METHOD FOR THE PRODUCTION OF POLYCRYSTALLINE SILICON
Patent Information
- Application Number
- DE502019012267
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-05-21
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2039-05-21
AI Technical Summary
The existing methods for producing polycrystalline silicon lack efficient control over morphology during deposition, leading to inconsistent quality and increased costs due to the need for constant monitoring and separate assessment of polysilicon morphology, which affects the crystallization behavior and yield in semiconductor and solar cell production.
A method that calculates a morphology index (M) based on real-time resistance measurements during deposition, allowing for continuous control of the deposition process to achieve specific morphology values (0.8 to 2.5) to produce polysilicon with desired properties for various applications.
This approach enables precise control over polysilicon morphology, improving the efficiency and quality of polysilicon production, enhancing productivity, and allowing for customized polysilicon types suitable for different applications, such as semiconductors and solar cells, by directly monitoring and adjusting the deposition process.
Description
[0001] The invention relates to a process for producing polycrystalline silicon, wherein the morphology of the silicon is determined during the process using a characteristic number. M is determined and the procedure is controlled in such a way that M assumes a value of 0.8 to 2.5.
[0002] Polycrystalline silicon (polysilicon) serves as a starting material in the production of single-crystal (monocrystalline) silicon, for example by crucible drawing (Czochralski or CZ process) or by zone melting (float zone process). Single-crystal silicon is used in the semiconductor industry for the manufacture of electronic components (chips).
[0003] Furthermore, polysilicon is needed to produce multicrystalline silicon, for example using ingot casting. The multicrystalline silicon obtained in block form can be used to manufacture solar cells.
[0004] Polysilicon can be produced using the Siemens process – a chemical vapor deposition process. In this process, support materials (usually made of polysilicon) are heated by direct electric current in a bell-shaped reactor (Siemens reactor), and a reaction gas containing a silicon-containing component and hydrogen is introduced. The silicon-containing component is generally monosilane (SiH₄) or a halosilane with the general composition SiH₄nX₄-n (n = 0, 1, 2, 3; X = Cl, Br, I). It is usually a chlorosilane or a chlorosilane mixture, typically trichlorosilane (SiHCl₃, TCS). SiH₄ or TCS is predominantly used in a mixture with hydrogen. The design of a typical Siemens reactor is described, for example, in EP 2 077 252 A2 or EP 2 444 373 A1. The base of the reactor (base plate) is generally equipped with electrodes that hold the support bodies.The support structures are usually silicon filament rods (thin rods). Typically, two filament rods are connected by a silicon bridge to form a pair, which creates an electrical circuit via the electrodes. The surface temperature of the filament rods is usually above 1000°C during deposition. At these temperatures, the silicon-containing component of the reaction gas decomposes, and elemental silicon is deposited from the gas phase as polysilicon. This increases the diameter of the filament rods and the bridge. Once a predetermined rod diameter is reached, the deposition process is usually stopped, and the resulting polysilicon rods are removed. After removing the bridge, approximately cylindrical silicon rods are obtained.
[0005] The morphology of polysilicon, polysilicon rods, and the fragments produced from them generally has a strong influence on performance during further processing. Fundamentally, the morphology of a polysilicon rod is determined by the parameters of the deposition process (e.g., rod temperature, silane and / or chlorosilane concentration, specific flow rate). Depending on the parameters, pronounced interfaces, even holes and grooves, can form. These are generally not distributed homogeneously within the rod. Rather, by varying the parameters, polysilicon rods with different (mostly concentric) morphological regions can develop, as described, for example, in EP 2 662 335 A1. The dependence of the morphology on the rod temperature is expressed, for example, in US 2012 / 0322175 A1.Here, a method for controlling the surface temperature by measuring the resistance of at least one polysilicon rod during deposition is described. However, the method does not allow any conclusions to be drawn about the morphology of the silicon; rather, it assumes a consistent morphology.
[0006] EP 1 992 593 A2 describes a process for producing a polysilicon rod, wherein the reaction conditions are changed during deposition depending on the growing diameter of the silicon rod in order to realize coaxial regions of different crystal structures.
