METHOD FOR SEPARING A SOLID LAYER FROM A SOLID BODY BY LASER IRRITATION

DE502017016503D1Active Publication Date: 2024-11-07SILTECTRA GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502017016503
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2016-12-12
Filing Date
2017-03-22
Publication Date
2024-11-07
Estimated Expiration
2037-03-22

AI Technical Summary

Technical Problem

Traditional semiconductor wafering methods using diamond or slurry-based wire sawing result in material loss, surface roughness, and subsurface damage, necessitating additional polishing and grinding steps, while stress-based spalling techniques face limitations in controlling wafer thickness and surface roughness due to Wallner lines.

Method used

A laser-assisted spalling method that uses short laser pulses with high numerical aperture to define a crack propagation plane, followed by thermal stress generation with a polymer layer, allowing for precise separation of semiconductor layers with reduced surface roughness and material loss.

Benefits of technology

The method achieves efficient separation with minimal surface roughness (Ra < 1 µm) and reduced material loss, eliminating the need for extensive polishing and grinding, thereby improving the efficiency and accuracy of semiconductor wafer production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates according to the preamble of claim 1 (see e.g. DE 10 2014 214940 A1) to a method for separating at least one solid layer from a solid.

[0002] Semiconductor materials, for example, are grown in large cylinders of crystalline material, called ingots, while industrial processes often require wafer material with varying thicknesses and surface qualities. Wafering of brittle semiconductor materials is often performed using diamond- or slurry-based wire-sawing processes. These sawing processes not only result in kerf loss of potentially valuable material, but also in surface roughness and subsurface damage to the crystal. These aspects of wafering with sawing processes necessitate polishing and grinding steps in the wafer manufacturing process, resulting in additional damage and process costs.

[0003] To address these problems in conventional wafering and thinning of semiconductors, so-called kerf-lessTechnologies have been developed that promise to reduce, if not eliminate, kerf losses, as well as subsurface damage and grinding process steps. In particular, externally applied spalling processes use stresses – often temperature-induced – to separate crystalline materials along crystal planes with well-defined thicknesses. Spalling can be performed using nickel-chromium alloys, silver-aluminum paste, epoxy resin, aluminum, and nickel. Kerf-free wafering techniques have the potential to drastically reduce damage in semiconductor manufacturing processes. Stress-based separation processes, such as spalling, use externally applied stresses to separate crystalline materials along their crystal planes with well-defined thicknesses. However, after spalling, substrates exhibit so-called Wallner lines, which result from crack propagation in the crystal.

[0004] Spalling was made possible by utilizing differences in the thermal expansion coefficients between a brittle material and a polymer adhered to the material's surface. Cooling the bonded materials below the polymer's glass transition temperature induces stresses that lead to material separation along a crack plane. An advantage of this particular process over other types of spalling is that the cooling process does not result in increased diffusion of unwanted chemical components through the material, unlike high-temperature processes also used for spalling.

[0005] However, spalling processes tend to be limited in their control over the achieved wafer thickness, and tuning the vertical location of crack propagation is complicated. Furthermore, spalling creates very prominent Wallner line patterns on the surface. This pattern consists of striped grooves and bumps originating from crack propagation in the semiconductor material, allowing for inference of the crack dynamics in the substrate. Typically, the crack initiates at a certain point at the periphery and then rapidly propagates from the edge of the substrate. Wallner lines from conventional spalling surfaces greatly increase the resulting surface roughness, often to the point where additional polishing or grinding steps are required prior to further processing and the fabrication of circuitry on the substrate.

[0006] As a solution to eliminate the Wallner patterns, a process step using a laser system was introduced, which takes place before the actual spalling process. This method is called laser-assisted spalling (LAS). Here, the horizontal plane of crack propagation is defined by the processing plane of the material using short laser pulses and a high numerical aperture of the optics. Because the laser photon energy is selected below the material's band gap energy, the material is transparent to the laser radiation, allowing deep penetration into the material. By translating the focusing optics along the optical axis, the plane of laser modification can be arbitrarily determined and is defined by the focal plane of the focusing optics, which can be adjusted with micrometer precision.

[0007] The object of the present invention is to improve the known manufacturing process, in particular to make it more efficient or accelerate it. The aforementioned object is achieved according to the invention by a method according to claim 1.

[0008] Further advantageous embodiments of this invention are defined in the dependent claims.

[0009] The present invention then relates to a method for separating at least one solid layer or ply, in particular a solid disc, from a solid or donor substrate. The method according to the invention preferably comprises at least the following steps: providing a solid; creating modifications inside the solid using laser beams, wherein the modifications define a detachment region or crack guide region along which the solid layer is separated from the solid; removing material from the solid, in particular to create a circumferential depression, wherein the removal of material exposes the detachment region.

[0010] Separating the solid layer from the solid. Preferably, the separation of the solid layer from the solid is achieved by weakening the solid in the crack-guiding region by the modifications in such a way that the solid layer detaches from the solid as a result of the material removal, or by creating such a number of modifications after the material removal that the solid in the crack-guiding region is weakened in such a way that the solid layer detaches from the solid, or by creating or arranging a stress-generating layer on a surface of the solid that is inclined to the circumferential surface, in particular a flat surface, and by thermally applying the stress-generating layer to the solid, wherein the mechanical stresses create a crack for separating a solid layer.which spreads along the modifications starting from the surface of the solid exposed by the material removal, or the solid is thermally exposed, in particular cooled, after the modifications have been created, and as a result of the thermal exposure, the solid layer detaches from the solid along the crack guide region.

[0011] Thus, the step of arranging or producing a receiving layer on the solid body preferably has the feature that the receiving layer comprises or consists of a polymer material, in particular polydimethylsiloxane or an elastomer or an epoxy resin or a combination thereof, and the polymer material undergoes a glass transition as a result of thermal loading of the receiving layer for, in particular mechanical, generation of crack propagation stresses in the solid body, wherein a crack in the solid body propagates along the crack guide region due to the crack propagation stresses.

[0012] This shows, for example: Fig. 1 schematically shows the compensation of material properties by adjusting the laser exposure depending on local property differences of the material; Fig. 2a schematically shows the creation of a modification that is sufficient to lead to a crack; Fig. 2b schematically shows the creation of a modification that is more effective than the modification from Fig. 2ahas a significantly greater extension in the longitudinal direction of the solid and, after the solid layer has been cleaved off, causes the solid layer to bulge or bend; Fig. 3 schematically shows the creation of a trench in a solid, wherein the trench is preferably spaced from the outer circumferential surface of the solid; Fig. 4a schematically shows an arrangement in which particles, such as dust, accumulate in the path of the laser radiation, in particular at the intersection point of the reflected beams; Fig. 4b schematically shows an arrangement in which a purge, in particular by means of gas, such as ionized gas, is provided, which removes particles from the intersection point of the reflected beams; Fig. 5 schematically shows an arrangement according to which one or more coatings are arranged on the solid, wherein the coating(s) preferably have at least one different optical property than the solid; Fig.6a schematically shows the irradiation of laser beams at the Brewster angle; Fig. 6b: curves to illustrate the relationship between angle of incidence and reflection; Fig. 7-18: examples for calculating the optimal angle of incidence for a 1 / e2 Gaussian profile and various numerical apertures, taking into account the refractive index dependence of the surface reflection; Fig. 19a schematically shows the course of the cold split process; Fig. 19b schematically shows the course of the laser-assisted spalling process; Fig. 19c: a photograph of a surface of a solid layer exposed according to process 19a; Fig. 19d: a photograph of a surface of a solid layer exposed according to process 19b; Fig. 20a: f: SEM images of surfaces; Fig. 21a: a microscopic image of a surface after spalling; Fig. 21bRaman spectra from three different locations in 6H silicon carbide; Fig. 22an example of a laser beam profile; and Fig.23a schematically shows an example of the bending of the produced solid-state layer resulting from a first number of modifications and / or modification layers; and Fig. 23b schematically shows a further example of the bending of the produced solid-state layer resulting from a second number of modifications and / or modification layers, wherein the second number is greater than the first number, and Fig. 24a shows a schematic structure of a Raman instrument as is preferably used according to the invention, in particular as it is preferably a component of the device according to the invention; Fig. 24b SiC, various exemplary oscillation states of the lattice oscillations of Figs. 25a and 25b two diagrams illustrating doping concentrations in a solid; Fig. 26a shows a feedforward process according to the invention, and Fig. 26b shows a feedback process according to the invention.

