AI Technical Summary
Existing coating solutions for multi-layer cardboard fail to prevent delamination and picking during printing, which affects the strength and smoothness of the coated surface.
A coating slip comprising an aqueous dispersion of vinyl acetate polymers and styrene copolymers, specifically formulated with a weight ratio of 77:23 to 93:7, along with inorganic pigments and auxiliary materials, to enhance the bonding strength and resistance to delamination and picking.
The solution significantly reduces delamination and picking, resulting in improved surface strength and printability of multi-layer cardboard, ensuring high dry picking resistance and smooth coating.
Description
[0001] The invention relates to a coating composition comprising an aqueous dispersion of a vinyl acetate polymer and a dispersion of a styrene copolymer.
[0002] One of the most important functions of cardboard is its function as a packaging material, and many of these materials are printed. However, a fibrous substrate such as cardboard has a relatively rough surface compared to paper. To improve its printability, as well as its quality in terms of smoothness and gloss, cardboard, like paper, is coated with coating slips. Aqueous paper coating slips essentially contain synthetic binders, pigments, other additives, and water. Copolymers based on styrene and butadiene and those based on styrene and acrylic acid ester have become particularly popular as binders for paper coating slips.
[0003] For example, US 2008 / 0081175 teaches styrene / acrylate copolymer as a binder for paper coating slips.
[0004] WO 2015 / 155159 and WO 2015 / 155157 teach polymers obtainable by radical polymerization of vinyl acetate and acrylates.
[0005] WO 2009 / 156341 teaches a paper coating slip containing metal salt pigments and polymer dispersions obtainable by polymerization of anionic monomers and nonionic monomers.
[0006] WO 2012 / 012231 teaches vinyl acetate / ethylene polymers with crosslinking monomers that, when used as binders in paper coating slips, result in good strength and reduced picking during printing. The ethylene content of these polymers is 12 or more parts by weight based on 100 parts by weight of monomer.
[0007] DE 10 2010 063 470 teaches a combination of a styrene-butadiene copolymer or a styrene-acrylic acid ester copolymer with a vinyl acetate-ethylene polymer stabilized with polyvinyl alcohol as a synthetic binder for paper coating slips. It is used to improve the whiteness and coating porosity of coated printing substrates. The mixtures used here have a ratio of vinyl acetate / ethylene polymer to styrene copolymer of 25:75.
[0008] US 2015 / 0125711 describes binder compositions for paper coating slips made from functionalized vinyl acetate / ethylene polymers and styrene / butadiene polymers, as well as blends of vinyl acetate / ethylene polymers and styrene / acrylate polymers. Some vinyl acetate / ethylene polymers are carboxyl-functionalized and have an ethylene content, based on the polymer, of 14 wt.% or more. Papers coated with such coating slips exhibit good strength and thus reduced picking. The weight fraction of the functionalized vinyl acetate / ethylene polymers in the total binder is 20 to 80%.
[0009] What all these publications have in common is that they deal with paper coating. However, none of them addresses the specific problems of coating multi-layer board.
[0010] Cardboard is typically multi-layered, meaning it consists of several layers of paper of varying thicknesses and sometimes of different materials, which are pressed together (cushioned) without the use of adhesive. Coated cardboard is used as packaging material for a wide variety of products. During the production of cardboard packaging, the fold lines are first defined to prevent the board from tearing during folding. Often, a layer breaks during folding. This separation of the individual cardboard layers, often a breakage of a softer middle layer of cardboard, is also known as delamination and frequently occurs during the printing process. Here, the viscous printing ink on the printing roller causes a tensile force in the z-direction of the paper surface, which also causes a breakage of a cardboard layer, a process known as "delamination."The effect of this tensile force in the z-direction during the printing process is also known from the coating of paper, where the damage occurs directly on the surface as parts of the paper coating detach from the base paper, a process known as picking. While picking affects pigments on the paper surface, the damage to multi-layer cardboard occurs in the fiber layer and manifests itself in the formation of ripples.
[0011] The objective of the present invention was to find a coating slip that reduces delamination when printing on multi-layer cardboard. Furthermore, the coated cardboard should also exhibit good strength, meaning the coating should not show any picking.
[0012] The object was achieved according to the invention by a coating composition comprising (i) an aqueous dispersion of one or more vinyl acetate polymers, obtainable by radically initiated emulsion polymerization of 77 to 99 wt.% vinyl acetate, 1 to 13 wt.% Ethylene and 0 to 10 wt.% one or more monoethylenically unsaturated monomers which is neither vinyl acetate nor ethylene, where the amounts of monomers add up to 100 wt.%, (ii) an aqueous dispersion of one or more styrene copolymers obtainable by radically initiated emulsion polymerization of a monomer composition containing 35 to 70 wt.% Styrene, 20 to 60 wt.% one or more esters of acrylic and / or methacrylic acid with alkanols having 1 to 12 C atoms, or one or more conjugated aliphatic dienes, 1 to 10 wt.% one or more monomers containing acid groups, where the amounts of monomers add up to 100 wt.%, (iii) inorganic pigments and (iv) where appropriate, other excipients, wherein the total amount of the emulsion polymers (i) and (ii) is 10 to 30 parts by weight based on 100 parts by weight of inorganic pigment (iii) and wherein the weight ratio of the styrene copolymer to the vinyl acetate polymer is 77:23 to 93:7, preferably 90:10.
[0013] The invention also relates to a process for producing the coating slip, its use for coating cardboard, a process for coating cardboard with the coating slip and the cardboard coated therewith.
[0014] In the following, the term "(meth)acrylic" and similar terms are used as abbreviations for "acrylic and methacrylic".
[0015] In the following, the term "cardboard" refers to a shaped body made of fibrous material which has a mass per unit area, colloquially also referred to as "basis weight", in the range of 150 to 600 g / m², determined in accordance with DIN EN ISO 536.
