wt.%.

[0109] Typically, the system used according to the invention is designed such that the flux bath contains the alcohol, based on the alcohol / water mixture, in an amount of up to 90 wt.%, in particular in an amount of up to 70 wt.%, preferably in an amount of up to 50 wt.%, particularly preferably in an amount of up to 30 wt.%, even more preferably in an amount of up to 25 wt.%.

[0110] According to the invention, the alcohol of the alcohol / water mixture of the flux bath is a water-miscible and / or water-soluble alcohol.

[0111] It is preferred if the alcohol of the alcohol / water mixture of the flux bath is an alcohol that forms an azeotropic mixture with water.

[0112] According to the invention, the alcohol of the alcohol / water mixture of the flux bath is selected from the group of linear or branched, saturated or unsaturated, aliphatic, cycloaliphatic or aromatic, primary, secondary or tertiary monohydric C 1 -C 4 alcohols.

[0113] According to a particularly preferred embodiment of the invention, the system is designed such that the alcohol of the alcohol / water mixture of the flux bath is selected from the group of methanol, ethanol, propan-1-ol, propan-2-ol, butan-1-ol, butan-2-ol and mixtures thereof.

[0114] Within the scope of the system used according to the invention, it can be provided that the flux bath also contains at least one wetting agent and / or surfactant, in particular at least one ionic or non-ionic wetting agent and / or surfactant, preferably at least one non-ionic wetting agent and / or surfactant.

[0115] The amounts of wetting agent and / or surfactant in the flux bath used according to the invention can vary within wide ranges: In particular, the flux bath can contain the at least one wetting agent and / or surfactant in amounts of 0.0001 to 15 wt.%, preferably in amounts of 0.001 to 10 wt.%, preferably in amounts of 0.01 to 8 wt.%, even more preferably in amounts of 0.01 to 6 wt.%, very particularly preferably in amounts of 0.05 to 3 wt.%, even more preferably in amounts of 0.1 to 2 wt.%, based on the flux bath.

[0116] Furthermore, the flux bath can contain the at least one wetting agent and / or surfactant in amounts of 0.0001 to 10 vol.%, preferably in amounts of 0.001 to 8 vol.%, preferably in amounts of 0.01 to 5 vol.%, even more preferably in amounts of 0.01 to 5 vol.%, very particularly preferably in amounts of 0.05 to 3 vol.%, even more preferably in amounts of 0.1 to 2 vol.%, based on the flux bath.

[0117] As previously explained in connection with the method used according to the invention, the amount or concentration of the flux composition used according to the invention in the flux bath designed according to the invention can equally vary within wide ranges: In particular, it can be provided that the flux bath contains the flux composition in an amount of at least 150 g / l, in particular in an amount of at least 200 g / l, preferably in an amount of at least 250 g / l, preferably in an amount of at least 300 g / l, particularly preferably in an amount of at least 400 g / l, very particularly preferably in an amount of at least 450 g / l, even more preferably in an amount of at least 500 g / l, in particular calculated as the total salt content of the flux composition.

[0118] Furthermore, it can be provided according to the invention that the flux bath contains the flux composition in an amount of 150 g / l to 750 g / l, in particular in an amount of 200 g / l to 700 g / l, preferably in an amount of 250 g / l to 650 g / l, preferably in an amount of 300 g / l to 625 g / l, particularly preferably in an amount of 400 g / l to 600 g / l, very particularly preferably in an amount of 450 g / l to 580 g / l, even more preferably in an amount of 500 g / l to 575 g / l, in particular calculated as the total salt content of the flux composition.

[0119] According to the invention, it is provided that the flux composition used according to the invention contains as ingredients (i) zinc chloride (ZnCl 2 ) in amounts in the range of 50 to 95 wt.%, preferably in the range of 55 to 90 wt.%, preferably in the range of 60 to 85 wt.%, particularly preferably in the range of 65 to 82.5 wt.%, even more preferably in the range of 70 to 82 wt.%, (ii) ammonium chloride (NH 4 Cl) in amounts in the range of 5 to 45 wt.%, preferably in the range of 7.5 to 40 wt.%, preferably in the range of 10 to 35 wt.%, particularly preferably in the range of 11 to 25 wt.%, even more preferably in the range of 12 to 20 wt.%, (iii) at least one alkali and / or alkaline earth metal salt in amounts in the range of 0.1 to 25 wt.%, preferably in the range of 0.5 to 20 wt.%, preferably in the range of 1 to 15 wt.%, particularly preferably in the range of 2 to 12.5 wt.%, more preferably in the range of 4 to 10 wt.-%, and (iv) at least one aluminum salt and / or at least one silver salt, in particular aluminum chloride (AlCl 3 ) and / or silver chloride (AgCl), preferably aluminum chloride (AlCl 3 ), in amounts in the range of 5 • 10 -5< to 2 wt.%, even more preferably in the range of 5 • 10 -5< to 5 • 10 -3< wt.%. contains, wherein all the above-mentioned quantities are based on the composition and are to be selected in such a way that a total of 100 wt.% results, and wherein the flux composition is completely free of lead chloride (PbCl 2 ) and Nickel chloride (NiCl 2 ) is formed.

[0120] As already described above in connection with the process used according to the invention, component (iii) of the flux composition used according to the invention can also vary within wide ranges: According to the invention, it is preferred if the flux composition contains an alkali metal and / or alkaline earth metal chloride as the alkali metal and / or alkaline earth metal salt of component (iii).

[0121] According to a typical embodiment, the flux composition used according to the invention can contain as alkali and / or alkaline earth salt of component (iii) at least one alkali and / or alkaline earth salt of an alkali and / or alkaline earth metal from the group of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr) and barium (Ba) and combinations thereof.

[0122] According to a further typical embodiment of the present invention, the flux composition used according to the invention can contain, as alkali and / or alkaline earth salt of component (iii), at least two different alkali and / or alkaline earth salts, in particular at least two alkali and / or alkaline earth salts of an alkali and / or alkaline earth metal from the group of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr) and barium (Ba) and combinations thereof.