[0013] In Fig. 1A schematic diagram of a structure for carrying out a method for separating at least one solid layer 14 from a solid body 1 is shown. Modifications 2 define a crack-guiding region 4 for guiding a crack to separate a solid portion 14, in particular a solid layer, from the solid body 1. Because laser beams 10, 11 are shown at different locations on the solid body 1, it is clear that the solid body 1 is moved relative to a laser irradiation device 8. The laser beams 10 and 11 shown thus represent situations at different times.Basically, laser beams 10 are generated by means of the laser irradiation device 8 to generate at least one modification 2, wherein the laser irradiation device 8 is adjusted for the defined modification generation depending on at least one parameter, namely the transmission of the solid body 1 at defined locations and for a defined solid body depth. In the illustration according to . Fig. 1 Laser beams 10, 11 thus represent laser beams with different properties or with at least one different property. The property that changes from laser beam 10 to laser beam 11 takes into account the changed material properties in the respective exposed region of solid body 1. In the case shown, laser beam 11, for example, strikes a region of solid body 1 that has a changed transmission, which can result, for example, from a doping spot.

[0014] Preferably, after the creation of the modifications 2, the separation of the solid layer 14 from the solid 1 takes place according to the representation of Fig. 19b .

[0015] Fig. 2a shows a situation in which modifications 2 are produced with a first extension in the longitudinal direction L of the solid body 1. The longitudinal direction L extends according to the invention orthogonally or substantially orthogonally to the irradiation surface 17 of the solid body 1, wherein the irradiation surface 17 of the solid body 1 is a component of the solid body layer 14 after the separation of the solid body layer 14. This preferably applies to all embodiments described in this document. The according to Fig. 2a The modifications 2 produced are sufficient to guide a crack to separate the solid layer 14.

[0016] Fig. 2b shows an embodiment according to which the modifications 2 produced have a Fig. 2ahave a greater extent in the longitudinal direction L. Additionally or alternatively, several, in particular two or three or more than two or three, layers of modifications 2 can be produced at least in sections.

[0017] This is advantageous because a greater than necessary extension of the laser layer in the beam direction (depth or solid length) can increase the stress generated by the laser layer in the unmodified material. Thus, more material can preferentially undergo a phase transition or be amorphized or otherwise modified than necessary for the polymer split (see [Fig. Fig. 19bThis increased stress serves to promote the spontaneous splitting of the material (without polymer). The laser parameters or laser beam parameters or parameters with which the laser application device is configured - for the spontaneous splitting and the polymer process - can therefore differ considerably, e.g., in the required numerical aperture and / or pulse length and / or pulse energy. A larger expansion of the laser layer leads to a higher pressure in the solid, thereby increasing the probability of spontaneous splitting. Furthermore, this embodiment is advantageoussince a solid layer 14 can be produced as a bent or curved solid layer 14. Thus, this method can preferably also be used to produce at least one solid layer 14 that is at least partially curved or bent. To produce a curved or bent solid layer (or bent or curved wafer), the method preferably comprises at least the following steps: moving the solid 1 relative to a laser irradiation device 8, successively generating laser beams 10 by means of the laser irradiation device 8 to produce at least one modification 2 in the interior of the solid, wherein the modifications 2 define a crack-guiding region 4 for guiding a crack to separate a solid portion 6, in particular a solid layer, from the solid 1, wherein the modifications cause a pressure increase in the solid,wherein the solid layer 14 is separated from the solid 1 due to the pressure increase along the crack propagation region 4, wherein at least a portion of the modifications 2 as a component of the solid layer 14 is separated from the solid 1, wherein the solid layer 14 is transformed into a curved or arched shape due to the modifications 2, wherein the further surface portion 16 of the solid layer resulting from the crack propagation region 4 is thus at least partially convex.

[0018] Fig. 3shows an arrangement according to which a crack-guiding region 4 is created in the solid body 1, at least in sections and preferably circumferentially, a trench 26 is created, starting from the irradiation surface 17 in the longitudinal direction L of the solid body 1. After the trench 26 has been created, the solid body layer 14 can be separated from the solid body by creating further modifications 2 using laser beams 10, which are preferably also introduced via the irradiation surface 17. Alternatively, a stress-generating layer 18 is preferably arranged or created at least on the region enclosed, surrounded, or delimited by the trench 26, in particular on the surface of the subsequent solid body layer 14.

[0019] The stress-generating layer preferably consists of a polymer material, in particular PDMS, and in a further step is preferably thermally exposed at least partially and particularly preferably completely, in particular cooled, in particular cooled below its glass transition temperature. This preferably applies to all embodiments described herein in which a stress-generating layer is used or employed.

[0020] As a result of the stress generation, a crack separates the solid layer 14 from the remaining solid 1.

[0021] Preferably, a further step involves a surface treatment of the solid body 1. Preferably, the frame 28 resulting between the trench 26 and the surrounding surface and / or the surface of the solid body 1 exposed by separating the solid body layer 14 is smoothed, in particular ground, lapped, polished, or etched. Preferably, the frame 28 and the exposed surface are treated, in particular by machining, such that their surfaces lie in the same plane.

[0022] Thus, according to the invention, a method is provided for separating at least one solid layer or solid layer, in particular a solid disc, 14 from a solid or donor substrate 1, which method preferably comprises at least the following steps: providing a solid 1, producing modifications 2 in the interior of the solid 1 by means of laser beams 10, wherein the modifications 2 predetermine a detachment region or crack guide region along which the solid layer 14 is separated from the solid 1, removing material at the edge of the solid 1, in particular for producing a circumferential depression 12, wherein the material removal takes place in the longitudinal direction of the solid, wherein the detachment region is exposed by the material removal, and separating the solid layer from the solid.

[0023] This is advantageous because laser processing up to the edge is problematic, and thus the produced solid-state layer 14 also has very homogeneous properties in its edge region. The basic concept presented here thus comprises laser ablation / grinding / material removal from above to create a notch or trench, whereby the previously produced laser layer is opened or exposed. Subsequently, the solid-state layer 14 or the target wafer with the stress-generating layer 18 is lifted out. The remaining edge or frame 28 can then be ground away again during further surface preparation. Thus, the laser layer can be exposed by ablation from above, in particular by waterjet cutting or laser ablation, and edge effects during polymer splitting can be avoided.

[0024] Fig. 4ashows an arrangement in which particles, such as dust, accumulate at the intersection point of the reflected radiation, marked with the reference numeral 30, and thus negatively influence the generation of modifications.

[0025] Fig. 4b shows an arrangement in which a flushing device 32 or flushing system is provided. Thus, a fluid, in particular a gas and preferably an ionized gas, is preferably supplied to the intersection point 30 in order to flush away the particles accumulating at the intersection point 30 by means of the fluid flow.