[0007] WO 2015 / 014590 A1 describes a process for the production of polysilicon in which an unaffected temperature measurement of the rod surface is carried out through a sight glass in the reactor wall.
[0008] The morphology of polysilicon can vary from compact and smooth to highly porous and fractured. Compact polysilicon is essentially free of cracks, pores, joints, and fissures. The bulk density of such polysilicon can be equated to, or at least closely approximates, the density of silicon. The density of silicon is 2.329 g / cm³.
[0009] A porous and fractured morphology has a particularly negative impact on the crystallization behavior of polysilicon. This is especially evident in the CZ process for producing single-crystal silicon. Here, the use of fractured and porous polysilicon leads to economically unacceptable yields. In general, particularly compact polysilicon results in significantly higher yields in the CZ process. However, the production of compact polysilicon is usually more expensive because a longer deposition process is required. Furthermore, not all applications require the use of particularly compact polysilicon. For example, the morphological requirements for the production of multicrystalline silicon using the ingot casting process are considerably lower.In general, a crystallization process or a specific form of such a process reaches an economic optimum when polysilicon is used as the starting material, the morphology of which does not exceed a limit value.
[0010] Accordingly, polysilicon is differentiated and classified not only by purity and fracture size but also by its morphology. Since the term morphology can encompass various parameters such as porosity (the sum of closed and open porosity), specific surface area, roughness, luster, and color, a reproducible determination of the morphology presents a significant challenge. Optical inspection of the polysilicon rods or fragments after deposition, as proposed, among others, in WO 2014 / 173596 A1, has the disadvantage that the internal morphology may differ considerably from the surface morphology.
[0011] For example, to determine porosity, the volume of the test object can be determined using the difference method, and the effective density can then be compared with the specific density. In the simplest case, the test object is immersed in a full container of water, with the volume of the overflowing water corresponding to that of the test object. When applied to polysilicon, a suitable fluid must be used to prevent oxidation and contamination and to ensure complete surface wetting. This is particularly complex for polysilicon rods produced using the Siemens process, which can be between 2 and 4 meters long. Methods for density measurement in polysilicon are described, for example, in WO 2009 / 047107 A2. A fundamental disadvantage of retrospectively examining the morphology is that it is too late to influence the deposition process and thus to control the morphology.
[0012] The invention was based on the objective of providing a method for determining the morphology of polysilicon during deposition in order to make the production and processing of polysilicon more efficient.
[0013] This problem is solved by a process for the production of polysilicon, comprising introducing a reaction gas containing, in addition to hydrogen, silane and / or at least one halosilane, into a reaction chamber of a gas-phase deposition reactor, wherein the reaction chamber includes at least one filament rod heated by an electric current, on which silicon is deposited to form a polycrystalline silicon rod. To determine the morphology of the silicon rod, measurements are taken during deposition at an average rod temperature. Ts a first resistance value R 1 of the silicon rod determined according to R 1 = U I with U= Voltage between two ends of the silicon rod [V], I = Current [A] a second resistance value R 2 of the silicon rod determined according to R 2 = ρ L A with ρ = specific resistance of silicon [Q*m], L = Length of the silicon rod [m], A = Cross-sectional area of the silicon rod [m²< ], and from the relationship R 1 / R 2 a morphology indicator M calculated, whereby the deposition (depending on M ) is controlled in such a way that M has a value of 1 to 1.8.
[0014] As described earlier, polysilicon with different morphologies can form depending on the deposition parameters. Even within the same polysilicon rod, particularly in the radial direction of its cross-sectional area, regions of varying morphologies can occur, separated by interfaces. Here, morphology refers specifically to the fragmentation of the polysilicon, resulting from the frequency and arrangement of holes, pores, and grooves. Morphology can also be understood as the overall porosity of the polysilicon, which comprises the sum of all cavities that are interconnected and connected to the surrounding environment, as well as the unconnected cavities. The overall porosity, i.e., the proportion of the total pore volume (open and closed pores) to the total volume of the polysilicon, can be determined according to DIN EN 1936.
