METHOD FOR PRODUCING A HOLLOW CORE FIBER AND FOR PRODUCING A PREFORM FOR A HOLLOW CORE FIBER
Patent Information
- Application Number
- DE502019012500
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-07-17
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2039-07-17
AI Technical Summary
Antiresonant hollow core fibers, especially those with nested structural elements, are difficult to produce accurately and reproducibly due to complex internal geometries and the need for precise positioning of antiresonance elements, which is challenging with conventional 'stack and draw' techniques, leading to issues with higher order mode suppression and optical attenuation.
A vertical drawing process without molds is used to produce antiresonance element preforms, allowing for precise and reproducible production of antiresonant hollow core fibers by elongating glass cylinders in multiple stages with controlled heating zones, ensuring high purity and low particle contamination, and using a sealing compound with amorphous SiO2 particles for precise positioning and fixation.
This method achieves high precision and reproducibility in the production of antiresonant hollow core fibers with improved geometric accuracy, reduced particle contamination, and enhanced optical and mechanical properties, leading to lower attenuation and wider transmission ranges.
Description
Technical background
[0001] The invention relates to a method for producing an anti-resonant hollow core fiber, which has a hollow core extending along a fiber longitudinal axis and a cladding region surrounding the hollow core, which comprises a number of anti-resonance elements, with the method steps: (a) Providing a cladding tube having a cladding tube inner bore and a cladding tube longitudinal axis along which a cladding tube wall bounded by an inner side and an outer side extends, (b) Providing tubular anti-resonance element preforms, each having at least one ARE outer tube and optionally at least one ARE inner tube, (c) Arranging the anti-resonance element preforms at desired positions on the inner side of the cladding tube wall to form a primary preform having a hollow core region and an inner shell region, and (d) Elongating the primary preform to form the hollow core fiber or further processing the primary preform to form a secondary preform from which the hollow core fiber is drawn, wherein the further processing comprises a single or repeated execution of one or more of the following hot forming processes: (i) Elongating, (ii) Collapsing, (iii) Collapsing and simultaneous elongating,(iv) Collapse of additional mantle material, (v) Collapse of additional mantle material and subsequent elongation, (vi) Collapse of additional mantle material and simultaneous elongation. ,
[0002] Furthermore, the invention relates to a method for producing a preform for an anti-resonant hollow core fiber, which has a hollow core extending along a fiber longitudinal axis and a cladding region surrounding the hollow core, which comprises a plurality of anti-resonance elements, with the method steps: (a) Providing a cladding tube having a cladding tube longitudinal axis along which a cladding tube wall bounded by an inner side and an outer side extends, (b) Providing tubular anti-resonance element preforms, each having at least one ARE outer tube and optionally at least one ARE inner tube, (c) Arranging the anti-resonance element preforms at desired positions on the inner side of the cladding tube wall to form a primary preform having a hollow core region and an inner cladding region, and (d) Optionally further processing the primary preform into a secondary preform for the hollow core fiber, wherein the further processing comprises a single or repeated execution of one or more of the following hot forming processes: (i) elongation, (ii) collapse, (iii) collapse and simultaneous elongation, (iv) collapsing additional cladding material,(v) Collapse of additional mantle material and subsequent elongation, (vi) Collapse of additional mantle material and simultaneous elongation. ,
[0003] Conventional single-mode optical fibers made of solid material have a glass core surrounded by a glass cladding region with a lower refractive index. Light transmission is based on total internal reflection between the core and cladding regions. However, the interactions of the guided light with the solid material are associated with increased latency in data transmission and relatively low damage thresholds for high-energy radiation.
[0004] These disadvantages are avoided or reduced by hollow-core fibers, in which the core contains an evacuated cavity filled with gas or liquid. In hollow-core fibers, the interaction of light with the glass is less than in solid-core fibers. The refractive index of the core is lower than that of the cladding, so light transmission by total internal reflection is not possible, and the light would normally escape from the core into the cladding. Depending on the physical mechanism of light transmission, hollow-core fibers are divided into photonic bandgap fibers and antiresonance reflection fibers.
[0005] In "photonic bandgap fibers," the hollow core region is surrounded by a cladding in which small hollow channels are periodically arranged. The periodic structure of the hollow channels in the cladding causes the effect referred to in semiconductor technology as the "photonic bandgap," whereby light of certain wavelength ranges scattered by the cladding structures experiences constructive interference in the central cavity due to Bragg reflection and cannot propagate transversely in the cladding.
[0006] In the design known as "antiresonant hollow-core fibers" (AR-HCF), the hollow core region is surrounded by an inner cladding region in which so-called "antiresonant elements" (or "antiresonant elements"; abbreviated to "AREs") are arranged. The walls of the antiresonant elements, evenly distributed around the hollow core, can act as Fabry-Perot cavities operating in antiresonance, reflecting the incident light and guiding it through the fiber core.
[0007] This fiber technology promises low optical attenuation, a very broad transmission spectrum (including in the UV or IR wavelength range) and low latency in data transmission.
[0008] Potential applications of hollow core fibers are in the field of data transmission, high-performance beam guidance, for example for material processing, modal filtering, nonlinear optics, in particular for supercontinuum generation, from the ultraviolet to the infrared wavelength range. State of the art
[0009] A disadvantage of antiresonant hollow core fibers is that higher order modes are not necessarily suppressed, so that over long transmission lengths they are often not purely single-mode and the quality of the output beam deteriorates.
[0010] In the paper by Francesco Poletti, "Nested antiresonant nodeless hollow core fiber"; Optics Express, Vol. 22, No. 20 (2014); DOI: 10.1364 / OE 22.023807, a fiber design is proposed in which antiresonant elements are not formed as a simple, singular structural element, but are composed of multiple, nested structural elements. The nested antiresonant elements are designed such that higher-order core modes are phase-matched to the cladding modes and are suppressed, but not the fundamental core mode. This ensures the propagation of the fundamental core mode at all times, and the hollow-core fiber can be effectively made single-mode over a limited wavelength range.
