METHOD FOR PRODUCE A FOAMED PLASTIC MOLD WITH A FILM COATING
Patent Information
- Application Number
- DE502020009463
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-10-15
- Filing Date
- 2020-10-13
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2040-10-13
AI Technical Summary
Existing methods for producing foamed plastic moldings result in products with microcavities and rough surfaces, making them unsuitable for painting and requiring additional film layers, which are applied in separate work steps, increasing production time and cost.
A manufacturing process using a tool mold with a film layer coating where granules are heated to form a liquid film layer, applied to the foamed plastic molding, and then cooled to create a closed, continuous film layer coating directly on the molding, eliminating the need for additional film application steps and enhancing surface quality.
The process produces foamed plastic moldings with a closed, smooth surface, allowing direct painting and integration into existing production lines, reducing production time and costs while ensuring a strong, burr-free finish.
Description
[0001] The invention relates to a method for producing a foamed plastic body with a film layer coating using a tool mold with at least one tool cavity for forming a shaping mold cavity.
[0002] Manufacturing processes and one-piece or multi-piece molds for producing a molded body from foamed plastic are known from the prior art. In the known processes, the one-piece or multi-piece mold, comprising at least one mold cavity to form a shaping cavity, is filled with expandable particles and / or foam beads and permeated with pressurized steam at temperatures and humidity levels such that the particles and / or foam beads expand and fuse together within the mold cavity (this process is also referred to as the steam chamber process).Furthermore, it is known from the prior art to heat the mold cavity via two opposing mold halves and the inner surfaces of the mold cavities, and subsequently to fill the mold cavity with expandable particles and / or foam beads. These absorb the heat energy via the heated mold cavities and expand within the mold cavity, fusing together to form a foamed plastic body. The mold cavity, defined by the at least one mold cavity, determines the geometry of the foamed plastic body to be produced. After cooling, the plastic body produced in the mold can be ejected from the mold by opening it.
[0003] Such a device and a method for producing a foamed plastic molded body are known, for example, from DE 10 2009 006 507 B3.
[0004] The foamed plastic molded parts known from the prior art do not have a closed or continuous surface after completion of the aforementioned manufacturing process. Rather, microcavities remain on the surface of the foamed plastic molded parts due to the expansion process, into which fluids, for example, can enter. A further disadvantage is that, due to the aforementioned cavities, the plastic molded parts do not have a closed, flat surface structure and are therefore not directly suitable for painting, for example, for use in automotive engineering.
[0005] Furthermore, the foamed plastic molded parts known to date only possess the color of the expanded or foamed plastic granules used as the starting material. For certain applications, such as in the food industry, but also in the automotive sector, it is a requirement to produce foamed plastic molded parts with a closed surface and low roughness so that the molded parts can be painted directly and used, for example, as bumpers in a motor vehicle.
[0006] It is already known from the prior art to coat the aforementioned foamed plastic molded bodies with additional film layers in order to obtain a closed and flat surface for the material molded body, whereby a disadvantage of the previous manufacturing processes is that the aforementioned plastic films have to be applied to the foamed plastic molded bodies in a separate work step.
[0007] From GB 2 494 484 A, a method for forming plastic from a particulate plastic material and a heat-activated, expandable foam filler material is known, comprising the following steps: (i) providing a first and a second mold part; (ii) heating the mold parts, at least on their surface sections, to a temperature of about 100 to about 500 degrees Celsius to make the particles meltable or sinterable; (iii) bringing the mold parts into contact with the particulate plastic material; (iv) bringing the expandable foam plastic filler material into contact with the particles; (v) melting or sintering at least a portion of the plastic particles on each mold part to form a molded skin of about 0.001 cm to 3.0 cm; (vi) bringing the heated mold parts together so that the heat from the heated mold parts activates the expandable foam to form a composite sandwich.
[0008] JP S63 312248 A describes the manufacture of a part for a vehicle interior, which is produced by laminating a skin of a synthetic resin, a foamed layer and a fiber-containing layered base material, which are joined together and brought into a predetermined shape.
[0009] GB 2 460 838 A discloses a machine and a method for molding plastic articles and comprises a pair of articulated hollow molds that are heated and cooled and can be clamped together. The method involves introducing a plastic particle material into each mold when they are in the open position and heating the molds to form a plastic skin that lines each mold. Subsequently, an expandable filler material is poured into one mold, and the two molds are closed to form a completely enclosed cavity. The plastic skins in the two molds fuse together to form a continuous plastic shell that completely encloses the filler material.
[0010] From DE 100 33 877 A1, a process for producing molded parts in a mold is known, wherein the molded parts are made of particle foam from polymer foam particles comprising at least one polymer cover layer. The particles are fused together, at least superficially, and form a closed surface.
[0011] Based on the prior art described above, the object of the present invention is to propose a simplified manufacturing process for producing a foamed plastic molded body with a film coating, which is more cost-effective and can be carried out in a reduced manufacturing time, and which also allows the properties of the plastic molded body to be specifically adjusted to the intended application.
