METHOD FOR PRODUCE A MICRO-ELECTRO-MECHANICAL SYSTEM FROM A DEPOSITATED PIEZOELECTRIC OR FERROELECTRIC LAYER
Patent Information
- Application Number
- DE602020041138
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-05
- Filing Date
- 2020-02-25
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2040-02-25
AI Technical Summary
Current methods for producing micro-electro-mechanical components with piezoelectric layers face challenges such as degradation of lower electrodes, complexity in achieving specific crystalline orientations, and difficulties in scaling up due to high-temperature processing and chemical reactivity, which limit the efficiency and compactness of filters and resonators.
A method involving epitaxial growth of piezoelectric layers, followed by thermal annealing and chemical etching to detach temporary substrates, allowing for the production of micro-electro-mechanical systems with piezoelectric materials like LiNbO3 or LiTaO3 without degrading lower electrodes, and enabling flexible crystalline orientations and scalable production.
This approach enables the production of high-quality micro-electro-mechanical components with improved piezoelectric coupling coefficients, enhanced manufacturing efficiency, and compactness, suitable for high-frequency applications without the limitations of existing techniques.
Description
Domaine technique de l'invention
[0001] The field of the invention is that of micro-electro-mechanical systems (MEMS, for Micro-Electro-Mechanical Systems) piezoelectrics used as information processing elements (resonators, filters, etc.), as sensors (physical sensors of temperature, pressure, acceleration, magnetic field, chemical species, etc.) or as actuators (micro-pumps for micro-fluidic systems, deformable micro-mirrors, etc.). Etat de l'art
[0002] Electromechanical components form a separate class of components used in various systems. These elements allow, for example, the generation of mechanical movements under the action of an electrical signal: we then speak of actuators. The most widespread examples of these components are inkjet printer print heads, fuel injectors used in automobiles, or micro- or nano-positioning systems used in precision mechanics or for scientific equipment. Conversely, other systems use the sensitivity of mechanical elements to different stimuli to provide electrical information to quantify them. We then speak of sensors. The most widespread examples in this case are accelerometer systems, gyrometers, pressure sensors (microphones), or others.Finally, a last category uses both effects simultaneously: a mechanical structure is made to vibrate under the influence of a periodic electrical signal; if the vibration of this mechanical structure is sufficiently stable, the transcription of this vibration into the electrical domain makes it possible to create a stable oscillating system. This is called a resonator. The most common examples of these components are quartz resonators used in watchmaking or oscillators used for the time synchronization of electrical circuits.
[0003] All these electromechanical systems rely on the transduction capacity of the structure, that is to say the capacity to transform a signal from one domain (electrical, mechanical, etc.) into another (electrical, mechanical, etc.). Several techniques are known, but one of the most common is the use of piezoelectric materials. Piezoelectricity, discovered in 1880 by the Curie brothers (P. Curie, Notice sur les travaux scientifiques de MP Curie, Gauthier-Villars (1902)) is the capacity of a crystal to polarize under the action of a mechanical constraint, or conversely to deform under the action of an electrical voltage. Piezoelectric materials therefore make it possible to ensure electromechanical, or mechano-electrical, transduction.
[0004] Early work on piezoelectric components used natural crystals, such as quartz or Rochelle salt. These materials immediately found applications in the manufacture of resonators and in early sonar systems. For the latter application, however, the piezoelectric properties of these materials proved too weak to allow the generation of high pressures in water, or conversely the detection of low acoustic pressures. Research therefore focused on the synthesis of artificial materials, the most widely used of which is still lead zirconate titanate (PbZr x Ti 1-x O 3 , or PZT) and its derivatives.The strong piezoelectricity of this material has enabled the development of sonar systems used for maritime transport or defense, ultrasound probes used for medical diagnosis, fuel injectors used in automobiles, or even sensitive elements for non-destructive testing systems. Despite its excellent piezoelectric properties, this material has some major drawbacks: being a lead-based compound, its synthesis, recycling and disposal in nature pose environmental toxicity problems. As a result, standards such as RoHS (. Restriction of the use of Hazardous Substances in electronic equipment ) and the European WEEE directive ( Waste Electrical and Electronic Equipment ) tend to prohibit its use in the long term. In addition, although this material has strong piezoelectric properties at low frequencies, its electrical and / or mechanical losses are prohibitive for high frequency applications. Finally, this material loses its piezoelectric properties at high temperatures. Research has therefore turned to alternative materials, such as lithium niobate or tantalate (LiNbO 3 , LiTaO 3 ), potassium niobate (KNbO 3 ) and its derivatives such as KNa 1-x Nb x O 3 , barium titanate (BaTiO 3 ) and its derivatives such as (Ba 1-x Ca x )(Ti 1-y Zr y )O 3 , bismuth and sodium titanates (Na 0.5 Bi 0.5 TiO 3 ) or other exotic materials such as langasite, langatate or their derivatives (La 3 Ga 5 SiO 14 , La 3 Ga 5.5 Ta 0.5 O 14 , ...).
[0005] In the 1980s, the emergence of micro-electro-mechanical components (MEMS) paved the way for the miniaturization of sensors, actuators, and resonators, which benefited the development of mobile telephony and automotive sensors. The production of piezoelectric MEMS was made possible by the development of piezoelectric thin films. These films are characterized by a thickness of the order of a micrometer or less. Currently, only a few materials, often polycrystalline, are available in the form of thin films: zinc oxide (ZnO), aluminum nitride (AIN), or again PZT. Currently, these last two materials are used successfully in industry.
