METHOD FOR OPTIMIZING TITANIUM DIOXIDE TRAITS IN MASSIVE TIO2-SIO2 SUBSTANT PRECASTERS
Patent Information
- Application Number
- DE502022002007
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-07-22
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2042-07-22
AI Technical Summary
The production of TiO2-SiO2 mixed glass substrates for EUV lithography faces challenges with macroscopic titanium gradients and microscopic layer structures, which affect the quality and homogeneity of the substrates, especially when producing large masses exceeding 50 kg, leading to imaging errors and reduced numerical aperture.
A method involving the introduction of silicon dioxide and titanium dioxide raw materials into a flame, followed by specific processing steps including division, spatial measurement, homogenization treatments, and reconfiguration to minimize titanium gradients and layer structures, optimizing the spatial distribution of titanium dioxide within the substrate precursor.
This method enables the production of substrate precursors with reduced macroscopic titanium gradients and microscopic layer structures, achieving higher numerical aperture and improved imaging properties suitable for EUV lithography, even for large masses exceeding 100 kg.
Description
Background of the invention
[0001] The invention relates to a method for producing a substrate precursor having a mass of more than 50 kg, in particular more than 100 kg, comprising a TiO2-SiO2 mixed glass. State of the art
[0002] EP2960219A1 describes how EUV lithography uses microlithographic projection devices to create highly integrated structures with a linewidth of less than 50 nm. This typically uses working radiation from the spectral range between 10 nm and 121 nm, known as the EUV range (extreme ultraviolet light, also known as "soft X-rays").
[0003] The projection devices are equipped with mirror elements consisting primarily of synthetic, high-silica, titanium dioxide-doped quartz glass (hereinafter also referred to as "TiO2-SiO2 mixed glass" or "TiO2-SiO2 glass") and coated with a reflective layer system. The TiO2-SiO2 mixed glass is characterized by an extremely low coefficient of thermal expansion (CTE). CTE is a glass property that depends on the glass's thermal history and several other parameters, but primarily on the titanium dioxide concentration.
[0004] The substrate precursor made of TiO2-SiO2 mixed glass is mechanically processed into the mirror substrate and mirrored to form a mirror element.
[0005] Due to the constantly increasing demands on the linewidths to be achieved, the requirements for the TiO2-SiO2 mixed glass are also increasing. To achieve smaller linewidths, the EUV source power is often increased. This increase in EUV power leads to higher stepper throughput, but also causes greater heating of the mirrors. Consequently, mirrors that are increasingly homogeneous and defined are required, since otherwise, aberrations increase with increasing source power.
[0006] In addition, ever-decreasing feature sizes inherently require better imaging properties. The numerical aperture plays a particularly important role here. The optical aperture angle of the mirror lens is directly related to the optical resolution. A higher numerical aperture (i.e., a higher beam angle) allows for better resolution. However, this requires larger mirror substrates.
[0007] Due to the manufacturing process, TiO2-SiO2 mixed glass exhibits a microscopic layer structure. JP2006240979A describes a process for reducing this layer structure. It has been found that, in addition to the microscopic, manufacturing-related layer structures, macroscopic, manufacturing-related titanium gradient also occurs during the production of a substrate precursor with a target mass of more than 100 kg. This manufacturing-related titanium gradient affects the quality of the final substrate precursor and cannot be eliminated using known methods. Technical task
[0008] In general, it is an object of the present invention to at least partially overcome a disadvantage arising from the prior art. A further object of the invention is to provide a substrate precursor in which the influences of macroscopic, production-related titanium variations are reduced. Furthermore, it is an object of the invention to provide a substrate precursor in which the influences of macroscopic, production-related property variations are reduced. Furthermore, it is an object of the invention to provide a substrate precursor with a mass of more than 50 kg, in particular more than 100 kg, with which a high numerical aperture is achieved. Preferred embodiments of the invention
[0009] A contribution to at least partially fulfilling at least one of the aforementioned objects is made by the features of the independent claims. The dependent claims provide preferred embodiments that contribute to at least partially fulfilling at least one of the objects.
[0010] In this description, range specifications also include the values referred to as limits. A specification such as "in the range from X to Y" with respect to a quantity A therefore means that A can assume the values X, Y, and values between X and Y. Unilaterally limited ranges such as "up to Y" for a quantity A correspondingly mean the value Y and less than Y.
[0011] Some of the described features are linked to the term "essentially." The term "essentially" is to be understood in such a way that, under real-world conditions and manufacturing techniques, a mathematically exact interpretation of terms such as "superposition," "perpendicular," "diameter," or "parallelism" can never be given literally, but only within certain manufacturing error tolerances. In particular, the term "essentially" can be understood as a variation of + / - 5% of the corresponding value. In particular, "essentially parallel axes" enclose an angle of -5 degrees to 5 degrees to each other, and "essentially equal volumes" encompass a deviation of up to 5% by volume. A "device consisting essentially of quartz glass," for example, comprises a quartz glass content of ≥ 95 to ≤ 100% by weight. Furthermore, "essentially perpendicular" encloses an angle of 85 degrees to 95 degrees. Detailed description
[0012] The invention relates to a process for producing a substrate precursor with a mass of more than 50 kg, comprising a TiO2-SiO2 mixed glass comprising the steps: Introducing a silicon dioxide raw material and a titanium dioxide raw material into a flame, producing a glass body with a titanium dioxide content of 3 wt% up to 10 wt%.-%, wherein the glass body: ∘ has a macroscopic, manufacturing-related titanium gradient, and ∘ has a microscopic, manufacturing-related layer structure, dividing the glass body into a plurality of rod-like glass body sections, spatially measuring the titanium gradient in each of the glass body sections, connecting the glass body sections to form an elongated first glass component, first homogenization treatment of the first glass component, pushing the first glass component together to create a spherical glass system, turning the glass system by more than 70 degrees, pulling the glass system apart to form an elongated second glass component, second homogenization treatment of the second glass component to create a substrate precursor, wherein the substrate precursor is substantially free of layer structure, .
[0013] In order to overcome the above-mentioned disadvantages of the prior art, the invention provides that the measuring step comprises the following steps: Predetermining a desired spatial titanium distribution in the substrate precursor, Providing a model of a titanium distribution in the substrate precursor, wherein the model is dependent on ∘ an arrangement of the plurality of glass body sections in the first glass component relative to one another, ∘ the spatial titanium distribution in each of the glass body sections, and ∘ the effects of the pushing together step and the turning step on the spatial titanium distributions in the glass body sections, Calculating an optimal arrangement of the glass body sections relative to one another using the model so that a difference between titanium distribution and titanium distribution is minimal, Positioning the glass body sections so that in the joining step the glass body sections are joined according to the calculated optimal arrangement.
[0014] The process described involves optimizing the spatial distribution of titanium dioxide, in particular titanium dioxide and at least one other property, in a substrate precursor. For linguistic reasons, the terms "titanium" and "titanium dioxide" are used synonymously below. In fact, the invention and the methods described do not refer to elemental titanium, but rather to its oxidized form, titanium dioxide. Furthermore, the following word endings are used to designate the spatial distributions of titanium dioxide and / or at least one other physical or chemical property in the various stages of the process: in the vitreous body and in the vitreous section the word ending "verlauf", in the substrate precursor the word ending "häufigkeit", in the model the word ending "aufteilung", and in the desired substrate precursor the word ending "verteilung".
[0015] In this respect, a titanium progression differs from a titanium frequency in that the first refers to a titanium dioxide content at spatially different points within a glass body and the second refers to a titanium dioxide content at spatially different points within a substrate precursor.
[0016] The process enables the production of substrate precursors with a mass of more than 50 kg, especially more than 100 kg, which meet the ever-increasing demands for EUV mirror elements. The process comprises the following steps: Introduce
[0017] In the introduction step, a silicon dioxide raw material (e.g., SiCl4 or OMCTS vapor) and a titanium dioxide raw material (e.g., TiCl4 or Ti alkoxide vapor) are subjected to flame hydrolysis. This produces SiO2 and TiO2 particles. Produce
[0018] The SiO2 and TiO2 particles produced during flame hydrolysis can be deposited in two ways. In direct deposition (DQ), deposition occurs on a stamp positioned below the flame. Typically, the temperature conditions are selected so that this deposition occurs with the formation of a compact TiO2-SiO2 mixed glass. In the axial vapor deposition (VAD) process, deposition occurs in the form of a film of SiO2 and TiO2 particles on a support rod. Subsequently, in a second step, the particles are vitrified to form a TiO2-SiO2 mixed glass.