[0012] The object of the present invention is solved according to the invention by a manufacturing process for producing a foamed plastic molded body with a film layer coating and the use of a tool mold with at least one tool cavity for forming a shaping mold cavity, comprising the process steps: A) Heating at least one cavity of the mold; B) Applying granules to the heated cavity; C) Melting the granules in the heated cavity to form a liquid film; D) Applying the liquid film to a foamed plastic body to form a film coating on the surface of the plastic body by fusing the liquid film with the surface; and E) Cooling the cavity and ejecting the plastic body coated with the film.
[0013] In process step E), the mold, and in particular the heated at least one mold cavity, is cooled down to the demolding temperature. Subsequently, the plastic molded body with its film coating is ejected or formed from the mold as a component falling out of the mold. The granules applied in process step B) are the desired material from which the film coating to be formed for the foamed plastic molded body is created. In process step A), the at least one mold cavity is heated to at least the melting temperature of the granules applied in process step B) to form a liquid film layer in process step C), which is formed from the melted granules. According to the invention, the temperature of the at least one mold cavity is controlled during the execution of the process.It must be controlled so that, throughout the entire period of carrying out at least process steps B) to D), the temperature is essentially at least above the melting temperature of the applied granules.
[0014] The method according to the invention has the advantage that a continuous film coating can be produced on the plastic molded body using existing tools, in particular multi-part molds. The additional devices previously required according to the prior art for applying, in particular, a plastic film layer or textile layers with a plastic layer to create a coating on the plastic molded body become obsolete. In particular, the method according to the invention is advantageous because it can be seamlessly integrated into or directly connected to the existing production process, resulting in significant time savings and increased efficiency.By melting the granules in process step C), a continuous film layer of the granulate material with a defined film layer thickness is formed in the heated mold cavity. This continuous film layer is present in a molten or liquid state in the heated mold cavity after completion of process step C). In process step D), the molten film layer is applied in its liquid state, at least partially, to the surface of the foamed plastic molded part to form a continuous film coating. The film layer then fuses or solidifies directly onto the existing surface of the molded plastic part. The film layer can cover the entire surface of the foamed plastic molded part or, alternatively, only partial surface areas.The inventive method further has the advantage that no burrs are formed on the manufactured plastic molded body, thus eliminating the need for any further work on the manufactured finished parts, for example to remove a sprue or a protruding burr.
[0015] According to the invention, it can be provided that, prior to carrying out process steps A) to E), the actual plastic mold body is initially produced in the mold using a foaming or expansion process, as is known, for example, from the prior art, the mold is then opened, the foamed plastic mold body remaining in at least one first mold cavity, and process steps A) to E) are subsequently carried out on at least one second opposing mold cavity, the application of the film layer according to process step D) is effected by closing the mold again around the already expanded plastic mold body, and cooling in process step E) of the at least one mold cavity takes place in the closed mold state.The aforementioned embodiment of the manufacturing process according to the invention has the advantage that the production of the film layer coating is carried out immediately following the prior art process for producing foamed plastic molded parts using known expansion processes, and the application of the film layer is made possible according to the invention using the existing mold. Due to the immediate subsequent production and application of the film layer following the manufacture of the plastic molded part, good bonding and adhesion of the film layer to the plastic molded part can be achieved, as intermediate contamination of the bonding surface of the plastic molded part is avoided.
[0016] The plastic molded body can be produced via an expansion process in the cavity of the mold using all foamable particle foams, such as: EPS (expandable polystyrene), EPP (expandable polypropylene), EPE (expandable polyethylene), expandable thermoplastic polyurethane (E-TPU), and polystyrene containing graphite or carbon. In an alternative embodiment of the manufacturing process, it is also possible to produce the plastic molded body via an expansion process in a first mold and subsequently carry out the process steps according to the invention in a second mold.
[0017] In a further preferred embodiment of the manufacturing process according to the invention, it can be provided that process steps A) to C) are first carried out in the area of the at least one tool cavity, then the tool mold is closed, and the mold cavity of the tool mold is filled with a first expandable plastic granulate or foam beads, and then the first expandable plastic granulate or foam beads are expanded in the mold cavity, wherein process step D) is carried out by expanding the plastic molded body against the liquid film layer formed on the at least one tool cavity and fusing it directly.
[0018] It is particularly advantageous to provide that the expansion process of the first expandable plastic granule is prematurely terminated or stopped after a defined period, so that only a portion of the plastic granule or foam beads expands. The unmelted or unexpanded portion of the first plastic granule is then removed from the mold cavity, leaving only a layer of the first expanded plastic granule adhering to the film layer. The resulting intermediate article can remain in the mold cavity for further processing or be demolded from it.
[0019] Preferably, if the intermediate article remains in the mold cavity after the removal of the unexpanded portion of the first plastic granules, the mold cavity can be filled with a second expandable plastic granule or foam beads, which are then expanded to form the plastic molded body. The described method can produce a plastic molded body with a film layer, wherein below this film layer is a layer of first expanded plastic particles or foam beads of a first material, which is fused to or bonded with the film layer, and below this is a second layer of second expanded plastic particles or foam beads, which is formed from a second material and is at least connected to or bonded with the first layer.The described process makes it possible to produce a plastic molded body consisting of two different foamed granules.