[0026] Thus, a method for separating at least one solid layer or solid layer, in particular a solid disc, 14 from a solid or donor substrate 2 is provided, which preferably comprises at least the following steps: providing a solid 1, adjusting a flow behavior of a gas, in particular air, located between the solid and the laser exposure device 8, in particular in the region of the radiation path, to prevent dust accumulation in the region of the laser radiation, generating modifications 2 in the interior of the solid 1 by means of LASER beams 10 of a laser exposure device 8, wherein the modifications 2 predetermine a detachment region or crack guidance region along which a separation of the solid layer 14 from the solid 1 takes place and separating the solid layer from the solid.This solution is advantageous because high laser intensities statically charge dust, and this dust can be flushed out of the area between the lens and the workpiece by flushing, particularly with ionized gas. The gas flush thus expels the dust from the space between the lens 9 of the laser irradiation device 8 and the workpiece or solid body 1. Additionally or alternatively, the fluid flow, particularly the gas flow, can be directed through the lens to generate a cooling effect against absorbed power. Thus, the lens is preferably designed to conduct a fluid, particularly the flushing fluid.

[0027] Furthermore, or additionally, compensation for spherical aberrations can be performed on the lens. This changes the focus at the surface (incorporating the material with a different refractive index through which it passes), which worsens the focus in air and thus results in lower intensity, which in turn leads to a reduced particle suction or vacuum effect. Additionally or alternatively, reduced reflection at the surface can be achieved. This can be achieved, for example, by applying certain layers or coatings, particularly spin coating, and / or by Brewster irradiation with polarized light.

[0028] Fig. 5shows a schematic arrangement according to which the solid body 1 is provided with at least one coating 34. The coating 34 can be single-layered or multi-layered. The coating preferably has a refractive index difference from the refractive index of the material of the solid body 1; in particular, the refractive index of the material of the solid body 1 is preferably higher than that of the coating 34. It is also conceivable for the coating 34 to be constructed from multiple layers, with at least two of the multiple layers preferably having a refractive index difference. The refractive index of the respective layer that is arranged closest to the solid body 1 is preferably greater than the refractive index of a layer that is further away from the solid body 1.

[0029] This schematic structure thus makes it possible, according to the invention, to provide a method for separating at least one solid layer or solid ply, in particular a solid wafer, 14 from a solid or donor substrate 1. This method preferably comprises at least the following steps: Providing a solid 1, wherein the solid 1 has at least one coating 34 whose refractive index is different from the refractive index of the surface of the solid 1 on which the coating 34 is arranged, or wherein a coating 34 is produced on the solid 1 whose refractive index is different from the refractive index of the surface of the solid 1 on which the coating 34 is arranged, Creating modifications 2 in the interior of the solid 1 by means of LASER beams 10 of a laser application device 8, wherein the modifications 2 create a crack guiding region 4 (cf. analogous Fig. 1) is specified, along which a separation of the solid layer 14 from the solid body 1 takes place.

[0030] The coating can be created using spin coating, for example. For example, a solvent mixed with nanoparticles of materials with a high refractive index applies one or more thin (sub-wavelength) layers with a slightly higher refractive index to the solid body 1 or workpiece 1. This creates an interface with a reduced difference in refractive index, less reflection on the surface, less contamination, and more power in the material for more efficient material processing. Spin coating is advantageous because it is quick and inexpensive. Possible nanoparticles include, among others, silicon (n=3.55), silicon carbide (n=2.6), titanium oxide (n=1.8), glass (n=1.5), and Al2O3 (n=1.72). In the case of multiple layers, with gradually increasing refractive index for even more efficient refractive index adaptation and anti-reflective effect, a multi-layer process is conceivable.Purely by way of example, a layer arrangement could then be produced which consists of the following layers or layers: 1st layer: Si, 2nd layer: SiC, 3rd layer: TiO2, each layer preferably 50-400 nanometers thick. This process is further advantageous because spin-coating of such layers can also compensate for the smallest roughness on the material surface (better material coupling due to less scattering at the interface, better wavefront overlap in the focus in depth, and thus lower laser power is required, which leads to more efficient processing because of a higher multiphoton transition probability). The spin-coating layer or the creation of a coating 34 can be applied as part of the step for surface conditioning and reprocessing the surface on the ingot or solid body 1 after the split or separation of the solid body layer 14.Thus, a grinding / lapping / etching or polishing step can be carried out first, followed by, or in combination with, one of the preceding steps by the spin-coating step or the coating step which applies the thin layer or coating 34.

[0031] Fig. 6shows a schematic of an arrangement for coupling laser beams 10, with this arrangement reducing reflection. Preferably, the laser beams 10 are coupled at the Brewster angle. The Brewster angle is an angle of incidence for light of a specific polarization (E vector points into the material, not along the surface) at which no reflection occurs. The prerequisites for this are that the light is irradiated at an angle dependent on the difference in refractive index between air and material. Furthermore, the light must be polarized (usually the case with laser light, but requires single-mode lasers and not photonic crystal fibers). The Brewster angle coupling thus serves to minimize back reflections. If irradiation occurs at the Brewster angle, the 30% surface reflection can be used almost entirely for material processing deep within the material.

[0032] Irradiation at the Brewster angle is complicated because the different beam components travel different distances in the high-refractive medium. The focus must therefore be adjusted by increasing energy and / or by beam shaping. Beam shaping is preferably carried out, for example, using one or more diffractive optical elements (DOEs), which compensate for this difference depending on the laser beam profile. The Brewster angle is relatively large, which, with a high numerical aperture, places demands on the optics and their dimensions as well as the working distance. Nevertheless, this solution is advantageous because reduced reflections at the surface also contribute to reduced surface damage, as the light intensity couples better into the material. For the purposes of this invention, laser beams 10 can also be irradiated at the Brewster angle or substantially at the Brewster angle in all other embodiments disclosed in this document.For Brewster angle coupling, reference is hereby made to the document "Optical Properties of Spin-Coated TiO2 Antireflection Films on Textured Single-Crystalline Silicon Substrates" (Hindawi Publishing Corporation International Journal of Photoenergy, Volume 2015, Article ID 147836, 8 pages, http: / / dx.doi.org / 10.1155 / 2015 / 147836). This document is incorporated in its entirety by reference into the present patent application. The aforementioned and incorporated document discloses, in particular, calculations for the optimal angle of incidence for various materials and thus refractive indices. The energy of the laser or laser irradiation device 8 is adjusted not so much as a function of the material, but rather according to the possible transmission at a specific angle. Therefore, if the optimal transmission is, for example, 93%, these losses must be reduced compared to tests with perpendicular irradiation and losses of, for example,then 17% must be taken into account and the laser power adjusted accordingly.

[0033] For example, 83% transmission perpendicularly compared to 93% at an angle means that to achieve the same energy at depth, only 89% of the laser power used for perpendicular irradiation is required (0.83 / 0.93=0.89). In the context of the invention, the portion of the oblique irradiation therefore serves preferentially to reduce light loss through surface reflection and to direct more light into the depth. A possible downstream problem that can arise in certain constellations is that the focus can acquire a "skewed" profile at depth, and thus the achieved intensities – the key parameter for multiphoton processing – are lower again, possibly even lower than with perpendicular irradiation, where all beam components follow the same optical path in the material.This can then preferably be achieved by one or more diffractive optical elements, or one or more continuous wedges—and / or other optical elements—in the beam path, which compensate for these additional paths and / or the influence on the individual beams—particularly different spherical aberrations across the beam profile. These DOEs can be calculated numerically using suitable software solutions (e.g., Virtuallab from Lighttrans, Jena) and then manufactured or provided.