[0006] Aluminum nitride layers are currently mainly used for the production of bulk acoustic wave filters. These filters are circuits using several bulk acoustic wave resonators, which rely on resonance on a thickness mode of the piezoelectric layer, generally made of AIN. For a long time, this material has indeed had piezoelectric coefficients relatively in line with what was required for mobile telephony applications.Indeed, there is a proportional relationship between the electromechanical coupling coefficient of a wave propagating in a piezoelectric material (this coupling coefficient being defined as the ratio between the quantity of energy converted from the electrical domain to the mechanical domain, or vice versa, and the quantity of energy stored in electrical and mechanical form in the structure) and the relative bandwidth that can be synthesized from a filter circuit. With the maturation of elastic wave filter technology, and the emergence of new telecommunications standards (for example, the 5th generation of mobile telephony, also called 5G), we are witnessing the opening of new frequency bands at high frequencies (above 3 GHz), the opening of relatively wide bands, or the reduction of the spacing between frequency bands used.In addition, research is currently active in the development of frequency-agile resonators or filter circuits. All of these cases require resonators with higher electromechanical coupling coefficients than aluminum nitride can provide.
[0007] In recent years, we have therefore seen the development of alloys derived from AlN, incorporating for example Scandium or Chromium (AIScN or AlCrN). Modifying the composition of the piezoelectric material allows substantial gains in piezoelectric coupling coefficients (from approximately 6% to more than 10%), without major changes in the production processes. However, the needs are such that these improvements are not entirely sufficient. It has therefore been proposed to base bulk acoustic wave resonators on materials such as lithium niobate or lithium tantalate. Lithium niobate theoretically makes it possible to excite shear waves that can have electromechanical coupling coefficients of up to 45%. This is, however, only true for certain very specific crystal orientations.
[0008] In practice, the most advanced work on this material is that of Kadota et al. (M. Kadota, Y. Suzuki et Y. Ito, IEEE International Ultrasonics Symposium 2010 ou M. Kadota, T. Ogami, K. Yamamoto, H. Tochishita, Y. Negoro, IEEE Transactions on Ultrasonics, Ferroelectrics and Frequency Control vol 57, n°11, p. 2564 (2010 )),who have produced Lamb wave and bulk wave resonators from a stack of substrate / sacrificial layer / electrode / epitaxial lithium niobate film / electrode. These lithium niobate layers have a so-called c-axis orientation, corresponding to the crystalline axis (000.6) or the Z direction according to the ANSI / IEEE 176-1987 standard. This orientation only has electromechanical coupling coefficients almost identical to those of aluminum nitride, which is of relatively little interest given the difficulty of depositing this material. Indeed, the growth of this material requires high temperatures (of the order of 500 to 700°C) and relatively long times (of the order of a few hours), during which the risks of lithium diffusion into the other layers present are high, making it difficult to control the chemical composition and interfaces.
[0009] To overcome these problems, several projects have been based on monocrystalline thin film transfer techniques. In this case, thin layers are taken from a solid monocrystalline substrate to be incorporated into the stack of acoustic components. Three techniques exist: bonding / thinning: the principle consists of bonding a piezoelectric substrate to the host substrate, then thinning the piezoelectric material by mechanical lapping, followed by polishing. In some cases, etching steps can also be used to consume the material more quickly; bonding / fracturing: the principle consists of implanting light ions at a given depth in the piezoelectric substrate, and at a relatively high dose. This substrate is then bonded to the host substrate. A heat treatment then weakens the interface where the implanted ions are trapped, which causes the material to fracture.What remains is a thin piezoelectric layer bonded to the host substrate on one side, and the thinned donor piezoelectric substrate on the other; bonding / dissolution: this variant of the previous method consists of using the fact that the piezoelectric material is damaged by the localized presence at a certain depth of a large quantity of implanted ions. It is therefore much more easily etched at this location by chemical dissolution than the surrounding regions. This effect can then be used to detach the thin layer bonded to the host substrate from the rest of the piezoelectric substrate.
[0010] These three techniques have the advantage of providing monocrystalline piezoelectric layers of excellent quality and, what is more, of virtually any crystalline orientation (provided that monocrystalline substrates with this orientation are available). They are therefore very versatile. However, requiring bonding steps and heavy treatments to detach the layer that one wishes to preserve, their installation is relatively delicate. This requires in particular consolidation annealing of the bonding interface, if necessary fracture and finally healing of damage to the material coming from fracturing, implantation, or even mechanical abrasion of the crystal. This can pose compatibility problems with structures present on the host substrate, which risk degradation due to the thermal budget applied during the healing annealing.Another problem can also come from the differences in expansion coefficients between the donor substrate (piezoelectric) and the receiving substrate (ideally silicon), which, when attempting to apply the bonding / fracturing process, can cause plate breakage during fracturing annealing, when the two thick substrates undergo a strong thermal expansion differential. Finally, a final limitation of these techniques lies in the difficulty of considering transposition to large substrates (diameters of 200 or 300 mm): in fact, monocrystalline piezoelectric substrates are currently available at best in diameters of 150 mm, and the problems of expansion differentials become more significant as the lateral dimensions of the substrates increase.