[0016] The polymer dispersions to be used according to the invention are dispersions of polymers in an aqueous medium. These can be, for example, completely demineralized water or mixtures of water and a miscible solvent such as methanol, ethanol or tetrahydrofuran. Preferably, no organic solvents are used. The solids contents of the dispersions are preferably from 15 to 75 wt. %, more preferably from 40 to 60 wt. %, in particular greater than 50 wt. The solids content can be adjusted, for example, by appropriately adjusting the amount of water used in the emulsion polymerization and / or the amount of monomer. The pH of the polymer dispersion is preferably adjusted to a pH greater than 3.5, in particular to a pH between 4.5 and 9.
[0017] According to the invention, the coating slip contains one or more vinyl acetate polymers (i), obtainable by radically initiated emulsion polymerization from 77 to 99 wt.% vinyl acetate, 1 to 13 wt.% preferably 5 to 13 wt.% ethylene and 0 to 10 wt.% at least one monoethylenically unsaturated monomer which is neither vinyl acetate nor ethylene, where the amounts of monomers add up to 100 wt.%.
[0018] The aqueous vinyl acetate polymers used according to the invention have an ethylene content of 1 to 13 wt.% based on the polymer. If other monoethylenically unsaturated monomers are used in addition to vinyl acetate and ethylene, the polymer advantageously has a vinyl acetate content of ≤ 85 wt.%.
[0019] Other monoethylenically unsaturated monomers that may be considered are: Vinyl esters of straight-chain or branched carboxylic acids with 3-18 C atoms, in particular vinyl esters of an alpha-branched carboxylic acid with 9 to 11 C atoms, acrylic, methacrylic, maleic or fumaric acid esters of aliphatic alcohols with 1-18 C atoms, vinyl chloride, isobutylene or higher α-olefins with 4 to 12 C atoms and their mixtures.
[0020] In addition to the combination of vinyl acetate and ethylene, suitable monomer combinations include vinyl acetate / vinyl pivalate / ethylene, vinyl acetate / vinyl 2-ethylhexanoate / ethylene, vinyl acetate / methyl methacrylate / ethylene and vinyl acetate / vinyl chloride / ethylene, from the group of so-called terpolymers.
[0021] Aqueous dispersions based on vinyl acetate and ethylene are generally known and are described, for example, in DE 102010063470, the disclosure of which is expressly incorporated by reference.
[0022] Vinyl acetate polymers with a glass transition temperature T g in the range of 10 to 30 °C, measured according to DIN EN ISO 11357-2 (2013-09), are preferred. The glass transition temperature of vinyl acetate polymers is advantageously in the range of 15 to 25 °C, particularly in the range of 15 to 20 °C.
[0023] It is also important that according to Fox (TG Fox, Bull. Am. Phys. Soc. 1956 [Ser. II] 1, page 123 and according to Ullmann's Encyclopedia of Technical Chemistry, Vol. 19, page 18, 4th edition, Verlag Chemie, Weinheim, 1980) the glass transition temperature of at most weakly crosslinked copolymers can be estimated with a good approximation according to the following equation 1 / Tg = x 1 / Tg 1 + x 2 / Tg 2 + … x n / Tg n , where x 1 , x 2 , .... xn are the mass fractions of the monomers 1, 2, .... n and Tg 1< , Tg 2< , .... Tg n< are the glass transition temperatures of the homopolymers each composed of only one of the monomers 1, 2, .... n in degrees Kelvin. The glass transition temperatures of these homopolymers of most ethylenically unsaturated monomers are known (or can be determined experimentally in a simple manner known per se) and are given, for example, in J. Brandrup, EH Immergut, Polymer Handbook 1st Ed. J. Wiley, New York, 1966, 2nd Ed. J. Wiley, New York, 1975 and 3rd Ed. J. Wiley, New York, 1989, and in Ullmann's Encyclopedia of Industrial Chemistry, page 169, Verlag Chemie, Weinheim, 1992.
[0024] According to a preferred embodiment, a vinyl acetate polymer is selected which is obtainable by radically initiated emulsion polymerization of 82 to 98 wt.% vinyl acetate, 1 to 13 wt.% Ethylene and 1 to 5 wt.% one or more monoethylenically unsaturated monomers selected from vinyl esters of α-branched monocarboxylic acids having 9 to 11 C atoms, vinyl laurate, (meth)acrylic acid esters of unbranched or branched alcohols having 1 to 15 C atoms, which also contain 1 to 40 wt.% ethylene, where the amounts of monomers add up to 100 wt.%.
[0025] According to a likewise preferred embodiment, the vinyl acetate polymers are obtainable by radically initiated emulsion polymerization of a monomer composition consisting of 87 to 95 wt.% vinyl acetate and 5 to 13 wt.% ethylene, the amounts of the monomers adding up to 100 wt.%.
[0026] The polymers are prepared in a known manner, for example by emulsion polymerization processes in the presence of emulsifiers or, preferably, protective colloids, preferably by the emulsion polymerization process as described below in the context of polymers (ii). The polymerization temperature for polymers (i) is generally from 20°C to 100°C, preferably from 60°C to 90°C. The copolymerization of gaseous comonomers, such as ethylene, is preferably carried out under pressure, generally between 5 bar and 100 bar.
[0027] Protective colloids commonly used to stabilize the polymerization mixture are also listed below in the context of polymers (ii).
[0028] The aqueous dispersions of the polymers (i) thus obtainable have a solids content of preferably 30 to 75% by weight, particularly preferably 50 to 60% by weight.