[0034] Thus, the present invention provides a method for separating at least one solid layer or ply, in particular a solid disc, 14 from a solid or donor substrate 1. The method according to the invention preferably comprises at least the following steps: providing a solid 1, creating modifications 2 inside the solid 1 using laser beams 10 from a laser irradiation device 8, wherein the modifications 10 define a crack guide region along which the solid layer 14 is separated from the solid 1, wherein the laser radiation radiates onto the solid 1 at the Brewster angle or with a deviation in the range of -10° to +10° from the Brewster angle. Furthermore, the method preferably comprises the step of separating the solid layer 14 from the solid 1.

[0035] Within the scope of the present invention, it was thus recognized that a large difference in refractive index between air and material results in power losses of up to 30% with perpendicular irradiation. With a 100W laser, 30W is therefore unavailable for material processing or has other effects. For example, it was further recognized that contamination can occur on the optics, as with so-called "optical tweezers." At high laser intensities, the smallest dust particles in both air and liquids always migrate to the focus of the laser beam (highest intensity) – reflected power at the surface has a focus in the air or near the optics, and the dust is driven / pulled toward the optics. Furthermore, it was recognized that at 100W laser power and 97% transmission at the lens, significant heat (3W) can also enter the lens, which must be dissipated / compensated to avoid thermal damage / changes in the process.It was also recognized that high power levels carry the risk of surface damage. This is because the absorption of the material can be increased due to surface conditions. Therefore, the smallest dust particles can first burn in the laser beam 10 and then form absorption nuclei, which can lead to further damage due to absorption. Furthermore, it was recognized that high power levels can be distributed across multiple foci in the focal plane using diffractive optical elements (DOEs). DOEs exhibit interference phenomena even before the focal plane. It was recognized that interference at the surface can generate local intensity maxima before the focal plane, which can lead to surface damage and reduced transmissivity for laser radiation for deep processing. Furthermore, it was recognized that some materials (e.g., SiC) exhibit local differences in refractive index and other material properties (e.g.,Absorption, transmission, scattering), e.g., due to material doping (frequent occurrence: doping spot). Furthermore, it was recognized that, depending on the surface roughness of the material at the laser coupling surface, the laser wavefront can be significantly impaired in the depth of the material, resulting in reduced focus intensity (lower multiphoton transition probability), which in turn would result in higher intensities with the aforementioned problems.

[0036] Individual, several, or all of these problems can be addressed by individual or combinations of the methods disclosed here. Thus, the present invention can preferably be understood as a method for separating at least one solid layer from a solid body. In this method, the modifications 2 preferably predetermine a crack guiding region 4 for guiding a crack for separating a solid portion 6, in particular a solid layer, from the solid body 1. The method according to the invention preferably comprises at least the steps of: moving the solid body 1 relative to a laser irradiation device 8, successively generating laser beams 10 by means of the laser irradiation device 8 to generate at least one modification 2 in each case, and separating the solid layer from the solid body.

[0037] According to the invention, a spalling process is described that scales favorably, particularly for large-area semiconductor substrates with diameters of up to 300 mm or more. To eliminate the Wallner line patterns, a laser conditioning process is used, particularly with a high numerical aperture, at photon energies preferably below the material's band gap energy. This process leads to multiphoton interactions in the material and, after the spalling process, yields a surface roughness of preferably Ra <1 µm.

[0038] Preferably, one or more of the aforementioned solutions according to the invention can be combined with one another, as this can result in even better solid layer production or solid layer separation. Thus, according to the method according to the invention, the laser application device 8 is adjusted for defined modification generation depending on at least one parameter, namely the transmission of the solid at defined locations and for a defined solid depth, and / or the modifications cause a pressure increase in the solid, wherein the solid layer is separated from the solid as a result of the pressure increase along the crack propagation region by crack propagation, wherein preferably at least a portion of the modifications is separated from the solid as a component of the solid layer, and wherein the solid layer is preferably converted into a curved or arched shape due to the modifications.wherein the further surface portion of the solid layer resulting from the crack-guiding region is thus at least partially convex and / or the solid has at least one coating whose refractive index differs from the refractive index of the surface of the solid on which the coating is arranged, or a coating is produced on the solid whose refractive index differs from the refractive index of the surface of the solid on which the coating is arranged, and / or the laser radiation radiates onto the solid at the Brewster angle or with a deviation in the range of -5° to +5°, in particular with a deviation in the range of -4° to +4° or with a deviation in the range of -3° to +3° or with a deviation in the range of -2° to +2° or with a deviation in the range of -1° to +1° from the Brewster angle,and / or the method additionally or alternatively comprises one or more of the following steps: removing material from the solid body 1, in particular to create a circumferential depression 12, wherein the material removal takes place in the longitudinal direction of the solid body, wherein the crack guide region is exposed by the material removal, or adjusting a flow behavior of a gas, in particular air, located between the solid body and the laser application device 8, in particular in the region of the radiation path, to prevent dust accumulation in the region of the laser radiation.

[0039] The Figures 7-18 show examples for the calculation of the optimal angle of incidence for a 1 / e2 Gaussian profile and different numerical apertures taking into account the refractive index dependence of the surface reflection.

[0040] The Figures 7-10 show the trends when using silicon carbide (n=2.7)

[0041] Goal: Maximize the laser power coupled into the sample, ideally by exploiting the Brewster angle for minimal surface reflection with p-polarized light. Result: For an NA of 0.8, Brewster coupling is not worthwhile (the beam cone already couples almost below Brewster on the outside). Smaller NAs can benefit from it, especially NAs of 0.2. Higher NAs have an ideal angle somewhere in between.

[0042] Fig. 7 shows in the upper figure: relative coupled power over angle of incidence for Gaussian profile and in the lower figure: reflection coefficient for p-(red) and s-(blue) polarized light and angular Gaussian profile for depicted NA=0.2 (green), optimal angle of incidence here 63.8°.

[0043] Fig. 8shows in the upper figure: relative coupled power over angle of incidence for Gaussian profile and in the lower figure: reflection coefficient for p-(red) and s-(blue) polarized light and angular Gaussian profile for depicted NA=0.4 (green), optimal angle of incidence here 52.5°.

[0044] Fig. 9 shows in the upper figure: relative coupled power over angle of incidence for Gaussian profile and in the lower figure: reflection coefficient for p-(red) and s-(blue) polarized light and angular Gaussian profile for depicted NA=0.6 (green), optimal angle of incidence here 35.6°.

[0045] Fig. 10 shows in the upper figure: relative coupled power over angle of incidence for Gaussian profile and in the lower figure: reflection coefficient for p-(red) and s-(blue) polarized light and angular Gaussian profile for depicted NA=0.8 (green), optimal angle of incidence here 0°.

[0046] The Figures 11-14show the trends when using silicon (n=3.6).

[0047] The goal here is to maximize the laser power coupled into the sample, ideally by exploiting the Brewster angle for minimal surface reflection with p-polarized light. The result: For an NA of 0.8, Brewster coupling is not worthwhile (the beam cone already couples almost below Brewster on the outside); smaller NAs can benefit from it, especially NAs of 0.2; higher NAs have an ideal angle in between.

[0048] Fig. 11 shows in the upper figure: relative coupled power over angle of incidence for Gaussian profile for silicon and in the lower figure: reflection coefficient for p-(red) and s-(blue) polarized light and angular Gaussian profile for depicted NA=0.2 (green), optimal angle of incidence here 67.9°.

[0049] Fig. 12shows in the upper figure: relative coupled power over angle of incidence for Gaussian profile for silicon and in the lower figure: reflection coefficient for p-(red) and s-(blue) polarized light and angular Gaussian profile for depicted NA=0.4 (green), optimal angle of incidence here 57.4°.

[0050] Fig. 13 shows in the upper figure: relative coupled power over angle of incidence for Gaussian profile for silicon and in the lower figure: reflection coefficient for p-(red) and s-(blue) polarized light and angular Gaussian profile for depicted NA=0.6 (green), optimal angle of incidence here 43.6°.