[0011] Using piezoelectric material deposition steps would therefore be simpler. However, obtaining a crystalline orientation other than the natural growth orientation requires epitaxial growth on ad hoc surfaces, generally atomic surface arrangements compatible with the crystalline planes of the piezoelectric material to be grown. The substrates must therefore be subjected to specific chemical and thermal treatments revealing atomic steps. These conditions are extremely restrictive and generally require the presence of layers that are themselves monocrystalline or epitaxial and have extremely controlled surface states.This is typically not the case for stacks obtained after a succession of manufacturing steps, and is especially not the case for metal electrodes on which it is generally desired to deposit the piezoelectric material, a fortiori when these electrodes have a given geometry and do not extend over the entire surface of the substrate. In addition, growth over significant thicknesses (several hundred nm to a few µm depending on the materials) leads to a relaxation of the constraints due to the crystal lattice mismatch between the substrate and the epitaxial layer, which leads to the formation of dislocations that can harm the integrity of the film if they are too numerous. For this reason, epitaxial films are generally limited in thickness.Furthermore, as mentioned, these structures have a high probability of being degraded due to the thermal budget required for deposition, and the chemical reactivity of the species present.
[0012] Document EP2464006 discloses a method in which an implantation step is provided so as to define a layer of material of interest which can be dissociated from the substrate from which it originates. The document Reinhardt Alexandre et al: “Acoustic filters based on thin single crystal LiNbO3 films: Status and prospects” 2014 IEEE International Ultrasonics Symposium, IEEE, September 3, 2014, pages 773-781, XP033266727, DOI: 10.1109 / ULTSYM.2014.0191, discloses an implantation step for defining a thin layer. Document US2013 / 0249648 describes a step of ionic implantation of atoms in order to create a defect zone at the desired depth. WO2011 / 042388 describes performing an ion implantation operation to create a buried fragile zone to define the piezoelectric thin layer. WO2019 / 129979 describes a fractured zone.Documents EP3591724 and WO2020006578 disclose a method of manufacturing a micro-electro-mechanical system.
[0013] US patent application 2017 0077386 A1 describes a technique for circumventing this problem: the material is epitaxially grown on a growth substrate, possibly including sub-layers to accommodate the epitaxial relationships between the substrate and the piezoelectric layer. The upper part of the resonator stack is then formed. Openings are then etched locally through the substrate, which releases the resonator and mechanically decouples it from the substrate. At the bottom of these openings, the lower electrodes are then deposited and structured. However, this technique has several drawbacks: the substrates are greatly weakened by the etching of the openings, which limits the density of patterns that can be produced. This therefore affects the compactness of the filters and / or the manufacturing yield; some growth substrates, for example sapphire, are notoriously difficult to etch over large thicknesses due to their chemical inertness and hardness. As a result, the etching step is expensive, even assuming that it is possible over great depths; the definition of the electrode patterns below the bottom of the cavities (several hundred µm deep) is delicate, since the photolithography equipment will have to be used outside its depth of field. The patterns cannot therefore be precisely defined.
[0014] This is why, in this context, the Applicant proposes in the present invention a method for producing micro-electro-mechanical components using a piezoelectric thin layer and particularly well suited in the case of an epitaxially grown piezoelectric thin layer sandwiched between two electrodes, making it possible not to degrade the lower electrode where appropriate, nor to suffer the defects of the techniques presented in the state of the art above.
[0015] More specifically, the present invention relates to a method for manufacturing a micro-electro-mechanical system according to independent method claim 1.
[0016] According to variants of the invention, the deposition of said piezoelectric material or said ferroelectric material is carried out by epitaxial growth.
[0017] According to variants of the invention, the micro-electro-mechanical system comprises at least one bulk elastic wave resonator or at least one surface elastic wave resonator or at least one Lamb wave resonator.
[0018] According to variants of the invention, the bonding comprises a thermal annealing step.
[0019] According to variants of the invention, the operation of removing the temporary substrate comprises: a step of thinning said temporary substrate; an operation of chemical etching said thinned temporary substrate.
[0020] According to variants of the invention, the operation of removing said temporary substrate comprises: a step of diffusion of elements causing precipitation or chemical reactions at the level of the material constituting said temporary substrate or a step of implantation of ions in said temporary substrate.
[0021] According to variants of the invention, the method comprises the deposition of a buffer layer on the surface of said temporary substrate, prior to the deposition of said piezoelectric material or said ferroelectric material.
[0022] According to variants of the invention, the method comprises the production of structured layers of metal which may be Molybdenum inserted into a dielectric which may be SiO 2 .
[0023] According to variants of the invention, the method comprises, prior to said bonding of said two assemblies: the production of electrodes on the surface of said layer of piezoelectric material or ferroelectric material; the production of an acoustic insulation structure in said second assembly.
[0024] According to variants of the invention, the piezoelectric material is LiNbO 3 or LiTaO 3 , or their solid solutions or KNbO 3 or AIN, GaN.
[0025] According to variants of the invention, the ferroelectric material is: LiNbO 3 or LiTaO 3 or PZT
[0026] According to variants, the temporary substrate is made of non-silicon material, such as for example materials of MgO, SrTiO 3 , LaAlO 3 , LSAT ((LaAlO 3 ) 0.3 (Sr 2 TaAlO 6 ) 0.7 ), DyScO 3 , Sapphire (Al 2 O 3 ) or lithium niobate (LiNbO 3 ), lithium tantalate, the piezoelectric material being able to advantageously be PZT.