[0029] The styrene copolymers used according to the invention are also used in the form of an aqueous dispersion. They are obtainable by free-radical emulsion polymerization of a monomer composition containing 35 to 70% by weight of styrene, preferably 40 to 65% by weight, more preferably 40 to 59% by weight of styrene, and 20 to 60% by weight, preferably 30 to 59% by weight of esters of acrylic and / or methacrylic acid with alkanols having 1 to 12 carbon atoms, or a monomer composition containing 35 to 70% by weight of styrene, preferably 45 to 70% by weight, more preferably 50 to 65% by weight of styrene, and 20 to 60% by weight, preferably 25 to 50% by weight of a conjugated aliphatic diene, in each case based on 100% by weight of total monomer.
[0030] Styrene in combination with the esters of acrylic and / or methacrylic acid are the main monomers of so-called "styrene-acrylates." Styrene in combination with a conjugated aliphatic diene are the main monomers of styrene / diene copolymers, or in the case of butadiene, of styrene / butadiene copolymers. The coating composition according to the invention contains dispersions of styrene-acrylate copolymers or styrene / diene copolymers, or mixtures thereof.
[0031] Suitable C 1 -C 12 alkyl (meth)acrylates are, for example, alkyl (meth)acrylates with a C 1 -C 12 alkyl radical, such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-propyl acrylate, n-propyl methacrylate, isopropyl acrylate, isopropyl methacrylate, n-butyl acrylate, n-butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, sec.-butyl acrylate, sec.-butyl methacrylate, tert.-butyl acrylate, tert.-butyl methacrylate, pentyl acrylates, pentyl methacrylates, 2-ethylhexyl acrylate, and 2-ethylhexyl methacrylate. Mixtures of alkyl (meth)acrylates are also particularly suitable. n-Butyl acrylate is preferred.
[0032] Examples of suitable conjugated aliphatic dienes include 1,3-butadiene, isoprene, 1,3-pentadiene, 1,3-dimethylbutadiene, and cyclopentadiene. Of this group of monomers, 1,3-butadiene and / or isoprene, especially butadiene, are preferred.
[0033] In addition to the main monomers, the styrene copolymer contains polymerized monomers with acid groups such as carboxylic acid, sulfonic acid, or phosphonic acid groups. Monomers containing acid groups are ethylenically unsaturated carboxylic acids, ethylenically unsaturated sulfonic acids, and vinylphosphonic acid, and salts of these acids. α,β-monoethylenically unsaturated mono- and dicarboxylic acids containing 3 to 6 carbon atoms in the molecule are preferably used as ethylenically unsaturated carboxylic acids. Examples include acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, crotonic acid, vinylacetic acid, and vinyllactic acid. Suitable ethylenically unsaturated sulfonic acids include, for example, vinylsulfonic acid, styrenesulfonic acid, acrylamidomethylpropanesulfonic acid, sulfopropyl acrylate, and sulfopropyl methacrylate. Acrylic acid and methacrylic acid are particularly preferred, especially acrylic acid.The acid-containing monomers can be used in the polymerization in the form of free acids or in a form partially or completely neutralized with suitable bases. Sodium hydroxide solution, potassium hydroxide solution, or ammonia are preferably used as neutralizing agents.
[0034] According to the invention, the content of monomers containing acid groups in the emulsion polymer is 1 to 10% by weight, preferably 1 to 8% by weight, in particular 2 to 6% by weight.
[0035] According to a likewise preferred embodiment, the monomer composition of the styrene copolymer consists of 40 to 59 wt.% Styrene, 40 to 59 wt.% one or more esters of acrylic and / or methacrylic acid with alkanols containing 1 to 12 carbon atoms, 1 to 10 wt.% one or more monomers containing acid groups and 0 to 9 wt.% one or more other monoethylenically unsaturated monomers where the amounts of monomers add up to 100 wt.%.
[0036] Such other monomers include monoethylenically unsaturated compounds which are neither styrene, nor esters of acrylic and / or methacrylic acid with alkanols containing 1 to 12 carbon atoms, nor monomers containing acid groups. Examples include ethylenically unsaturated carboxylic acid amides, such as acrylamide and methacrylamide in particular, ethylenically unsaturated carboxylic acid nitriles, such as acrylonitrile and methacrylonitrile in particular, vinyl esters of saturated C 1 - to C 18 -carboxylic acids, preferably vinyl acetate, allyl esters of saturated carboxylic acids, vinyl ethers, vinyl ketones, dialkyl esters of ethylenically unsaturated dicarboxylic acids, N-vinylpyrrolidone, N-vinylpyrrolidine, N-vinylformamide, N,N-dialkylaminoalkylacrylamides, N,N-dialkylaminoalkylmethacrylamides, N,N-dialkylaminoalkylacrylates, N,N-dialkylaminoalkylmethacrylates, vinyl chloride, and vinylidene chloride. This group of monomers is optionally used to modify the polymers.
[0037] Preferred other monomers are monomers containing hydroxyl groups, in particular C 1 -C 10 hydroxyalkyl (meth)acrylates, and amides of unsaturated carboxylic acids, such as (meth)acrylamide.
[0038] According to a preferred embodiment, the monomer composition of the styrene copolymer contains no other monomer.
[0039] Preference is given to dispersions of one or more styrene copolymers containing, preferably consisting of, 40 to 59 wt.% Styrene, 40 to 59 wt.% one or more esters of acrylic and / or methacrylic acid with alkanols containing 1 to 12 C atoms, preferably n-butyl acrylate, and 1 to 10 wt.% a monomer containing acid groups, where the amounts of monomers add up to 100 wt.%, in polymerized form.
[0040] Such styrene copolymers are generally known and are described, for example, in WO 2009 / 047233, as well as their preparation.
[0041] In emulsion polymerization, ionic and / or non-ionic emulsifiers and / or protective colloids or stabilizers are typically used as surfactants to assist the dispersion of the monomers in the aqueous medium. Protective colloids are polymeric compounds that bind large amounts of water upon solvation and are capable of stabilizing dispersions of water-insoluble polymers. Unlike emulsifiers, they generally do not lower the interfacial tension between polymer particles and water. A detailed description of suitable protective colloids can be found in Houben-Weyl, Methods of Organic Chemistry, Volume XIV / 1, Macromolecular Substances, Georg-Thieme-Verlag, Stuttgart, 1961, pages 411 to 420. If emulsifiers and / or protective colloids are used as aids for dispersing the monomers, the amounts used are, for example, 0.1 to 5 wt.%, based on the monomers.The surfactant is usually used in amounts of 0.1 to 10 wt.%, based on the monomers to be polymerized.