[0051] Fig. 14 shows in the upper figure: relative coupled power over angle of incidence for Gaussian profile for silicon and in the lower figure: reflection coefficient for p-(red) and s-(blue) polarized light and angular Gaussian profile for depicted NA=0.8 (green), optimal angle of incidence here 0°.

[0052] The Figures 15-18 show the progressions when using sapphire / ALO (n=1.72)

[0053] The goal here is to maximize the laser power coupled into the sample, ideally by exploiting the Brewster angle for minimal surface reflection with p-polarized light. The result: For an NA of 0.8, Brewster coupling is not worthwhile (the beam cone already couples almost below Brewster's angle on the outside). Smaller NAs can benefit from it, especially NAs of 0.2. Higher NAs have an ideal angle somewhere in between, with NAs of 0.6 requiring almost no angle for irradiation.

[0054] Fig. 15 shows in the upper figure: relative coupled power over angle of incidence for Gaussian profile for ALO and in the lower figure: reflection coefficient for p-(red) and s-(blue) polarized light and angular Gaussian profile for depicted NA=0.2 (green), optimal angle of incidence here 54.9°.

[0055] Fig. 16shows in the upper figure: relative coupled power over angle of incidence for Gaussian profile for ALO and in the lower figure: reflection coefficient for p-(red) and s-(blue) polarized light and angular Gaussian profile for depicted NA=0.4 (green), optimal angle of incidence here 41.2°.

[0056] Fig. 17 shows in the upper figure: relative coupled power over angle of incidence for Gaussian profile for ALO and in the lower figure: reflection coefficient for p-(red) and s-(blue) polarized light and angular Gaussian profile for depicted NA=0.6 (green), optimal angle of incidence here 14.5°.

[0057] Fig. 18 shows in the upper figure: relative coupled power over angle of incidence for Gaussian profile for ALO and in the lower figure: reflection coefficient for p-(red) and s-(blue) polarized light and angular Gaussian profile for depicted NA=0.8 (green), optimal angle of incidence here 0°.

[0058] Figure 19aOutlines a standard procedure for laser-free spalling of large-area substrates. The wafer samples typically used have sharp edges to avoid complications caused by rounded edges. Rounded edges are used on conventional wafers to prevent cracks from appearing at the wafer edges, which can propagate inward and disrupt the substrate and manufacturing processes on it.

[0059] The process preferably proceeds as follows: after a standard cleaning procedure, the wafers are coated with a primer layer to improve surface adhesion and a sacrificial layer to facilitate polymer-wafer separation at the end. The wafer is then coated with a PDMS (polydimethylsiloxane) polymer film of varying thickness and a PDMS adhesive containing a platinum polymerization catalyst.

[0060] The samples are then pre-cooled to a temperature just above the polymer glass transition temperature before being immersed in liquid nitrogen. Depending on the sample size, the sample will reach liquid nitrogen temperature up to 20 seconds later. The system is in thermal equilibrium at this point. The semiconductor layers then separate in a spontaneously occurring spalling event. The spalling process is induced by the polymer glass transition, and as a result, the Young's modulus in the polymer increases greatly. The additional difference in the coefficients of thermal expansion (CTE) between semiconductor and polymer then induces sufficient stress to separate the crystal horizontally. Importantly, the process requires a relative contraction of the polymer with respect to the semiconductor.The next process step is to immerse the semiconductor parts with attached PDMS foils in a separation bath, which ultimately dissolves the sacrificial layer and thus enables the recycling of the polymer as well as the preparation of the semiconductor wafers for further processing steps.

[0061] Fig. 19a This shows an illustration of conventional spalling of substrates with an ensemble of preferably two stress layers, i.e., polymer films. The films are attached to both sides of the substrate, followed by a rapid cooling step to induce thermal cycling, followed by cracking and separation of the substrate.

[0062] The laser-assisted spalling process, shown in Figure 19b, is remarkably similar. The main difference is an additional laser processing step in which a laser beam is focused on a defined plane or pattern within the sample and then scanned. The laser layer created in this way then defines the plane of crack formation and thus also separation in the subsequent spalling process.

[0063] Fig. 19b This shows the laser-assisted spalling process. In addition to the process steps shown in Figure 19a, a further process step is used to create a structurally weakened layer in the material using a modification layer or laser system generated by laser beams. This layer defines a preferred plane for spalling crack propagation.

[0064] A typical resulting wafer surface from laser-free spalling is shown in Figure 19cA pattern of Wallner lines results from the crack propagation within the material. Grooves can be identified on the surface of the material, which trace the crack behavior along the parting line in the material. Cracks originate at the edges of the sample and migrate inward, creating a detailed pattern, as shown in Figure 19cThe fourfold symmetry of the pattern is a consequence of the fourfold crystal symmetry in silicon, with a singularity or center of the crack waves in the middle of the sample. However, to compete technologically with wire sawing processes, the surface quality after separation is crucial for any spalling process. The resulting total thickness variation (TTV) of spalled surfaces without a laser process is usually far above industry requirements. The typical TTV of spalling processes is on the order of 50 µm, which would require grinding steps before further processing, which would drive up costs. Using the LAS process instead results in surface roughness values ​​of Sa <1 µm being achieved. Sa is the arithmetic mean of the absolute values ​​of the surface coordinates z (x, y).

[0065] Fig. 19cThis image shows a picture of one half of a 300 mm silicon wafer after separation using conventional spalling. Wallner lines are clearly visible as crack grooves and are indicative of high surface height variation (TTV).

[0066] Fig. 19d shows an image of one half of a 300 mm silicon wafer after laser-assisted spalling. The surface is homogeneous with a surface roughness below 1 µm and no visible streaks from crack propagation. The vertical line on the left side of the substrate is due to a limitation of the travel of the laser system's substrate holding table.

[0067] The Figures 20a-f show an overview of the material surfaces after laser-assisted spalling. Fig. 20a shows a silicon surface of the Figure 19d shown sample, with a surface roughness of Sa = 0.79µm. Fig. 20bshows a sapphire (Al 2 O 3 ) substrate surface (C-plane) after laser-assisted spalling, with a surface roughness of Sa = 1.96µm. Fig. 20c and Fig. 20d show surfaces of silicon carbide polymorphs 4H and 6H (both with N-doping) after laser-assisted spalling with surface roughnesses Sa = 1.85µm and Sa = 1.29µm. Fig. 20e shows an example of spalling of non-crystalline material, surface of polycrystalline Al 2 O 3 , with a surface roughness Sa = 3.89µm. Fig. 20f shows quartz glass, principle study, experiment of laser-assisted spalling, with surface roughness of Sa = 6.89µm.

[0068] Fig. 21a shows a microscopic image of a surface after spalling. Fig. 21b shows Raman spectra from three different locations in 6H-silicon carbide. The Raman spectra from the darker area (on the right side of Fig. 21a) are curve K1 and curve K2, with curve K3 as Raman spectrum from the brighter area on the left side in Fig. 21a The peak height is reduced for the darker areas for almost all peaks and at position 2 in the darker area no Raman peaks are visible anymore.

[0069] Fig. 22 shows another additional or alternative beam profile. According to the invention, the laser beam profile is adaptable for Brewster exposure with high numerical apertures. Thus, at high NA, more intensity can result in the flanks of the incident laser beam profile. In the extreme case, this is a kind of donut profile with a clear intensity minimum in the center. However, it is also conceivable for the laser beam profile to be designed as a Gaussian profile flattened in the center. This makes preferential use of the fact that at high NA, the edge regions of the laser profile can already approach the Brewster angle. Fig. 22 The example profile shown could thus preferably be generated with a relatively higher intensity component (compared to the other embodiments) in the flanks.