[0027] According to variants of the invention, the bonding layers are made of oxide or polymer.
[0028] The invention also relates to a micro-electro-mechanical system obtained by the method of the invention.
[0029] The invention will be better understood and other advantages will appear on reading the description which follows, given without limitation and thanks to the appended figures among which: [ Fig.1a ] illustrates the first step of a first example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a released sacrificial structure; [ Fig.1b ] illustrates the second step of a first example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a released sacrificial structure; [ Fig.1c ] illustrates the third step of a first example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a released sacrificial structure; [ Fig.1d ] illustrates the fourth step of a first example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a released sacrificial structure; [ Fig.1e ] illustrates the fifth step of a first example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a released sacrificial structure; [ Fig.1f ] illustrates the sixth step of a first example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a released sacrificial structure; [ Fig.1g ] illustrates the seventh step of a first example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a released sacrificial structure; [ Fig.1h ] illustrates the eighth step of a first example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a released sacrificial structure; [ Fig.1i ] illustrates the ninth step of a first example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a released sacrificial structure; [ Fig.1j ] illustrates the tenth step of a first example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a released sacrificial structure; [ Fig.1k ] illustrates the eleventh step of a first example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a released sacrificial structure; [ Fig.1l ] illustrates the twelfth step of a first example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a released sacrificial structure; [ Fig.1m ] illustrates the thirteenth step of a first example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a released sacrificial structure; [ Fig.1n ] illustrates the fourteenth step of a first example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a released sacrificial structure; [ Fig.1o ] illustrates the fifteenth step of a first example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a released sacrificial structure; [ Fig.2a ] illustrates the first step of a second example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a Bragg mirror structure; [ Fig.2b ] illustrates the second step of a second example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a Bragg mirror structure; [ Fig.2c ] illustrates the third step of a second example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a Bragg mirror structure; [ Fig.2d ] illustrates the fourth step of a second example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a Bragg mirror structure; [ Fig.2e ] illustrates the fifth step of a second example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a Bragg mirror structure; [ Fig.2f ] illustrates the sixth step of a second example of a method for producing a system comprising a bulk wave resonator according to the invention comprising a Bragg mirror structure; [ Fig.3a ] illustrates the first step of an example of a method for producing a system comprising a plate wave resonator according to the invention; [ Fig.3b ] illustrates the second step of an example of a method for producing a system comprising a plate wave resonator according to the invention; [ Fig.3c ] illustrates the third step of an example of a method for producing a system comprising a plate wave resonator according to the invention; [ Fig.3d ] illustrates the fourth step of an example of a method for producing a system comprising a plate wave resonator according to the invention; [ Fig.3e ] illustrates the fifth step of an exemplary method of producing a system comprising a plate wave resonator according to the invention; [ Fig.4a ] illustrates the first step of an example of a method for producing a transformer comprising two Lamb wave resonators according to the invention; [ Fig.4b ] illustrates the second step of an example of a method for producing a transformer comprising two Lamb wave resonators according to the invention; [ Fig.4c ] illustrates the third step of an example of a method for producing a transformer comprising two Lamb wave resonators according to the invention; [ Fig.4d ] illustrates the fourth step of an example of a method for producing a transformer comprising two Lamb wave resonators according to the invention; [ Fig.4e ] illustrates the fifth step of an example of a method for producing a transformer comprising two Lamb wave resonators according to the invention; [ Fig.4f ] illustrates the sixth step of an example of a method for producing a transformer comprising two Lamb wave resonators according to the invention; [ Fig.4g ] illustrates the seventh step of an example of a method for producing a transformer comprising two Lamb wave resonators according to the invention; [ Fig.4h ] illustrates the eighth step of an example of a method for producing a transformer comprising two Lamb wave resonators according to the invention; [ Fig.4i ] illustrates the ninth step of an example of a method for producing a transformer comprising two Lamb wave resonators according to the invention; [ Fig.4j ] illustrates the tenth step of an example of a method for producing a transformer comprising two Lamb wave resonators according to the invention; [ Fig.4k ] illustrates the eleventh step of an example of a method for producing a transformer comprising two Lamb wave resonators according to the invention; [ Fig.4l ] illustrates the twelfth step of an example of a method for producing a transformer comprising two Lamb wave resonators according to the invention; [ Fig.4m ] illustrates the thirteenth step of an example of a method for producing a transformer comprising two Lamb wave resonators according to the invention; [ Fig.4n ] illustrates the fourteenth step of an example of a method for producing a transformer comprising two Lamb wave resonators according to the invention.
[0030] The method of the present invention thus comprises the following main steps, broken down according to certain variants and certain options: the preparation of a temporary substrate that can correspond to a suitable growth substrate. This may require surface treatments of the substrate and / or the deposition of layers to adapt the epitaxial relationships between the layer to be deposited and the growth substrate; the deposition of the piezoelectric or ferroelectric layer using a suitable technique to achieve the growth of a monocrystalline material, or failing that, a textured one; the production of the lower part of the component over the deposited layer, or on another substrate (the future host substrate). This lower part may include electrodes or other elements, or a minima an acoustic insulation structure of the acoustic wave resonator which will be formed: release box which will allow the insertion of a Bragg mirror; the bonding of the growth substrate comprising the epitaxial layer where appropriate and part of the structures of the lower part of the component on the host substrate possibly having the complement of this lower part (which may be a sacrificed layer structure, at least one electrode, etc.); the detachment of the temporary substrate which may be a growth substrate, by means known to those skilled in the art (chemical or physical etching of the substrate or of one of the layers incorporated in the growth substrate); the finalization of the manufacture of the component by producing the upper part of the component.