[0123] Finally, according to a typical embodiment, the flux composition used according to the invention can contain, as alkali and / or alkaline earth salt of component (iii), at least two different alkali salts, in particular two different alkali chlorides, preferably sodium chloride andPotassium chloride, in particular with a sodium / potassium weight ratio in the range of 50:1 to 1:50, in particular in the range of 25:1 to 1:25, preferably in the range of 10:1 to 1:10.

[0124] According to the invention, it is preferred if the flux composition used according to the invention is completely free of cobalt chloride (CoCl 2 ), manganese chloride (MnCl 2 ), tin chloride (SnCl 2 ), bismuth chloride (BiCl 3 ) and Antimony chloride (SbCl 3 ) is formed.

[0125] It is furthermore advantageous according to the invention if the flux composition used according to the invention is completely free of lead chloride (PbCl 2 ), nickel chloride (NiCl 2 ), cobalt chloride (CoCl 2 ), manganese chloride (MnCl 2 ), tin chloride (SnCl 2 ), bismuth chloride (BiCl 3 ) andAntimony chloride (SbCl 3 ) is formed and / or if the flux composition is completely free of chlorides from the group of lead chloride (PbCl 2 ), nickel chloride (NiCl 2 ), cobalt chloride (CoCl 2 ), manganese chloride (MnCl 2 ), tin chloride (SnCl 2 ), bismuth chloride (BiCl 3 ) and Antimony chloride (SbCl 3 ) is formed.

[0126] It is also preferred according to the invention if the flux composition used according to the invention is completely free of salts and compounds of metals from the group of lead (Pb), nickel (Ni), cobalt (Co), manganese (Mn), tin (Sn), bismuth (Bi) and Antimony (Sb) is formed.

[0127] Finally, it is particularly advantageous according to the invention if the flux composition, apart from zinc chloride (ZnCl 2 ) and aluminum and / or silver salt, in particular silver chloride (AgCl) and / or aluminum chloride (AlCl 3 ), is completely free of salts and compounds of transition and heavy metals.

[0128] Furthermore, it can be provided according to the invention that the flux treatment device (E) comprises a device for bringing the iron or steel component into contact with the flux bath and / or the flux composition, in particular a device for dipping or spray application, preferably a device for dipping. In particular, it can be provided that the device for bringing the iron or steel component into contact with the flux bath and / or the flux composition is controllable and / or is controlled in such a way, in particular by means of a control device, that the iron or steel component is brought into contact with the flux bath and / or the flux composition, in particular is dipped into the flux bath, for a period of 0.001 to 30 minutes, in particular 0.01 to 20 minutes, preferably 0.1 to 15 minutes, preferably 0.5 to 10 minutes, particularly preferably 1 to 5 minutes.Furthermore, it can be provided according to the invention in particular that the device for bringing the iron or steel component into contact with the flux bath and / or the flux composition is controllable and / or is controlled in such a way, in particular by means of a control device, that the iron or steel component is brought into contact with the flux bath and / or the flux composition, in particular is immersed in the flux bath, for a period of up to 30 minutes, in particular up to 20 minutes, preferably up to 15 minutes, preferably up to 10 minutes, particularly preferably up to 5 minutes.

[0129] Furthermore, it is provided according to the invention that the drying device (F) is controllable and / or is controlled in such a way, in particular by means of a control device, that the drying treatment takes place at a temperature in the range 100 to 300 °C, preferably in the range from 125 to 275 °C, particularly preferably in the range from 150 to 250 °C, and / or that the drying treatment takes place at a temperature up to 300 °C, preferably up to 275 °C, particularly preferably up to 250 °C.

[0130] Furthermore, it is provided according to the invention that the drying device (F) can be controlled by means of a control device and / or is controlled in such a way that the drying treatment is carried out in such a way that the surface of the iron or steel component has a temperature in the range from 100 to 300 °C, in particular in the range from 125 to 275 °C, preferably in the range from 150 to 250 °C, more preferably in the range from 160 to 225 °C, particularly preferably in the range from 170 to 200 °C, during drying.

[0131] Typically, the drying treatment is carried out in the presence of air. For this purpose, the drying device (F) has at least one inlet for introducing and / or admitting air.

[0132] According to the invention, the drying device (F) comprises at least one drying device, in particular at least one oven.

[0133] As regards the hot-dip galvanizing device (G) of the plant used according to the invention, it comprises at least one aluminum-containing, in particular aluminum-alloyed, zinc melt ("Zn / Al melt"), in particular at least one galvanizing bath containing an aluminum-containing, in particular aluminum-alloyed zinc melt, preferably designed for dipping iron or steel components.

[0134] In this context, the plant used according to the invention is typically designed such that the aluminum-containing, in particular aluminum-alloyed zinc melt ("Zn / Al melt") and / or the galvanizing bath has an amount of aluminum in the range from 0.0001 to 25 wt.%, in particular in the range from 0.001 to 20 wt.%, preferably in the range from 0.005 to 17.5 wt.%, more preferably in the range from 0.01 to 15 wt.%, particularly preferably in the range from 0.02 to 12.5 wt.%, very particularly preferably in the range from 0.05 to 10 wt.%, even more preferably in the range from 0.1 to 8 wt.%, based on the aluminum-containing, in particular aluminum-alloyed zinc melt ("Zn / Al melt") and / or the galvanizing bath, in particular wherein the aluminum-containing.In particular, the aluminum-alloyed zinc melt ("Zn / Al melt") and / or the galvanizing bath, based on the aluminum-containing, in particular aluminum-alloyed zinc melt ("Zn / Al melt") and / or the galvanizing bath, can contain a zinc content of at least 75 wt.%, in particular at least 80 wt.%, preferably at least 85 wt.%, preferably at least 90 wt.%, and optionally at least one further metal, in particular in amounts of up to 5 wt.% and / or in particular selected from the group consisting of bismuth (Bi), lead (Pb), tin (Sn), nickel (Ni), silicon (Si), magnesium (Mg), and combinations thereof. All of the aforementioned quantities must be selected such that a total of 100 wt.% results.