[0070] Fig. 23 a describes a first solid-state generation configuration. According to this configuration, it is possible to separate the solid-state layer 14 from the solid-state 1. According to this configuration, a first number of modifications 2 are created in the solid-state. The modifications 2 preferably already cause a bending of the separated solid-state layer 14.

[0071] In Fig. 23ba second solid-state production configuration is shown. According to this configuration, it is also possible to separate the solid-state layer 14 from the solid-state. According to this configuration, however, a second number of modifications 2 is produced in the solid-state 1. The second number of modifications 2 is preferably greater than the first number of modifications. Additionally or alternatively, it is possible for the configuration to have a plurality of modification layers 2.1, 2.2 or to have more modification layers 2.1, 2.2 than the first configuration, in which a plurality of modification layers can also be provided. Additionally or alternatively, it is also conceivable for individual or the majority of the modifications 2 to be more thicker in the second configuration than in the first configuration. Thicker in this case preferably means that the individual modifications each extend over a larger volume than in the first configuration.The laser beams 10 preferably penetrate into the solid body 1 in the longitudinal direction of the solid body 1 or at an angle of up to 60° inclined to the longitudinal direction L of the solid body 1 via a, in particular flat, surface, which is preferably part of the solid body layer, and the crack guidance region 4 is then preferably formed from several layers of modifications 2. The layers are preferably produced spaced apart or offset from one another in the longitudinal direction L. Preferably, at least several of the modifications 2 have an extent in the longitudinal direction L of between 1 and 50 µm, and / or the laser beams 10 are preferably introduced into the solid body 1 to produce the modifications 2 in such a way that the numerical aperture is less than 1, preferably less than 0.9 or less than 0.8 or less than 0.7 or less than 0.6 or less than 0.5.

[0072] Thus, the invention describes a method for separating at least one solid layer from a solid, wherein the modifications define a crack guiding region for guiding a crack for separating a solid portion, in particular a solid layer, from the solid, at least comprising the steps of: moving the solid relative to a laser irradiation device, successively generating laser beams by means of the laser irradiation device to generate at least one modification each, wherein the laser irradiation device is adjusted for defined modification generation depending on at least one parameter, in particular the transmission of the solid, at defined locations and for a defined solid depth,whereby inhomogeneities of the solid in the area of ​​the exposed surface and / or in the area of ​​the exposed volume of the solid are compensated by the adjustment of the laser exposure device, separating the solid layer from the solid.,

[0073] Fig. 24ashows a Raman instrument 58. The Raman instrument 58 shown here has a laser 60 for emitting radiation. The radiation is preferably fed to an optical system for excitation by means of at least one optical fiber 61 and is preferably focused by this optical system, in particular lens 64, in particular focused into the solid. This radiation is at least partially scattered, with light components having the same wavelength as the radiation emitted by the laser being filtered out, preferably by means of a filter device or excitation filter 62. The remaining radiation components are then fed to a spectrograph 68 and captured by a camera device, in particular a CCD detector 70, and evaluated or processed by a control device 14, 72, in particular a computer.

[0074] Atomic vibrations in the crystal are thus preferably excited by a laser, preferably an external one or, even more preferably, another laser. These vibrations are generated by light scattering off crystal atoms, resulting in observable scattered light, which has a photon energy that is altered by the amount of vibrational energy. If multiple excitable vibrations are present, multiple peaks will appear in the spectrum of the scattered light. The resulting Raman scattering spectrum can then be examined more closely using a spectrometer (grating spectrometer) (so-called Raman spectroscopy). With this method, the local conditions in the crystal are imposed on the shape of the individual Raman lines, and by analyzing the shape of the Raman line, the degree of doping can be deduced.

[0075] Fig. 24bshows what possible lattice vibrations in SiC look like, where these modes are determined by crystal symmetry and directions and can also be excited simultaneously. The views shown extend along the crystal axis A. Here, vibrations of the atoms are only possible in certain directions, with the directions determined by the symmetry of the crystal.

[0076] Fig. 25a shows a section of a Raman curve of a nitrogen-doped 4H silicon carbide solid (example spectrum for Raman on doped SiC). The shape of the LO(PC) mode is used and fitted to measure the doping concentration. Lower panel: fitting residual.

[0077] Fig. 25b shows a smaller section of the Raman curve.

[0078] As shown, a direct method to determine the dopant concentration using Raman measurements results from a shape measurement and subsequent fit to the LO(PC) mode.

[0079] In general, the goal is to set the optimal (smallest possible, shortest possible) crack path in the material by adjusting the laser parameters, which still leads to successful cutting as a result of crack propagation, but otherwise minimizes or reduces all material losses (including in grinding steps).

[0080] Fig. 26a and Fig. 26b show two possibilities for lifting individual wafers from the boule / ingot.

[0081] According to Fig. 26a This is called a feedforward loop and according to Fig. 26b designed as a feedback loop.

[0082] In feedforward, the distribution is characterized before the laser process, and from this, a map or treatment instructions or parameter adjustments, particularly location-dependent, are calculated for the laser process, especially for the creation of modifications. Feedforward is preferably performed on the ingot / boule.

[0083] Alternatively, as in Fig. 26b As shown, a feedback loop can be implemented, according to which the resulting wafer is characterized after each separation step and serves as a template for the next one.

[0084] Depending on the material and doping, different adjustments can be made during the laser process: For SiC, different adjustments of the laser parameters can be made at different depths depending on the doping. This can lead to the following functions under the following boundary conditions: depth 180µm, pulse duration 3ns, numerical aperture 0.4 Low doping: 7µJ - 21 mOhmcm high endowment: 8µJ 16mOhmcm Depth 350µm, pulse duration 3ns, numerical aperture 0.4 Low doping: 9.5µJ - 21mOhmcm high endowment: 12µJ - 16mOhmcm

[0085] Formula for 180µm depth: EEnergy in µJ E0Offset energy at lowest doping KFactor Energy scaling Rmeasured doping level BBase doping level (21 mOhmcm) E=E0+B−R*K Here

[0086] K = 1 / (21-16) µJ / mOhmcm = 0.2µJ / mOhmcm E0 = 7µJ B = 21mOhmcm

[0087] Example: measured doping level of 19mOhmcm: E = 7.4µJ

[0088] Formula for 350µm depth: EEnergy in µJ E0Offset energy at lowest doping KFactor Energy scaling Rmeasured doping level BBase doping level (21 mOhmcm) E=E0+B−R*K Here

[0089] K = 2.5 / (21-16) µJ / mOhmcm = 0.5µJ / mOhmcm E0 = 95µJ B = 21 mOhmcm

[0090] Example: measured doping level of 19mOhmcm: E = 10.5µJ

[0091] The Figures 27a to 27i show various arrangements that can be provided after the production of the further material layers or components 150 for initiating the crack.

[0092] The Figures 27a-27i show various solid arrangements 176 which are advantageous for introducing crack guiding and / or crack initiation stresses.

[0093] Fig. 27a shows a processed solid body 1 or wafer with structures or components 150.

[0094] Compared to the Fig. 27a The solid 1 shown in Fig. 27b In the solid body 1 shown, a receiving layer 140 is arranged or produced on the component side, in particular on the components 150 or the additional material layers 150. The receiving layer 140 is preferably arranged on the solid layer to be separated. The receiving layer 140 can also be referred to as a split film and is thus preferably laminated to the structural side. In the subsequent step, the entire arrangement is then cooled, causing the split or crack initiation and / or crack guidance.

[0095] Compared to the representation of the Fig. 27b is according to the Fig. 27cA holding layer / bonded wafer is arranged on the underside of the solid body or on the exposed surface of the solid body. The holding layer can also be a tool carrier or Chuck 300. In the subsequent step, the entire assembly is cooled, which causes the split or crack initiation and / or crack guidance.