[0031] The Applicant describes below several examples of processes, the steps of which are illustrated by figures in which the same references are used and which correspond respectively to the following elements: 100 : a temporary substrate 200 : a buffer layer 300 : a layer of piezoelectric material or ferroelectric material 400 : at least one lower electrode 500a, 500b, 500c -> 500 : dielectric material, particularly intended for bonding 600 : a sacrificial layer structure MR : a Bragg mirror structure 700 : a host substrate 800 : at least one upper electrode 900 : an upper dielectric layer 1000 : contact pads
[0032] The following examples are described in the context of piezoelectric materials, but can just as easily be applied in the context of ferroelectric materials.
[0033] Example of a manufacturing process for a bulk wave resonator comprising a released sacrificial structure: Etape 1.1 : The preparation of a silicon substrate corresponding to the temporary substrate is carried out 100 by high temperature annealing (> 1000°C) to obtain a smooth surface at the atomic level, as illustrated in figure 1a . Etape 1.2 : A buffer layer is deposited 200, for example of ZnO by molecular beam epitaxy (MBE, for Molecular Beam Epitaxy ), with a thickness of 20 nm for example, as illustrated in figure 1b . Etape 1.3 : We proceed to the deposition of a layer of LiNbO 3 for example by PI-MOCVD ( Pulsed Injection Metal-Organic Chemical Vapor Déposition ), for example 250 nm thick. The crystal lattice agreement between Si / ZnO / LiNbO 3 leads, for example, to the growth of a lithium niobate layer along the c axis 300, as illustrated in figure 1c . Etape 1.4 : A lower electrode is deposited 400,for example in 100 nm thick molybdenum, by sputtering, then structuring by photolithography, reactive ion etching and resin removal, as illustrated in figure 1d . Etape 1.5 : A protective layer of SiO 2 dielectric is deposited 500a for example in PECVD ( Plasma Enhanced Chemical Vapor Deposition ), for example 100 nm thick, then the deposition of a sacrificial layer of amorphous silicon, for example 1 µm, by sputtering. This is structured by photolithography, reactive ion etching and resin removal, to obtain a sacrificial layer structure 600 as illustrated in figure 1e . Etape 1.6 : We proceed to the deposition of SiO 2 dielectric 500b for example, 2 µm thick for example, by reactive sputtering of Si by an Ar / O 2 plasma and chemical-mechanical polishing (CMP, for Chemical Mechanical Polishing ), as illustrated in figure 1f . Etape 1.7 : In addition, a substrate is prepared covered with a layer 500c by thermal oxidation of a host silicon substrate 700, for example on a thickness of 500 nm, as illustrated in figure 1g . Etape 1.8 : We then proceed to the activation of the surfaces and direct bonding between host substrate 700 and temporary substrate 100 corresponding to a growth substrate then to an annealing operation to consolidate the bonding via the dielectric 500 as illustrated in figure 1h . Etape 1.9 : An operation is carried out to detach the temporary growth substrate 100. Thinning is carried out by mechanical lapping to leave only about ten microns of thickness, then chemical etching of the temporary growth substrate in a TMAH solution ( Tetramethylammonium Hidroxide ) and chemical etching of the buffer layer 200 of ZnO for example by HCl, as illustrated in figure 1i . Etape 1.10 : The etching intended for electrical contacts towards the lower electrode is carried out by photolithography, ion beam etching (IBE, for Ion Beam Etching ) of the piezoelectric layer 300, and resin removal, as shown in figure 1j . Etape 1.11 : We proceed to the deposition and structuring of an upper electrode 800 (still in Mo, for example 100 nm thick), as illustrated in figure 1k . Etape 1.12 : The upper electrode is then encapsulated with a layer of SiO 2 900 deposited for example by PECVD, for example again 100 nm thick. Then electrical contacts are opened in the film by photolithography, reactive ion etching and resin removal, as illustrated in figure 1l . Etape 1.13 : We proceed to the deposit of electrical contacts 1000,for example in aluminum by sputtering, on a thickness of 1µm, photolithography, chemical etching and resin removal as illustrated in figure 1m . Etape 1.14 : Release openings are etched by ion beam etching of a SiO 2 / LiNbO 3 / SiO 2 stack as shown in figure 1n . Etape 1.15 : The resonator (layer of piezoelectric material between electrodes) is released by etching the sacrificial layer structure in amorphous silicon. 600 by gaseous XeF 2 as illustrated in figure 1o . Etape 1.16 : Finally, an electrical voltage is applied to the terminals of the component and it is heated in order to orient the ferroelectric domains in the lithium niobate layer in a preferential direction. Example of a process for producing a bulk acoustic wave resonator in epitaxial lithium niobate, on a Bragg mirror
[0034] A variant of the previous production method consists of replacing the acoustic confinement provided by the air cavity located under the resonator with an acoustic confinement provided by a Bragg mirror consisting of a stack of layers alternately with low and high acoustic impedances. Among the materials with a high acoustic impedance, layers of tungsten (W), molybdenum (Mo), silicon nitride (SiN) or aluminum nitride (AIN) are usually considered. For materials with a low acoustic impedance, the literature mainly mentions the use of silicon oxide (SiO 2 ), but also cites silicon oxycarbide (SiOC). These lists are not exhaustive.
