Microgranules for rotary forming, methods for their production and their use
Patent Information
- Application Number
- DE502022002064
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-09-24
- Filing Date
- 2022-09-14
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2042-09-14
AI Technical Summary
Existing methods for producing microgranules from amorphous and semi-crystalline thermoplastics, such as polycarbonate, face interruptions in the extrusion process due to the melting plastic getting stuck in micro-perforated plates, leading to inefficiencies and increased production costs, especially when dealing with high-melting-point materials like polycarbonate.
Increasing the water process temperature to at least 90°C at the micro-hole plate and adding a surface-active surfactant, such as a non-ionic silicone-based surfactant, to the water to prevent agglomeration and clogging, allowing for uninterrupted extrusion and direct use of microgranules in rotational molding.
The method enables continuous and uninterrupted production of microgranules suitable for rotational molding, eliminating the need for further processing steps and reducing production costs, while maintaining high-quality microgranules with low residual moisture and improved flowability.
Description
Field of the invention
[0001] The invention relates to a process for producing microgranules from thermoplastic material for rotational molding. Amorphous, but also semi-crystalline plastics can be used in this process. The microgranules are produced by underwater granulation, as is already known in the art. Such a process comprises the following steps: First, the plastic is melted. Plastic is continuously extruded from the melt. Extrusion occurs through a micro-perforated plate. As the plastic emerges from the micro-perforated plate, it is granulated underwater. The granulated plastic is then dried, for example, by centrifugation. State of the art
[0002] The production of molded articles from plastics by means of rotational molding - also known as rotational casting, rotational melting and Rotomoulding - allows the production of a wide variety of molded articles, especially with large dimensions. Typically, this process involves using plastic ground into a powder, which is placed in a mold. The mold is then placed in an oven and heated there, while continuously rotating around usually two axes. The powder melts and is distributed essentially evenly over the inside of the mold. After the process is complete, cooling takes place, after which the finished molded article can be removed.
[0003] However, the use of powder for rotational molding has several disadvantages. Production takes place in a two-step process. In the first step, granules are produced with grains a few millimeters in length and diameter. In a subsequent second step, these granules are then ground into powder. Depending on the plastic, different processes are used for this second step.
[0004] Polyethylene (PE) is typically ground in powder mills operating at normal ambient temperature and pressure, with the grinding discs operating either vertically or horizontally. Polypropylene (PP), polycarbonate (PC), or polyamide PA 6, on the other hand, are ground using cryogenic or cold powder mills. The plastic is cooled to 50°C to 60°C below zero before it can be processed into a powder by the grinding discs. However, the costs are significantly higher than for grinding PE. Drying the powder plays a key role in engineering plastics, as excessive residual moisture in the powder can contribute to color shifts due to thermo-oxidative degradation of the plastic. This can lead to, among other things, surface defects and reduced mechanical stability under tensile, compressive, or flexural stress.If the residual moisture content is too high, the powder must be pre-dried as a third step before it can be used for rotational molding.
[0005] Since the powder manufacturing process is technically complex, from a commercial perspective, the quantities of material required must be significantly large to reduce production costs. Customized applications, which typically involve small quantities and / or numerous color combinations, are therefore not very cost-effective, resulting in limited flexibility in the procurement process. Providing powder from colored granules requires significant post-milling cleaning effort for the operator of a powder mill to prevent contamination during subsequent orders.
[0006] Many raw material suppliers therefore only grind non-dyed material. The color is then used as a dry color mixture – a so-called Dryblend - This has a detrimental effect on the homogeneous coloring of the finished part, and can also lead to the mechanical instabilities described above.
[0007] In addition, the grinding process is associated with high noise emissions and generates large amounts of dust, which has a detrimental impact on the working environment.
[0008] The direct use of microgranules for rotational molding is therefore desirable. This is also described in the prior art. The production of microgranules suitable for rotational molding from an olefin polymer using underwater granulation is described, for example, in DE 699 10 612 T3.
[0009] WO 2009 / 032745 A2 generally discusses the use of microgranules made from various plastics for rotational molding.