[0020] Preferably, at least two different expandable plastic granules with different material properties are used for the manufacturing process. In a first exemplary embodiment, the first expandable plastic granule can be selected such that it results in a local foam body with a low density and simultaneously high elasticity, and the second granule results in a local foam body with a higher density and lower elasticity compared to the first expandable plastic granule. Consequently, a resulting foamed plastic molded body can be obtained which has a soft and stretchable surface below the film coating in the surface area, wherein the lower local foam area is structurally stable and non-deformable.
[0021] In an alternative embodiment, the first expandable plastic granulate can have a higher stiffness and density than the second expandable plastic granulate, such that an article with a very stiff surface and reduced weight can be obtained. The provision of a first foam layer formed from an expandable plastic granulate with high stiffness and simultaneously high density has the advantage that film coatings with a low film thickness can be achieved.
[0022] By selectively choosing the first and second expandable plastic granules, the resulting local properties of the foam layers forming the plastic molded body can be specifically influenced. Furthermore, it is possible to use more than two different expandable plastic granules to form the plastic molded body by repeating the process. In a preferred embodiment, it is accordingly possible to fill the mold cavity with at least two further expandable plastic granules or foam beads after removing the unexpanded portion of the first plastic granule, while leaving the intermediate article in the mold cavity. These are then expanded to form the plastic molded body. The expansion process of each of these further expandable plastic granules can be prematurely terminated.The process can be stopped prematurely after a defined period, allowing only a portion of the additional plastic granules or foam beads to expand. The unfused or unexpanded portion of the additional plastic granules can then be removed from the mold cavity, enabling the production of layers of defined thicknesses of the additional expanded plastic granules. The described process makes it possible to produce a plastic molded body with a film layer. Beneath this film layer is a layer of initial expanded plastic particles or foam beads of a primary material, which is fused to or bonded to the film layer. Below this are any number of further layers of additional expanded plastic particles or foam beads.The process involves the production of foam beads, which can be formed from other materials and which are at least connected to or bonded to the first layer. The described method makes it possible to produce a molded plastic body with a film layer and any number of underlying layers of expanded plastic particles. Consequently, a so-called multilayer molded body with, in particular, 3 to 6 layers can be produced.
[0023] Furthermore, it can be provided that in process step B) the granules are applied to the surface of the multi-part mold beyond the area of the at least one mold cavity, and that at least one part of the multi-part mold includes a sealing ring which, when the mold is closed, causes the granules to form a bead outside the area of the at least one mold cavity in the edge region of the at least one first and / or second mold cavity. The sealing ring is arranged on a first part of the mold and, when the mold is closed, extends over the surrounding area of the opposite mold cavity of the at least one second mold part.In the aforementioned coating process, the granules applied outside the mold cavity, while molten, are compressed relative to the opposite mold cavity by the movement of the sealing ring, forming a bead that defines the cavity. This prevents a visible edge at the end of the film coating when applied only to a portion of the surface of the plastic molded part. Furthermore, the bead provides a better bond between the circumferential edge of the film coating and the foam body, thus preventing detachment at the edges of the film coating. A particularly preferred feature is a conical mold shape opposite the sealing ring, facilitating its insertion into the mold.
[0024] Furthermore, it is preferably provided according to the invention that the granules for the film layer coating are applied to the at least one tool cavity in process step B) by means of a spray gun.
[0025] According to a further preferred embodiment of the manufacturing process according to the invention, it can be provided that in process step A) the at least one tool cavity to be heated is heated by introducing a heating medium via corresponding heating channels in the at least one tool cavity. For example, heated oil, water, or a water vapor mixture can be supplied as the heating medium.
[0026] Alternatively, the at least one tool cavity can be heated by at least one active heating device, such as an electric heating element, in particular a resistance heating element, a PTC thermistor, or an inductive heating element.
[0027] It is also preferable to provide for the heating of at least one tool cavity directly with an external heat source, such as a flow of heated air.
[0028] According to another embodiment, the at least one tool cavity can be heated via a radiant heater, such as an infrared heater, or alternatively also via at least one heating burner.
[0029] Furthermore, it may be provided that in process step A) the at least one tool cavity to be heated is heated to at least a temperature above the melting temperature of the applied granulate, in particular to a temperature in the range of 80°C to 260°C.
[0030] According to a preferred embodiment, in process step B) a powdered thermoplastic granulate is applied to the at least one tool cavity. The thermoplastic granulate can then be melted by heating the tool cavity, resulting in a continuous molten layer of the thermoplastic material within the tool cavity.
[0031] The granules can also be mixed with additives and applied to at least one tool cavity. Glass fibers and / or carbon fibers, in particular, could be used as granulated additives.