[0035] A process suitable for the production of SMR resonators (for Solidly Mounted Resonator ), the name given to bulk wave resonators on Bragg mirrors, is described below: Step 2.1: Steps 1.1 to 1.4 of the first method are carried out until the lower electrodes are produced as described in Figure 2a , so as to define on a temporary substrate 100, a buffer layer 200, a layer of piezoelectric material 300 and a lower electrode 400. Step 2.2 . : A protective layer of SiO 2 is deposited 500a for example in PECVD ( Plasma Enhanced Chemical Vapor Deposition ), for example 600 nm thick and planarization of the topography provided by the lower electrode. The remaining SiO 2 layer will act as the upper layer of the Bragg mirror, as illustrated in Figure 2b . Step 2.3 : We proceed to the deposition of the following layers constituting the Bragg mirror MR, here for example a SiO 2 / Mo (250 nm) / SiO 2 (250 nm) / Mo (400 nm) mirror. Then we proceed to photolithography and reactive ion etching operations of the Mo / SiO 2 / Mo trilayer as illustrated in Figure 2c . Step 2.4 : A 2 µm layer of SiO 2 is deposited 500b, for example by PECVD, and planarization of the topography provided by the Bragg mirror MR as illustrated in figure 2d . Step 2.5 : We proceed to the activation of the surfaces and direct bonding between host substrate (an oxidized silicon substrate) 700 + 500c and temporary growth substrate 100 with Bragg mirror MR . A consolidation annealing operation is carried out on the bonding as illustrated in figure 2e . Step 2.6 : The temporary growth substrate is detached 100, as in the previous embodiment, then the steps are continued in a similar manner to those of the production method until the electrical contacts are finalized. Due to the presence of a Bragg mirror MR as a replacement for the sacrificial layer boxes, the release step is no longer necessary, as illustrated in Figure 2f . Example of a process for producing a Lamb wave resonator in epitaxial lithium niobate
[0036] The methods described above do not only apply to bulk acoustic wave resonators, but can also be used for the production of plate acoustic wave resonators, also known as Lamb wave resonators. These resonators are distinguished by the excitation of acoustic waves not by two solid electrodes sandwiching the piezoelectric layer, but by two electrodes in the form of interdigitated combs positioned on one of the faces (lower or upper) of the piezoelectric layer. The other face may be in contact with an electrode covering the surface of the component (in order to excite plate waves from the vertical electric field thus formed), or on the contrary not have an electrode, in order to excite waves from the horizontal electric field formed between the electrodes of the interdigitated comb.More generally, this process can be applied to a whole family of acoustic micro-resonators benefiting from an epitaxial piezoelectric layer.
[0037] Furthermore, variant embodiments can be introduced into the preceding methods. In particular, other techniques for detaching the growth substrate are conceivable.
[0038] Indeed, step 1.9) of the first process example is based on chemical etching of the growth substrate. In the case where the latter is not made of silicon and is therefore difficult to dissolve chemically, or to save time, it may be advantageous to carry out mechanical thinning ( grindingin English) using chemical-mechanical lapping and polishing techniques. One drawback remains: the process results in consumption of the growth substrate, and therefore its loss, which results in a significant cost. To circumvent this problem, it may be interesting to cause a mechanical fracture of the growth substrate, which can then be reused through reconditioning steps. This fracture can be achieved in different ways. These include: the generation of a fragile interface during the growth of the piezoelectric layer. This can occur mainly when there is diffusion of an element causing precipitation or chemical reactions leading to an increase in volume of one of the encapsulated materials present, and therefore spontaneous detachments during mechanical stress; another technique consists of forming a fragile interface after the growth of the piezoelectric layer. This interface can be formed by implantation of ions in the growth substrate, then thermal annealing to cause fracture of the material, using a process similar to the Smart Cut ™ process. This is possible when the epitaxial layer and all the sub-layers accommodating the lattice parameters have a relatively small thickness, so that they can be crossed by the flow of ions during implantation.
[0039] Thus, a production method variant intended for example to produce a plate acoustic wave resonator is described below: Step 3.1 : Epitaxial growth of a layer of lithium niobate on silicon is carried out 300, including a buffer layer 200 allowing the accommodation of the lattice parameter between the lithium niobate and the temporary silicon substrate 100 (identical to steps 1.1 to 1.3 described in the first process example) as illustrated in Figure 3a . Step 3.2. : Helium and Hydrogen ions are implanted through the epitaxial layer, so as to form a fragile interface I inside the silicon substrate as illustrated in Figure 3b . Step 3.3 : At this stage of the process, we can proceed with the possible formation of the electrodes and that of a passivation layer, and formation of the release boxes. 600in a sacrificial layer, then bonding via the dielectric 500 on the host substrate 700 according to steps 1.4 to 1.8 of the previous method. In this case the resonator does not have a lower electrode under the piezoelectric layer, as illustrated in Figure 3c . Step 3.4: The temporary growth substrate is detached 100. In this example, annealing is carried out to cause the growth substrate to fracture at the weakened interface. I by ion implantation. Chemical etching is then carried out on the thin layer of growth substrate remaining attached to the structure, then on the buffer layer, as illustrated in 3d figure In the case of a silicon growth substrate, a TMAH solution allows the removal of residual silicon, and the chemical etching of the buffer layer can be done by a solution of HCl or H 3 PO 4 if it is ZnO. Step 3.5:The manufacturing of the component is finalized. To do this, we proceed by following steps 1.10 to 1.16 of the previous process, as illustrated in figure 3e which shows the Lamb wave resonator thus produced with a single level of electrodes 800 on the layer 300, a layer of dielectric 900 and contact pads 1000, on the host substrate 700.