[0010] DE 10 2012 103 976 A1 describes the production of microgranulated polypropylene for rotational molding. The polypropylene is processed into granules using an extruder with a granulating tool, using the underwater granulation process. The openings in the die plate are heated evenly. While the melting point of the polypropylene described in DE 10 2012 103 976 A1 is approximately 160 °C to 170 °C, the temperature of the melt in the extruder is set at 240 °C to 270 °C, whereas the temperature of the die plate is set to a temperature in the range of 290 °C to 320 °C. A range of 38 °C to 45 °C is stated to be advantageous for the process water temperature.
[0011] US 5,726,239 A describes the production of microgranules for rotational molding from monovinyl polymer blends by underwater pelletizing. The process water temperature is between 55 °C and 65 °C. The produced grain sizes are between 200 µm and 1100 µm. US 2005 / 077644 A1 relates to a system and method for pelletizing extruded materials, such as thermoplastic polymers, in various pelletizing applications. A high-pressure liquid jet is used to cut the extruded polymer strand into pellets. The application can also be in underwater pelletizing, but is not limited to this. DE 10 2008 023 046 A1 relates to a plastic pelletizing system with a pelletizing device cooled by the pelletizing water for producing plastic pellets. A bulk material heat exchanger with a heat exchange medium for heating a plastic bulk material is installed upstream of the granulation device.The bulk material heat exchanger is followed by an extruder for extruding the preheated bulk material. The plastics granulation system is designed so that the bulk material heat exchanger is in thermal contact with the granulation water, so that heat is transferred from the granulation water to the bulk material in the bulk material heat exchanger.
[0012] US Pat. No. 7,393,201 B2 describes the production of microgranules from a thermoplastic by strand granulation. EP 3 683 272 A1 describes blends of polyamides and polyolefins suitable for rotational molding.
[0013] However, it has been shown that conventional underwater pelletizing processes fail in the production of microgranules from amorphous, engineering thermoplastics – especially those with high melting temperatures, such as polycarbonate (PC) with a melting point of more than 260 °C – because they repeatedly interrupt the extrusion process: the molten plastic becomes trapped in the openings of the micro-perforated plate, causing the holes to gradually close. This leads to a rapid increase in melt pressure in the extruder upstream of the micro-perforated plate, clogging its holes. As a result, the entire extrusion process for producing the microgranules must be stopped and the perforated plate cleaned. This is inefficient and increases the production costs for the microgranules.Engineering plastics are understood to be plastics that are designed for a continuous use temperature of approximately 90 °C to approximately 150 °C, whereas standard plastics cover the temperature range below this and high-performance plastics cover the temperature range above this. Description of the invention
[0014] The object of the invention is therefore to further develop a method of the type described above for producing microgranules from thermoplastics such that the extrusion process, particularly for amorphous and semi-crystalline, especially engineering thermoplastics, can proceed uninterrupted and without disruption. Furthermore, the produced microgranules should be immediately usable for rotational molding without any further preparatory steps, i.e., the production and preparation of the material actually used for rotational molding should take place in a single step.
[0015] This object is achieved according to the invention by means of a method according to claim 1 in that, firstly, the process temperature of the water in which the granulation of the plastic—a plastic based on polycarbonate (PC), polyamides (PA), polymethyl methacrylate (PMMA), polyethylene terephthalate (PET), cycloolefin polymer (COP), or cycloolefin copolymer (COC)—takes place is at least 90°C, at least in the region of the micro-hole plate, and, secondly, a surfactant is added to the water. "In the region of the micro-hole plate" means that the water is in direct contact with the micro-hole plate at the extruder head.
[0016] Increasing the process water temperature to 90 °C and above requires, on the one hand, stricter safety measures to prevent scalding due to the hot water and the associated generation of hot steam. On the other hand, however, this reduces the temperature drop between the melt in the extruder and the outside of the die plate—even with a heated die plate—to such an extent that the hot water, which is in direct contact with the micro-die plate, prevents the plastic from solidifying in the channels of the micro-die plate and clogging them.
[0017] The process temperature of the water in the area of the micro-hole plate is at least 90 °C, but preferably higher. Depending on the process, the process temperature can preferably be between 92 °C and 98 °C or between 94 °C and 96 °C. A process temperature of at least -95 °C has proven particularly suitable for a wide range of plastics.