[0011] The effective mode suppression depends on the center wavelength of the transmitted light and on structural parameters of the fiber design, such as the radius of the hollow core and the diameter difference of nested ring structures in the antiresonance elements.
[0012] EP 3 136 143 A1 discloses an antiresonant hollow-core fiber (referred to therein as a "hollow-core fiber with no band gap") in which the core can conduct additional modes in addition to the fundamental mode. For this purpose, it is surrounded by an inner cladding with "non-resonant elements" that provide phase matching of antiresonant modes with the higher modes. The hollow-core fiber is manufactured using a so-called "stack-and-draw" technique, in which the starting elements are arranged in an axis-parallel ensemble and fixed to a preform, which is then elongated. A cladding tube with a hexagonal inner cross-section is used, and six so-called "ARE preforms" (anti-resonance element preforms) are fixed in the inner edges of the cladding tube. This preform is drawn into a hollow-core fiber in two stages.
[0013] WO 2018 / 169487 A1 discloses a method for producing a preform for anti-resonant hollow-core fibers, in which a first cladding region comprises a plurality of rods and a second cladding region comprises a plurality of tubes surrounded by an outer cladding tube. The rods, tubes, and cladding tube are assembled using a "stack and draw" technique to form a preform. Before the preform is elongated, the preform end is sealed by applying a sealing compound. A UV adhesive, for example, is used as the sealing compound.
[0014] AF Kosolapov et al.: "Hollow-core revolver fiber with a double-capillary reflective cladding", Quantum Electronics, Vol. 46, No. 3, March 29, 2016 (2016-03-29), Pages 267-270, DOI: 10.1070 / QEL15972, describes a method for manufacturing an antiresonant hollow-core fiber by providing a cladding tube and a number of antiresonant element preforms, which are assembled as a double tube consisting of an ARE outer tube and an ARE inner tube welded to its inner wall. A standard drawing furnace is used to elongate the double tube.
[0015] DE 10 2005 028219 B3 describes a method for producing a quartz glass tube by elongating a quartz glass hollow cylinder in a vertical drawing process. The quartz glass hollow cylinder is continuously fed into a heating zone with a vertically oriented heating tube, softened zone by zone, and a tube strand is drawn from the softened area and cut to length to form the quartz glass tube. To optimize the dimensional accuracy of the resulting quartz glass tube, it is recommended that the ratio of heating zone length to heating zone inner diameter be less than 0.9. Technical task
[0016] Antiresonant hollow-core fibers, especially those with nested structural elements, have complex internal geometries, making their precise and reproducible manufacturing difficult. This is all the more true because, in order to maintain resonance or antiresonance conditions, even small dimensional deviations on the order of magnitude of the operating wavelength of the guided light are intolerable. Deviations from the target geometry can be caused by the configuration of the fiber preform, and they can also occur due to unintentional off-scale deformations during the fiber drawing process.
[0017] With the well-known "stack-and-draw" technique, many elements must be assembled with precise positioning. For example, to produce the hollow-core fiber in the "NANF" design known from the paper mentioned above, six antiresonance element preforms, each consisting of an antiresonance element outer tube (abbreviated to ARE outer tube) and an antiresonance element inner tube (abbreviated to ARE inner tube) welded to one side of the ARE outer tube's inner surface, must be attached to the inside of a cladding tube.
[0018] To achieve low attenuation values and wide transmission ranges, in addition to a uniform wall thickness of the antiresonance elements, the azimuthal positioning of the antiresonance elements within the cladding tube is also important. This cannot be easily achieved using the "stack-and-draw" technique. The aim of the invention is to provide a method for the cost-effective production of an antiresonant hollow-core fiber that avoids the limitations of conventional manufacturing processes.
[0019] In particular, it is an object of the invention to provide a method for producing an antiresonant hollow core fiber and a preform for antiresonant hollow core fibers, with which a high precision of the structural elements and an exact positioning of the antiresonant elements in the fiber can be achieved in a sufficiently stable and reproducible manner.
[0020] In addition, disadvantages of the classic "stack and draw" technique, with which the required structural accuracies, in particular a uniform wall thickness of the anti-resonance elements and exact positioning at specified azimuthal positions, are not easy to achieve, should be avoided as far as possible. Summary of the invention
[0021] With regard to the method for producing the antiresonant hollow core fiber, this object is achieved according to the invention, starting from a method of the type mentioned at the outset, in that, in order to provide the tubular antiresonant element preforms according to method step (b), the ARE outer tube and / or the ARE inner tube is produced using a vertical drawing process without a mold, which comprises the following method steps: (aa) Providing a starting hollow cylinder made of glass, which has a cylinder longitudinal axis and an outer cylinder surface as well as an inner cylinder surface, (bb) a first elongation process in which the starting hollow cylinder with a vertically oriented longitudinal axis is continuously fed to a first heating zone with a first heating zone length L H1, softened in some areas therein, and an intermediate cylinder is withdrawn from the softened area without a forming tool, (cc) a second elongation process in which the intermediate cylinder or an elongated intermediate cylinder obtained from the intermediate cylinder by elongation with a vertically oriented longitudinal axis is continuously fed to a second heating zone with a second heating zone length L H2, softened in some areas therein, and a tube strand with an outer diameter T a and an inner diameter T i is withdrawn from the softened area without a forming tool, where: L H2 < L H1 and T a / T i < 1.5,and (dd) cutting the pipe string to length into ARE outer pipes or ARE inner pipes, The heating zone length is understood to be the length within which the temperature measured in degrees Celsius is at least 90% of a maximum drawing temperature.