[0019] The result of this step is a glass body with a titanium dioxide content of 3 weight percent (wt%) to 10 weight percent (wt%) TiO2, which has a microscopic, manufacturing-related layered structure - also called short-wave layered structure - resulting from the layered deposition of the SiO2 and TiO2 particles.
[0020] The masses given here and below always refer to the amount of TiO2 (titanium dioxide), not the elemental titanium.
[0021] Due to fluctuations in the mass flow controllers (MFCs), mechanical inaccuracies in the burners or the mounts of the burner and deposition systems, or stochastically and / or deterministically varying thermal boundary conditions during assembly, glass bodies with a weight of more than 50 kg, in particular more than 100 kg, and in particular more than 200 kg, exhibit not only the described microscopic, manufacturing-related layer structure but also a macroscopic, manufacturing-related titanium gradient. The short-wave layer structure has a size of less than 1 mm, in particular less than 0.5 mm.
[0022] This macroscopic titanium gradient—also referred to as long-wave fluctuations or long-wave titanium gradient—has specific fluctuation lengths of 0.15 m to 0.75 m, in particular 0.17 m to 0.5 m, within which the titanium dioxide content fluctuates by a maximum of 0.5 wt.%, in particular a maximum of 0.3 wt.%, in particular between 0.02 wt.% and 0.25 wt.%, in particular between 0.05 wt.% and 0.2 wt.%. In an exemplary glass body with a length of one meter and a titanium dioxide content of 10 wt.% and a macroscopic, production-related fluctuation of + / - 0.5 wt.%, the titanium dioxide content can thus fluctuate spatially, in particular multiple times, between 10.5 wt.% and 9.5 wt.%. Split
[0023] The glass bodies created in the manufacturing step can have a cylindrical, rod-like, or tubular shape. The glass body is divided into a plurality of rod-like glass body sections along a predetermined longitudinal axis. Surveying
[0024] In the measuring step, the titanium dioxide content is determined at several spatially distinct points. This way, an individual titanium profile is determined for each of the glass body sections created in the dividing step. For this purpose, the titanium dioxide content and / or a property is measured along a longitudinal axis of the glass body section. The measurement points are spaced less than 5 cm apart, in particular less than 2 cm apart. The measurement accuracy for determining the titanium dioxide content is 0.005 wt.%. Connect
[0025] A plurality of glass body sections are joined together in the joining step to form an elongated first glass component. The joining can be carried out, in particular, by means of a material bond during a hot process. The term hot process refers to a process step in which the temperature of an element is increased by the introduction of heat. Examples of hot processes: Flame-based hot processes rely on the oxidation of an exothermic gas. One example is the use of hydrogen—also known as "H2"—as a fuel gas (flame hydrolysis). It reacts with the oxygen—also known as "O2"—in the air. Flameless hot processes utilize other heating systems that do not require an open flame. One example is the use of a resistor to convert electrical energy into thermal energy (heat). First homogenization treatment
[0026] In a first homogenization treatment, the short-wave, microscopic layer structures of the first glass component are removed in a single plane using a crucible-free melting process. For this purpose, the first glass component can be clamped into the chucks of a glass lathe and softened zone by zone, with the chucks simultaneously rotating at different speeds or in opposite directions around a rotational axis. The different rotations of the first glass component on either side of the softening zone cause torsion (twisting) and thus mechanical mixing within the glass volume. The area of thermal-mechanical mixing is also referred to as the "shear zone." The shear zone has a length of 2 cm to 8 cm, which is more than an order of magnitude longer than the length of the short-wave layer structures, which have lengths of less than 1 mm.The shear zone is shifted along a longitudinal axis of the first glass component, thereby mixing the component along its length. Microscopic, manufacturing-related layer structures are thus reduced or eliminated in one plane, particularly the plane of the shear zone.
[0027] When the TiO2-SiO2 mixed glass that has undergone a homogenization treatment is examined using a stress detector and interferometer, it is observed that the optical layer structure freedom parallel to the shear zone plane used during homogenization is lower than the layer structure freedom observed perpendicular to the shear zone plane. This shows that the mixing effect used in the shear zone, which serves to achieve layer structure freedom, is lower perpendicular to the rotation axis used during the homogenization treatment than the mixing effect observed along the rotation axis. Push together
[0028] After the initial homogenization treatment, the first glass component is thermally heated and mechanically pushed together. By pushing both ends together along the longitudinal axis of the first glass component, a spherical glass system is created. Turn around
[0029] Relative to the longitudinal axis of the first glass component, the spherical glass system is rotated by more than 70 degrees. The angle of rotation can be between 70 and 110 degrees, particularly between 80 and 100 degrees. Pull apart
[0030] After turning, the glass system is thermally heated to enable longitudinal expansion. This allows the spherical glass system to be formed into an elongated, particularly rod-like, second glass component. Second homogenization treatment
[0031] In order to eliminate any remaining microscopic, manufacturing-related layer structures, the second glass component undergoes a second homogenization treatment. The second homogenization treatment is carried out in the same way as the first homogenization treatment. For this purpose, the second glass component can be clamped in the chuck of the glass lathe and softened zone by zone, with the chucks simultaneously rotating at different speeds or in opposite directions around a rotation axis. The different rotation of the second glass component on either side of the softening zone again causes torsion (twisting) and thus mechanical mixing in the glass volume. The shear zone is moved along a second length of the second glass component, which is thereby reshaped and mixed along its length. Microscopic, manufacturing-related layer structures are thus reduced or eliminated in one plane, particularly the plane of the shear zone.
[0032] If the TiO2-SiO2 mixed glass, which has undergone both homogenization treatments, is examined using a stress detector and interferometer, it can be seen that the microscopic, manufacturing-related layer structures have been essentially removed, in particular to at least 99% compared to the glass body.
[0033] As a result of the second homogenization treatment of the second glass component, a substrate precursor is created that is essentially free of microscopic, manufacturing-related layer structures.
[0034] In one embodiment, the first glass component and / or the second glass component is clamped in the rotation device with a horizontally oriented longitudinal axis, wherein holding elements can be welded to the ends of the first glass component and / or the second glass component in order to minimize the loss of good material. Inventive measurement:
[0035] To overcome the above-mentioned disadvantages in the prior art, it is provided that the measuring step comprises the following steps: predetermining a desired spatial titanium distribution in the substrate precursor, providing a model of a titanium distribution in the substrate precursor, wherein the model is dependent on ∘ an arrangement of the plurality of glass body sections in the first glass component relative to one another, ∘ the spatial titanium distribution in each of the glass body sections, and ∘ the effects of the pushing together step and the turning step on the spatial titanium distributions in the glass body sections, calculating an optimal arrangement of the glass body sections relative to one another using the model, so that a difference between titanium distribution and titanium distribution is minimal, positioning the glass body sections so that in the joining step the glass body sections are joined according to the calculated optimal arrangement.
[0036] When calculating the optimal arrangement, the positions of the vitreous segments relative to each other are permuted. From each permutation, the model calculates a titanium distribution, which is then compared with the titanium distribution by subtraction. From the set of differences, the optimal arrangement of the vitreous segments relative to each other can then be determined, where the difference, especially the spatial difference between the titanium distribution and the titanium distribution, is minimal. Predetermine
[0037] During the predetermination step, an optimal spatial distribution of titanium dioxide in the SiO2 matrix is determined. This titanium distribution represents the target spatial distribution of titanium in the substrate precursor that should be optimally achieved during production.