[0032] According to the invention, it can be provided that during or after carrying out process step C), a layer of nonwoven fabric or textile, such as a woven or knitted fabric, is inserted into at least partial areas of the surface of the at least one tool cavity and preferably embedded in or impregnated by the liquid film layer. The inserted layer is particularly preferably able to have defined outer contours and dimensions.
[0033] A thermoplastic granulate in a defined RAL color can be applied to at least one mold cavity, creating a film coating in the desired RAL color. Furthermore, granulates with special properties can be used, such as dissipative properties, flame resistance, food-grade suitability, UV resistance, heat resistance, increased water resistance, increased dielectric strength, and increased abrasion resistance. Additionally, a plastic that forms a material-bonded connection with the molded plastic part can be used for the film coating. This allows for further customization of the manufactured molded plastic part with desired properties.
[0034] According to the invention, it can also be provided that both the molded plastic body and the film coating are made of the same thermoplastic material to create a mono-material composite; for example, a combination of PP and EPP or PS and EPS can be used. Due to the mono-material composite, the manufactured molded plastic body with film coating can be recycled more easily because of the uniform material.
[0035] Furthermore, according to the invention, at least one tool cavity can be used with a defined surface texture, which creates a defined surface feature of the film layer. For example, the surface of the film layer coating can be provided with defined textures, extremely smooth or rough surfaces with defined roughness, or hook-and-loop surfaces.
[0036] According to a particularly preferred embodiment of the manufacturing process according to the invention, it is provided that in process step B) a powdered polypropylene (PP) is applied to the at least one tool cavity.
[0037] According to a further particularly preferred embodiment, it can be provided that in process step B) granules are applied only to defined partial areas of the at least one tool cavity to form at least one partial film layer, wherein in particular partial areas of the at least one tool cavity can be covered in order to prevent granule application there in process step B).
[0038] It is also preferable to apply the granules in defined, different layer thicknesses to different sections of the mold cavity, such that a film coating with locally varying thicknesses can be produced on the foamed plastic body. The aforementioned method makes it possible for the first time to selectively create surface areas with different strengths or flexural stiffnesses within the film coating. In particular, it allows for the introduction of weakened areas in the surface, which, for example, when the plastic body is used in the automotive sector, result in defined deformation behavior, such as in the event of an impact.
[0039] In particular, it may be provided that in process step B) a granulate with a layer thickness in the range of 0.05 mm to 2 mm is applied to the tool cavity. The layer thickness of the granulate can be determined depending on the underlying expanded plastic granulate.
[0040] According to a further preferred embodiment, it can be provided that in process step E) the at least one tool cavity to be cooled is cooled convectively and / or conductively.
[0041] According to a particularly preferred embodiment, in process step E) the at least one tool cavity to be cooled is cooled by passing a cooling medium through channels of the at least one tool cavity. The supplied cooling medium can be, for example, a cooling liquid, in particular oil, cooling air or cooling water.
[0042] Alternatively, it may be provided that in process step E) the at least one tool cavity to be cooled is cooled by spraying a cooling medium onto at least one tool cavity to be cooled via at least one nozzle device, in particular it may be provided that water in the liquid state is sprayed onto the at least one tool cavity to be cooled via several nozzle devices, in particular atomizing nozzles.
[0043] According to the invention, it can further be provided that the temperature of the at least one tool cavity to be heated in process step A) is monitored by means of a temperature sensor. Preferably, the desired process temperatures can also be monitored by means of the temperature sensor during the entire manufacturing process or in defined process steps and controlled specifically depending on the measured values.
[0044] Furthermore, it may be possible to use the temperature sensor to control the supply of heating medium or, alternatively, the electric nozzle devices.
[0045] In particular, it may be preferably provided that, for the production of the foamed plastic molded body, after carrying out process steps A) to C), at least one particle foam granulate is fed into the closed mold via at least one injector device. The mold can also be locally filled with different expandable plastic granulates via several injector devices.
[0046] Furthermore, according to the invention, process steps A) to C) can be carried out on at least one external tool cavity, which is brought together with the tool shape in process steps D) and E) by means of a displacement to form the mold cavity. For example, a rotary table tool with several tool cavities can be used according to the invention.