[0135] Typically, the plant used according to the invention is designed such that the aluminum-containing, in particular aluminum-alloyed zinc melt ("Zn / Al melt") and / or the galvanizing bath has the following composition, wherein all quantities mentioned below are based on the aluminum-containing, in particular aluminum-alloyed zinc melt ("Zn / Al melt") and / or the galvanizing bath and are to be selected such that a total of 100 wt.% results: (i) zinc (Zn), in particular in amounts in the range from 75 to 99.9999 wt.%, in particular in the range from 80 to 99.999 wt.%, preferably in the range from 82.5 to 99.995 wt.%, preferably in the range from 85 to 99.99 wt.%, particularly preferably in the range from 87.5 to 99.98 wt.%, very particularly preferably in the range from 90 to 99.95 wt.%, even more preferably in the range from 92 to 99.9 wt.%, (ii) aluminum (Al), in particular in amounts in the range from 0.0001 to 25 wt.%, in particular in the range from 0.001 to 20 wt.%, preferably in the range from 0.005 to 17.5 wt.%, preferably in the range from 0.01 to 15 wt.%, particularly preferably in the range from 0.02 to 12.5 wt.%, very particularly preferably in the Range of 0.05 to 10 wt.%, more preferably in the range of 0.1 to 8 wt.%, (iii) optionally bismuth (Bi), in particular in amounts of up to 0.5 wt.%, preferably in amounts of up to 0.3 wt.%, preferably in amounts of up to 0.1 wt.-%, (iv) optionally lead (Pb), in particular in amounts of up to 0.5 wt.%, preferably in amounts of up to 0.2 wt.%, preferably in amounts of up to 0.1 wt.%, (v) optionally tin (Sn), in particular in amounts of up to 0.9 wt.%, preferably in amounts of up to 0.6 wt.%, preferably in amounts of up to 0.3 wt.%, (vi) optionally nickel (Ni), in particular in amounts of up to 0.1 wt.%, preferably in amounts of up to 0.08 wt.%, preferably in amounts of up to 0.06 wt.%, (vii) optionally silicon (Si), in particular in amounts of up to 0.1 wt.%, preferably in amounts of up to 0.05 wt.%, preferably in amounts of up to 0.01 wt.%, (viii) optionally magnesium (Mg), in particular in amounts of up to 5 wt.%, preferably in amounts of up to 2.5 wt.%, preferably in amounts of up to 0.8 % by weight. .

[0136] According to one embodiment of the present invention, the aluminum-containing, in particular aluminum-alloyed zinc melt ("Zn / Al melt") and / or the galvanizing bath may have a temperature in the range of 375 °C to 750 °C, in particular a temperature in the range of 380 °C to 700 °C, preferably a temperature in the range of 390 °C to 680 °C, even more preferably in the range of 395 °C to 675 °C.

[0137] Typically, the system used according to the invention is designed such that the hot-dip galvanizing device (G) is configured and / or operable and / or is configured and / or operated in such a way, in particular is controllable and / or is controlled in such a way, in particular by means of a control device, that the iron or steel component is immersed in the aluminum-containing, in particular aluminum-alloyed, zinc melt ("Zn / Al melt") and / or in the galvanizing bath, in particular immersed therein and moved, in particular for a period of time sufficient to ensure effective hot-dip galvanizing (hot-dip galvanizing), in particular for a period of time in the range of 0.0001 to 60 minutes, preferably in the range of 0.001 to 45 minutes, more preferably in the range of 0.01 to 30 minutes, even more preferably in the range of 0.1 to 15 minutes.

[0138] According to a typical embodiment of the present invention, it can be provided that the hot-dip galvanizing device (G) has at least one device for contacting and / or flushing or passing the aluminum-containing, in particular aluminum-alloyed, zinc melt ("Zn / Al melt") and / or the galvanizing bath with at least one inert gas, in particular nitrogen.

[0139] As already described above in connection with the method used according to the invention, the plant used according to the invention can in principle be designed to be continuously or discontinuously operated or can in principle be operated continuously or discontinuously.

[0140] In particular, the system used according to the invention can be designed such that the iron or steel component can be hot-dip galvanized as a single product or as a plurality of individual products or that the iron or steel component can be hot-dip galvanized as a long product, in particular a wire, pipe, sheet, coil material or the like.

[0141] Furthermore, it can be provided according to the invention that the system used according to the invention, downstream of the hot-dip galvanizing device (F) in the process direction, also has at least one cooling device (H) for cooling the iron or steel component hot-dip galvanized in the hot-dip galvanizing device (F). In particular, the cooling device (H) can be designed and / or operated in the presence of air. Furthermore, the system used according to the invention, downstream of the optional cooling device (H) in the process direction, also has at least one post-processing and / or post-treatment device (I) for post-processing and / or post-treatment of the hot-dip galvanized and cooled iron or steel component.

[0142] For further details on the system used according to the invention, in order to avoid unnecessary repetition, reference can be made to the above statements on the method used according to the invention, which apply accordingly with regard to the system used according to the invention.

[0143] Within the scope of the use according to the invention, hot-dip galvanized (hot-dip galvanized) iron or steel components can be produced which are obtainable by a process as described above and in a plant used according to the invention as described above.

[0144] As already described at the outset and in particular also documented by the exemplary embodiments according to the invention, the products obtainable within the scope of the use according to the invention are associated with particular advantages, in particular a reduced transition or heavy metal content as well as improved mechanical properties and corrosion protection properties.