[0022] The starting point for the production of the antiresonant hollow-core fiber is a preform, also referred to here as the "primary preform." The production of the primary preform involves the installation and connection of antiresonant element preforms to a cladding tube to form a so-called "cane." The primary preform can be elongated to form the hollow-core fiber; however, additional cladding material is typically added to the primary preform to create a preform, referred to here as the "secondary preform." If necessary, the hollow-core fiber is created by elongating the secondary preform. Alternatively, the primary preform or the secondary preform are surrounded by one or more overwrapped cylinders to form a coaxial assembly of components, and the coaxial assembly is elongated directly to form the hollow-core fiber.The general term "preform" is understood here to refer to the component or coaxial ensemble of components from which the hollow core fiber is ultimately drawn.
[0023] Preform production involves a number of process steps in which initial elements of the hollow core fiber are manufactured and positioned relative to one another, and at least one hot-forming step. Each of the initial elements exhibits a certain deviation from its target geometry, and each positioning and forming step inevitably leads to geometric deviations that add up to an absolute geometric error in the finished preform. In particular, the hot-forming of glass can lead to unwanted and irreproducible deformation even with the slightest deviations from an ideal, usually cylindrically symmetrical, temperature profile of the heating zone.
[0024] The primary preform used in the process according to the invention contains anti-resonance elements, at least some of which, preferably all of which, are produced in a vertical drawing process without a mold. A forming tool is understood here to mean, for example, a forming nozzle, a forming mandrel, or another glassblowing tool that is brought into direct contact with the hot glass mass during the forming process for the purpose of shaping. Such forming tools are made of a high-temperature-resistant material, such as tungsten, and they often cause impurities in the glass. Furthermore, contact with the hot glass mass can damage the surface of the drawn-off glass strand. Since the process according to the invention is a non-contact forming process, i.e., without the use of forming tools, all of these disadvantages are avoided. ARE outer tubes and ARE inner tubes are obtained that are characterized by high purity and a low-damage surface. In particular, an ARE outer tube and ARE inner tube are obtained from quartz glass that contains a tungsten concentration of less than 2 wt. ppb.In known methods for elongating a starting cylinder, the forming process takes place in a heating zone with the starting cylinder's longitudinal axis oriented horizontally. Such horizontal drawing processes are used particularly for elongating long tubes. Particles formed in the heating zone, for example, of metal, graphite, or SiC, can easily be drawn onto the hot glass mass by gravity. Such particles lead to a deterioration of both the optical properties (absorption, refractive index) and the mechanical properties (bubbles or particles) and typically cause fiber breakage during the fiber drawing process.
[0025] In the vertical drawing process according to the invention, this effect does not occur, since the particles formed in the heating zone fall laterally towards the elongated pipe string due to gravity. The result is ARE outer pipes and ARE inner pipes that are characterized by a high degree of particle freedom.
[0026] In particular, after completion of the vertical drawing process, an ARE outer tube or an ARE inner tube is obtained with an outer surface that is free of particles with a size of more than 0.005 mm.
[0027] Overall, ARE outer and inner tubes can be produced with higher fracture strength (due to low particle contamination) and improved geometric accuracy, which also contributes to improved damping properties and bandwidth performance. The components can be manufactured with a dimensional deviation of less than 0.1 mm in wall thickness.
[0028] The vertical drawing process includes the following process steps: (aa) Providing a starting hollow cylinder made of glass, which has a cylinder longitudinal axis and an outer cylinder surface as well as an inner cylinder surface, (bb) a first elongation process in which the starting hollow cylinder with a vertically oriented longitudinal axis is continuously fed to a first heating zone with a first heating zone length L H1, softened in some areas therein, and an intermediate cylinder is withdrawn from the softened area without a forming tool, (cc) a second elongation process in which the intermediate cylinder or an elongated intermediate cylinder obtained from the intermediate cylinder by elongation with a vertically oriented longitudinal axis is continuously fed to a second heating zone with a second heating zone length L H2, softened in some areas therein, and a tube strand with an outer diameter T a and an inner diameter Ti is withdrawn from the softened area without a forming tool, where: L H2 < L H1 and T a / T i < 1.5,and (dd) cutting the pipe string to length into ARE outer pipes or ARE inner pipes.
[0029] The elongation process takes place in at least two stages and in at least two different drawing systems. The drawing systems used differ primarily in the length of their heating zone. For a heating zone with a constant temperature profile in the vertical direction, this refers to the heated length within which the temperature has its nominal setpoint. For a heating zone with a non-constant temperature profile in the vertical direction, this refers to the length section within which the temperature, measured in degrees Celsius, is at least 90% of the maximum drawing temperature. The comparatively longer heating zone in the first elongation step contributes to a more homogeneous radial temperature distribution within the volume of the initial cylinder to be formed and enables a high material throughput. The first heating zone length L H1 is at least 200 mm and is preferably between 250 and 400 mm. The comparatively shorter heating zone in the second elongation step creates a steeper temperature gradient in the axial direction of the intermediate cylinder to be formed. This results in a relatively short drawing bulb with a low drawing bulb mass. Due to the lower softened mass, its natural vibrations are reduced, resulting in smaller dimensional deviations in the drawn tube strand. The second, shorter heating zone length L H2 is a maximum of 180 mm and is preferably between 50 and 150 mm.
[0030] In a particularly advantageous variant of the two-stage elongation process, the provision of the initial hollow cylinder according to process step (aa) comprises a mechanical machining of the cylinder jacket surfaces for setting initial hollow cylinder final dimensions, comprising an outer diameter C a of at least 90 mm, an inner diameter Ci and a diameter ratio C a / C i of less than 2.8.
[0031] The mechanical machining of the cylinder surface of the initial hollow cylinder is preferably carried out by machining by cutting, drilling, milling, grinding, honing and / or polishing.
[0032] Compared to other known forming techniques for hollow cylinder production using heat and pressure, these processing techniques provide more precise and delicate structures and they avoid contamination of the surfaces by forming tools such as nozzles, presses or melt molds.
[0033] A comparatively large hollow cylinder with an outer diameter C a of at least 90 mm, preferably at least 150 mm, and particularly preferably at least 180 mm, is used as the starting cylinder. The diameter ratio C a / C i is a measure of the wall thickness of the starting cylinder.