[0015] It was observed that the holes and grooves, in particular, are not homogeneously distributed in the deposited polysilicon, but rather inhomogeneously according to the deposition process. The longitudinal direction preferentially points in the radial direction, i.e., in the growth direction. This can cause certain transport processes in the polysilicon to become direction-dependent (anisotropic). In other words, polysilicon can exhibit macroscopically anisotropic material properties.
[0016] This effect is particularly relevant in the case of electrical resistance. R , since the current flow increases predominantly in the axial direction (longitudinal direction) of the polysilicon rod R compared to compact polysilicon. R The potential of a polysilicon rod is therefore greater the more pronounced its fractured or porosity is.
[0017] In the inventive method, the morphology is determined directly during ash separation, using an electrothermal model that directly accesses process data. A generally complex and often inaccurate optical analysis of the polysilicon rods, either whole or in fragmentary form, after deposition is not required. By using readily available process data, the inventive method is arbitrarily scalable. The use of the morphology parameter M Process control offers significant potential for quality assurance and maximizing productivity. In particular, continuous monitoring of the morphology and process control based on the morphology allows polysilicon to be produced precisely according to customer specifications.
[0018] For the production of type A polysilicon, the control is preferably such that M has a value of 0.8 to 1.2. Type A is generally very compact and intended for the production of semiconductors, particularly for the CZ process with the aim of maximizing the dislocation-free yield.
[0019] For the production of type B polysilicon, the control is preferably such that M has a value of 1.2 to 1.4. Type B typically exhibits medium compactness and is used in particular for cost-optimized, robust semiconductor applications and demanding solar applications with monocrystalline silicon (CZ process).
[0020] For the production of type C polysilicon, which is particularly needed for robust solar applications with monocrystalline silicon, the control is preferably such that M has a value of 1.4 to 1.7. Type C is less compact than type B, less expensive, and particularly suitable for post-charging processes in the CZ process.
[0021] For the production of type D polysilicon, the control is preferably carried out in such a way that M Type C has a value above 1.7. It exhibits a high popcorn content, a relatively jagged surface, and high porosity. It is used particularly for the production of multicrystalline silicon for solar applications via directional solidification or ingot casting.
[0022] Particularly preferred points M a value of 1.2 to 1.6.
[0023] Preferably Mkept essentially constant during deposition. "Essentially" means, in particular, that temporary deviations of plus / minus 0.1 from a target value for M can occur.
[0024] Determining the key figure M The determination can be carried out continuously throughout the entire duration of the deposition or discontinuously at different times, preferably at equal time intervals, during the deposition. Preferably, the determination of M continuously, to ensure particularly precise control of the deposition.
[0025] Furthermore, the determination of M can be discretized over a time interval, where the time interval can correspond, in particular, to a predetermined increase in the diameter of the silicon rod. In this way, a statement can be made about the morphology of a region (coaxial region) of the silicon rod that has grown over a specific time interval. In this regard, reference can be made to Example 2 in conjunction with the Figur 2 be referred.
[0026] At M It is a dimensionless parameter derived from the ratio of the first directly measurable resistance. R 1 to the second theoretical resistance R 2 The more fractured / porous a polysilicon rod is, the greater the M. For example, polysilicon rods, for which MIf the coefficient of friction is greater than 1.5, a significant proportion of so-called popcorn is present. Popcorn means that the polysilicon has cracks, fissures, and breaks, and as a result of this fragmentation, it has a very large surface area.
[0027] The determination of R 1 , which can also be called heating resistance, is derived from the voltage measured on the silicon rod U and the current I according to Ohm's law. At I (Rod current) refers to the current intensity with which a filament rod / silicon rod is heated (Joule heating). UThis refers to the voltage applied between the ends of a silicon rod or filament rod to generate the rod current. Preferably, the filament rod consists of two thin silicon rods connected by a silicon bridge to form a rod pair. The two free ends of the rod pair are typically connected to electrodes at the bottom of the reactor. The measurement of U and I This can be done using commercially available measuring devices. Usually, U and I always displayed at a process control station and recorded if necessary.