[0018] By increasing the process temperature of the water in the area of the micro-perforated plate, the extrusion process can run more smoothly. However, this measure is not sufficient to maintain the process over several days. This is because the higher process temperature of the water also increases the surface temperature of the microgranules. This causes the grains to stick together and form agglomerates.
[0019] In the production of films based on polyolefins, polyamides, or PET, sticking plays a negative role. This problem is solved by adding additional anti-blocking agents—for example, silicon dioxide, chalk, or quartz—to the polymer mixture before or during extrusion, which can reduce or completely prevent sticking of the films.
[0020] However, experiments have shown that agglomeration can be effectively prevented by adding a surfactant to the water. The surfactant should preferably be in aqueous form and be surface-active. A variety of surfactants, particularly non-ionic surfactants, can be used. In experiments, for example, a non-ionic silicone-based surfactant has proven to be effective in preventing agglomeration. Another advantage of silicone-based surfactants is their resistance to high temperatures. The surfactant reduces the surface tension of the water, allowing it to better wet the surface of the granules. This prevents agglomeration.
[0021] The absolute dosage of surfactant added depends on the capacity of the underwater granulation system. The volume fraction of surfactant in the mixture of water and surfactant is preferably between 0.05% and 2%. However, lower volume fractions are generally sufficient; the volume fraction is therefore preferably between 0.1% and 0.5%. A volume fraction of 0.2% has proven particularly preferred in terms of effectiveness and the amount of surfactant. The volume fraction specified refers to an operating time of the underwater granulation system of 24 hours, i.e. surfactant must be added at regular intervals to keep the volume fraction essentially constant.
[0022] The process described above can be applied not only to polycarbonate (PC) and polyamides (PA), but also to other plastics with a narrow melting point range, such as polymethyl methacrylate (PMMA), polyethylene terephthalate (PET), cycloolefin polymer (COP), or cycloolefin copolymer (COC), provided the process temperature of the cooling water does not fall below 90 °C, preferably not below 95 °C, and the addition of a surface-active, aqueous surfactant with a volume fraction of, for example, 0.2% over a 24-hour operating time is ensured. Suitable polyamides include PA6, PA 6.6, PA 11, or PA 12, to name just a few.In particular, the microgranulation of COP and COC is not trivial, since although they are chemically polyolefins, their cyclic structure creates an amorphous structure - corresponding to a high transparency - which can be used for special purposes, for example as a glass replacement in optical applications.
[0023] Microgranules produced in this way from one of the aforementioned plastics preferably have a particle size of at least 300 µm in at least one spatial dimension. The particle size is preferably between 500 µm and 700 µm. The microgranules have a residual moisture content of no more than 0.5% water, measured according to DIN 53723, and a bulk density of at least 0.45 g / cm³, measured according to ISO / R 60. Furthermore, the flowability (also referred to as dry flow rate, "flowability," "dry flow rate," or simply "dry flow") is a maximum of 13 seconds. Flowability is measured according to the adapted specifications of the ARMO Association ("Association of Rotational Moulders") based on the ASTM D1895-96 and ISO / R 60 standards.
[0024] The microgranulate according to claim 4 produced by the method described above is particularly suitable for the production of products by rotational molding. The products produced thereby have, in particular, a uniform surface structure and, if colored granulate is used, a uniform color. The microgranulate is used immediately after its production, i.e., without further processing or intermediate steps, by filling a rotational mold with it. The product—the molded body—is then rotationally molded in the usual manner, as is known in the art.
[0025] The invention is explained in more detail below using exemplary embodiments. These exemplary embodiments are merely illustrative; for example, a description of an embodiment with a plurality of elements or components should not be interpreted to mean that all of these elements or components are necessary for implementation. Rather, other embodiments may also include alternative elements and components, fewer elements or components, or additional elements or components. Elements or components of different embodiments may be combined with one another unless otherwise stated. Modifications and variations described for one of the exemplary embodiments may also be applicable to other embodiments.