[0034] This is advantageously drawn via the intermediate step of at least one intermediate cylinder to form a pipe string with an outer diameter T a in the range of 7 to 25 mm.
[0035] In a first process variant, the wall thickness of the pipe string is preferably set to a value between 0.2 and 2 mm, preferably to a value between 0.22 and 1.2 mm, and the diameter ratio T a / T i to a value in the range of 1.02 and 1.14, preferably to a value in the range of 1.04 to 1.08.
[0036] In a second process variant, the wall thickness of the pipe string is preferably set to a value between 0.2 and 2 mm, preferably to a value between 0.22 and 1.2 mm, and the diameter ratio T a / T i to a value in the range of 1.02 and 1.14, preferably to a value in the range of 1.04 to 1.08.
[0037] Particularly with regard to achieving the smoothest possible inner surface of the drawn pipe string, it has proven advantageous if the pull-out ratio in the sum of the elongation processes is set to a value in the range of 38 to 7800.
[0038] The draw ratio is defined here as the ratio of the total cross-sectional areas of the drawn tubing and the initial cylinder. It is a measure of the intensity / degree of the forming process. Using a larger initial cylinder also allows for higher production productivity.
[0039] It has been shown that the quality of the inner wall of the drawn tubing depends on the intensity of the forming process. A more intensive forming process tends to result in a better, smoother inner surface.
[0040] The non-contact vertical drawing process can also be advantageously used to produce the cladding tube of the primary preform. The cladding tube is preferably characterized by a diameter in the range of 20 to 70 mm, preferably by an outer diameter in the range of 30 to 60 mm. This is a comparatively large outer diameter. In the prior art, the outer diameters of the primary preforms (canes) are typically 4 to 6 mm. This makes the production of hollow-core fibers on an industrial scale virtually impossible.
[0041] Since the absolute geometric errors during fiber drawing are scaled down more significantly with the preform diameter, more precise production of the hollow-core fiber is fundamentally possible. The larger the diameter, the slower the tracking speed during elongation and the longer the duration for which each axial section of the preform is exposed to the high temperature of the heating zone. However, if the tracking speed during elongation is too slow, the structural elements of the anti-resonance element preforms deform. For diameters smaller than 20 mm, the thermal inertia of the preform is low, making it more difficult to compensate for any temperature fluctuations in the heating zone.
[0042] In a preferred method variant, the arrangement of the anti-resonance element preforms and / or the elongation of the primary preform, and / or the drawing of the hollow core fiber comprises a fixing measure and / or a sealing measure using a sealing or bonding compound containing amorphous SiO 2 particles.
[0043] The sealing or bonding compound used for sealing or fixing contains amorphous SiO2 particles, which are suspended, for example, in a dispersion liquid. This compound is applied between the surfaces to be bonded or sealed and is usually pasty during use. Upon drying at low temperature, the dispersion liquid is partially or completely removed and the compound solidifies. The sealing or bonding compound, and in particular the solidified SiO2-containing sealing or bonding compound obtained after drying, meets the requirements for fixing and compaction. The temperature required for drying is below 300°C, which promotes compliance with the dimensional stability of the preform and avoids thermal impairments.Heating to higher temperatures around 800 °C, for example, during elongation of the preform into a hollow-core fiber, leads to further thermal strengthening of the sealing or bonding compound, which is also suitable for forming opaque or transparent glass. This occurs through sintering or vitrification, whereby sintering to opaque glass requires comparatively lower temperatures and / or shorter heating times than vitrification to complete transparency. The sealing or bonding compound can thus be fully densified by heating and vitrified by heating during the hot-forming process.
[0044] During the hot-forming process, the sealing or bonding compound does not decompose and releases few impurities. It is thus characterized by thermal stability and purity during the hot-forming process and avoids deformation due to different thermal expansion coefficients.
[0045] The sealing and bonding compound can also be used advantageously to wear open ends of the anti-resonance element preforms and / or individual structural elements of the anti-resonance element preforms and / or any annular gap between tube elements during elongation of the primary preform and / or during drawing of the hollow core fiber.
[0046] In this way, the individual components of the primary preform and / or secondary preform can be exposed to different internal pressures during the elongation or fiber drawing process.
[0047] The accuracy of the positioning of the preforms on the inner surface of the cladding tube is further improved by producing the cladding tube inner side and / or the cladding tube outer side and / or the ARE outer tube inner side and / or the ARE outer tube outer side by machining, in particular by drilling, milling, grinding, honing and / or polishing
[0048] Compared to other known forming techniques using heat and pressure, these processing techniques produce more precise and delicate structures and avoid surface contamination by forming tools such as nozzles, presses or melt molds.
[0049] The machining preferably also includes structuring the cladding tube interior in the region of the target positions of the anti-resonance element preforms by providing them with a longitudinal structure extending in the direction of the cladding tube's longitudinal axis. This longitudinal structure comprises, for example, longitudinal slots and / or longitudinal grooves in the cladding tube's interior wall, which run parallel to the cladding tube's longitudinal axis and are preferably created by drilling, sawing, milling, cutting, or grinding.
[0050] The longitudinal structure extending along the cladding tube's longitudinal axis serves as a positioning aid for the anti-resonance element preforms. It facilitates the anti-resonance element preforms' adoption of predefined positions on the inside of the cladding tube.
[0051] The accuracy of positioning the preforms on the inner surface of the cladding tube is improved if the upper front ends of the structural elements are positioned at the desired position using a positioning template.
[0052] The positioning template has, for example, a shaft projecting into the inner bore of the cladding tube, which is provided with holding elements in the form of several radially outward-pointing holding arms.
[0053] The star-shaped arrangement of the retaining elements, as specified by the design, facilitates the precise positioning of the anti-resonance element preforms at the respective target positions and their fixation, for example, using the sealing or bonding compound described above. The positioning template is preferably used exclusively in the area of the cladding tube end faces, preferably in the area of both cladding tube end faces.