[0042] Emulsion polymerization is generally carried out at 30 to 130 °C, preferably 50 to 90 °C. The polymerization medium can consist of water alone or of mixtures of water and water-miscible liquids such as methanol. Preferably, only water is used. Emulsion polymerization can be carried out either as a batch process or as a feed process, including stepwise or gradient procedures. The feed process is preferred, in which a portion of the polymerization batch is initially introduced, heated to the polymerization temperature, polymerized, and then the remainder of the polymerization batch is added continuously or stepwise, usually via several spatially separate feeds, one or more of which contain the monomers in pure or emulsified form.
[0043] In emulsion polymerization, the usual and known auxiliaries, such as water-soluble initiators and regulators, can be used.
[0044] According to a preferred embodiment, preference is given to styrene copolymers, in particular styrene-acrylate polymers, which are obtainable by radically initiated emulsion polymerization in the presence of 10 to 80 wt.%, based on total monomer of the styrene copolymer, of a degraded starch.
[0045] Styrene acrylate polymers prepared in the presence of a degraded starch are described, for example, in EP 2580257, to whose teaching express reference is made.
[0046] Styrene / diene polymers, in particular styrene / butadiene polymers, which were prepared in the presence of a degraded starch, are described, for example, in EP 2197925, to whose teachings express reference is made.
[0047] The term "degraded starch" is understood by those skilled in the art to mean a starch whose polymer chain has been degraded by cleavage of glycosidic bonds. It therefore contains fewer repeating units than the polymer chain of the underlying native starch. The degradation of the starch is reflected, for example, in its intrinsic viscosity.
[0048] All native starches, such as those from corn, wheat, oats, barley, rice, millet, potatoes, peas, tapioca, sorghum, or sago, are suitable as starting starches for the production of the preferred degraded starches. Natural starches with a high amylopectin content, such as waxy maize starch and waxy potato starch, are also of interest as starting starches. The amylopectin content of these starches is above 90%, usually between 95 and 100%.
[0049] Starch degradation can occur enzymatically, oxidatively, or hydrolytically through the action of acids or bases. Starch degradation is well known and is described, for example, in EP 2197925. Degraded starches are commercially available. A degraded starch can be used for polymerization, or it can be produced in situ and then polymerized in its presence.
[0050] Particularly preferred are degraded native starches, especially native starches degraded to maltodextrin.
[0051] Preference is given to degraded starches with an intrinsic viscosity ηi of ≤0.07 dl / g or ≤0.05 dl / g. The intrinsic viscosity ηi of the degraded starches is preferably in the range of 0.02 to 0.06 dl / g. The intrinsic viscosity ηi is determined according to DIN EN 1628 at a temperature of 23 °C.
[0052] The dispersions are generally monomodal. According to a preferred embodiment, a bimodal dispersion is used.
[0053] The coating slip according to the invention contains the aqueous dispersion of one or more vinyl acetate polymers (i) and the aqueous dispersion of one or more styrene copolymers (ii), preferably styrene acrylate polymers, and inorganic pigment (iii), the total amount of the emulsion polymers (i) and (ii) being 10 to 30 parts by weight based on 100 parts by weight of inorganic pigment (iii), the weight ratio of the styrene copolymer to the vinyl acetate polymer being 77:23 to 93:7, preferably 77:23 to 90:10, in particular 80:20 to 90:10, especially 83:17 to 88:12. The dispersions of the vinyl acetate polymer and the styrene copolymer preferably comprise the total amount of binder.
[0054] Particularly preferred is a combination of a vinyl acetate polymer obtainable by radically initiated emulsion polymerization of 90 to 99 wt.% vinyl acetate, 1 to 10 wt.% Ethylen and a styrene copolymer obtainable by radically initiated emulsion polymerization of a monomer composition consisting of 40 to 59 wt.% Styrene, 40 to 59 wt.% one or more esters of acrylic and / or methacrylic acid with alkanols having 1 to 12 C atoms, preferably n-butyl acrylate, and 1 to 10 wt.% Acrylic acid where the amounts of monomers each add up to 100 wt.%.
[0055] The coating slip according to the invention contains inorganic pigments in an amount of preferably at least 80% by weight, for example 80 to 95% by weight or 80 to 90% by weight, based on the total solids content.
[0056] White pigments are particularly suitable. Suitable pigments include, for example, metal salt pigments such as calcium sulfate, calcium aluminate sulfate, barium sulfate, magnesium carbonate and calcium carbonate, of which carbonate pigments, in particular calcium carbonate, are preferred. The calcium carbonate can be ground calcium carbonate (GCC, natural ground calcium carbonate), precipitated calcium carbonate (PCC, precipitated calcium carbonate), lime or chalk. Suitable calcium carbonate pigments are available, for example, as Covercarb ®< 60, Hydrocarb ®< 60 or Hydrocarb ®< 90. Other suitable pigments include, for example, silicas, aluminum oxides, aluminum hydrate, silicates, titanium dioxide, zinc oxide, kaolin, clay, talc or silicon dioxide. Suitable additional pigments are available, for example, as Capim ®< MP 50 (clay), Hydragloss ®< 90 (clay) or Talcum C10. Kaolin and / or calcium carbonate (PCC and GCC) are preferred.
[0057] For example, 1 to 50 parts by weight, preferably 1 to 25 parts by weight or 5 to 20 parts by weight of the binder composition according to the invention (solid, ie without water or other solvents which are liquid at 21 °C, 1 bar) are used per 100 parts by weight of pigments.