[0028] The number of silicon rods or silicon rod pairs arranged in the gas-phase deposition reactor is generally irrelevant for the implementation of the process according to the invention. Preferably, the gas-phase deposition reactor is a Siemens reactor as described in the introduction and, for example, in EP 2 662 335 A1. Typical examples of the number of silicon rods in a reactor are 36 (18 rod pairs), 48 (24 rod pairs), 54 (27 rod pairs), 72 (36 rod pairs), or 96 (48 rod pairs). The silicon rods can be considered to be approximately cylindrical at any point during deposition. This is particularly true regardless of whether the thin rods are cylindrical or, for example, square. Accordingly, the following can be used to determine R 1 also mean values of U and I These can be used, for example, from measurements taken on each pair of rods in the reactor.
[0029] The determination of R 2 This is done by multiplying the specific resistance. ρ of silicon with length L of the silicon rod and division by the cross-sectional area A of the silicon rod.
[0030] L This generally corresponds to the length of the silicon rod, measured from one electrode to the other in the reactor base. To determine L, the length of the filament rod and, if applicable, the bridge, is usually used. This length is known or can be measured before installation in the reactor. For a silicon rod pair as described above, this would... L The length of the silicon rod is the sum of the lengths of the two thin rods and the bridge. The fact that the shape of the silicon rod may differ from that of the filament rod after deposition is irrelevant to the implementation of the invention. Likewise, the portion of the thin rods that is embedded in the electrodes or electrode holders is irrelevant and can be neglected.
[0031] Preferably is L 2 to 8 m, particularly preferably 3 to 7 m, particularly 4 to 6.6 m, particularly preferably 5.6 to 6.4 m.
[0032] The cross-sectional area A This can be done by measuring the diameter or circumference of at least one silicon rod. Since it can be assumed that the silicon rods are cylindrical and that the diameter of all silicon rods in the reactor is essentially the same, especially when comparing measurements at the same rod height, A after A = π*d 2< / 4,with d = rod diameter. This approximation is justified because modern Siemens reactors are designed to ensure the most homogeneous deposition possible, i.e., to generate silicon rods of the same quality and shape. This can be achieved through a homogeneous gas flow within the reactor and a substantially symmetrical arrangement of the rods. The rod or rods on which the diameter is determined (the same applies to the determination of the surface temperature TOF) are fundamentally irrelevant for the implementation of the invention.
[0033] Preferably, to determine A of the silicon rod, at least one diameter of the silicon rod and / or at least one diameter of at least another silicon rod is determined. Particularly preferably, the diameter of at least two, and especially three or four, silicon rods is determined. An average value can be calculated from the determined values, thereby increasing the measurement accuracy.
[0034] The diameter is preferably determined from outside the reactor through a viewing window, particularly using a camera. Two or more cameras, positioned differently around the reactor, can also be used. Preferably, the cameras are positioned side by side (in the circumferential direction of the reactor) in front of separate viewing windows. They can also be positioned side by side or one above the other in front of a single viewing window. The cameras can be at different heights. The diameter is usually determined on a silicon rod closest to the viewing window. Generally, it is not essential whether the diameter measurement (the same applies to the determination of the surface temperature TOF) is performed, for example, at the level of the rod's midpoint (midway between the bridge and the electrode) or at the level of the upper or lower third of the rod. Preferably, the measurement is taken at the rod's midpoint.
[0035] The camera can be an optical camera (e.g., a digital / CCD camera) and / or a thermal imaging camera. The diameter can be determined by (especially digital) image processing of one or more of the generated images or image sections. It can also be provided to generate a video, preferably with individual frames of the video being subjected to image processing. The image processing can be performed, in particular, by software that is preferably integrated into the process control system.
[0036] For example, the diameter can be determined by selecting the camera's focus so that at least one silicon rod is visible in its entirety against the inner reactor wall. Pixel analysis can then be used to identify a left and a right contour of the silicon rod and determine the distance between them. The camera is typically calibrated so that the width of the captured image corresponds to a specific distance along the circumference of the reactor's inner wall. The reactor geometry, particularly its circumference at the camera's position, is generally known. The position of the silicon rod, and thus its distance to the reactor's inner wall and the camera, is also usually known. It is also possible to measure the distance between two adjacent rods against the reactor wall and calculate their diameters from this measurement, particularly using triangulation.In this variant, the two adjacent bars do not necessarily need to be visible in their full width. By correlating the distances known from the reactor configuration, the diameter can be calculated based on the distance between the bars.