[0047] Some examples of the manufacturing process according to the invention are described below. Examples 1, 2 and 3:
[0048] A square mold measuring 370 × 370 × 60 mm was used to produce sheets using a steam chamber process based on EPP (expanded polypropylene foam particles, trade names Eperan-PP VB45, M30, and VB15 from Kaneka Belgium NV). The sheets were stabilized in an oven at 80°C for 24 hours and stored at ambient conditions (23°C - 50% relative humidity). A circular heating plate was electrically heated to 220°C, and granules (polypropylene "Gray EX1Y 1876" from Axalta Coating Systems GmbH) were sprayed onto the heated plate and melted. The EPP sheet was pressed onto the layer of molten granules, the sheet was cooled with air, and the result was a film-coated foamed plastic part. Examples 4 and 5:
[0049] A cavity of a tool for manufacturing bowls (Example 4) and a cavity of a tool for manufacturing an A-pillar trim for vehicles (Example 5) were heated to 185°C and 180°C, respectively, using Variotherm technology. Variotherm technology is a heating and cooling system that allows for precise temperature control in all areas of a tool. The tool cavity does not necessarily have to be integrated into the steam chamber of the molding machine. Granules (polypropylene "Black EX1Y 1886" or "EX1Y 1886 Blue 565" from Axalta Coating Systems GmbH) were sprayed onto the heated cavity and melted. The tool was closed and the cavity was filled with EPP - expanded polypropylene foam particles (trademarks "Eperan-PP MN20" and "Eperan-PP VB 20" of Kaneka Belgium NV) and the steam chamber process was applied.In both cases, a foamed plastic part could be manufactured that was partially 100% covered with a film layer in the desired areas. Examples 6, 7, 8, 9, 10 and 11:
[0050] Tools for manufacturing a bowl (Examples 6, 7) and an A-pillar trim for vehicles (Examples 8, 9, 10, 11) were used to produce foamed plastic parts using a steam chamber process based on EPP foam particles made of expanded polypropylene (trademarks Eperan-PP VB30, VB20, M30 and MN20 from Kaneka Belgium NV). At the end of the cycle, the part was not ejected but remained in one cavity. The other cavity was heated to 180–185°C using variotherm technology. Granules (polypropylene "Black EX1Y 1886" and "EX1Y 1886 Blue 565" from Axalta Coating Systems GmbH) were sprayed onto the surface of the heated cavity and melted. The tool was then closed and cooled. In both cases, a foamed plastic part could be manufactured that was partially 100% covered with a film layer in the desired areas. Examples 12 and 13
[0051] A vehicle A-pillar trim was manufactured using a steam chamber process based on EPP – expanded polypropylene foam particles (trademarks Eperan-PP VB20 and M30 from Kaneka Belgium NV). The A-pillar trim was stabilized in an oven at 80°C for 24 hours and stored at ambient conditions (23°C – 50% relative humidity). A cavity of the A-pillar trim was heated to 180°C using Variotherm technology. Granules (polypropylene "Black EX1Y 1886" from Axalta GmbH) were sprayed onto the heated cavity and melted. The foamed A-pillar trim was pressed onto the layer of molten granules, the sheet was cooled, and a foamed plastic part with a film coating was produced. This method has proven very practical for small production runs. Example 14:
[0052] The cavity of the A-pillar trim was heated to 180°C using Variotherm technology. A granulate (polypropylene "Black EX1Y 1886" from Axalta Coating Systems GmbH) was sprayed onto the heated cavity and melted. The mold with the hot cavity was closed, and expanded polypropylene foam particles (trademark EPERAN-PP M30 from Kaneka Belgium NV), type X, were filled into the mold. Some of these particles adhered to the molten film layer, forming a first, low-density (soft) layer. The non-adherent, excess foam particles were vacuumed out of the cavity. Type Y foam particles (trademark EPERAN-PP VB20 from Kaneka Belgium NV) were then filled into the mold, and the steam chamber process was applied. This resulted in the production of a foamed plastic part that was partially, and in the desired areas, 100% covered with a film layer.Furthermore, by using type X and type Y, it was possible to create two layers with different densities (soft and hard). Example 15:
[0053] The cavity of the A-pillar trim was heated to 180°C using Variotherm technology. Granules (polypropylene "Black EX1Y 1886" from Axalta Coating Systems GmbH) were sprayed onto the heated cavity and melted. The mold with the hot cavity was closed, and expanded polypropylene foam particles (trademark EPERAN-PP M30 from Kaneka Belgium NV), type X, were added. Some of these particles adhered to the molten film layer, forming a low-density (soft) first layer. The cavity was then cooled. The non-adherent, excess expanded polypropylene foam particles were vacuumed out of the mold, and the film layer, including the layer of adhering foam particles of type X, was removed and stored. At a later time, this film layer with the partially melted layer of foam particles was reintroduced into a mold.Expanded polypropylene