[0040] The previous process examples concern the production of components from layers of epitaxially grown lithium niobate.
[0041] The present invention may also be used with other materials that can be subjected to epitaxial growth. Examples include AIN, GaN, LiTaO 3 , KNbO 3 , etc.
[0042] The approach of the invention is however in no way reduced to epitaxial layers. It can a prioriapply to any type of deposited layer, provided that the incorporation of the deposition step into the complete integration of the component proves to be complex (for example, very high temperature depositions in the presence of metals and / or on a surface presenting topography).
[0043] An example of this type of scenario is the use of thin PZT layers to produce piezoelectric microtransformers. This type of component is similar to the Lamb wave resonators described above, but is composed of two interdigitated comb transducers, one corresponding to the primary of the transformer, and the other to the secondary. The plate waves then ensure the transfer of power from the primary to the secondary. In order to effectively excite these waves in the PZT, it is necessary to have a lower electrode. To ensure electrical insulation between the primary and secondary, it is therefore necessary to have two distinct lower electrodes, and therefore to define the lower metal level. However, conventional PZT growth processes (by sol-gel process, cathode sputtering or laser ablation, ...) are generally optimized for growth on a metallic film (usually Platinum) covering the entire substrate. In particular, it has been observed that the deposition of PZT on defined electrodes raises a number of issues: the nature of the surface on which the PZT film is deposited is different depending on whether it is metal (textured Pt) or another sub-layer (amorphous SiO 2 or partially textured TiO 2, ...); moreover, the thermal expansion coefficients of the materials present are different. All this leads to the appearance of distinct residual stresses between the metallized and non-metallized regions. Furthermore, the presence of metal can provide a barrier to the diffusion of certain elements (notably Pb).We are therefore witnessing the appearance of parasitic phases (pyrochlore phase deficient in Pb) in the non-metallized regions, which proves prohibitive in terms of manufacturing and operation of the components. Even if the insertion of adequate sub-layers makes it possible to partially resolve this problem as described in the article: M. Bousquet, B. Viala, H. Achard, J. Georges, A. Reinhardt, E. Nolot, G. Le Rhun, E. Defaÿ, Pt-less silicon integration of PZT sol-gel thin films for microelectronics, Electroceramics XIV, 2014, it remains difficult to obtain an identical material between the metallized and non-metallized regions.
[0044] The present invention makes it possible to solve this problem. Indeed, it makes it possible to deposit a PZT film on a growth substrate having a full plate electrode, then to transfer this film to a host substrate by integrating this time a defined electrode. Furthermore, the present invention makes it possible to improve the growth of PZT films by using non-silicon substrates, such as for example MgO, SrTiO 3 , LaAlO 3 , LSAT ((LaAlO 3 ) 0.3 (Sr 2 TaAlO 6 ) 0.7 ), DyScO 3 , Sapphire (Al 2 O 3 ) or lithium niobate (LiNbO 3 ), lithium tantalate (LiTaO3). These monocrystalline substrates have the advantage of allowing epitaxial growth of PZT and not polycrystalline as on most films deposited on silicon. In addition, the choice of substrate makes it possible to modulate the crystalline orientation of the deposited film, the structuring in ferroelectric domains (proportion of ferroelectric domains of orientation a / c ), as well as the Curie temperature of the material formed. Example of a process for producing a PZT piezoelectric transformer Step 4.1 :
[0045] A SrTiO 3 substrate is prepared 100 : Chemical treatment (H 2 O + buffered HF) + high temperature annealing (> 1000°C) in order to obtain atomic steps (TiO 2 planes on the surface), as illustrated in Figure 4a . Step 4.2 :
[0046] We proceed to deposit a layer 300 of PZT, for example by laser ablation, sputtering or sol-gel, preferably to a thickness of 2 µm, as illustrated in Figure 4b . Step 4.3 :
[0047] A metallic layer, for example ruthenium, 100nm thick, is deposited by sputtering, then this layer is structured to define lower electrodes. 400 by photolithography, reactive ion etching and resist removal, as shown in Figure 4c . Step 4.4 :
[0048] A planarization layer is deposited 500a in SiO2 by PECVD and polishing, as shown in figure 4d . Step 4.5 :
[0049] Photolithography operations are also carried out, followed by reactive ion etching of a host silicon substrate. 700, covered with a layer of oxide 500b to define cavities for example 3 µm deep, as illustrated in Figure 4e . Step 4.6 :
[0050] Polysilicon is deposited to a thickness of 3 µm in the pre-defined cavities in order to create a sacrificial polysilicon structure. 600 then a planarization operation is carried out, as illustrated in Figure 4f . Step 4.7 :
[0051] A new thermal operation is carried out on 200nm, in order to encapsulate the sacrificed structure 600,by oxide 500c, as illustrated in figure 4g . Step 4.8 :
[0052] The temporary growth substrate is glued 100 on the host substrate 700 silicon, with alignment of electrode patterns 400 compared to polysilicon boxes 600 as illustrated in figure 4h , then a consolidation annealing of the substrate is carried out. Step 4.9 :