[0037] Alternatively or additionally, the diameter can also be determined from parameters of the deposition process that are usually continuously monitored. These parameters can include, for example, the volume flow rate of the reaction gas and the surface temperature. T OF the silicon rods, I, U, R 1 and deposition time. For example, using comparative data from previous deposition processes, the rod diameter can be calculated as a function of the deposition time.
[0038] Specific resistance ρ This indicates the electrical resistance of a conductor made of a material (e.g., silicon) that is 1 m long and has a continuous cross-sectional area of 1 mm². Basically, ρ depending on the temperature. ρ The temperature of silicon can be found in tables (see Chemical Encyclopedia, Moscow, 1990; Volume 2: page 1007, see also Table 2) and lies within the temperature range relevant for deposition, from 800 to 1300°C, at values of 0.00001 and 0.0005 2*m. The determination of the mean rod temperature Ts, in which both R 1 as well as R 2 Therefore, determining the information is of particular importance.
[0039] Ts is called surface temperature T OF of the silicon rod or as an average of two or more surface temperatures T OF determined using the same or different silicon rods. T OF This is an important influencing factor that is typically controlled during deposition and can be adjusted by varying the current flow. Basically, the heat flux leaving the silicon rods increases with the deposition time, as the diameter and thus the surface area of the rods grows. Therefore, adjusting the current is usually necessary during deposition.
[0040] Ts can be determined by adding a constant or variable temperature offset to the surface temperature T OF . The temperature offset is preferably in the range of 0 to 120 K, particularly preferably in the range of 30 to 80 K. This allows for consideration of the fact that Ts above the measured surface temperature T OF The temperature offset is generally greater the higher the heating power. U*I or the rod diameter d. The temperature offset can therefore be varied depending on U*I and d are specified.
[0041] Preferably the measurement of T OF with at least one thermographic camera (radiation pyrometer), especially from outside the reactor through a viewing window. For the determination of T OF (Particularly regarding the positioning of the measuring instrument and the location of the measurement), the same principles apply as for diameter determination. In this respect, reference can be made to the above explanations. Furthermore, reference can be made to WO 2019 / 110091 A1.
[0042] Since both the diameter and T OF Since both values can be determined using a thermographic camera, they can be determined on the same silicon rod.
[0043] Ts can also be determined according to T S = k U ∗ I A OF ∗ λ ∗ r II − r S + T OF , with k = Adjustment factor, A OF = rod surface area along the rod length, A = thermal conductivity of silicon, r II = Radius of the silicon rod, r S = Radius of the centroid of the cross-sectional area of the silicon rod.
[0044] This model for determining Ts The diagram in the Figur 1 Illustrated. The model is based on the measured T OF , the rod diameter d (2* r II ), the electrical heating power ( U * I ) and the thermal conductivity A. The thermal conductivity A of silicon is approximately 18 to 30 W / (m*K) in the relevant temperature range of 800 to 1300°C. A constant value of 22 W / (m*K) can be assumed for A.
[0045] At U*I / A OF *λ This refers to the temperature gradient. gradT OF on the rod surface, the latter being over n*d*L is determined. This approach takes into account that the entire electrical power is essentially conducted as heat flow across the rod surface. Since the silicon rod is approximately cylindrical (this can also be approximately assumed for the bridge) and the electrical heating power is distributed across the rod's cross-section, the temperature gradient decreases towards the rod's interior. At the rod's center, the temperature gradient reaches zero (the first derivative of the curve at r II corresponds to the straight line (slope) gradT OF ). As Ts According to this model, the temperature prevailing at the centroid of the rod's cross-section is defined ( T S at r S The centroid is the radius r S , where the area of an inner circle is equal to that of an outer ring. By multiplying the temperature gradient gradT OF with the adjustment factor k surrendered k*gradT OF (dashed line next to the tangent) gradT OF ) Together with the distance to the rod surface ( r II - r S ) and the addition to T OF can the determination of Ts This will be done. The adjustment factor k This value preferably lies in the range of 0 to 1.2, particularly preferably between 0.7 and 0.9. A typical value for k For example, 0.8.