[0096] Fig. 27d shows opposite the Fig. 27ban arrangement according to which the solid body is provided with receiving layers 140, 146 on both sides. The further receiving layer 146 is arranged on a surface of the remaining solid body, wherein an adhesion-promoting layer 148 and / or sacrificial layer 149 and / or protective layer 142 can be arranged or created between the further receiving layer 146 and the solid body 1. The two receiving layers 140 and 146 are preferably laminated. In the subsequent step, the entire arrangement is cooled, which causes the split or crack initiation and / or crack guidance.

[0097] Fig. 27e shows an arrangement according to which, compared to the Fig. 27dIn the known arrangement, no adhesion-promoting layer 148 and / or sacrificial layer 149 and / or protective layer 142 is arranged or produced between the further receiving layer 146 and the solid body 1. In the subsequent step, the entire arrangement is then cooled, causing the split or crack initiation and / or crack guidance.

[0098] Fig. 27f shows an arrangement that is inverse to that of Fig. 27dknown arrangement, ie the adhesion-promoting layer 148 and / or sacrificial layer 149 and / or protective layer 142 is not arranged or produced between the further receiving layer 146 and the solid body 1, but is / are arranged or produced between the receiving layer 140 and the solid body 1 and thus is / are produced or arranged on the solid body layer to be separated. One or more layers can be produced on the components 150 or the structures, for example by means of spin coating. The subsequent step is then cooling the entire arrangement, which causes the split or the crack initiation and / or crack guidance.

[0099] Fig. 27g shows an arrangement or characteristic that is a combination of the arrangements of the Figures 27d and 27fThe solid body is preferably laminated on both sides with split film; a protective layer and / or adhesion-promoting layer and / or sacrificial layer can also be provided on both sides beneath the split film. Spin coating, for example, is also possible on the structures. The subsequent step is cooling the entire assembly, which causes the split or crack initiation and / or crack propagation.

[0100] Fig. 27h shows an arrangement similar to that shown in Fig. 27b The arrangement shown is that the receiving layer is not arranged or laminated on a surface of the solid layer to be separated, but rather on the residual solid remaining after separation. The separation then occurs as a result of cooling, analogous to the separation from an ingot or as in an ingot process.

[0101] Fig. 27i shows an arrangement similar to that of Fig. 27cknown arrangement, wherein one or more of the following layers or devices is / are arranged or produced on the component side of the solid body or on or above the components 150. These layers or devices are preferred: at least or exactly one adhesion-promoting layer 148 and / or at least or exactly one sacrificial layer 149 and / or at least or exactly one protective layer 142 and / or at least or exactly one stabilizing device 3, in particular a tool carrier or chuck 300 (preferably a cooling device) or another wafer. The subsequent step is then to cool the entire arrangement, which causes the split or crack initiation and / or crack guidance.

[0102] Fig. 28shows an illustration of an example of a writing pattern during XY machining: Arrows 170, 172 represent the laser feed direction, the black circles represent the different laser shots or modifications 9, which do not overlap in their damaging effect on the material. It is preferable for the laser to first move in one direction and create modifications 9 before reversing and writing modifications 9 in the second (lower) direction.

[0103] The Figures 29a to 29d show various cooling devices 174. The solid state arrangements 176 processed in these cooling devices 174 result from the various Figures 27a to 27i shown and described characteristics or

[0104] Design of the solid bodies 1 provided with one or more receiving layers 140, 146. The cooling devices 174 shown here all use a liquefied gas 178 as the initial cooling medium for cooling. This initial cooling medium is either nebulized or vaporized, depending on the embodiment. The initial cooling medium is preferably liquid nitrogen. Alternative cooling methods, e.g., using piezo elements, are also conceivable and possible.

[0105] The cooling device 174 preferably serves to cool the receiving layer 140, 146 to a temperature between -85°C and -10°C, in particular to a temperature between -80°C and -50°C.

[0106] According to Fig. 29aThe cooling device 174 comprises a nitrogen bath, wherein the receiving layer is positioned at a distance, in particular by means of an adjustable positioning device 180, from the liquid nitrogen held in the nitrogen bath. Thus, the solid-state arrangement is preferably arranged on a positioning device or on a holder above a nitrogen bath. This results in a temperature gradient across the chamber height, and the temperature at the solid-state arrangement can be adjusted via the fill level with the initial cooling medium or the position of the solid-state arrangement 176 (distance from the bottom of the chamber).

[0107] According to the embodiments of the Figures 29b to 29dthe cooling device can preferably comprise a nebulizing means, in particular at least or exactly one perforated pipe, for nebulizing liquid nitrogen or a nebulizing means for nebulizing liquid nitrogen and the cooling effect can be generated by nebulized or vaporized nitrogen.

[0108] According to Fig. 29b A homogeneous sprayer / fogger is preferably provided for spraying or atomizing. The spraying or atomizing preferably takes place above the solid-state arrangement 176. Furthermore, temperature measurements are preferably performed for temperature control, which output data for controlling a valve, in particular a nitrogen valve. The temperature measurements are preferably performed on the substrate or on the solid-state 1 or on the receiving layer 140.

[0109] The substrate or the solid body 1 or the solid body arrangement 176 preferably rests above the chamber floor in order to avoid nitrogen settling at the bottom of the chamber.

[0110] According to Fig. 29c A perforated pipeline is preferably used as a homogeneous spray device. Furthermore, temperature measurements are preferably performed for temperature control, which provide output data for controlling a valve, in particular a nitrogen valve. The temperature measurements are preferably performed on the substrate or on the solid body 1 or on the receiving layer 140.

[0111] The substrate or the solid body 1 or the solid body arrangement 176 preferably rests above the chamber floor in order to avoid nitrogen settling at the bottom of the chamber.

[0112] According to Fig. 29dshows a cooling device 176 that has a homogeneous sprayer / fogger 182 for cooling preferably several or each side. Furthermore, temperature measurements are preferably performed for temperature control, which output data for controlling a valve, in particular a nitrogen valve. The temperature measurements are preferably performed on the substrate or on the solid body 1 or on the receiving layer 140.

[0113] The substrate or the solid body 1 or the solid body arrangement 176 preferably rests above the chamber floor in order to avoid nitrogen settling at the bottom of the chamber.

[0114] The chamber 184 of the cooling device 174 is preferably closed in order to reduce a temperature gradient as much as possible by insulation.

[0115] Fig. 30shows three examples of preferred relationships between crystal lattice orientation and modification generation. This method is particularly useful for separating solid layers from a solid consisting of SiC or containing SiC. These relationships result in a further method according to the invention. This further method according to the invention is preferably used for separating at least one solid layer from at least one solid 1, in particular from a wafer from an ingot or for thinning a wafer.The further method according to the invention preferably comprises at least the steps: generating a plurality of modifications 2 by means of laser beams in the interior of the solid body 1 to form a detachment plane 4, and introducing an external force into the solid body 1 to generate stresses in the solid body 1, wherein the external force is so strong that the stresses cause crack propagation along the detachment plane 4.

[0116] According to the invention, the modifications are produced one after the other in at least one row or series or line, wherein the modifications 2 produced in a row or series or line are preferably produced at a distance X and with a height H, so that a crack propagating between two successive modifications, in particular a crack propagating in the crystal lattice direction, the crack propagation direction of which is oriented at an angle W to the detachment plane, connects the two modifications to one another. The angle W is preferably between 2° and 6°, in particular 4°. The crack preferably propagates from an area below the center of a first modification to an area above the center of a second modification. The essential relationship here is therefore that the size of the modification can or must be changed depending on the distance between the modifications and the angle W.