[0038] The titanium distribution includes both the absolute amount of titanium dioxide in the substrate precursor and its spatial distribution. For example, the substrate precursor can have a cuboid shape. The titanium distribution can be parabolic, with the maximum of the titanium distribution located at the center of a surface of the substrate precursor. Additionally, different edge regions of the substrate precursor can have the same or different titanium distributions. In a further embodiment, the titanium distribution can be flat, i.e., homogeneous, across the entire substrate precursor. Provide
[0039] The method according to the invention involves the use of a model of titanium partitioning in the substrate precursor. This model calculates the spatial distribution of titanium dioxide in the SiO2 matrix. The model uses the following input parameters: A / an arrangement of the plurality of vitreous body sections in the first glass component relative to one another, B / the individual spatial titanium progression in a plurality of vitreous body sections, and C / the effects of the pushing together step and the turning step on the spatial titanium progressions in the vitreous body sections.
[0040] When calculating the spatial distribution of titanium dioxide in the SiO2 matrix based on the input parameters mentioned, the model can take into account further aspects.
[0041] During the production of a glass body, long-wave and short-wave fluctuations in the amount of titanium and / or other properties in the SiO2 matrix arise. Both types are influenced differently in the process steps of the method disclosed here. Using the model, the titanium distribution for a variety of arrangements of the glass body sections can be calculated in the joining step and compared with a target value. This allows the required quality of large substrate precursors to be achieved and waste to be reduced.
[0042] The starting point is that both the first and second homogenization treatments only affect the short-wavelength (microscopic) layer structures and / or short-wavelength (microscopic) changes in the titanium dioxide content. In contrast, long-wavelength changes in the titanium dioxide content remain unaffected by the two homogenization treatments. This fact results from the different length scales of the shear zone and the macroscopic, production-related titanium distribution. The shear zone has an elongated extension of only a few centimeters. Within this shear zone, only short-wavelength structures lying in the plane of the shear zone are compensated.
[0043] The long-wavelength variations in the titanium dioxide content are not affected by the two homogenization treatments. This is because the fluctuation lengths of the long-wavelength variations in the titanium dioxide content and / or a property are at least twice the width of the shear zone.
[0044] The turning step does not affect the short-wavelength (microscopic) layer structures and / or short-wavelength (microscopic) changes in the titanium dioxide content. However, the turning step ensures that the shear zones of the first and second homogenization treatments are arranged essentially perpendicular to each other with respect to the longitudinal axis of the first glass component. This is intended to level out short-wavelength fluctuations as completely as possible.
[0045] The turning step influences the long-wavelength fluctuations. By pushing the first glass component together in the pushing-together step, different long-wavelength fluctuations from different glass body sections are mixed together. Distant volume elements of the first glass component are brought into close proximity by the process and can be mixed in the following step. This can, in particular, depending on the titanium gradient and / or property gradient, lead to an amplification or attenuation of the fluctuation magnitude of the long-wavelength fluctuations. The amplification or attenuation of the fluctuation magnitude therefore depends on the titanium gradients and / or the properties, as well as the relative arrangement of the individual glass body sections.
[0046] Finally, the glass body sections are found in different levels of the substrate precursor. The number of levels depends on the mass of the substrate precursor as well as the number and mass of the glass body sections. In one variant, for a substrate precursor with a mass of more than 50 kg, the number of levels shall be between 2 and 5; for a substrate precursor with a mass of more than 100 kg, the number of levels shall be between 3 and 10; for a substrate precursor with a mass of more than 200 kg, the number of levels shall be between 5 and 20; for a substrate precursor with a mass of more than 300 kg, the number of levels shall be between 10 and 30.
[0047] An exception to the statement that the turning step influences the long-wavelength fluctuations applies to a macroscopic quartz glass volume element that is arranged in the center of the elongated first glass component and, in particular, has a size between 20 cm3 and 100 cm3. Long-wavelength variations in the properties, such as the amount of titanium in the SiO2 matrix, are also found in this macroscopic volume element. The turning step only changes the position of this volume element such that it is located in the center of the spherical glass system. During the subsequent pulling apart, this volume element is again arranged in the center of the elongated second glass component. Consequently, the said volume element, with its long-wavelength fluctuations unaffected by the homogenization, is again arranged centrally in the second glass component.
[0048] In another embodiment, the step of flowing into a graphite mold follows the second homogenization treatment. After the flowing step, the described quartz glass element is found in the center of the substrate precursor and thus significantly determines its behavior. This is all the more true since a convex recess is often ground into the substrate precursor to accommodate the actual mirror, and thus the volume element located directly below the recess strongly influences the behavior of the mirror in use.
[0049] Consequently, the model can consider at least one of the following aspects to seek an optimum where the following aspects are minimal and / or optimal: D / the content of titanium dioxide in functionally essential areas, in particular in a central volume element of the substrate precursor, and E / the content of titanium dioxide in different levels of the substrate precursor.
[0050] The model, which depends at least on the three listed input parameters A / to C / , calculates the spatial distribution of titanium dioxide in the SiO2 matrix of the substrate precursor that potentially results when passing through the process steps, which results in the case of different arrangements of the plurality of glass body sections relative to one another in the first glass component, and / or in the case of a selection of the plurality of glass body sections from a larger plurality of glass body sections connected with different arrangements of the plurality of glass body sections relative to one another in the first glass component. Calculate
[0051] The possible titanium distributions in the substrate precursor, calculated by permuting the arrangement of the vitreous body sections relative to each other using the model, are compared with the desired titanium distribution in the substrate precursor. Since the titanium distribution represents the desired target, the arrangements of the majority of vitreous body sections are selected in which the difference between the titanium distribution and the titanium distribution is minimal.
[0052] As explained, the titanium distribution is determined point by point during the spatial measurement step. In one embodiment, the model only determines a set of points and not a complete curve of the titanium distribution. According to the invention, a difference is calculated for each of the possible permutations of the arrangement of the vitreous segments.
[0053] In one embodiment, the difference in the series of numbers is determined using the root mean square (RMS). The model then examines which of all possible permutations of the arrangement of the vitreous segments results in a minimal, i.e., smallest, difference. The arrangement of the vitreous segments whose calculated difference between titanium distribution and titanium distribution is minimal is then used in the joining step.
[0054] In one embodiment, the difference of the number series is determined by the sum of the magnitude of the differences.
[0055] In one embodiment, the difference of the number series is determined via the arithmetic mean.
[0056] In one embodiment, a minimal difference is understood to mean that the difference between the amount of titanium distribution and the amount of titanium distribution is less than 1.5% of a maximum value of the titanium distribution, in particular less than 1.0%, in particular less than 0.5%. The stated amounts of the difference are therefore relative values, based on the maximum value of the titanium distribution.
[0057] In one embodiment, at least 75%, in particular over at least 85%, in particular at least 90% of a surface of the substrate precursor is taken into account to determine the difference.
[0058] In one embodiment, at least 75%, in particular over at least 85%, in particular at least 90% of a surface of the substrate precursor, which is mirrored in a further step to form a mirror element, is taken into account to determine the difference. Positioning
[0059] The desired substrate precursor is then obtained by joining the glass body sections according to the calculated optimal arrangement in the joining step.
[0060] One embodiment is characterized in that the substrate precursor has a mass of more than 200 kg, in particular more than 300 kg. The macroscopic, production-related titanium variation can, within the context of OVD or DQ processes, result in a spatial variation in the titanium dioxide content of up to 0.5%, based on the desired titanium dioxide content, within a 200 kg TiO2-SiO2 mixed glass. The spatial variation in the titanium dioxide content generally exhibits a continuous pattern, with the fluctuation lengths being between 10 cm and 50 cm. In contrast, the shear zone and second shear zone, in which mixing of the TiO2-SiO2 mixed glass occurs during the two homogenization treatments, have a length of 2 cm to 8 cm.
[0061] For substrate precursors with a mass of more than 100 kg, in particular more than 200 kg, in particular more than 300 kg, the first glass component has a length of more than 2 m, in particular more than 2.8 m. Consequently, a number of macroscopic, production-related fluctuations in the titanium profile can occur, which would have no effect on smaller substrate precursors with a mass of less than 30 kg. One embodiment is characterized in that the method comprises the following step after the second homogenization treatment: Forming the second glass component by softening and flowing into a heated mold into which the second glass component flows under the action of a force to form the substrate precursor.