[0058] Preference is given to a coating slip containing, preferably consisting of, the polymers (i) and (ii) in a total amount of 10 to 30 parts by weight, based on 100 parts by weight of inorganic pigment (iii), and also 5 to 15 parts by weight of one or more auxiliaries, and whose pigment is selected from the group consisting of calcium sulfate, calcium aluminate sulfate, barium sulfate, magnesium carbonate, calcium carbonate, silicic acids, aluminum oxides, aluminum hydrate, silicates, titanium dioxide, zinc oxide, kaolin, clay, talc and silicon dioxide and whose auxiliaries are selected from the group consisting of thickeners (rheology aids), co-binders, preferably polyvinyl alcohol and starch, optical brighteners, flow control agents, dispersants, surfactants, lubricants, neutralizing agents, defoamers, deaerating agents, preservatives and dyes.
[0059] Naturally based binders, in particular starch-based binders and lignin-based binders, can be considered as co-binders.
[0060] In this context, starch-based co-binders are understood to mean any native, modified, or degraded starch. Native starches can consist of amylose, amylopectin, or mixtures thereof. Modified starches can be oxidized starch, starch esters, or starch ethers. Hydrolysis can reduce the molecular weight of the starch (degraded starch). Possible degradation products are oligosaccharides or dextrins. Preferred starches are cereal, corn, and potato starch. Cereal and corn starch are particularly preferred, with corn starch being even more preferred.
[0061] In this context, lignin-based co-binders are understood to mean kraft lignin and lignin sulfonate.
[0062] Polyvinyl alcohols are also suitable as co-binders.
[0063] It is preferably an aqueous coating slip; it already contains water, particularly due to the preparation of the components (aqueous polymer dispersions, aqueous pigment slurries); the desired viscosity can be adjusted by adding additional water. Typical solids contents of the coating slips are in the range of 30 to 80 wt.%. A solids content in the range of 60 to 75 wt.% is preferred. The pH of the coating slip is preferably adjusted to values of 6 to 11, in particular 7 to 10.
[0064] The present invention also relates to a process for producing the coating composition by (i) the aqueous dispersion of one or more vinyl acetate polymers (ii) the aqueous dispersion of one or more styrene copolymers, (iii) inorganic pigments and (iv) optionally further auxiliaries, (v) optionally water, wherein the total amount of the emulsion polymers (i) and (ii) is 10 to 30 parts by weight based on 100 parts by weight of inorganic pigment (iii) and wherein the weight ratio of the styrene copolymer (ii) to the vinyl acetate polymer (i) is 77:23 to 93:7, preferably 77:23 to 90:10.
[0065] The coating slips according to the invention are particularly suitable for producing a coated cardboard having a basis weight in the range from 150 to 600 g / m 2< , preferably in the range from 200 to 350 g / m 2< .
[0066] The invention also relates to a process for producing a coated cardboard by a multi-layer cardboard having a basis weight in the range from 150 to 600 g / m 2< , in particular 200 to 350 g / m 2<, is provided, the coating slip according to the invention is applied to at least one surface of this cardboard in such a way that the application weight of the coating slip as a dry weight on a surface of the substrate is 5 to 30 g / m 2< and the coated cardboard is then dried.
[0067] The cardboard to be coated has a basis weight in the range of 150 to 600 g / m². The coating composition according to the invention is particularly suitable for coating multi-layer cardboard. "Multi-layer" refers to two, three, four, or five layers of paper pressed together. These underlying paper layers typically have a basis weight in the range of 20 to 200 g / m². The sum of the paper layers determines the basis weight of the uncoated cardboard. Multi-layer cardboard with a basis weight in the range of 200 to 350 g / m² is preferred.
[0068] For example, a standard coated folding boxboard is made up of a top coat with a basis weight of 20 g / m 2<, a middle layer of bleached chemical pulp with a basis weight of 20 g / m 2<, a middle layer of mechanical groundwood with a basis weight of 140 g / m 2< and a base layer of bleached chemical pulp with a basis weight of 20 g / m 2<.
[0069] The quantity of coating applied to one side of the cardboard is generally 1 to 30 g / m 2< , preferably 5 to 30 g (solid, ie without water or other solvents liquid at 21 °C, 1 bar) per square meter.
[0070] The coating can be a single or double coat (primer and / or topcoat). The coating can be applied using conventional application methods, e.g., size press, film press, blade coater, air brush, doctor blade, curtain coating, or spray coater.
[0071] Furthermore, the present invention relates to the coated cardboard obtainable by this process.
[0072] The coating slips according to the invention have good application properties. They exhibit good runnability in paper coating processes and high bond strength. The coated cardboards have good surface strength, in particular very high dry pick resistance and low delamination. They are easily printable using conventional printing processes, such as letterpress, gravure, offset, digital, flexographic, or a combination of these printing processes.
[0073] The present invention also relates to the binder composition on which the coating composition according to the invention is based. Examples
[0074] Unless the context indicates otherwise, percentages always mean percentages by weight.
[0075] The indication of a content refers to the content in aqueous solution or dispersion.
[0076] When water was used in the examples, demineralized water was used. Measurement methods
[0077] Glass transition temperature: The glass transition temperature T g of a dispersion was generally determined using a Q 2000 differential scanning calorimeter from TA Instruments. The heating rate was 10 K per minute.
[0078] Determination of the viscosity of the coating slip: The viscosity of the dispersion was determined according to ASTM D2196 using a Brookfield viscometer with RV spindle 4 at 100 rpm and at a temperature of 23°C.