[0145] As regards the hot-dip galvanized iron or steel component obtainable within the scope of the use according to the invention, said component is provided on its surface with a hot-dip galvanizing layer of 0.5 to 300 µm thickness, in particular 1 to 200 µm thickness, preferably 1.5 to 100 µm thickness, more preferably 2 to 30 µm thickness.

[0146] As regards the hot-dip galvanized iron or steel component obtainable within the scope of the use according to the invention, this hot-dip galvanized iron or steel component is provided on its surface with a hot-dip galvanizing layer, wherein the hot-dip galvanizing layer is completely free of lead (Pb) and / or nickel (Ni) originating from the flux treatment.

[0147] According to the invention, it is particularly preferred if the hot-dip galvanized iron or steel component obtainable within the scope of the use according to the invention is provided with a hot-dip galvanizing layer on its surface, wherein the hot-dip galvanizing layer is completely free of heavy metals originating from the flux treatment from the group of lead (Pb), nickel (Ni), cobalt (Co), manganese (Mn), tin (Sn), bismuth (Bi) and Antimony (Sb) is formed.

[0148] For further details on this aspect, in order to avoid unnecessary repetition, reference can be made to the above comments on the other aspects, which apply accordingly.

[0149] Further features, advantages and possible applications of the present invention will become apparent from the following description of exemplary embodiments with reference to drawings and the drawings themselves. All described and / or illustrated features, individually or in any combination, form the subject matter of the present invention, regardless of their summary in the claims and their dependencies.

[0150] It shows: Fig. 1 shows a schematic process flow of the individual stages or process steps of the process used according to the invention according to a particular embodiment of the present invention, Fig. 2 shows a schematic representation of a plant used according to the invention according to a particular embodiment of the present invention.

[0151] In the Fig. 1 The process flow diagram shown schematically shows the successive process stages or process steps a) to i), whereby the process steps b), d), f), h) and i), in particular the process steps h) and i), are optional.

[0152] According to the Fig. 1The process sequence shown in the diagram is as follows, wherein the process used according to the invention comprises the following steps successively in this order: degreasing (step a)), rinsing (step b), optional), pickling (step c)), rinsing (step d), optional), flux bath treatment (step e)), drying (step f), optional), hot-dip galvanizing (step g)), cooling (step h), optional) and post-processing or post-treatment (step i), optional).

[0153] For further details on the process sequence used according to the invention, reference can be made to the above general statements on the process used according to the invention.

[0154] In Fig. 2The system used according to the invention is shown schematically with the individual devices (A) to (I), wherein the devices (B), (D), (F), (H) and (I), in particular the devices (H) and (I), are optional.

[0155] According to the Fig. 2 The diagram of the plant used according to the invention shown comprises the following devices in the sequence listed below: degreasing device (A), optionally rinsing device (B), pickling device (C), optionally rinsing device (D), flux treatment device (E), optionally drying device (F), hot-dip galvanizing device (G), optionally cooling device (H) and optionally post-processing or post-treatment device (I).

[0156] For further details on the system used according to the invention, reference can be made to the above general statements on the system.

[0157] Further embodiments, modifications and variations of the present invention will be readily apparent and achievable to a person skilled in the art upon reading the description without departing from the scope of the present invention.

[0158] The present invention is illustrated by the following embodiments, which are not intended to limit the present invention in any way, but merely to explain the exemplary and non-limiting implementation and design. EXAMPLES OF IMPLEMENTATION General procedure for implementation (according to the invention)

[0159] Various hot-dip galvanizing cycles with sample sheets of type S235 (2 mm thickness, 100 mm x 100 mm width) are carried out according to the process sequence used according to the invention Fig. 1 and with the system used in accordance with the invention Fig. 2The flux composition and the zinc bath alloys are varied according to the following specifications.

[0160] The hot-dip galvanizing process carried out in each case comprises the following process steps in the following order (the system used according to the invention is designed accordingly): (a) alkaline degreasing treatment in a degreasing bath (15 minutes, 70 °C, composition of the degreasing bath according to Example 1 of EP 1 352 100 B1), (b) double rinsing in two consecutive rinsing baths with water, (c) acidic pickling treatment (40 minutes, 30 °C, composition of the pickling bath according to Example 1 of EP 1 352 100 B1), (d) double rinsing in two consecutive rinsing baths with water, (e) flux treatment in a flux bath according to the following specifications (3 minutes, 60 °C, immersion treatment), (f) drying treatment (260 °C hot air stream, 30 seconds), (g) hot-dip galvanizing (hot-dip galvanizing) with an aluminum-containing or aluminum-alloyed zinc melt ("Zn / Al melt") in a galvanizing bath according to the following specifications (50 seconds immersion treatment of the preheated and fluxed sheet in the galvanising bath, 450 °C), (i) cooling of the hot-dip galvanised sheet removed from the galvanising bath in air. Example series 1 (according to the invention)

[0161] Various sample sheets are subjected to hot-dip galvanizing as described above, including the corresponding pretreatment steps described above. The specifications for the flux composition and flux bath used are as follows: Flux composition:

[0162] 78.995% by weight ZnCl 2 13% by weight NH 4 Cl, 6% by weight NaCl, 2% by weight KCl, 0.005% by weight (50 ppm) AlCl 3 Flux bath:

[0163] Flux quantity / concentration (total salt content): 550 g / l Ammonia solution (5%): 10 ml per liter of flux bath to adjust (raise) the pH value pH value: 3.5 (without ammonia solution: 3.2) Wetting agent (non-ionic surfactant): 0.3% Variation of the alcohol content in the flux bath

[0164] a) 0% propanol (100% water) b) 5% propanol (40 g propanol, remainder made up to 1000 ml with water) c) 20% propanol (160 g propanol, remainder made up to 1000 ml with water) d) 71.8% propanol (574.4 g propanol, remainder made up to 1000 ml with water) e) 100% propanol Galvanizing bath

[0165] 100 ppm aluminum, 0.05 wt% bismuth, 0.3 wt% tin, 0.04 wt% nickel, balance zinc (ie ad 100 wt%) Results

[0166] ad a) The sheet metal is completely coated with salts by immersion in the flux solution. After the drying step, the surface of the component is still completely wet. A largely homogeneous zinc layer forms, but with minimal defects.