[0053] The temporary growth substrate is removed 100, by mechanical thinning and finalization by chemical etching, as illustrated in figure 4i . Step 4.10 :
[0054] The metal constituting the upper electrodes is deposited, for example with 100 nm of ruthenium. Photolithography and ion etching are carried out, followed by resin removal, to structure the electrodes. 800 as illustrated in figure 4j . Step 4.11 :
[0055] A new photolithography operation is carried out, then ion etching of the layer 300 of PZT to open contacts to the lower electrodes 400 as illustrated in figure 4k . Step 4.12 :
[0056] The oxide is deposited 900 by PECVD, for example on a thickness of 200 nm, then photolithography operations are carried out to open the electrical contacts towards the lower electrodes 400 and above 800, as illustrated in figure 4l . Step 4.13 :
[0057] Cr / Au (1µm) is deposited by sputtering, photolithography and wet etching, in order to form the electrical contact pads. 1000, as illustrated in figure 4m . Step 4.14 :
[0058] Photolithography and ion etching operations are again carried out on the SiO 2 / PZT / SiO 2 assembly, i.e. 500 / 300 / 900, to open access to the sacrificial polysilicon structure 600. The polysilicon is then removed by etching with gaseous XeF2, as illustrated in figure 4n . Step 4.15 :
[0059] The ferroelectric material is polarized by applying an electric voltage.
[0060] This process also makes it possible to consider the integration of PZT layers on substrates incompatible with the deposition temperatures required to obtain a crystallized PZT film. The invention therefore makes it possible, for example, to produce PZT actuators on glass.
[0061] Finally, the present invention is not necessarily limited to resonator applications. It can be applied to other micro-systems such as actuators or sensors.
Claims
1. A method for manufacturing a micro-electro-mechanical system, comprising the following steps: - producing a stack on the surface of a temporary substrate (100) so as to produce a first assembly, comprising: - at least depositing a piezoelectric material or a ferroelectric material to produce a layer of piezoelectric material or of ferroelectric material (300); - producing a first bonding layer (500a, 500b); - producing a second assembly comprising at least the production of a second bonding layer (500c) on the surface of a host substrate (700); the method further containing: - the production of at least one acoustic isolation structure in said first assembly and the production of at least one so-called lower electrode (400) on the surface of said layer of piezoelectric material or of ferroelectric material; - the bonding of said first and second assemblies via said first and second bonding layers, after the production of the lower electrode (400) and of the acoustic isolation structure; - the removal of said temporary substrate (100); - then, the production of at least one so-called upper electrode (800) on said layer of piezoelectric material or of ferroelectric material; and wherein the production of the acoustic isolation structure comprises producing a Bragg mirror (MR) structure.
2. The method according to claim 1, wherein said piezoelectric material or of said ferroelectric material is deposited by epitaxial growth.
3. The method according to one of claims 1 to 2, wherein the micro-electro-mechanical system comprises at least one volume elastic wave resonator or at least one surface elastic wave resonator or at least one Lamb wave resonator.
4. The method according to one of claims 1 to 3, wherein the bonding comprises a step of thermal annealing.
5. The method according to one of claims 1 to 4, wherein the operation of removing the temporary substrate comprises: - a step of thinning said temporary substrate; - an operation of chemically etching said thinned temporary substrate.
6. The method according to one of claims 1 to 4, wherein the operation of removing said temporary substrate comprises: - a step of diffusing elements that cause precipitation or chemical reactions in the material from which said temporary substrate is made, or - a step of implanting ions into said temporary substrate.
7. The method according to one of claims 1 to 6, comprising the deposition of a buffer layer (200) on the surface of said temporary substrate (100), prior to the deposition of said piezoelectric material or of said ferroelectric material.
8. The method according to one of claims 1 to 7, comprising the production of structured layers made of metal, that may be molybdenum, inserted into the dielectric that may be SiO2.
9. The method according to any one of claims 1 to 8, containing, prior to said bonding of said first and second assemblies: - the production of electrodes on the surface of said layer of piezoelectric material or of ferroelectric material; - the production of an acoustic isolation structure in said second assembly.
10. The method according to one of claims 1 to 9, wherein the piezoelectric material is LiNbO3 or LiTaO3 or solid solutions thereof, or KNbO3 or AIN, GaN.
11. The method according to one of claims 1 to 9, wherein the ferroelectric material is: LiNbO3 or LiTaO3 or PZT.
12. The method according to any one of claims 1 to 11, wherein the temporary substrate is made of MgO or of SrTiO3 or of LaAlO3 or of LSAT ((LaAlO3)0.3(Sr2TaAlO6)0.7) or of DyScO3, or of sapphire (Al2O3) or of lithium niobate (LiNbO3), lithium tantalate (LiTaO3), quartz, wherein the piezoelectric material can advantageously be PZT.
13. The method according to any one of claims 1 to 12, wherein the first and second bonding layers are made of oxide or made of polymer.