[0054] A procedure has also proven successful in which, during elongation of the primary preform according to process step (d) and / or during drawing of the hollow core fiber according to process step (e), several components of the preform made of quartz glass are heated and softened together, wherein the quartz glass of at least some of the preform components contains at least one dopant which reduces the viscosity of quartz glass.
[0055] Components of the primary preform include the cladding tube and the anti-resonance element preforms arranged therein. The secondary preform contains additional cladding material, which is provided, for example, in the form of one or more overlay cylinders and is collapsed onto the primary preform or drawn together with it to form the hollow core fiber.
[0056] Fluorine, chlorine and / or hydroxyl groups are preferably used as dopants to reduce the viscosity of quartz glass.
[0057] Doping allows the thermal expansion coefficients of adjacent preform components to be adjusted to avoid or reduce stresses. It can also be used to reduce the thermal stability of one preform component to benefit the stability of a neighboring preform component.
[0058] For example, it has proven advantageous if the quartz glass of the cladding tube has a viscosity at least 0.5 dPa.s higher, preferably at least 0.6 dPa.s higher, at a measuring temperature of 1250 °C than the quartz glass of additionally applied cladding material (when the viscosity is specified as a logarithmic value in dPas).
[0059] In particular with regard to low optical attenuation and a large optical transmission bandwidth of the hollow core fiber, it has proven particularly advantageous if the antiresonance elements are arranged around the hollow core with an odd symmetry.
[0060] With regard to the production of the preform for the hollow core fiber, the above-mentioned technical problem is solved according to the invention on the basis of a method of the type mentioned at the outset in that, in order to provide the tubular anti-resonance element preforms according to method step (b), the ARE outer tube and / or the ARE inner tube is produced using a vertical drawing process without a mold, which comprises the following method steps: (aa) Providing a starting hollow cylinder made of glass, which has a cylinder longitudinal axis and an outer cylinder surface as well as an inner cylinder surface, (bb) a first elongation process in which the starting hollow cylinder with a vertically oriented longitudinal axis is continuously fed to a first heating zone with a first heating zone length L H1, softened in some areas therein, and an intermediate cylinder is withdrawn from the softened area without a forming tool, (cc) a second elongation process in which the intermediate cylinder or an elongated intermediate cylinder obtained from the intermediate cylinder by elongation with a vertically oriented longitudinal axis is continuously fed to a second heating zone with a second heating zone length L H2, softened in some areas therein, and a tube strand with an outer diameter T a and an inner diameter Ti is withdrawn from the softened area without a forming tool, where: L H2 < L H1 and T a / T i < 1.5,and (dd) cutting the pipe string to length into ARE outer pipes or ARE inner pipes, The heating zone length is understood to be the length within which the temperature measured in degrees Celsius is at least 90% of a maximum drawing temperature.
[0061] This process enables more precise production of the hollow-core fiber. Preform manufacturing steps are explained above in the context of hollow-core fiber production, and these explanations are incorporated here. Definitions
[0062] Individual process steps and terms from the above description are defined in more detail below. These definitions are part of the description of the invention. In the event of a factual contradiction between one of the following definitions and the rest of the description, the statement in the description shall prevail. Anti-resonance elements
[0063] The antiresonance elements can be simple or nested structural elements of the hollow-core fiber. They have at least two walls that, viewed from the direction of the hollow core, have a negative curvature (convex) or no curvature (flat, straight). They are typically made of a material that is transparent to the working light, for example, glass, particularly doped or undoped SiO2, a plastic, particularly a polymer, a composite material, or a crystalline material. Anti-resonance element preform / anti-resonance element precursor
[0064] Anti-resonance element preforms are components or parts of the preform that essentially become anti-resonance elements in the hollow core fiber through simple elongation during the fiber drawing process. Anti-resonance element precursors are components or parts of the preform that only become anti-resonance element preforms through forming or directly. These can be simple or nested components to which additional positioning aids can be attached. They are originally present in the primary preform (cane).
[0065] Further processing of the primary preform, particularly through hot forming steps, can produce intermediate products in which the original anti-resonance element preforms are present in a modified form compared to the original. This modified form is also referred to here as an anti-resonance element preform or anti-resonance element precursor. Preform / primary preform / secondary preform
[0066] The preform is the component from which the antiresonant hollow-core fiber is drawn. It is a primary preform or a secondary preform created by further processing the primary preform. Further processing of the primary preform into a secondary preform from which the hollow-core fiber is drawn may involve a single or repeated execution of one or more of the following hot-forming processes: (i) elongation, (ii) collapse, (iii) collapse and simultaneous elongation, (iv) collapse of additional mantle material, (v) collapse of additional mantle material and subsequent elongation, (vi) collapse of additional mantle material and simultaneous elongation. Elongation / Collapse
[0067] During elongation, the primary preform is elongated. Elongation can occur without simultaneous collapse. Elongation can be performed to scale, so that, for example, the shape and arrangement of components or parts of the primary preform are reflected in the elongated final product. During elongation, the primary preform can also be drawn out of scale, and its geometry can be altered.
[0068] During collapse, an internal bore is narrowed or annular gaps between tubular components are closed or narrowed. Collapse is usually accompanied by elongation. Hollow core / Inner shell area / Outer shell area / Cane
[0069] The assembly consisting of at least one cladding tube and loosely or firmly fixed preforms or precursors for anti-resonance elements is also referred to here as the "primary preform" or "cane." The primary preform (cane) comprises the hollow core and a cladding region. This cladding region is also referred to as the "inner cladding region" if there is also an "outer cladding region," created, for example, by collapsing onto the cane, and if a distinction is to be made between these cladding regions. The terms "inner cladding region" and "outer cladding region" are also used for the corresponding regions in the hollow core fiber or in intermediate products obtained by further processing the primary preform.