[0079] Solids content: The solids content of a coating slip or dispersion was determined by distributing 0.5 to 1.5 g of the coating slip / dispersion in a 4 cm diameter metal lid and then drying it in a circulating air drying cabinet at 140°C for 30 minutes. The ratio of the mass of the sample after drying under the above conditions to the mass at sampling gives the solids content. General preparation of coating pastes:
[0080] The coating slip was prepared in a stirred unit, into which the individual components were added sequentially. The pigments were predispersed as a slurry. The rheological aid was then added first, then adjusted to a pH of 9 with sodium hydroxide solution, and finally the emulsion polymer.
[0081] The final solids content was adjusted by adding water.
[0082] The quantities given refer to the solid. 100 parts by weight Calcium carbonate (Hydrocarb 90 slurry from OMYA, solids content 78.6 wt.%) 0.11 parts by weight Rheology aid (Sterocoll FS from BASF SE) 16 parts by weight Emulsion polymer of the respective example
[0083] A three-ply uncoated cardboard with a basis weight of 225 g / m² (4.5% residual moisture by weight) was coated with the coating compound. The coating compound was applied to one side of the cardboard using a laboratory coating machine and dried to 4.5% residual moisture by weight using an IR lamp. The coating was applied using the blade coating method. One layer was applied. The coating weight was 10 g / m² (solid). Determination of delamination
[0084] Principle: To determine the delamination behavior of a coating slip, a coated board sample is printed with a pick oil test ink using an IGT Printability Tester AIC 2-5. The tensile force of the pick oil test ink causes more or less damage to the surface (rippling). The less damage, the less delamination the coating slip exhibits. Preparation: Five strips measuring 340 mm x 40 mm are cut from the coated board samples to be tested in the direction of travel of the board web. The polyurethane rollers are inserted into the roller mill. 1.3 ml (+ / - 0.01 ml) of the selected IGT test pick oil (Standard IGT Testing System IGT Pick Oil, Medium Viscosity No. 404.004.020) are applied to the left roller and 0.93 ml (+ / - 0.01 ml) to the right. The grinding time is 45 minutes. Then two metal printing wheels on the left roller are inked for 90 seconds and then for another 90 seconds on the right roller.The printing speed is set to a value of 200 cm / s (standard) with increasing speed, and the line pressure is 700 N (=350 N / cm). Test: A cardboard strip is stretched over the circular segment and the printing process is started. Evaluation: The printed cardboard strip is then viewed under light and normalized, and the beginning of the curling on the side of the print is marked with a line. The length of the distance from the start of printing to the marks is used to determine delamination. Five strips are tested per test point. Measurement of dry pick resistance with IGT test printer (IGT dry):
[0085] Strips were cut from the coated board to be tested and printed using the IGT test printer. The printing inks used were specific test inks from Lorilleux, which transmit different tensile forces. The test strips were passed through the press at a continuously increasing speed (maximum speed 200 cm / s). To evaluate the results, the point on the sample print strip where 10 picking points appeared on the paper surface after printing began was determined.
[0086] The measure used to determine dry pick resistance is the speed in cm / s at that point during printing, as well as the test ink used. The higher this printing speed at the tenth pick point, the better the quality rating of the paper surface.
[0087] In the examples, the following aqueous binder dispersions were used as starting materials: SA1:Bimodal styrene / n-butyl acrylate / acrylic acid dispersion with a solids content (FS) of 50 wt% and a glass transition temperature T g of 20°C SA2:Monomodal styrene / n-butyl acrylate / acrylic acid dispersion with FS 50 wt% and T g of 20°C SA3:Monomodal styrene / n-butyl acrylate / acrylic acid dispersion with FS 50 wt% and prepared in the presence of 10 parts by weight of maltodextrin (dextrose equivalent DE= 18, M w of 11000 and an intrinsic viscosity of ηi 0.052 dl / g) based on 100 parts by weight of monomer.
[0088] The monomer composition of the styrene / butyl acrylate / acrylic acid polymers was 46 / 50 / 4 for all three dispersions. SB1: Styrene / butadiene / acrylic acid dispersion with FG 50 wt% and Tg of 20°C SB2: Styrene-butadiene / acrylic acid dispersion with FG 50 wt% and Tg of 6°C, prepared in the presence of 60 parts by weight of maltodextrin (DE= 18, Mw of 11000 and an intrinsic viscosity of ηi 0.052 dl / g) based on 100 parts by weight of monomer
[0089] The monomer composition of the styrene / butadiene / acrylic acid polymers was 65 / 30 / 5 (SB1) and 57 / 39 / 4 (SB2). D1: Vinyl acetate / ethylene copolymer dispersion (89.5 / 10.5 vinyl acetate / ethylene) with FW 60 wt.% and T g of 10°C D2: Vinyl acetate / ethylene copolymer (87 / 13 vinyl acetate / ethylene) dispersion with FW 55 wt.% and T g of 5°C D3: Vinyl acetate / ethylene copolymer dispersion (93.3 / 6.7 vinyl acetate / ethylene) with FW 58 wt.% and T g of 18°C D4: Vinyl acetate homopolymer dispersion with FW 50 wt.% and T g of 33°C Production of coating slips S1 to S4 (styrene / acrylate polymer (SA1) and vinyl acetate / ethylene polymer (D1))
[0090] Using the binder dispersions listed above, coating slips were produced, consisting of 100 parts by weight pigment (Omya Hydrocarb 90) 0.11 parts by weight rheology aid (Sterocoll FS) 16 parts by weight binder (total).
[0091] All weight data refer to the respective solids content of the components. The ratio of the two binder polymers (solid styrene acrylate polymer / vinyl acetate / solid ethylene polymer) can be found in Table 1. The solids content of the coating slip was 65 wt.%, and the pH was 8.8. Table 1: Delamination values depending on different compositions of SA1 and D1 e.g. SA1 [wt%] D1 [wt.%] Delamination [cm / s] % based on Example 1 1 no 100 0 116 0 2 90 10 126 8,6 3 80 20 131 12,9 4 new 70 30 135* 16,4 no: not according to the invention *) delamination of the cardboard layers and additionally tearing of the coating was observed.