[0062] In one embodiment, the flow-out step can serve, in particular, to convert the rod-shaped TiO2-SiO2 mixed glass in the second glass component into a block-shaped substrate precursor. For this purpose, the mold can have a block-like interior space into which the TiO2-SiO2 mixed glass of the second glass component flows. In particular, the mold can have an interior space that corresponds to the desired contour and geometry of the desired mirror, and the substrate precursor does not require any significant post-processing (so-called "near net shape").
[0063] During the flow-out step, the second glass component can be placed in the heated mold and flow out under its own weight or under an additional force acting in the axial direction. Instead of slowly flowing out in the heated mold, the same deformation can also be achieved by continuously feeding the second glass component into a heating zone, where it softens the mold arranged in the heating area along its length.
[0064] One embodiment is characterized in that the method comprises the following step: Producing a second glass body having a titanium dioxide content of 3 wt.% up to 10 wt.%, wherein the second glass body: has a second, macroscopic, production-related titanium gradient, and has a second, microscopic, production-related layer structure, dividing the glass body into a plurality of rod-like glass body sections.
[0065] In order to produce substrate precursors with a mass of more than 100 kg, in particular more than 200 kg, in particular more than 300 kg, it may be necessary to produce not only a first glass body but also a second glass body.
[0066] The first and second vitreous bodies exhibit different macroscopic, manufacturing-related titanium gradients. After the manufacturing step, the vitreous body is divided into a plurality of rod-like vitreous body sections, and the second vitreous body is divided into a plurality of rod-like vitreous body sections.
[0067] In one embodiment, all of the plurality of rod-like glass body sections resulting from the first glass body and the plurality of rod-like glass body sections resulting from the second glass body are joined together to form the first glass component.
[0068] In one embodiment, the sum of the plurality of rod-like glass body sections resulting from the first glass body and the plurality of rod-like glass body sections resulting from the second glass body The resulting number of glass body sections is greater than the required number of rod-like glass body sections to create the first glass component. In this case, during the calculation step, a selection is made from the number of available glass body sections for the required number, so that the difference between the titanium distribution and the titanium distribution is minimal.
[0069] In one embodiment, the plurality of glass body sections is a multiple of the plurality by a factor of 1.1 to 2, in particular the plurality of glass body sections is at least twenty and the majority of the glass body sections joined together to form the first glass component is a maximum of fifteen, in particular the plurality of glass body sections is at least fifteen and the majority of the glass body sections joined together to form the first glass component is a maximum of ten.
[0070] By means of the disclosed method, a selection can be made that overcomes the above-mentioned disadvantages in the prior art.
[0071] One embodiment is characterized in that at least three, in particular at least five, in particular at least eight glass body sections are connected to form the first glass component.
[0072] For substrate precursors with a mass of more than 100 kg, a plurality of glass body sections are required that are bonded together. Due to the spatial variations in the titanium dioxide content, which vary between 10 cm and 50 cm, the method according to the invention is particularly suitable for a combination of more than three, in particular more than five, and especially more than eight glass body sections, in order to create a substrate precursor that meets the stringent requirements of EUV microlithography.
[0073] One embodiment is characterized in that the difference between titanium distribution and titanium distribution is less than 1.5% relative to a maximum value of the titanium distribution, in particular less than 1.0%, in particular less than 0.5%.
[0074] During the measurement step, a minimum difference between the titanium distribution and the titanium distribution is determined by comparing the model with the desired titanium distribution. Due to the ever-increasing demands on the material properties of the substrate precursors, the absolute value of the difference may be subject to the aforementioned limits.
[0075] One embodiment is characterized in that the glass body has at least one of the following property profiles: a macroscopic, manufacturing-related OH curve, a macroscopic, manufacturing-related CTE curve, a macroscopic, manufacturing-related fluorine curve, a macroscopic, manufacturing-related bubble curve, a macroscopic, manufacturing-related ODC curve, a macroscopic, manufacturing-related Ti3+ curve, a macroscopic, manufacturing-related metallic impurity curve.
[0076] During OVD or DQ processes, macroscopic, manufacturing-related variations in the properties listed above may occur. The resulting variation lengths are comparable to those of titanium dioxide and range between 12.5 cm and 50 cm, particularly for OH, CTE, and Ti3+, and between 15 cm and 85 cm for fluorine, bubbles, ODC, and metallic impurities.
[0077] An embodiment is characterized in that in the measuring step at least one of the property curves is measured in each of the glass body sections.
[0078] One embodiment is characterized in that the measuring step comprises the following steps: Predetermining a desired spatial property distribution in the substrate precursor, Providing a model of a property distribution in the substrate precursor, wherein the model is dependent on an arrangement of the plurality of glass body sections in the first glass component relative to one another, a spatial property profile in each of the glass body sections, and the effects of the pushing together step and the turning step on the spatial property profile in the glass body sections, Calculating an best possible arrangement of the glass body sections relative to one another using the model such that a total difference is minimal, wherein the total difference comprises the difference between titanium distribution and titanium distribution and the difference between property distribution and property distribution, Positioning the glass body sections such that in the joining step the glass body sections are joined according to the calculated best possible arrangement.
[0079] In parallel with the step of predetermining the titanium distribution, in this embodiment, at least one desired spatial property distribution is predetermined in the substrate precursor. The at least one property distribution thus represents, in addition to the titanium distribution, a second target variable that is optimally fulfilled and / or desired in the substrate precursor.
[0080] In one variant, the total difference can be calculated from the sum the amount of the difference between titanium distribution and titanium distribution and the amount of the difference between property distribution and property distribution be calculated.
[0081] Like the titanium gradient, the property gradient is also measured point by point. The model then calculates the values of the property in the substrate precursor (the property distribution) from the set of values. The model can thus calculate a difference between the property distribution and the property distribution for each of the possible permutations of the arrangement of the vitreous segments.
[0082] Based on this, the model can calculate two independent differences for each of the possible permutations of the arrangement of the vitreous sections, namely Determine the difference between the titanium distribution and the titanium distribution, and the difference between the property distribution and the property distribution. In one embodiment, each of the two differences is determined using the root mean square (RMS). In one embodiment, each of the two differences is determined using the arithmetic mean.
[0083] The model then calculates a sum difference for each possible permutation. The two differences to be considered can be added together in different ways. Thus, the sum difference can be calculated from the sum of the amounts of the two differences to be considered, or the arithmetic mean or geometric mean of the two differences to be considered, or the weighted mean of the two differences to be considered.
[0084] In one variant, the model can be used to determine the total difference The difference between titanium distribution and titanium weighting and the difference between property distribution and property distribution are weighted differently. For example, the difference between titanium distribution and titanium weighting can be considered twice or three times when searching for the minimum of the total difference, since the amount of titanium dioxide significantly influences the CTE and therefore requires special consideration for the intended use.
[0085] In one embodiment, a minimum sum difference is understood to mean that the difference between the titanium distribution and the titanium distribution over at least 75%, in particular over at least 85%, in particular at least 90% of a surface of the substrate precursor is less than 1.5% based on a maximum value of the titanium distribution, in particular less than 1.0%, in particular less than 0.5%, and the difference between the property distribution and property distribution over at least 75%, in particular over at least 85%, in particular at least 90% of a surface of the substrate precursor is less than 1.5% based on a maximum value of the property distribution, in particular less than 1.0%, in particular less than 0.5%.
[0086] In one embodiment, a minimum sum difference is understood to mean that the difference between the titanium distribution and the titanium distribution over at least 75%, in particular over at least 85%, in particular at least 90% of a surface of the substrate precursor which is mirrored in a further step to form a mirror element is less than 1.5% of a maximum value of the titanium distribution, in particular less than 1.0%, in particular less than 0.5%, and the difference between the property distribution and property distribution over at least 75%, in particular over at least 85%, in particular at least 90% of a surface of the substrate precursor which is mirrored in a further step to form a mirror element is less than 1.5% of a maximum value of the property distribution, in particular less than 1.0%, in particular less than 0.5%.