[0046] The separation is achieved by varying at least one parameter selected from the group containing U, I, T OF , Reaction gas composition and volume flow, controlled.
[0047] This is usually achieved through continuous or discontinuous feedback at the process control station, depending on the determined morphology index. M The parameters are adjusted to determine a target value for M to achieve.
[0048] The tension U(per pair of rods) lies in a range of 50 and 500 V, preferably 55 and 250 V, particularly preferably 60 and 100 V.
[0049] The current strength I (per pair of bars) lies in a range of 500 and 4500 A, preferably 1500 and 4000 A, particularly preferably 2500 and 3500 A.
[0050] T OF The temperature range is between 950 and 1200°C, preferably between 1000 and 1150°C.
[0051] The reaction gas contains hydrogen in a proportion of 50 to 90%, preferably 60 to 80%, before entering the reactor. The composition of the reaction gas can be determined before it is fed into the reactor by Raman and infrared spectroscopy as well as gas chromatography.
[0052] The standard volume flow rate (measurable according to DIN EN 1343) of the reaction gas is 1500 to 9000 m³ / h, preferably 3000 to 8000 m³ / h.
[0053] Controlling the deposition process allows for the production of polysilicon of various qualities (e.g., types A, B, C, and D). For example, silicon rods with coaxial regions of differing morphologies can also be produced. A particular advantage is that the entire deposition process can be adapted to specific quality requirements, ensuring the most economical reactor operation is always selected. Fig. 1 graphically shows a model for determining the average rod temperature Ts. Fig. 2 shows the cross-sectional area of a polysilicon rod. Fig. 3 shows the course of the morphology index M depending on the rod diameter d for two types of polysilicon. Beispiele
[0054] Beispiel 1 : discretized determination of M.
[0055] The determination of M for a section of a polysilicon rod of type C, which grew over a period of time, is presented.
[0056] In the Fig. 1 The area corresponds to I a polysilicon rod with a diameter d I and the temperature T I at a time t 0 . the area II corresponds to a rod section grown in a time interval Δt = t 1 - t 0 with a thickness d II - d I (diameter increase) and the temperature T II . The determination of M of area II is carried out according to M II = 1 R 1 ,I + II − 1 R 1 , I − 1 1 R 2 , I + II − 1 R 2 , I with R 1 , I + II = = U t 1 I t 1 ; R 1 , I = U t 0 I t 0 R 2 , I + II = ρ T II 4 L d II 2 π ; R 2 , I = ρ T I 4 L d I 2 π Table 1: Values Example 1 Zeitpkt. Bereich d T OF T s ρ L R 2 U I R 1 M [m] [°C] [°C] [Ω*m] [m] [Ω] [V] [A] [Ω] - t_0 I 0,09 1005 1073 0,000089 2,8 0,031 95 1450 0,065 1,67 t_1 I+II 0,1 1000 1080 0,000087 2,8 0,030 87 1700 0,0511 1,65 t_1 II 0,146 0,2338 1,59 Table 2: Values for p T [°C] ρ [Ω*m] 800 0,00032 900 0,00019 1000 0,00012 1100 0,00008 1200 0,00006 1300 0,00004 Beispiel 2: Deposition of polysilicon type B and type C
[0057] In the Figur 3 The graph shows the curve of M for two different deposition processes, i.e., two different polysilicon grades, plotted against the silicon rod diameter d [mm]. The dashed curve (---) represents the production of type C. The curve shown in lines and dots (- -) represents the production of type C. Type B is more compact than type C and is used for more sensitive applications. Type B should have a value for M from 1.2 to 1.4, while type C should have a value of 1.4 to 1.7. Both processes were carried out in the same Siemens reactor, however, with different specifications for at least one parameter from the group with U, I, T OF , Reaction gas composition and volume flow rate were determined. M The measurement was performed continuously throughout the entire deposition period. The rod diameter was determined on two rods using a CCD camera and image processing. The determination of T OFThis was also done using two rods with a pyrometer.