[0167] b) The sheet metal is completely coated with salts by immersing it in the flux solution. After the drying step, the surface of the component is already slightly dry. For control purposes, the sheets are weighed after pickling and drying. Compared to variant a), the flux film weighs 2.5% less, which is due to a lower residual moisture content due to faster drying. After galvanizing, a homogeneous zinc layer forms without any defects.

[0168] ad c) The sheet metal is completely coated with salts by immersion in the flux solution. After the drying step, the surface of the component is largely dry. Comparing the weight of the flux film with variant a) shows an 11.5% weight reduction. After galvanizing, a homogeneous zinc layer forms without any defects.

[0169] Ad d) The sheet metal is completely coated with salts by immersion in the flux solution. After the drying step, the surface of the component is completely dry. Comparing the weight of the flux film with variant a) shows a 15% reduction. After galvanizing, a homogeneous zinc layer forms without any defects.

[0170] Re e) The flux salts form a sediment that cannot be dissolved. Consequently, when the sheet is immersed in the flux, the steel surface is not efficiently wetted with the flux salts. During galvanizing, no reaction occurs between the zinc alloy and the steel, meaning that efficient galvanization is not possible. General findings

[0171] Under the same drying conditions (i.e., the same drying times and temperatures), the use of alcohol in the flux bath, even at low and even high concentrations, leads to faster drying of the flux film and improved galvanizing quality. This means that better drying leads to better galvanizing quality.

[0172] Even in corrosion tests (salt spray test or salt spray test according to DIN EN ISO 9227:2012), the hot-dip galvanized sheets pretreated with the alcohol-containing flux show significantly longer service life (up to 40% service life improvement) compared to hot-dip galvanized sheets pretreated with the otherwise identical flux (but without any alcohol content, i.e. purely aqueous). Example series 2 to 5 (according to the invention)

[0173] Example series 1 is repeated, but with a different composition of the galvanizing bath. Galvanizing bath for example series 2

[0174] 500 ppm aluminum, 0.05 wt% bismuth, 0.3 wt% tin, 0.04 wt% nickel, balance zinc (ie ad 100 wt%) Galvanizing bath for example series 3

[0175] 1,000 ppm aluminum, 50 ppm silicon, balance zinc (ie ad 100 wt%) Galvanizing bath for example series 4

[0176] 5.42 wt.% aluminum, balance zinc (ie ad 100 wt.%) Galvanizing bath for example series 5

[0177] Aluminium 4.51 wt.%, balance zinc (ie ad 100 wt.%) Results

[0178] Analogous results to example series 1 are obtained, whereby especially in the case of example series 4 and 5, optically significantly improved, ie particularly shiny surfaces are also obtained. Example series 6 to 10 (according to the invention)

[0179] Example series 1 to 5 are repeated, but with different flux composition (use of 0.005 wt.% or 50 ppm AgCl instead of AlCl 3 ). Results

[0180] Analogous results to example series 1 to 5 are obtained. Example series 11 to 15 (according to the invention)

[0181] Example series 1 to 5 are repeated, but with different flux composition (using a combination of 0.0025 wt.% or 25 ppm AgCl and 0.0025 wt% or 25 ppm AlCl 3 instead of AlCl 3 alone). Results

[0182] Analogous results to example series 1 to 5 are obtained. Example series 16 to 30 (comparison)

[0183] Example series 1 to 15 are repeated, but with different flux composition (complete omission of AlCl 3 and AgCl). Results

[0184] In the case of alcohol contents a) to d), highly inhomogeneous zinc layers with a significant number of defects and clearly visible defect structures result after galvanizing.

[0185] In the case of the alcohol contents of e), galvanization is not possible at all, since the flux salts form an insoluble sediment. General flux formulations (according to the invention)

[0186] In the following, general recipe information is given for typical flux compositions and flux baths used according to the invention with optimization depending on the composition of the zinc / aluminium melt. Flux composition ZnCl2 56 to 85% For AI = 4.2 to 6.2%: typically 77 to 82% For AI up to 1,000 ppm: typically 56 to 62% NH 4 Cl 10 to 44% For AI = 4.2 to 6.2%: typically 10 to 15% For AI up to 1,000 ppm: typically 38 to 44% NaCl > 0 to 6% For AI = 4.2 to 6.2%: typically 5 to 7% For AI up to 1,000 ppm: typically > 0 to 1% KCI > 0 to 2% For AI = 4.2 to 6.2%: typically 1 to 3% For AI up to 1,000 ppm: typically > 0 to 0.5% AgCl / AlCl 3 0.5 to 500 ppm

[0187] All above percentages (wt%) are based on the solid salt content (dry weight). flux bath

[0188] Total salt content (flux composition) 200 to 700 g / l, typically 450 to 550 g / l pH in the range of 25 to 5 For AI = 4.2 to 6.2%: typically 2.5 to 3.5 For AI up to 1,000 ppm: typically 4 to 5% sufficient amount of inorganic acid and ammonia solution to adjust the required pH value (fine adjustment with ammonia solution) Flux temperature in the range of 15 to 80 °C For AI = 4.2 to 6.2%: typically 50 to 70°C For AI up to 1,000 ppm: typically 35 to 60°C Wetting agent content 0.2 to 5% Solution with a proportion of propanol and / or ethanol of 0.2 to 72% For AI=4.2 to 6.2%: typically 5 to 20% For AI up to 1,000 ppm: typically 5 to 20%