foam particles of type Y (trademark Eperan-PP VB20 by Kaneka Belgium NV) were blown into the mold and the steam chamber process was applied. A foamed plastic part was produced that was partially, in the desired areas, 100% covered with a film layer. Furthermore, by using types X and Y, two layers with different densities (soft and hard) could be achieved. Table 1: Description of examples 1 to 15 and of comparison example 1 Example shape Pre-foamed foam particles method Molded part density Heating system used Heating temperature Granule designation Thickness range of the film coating Coverage by film coating Embossing Unit - - Table 2 g / l - °C - mm % - Ex 1 plate Eperan-PP VB45 3 20 Electrically heated and air-cooled plate 220 EX1Y 1876 Grey 0,45 - 0,55 100 No unwanted unevenness Ex 2 plate Eperan-PP M30 3 45 Electrically heated and air-cooled plate 220 EX1Y 1876 Grey 0,45 - 0,55 100 No unwanted unevenness Ex 3 plate Eperan-PP VB15 3 60 Electrically heated and air-cooled plate 220 EX1Y 1876 Grey 0,45 - 0,55 100 No unwanted unevenness Ex 4 Bowl Eperan-PP MN20 1 45 Variotherm 185 EX1Y 1886 Black 0,65 - 0,85 100 No unwanted unevenness Ex 5 A-pillar Eperan-PP VB20 1 45 Variotherm 180 EX1Y 1886 Blue 565 0,90- 1,10 100 No unwanted unevenness Ex 6 Bowl Eperan-PP MN20 2 45 Variotherm 185 EX1Y 1886 Black 0,65 - 0,85 100 No unwanted unevenness Ex 7 Bowl Eperan-PP VB30 2 30 Variotherm 185 EX1Y 1886 Black 0,65 - 0,85 100 No unwanted unevenness Ex 8 A-pillar Eperan-PP M 30 2 30 Variotherm 180 EX1Y 1886 Black 0,90- 1,10 100 No unwanted unevenness Ex 9 A-pillar Eperan-PP M3 0 2 30 Variotherm 180 EX1Y 1886 Blue 565 0,90- 1,10 100 No unwanted unevenness Ex 10 A-pillar Eperan-PP VB 20 2 45 Variotherm 180 EX1Y 1886 Black 0,90- 1,10 100 No unwanted unevenness Ex 11 A-pillar Eperan-PP VB 20 2 45 Variotherm 180 EX1Y 1886 Blue 565 0,90- 1,10 100 No unwanted unevenness Ex 12 A-pillar Eperan-PP M 30 3 30 Variotherm 180 EX1Y 1886 Black 0,90- 1,10 100 No unwanted unevenness Ex 13 A-pillar Eperan-PP VB20 3 45 Variotherm 180 EX1Y 1886 Black 0,90- 1,10 100 No unwanted unevenness Ex 14 A-pillar Eperan-PP M30 (X) Eperan-PP VB2 0 (Y) 4 30 (X) 4 5 (Y) Variotherm 180 EX1Y 1886 Black 0,90- 1,10 100 No unwanted unevenness Ex 15 A-pillar Eperan-PP M30 (X) Eperan-PP VB2 0 (Y) 5 30 (X) 4 5 (Y) Variotherm 180 EX1Y 1886 Black 0,90- 1,10 100 No unwanted unevenness Comparison example 1 plate Eperan-PP VB30 - 30 - - - - - Presence of microcavities Table 2: Methods used in samples Ex 1 to Ex 15 to produce foamed plastic parts with a film coating: Proceedings Step 1 Step 2 Step 3 Step 4 Step 5 Step 6 Step 7 Step 8 Step 9 1 A: Heating the tool cavity using a variotherm (1)< B + C: Spray (2) and melt the granules Close tool D: Application of the film layer in the steam chamber process for the production of foamed plastic parts E: Cooling and ejection of the foamed plastic part with film coating 2 Steam chamber process for the production of foamed plastic parts Opening the tool without ejecting the foamed plastic part A: Heating the tool cavity using a variotherm (1)< B + C: Spray (2) and melt the granules D: Close the tool and apply the film to the foamed plastic part. E: Cooling and ejection of the foamed plastic part with film coating 3 Steam chamber process for the production of foamed plastic parts Stabilizing the foamed plastic part in the oven at 80°C Storage of the foamed plastic parts A: Heating the tool cavity using a variotherm (1)< B + C: Spray (2) and melt the granules D: By pressing, join the intermediately stored foamed plastic part with the molten granulate film. E: Cooling and ejection of the foamed plastic part with film coating 4 A: Heating the tool cavity using a variotherm (1)< B + C: Spray (2) and melt the granules Close tool Filling the tool with X-type foam particles Extraction of excess (non-film-attached) foam particles of type X D: Steam chamber process for the production of foamed plastic parts with Y-type foam particles E: Cooling and ejection of the foamed plastic part with film coating 5 A: Heating the B + C: Spray (2) and melt Close tool Filling the tool with X-type foam particles Cooling the cavity and suctioning away excess foam particles (not bonded to the film). Storage of the film layer with molten foam particles of type X Insertion of the film layer with melted foam particles from D: Steam chamber process for production E: Cooling and ejection of the foamed Tool cavity using variotherm (1)< of the granules and removal of the film with the foam particles of type X that are bonded together by melting Type X in a tool foamed plastic parts with Y-type foam particles Plastic part with film coating (1) Variotherm is a heating and cooling system that allows precise temperature control in all areas of a mold. The mold cavity does not necessarily have to be integrated into the steam chamber of the molding machine. (2) Spray system from Nordson Deutschland GmbH: Powder is transferred from a storage or feed container to a powder spray gun (Encore HD system) using Dense Phase Pump technology. The powder is applied with or without electrostatic charging.