[0117] Furthermore, this method can also comprise the step of creating a composite structure by arranging or creating layers and / or components 150 on or above an initially exposed surface of the solid body 1, wherein the exposed surface is preferably a component of the solid body layer to be separated. Particularly preferably, the modifications for forming the detachment plane 4 are created before the creation of the composite structure.

[0118] To introduce the external force, a receiving layer 140 can be arranged on an exposed surface of the composite structure or the solid body, for example, analogously to the previously described methods.

[0119] The three figures 30a to 30c illustrate how the size of the laser-amorphized / phase-transformed damage / modification zone influences the height traversed by the sawtooth pattern of the crack. Generally, the crack runs along the crystal planes, i.e., between individual atoms of the crystal. In the modified zone, these clear planes no longer exist, so the crack stops.

[0120] By preferably using the highest possible numerical aperture, the damage zone can be reduced along the beam direction, as well as laterally in the focal plane. Since only the threshold intensity needs to be reached, a lower pulse energy is sufficient.

[0121] If the damage zone is suitably smaller, the laser modifications can be placed more densely, which makes the sawtooth run shorter and results in an overall smaller height extension of the modified plane (first image).

[0122] However, if the damage zone is larger (higher energy and / or lower numerical aperture - Fig. 30b ) - the increased pressure of the amorphized zone also triggers a larger microcrack, which can be captured (ie stopped in a controlled manner) by a damage zone of greater extent at a greater distance.

[0123] Fig. 30c Finally, the danger arises when the damaged area is not sufficiently large and excessive cracks are triggered by the laser modification. Firstly, the cracks extend too far – meaning the height difference caused by the cracks is greater than desired – and secondly, the cracks are driven beneath the other damaged areas and not stopped by the amorphized material. This then leads to material loss, as all torn material layers must be removed for the final product or for further laser processing.

[0124] Fig. 31shows a schematically illustrated snapshot from a further method according to the invention. This further method is preferably used for separating at least one solid layer from at least one solid body 1, in particular from a wafer from an ingot or for thinning a wafer. The further method according to the invention preferably comprises at least the steps: generating a plurality of modifications 2 by means of laser beams inside the solid body 1 to form a detachment plane 4, and introducing an external force into the solid body 1 to generate stresses in the solid body 1, wherein the external force is so strong that the stresses cause crack propagation along the detachment plane 4.

[0125] According to the invention, in a first step the modifications are produced on a line 103 and preferably at the same distance from one another. Furthermore, it is conceivable that a plurality of these lines produced in the first step are produced. These first lines are particularly preferably produced parallel to the crack propagation direction and preferably in a straight line or in the shape of a circular arc, in particular in the same plane. After the production of these first lines, second lines 105 are preferably produced for initiating and / or driving preferably subcritical cracks. These second lines are also preferably produced in a straight line. The second lines are particularly preferably inclined with respect to the first lines, in particular oriented orthogonally. The second lines preferably extend in the same plane as the first lines or particularly preferably in a plane that is parallel to the plane in which the first lines extend.Subsequently, third lines are preferably created to connect the subcritical cracks.

[0126] This process is particularly useful for separating solid layers from a solid made of SiC or containing SiC.

[0127] Furthermore, the modifications can be generated one after the other in at least one row, series or line, wherein the modifications 2 generated in a row, series or line are preferably generated at a distance X and with a height H, so that a crack propagating between two successive modifications, in particular a crack propagating in the crystal lattice direction, the crack propagation direction of which is oriented at an angle W to the detachment plane, connects the two modifications to one another. The angle W is preferably between 2° and 6°, in particular 4°. The crack preferably propagates from an area below the center of a first modification to an area above the center of a second modification. The essential relationship here is therefore that the size of the modification can or must be changed depending on the distance between the modifications and the angle W.

[0128] Furthermore, this method can also comprise the step of creating a composite structure by arranging or creating layers and / or components 150 on or above an initially exposed surface of the solid body 1, wherein the exposed surface is preferably a component of the solid body layer to be separated. Particularly preferably, the modifications for forming the detachment plane are created before the creation of the composite structure.

[0129] To introduce the external force, a receiving layer 140 can be arranged on an exposed surface of the composite structure or the solid body, for example, analogously to the previously described methods.

[0130] Thus, in the further laser process according to the invention, lines parallel to the crack propagation direction (preferably called transverse lines) are generated, preferably on SiC (but also other materials), to first define a plane for preferential crack initiation (crack initiation) before longitudinal lines drive the cracks. The cracks are first initialized transversely, then longitudinally, before a final step inserts lines between the longitudinal lines of the second step to initiate the cracks across the entire surface. This enables shorter crack propagation paths, which minimizes the final surface roughness.

[0131] Example image for transverse lines (with the sawtooth) and crack initiation lines (on the crests of the sawtooth). List of reference symbols

[0132] 1Solid 2Modification 3Location of modification 4Crack guiding area 6Solid portion 8Laser application device 9Lens 10Laser beams 11Modified laser beams 12Recess 14Solid layer 16Surface of the solid layer 17Irradiation surface 18Stress generation layer or receiving layer 140 19Adhesive or further stress generation layer 24Local property change of the solid (e.g., transmission) 26Trench 28Frame 30Intersection point of the reflected beams 32Flushing 34Coating 300Chuck Longitudinal direction of the solid

Claims

1. Method for separating a solid body layer (14), in particular a solid body wafer (14), from a solid body (1), wherein the method comprises: providing a solid body (1), generating modifications (2) in the interior of the solid body (1) by means of LASER beams (10) which penetrate into the solid body (1) via an irradiation surface (17), wherein a crack guide region (4) is predefined by the modifications (2), along which the solid body layer (14) is separated from the solid body (1), characterized by: removing material of the solid body (2) in the longitudinal direction (L) of the solid body (1), which is orthogonal or substantially orthogonal to the irradiation surface (17), wherein the crack guide region (4) is exposed by the material removal, and separating the solid body layer (14) from the solid body (1), wherein the solid body is weakened in the crack guide region (4) by the modifications in such a way that the solid body layer (1) detaches from the solid body (2) as a result of the material removal, or wherein such a number of modifications is generated after the material removal that the solid body is weakened in the crack guide region in such a way that the solid body layer (1) detaches from the solid body (2), or wherein a stress-generating layer (18) is generated or arranged on a surface (16) of the solid body (1) oriented at an angle to the circumferential surface and mechanical stresses are generated in the solid body (1) by a thermal application of the solid body layer (14), wherein a crack for separating a solid body layer (14) arises as a result of the mechanical stresses, which propagates along the modifications (2) starting from the surface of the solid body exposed by the material removal, or wherein the solid body is thermally exposed, in particular cooled, after the generation of the modifications (2) and the solid body layer (14) detaches from the solid body (1) along the crack guide region (4) as a result of the thermal application.

2. Method according to claim 1, wherein a circumferential depression (12) is generated by the removal of material of the solid body (1).

3. Method according to claim 1, wherein the surface (16) oriented at an angle is a planar surface.

4. Method according to claim 1, wherein the material removal takes place starting from an exposed surface of the solid body (1), in particular parallel to the circumferential surface of the solid body (1), in the longitudinal direction (L) of the solid body (1) and at least in sections at a distance from the circumferential surface of the solid body (1), and / or wherein the material removal takes place in the form of a trench (26) running continuously at least in sections, wherein the trench (26) is at a distance from the circumferential surface.

5. Method according to claim 4, wherein the exposed surface of the solid body (1) is a planar surface.

6. Method according to claim 4, wherein the trench is at a distance of at least 30 µm or at least 100 µm or at least 500 µm or at least 1 mm from the circumferential surface.