Claims

1. Use of a system for hot-dip galvanizing iron or steel components, wherein the system comprises the following treatment devices in the sequence listed below: (A) at least one degreasing device for the degreasing treatment of iron or steel components; downstream in the process direction or downstream to (A) (B) optionally, at least one rinsing device for rinsing the iron or steel components degreased in the degreasing device (A); downstream in the process direction or downstream to (B) (C) at least one pickling device for the pickling treatment of the iron or steel components degreased in the degreasing device (A) and optionally rinsed in the rinsing device (B); downstream in the process direction or downstream to (C) (D) optionally, at least one rinsing device for rinsing the iron or steel components pickled in the pickling device (C); downstream in the process direction or downstream to (D) (E) at least one flux treatment device for the flux treatment of the iron or steel components pickled in the pickling device (C) and optionally rinsed in the rinsing device (D), wherein the flux treatment device contains at least one flux bath with a flux composition, wherein the flux bath comprises a liquid phase containing an alcohol / water-mixture, wherein the liquid phase of the flux bath contains the flux composition, wherein the alcohol of the alcohol / water-mixture of the flux bath is a water-miscible and / or a water-soluble alcohol and is selected from the group of linear or branched, saturated or unsaturated, aliphatic, cycloaliphatic or aromatic, primary, secondary or tertiary monohydric C1-C4 alcohols and mixtures thereof, and wherein the flux composition contains as ingredients (i) zinc chloride (ZnCl2) in amounts in the range of from 50 to 95 % by weight, (ii) ammonium chloride (NH4Cl) in amounts in the range of from 5 to 45 % by weight, (iii) at least one alkali metal and / or alkaline earth metal salt in amounts in the range of from 0.1 to 25 % by weight and (iv) at least one aluminum salt and / or at least one silver salt in amounts in the range of from 5 • 10-5 to 2 % by weight, wherein all above amounts are based on the composition and are to be selected such that a total of 100 % by weight results, and wherein the flux composition is completely free of lead chloride (PbCl2) and nickel chloride (NiCl2); downstream in the process direction or downstream to (E) (F) at least one drying device (F) for drying the iron or steel components subjected to the flux treatment in the flux treatment device (E), wherein the drying device (F) is controlled by means of a control device such that the drying treatment is carried out such that the surface of the iron or steel component has a temperature in the range of from 100 to 300 °C during drying, wherein the drying device (F) has at least one inlet for introducing and / or letting in air, and wherein the drying device (F) comprises at least one drying means; downstream in the process direction or downstream to (F) (G) at least one hot-dip galvanizing device for hot-dip galvanizing the iron or steel components subjected to the flux treatment in the flux treatment device (E) and optionally dried in the drying device (F), wherein the hot-dip galvanizing device comprises at least one galvanizing bath containing an aluminum-containing zinc melt designed for dipping iron or steel components.

2. Use according to claim 1, wherein the flux bath is acidic; and / or wherein the flux bath is adjusted to a defined and / or predetermined, especially acidic pH value, especially in the pH value range of from 0 to 6.9, preferentially in the pH value range of from 0.5 to 6.5, preferably in the pH value range of from 1 to 5.5, more preferably in the pH value range of from 1.5 to 5, even more preferably in the pH value range of from 2 to 4.5, further preferably in the pH value range of from 2 to 4; and / or wherein the flux bath is adjusted to a defined and / or predetermined, especially acidic pH value, wherein the pH value is adjusted by means of a preferentially inorganic acid in combination with a preferentially inorganic basic compound, especially ammonia (NH3).

3. Use according to claim 1 or 2, wherein the flux bath contains the alcohol / water-mixture in a weight-related alcohol / water quantity ratio in the range of from 0.5 : 99.5 to 99 : 1, especially in the range of from 2 : 98 to 95 : 5, preferentially in the range of from 5 : 95 to 90 : 10, preferably in the range of from 5 : 95 to 50 : 50, more preferably in the range of from 5 : 95 to 45 : 55, even more preferably in the range of from 5 : 95 to 50 : 50, further more preferably in the range of from 10 : 90 to 30 : 70, based on the alcohol / water-mixture; and / or wherein the flux bath contains the alcohol, based on the alcohol / water-mixture, in an amount of at least 0.5 % by weight, especially in an amount of at least 1 % by weight, preferentially in an amount of at least 2 % by weight, more preferably in an amount of at least 3 % by weight, even more preferably in an amount of at least 4 % by weight; and / or wherein the flux bath contains the alcohol, based on the alcohol / water-mixture, in an amount of up to 90 % by weight, especially in an amount of up to 70 % by weight, preferentially in an amount of up to 50 % by weight, more preferably in an amount of up to 30 % by weight, even more preferably in an amount of up to 25 % by weight; and / or wherein the alcohol of the alcohol / water-mixture of the flux bath is selected from the group consisting of methanol, ethanol, propan-1-ol, propan-2-ol, butan-1-ol, butan-2-ol and mixtures thereof.

4. Use according to any of the preceding claims, wherein the flux bath also contains at least one wetting agent and / or surfactant, especially at least one ionic or non-ionic wetting agent and / or surfactant, preferably at least one non-ionic wetting agent and / or surfactant; especially wherein the flux bath contains the at least one wetting agent and / or surfactant in amounts of 0.0001 to 15 % by weight, preferentially in amounts of 0.001 to 10 % by weight, preferably in amounts of 0.01 to 8 % by weight, more preferably in amounts of 0.01 to 6 % by weight, even more preferably in amounts of 0.05 to 3 % by weight, further preferably in amounts of 0.1 to 2 % by weight, based on the flux bath; and / or especially wherein the flux bath contains the at least one wetting agent and / or surfactant in amounts of 0.0001 to 10 % by volume, preferentially in amounts of 0.001 to 8 % by volume, preferably in amounts of 0.01 to 5 % by volume, more preferably in amounts of 0.01 to 5 % by volume, even more preferably in amounts of 0.05 to 3 % by volume, further preferably in amounts of 0.1 to 2 % by volume, based on the flux bath.