[0054] The melting of the granules can also be carried out on a cavity copy, either fully or partially, outside the molding machine. This allows for shorter cycle times and also enables the coating of thick, foamed plastic parts if steam nozzles are required on all sides. EVALUATION METHODS Density of the foam part:
[0055] The part density MD (g / l) of the foamed plastic part listed in Table 3 was calculated by dividing the weight W1 (g / l) of the foamed plastic part by the volume V1 (L) of the foamed plastic part: MD = W1 / V1 (g / l) Water permeability
[0056] A 1% water-based soap solution was prepared by adding 25 g of dishwashing liquid (trademark "Dreft Original" by Procter & Gamble) to 2500 ml of water at a temperature of 25°C.
[0057] A foam insert in the shape of a cylindrical bowl has a total volume of 1600 ml. The inner surface of the bowl is coated with a film. It has an open diameter D of 190 mm, and the thickness of the base and walls is 10 mm. The bowl is stored at ambient conditions (23 °C - 50% relative humidity), and its weight W2 (g) is measured.
[0058] A volume V2 of 800 ml or 800,000 mm³, corresponding to 50% of the total volume of the bowl, of soap dispersion is poured into the bowl. The water column in the bowl has a height of 28.32 mm = 800,000 / ((π*190²) / 4). The bowl is stored for 24 hours at ambient conditions (23 °C - 50% relative humidity).
[0059] Next, the remaining soap solution is removed from the bowl, the inner surface of the bowl is rubbed dry with a paper towel, and the "wet weight" W3 (g) of the bowl is measured within 5 minutes after the removal of the soap dispersion.
[0060] The water permeability WP is expressed as a percentage of the weight increase of the shell: WP % = W3 − W2 / W2 * 100 hardness
[0061] The hardness of the foamed plastic part is measured according to ASTM D2240. The result is given as a "Shore A" value. Color homogeneity
[0062] The color of a foamed plastic part, with and without a film coating, is measured using a BYK Gardner device with a color ball system based on the CIElab color system. The result of a color measurement is expressed as a set of L, a*, and b* values.
[0063] The L-value varies from 0 to 100, from white to black.
[0064] The a * value varies from -127 to +127, from green to red.
[0065] The b* value varies from -127 to +127, from blue to yellow.
[0066] Color measurements are taken at five different locations on an area of 20,000 mm² and the average L, a* and b* values are calculated.
[0067] The color difference between two measurements is represented as ΔE and calculated as follows: Δ E ab ∗ = L 2 ∗ − L 1 ∗ 2 + a 2 ∗ − a 1 ∗ 2 + b 2 ∗ − b 1 ∗ 2
[0068] For each individual color measurement, ΔE i is calculated relative to the mean of L, a* and b* values, with i from 1 to 5. Finally, the varying total ΔE is calculated as the mean of five ΔE i values. Table 3 granules Composition of foamed plastic part Density of foamed plastic part (g / l) Color homogeneity (ΔE) Hardness (Shore A) Water permeability (%) Ex. 7 Schwarz EX1Y 1886 Eperan-PP VB30 30 0,22 97 0.0 Comparison example - Eperan-PP MN20 45 0,77 42 5.5
[0069] Preferred embodiments of the method according to the invention are explained below with reference to the accompanying drawings. The drawings show: Figure 1 shows a sectional view through a tool mold in the closed state; Figure 2 shows a sectional view of a cavity during the application of granules; Figure 3 shows an embodiment of a tool mold with a foamed plastic mold produced according to the invention; and Figure 4 shows a further embodiment of a tool mold with an external heating system.
[0070] The Figure 1 Figure 1 shows a sectional view of a tool mold 2 in the closed state, wherein the tool mold 2 is formed by two opposing tool cavities 21a and 21b, the aforementioned opposing tool cavities 21a and 21b enclosing a forming mold cavity 22. In the illustrated embodiment, the first tool cavity 21a is equipped with a plurality of heating channels 24, through which a heating medium can be supplied to the first tool cavity 21a, allowing the first tool cavity 21a to be heated to a defined temperature.
[0071] In the Figure 2 An exemplary embodiment of a tool cavity 21 of a tool shape 2 is shown, wherein the illustrated tool cavity includes a temperature sensor 4 by means of which the temperature of the tool cavity 21 can be measured. In the Figure 2 The process of applying the granules 3 using a spray gun 32 is shown, wherein the applied granules form a film layer 31 with a film layer thickness 33 in the area of the tool cavity 21. As is also shown by the Figure 2 The layer thicknesses 33 of the applied granules 3 can be adjusted or specifically influenced section by section in the tool cavity 21 by means of the spray gun 32, which is removable.
[0072] The Figure 3The figure shows a plastic molded body with a partial film layer coating 11, wherein the foam molded body was produced using the tool mold 2, which is formed from a first tool cavity 21a and a second opposing tool cavity 21b, by applying plastic granules 3 to the second tool cavity 21, and the film layer coating 11 was applied to the plastic molded body 1 according to the invention.
[0073] The Figure 4 Figure 1 shows another embodiment of a tool cavity 21 with a temperature sensor 4 and an external heat source 55 in the form of several radiant heaters with directional baffles. The tool cavity 21 can be heated to a defined temperature by means of the external heat source 55, and the sensor 4 can be used to control the heat source 55.