[0087] The model used in this version is functionally dependent on an arrangement of the plurality of glass body sections in the first glass component relative to one another, the spatial titanium profile and a spatial property profile in each of the glass body sections, and the effects of the pushing-together step and the turning-over step on the spatial titanium profile and on the spatial property profile in the glass body sections.
[0088] Consequently, both the aspects concerning titanium dioxide and the aspects concerning at least one other property (e.g. ODC, Ti3+ etc.) are taken into account when calculating the optimal arrangement of the vitreous body sections.
[0089] Based on the solution space of possible arrangements of the vitreous segments relative to each other, the best possible arrangement of the vitreous segments is determined by permutation. The goal is to minimize the sum difference, whereby the sum difference the difference between titanium distribution and titanium distribution and the second difference between the at least one property distribution and the at least one property distribution.
[0090] Subsequently, the vitreous body sections are positioned in such a way that in the joining step the vitreous body sections are joined according to the calculated best possible arrangement.
[0091] An embodiment is characterized in that the sum difference is less than 1.5% of the sum of a maximum value of the titanium distribution and a maximum value of the property distribution, in particular less than 1.0%, in particular less than 0.5%.
[0092] One embodiment is characterized in that the difference between the titanium distribution and the titanium distribution is less than 1.5%, in particular less than 1.0%, in particular less than 0.5% of the maximum value of the titanium distribution, and the second difference between the at least one property distribution and the at least one property distribution is less than 1.5%, in particular less than 1.0%, in particular less than 0.5% of the maximum value of the respective property distribution.
[0093] This embodiment is particularly suitable for meeting the stringent requirements for EUV substrate precursors. Substrate precursors with differences and second differences above the listed values are often unusable for creating mirror substrates with deviations from predicted line edges of less than 3 nm.
[0094] One embodiment is characterized in that the difference between titanium distribution and titanium distribution is between 0.15% and 1% of the maximum value of the titanium distribution, and the second difference ∘ between the Ti3+ distribution and the Ti3+ distribution is less than 5.0%, in particular less than 2.0% of the maximum value of the Ti3+ distribution, and ∘ between the OH distribution and the OH distribution is less than 2.0%, in particular less than 1.0%, in particular less than 0.5% of the maximum value of the OH distribution.
[0095] This embodiment is particularly suitable for producing substrate precursors from which mirror substrates can be produced that have deviations from predicted line edges of less than 3 nm.
[0096] An embodiment is characterized in that the step of producing the glass body comprises at least the following steps: Creating a porous soot body, with the macroscopic, manufacturing-related titanium structure running along a longitudinal axis and the microscopic, process-related layer structure running along a growth axis, vitrifying the soot body to create the cylindrical glass body.
[0097] In one embodiment of the invention, the step of creating a porous soot body comprises the following process steps: Providing a liquid SiO2 feed material comprising more than 60 wt.% of the polyalkylsiloxane D4, evaporating the liquid SiO2 feed material into a gaseous SiO2 feed vapor, evaporating a liquid TiO2 feed material into a gaseous TiO2 feed vapor, converting the SiO2 feed vapor and the TiO2 feed vapor to SiO2 particles and TiO2 particles, depositing the SiO2 particles and the TiO2 particles on a deposition surface to form the porous soot body.
[0098] Octamethylcyclotetrasiloxane (also referred to here as D4) is the main component in the production of the soot body. The production of a soot body according to the above-mentioned steps reduces the strengths of the macroscopic, manufacturing-related titanium dioxide and / or property variations.
[0099] One embodiment is characterized in that the first glass component is heated prior to the pushing-together step. The heating causes the first glass component to become at least partially viscous, which facilitates mechanical deformation. The heating can be carried out using a flame-based hot process or a flame-free hot process.
[0100] One embodiment is characterized in that the connection takes place at a respective contact surface of the glass body sections.
[0101] The features disclosed in the description may be essential for various embodiments of the claimed invention, both separately and in any combination with one another.
[0102] The values given for the difference, the total difference and the second difference are relative quantities that refer to the respective distribution - i.e. the respective desired amount in the substrate precursor.
[0103] In this document, embodiments that disclose two or more features, each having preferred ranges or alternatives, are to be understood as including all possible combinations of those features.
[0104] In this description, range specifications also include the values referred to as limits. A specification such as "in the range from X to Y" with respect to a quantity A therefore means that A can assume the values X, Y, and values between X and Y. Unilaterally limited ranges such as "up to Y" for a quantity A correspondingly mean the value Y and less than Y.
[0105] The invention is further illustrated below by means of exemplary figures. The invention is not limited to the figures. Figures
[0106] It shows Fig. 1 shows the creation of a soot body, Fig. 2 shows the vitrification of the soot body to form a glass body, Fig. 3 shows the glass body, Fig. 4 shows a glass body section created by dividing the glass body, Fig. 5 shows a representation of a two-dimensional macroscopic, production-related titanium profile in a glass body section, Fig. 6 shows an arrangement of two glass body sections, Fig. 7a shows a substrate precursor, Fig. 7b shows a representation of a titanium profile of several glass body sections in comparison to a desired titanium distribution, Fig. 8 shows a further representation of a titanium profile of several glass body sections in comparison to a desired titanium distribution, Fig. 9 shows a first homogenization treatment, Fig. 10 shows the pushing together of the first glass component, Fig. 11 shows a second homogenization treatment, and Fig. 12 shows an illustration of the method according to the invention. Description of the characters
[0107] Figure 1shows an apparatus 100 for producing a titanium-doped SiO2 soot body 200. A plurality of flame hydrolysis burners 220 arranged in a row are arranged along a support tube 210 made of aluminum oxide.
[0108] A silicon dioxide raw material and a titanium dioxide raw material are fed into the reaction zone of the flame hydrolysis burner 220 in gaseous form and decomposed by oxidation and / or hydrolysis and / or pyrolysis. In the reaction zone, SiO2 particles and TiO2 particles are formed, both of which are deposited in layers on the support tube 210 to form the SiO2-TiO2 soot body 200. The SiO2-TiO2 particles themselves are in the form of agglomerates or aggregates of SiO2 primary particles with particle sizes in the nanometer range. In particular, the layered structure allows the soot body 200 to have a microscopic layered structure.
[0109] In particular, during the production 1100 of large-volume cylindrical soot bodies 200 for producing a substrate precursor 900 with a mass of more than 50 kg, in particular more than 100 kg, in particular more than 200 kg, the flame hydrolysis burners 220 can be mounted on a common burner block which is moved back and forth parallel to a longitudinal axis of the support tube 210 between two turning points which are fixed with respect to the longitudinal axis.
[0110] This movement of the flame hydrolysis burners 220, mechanical inaccuracies in the feed lines of the raw materials or the burners 220, or even variations in the process temperatures can lead to the soot body 200 exhibiting a macroscopic, production-related spatial fluctuation in the physical properties, such as the TiO2 content.
[0111] In the Figure 2vitrification of the soot body 200 is shown. The vitrification preferably takes place in a process chamber. The vitrification temperature is preferably in a range from 1200 to 1500 °C, preferably 1250 to 1350 °C. In order to avoid bubble formation in the subsequent quartz glass, it has proven advantageous if the pressure inside the process chamber is lower than outside the process chamber during vitrification, i.e., the vitrification is carried out at reduced pressure. This also has the advantage that the material of the process chamber is not attacked by aggressive and corrosive gases and is therefore subject to reduced wear. Therefore, an embodiment is preferred in which vitrification preferably takes place at a pressure of less than 1 mbar. During vitrification, the soot body 200 can be moved through a vitrification furnace 250 according to movement arrow 251.
[0112] Vitrification transforms the soot body 200 into a glass body 300 with a titanium dioxide content of 3 wt.% to 10 wt.%. The manufacturing-related variations in the physical properties that already occurred in the soot body 200 are transferred to the glass body 300, so that it has a macroscopic, manufacturing-related titanium gradient, and a microscopic, manufacturing-related layer structure.
[0113] The mass specified for titanium, ranging from 3 wt.% to 10 wt.%, refers to the amount of TiO2 (titanium dioxide), not elemental titanium.