5. Use according to any of the preceding claims, wherein the flux bath contains the flux composition in an amount of at least 150 g / l, especially in an amount of at least 200 g / l, preferentially in an amount of at least 250 g / l, preferably in an amount of at least 300 g / l, more preferably in an amount of at least 400 g / l, even more preferably in an amount of at least 450 g / l, further preferably in an amount of at least 500 g / l, especially calculated as the total salt content of the flux composition; and / or wherein the flux bath contains the flux composition in an amount of 150 g / l to 750 g / l, especially in an amount of 200 g / l to 700 g / l, preferentially in an amount of 250 g / l to 650 g / l, preferably in an amount of 300 g / l to 625 g / l, more preferably in an amount of 400 g / l to 600 g / l, even more preferably in an amount of 450 g / l to 580 g / l, further preferably in an amount of 500 g / l to 575 g / l, especially calculated as the total salt content of the flux composition.

6. Use according to any of the preceding claims, where the flux composition contains as ingredients (i) zinc chloride (ZnCl2) in amounts in the range of from 55 to 90 % by weight, preferably in the range of from 60 to 85 % by weight, more preferably in the range of from 65 to 82.5 % by weight, even more preferably in the range of from 70 to 82 % by weight, (ii) ammonium chloride (NH4Cl) in amounts in the range of from 7.5 to 40 % by weight, preferably in the range of from 10 to 35 % by weight, more preferably in the range of from 11 to 25 % by weight, even more preferably in the range of from 12 to 20 % by weight, (iii) at least one alkali metal and / or alkaline earth metal salt in amounts in the range of from 0.5 to 20 % by weight, preferably in the range of from 1 to 15 % by weight, more preferably in the range of from 2 to 12.5 % by weight, even more preferably in the range of from 4 to 10 % by weight, and (iv) at least one aluminum salt and / or at least one silver salt in amounts in the range of from 5 • 10-5 to 5 • 10-3 % by weight wherein all the above amounts are based on the composition and are to be selected such that a total of 100 % by weight results, and wherein the flux composition is completely free of lead chloride (PbCl2) and nickel chloride (NiCl2).

7. Use according to any of the preceding claims, wherein the flux composition contains an alkali metal and / or alkaline earth metal chloride as the alkali metal and / or alkaline earth metal salt of component (iii); and / or wherein the flux composition contains as alkali metal and / or alkaline earth metal salt of component (iii) at least one alkali metal and / or alkaline earth metal salt of an alkali metal and / or alkaline earth metal from the group of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr) and barium (Ba) and combinations thereof; and / or wherein the flux composition comprises, as alkali metal and / or alkaline earth metal salt of component (iii), at least two different alkali metal and / or alkaline earth metal salts, especially at least two alkali metal and / or alkaline earth metal salts of an alkali metal and / or alkaline earth metal from the group consisting of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), caesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr) and barium (Ba) and combinations thereof; and / or wherein the flux composition contains as alkali metal and / or alkaline earth metal salt of component (iii) at least two alkali metal salts different from each other, especially two different alkali metal chlorides, preferentially sodium chloride and potassium chloride, especially with a sodium / potassium weight ratio in the range of from 50 : 1 to 1 : 50, especially in the range of from 25 : 1 to 1 : 25, preferentially in the range of from 10 : 1 to 1 : 10.

8. Use according to any of the preceding claims, wherein the flux composition is also completely free of cobalt chloride (CoCl2), manganese chloride (MnCl2), tin chloride (SnCl2), bismuth chloride (BiCl3) and antimony chloride (SbCl3); and / or wherein the flux composition is completely free of lead chloride (PbCl2), nickel chloride (NiCl2), cobalt chloride (CoCl2), manganese chloride (MnCl2), tin chloride (SnCl2), bismuth chloride (BiCl3) and antimony chloride (SbCl3) and / or wherein the flux composition is completely free of chlorides from the group of lead chloride (PbCl2), nickel chloride (NiCl2), cobalt chloride (CoCl2), manganese chloride (MnCl2), tin chloride (SnCl2), bismuth chloride (BiCl3) and antimony chloride (SbCl3); and / or wherein the flux composition is completely free of salts and compounds of metals selected from the group of lead (Pb), nickel (Ni), cobalt (Co), manganese (Mn), tin (Sn), bismuth (Bi) and antimony (Sb); and / or wherein the flux composition, apart from zinc chloride (ZnCl2) and aluminum and / or silver salt, especially silver chloride (AgCI) and / or aluminum chloride (AlCl3), is completely free of salts and compounds of transition and heavy metals.

9. Use according to any of the preceding claims, wherein the flux treatment device (E) comprises a device for bringing the iron or steel component into contact with the flux bath and / or the flux composition, especially a device for dipping or for spray application, preferentially a device for dipping, especially wherein the device for bringing the iron or steel component into contact with the flux bath and / or the flux composition can be controlled and / or is controlled, especially by means of a control device, such that the iron or steel component is brought into contact with the flux bath and / or the flux composition, especially is immersed in the flux bath, for a duration of 0.001 to 30 minutes, especially 0.01 to 20 minutes, preferentially 0.1 to 15 minutes, preferably 0.5 to 10 minutes, more preferably 1 to 5 minutes, and / or especially wherein the device for bringing the iron or steel component into contact with the flux bath and / or the flux composition can be controlled and / or is controlled, especially by means of a control device, such that the iron or steel component is brought into contact with the flux bath and / or the flux composition, especially is immersed in the flux bath, for a duration of up to 30 minutes, especially up to 20 minutes, preferentially up to 15 minutes, preferably up to 10 minutes, more preferably up to 5 minutes; and / or wherein the drying device (F) comprises at least one oven.