[0070] The term "pipe inside" is also used as a synonym for "pipe inner surface," and the term "pipe outside" is also used as a synonym for "pipe outer surface." The term "internal bore" in connection with a pipe does not imply that the internal bore was created by a drilling process. Machining
[0071] This refers to mechanical manufacturing processes for the separation of a workpiece, in particular turning, cutting, drilling, sawing, milling, and grinding. This machining creates a longitudinal structure extending along the longitudinal axis of the cladding tube, which serves as a positioning aid for the anti-resonance element preforms. The longitudinal structure is accessible from the cladding tube's inner surface; it can also extend through the entire cladding tube wall to the outer surface. Particle size and particle size distribution
[0072] The particle size and particle size distribution of the SiO2 particles are characterized using the D50 values. These values are taken from particle size distribution curves, which show the cumulative volume of the SiO2 particles as a function of the particle size. The particle size distributions are often characterized using the respective D10, D50, and D90 values. The D10 value indicates the particle size not reached by 10% of the cumulative volume of the SiO2 particles, and accordingly the D50 and D90 values indicate the particle sizes not reached by 50% and 90% of the cumulative volume of the SiO2 particles, respectively. The particle size distribution is determined by light scattering and laser diffraction spectroscopy according to ISO 13320. Example
[0073] The invention is explained in more detail below with reference to an embodiment and a drawing. The drawing shows a schematic representation Figure 1 a primary preform with a cladding tube and anti-resonance element preforms positioned and fixed therein for producing a preform for a hollow core fiber based on a view of the radial cross-section, and Figure 2 a device for use in the tool-free production of ARE outer pipes and ARE inner pipes using a vertical drawing process.
[0074] During the production of the hollow core fiber or the preform for the hollow core fiber, a large number of components must be joined together. In addition, it can be helpful to seal existing gaps or channels in the preform during hot forming processes. For joining or sealing, an SiO 2 -based sealing or bonding compound is used, as known from DE 10 2004 054 392 A1. In this process, an aqueous slurry is produced by wet grinding quartz glass grains. This slurry contains amorphous SiO 2 particles with a particle size distribution characterized by a D 50 value of approximately 5 µm and a D 90 value of approximately 23 µm. Additional amorphous SiO 2 grains with an average grain size of approximately 5 µm are mixed into the base slurry. The slip used as a bonding compound has a solids content of 90%, which consists of at least 99.9 wt.% SiO2.
[0075] Figure 1 schematically shows a cane (primary preform 23) with a cladding tube 21 with a cladding tube wall 22, on whose inner surface anti-resonance element preforms 24 are fixed at previously defined azimuthal positions at equal intervals; in the exemplary embodiment, there are six preforms 24, in another preferred embodiment not shown, there is an odd number of preforms.
[0076] The cladding tube 21 is made of quartz glass and has a length of 1000 mm, an outer diameter of 27 mm, and an inner diameter of 20 mm. The antiresonance element preforms 24 are present as an ensemble of nested structural elements consisting of an ARE outer tube 24a and an ARE inner tube 24b. The ARE outer tube 24a has an outer diameter of 6.2 mm, and the ARE inner tube 24b has an outer diameter of 2.5 mm. The wall thickness of both structural elements (24a; 24b) is the same, amounting to 0.3 mm. The diameter ratio of the ARE outer tube is thus 1.107 and that of the ARE inner tube is 1.315. The lengths of the ARE outer tube 24a and ARE inner tube 24b correspond to the cladding tube length.
[0077] The anti-resonance element preforms 24 are fixed to the inner wall of the cladding tube 21 by means of the SiO 2 -based bonding compound 25.
[0078] The bonding compound 25 is applied locally to the cladding tube's inner surface in the area of the front ends, and the anti-resonance element preforms are placed thereon using a positioning template with a structurally predetermined star-shaped arrangement of holding arms for the individual anti-resonance element preforms 24. The positioning template is limited to the area around the two front ends of the cladding tube.
[0079] This method creates a precise and reproducible connection between the cladding tube 21 and the anti-resonance element preforms 24. For fixation, solidification of the bonding compound 25 at a low temperature is sufficient, thus avoiding excessive heating of the surrounding areas and thus deformation of the anti-resonance element preforms 24.
[0080] The temperature required for drying is below 300°C, which promotes dimensional stability of the preform and prevents thermal deterioration. Heating to higher temperatures around 800°C, for example during elongation of the preform into a hollow-core fiber, leads to further thermal hardening of the sealing or bonding compound, which is also suitable for forming opaque or transparent glass. This occurs through sintering or vitrification, whereby sintering to opaque glass requires comparatively lower temperatures and / or shorter heating times than vitrification to complete transparency. The sealing or bonding compound can thus be fully densified by heating and vitrified by heating during the hot-forming process. The sealing or bonding compound behaves like quartz glass; it becomes viscous and malleable.
[0081] The primary preform 23 is overclad with a quartz glass overcladding cylinder, whereby the overcladding cylinder collapses onto the cladding tube 1, and simultaneously the tube assembly is elongated into a secondary preform. The overcladding cylinder has an outer diameter of 63.4 mm and a wall thickness of 17 mm.
[0082] During the collapsing and elongation process, the coaxial arrangement of cladding tube 1 and overlay cylinder is fed from below into a temperature-controlled heating zone with the longitudinal axis oriented vertically and is softened zone by zone, starting with the upper end of the arrangement.
[0083] The heating zone is maintained at a target temperature of 1600 °C with a control accuracy of + / - 0.1 °C. This allows temperature fluctuations during the hot forming process to be limited to less than + / - 0.5 °C.
[0084] The secondary preform formed in the collapsing and elongation process has an outer diameter of approximately 50 mm and a cladding wall thickness of 16.6 mm, consisting of the outer cladding and inner cladding. The maximum wall thickness variation (largest value minus smallest value) of the antiresonance element preforms is less than 4 µm. The secondary preform is then drawn into the antiresonance hollow-core fiber.