[0114] In the Figure 3 The cylindrical glass body 300 is shown. A dotted line indicates a section that is cut out of the glass body during the dividing step 1200. The rod-like glass body section 400 thus created is shown in the Figure 4In particular, the glass body 300 can be divided into a plurality of rod-like glass body sections 400, which have a longitudinal slit 440. In particular, the glass body sections 400 can have a circular sector-like cross-section.
[0115] Through a first homogenization treatment 1600 of a first glass component and a second homogenization treatment 2000 of a second glass component, the microscopic, manufacturing-related layer structure is reduced to such an extent that the glass body portion 400 is essentially free of layer structure. However, the two homogenization treatments 1600, 2000 do not allow the substrate precursor 900 to be free of long-wavelength titanium gradients, which significantly influence the quality and usability of the substrate precursor 900 in EUV lithography.
[0116] In Figure 4The glass body section 400 is shown, where a titanium gradient 410 is spatially measured. For this purpose, the titanium dioxide content is measured at several measuring points (P1, P2, P3, P4, P5, P6) along the longitudinal axis 420. These measuring points are spaced less than 5 cm apart, in particular less than 2 cm apart. This selective measurement of the titanium dioxide content provides a clear picture of the conditions in the glass body section 400. Any fluctuations in the titanium gradient occur on length scales of 0.15 m to 0.75 m.
[0117] In addition, during the manufacturing 1100 of the soot body 200, further macroscopic, manufacturing-related variations in the chemical and / or physical properties of the glass body 300 can arise due to mechanical influences. At least one of these variations, referred to as property profile 510, can also be determined in the measuring step 1300. The following chemical and / or physical properties, which have macroscopic, manufacturing-related property profiles 510, can be measured individually or in any combination: OH content, CTE, fluorine content, bubble content, ODC content, Ti3+ content, and content of metallic impurities.
[0118] The property profile 510 can be measured in parallel and analogous to the titanium profile 410. For this purpose, the physical property is measured at several measuring points (P1, P2, P3, P4, P5, P6) along the longitudinal axis 420. Here, too, the measuring points are spaced less than 5 cm apart, in particular less than 2 cm apart.
[0119] In the Figure 5 The result of a measurement 1300 of a titanium profile 410 and a property profile 510 in the glass body section 400 is shown schematically. The amount in wt.% of titanium dioxide or in ppm of the property is plotted as a function of the position along the longitudinal axis 440 of the glass body section 400. To simplify the description, Figure 4 and 5 only measurement results for six measuring points (P1, P2, P3, P4, P5, P6) are shown.
[0120] The steps and / or aspects of the spatial measurement 1300 of the titanium profile 410 described below also apply to a spatial measurement of at least one property profile 510.
[0121] As can be seen from the diagram, the titanium dioxide content lies within the specified range of 3 wt.% to 10 wt.%. However, due to manufacturing reasons, this titanium dioxide content fluctuates between 5.4 wt.% and 6.1 wt.% along the longitudinal axis 420 of the glass body portion 400.
[0122] Also shown is the amount of a property measured at the six measuring points (P1, P2, P3, P4), here the OH content in ppm as an example, as property curve 510. Due to manufacturing reasons, this OH content fluctuates along the longitudinal axis 420 of the glass body section 400 between 150 ppm and 175 ppm.
[0123] In the Figure 6a connection 1500 of a plurality - here two - rod-like glass body sections 400,400' to form an elongated first glass component 600 is shown.
[0124] For this purpose, a flat contact surface 401 of the first glass body section 400 and a flat contact surface 401' of the second glass body section 400' can be joined by wringing and welded together. This is a "cold joining process" in which only the immediate area of the contact surface experiences any significant heating.
[0125] Alternatively, the joining 1500 may include a joining step in which both glass body sections 400, 400' are softened in a furnace and joined together. This is a "hot joining process" in which the individual glass body sections 400, 400' are joined together by welding. As described, the titanium dioxide and / or property profiles are measured at several measuring points. For the glass body section 400, for example, the titanium profile 410 is measured at measuring points P1, P2, P3, P4, P5, P6. For the glass body section 400', the titanium profile 410' is measured at measuring points P7, P8, P9, P10, P11, P12.
[0126] Within the scope of the method, at least three, in particular at least five, in particular at least eight glass body sections can be connected to one another to form a first glass component 600, which also Figure 9 clarified.
[0127] How Figure 5As illustrated, the titanium gradient 410 fluctuates along the longitudinal axis of the glass body section 400. In addition, the titanium gradient also fluctuates between different glass body sections 400, 400'. In the prior art, these macroscopic, production-related fluctuations of the individual titanium gradients between different glass body sections 400, 400' were not further taken into account. Rather, for substrate precursors 900 with a low mass, only a few, in particular only two, glass body sections 400, 400' were required, so that the fluctuations occurring between the long-wave titanium gradients 410 in the glass body sections 400, 400' could be ignored. This is no longer possible when producing substrate precursors with a mass of more than 50 kg, in particular more than 100 kg, especially when at least four glass body sections have to be connected to one another.
[0128] The Figure 7a , 7band the Figure 8 illustrate the steps used in the Measure 1300 step, which serve to overcome the disadvantages mentioned above.
[0129] It is intended to show how, by permuting the arrangement of the vitreous body sections 400, 400', 400", 400‴ relative to one another, a titanium distribution 430 is calculated with the aid of the model and compared with the desired titanium distribution 420.
[0130] The steps and / or aspects of minimizing a difference between titanium distribution and titanium distribution described below also apply to minimizing a second difference between at least one property distribution and at least one property distribution.
[0131] The starting point is a predetermination 1400 of a desired titanium distribution 420 in the substrate precursor. In one embodiment, the titanium distribution 420 represents the two-dimensional distribution of the amount of TiO2 in the substrate precursor, in particular along a center line, in particular on the outer surface to be mirrored later, through the substrate precursor. In this embodiment, the model can calculate a two-dimensional titanium distribution in the substrate precursor from the two-dimensionally determined titanium profiles and their relative arrangement.
[0132] In Figure 7a A substrate precursor 900 is shown. This should optimally have a titanium distribution 420, as shown in the upper diagram in Figure 7b As an example, a parabolic titanium distribution 420 within an interval of 4.75 wt.% to 5.5 wt.% TiO2 is desired, which has a maximum in a center of the substrate precursor.
[0133] The desired two-dimensional titanium distribution 420 can be found in the substrate precursor 900 on the outer surface 910 to be later mirrored along a center line 920. The type and configuration of the titanium distribution 420 can depend in particular on the application and the operating conditions of the subsequent EUV mirror. A titanium distribution that has a parabolic (or Gaussian) profile with a maximum in the center of the substrate precursor is particularly preferred. In particular, the titanium distribution—and thus the CTE—can be adapted to the distribution of the incident EUV radiation.
[0134] To clarify the procedure, Figure 7b assumed that the substrate precursor 900 is formed from only four glass body sections 400, 400', 400", 400‴. These are - analogous to Figure 6- arranged relative to one another in such a way that a rod-like glass body 300 is formed. The four glass body sections 400, 400', 400", 400‴ are assembled in the following arrangement to form the first glass component 600: The end side of the glass body section 400 is connected to the front side of the glass body section 400' (point E2), the end side of the glass body section 400' is connected to the front side of the glass body section 400" (point E3), the end side of the glass body section 400" is connected to the front side of the glass body section 400‴ (point E4).
[0135] In the middle diagram in Figure 7b The titanium profiles 410, 410', 410", 410‴ of the four glass body sections 400, 400', 400", 400‴ are shown, which were created from at least one glass body 300. The family of measured values for the amounts of TiO2 in wt.% in each of the four glass body sections 400, 400', 400", 400‴ is plotted.
[0136] To overcome the above-mentioned disadvantages, a model is used that can calculate a titanium distribution 430 in the substrate precursor 900. The model uses the following input parameters: the arrangement of the plurality of glass body sections 400, 400', 400", 400‴ in the first glass component 600 relative to one another, the spatial titanium gradients 410, 410', 410", 410‴ in each of the glass body sections 400, 400', 400", 400‴, and the effects of the pushing together step 1700 and the turning step 1800 on the spatial titanium gradients 410, 410', 410", 410‴ in the glass body sections 400, 400', 400", 400‴.