[0058] Both processes begin with compactly deposited polysilicon with values for M close to 1. Filament rods made of very compact silicon were also used. Subsequently, it rises. M for both processes. In the production of type C, for M A relatively steep gradient was chosen shortly after the start of the separation process. The targeted level of M A coefficient of friction of 1.4 to 1.7 should already be achieved with a rod diameter of 50 mm. Subsequently, M set to a value of approximately 1.45 to 1.5. For the production of type B, a flatter profile was used up to a diameter of about 100 mm. M specified. From a diameter of approximately 140 mm, M lowered again to separate the outer 40 mm in a more compact manner.
[0059] The example clearly demonstrates how convenient it is to use the key figure.M The deposition process can be controlled to produce a wide variety of polysilicon types.
Claims
1. Method for producing polycrystalline silicon, comprising introducing a reaction gas, which in addition to hydrogen contains silane and / or at least one halosilane, into a reaction space of a vapour deposition reactor, wherein the reaction space comprises at least one filament rod which is heated by way of the passage of current and on which by means of deposition silicon is deposited to form a polycrystalline silicon rod, wherein for the determination of the morphology of the silicon rod during the deposition at a rod temperature TS - a first resistance value R1 of the silicon rod is determined according to R 1 = U I where U = voltage between two ends of the silicon rod, I = current strength - a second resistance value R2 of the silicon rod is determined according to R 2 = ρ L A where ρ = resistivity of silicon, L = length of the silicon rod, A = cross-sectional area of the silicon rod, and a morphology index M is calculated from the ratio R1 / R2, wherein the deposition is controlled by varying at least one parameter selected from the group comprising U, I, surface temperature TOF, reaction gas composition and standard volume flow rate in such a way that M - for the production of type B polysilicon has a value from 1.2 to 1.4, - for the production of type C polysilicon has a value from 1.4 to 1.7 or - for the production of type D polysilicon has a value greater than 1.7, wherein U is in a range from 50 to 500 V, I is in a range from 500 to 4500 A, TOF is in a range from 950 to 1200°C, the standard volume flow rate of the reaction gas is 1500 to 9000 m3 / h and the reaction gas prior to entry into the reactor contains hydrogen in a proportion of 50% to 90%, and wherein Ts is the surface temperature TOF of the silicon rod or the arithmetic mean of two or more surface temperatures TOF of the same or different silicon rods.
2. Method according to Claim 1, characterized in that the index M is kept constant during the deposition.
3. Method according to either of the preceding claims, characterized in that the index M is determined continuously during the entire deposition or discontinuously at various points in time in the deposition.
4. Method according to any of the preceding claims, characterized in that the index M is determined in discretized form in a time interval corresponding to a specified growth in the diameter of the silicon rod.
5. Method according to any of the preceding claims, characterized in that for the determination of the cross-sectional area A of the silicon rod at least one diameter of the silicon rod and / or at least one diameter of at least one other silicon rod is determined.
6. Method according to any of the preceding claims, characterized in that the length L of the silicon rod is 2 to 8 m, preferably 3 to 7 m, particularly preferably 4 to 6.6 m, especially 5.6 to 6.4 m.
7. Method according to any of the preceding claims, characterized in that the voltage U is in a range from 55 to 250 V, preferably from 60 to 100 V.
8. Method according to any of the preceding claims, characterized in that the current strength I is in a range from 1500 to 4000 A, preferably from 2500 to 3500 A.
9. Method according to any of the preceding claims, characterized in that the temperature of the rod surface TOF is in a range from 1000 to 1150°C.
10. Method according to any of the preceding claims, characterized in that the reaction gas prior to entry into the reactor contains hydrogen in a proportion of 60% to 80%.
11. Method according to any of the preceding claims, characterized in that the standard volume flow rate of the reaction gas is 3000 to 8000 m3 / h.