[0085] The following table lists the pull-off parameters for different outer diameters before (BEFORE) and after (AFTER) the forming process. Table 1 Outer diameter VOR [mm] Outside diameter AFTER [mm] Sheath tube length [mm] Feed rate [mm / min] Extraction [mm / min] 90 70 1000 15 9,80 80 70 1000 15 4,59 40 20 1000 5 15 25 20 1000 10 5,63
[0086] The heating zone has a length of 100 mm. For example, a cladding tube with an outer diameter of 90 mm and a wall thickness of 10 mm results in a throughput of 27.6 g / min into the heating zone at a feed rate of 5 mm / min. At a feed rate of 15 mm / min, the throughput is 83 g / min. At a feed rate of 15 mm / min, a tube with an outer diameter of 25 mm and a wall thickness of 1 mm results in a throughput of 2.49 g / min.
[0087] The maximum deviation in the wall thickness of the anti-resonance element preforms in the preform is approximately 4 µm for all examples. Hollow-core fibers with an outer diameter of 200 µm and 230 mm, respectively, were drawn from the preforms, and the wall thicknesses of the anti-resonance elements were determined.
[0088] The Figure 2 The device shown is used for tool-free elongation of an initial cylinder 4 made of undoped quartz glass to an intermediate cylinder.
[0089] The outer surface of the starting cylinder is roughly ground using a peripheral grinder equipped with a #80 grinding stone, thereby essentially achieving the specified target outer diameter. The outer surface is then finely ground using an NC peripheral grinder. The inner surface of the resulting tube is honed entirely using a honing machine equipped with an #80 honing stone, with the degree of smoothness being continuously refined, and the final treatment is carried out with an #800 honing stone. The starting cylinder is then briefly etched in a 30% hydrofluoric acid etching solution. In this way, a starting cylinder with an outer diameter of 200 mm and an inner diameter of 70 mm is produced. This is then subjected to a vertical drawing process in a device according to Figure 2 elongated to an intermediate cylinder.
[0090] The device comprises a vertically oriented resistance heating furnace 1 enclosing a heating chamber 3 with a circular cross-section. The heating tube 1 consists of an annular element with an inner diameter of 240 mm, an outer diameter of 260 mm, and a length of 200 mm. The graphite heating tube 1 encloses the actual heating zone. It is extended on both sides by 55 mm wide extension pieces 5 made of graphite tube, which have an inner diameter of 250 mm and an outer diameter of 280 mm. The internal volume of the heating zone Vc is approximately 8140 mm 3
[0091] At the level of an upper detection level E1 (at the upper edge of the upper extension piece 5), a pyrometer 6 is arranged, which measures the surface temperature of the output cylinder 1. At the level of a lower detection level E2 (at the lower edge of the lower extension piece 5), another pyrometer 7 is arranged, which measures the surface temperature of the elongated pipe string 12. The temperature measured values of the pyrometers 6 and 7, as well as the temperature of the heating pipe 1 measured by the pyrometer 16, are each fed to a computer 8.
[0092] The upper end of the output cylinder 4 is connected via a welded joint 9 to a quartz glass holding tube 10, by means of which it can be displaced in the horizontal and vertical directions.
[0093] The starting cylinder 4 is aligned so that its longitudinal axis runs as coaxially as possible to the central axis 2 of the heating tube 1. It is fed into the heating chamber 3 (starting with its lower end) from above at a constant feed rate, where it is softened. From the softened area, an intermediate cylinder tube strand 12 is drawn vertically downwards, forming a drawing bulb 11. The intermediate cylinder tube strand 12 is guided along a wall thickness gauge 14, which is also connected to the computer 8, so that the wall thickness of the drawn tube strand 12 can be recorded during the drawing process and evaluated using the computer 8. The continuous internal bore of the starting cylinder 4 and the intermediate cylinder tube strand 12 is designated 13. The tube withdrawal speed is measured by a withdrawal device 15 and adjusted via the computer 8.
[0094] In the vertically aligned heating tube 1, a quartz glass hollow cylinder 4 with an outer diameter of 200 mm and an inner diameter of 75 mm is adjusted so that its longitudinal axis is coaxial with the central axis 2 of the heating tube 1. The starting cylinder 4 is heated in the heating zone to a temperature above 2,200 °C and drawn off at a predetermined feed rate. From the forming drawing bulb 11, the quartz glass tube strand 12 is drawn at a controlled drawing speed to a nominal outer diameter of 40 mm and an inner diameter of 30 mm (wall thickness: 5 mm) as an intermediate cylinder. This exhibits a smooth, molten and particle-free surface. It is used in a second elongation step in a second drawing machine as the starting cylinder for the production of ARE outer tubes and ARE inner tubes, respectively. The second drawing machine used for this purpose is similar to that used by Figure 2, it differs primarily in the length and inner diameter of its heating zone. The heating zone (the heating tube) has an inner diameter of 120 mm, an outer diameter of 140 mm, and a length of 100 mm.