[0137] Based on this arrangement, the model calculates the titanium distribution 430 in the substrate precursor 900. This titanium distribution 430 is shown in the lower diagram in Figure 7b shown.
[0138] How Figure 7bAs illustrated, the illustrated course of the calculated titanium distribution 430 does not simply correspond to a linear sequence of the illustrated courses of the titanium courses 410, 410', 410", 410‴ in the assumed arrangement. Rather, the method steps of the method disclosed here result in the spatial position and orientation of a titanium course 410, 410', 410", 410‴ after running through the method no longer corresponding to the spatial position that the glass body section 400, 400', 400", 400‴ corresponding to the titanium course had in the first glass body 300. Thus, the spatial position of the titanium course 410, 410', 410", 410‴ changes in such a way that a model is required to determine the position and quantity of TiO2 in the titanium distribution 430 of the substrate precursor. 900 to be calculated.
[0139] The Figure 7bThe calculated titanium distribution 430 shown has a zigzag shape and thus deviates significantly from the desired parabolic titanium distribution 420.
[0140] To achieve an optimal arrangement, the possible arrangements of the vitreous sections are permuted. The model calculates the effects of all possible arrangements of the vitreous sections on the titanium distribution 430. This is intended Figure 8 The starting point is a Figure 7 different arrangement of the four glass body sections 400, 400', 400", 400‴, which are assembled in the following arrangement to form the first glass component 600: The end side of the glass body section 400" is connected to the front side of the glass body section 400‴ (point E2), the end side of the glass body section 400‴ is connected to the front side of the glass body section 400' (point E3), the end side of the glass body section 400' is connected to the front side of the glass body section 400 (point E4).
[0141] The model calculates a titanium distribution 430` in the substrate precursor 900 from the titanium distributions 410", 410‴, 410`, 410. This titanium distribution 430' is more similar in both magnitude and progression to the desired titanium distribution 420 than the one in Figure 7b shown titanium distribution 430.
[0142] In particular, the model calculates the corresponding titanium distribution 430, 430' from each possible arrangement of the glass body sections 400, 400', 400", 400‴ and compares this with the desired titanium distribution 420. For this purpose, all possible arrangements of the glass body sections 400, 400', 400", 400‴ are permuted. Based on this information, the model calculates a difference between the titanium distribution and the titanium distribution 420. The optimal arrangement is the arrangement in which the amount of the difference, in particular the maximum difference amount between two spatially identical points on the substrate precursor, is minimal.
[0143] Subsequently, the glass body sections 400, 400', 400", 400‴ are positioned and connected according to the optimal arrangement.
[0144] Analogously, at least one property distribution in addition to the titanium distribution can represent a second target value that is optimally fulfilled and / or aimed for in the substrate precursor 900. The model used in this embodiment is functionally dependent on an arrangement of the plurality of glass body sections 400, 400', 400", 400‴ in the first glass component 600 relative to one another, the spatial titanium profile 410, 410', 410", 410‴ and a spatial property profile 510 in each of the glass body sections 400, 400', 400", 400‴, and the effects of the pushing-together step and the turning step on the spatial titanium profile 410, 410', 410", 410‴ and on the spatial property profile 510 in the glass body sections 400, 400', 400", 400‴.
[0145] Consequently, both the aspects concerning the element titanium dioxide and the at least one other property (e.g. ODC, Ti3+ etc.) are taken into account when calculating the optimal arrangement of the glass body sections.
[0146] Based on the solution space of possible arrangements of the vitreous body sections to each other, the best possible arrangement of the vitreous body sections 400, 400', 400", 400‴ is determined. The aim is that the sum difference is minimal, whereby the sum difference the difference between titanium distribution and titanium distribution and the second difference between the at least one property distribution and the at least one property distribution.
[0147] In the Figure 916 shows a first homogenization treatment 1600 of the first glass component 600, which is created from the glass body sections 400", 400‴, 400', 400. Both the glass body and the first glass component 600 created from the glass body sections 400", 400‴, 400', 400 have microscopic, production-related layer structures. In order to reduce this and / or to enable the production of a substrate precursor 900 that is essentially free of layer structures, two homogenization treatments are carried out sequentially.
[0148] In the first homogenization treatment 1600, the first glass component 600 is clamped in a glass lathe 605 equipped with one or more burners 220 and homogenized by means of a forming process as described in EP 673 888 A1 for the purpose of completely removing layer structures.
[0149] The glass lathe 605 has two chucks 610, 610', which can be set into rotation 650, 650' independently of each other. The first glass component 600 is clamped between the two chucks 610, 610'. Two holding elements 620, 620' can ensure a better fit between the chucks 610, 610' and the first glass component 600. Using the burner 220, the first glass component 600 is heated at specific points and softened, creating a shear zone 630. This shear zone 630 allows the application of an external force, such as a torsional force, tensile force, or compressive force, to the rod-shaped first glass component 600. Within the shear zone 630, regions are created that exhibit different stresses or experience different movements, which is accompanied by a shearing effect or stretching and compressing effect. To generate this force, the two chucks 610, 610` can rotate in opposite directions 650, 650`.
[0150] During the first homogenization treatment 1600, microscopic, manufacturing-related layer structures in a plane of the shear zone of the first glass component 600 are effectively reduced. However, the reduction of microscopic, manufacturing-related layer structures perpendicular to the plane of the shear zone of the first glass component 600 is significantly lower.
[0151] In order to remove the remaining residues of the layer structures in a second homogenization treatment 2000, the first glass component 600 must be reshaped. Figure 10illustrates a pushing together 1700 of the first glass component 600 to create a spherical glass system 700. For this purpose, the first glass component 600 is heated and compressed using the burner 220. The pushing together 1700 can be achieved by moving the two chucks 610, 610' towards each other, as illustrated by the movement arrow 612. Subsequently, the glass system 700 is rotated 1800 by more than 70 degrees. For this purpose, the glass system 700 is removed from the chucks 610, 610' and rotated, as illustrated by the movement arrow 615. This rotation ensures that the portion of the layer structure that was only slightly or not at all equalized in the first homogenization treatment 1600 can be effectively reduced in the second homogenization treatment 2000. After turning the glass system 700 by more than 70 degrees (1800), it is clamped again into the chucks 610, 610'. Subsequently, the glass system 700 is pulled apart (1900).This mechanical deformation of the spherical glass system 700 into an elongated second glass component 800 is carried out by heating the glass system 700 with the burner 220 and moving the chucks 610, 610' away from each other, which is illustrated by the movement arrow 613.
[0152] In the Figure 11A second homogenization treatment 2000 of the second glass component 800 is shown. The second homogenization treatment 2000 proceeds essentially analogously to the first homogenization treatment 1600. The crucial difference is that, due to the turning 1800, the layer structure that was previously essentially perpendicular to the longitudinal axis of the glass lathe 605 now lies in the direction of the longitudinal axis of the glass lathe 605. The second glass component 800 is clamped between the two chucks 610, 610' of the glass lathe 605. By means of the burner 220, the second glass component 800 is heated at specific points and softened, creating a second shear zone 640. This second shear zone 640 allows the application of an external force, such as a torsional force, tensile force, or compressive force, to the rod-shaped second glass component 800.Within the second shear zone 640, this creates areas that exhibit different stresses or experience different movements, resulting in a shearing effect or stretching and compressing effect. To generate this force, the two chucks 610, 610' can rotate in opposite directions (650, 650').
[0153] During this second homogenization treatment 2000, microscopic, production-related layer structures are effectively reduced in the direction perpendicular to the longitudinal axis of the first glass component 600 and / or in the direction of a longitudinal axis of the second glass component 800. After passing through both the first homogenization treatment 1600 and the second homogenization treatment 2000, a substrate precursor 900 is formed that is essentially free of layer structures.