[0026] In a first embodiment, commercially available polyamide PA 6 with a relative viscosity of 2.7 was extruded through a twin-screw extruder. The melt was forced through a micro-perforated plate using a melt pump. The holes had individual diameters between 0.3 mm and a maximum of 0.7 mm. Granulation was carried out by underwater cutting using a commercially available underwater granulation system. The process temperature of the water was at least 90 °C, preferably 95 °C. The water contained a volume fraction of 0.2% of an aqueous, silicone-based surface-active surfactant. The microgranules were then removed from the granulation water circuit, separated from the remaining water, dried in situ, and optionally packaged airtight in aluminum bags.
[0027] In a second example, a commercially available polycarbonate (PC) with a maximum MVR ("melt volume-flow rate") of 40 g / 10 min was extruded through a twin-screw extruder under test conditions with a test temperature of 300 °C and a test load of 1.2 kg. The melt was forced through a micro-perforated plate using a melt pump. The holes had individual diameters between 0.3 mm and a maximum of 0.7 mm. Granulation was carried out by underwater cutting using a commercially available underwater granulation system. The process water temperature was at least 90 °C, preferably 95 °C. The water contained a volume fraction of 0.2% of an aqueous, silicone-based surface-active surfactant. The microgranules were then removed from the water granulation circuit, separated from the remaining water, dried in situ, and optionally packaged airtight in aluminum bags.
[0028] The microgranulate produced in this way can then be used immediately for rotational molding without interruption and without further disruptive processing steps, i.e., directly and without further processing steps. It does not need to be processed into powder like other granulates. PC or PA 6, in particular, previously had to be ground (cold) into powder in order to be used for rotational molding. This step, and any additional step for necessary pre-drying, can be completely omitted. Therefore, only a single step is necessary to prepare the material actually used for rotational molding, namely the microgranulate itself: the production of the microgranulate.
[0029] The microgranulate made of PA 6 or PC is then used to produce molded bodies by rotational molding. A rotational mold is filled with the microgranulate. The molded body is then produced in this mold by heating and rotating the mold in a manner known in the art. Rotational molding can be carried out on gas-fired systems. However, due to the high demands on precision when maintaining process parameters, particularly process temperatures, electrically heated tools are advantageous. In an inert gas atmosphere and vacuum inside the tool, higher temperatures are necessary to avoid or at least reduce thermo-oxidative degradation of the materials due to residual moisture and oxygen. Additional pre-drying of the microgranulate is therefore no longer necessary compared to using powder for rotational molding.
[0030] The process described above can be used to process amorphous, engineering plastics such as polycarbonate, as well as semi-crystalline plastics such as PET, PBT, PA6, and standard plastics such as PMMA, into microgranules suitable for rotational molding. Unlike powder, the microgranules can be efficiently prepared as a raw material for rotational molding in a single step without interruption.
Claims
1. A method for manufacturing microgranules of thermoplastic based on polycarbonate (PC), polyamides (PA), polymethyl methacrylate (PMMA), polyethylene terephthalate (PET), cycloolefin polymer (COP) or cycloolefin copolymer (COC) for rotational molding, comprising the following steps: - melting of the plastic, - continuous extrusion of the plastic through a micro-perforated plate, - pelletizing of the extruded plastic under water as the plastic emerges from the micro-perforated plate, - drying of the pelletized plastic by centrifugation, characterized in that - the process temperature of the water in which the plastic is pelletized is at least 90 °C, at least in the area of the micro-perforated plate, and - a surfactant is added to the water to prevent agglomeration of grains of the microgranules.
2. The method according to claim 1, characterized in that a silicone-based surfactant is used as the surfactant.
3. The method according to claim 1 or 2, characterized in that the volume percentage of surfactant in the mixture of water and surfactant is between 0.05 % and 2 %, preferably between 0.1 % and 0.5 %, particularly preferably 0.2 %.
4. Microgranules for rotational moulding, manufactured by a method according to any one of claims 1 to 3, characterized by a particle size of at least 300 µm, a residual moisture content by mass of not more than 0.5% water, measured according to DIN 53723, a flowability of at most 13 seconds, measured according to the adapted regulations of the ARMO association based on the ASTM D1895-96 and ISO / R 60 standards, and a bulk density of at least 0.45 g / cm3, measured according to ISO / R 60.
5. Use of microgranules according to claim 4 for the manufacture of products by means of rotational molding, comprising filling a rotational mold with the microgranules and then rotationally molding the product.