Claims
1. A method for producing an anti-resonant hollow-core fiber which comprises a hollow core extending along a fiber longitudinal axis and an inner casing region that surrounds the hollow core and comprises a plurality of anti-resonant elements, comprising the method steps of: (a) providing a cladding tube (21) having a cladding tube longitudinal axis, along which a cladding tube wall (22) extends, which wall is delimited by an inner face and an outer face, (b) providing tubular anti-resonant element preforms (24), each having at least one ARE outer tube (24a) and optionally at least one ARE inner tube (24b), (c) arranging the anti-resonant element preforms (24) at desired positions on the inner face of the cladding tube wall (22) to form a primary preform (23), which primary preform comprises a hollow core region and an inner casing region, and (d) elongating the primary preform (23) to form the hollow-core fiber or further processing the primary preform (23) to form a secondary preform from which the hollow-core fiber is drawn, the further processing comprising carrying out one or more of the following hot-forming processes once or repeatedly: (i) elongation, (ii) collapse, (iii) collapse and simultaneous elongation, (iv) collapse of additional casing material, (v) collapse of additional casing material and subsequent elongation, (vi) collapse of additional casing material and simultaneous elongation, characterized in that in order to provide the tubular anti-resonant element preforms according to method step (b), the ARE outer tube (24a) and / or the ARE inner tube (24b) is produced using a vertical drawing process without a mold, which comprises the following method steps: (aa) providing a starting hollow cylinder (4) made of glass, which has a cylinder longitudinal axis (2) and an outer cylinder lateral face and an inner cylinder lateral face, (bb) a first elongation process, in which the starting hollow cylinder (4) having the vertically oriented longitudinal axis (2) is continuously fed to a first heating zone (3) having a first heating zone length LH1, softened in regions therein, and an intermediate cylinder (12) is withdrawn from the softened region without a mold, (cc) a second elongation process, in which the intermediate cylinder (12) or an elongated intermediate cylinder obtained from the intermediate cylinder (12) by elongation and having a vertically oriented longitudinal axis is continuously fed to a second heating zone having a second heating zone length LH2, softened in regions therein, and a tube string having an outer diameter Ta and an inner diameter Ti is withdrawn from the softened region without a mold, where: LH2 < LH1 and Ta / Ti < 1.5, and (dd) cutting the tube string to length to form ARE outer tubes (24a) or ARE inner tubes (24b), the heating zone length being understood to be the length within which the temperature measured in degrees Celsius is at least 90% of a maximum drawing temperature.
2. The method according to claim 1, characterized in that the provision of the starting hollow cylinder (4) according to method step (aa) comprises a mechanical machining of the cylinder lateral faces for setting starting hollow cylinder final dimensions, comprising an outer diameter Ca of at least 90 mm, an inner diameter Ci and a diameter ratio Ca / Ci of less than 2.8.
3. The method according to claim 2, characterized in that the mechanical machining of the cylinder lateral faces of the starting hollow cylinder (4) is carried out by cutting, milling, drilling, grinding, honing and / or polishing.
4. The method according to either claim 2 or claim 3, characterized in that the outer diameter Ca is set to at least 150 mm, preferably at least 180 mm.
5. The method according to any of claims 1 to 4, characterized in that the tube string is drawn with an outer diameter Ta in the range of 7 to 35 mm.
6. The method according to any of claims 1 to 5, characterized in that the first heating zone length LH1 is at least 200 mm, and preferably between 150 and 400 mm, and in that the second heating zone length LH2 is at most 140 mm, and preferably between 50 and 140 mm.
7. The method according to any of claims 1 to 6, characterized in that the wall thickness of the tube string is set to a value between 0.2 and 2 mm, preferably to a value between 0.22 and 1.2 mm, and in that the diameter ratio Ta / Ti is set to a value in the range of 1.02 to 1.14, preferably to a value in the range of 1.04 to 1.08.
8. The method according to any of claims 1 to 6, characterized in that the wall thickness of the tube string is set to a value between 0.2 and 2 mm, preferably to a value between 0.22 and 1.2 mm, and in that the diameter ratio Ta / Ti is set to a value in the range of 1.05 to 1.5, preferably to a value in the range of 1.14 to 1.35.
9. The method according to any of claims 1 to 8, characterized in that the drawing ratio in the sum of the elongation process is set to a value in the range of 38 to 78.
10. The method according to any of the preceding claims, characterized in that the ARE outer tube (24a) or the ARE inner tube (24b) has an outer lateral face, and in that after completion of the vertical drawing process, the outer lateral face is free of particles with a size of more than 0.005 mm, and in that the ARE outer tube (24a) or the ARE inner tube (24b) is made of quartz glass containing a tungsten concentration of less than 2 ppb by weight.
11. A method for producing a preform for an anti-resonant hollow-core fiber which comprises a hollow core extending along a longitudinal axis of the fiber and an inner casing region that surrounds the hollow core and comprises a plurality of anti-resonant elements, comprising the method steps of: (a) providing a cladding tube (21) having a cladding tube longitudinal axis, along which a cladding tube wall (22) extends, which wall is delimited by an inner face and an outer face, (b) providing tubular anti-resonant element preforms (24), each having at least one ARE outer tube and optionally at least one ARE inner tube, (c) arranging the anti-resonant element preforms (24) at desired positions on the inner face of the cladding tube wall (22) to form a primary preform (23), which primary preform comprises a hollow core region and an inner casing region, and (d) optionally further processing the primary preform (23) to form a secondary preform for the hollow-core fiber, the further processing comprising carrying out one or more of the following hot-forming processes once or repeatedly: (i) elongation, (ii) collapse, (iii) collapse and simultaneous elongation, (iv) collapse of additional casing material, (v) collapse of additional casing material and subsequent elongation, (vi) collapse of additional casing material and simultaneous elongation, characterized in that anti-resonant element preforms (24) are provided, each having at least one ARE outer tube (24a) and optionally at least one ARE inner tube (24b), the ARE outer tube (24a) and / or the ARE inner tube (24b) being produced by means of a vertical drawing process without a mold, which comprises the following method steps: (aa) providing a starting hollow cylinder (4) made of glass, which has a cylinder longitudinal axis (2) and an outer cylinder lateral face and an inner cylinder lateral face, (bb) a first elongation process, in which the starting hollow cylinder (4) having the vertically oriented longitudinal axis (2) is continuously fed to a first heating zone (3) having a first heating zone length LH1, softened in regions therein, and an intermediate cylinder (12) is withdrawn from the softened region without a mold, (cc) a second elongation process, in which the intermediate cylinder (12) or an elongated intermediate cylinder obtained from the intermediate cylinder (12) by elongation and having a vertically oriented longitudinal axis is continuously fed to a second heating zone having a second heating zone length LH2, softened in regions therein, and a tube string having an outer diameter Ta and an inner diameter Ti is withdrawn from the softened region without a mold, where: LH2 < LH1 and Ta / Ti < 1.5, and (dd) cutting the tube string to length to form ARE outer tubes (24a) or ARE inner tubes (24b), the heating zone length being understood to be the length within which the temperature measured in degrees Celsius is at least 90% of a maximum drawing temperature.