10. Use according to any of the preceding claims, wherein the aluminum-containing, especially aluminum-alloyed zinc melt ("Zn / AI-melt") and / or the galvanizing bath contains an amount of aluminum in the range of from 0.0001 to 25 % by weight, especially in the range of from 0.001 to 20 % by weight, preferentially in the range of from 0.005 to 17.5 % by weight, preferably in the range of from 0.01 to 15 % by weight, more preferably in the range of from 0.02 to 12.5 % by weight, even more preferably in the range of from 0.05 to 10 % by weight, further preferably in the range of from 0.1 to 8 % by weight, based on the aluminum-containing, especially aluminum-alloyed zinc melt ("Zn / AI-melt") and / or the galvanizing bath, especially wherein the aluminum-containing, especially aluminum-alloyed zinc melt ("Zn / AI-melt") and / or the galvanizing bath, based on the aluminum-containing, especially aluminum-alloyed zinc melt ("Zn / AI-melt") and / or the galvanizing bath, contains an amount of zinc of at least 75 % by weight, especially at least 80 % by weight, preferentially at least 85 % by weight, preferably at least 90 % by weight, and optionally at least one further metal, especially in amounts of up to 5 % by weight and / or especially selected from the group of bismuth (Bi), lead (Pb), tin (Sn), nickel (Ni), silicon (Si), magnesium (Mg) and combinations thereof, wherein all the above-mentioned amounts are to be selected such that a total of 100 % by weight results.

11. Use according to any of the preceding claims, wherein the aluminum-containing, especially aluminum-alloyed zinc melt ("Zn / AI-melt") and / or the galvanizing bath has the following composition, wherein all the amounts stated below are related to the aluminum-containing, especially aluminum-alloyed zinc melt ("Zn / AI-melt") and / or the galvanizing bath and are to be selected such that a total of 100 % by weight results: (i) zinc (Zn), especially in amounts in the range of from 75 to 99.9999 % by weight, especially in the range of from 80 to 99.999 % by weight, preferentially in the range of from 82.5 to 99.995 % by weight, preferably in the range of from 85 to 99.99 % by weight, more preferably in the range of from 87.5 to 99.98 % by weight, even more preferably in the range of from 90 to 99.95 % by weight, further preferably in the range of from 92 to 99.9 % by weight, (ii) aluminum (Al), especially in amounts in the range of from 0.0001 to 25 % by weight, especially in the range of from 0.001 to 20 % by weight, preferentially in the range of from 0.005 to 17.5 % by weight, preferably in the range of from 0.01 to 15 % by weight, more preferably in the range of from 0.02 to 12.5 % by weight, even more preferably in the range of from 0.05 to 10% by weight, further preferably in the range of from 0.1 to 8 % by weight, (iii) optionally bismuth (Bi), especially in amounts of up to 0.5 % by weight, preferentially in amounts of up to 0.3 % by weight, preferably in amounts of up to 0.1 % by weight, (iv) optionally lead (Pb), especially in amounts of up to 0.5 % by weight, preferentially in amounts of up to 0.2 % by weight, preferably in amounts of up to 0.1 % by weight, (v) optionally tin (Sn), especially in amounts of up to 0.9 % by weight, preferentially in amounts of up to 0.6 % by weight, preferably in amounts of up to 0.3 % by weight, (vi) optionally nickel (Ni), especially in amounts of up to 0.1 % by weight, preferentially in amounts of up to 0.08 % by weight, preferably in amounts of up to 0.06 % by weight, (vii) optionally silicon (Si), especially in amounts of up to 0.1 % by weight, preferentially in amounts of up to 0.05 % by weight, preferably in amounts of up to 0.01 % by weight (viii) optionally magnesium (Mg), especially in amounts of up to 5 % by weight, preferentially in amounts of up to 2.5 % by weight, preferably in amounts of up to 0.8 % by weight.

12. Use according to any of the preceding claims, wherein the aluminum-containing, especially aluminum-alloyed zinc melt ("Zn / AI-melt") and / or the galvanizing bath has a temperature in the range of from 375 °C to 750 °C, especially a temperature in the range of from 380 °C to 700 °C, preferentially a temperature in the range of from 390 °C to 680 °C, more preferably in the range of from 395 °C to 675 °C; and / or wherein the hot-dip galvanizing device (G) is designed and / or can be operated and / or is designed and / or operated, especially can be controlled and / or is controlled, especially by means of a control device, such that the iron or steel component is immersed in the aluminum-containing, especially aluminum-alloyed zinc melt ("Zn / AI-melt") and / or in the galvanizing bath, especially immersed and moved therein, especially for a period of time which is sufficient to ensure effective hot-dip galvanizing, especially for a period of time in the range of from 0.0001 to 60 minutes, preferentially in the range of from 0.001 to 45 minutes, preferably in the range of from 0.01 to 30 minutes, more preferably in the range of from 0.1 to 15 minutes; and / or wherein the hot-dip galvanizing device (G) has at least one device for contacting and / or flushing or passing through the aluminum-containing, especially aluminum-alloyed zinc melt ("Zn / AI-melt") and / or the galvanizing bath with at least one inert gas, especially nitrogen.

13. Use according to any of the preceding claims, wherein the system is designed to be operated continuously or discontinuously and / or is operated continuously or discontinuously; and / or wherein the system is designed such that the iron or steel component can be hot-dip galvanized as a single product or as a plurality of individual products or that the iron or steel component can be hot-dip galvanized as a long product, especially a wire, tube, sheet, coil material or the like.

14. Use according to any of the preceding claims, wherein the system, connected downstream or downstream of the hot-dip galvanizing device (F) in the process direction, further comprises at least one cooling device (H) for cooling the iron or steel component hot-dip galvanized in the hot-dip galvanizing device (F), especially wherein the cooling device (H) is designed and / or operated so as to be operable in the presence of air and / or especially wherein the system further comprises at least one post-processing and / or post-treatment device (l) for post-processing and / or post-treating the hot-dip galvanized and cooled iron or steel component hot-dip galvanized in the hot-dip galvanizing device (F), downstream or downstream of the cooling device (H) in the process direction.