[0092] The examples show that the binder compositions of Examples 2 and 3, formulated as coating slips and applied to cardboard, only lead to delamination at higher tensile forces, with no picking observed. These two coating slips are therefore better than the coating slip with pure styrene acrylate from Example 1. Example 4 shows a good delamination value, but at the same time, severe picking is already observed. Picking indicates a poor coating and poor surface cohesion. Production of coating slips S5 to S9 (styrene / acrylate polymer (SA2) and various vinyl acetate polymers)
[0093] Coating slips were prepared using the binder dispersions listed above, consisting of 100 parts by weight of pigment (Omya Hydrocarb 90), 0.11 parts by weight of rheology aid (Sterocoll FS), and 16 parts by weight of binder (total binder solids). The components of the binder compositions were styrene / acrylate copolymer SA2 and various vinyl acetate / ethylene copolymers, the latter differing in their glass transition temperatures. The respective compositions of the two binder components can be found in Table 2 (also based on the respective solids content). All weight data refer to the respective solids content of the components. The solids content of the coating slip was 65 wt.%, and the pH was 8.8. Table 2: Delamination values depending on compositions with different vinyl acetate polymers having different glass transition temperatures e.g. SA2 [wt.%] 20 wt.% vinyl acetate polymer Tg of vinyl acetate / polymer [°C] Delamination [cm / s] % based on Example 9 5 80 D1 10 111 12,1 6 new 80 D2 5 106 7,0 7 80 D3 18 123 24,2 8 new 80 D4* 33 97 -2,1 9 new 100 - - 99 0 *) Instead of the vinyl acetate / ethylene polymer, a vinyl acetate homopolymer was used. ne: not according to the invention
[0094] The examples show that binder compositions containing vinyl acetate / ethylene polymers with a T g in the range of 10 to 25 °C, formulated as a coating slip and applied to cardboard, lead to better delamination values of the cardboard than a pure styrene acrylate as a binder in the coating slip. Production of coating slips S10 to S15 (styrene / acrylate polymers (SA1) or (SA2) with vinyl acetate / ethylene polymer (D3))
[0095] Using the binder dispersions listed above, coating slips were produced, consisting of 100 parts by weight Pigment (80 parts by weight calcium carbonate and 20 parts by weight kaolin) 0.9 parts by weight Polyvinyl alcohol BF-05 0.12 parts by weight Rheology aid (Sterocoll FS (FG: 40%)) 15.5 parts by weight Binder polymer
[0096] The solids content of the coating composition was 65 wt.%, the pH value was 9. The addition was carried out according to the following table.
[0097] This coating slip was applied to single-coated cardboard (precoat weight was 10 g / m² solid) using a bent-blade pilot plant (manufactured by Voith). The coating weight was 10 g / m² solid. All weights refer to the respective solids content of the components. The ratio of the two binder polymers (styrene / acrylate polymer solid / vinyl acetate polymer solid) can be found in Table 3. Table 3: Delamination values depending on compositions with vinyl acetate / ethylene copolymers with different T g e.g. SA1 [wt%] SA2 [wt.%] D3 [wt.%] Delamination 1)< [cm / s] IGT length (cm / s) 10 new 100 0 0 131 >400* 11 90 0 10 292 >400* 12 80 0 20 326 >400* 13 new 0 100 0 103 >400* 14 0 90 10 335 >400* 15 0 80 20 372 >400* ne: not according to the invention *) No picking observed 1)< To determine the delamination, the 5 cardboard samples were cut in the transverse direction of the cardboard web in the format 340 mm x 40 mm. Production of coating slips S16 to S19 (styrene / butadiene polymer (SB1) or (SB2) and vinyl acetate / ethylene polymer (D3))
[0098] Using the binder dispersions listed above, coating slips were produced, consisting of 100 parts by weight pigment (Omya Hydrocarb 90) 0.11 parts by weight rheology aid (Sterocoll FS) 16 parts by weight binder (total).
[0099] All weight data refer to the respective solids content of the components. The ratio of the two binder polymers (solid styrene / butadiene polymer / solid vinyl acetate / ethylene polymer) can be found in Table 4. The solids content of the coating slip was 65 wt.%, and the pH was 8.8. Table 4: Delamination values for the same monomer composition of the styrene / butadiene / acrylic acid polymer as a function of its preparation in the presence of degraded starch e.g. SB1 [wt%] SB2 [wt.%] D3 [wt.%] Delamination [cm / s] % based on example 16 or 18 16 new 100 0 0 125 0 17 80 0 20 152 21,6 18 new 0 100 0 138 0 19 0 80 20 182 37,8 ne: not according to the invention Production of coating slips S20 to S23 (styrene / butadiene polymer (SA2) or (SA3) and vinyl acetate / ethylene polymer (D3))
[0100] Using the binder dispersions listed above, coating slips were produced, consisting of 100 parts by weight pigment (Omya Hydrocarb 90) 0.11 parts by weight rheology aid (Sterocoll FS) 16 parts by weight binder (total).
[0101] All weight data refer to the respective solids content of the components. The ratio of the two binder polymers (solid styrene / acrylate polymer / solid vinyl acetate / ethylene polymer) can be found in Table 5. The solids content of the coating slip was 66 wt.%, and the pH was 8.8. Table 5: Delamination values for the same monomer composition of the styrene / acrylate polymer as a function of its preparation in the presence of degraded starch e.g. SA2 [wt.%] SA3 [wt%] D3 [wt.%] Delamination (cm / s) % based on example 20 or 22 20 new 100 0 0 103 0 21 80 0 20 126 22,3 22 new 0 100 0 105 0 23 0 80 20 129 22,8 ne: not according to the invention Examples 24 and 25: Comparison tests with SA2 and D3 respectively
[0102] Using the binder dispersions listed above, coating slips were produced, consisting of 100 parts by weight pigment (Omya Hydrocarb 90) 0.11 parts by weight rheology aid (Sterocoll FS) 16 parts by weight binder (total). Table 6: Delamination values for the coating slips containing SA2 or D3 as binder e.g. SA2 [wt.%] D3 [wt.%] Delamination (cm / s) 24 new 100 0 103 25 new 0 100 104* *: The stripes show additional plucking
[0103] Cardboard coated with the coating slip from Example 24 or Example 25 yielded comparable delamination values. However, the cardboard coated with the coating slip containing D3 as the binder also exhibited poorer surface cohesion, as picking was also observed. The inventive blend of the two polymers SA2 and D3 (Example 21) demonstrates the presence of a synergy, as both an improved delamination value and good surface cohesion (no picking) were observed.