[0154] In the Figure 12A process for producing a substrate precursor 900 with a mass of more than 100 kg, comprising a TiO2-SiO2 mixed glass, is shown. It comprises the following steps: Introducing 1000 a silicon dioxide raw material and a titanium dioxide raw material into a flame, producing 1100 a glass body with a titanium dioxide content of 3 wt% up to 10 wt.-%, wherein the glass body: has a macroscopic, manufacturing-related titanium gradient, and has a microscopic, manufacturing-related layer structure, dividing 1200 the glass body into a plurality of rod-like glass body sections, spatially measuring 1300 the titanium gradient in each of the glass body sections, connecting 1500 the glass body sections to form an elongated first glass component, first homogenization treatment 1600 of the first glass component, pushing together 1700 the first glass component to create a spherical glass system, turning 1800 the glass system by more than 70 degrees, pulling apart 1900 the glass system to form an elongated second glass component, second homogenization treatment 2000 of the second glass component to create a substrate precursor 900, wherein the substrate precursor 900 is substantially free of layer structure.
[0155] The method is characterized by the fact that the measuring step 1300 includes the following steps: Predetermining 1400 a desired spatial titanium distribution in the substrate precursor 900, providing 1420 a model of a titanium distribution in the substrate precursor 900, wherein the model is dependent on an arrangement of the plurality of glass body sections in the first glass component relative to one another, the spatial titanium distribution in each of the glass body sections, and the effects of the pushing together step and the turning step on the spatial titanium distributions in the glass body sections, calculating 1450 an optimal arrangement of the glass body sections relative to one another using the model such that a difference between the titanium distribution and the titanium distribution is minimal, positioning 1470 the glass body sections such that in the joining step the glass body sections are joined according to the calculated optimal arrangement. Reference symbol
[0156] 100Device 200Soot body 210Support tube 220Burner or flame hydrolysis burner 225Flame 250Viagrain furnace 251Movement arrow 300 glass bodies 400, 400', 400"Vitreous section 401, 401'Contact surface 410, 400', 400", 400‴Titanium gradient 420Titanium distribution 430Titanium division 440Longitudinal axis 510Property History 600First glass component 605Glass lathe 610, 610`Chuck 612Movement arrow 613Movement arrow 615Movement arrow 620, 620`Two holding elements 630Shear zone 640Second shear zone 650, 650`Rotation 700Spherical glass system 800Second glass component 900Substrate precursor 910Outer surface 920Center line 1000Insertion 1100Manufacture 1200Division 1300Spatial measurement 1400Predetermination 1420Preparation of a model 1450Calculation of an optimal arrangement 1470Positioning the glass body sections 1500Connecting the glass body sections 1600First homogenization treatment 1700Pushing together 1800Turning the glass system 1900Pulling apart 2000Second homogenization treatment
Claims
1. A method for producing a substrate precursor (900) having a mass of more than 50 kg, comprising a TiO2-SiO2 mixed glass, comprising the steps of: • introducing (1000) a silicon dioxide raw material and a titanium dioxide raw material into a flame (225), • producing (1100) a glass body (300) having a titanium dioxide content of 3 wt.% up to 10 wt.%, the glass body (300) comprising: • a macroscopic, production-related titanium profile (410, 410', 410", 410‴), and • a microscopic, production-related layer structure, • dividing (1200) the glass body into a plurality of rod-like glass body portions (400, 400', 400", 400‴), • spatially measuring (1300) the titanium profile (410, 410', 410", 410‴) in each of the glass body portions (400, 400', 400", 400‴), • connecting (1500) the glass body portions (400, 400', 400", 400‴) to form an elongate first glass component (600), • first homogenization treatment (1600) of the first glass component (600), • pushing together (1700) the first glass component (600) in order to produce a spherical glass system (700), • turning (1800) the glass system (700) by more than 70 degrees, • pulling apart (1900) the glass system (700) to form an elongate second glass component (800), • second homogenization treatment (2000) of the second glass component (800) in order to produce a substrate precursor (900), the substrate precursor (900) being substantially layer-structure-free, characterized in that the step of measuring comprises the following steps: • predetermining (1400) a desired spatial titanium distribution (420) in the substrate precursor (900), • providing (1420) a model of a titanium partition (430) in the substrate precursor (900), the model being dependent on • an arrangement of the plurality of glass body portions (400, 400', 400", 400‴) in the first glass component (600) relative to one another, • the spatial titanium profile (410, 410', 410", 410‴) in each of the glass body portions (400, 400', 400", 400‴), and • the effects of the step of pushing together (1700) and the step of turning (1800) on the spatial titanium profiles (410, 410', 410", 410‴) in the glass body portions, • calculating (1450) an optimal arrangement of the glass body portions (400, 400', 400", 400‴) relative to one another using the model, so that a difference between the titanium partition (430) and the titanium distribution (420) is minimal, • positioning (1470) the glass body portions (400, 400', 400", 400‴) so that in the step of connecting (1500) the glass body portions (400, 400', 400", 400‴) are connected according to the calculated optimal arrangement.
2. The method according to claim 1, characterized in that the substrate precursor (900) has a mass of more than 100 kg, in particular more than 200 kg, in particular more than 300 kg.
3. The method according to either claim 1 or claim 2, characterized in that the method comprises the following step: • producing a second glass body having a titanium dioxide content of 3 wt.% up to 10 wt.%, the second glass body comprising: • a second, macroscopic, production-related titanium profile, and • a second microscopic, production-related layer structure, • dividing the second glass body into a plurality of rod-like glass body portions.
4. The method according to at least one of the preceding claims, characterized in that at least three, in particular at least five, in particular at least eight glass body portions are connected to form the first glass component.
5. The method according to at least one of the preceding claims, characterized in that the difference between the titanium partition (430) and the titanium distribution (420) is less than 1.5% based on a maximum value of the titanium distribution (420), in particular less than 1.0%, in particular less than 0.5%.
6. The method according to at least one of claims 1 to 5, characterized in that the glass body has at least one of the following property profiles (510): • a macroscopic, production-related OH profile, • a macroscopic, production-related CTE profile, • a macroscopic, production-related fluorine profile, • a macroscopic, production-related bubble profile, • a macroscopic, production-related ODC profile, • a macroscopic, production-related Ti3+ profile, • a macroscopic, production-related profile of metal contamination.
7. The method according to claim 6, characterized in that in the step of measuring, at least one of the property profiles (510) in each of the glass body portions (400, 400', 400", 400‴) is measured.
8. The method according to claim 7, characterized in that the step of measuring comprises the following steps: • predetermining a desired spatial property distribution in the substrate precursor (900), • providing a model of a property partition in the substrate precursor (900), the model being dependent on • an arrangement of the plurality of glass body portions in the first glass component relative to one another, • a spatial property profile (510) in each of the glass body portions, and • the effects of the step of pushing together and the step of turning on the spatial property profile in the glass body portions, • calculating the best possible arrangement of the glass body portions (400, 400', 400", 400‴) relative to one another using the model, so that a total difference is minimal, the total difference comprising • the difference between the titanium partition (430) and the titanium distribution (420) and • the second difference between the property partition and property distribution, • positioning the glass body portions (400, 400', 400", 400‴) so that in the step of connecting (1500), the glass body portions (400, 400', 400", 400‴) are connected according to the calculated best possible arrangement.
9. The method according to claim 8, characterized in that the total difference is less than 1.5% based on a sum of a maximum value of the titanium distribution (420) and a maximum value of the property distribution, in particular less than 1.0%, in particular less than 0.5%.
10. The method according to at least one of the preceding claims, characterized in that the step of producing (1100) the glass body comprises at least the following steps: • producing a porous soot body (200), the macroscopic, production-related titanium profile extending substantially along a longitudinal axis and the microscopic, process-related layer structure extending substantially along a growth axis, • vitrifying the soot body in order to produce the cylindrical glass body.
11. The method according to at least one of the preceding claims, characterized in that the first glass component (600) is heated before the step of pushing together (1700).
12. The method according to at least one of the preceding claims, characterized in that the connection (1500) takes place at a particular contact surface (401) of the glass body portions (400, 400', 400", 400‴).