Claims
1. A method for manufacturing a foamed plastic molded body (1) with a film layer coating (11) by using a tool mold (2) with at least one tool cavity (21) to form a shaping mold cavity (22), comprising the following method steps: - A) heating at least one tool cavity (21) of the tool mold (2); - B) applying a granulate (3) to the at least one heated tool cavity (21); - C) fusing the granulate (3) in the heated tool cavity (21) to form a liquid film layer (31); - D) applying the liquid film layer (31) to a foamed plastic molded body (1) to form a film layer coating (11) on the surface of the plastic molded body (1) by fusing the liquid film layer (31) with the surface of the plastic molded body (1); - E) cooling the at least one tool cavity (21) and ejecting the plastic molded body (1) coated with the film layer (11), wherein the temperature of the at least one tool cavity is controlled or regulated, respectively, while performing the method such that said temperature is at least above the melting temperature of the applied granulate during the entire period of performing at least the method steps B) to D).
2. The method for manufacturing according to claim 1, characterized in that, before performing method steps A) to E), the plastic molded body (1) is produced in the tool mold (2) by an expansion method, then the tool mold (2) is opened, wherein the plastic molded body (1) remains in at least one first tool cavity (21a) and method steps A) to E) are then performed for at least one second opposite tool cavity (21b), wherein applying the liquid film layer (31) by fusing the liquid film layer (31) with the surface of the plastic molded body (1) is performed according to method step D) by closing the tool mold (2) again, and the cooling in method step E) of the at least one tool cavity (21) is performed in the closed molding condition.
3. The method for manufacturing according to claim 1 or 2, characterized in that the area of the at least one tool cavity (21a, 21b) first method steps A) to C) are performed, then the tool mold (2) is closed and the mold cavity (22) of the tool mold (2) is filled with a first expandable plastic granulate or with foam pearls, respectively, and then the first plastic granulate or the foam pearls, respectively, are expanded in the mold cavity (22), wherein method step D) is performed by the fact that the plastic molded body (1) or the first expandable plastic granulate or the foam pearls, respectively, is expanded against the liquid film layer (31) formed on the at least one tool cavity (21) and fuses therewith.
4. The method for manufacturing according to claim 1 or 2, characterized in that the granulate (3) is applied in method step B) beyond the region of the at least one tool cavity (21a, 21b) to the multi-part tool mold (2), and that at least one part of the multi-part tool mold (2) comprises a sealing ring which, when closing the tool mold (2), throws up the granulate (3) outside the region of the at least one first and / or second tool cavity (21a, 21b) to a bead in the edge area of the at one first and / or second tool cavity (21a, 21b).
5. The method for manufacturing according to claim 3 or 4, characterized in that, in the method step of the expansion of the first expandable plastic granulate or the foam pearls, respectively, the expansion process is terminated after a defined period of time, and the first plastic granulate or the foam pearls, respectively, which are not yet melted or expanded are removed from the mold cavity (22) such that only a layer of the first expanded plastic granulate or of the foam pearls, respectively, adheres to the film layer (31).
6. The method for manufacturing according to claim 5, characterized in that after removing the non-expanded proportions of the first plastic granulate or of the foam pearls, respectively, the mold cavity (22) is filled with a second expandable plastic granulate or with foam pearls, respectively, which are then expanded to form the plastic molded body (1).
7. The method for manufacturing according to any one of the preceding claims, characterized in that the granulate (3) is applied in method step B) by means of a spray pistol (32) to the at least one tool cavity (21).
8. The method for manufacturing according to any one of the preceding claims, characterized in that the at least one tool cavity (21) to be heated is heated in method step A) by introducing a heating medium through the corresponding heating channels (24) in the at least one tool cavity (21).
9. The method for manufacturing according to any one of the preceding claims, characterized in that, in method step A), the at least one tool cavity (21) to be heated is heated to at least a temperature above the melting temperature of the granulate (3), in particular to a temperature in the range of 80°C to 260°C.
10. The method for manufacturing according to any one of the preceding claims, characterized in that, in method step B), a powdery thermoplastic plastic granulate (3) is applied to the at least one tool cavity (21).
11. The method for manufacturing according to any one of the preceding claims, characterized in that the at least one tool cavity (21) to be heated is heated in method step A) by an external heating source (55) which is arranged to be spaced apart from the at least of tool cavity (21), such as in particular a radiant heater.
12. The method for manufacturing according to any one of the preceding claims, characterized in that, in method step B), granulate (3) is only proportionately applied to defined partial regions of the at least one tool cavity (21) to form at least one film layer (31) in certain areas, wherein in particular subregions of the at least one tool cavity (21) can be covered in order to prevent a granulate application in method step B).
13. The method for manufacturing according to any one of the preceding claims, characterized in that, in method step B), a granulate (3) is applied to the tool cavity (21) with a layer thickness (33) in the range of 0.05 mm to 2 mm.
14. The method for manufacturing according to any one of the preceding claims, characterized in that, in method step E), the at least one tool cavity (21) to be cooled is cooled convectively and / or conductively.