Claims
1. A coating slip comprising (i) an aqueous dispersion of one or more vinyl acetate polymers, obtainable by free-radically initiated emulsion polymerization of 77% to 99% by weight of vinyl acetate, 1% to 13% by weight of ethylene and 0% to 10% by weight of one or more monoethylenically unsaturated monomers that are neither vinyl acetate nor ethylene, where the amounts of the monomers add up to 100% by weight, (ii) an aqueous dispersion of one or more styrene copolymers, obtainable by free-radically initiated emulsion polymerization of a monomer composition comprising 35% to 70% by weight of styrene, 20% to 60% by weight of one or more esters of acrylic and / or methacrylic acid with alkanols having 1 to 12 carbon atoms, or of one or more conjugated aliphatic dienes, 1% to 10% by weight of one or more monomers comprising acid groups, where the amounts of the monomers add up to 100% by weight, (iii) inorganic pigments and (iv) optionally further auxiliaries, where the total amount of emulsion polymers (i) and (ii) is 10 to 30 parts by weight based on 100 parts by weight of inorganic pigment (iii) and where the weight ratio of the styrene copolymer to the vinyl acetate polymer is 77:23 to 93:7.
2. The coating slip according to claim 1, wherein the vinyl acetate polymer has a glass transition temperature Tg in the range from 10 to 30°C, measured to DIN EN ISO 11357-2 (2013-09).
3. The coating slip according to claim 1 or 2, wherein the one or more vinyl acetate polymer(s) is / are obtainable by free-radically initiated emulsion polymerization of 82% to 98% by weight of vinyl acetate, 1% to 13% by weight of ethylene and 2% to 5% by weight of one or more monoethylenically unsaturated monomers selected from vinyl esters of α-branched monocarboxylic acids having 9 to 11 carbon atoms, vinyl laurate or vinyl esters of an α-branched carboxylic acid having 9 to 11 carbon atoms, (meth)acrylic esters of alcohols having 1 to 15 carbon atoms that also comprise 1 to 40% by weight of ethylene, where the amounts of the monomers add up to 100% by weight.
4. The coating slip according to any of claims 1 to 3, wherein the styrene copolymer is obtainable by free-radically initiated emulsion polymerization of a monomer composition comprising 40% to 59% by weight of styrene, 40% to 59% by weight of one or more esters of acrylic and / or methacrylic acid with alkanols having 1 to 12 carbon atoms, and 1% to 10% by weight of a monomer comprising acid groups, where the amounts of the monomers add up to 100% by weight.
5. The coating slip according to any of claims 1 to 4, wherein the styrene copolymer is obtainable by free-radically initiated emulsion polymerization in the presence of 10% to 80% by weight, based on total monomers of the styrene copolymer, of a degraded starch.
6. The coating slip according to any of claims 1 to 5, wherein the weight ratio of the styrene copolymer to the vinyl acetate polymer is 80:20 to 90:10.
7. The coating slip according to any of claims 1 to 6, wherein at least 80% by weight of the total solids content of the coating slip is inorganic pigment.
8. The coating slip according to any of claims 1 to 7, having a solids content of 30% to 80% by weight.
9. A process for producing the coating slip according to any of claims 1 to 8 by mixing (i) the aqueous dispersion of one or more vinyl acetate polymers, (ii) the aqueous dispersion of one or more styrene copolymers, (iii) inorganic pigments and (iv) optionally further auxiliaries, (v) optionally water, where the total amount of emulsion polymers (i) and (ii) is 10 to 30 parts by weight based on 100 parts by weight of inorganic pigment (iii) and where the weight ratio of the styrene copolymer (ii) to the vinyl acetate polymer (i) is 77:23 to 93:7.
10. The use of the coating slip according to any of claims 1 to 8 for production of a coated board having a basis weight in the range from 150 to 600 g / m2.
11. A method of producing a coated board by - providing a multilayer board having a basis weight in the range from 150 to 600 g / m2, - applying a coating slip according to any of claims 1 to 8 to at least one surface of said board such that the coatweight of the coating slip as dry weight on a surface of the substrate is 5 to 30 g / m2 and - then drying the coated board.
12. The coated board obtainable by the method according to claim 11.
13. A binder composition comprising (i) an aqueous dispersion of one or more vinyl acetate polymers, obtainable by free-radically initiated emulsion polymerization of 77% to 99% by weight of vinyl acetate, 1% to 13% by weight of ethylene and 0% to 10% by weight of one or more monoethylenically unsaturated monomers that are neither vinyl acetate nor ethylene, where the amounts of the monomers add up to 100% by weight, (ii) an aqueous dispersion of one or more styrene copolymers, obtainable by free-radically initiated emulsion polymerization of a monomer composition comprising 35% to 70% by weight of styrene, 20% to 60% by weight of one or more esters of acrylic and / or methacrylic acid with alkanols having 1 to 12 carbon atoms, or of one or more conjugated aliphatic dienes, 1% to 10% by weight of one or more monomers comprising acid groups, where the amounts of the monomers add up to 100% by weight, where the weight ratio of the styrene copolymer to the vinyl acetate polymer is 77:23 to 93:7.