Novel water-soluble polymer complexes in the form of an inverse emulsion and uses thereof
Patent Information
- Application Number
- DE602021020639
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-20
- Filing Date
- 2021-03-17
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2041-03-17
AI Technical Summary
Current polymer complexes used in paper and cardboard manufacturing lack stability and efficiency in drainage properties, and existing flocculation agents do not meet the requirements for speed and efficiency in technical flocculation processes.
A polymer complex is developed through reverse emulsion polymerization using a cationic water-soluble host polymer, such as poly-(dimethylamine-co-epichlorohydrin) and poly(dimethylamine-co-epichlorohydrin-co-ethylenediamine), which acts as a transfer agent to control polymer chain length, resulting in a stable and efficient drainage and turbidity reduction agent.
The polymer complex demonstrates improved drainage and turbidity reduction in paper and cardboard manufacturing, reducing the amount of product required and energy consumption during drying, while maintaining stability and efficiency over time.
Description
Field of invention
[0001] The present invention relates to a water-soluble polymer complex resulting from the inverse emulsion polymerization of one or more water-soluble monomers in the presence of a previously prepared polymer.
[0002] Another aspect of the invention relates to the use of this complex as a draining agent and in particular for their use in the manufacture of paper, cardboard or the like. Prior art
[0003] The Applicant's US patent 9,546,246 overcomes the problem of phase shift between polymers. This patent describes a polymer complex and its use as an agent for treating mineral fillers and in particular for its use in the manufacture of paper, cardboard or the like.
[0004] Patent FR 3 080 853 B1, also from the Applicant, describes a polymer complex and its use in a process for manufacturing paper, cardboard or the like. This polymer complex is obtained by polymerization of water-soluble monomers in the presence of a host polymer comprising vinylamine functions, a non-polymeric transfer agent, and in the absence of a branching or crosslinking agent of ethylenic polyfunctional type. US patents 7,001,953 and US 8,021,516 describe water-soluble polymers that can be used in sludge treatment and in paper manufacturing. These polymers are obtained by polymerization of monomers in the presence of a polymer that has been prepared previously and independently. As indicated in these documents, the already synthesized polymer and the polymer being synthesized do not substantially graft.
[0005] EP 262 945 A2 describes mixtures of cationic flocculating agents composed of two different polymers and their production methods. The agents are formed by polymerizing cationic monomers into a high molecular weight cationic polymer component (flocculant) in the presence of a low molecular weight cationic polymer component (coagulant). The properties of these flocculating agents do not meet the requirements for speed and efficiency imposed by technical flocculation processes.
[0006] In any case, there is a demand for polymer complexes that are stable and have satisfactory drainage properties when used in the manufacture of paper, cardboard or the like. Statement of the invention
[0007] The present invention relates to a polymer complex comprising a cationic water-soluble polymer (host polymer) selected from poly-(dimethylamine (co) epichlorohydrin) and poly (dimethylamine-co-epichlorohydrin-co-ethylenediamine) and one or more water-soluble monomers polymerized in the presence of said water-soluble host polymer.
[0008] The term "water-soluble" means a compound (especially a polymer complex or a polymer or a monomer) forming an aqueous solution without insoluble particles when added with stirring for 4 hours at 25°C at a concentration of 20 gL -1< in water.
[0009] More specifically, the subject of the present invention relates to a polymer complex obtained by inverse emulsion polymerization of water-soluble monomers in the presence of one (or more) cationic water-soluble host polymer comprising amine functions chosen from poly-(dimethylamine (co) epichlorohydrin) and poly (dimethylamine-co-epichlorohydrin-co-ethylenediamine)
[0010] Water-soluble monomer polymerization refers to the polymerization of a single type of water-soluble monomer (e.g., acrylamide) or multiple types of water-soluble monomer (e.g., acrylamide and ADAME quaternized with methyl chloride).
[0011] In the complex thus obtained, the polymer(s) resulting from the polymerization of the monomers branches with the host polymer. It is not a mixture of polymers but a complex in which the host polymer acts as a transfer agent during the polymerization of the monomers.
[0012] The transfer agent, in this case the host polymer, allows the length of the polymer chains formed during the polymerization of the water-soluble monomers to be controlled.
[0013] By polymer is meant a homopolymer or a copolymer resulting from the polymerization of monomers which are respectively identical or distinct.
[0014] Another aspect of the invention is the use of this water-soluble polymer complex as a drainage and turbidity-reducing agent in the manufacture of paper, cardboard or the like. * Host polymer
[0015] The host polymer is a polyamine having ammonium groups and hydroxyl groups selected from poly-(dimethylamine (co) epichlorohydrin) and poly (dimethylamine-co-epichlorohydrin-co-ethylenediamine). It may also comprise secondary amine groups.
[0016] The host polymer is a polyamine selected from the group comprising poly-(dimethylamine (co) epichlorohydrin) and poly (dimethylamine-co-epichlorohydrin-co-ethylenediamine). Preferably, the polyamine is a poly (dimethylamine-co-epichlorohydrin-co-ethylenediamine).
[0017] According to a variant of the invention, the host polymer may be a poly(epichlorohydrin-dimethylamine) generally comprising the repeating unit -[N +< (CH 3 ) 2 CH 2 CHOHCH 2] Cl -< -. The poly(epichlorohydrin-dimethylamine) may be obtained by the reaction between dimethylamine and epichlorohydrin, advantageously in a stoichiometric ratio.
[0018] According to another variant of the invention, the host polymer may be a poly(dimethylamine-co-epichlorohydrin-coethylenediamine). Polymers of this type may be obtained by reacting dimethylamine, ethylenediamine and epichlorohydrin
[0019] According to a preferred characteristic of the invention, the host polymer is structured. In other words, it can advantageously have a branched, or star (star-shaped), or comb (comb-shaped) shape.
[0020] According to the invention, the host polymer has a molecular weight of at least 1000 g / mol, preferably at least 2000 g / mol, and even more preferably at least 5000 g / mol. In general, the molecular weight of the host polymer is advantageously less than 2 million g / mol, more advantageously less than 1 million g / mol. * The water-soluble polymer complex
[0021] It is derived from the inverse emulsion polymerization of water-soluble monomers during which the pre-existing host polymer acts as a transfer agent. Thus, the present invention can be carried out in the absence of a non-polymeric transfer agent. Advantageously, the molecular weight of a non-polymeric transfer agent is less than 200 g / mol.
[0022] The water-soluble monomer(s) used during the preparation of the water-soluble polymer complex may in particular be at least one cationic monomer and / or at least one non-ionic monomer and / or at least one anionic monomer. They may also be zwitterionic monomer(s). Preferably, the water-soluble monomers used during the preparation of the water-soluble polymer complex are at least one cationic monomer and at least one non-ionic monomer.
[0023] According to a preferred embodiment, the polymer complex is produced in the absence of non-water-soluble monomers, in particular monomers of the (meth)acrylate ester type.
[0024] The cationic monomer(s) that can be used in the context of the invention can advantageously be chosen from diallyldialkyl ammonium salts such as diallyl dimethyl ammonium chloride (DADMAC); acidified or quaternized salts of dialkylaminoalkyl acrylates and methacrylates, in particular dialkylaminoethyl acrylate (ADAME) and dialkylaminoethyl methacrylate (MADAME); acidified or quaternized salts of dialkylaminoalkylacrylamides or methacrylamides, such as for example methacrylamidopropyl trimethyl ammonium chloride (MAPTAC), acrylamidopropyl trimethyl ammonium chloride (APTAC) and Mannich products such as quaternized dialkylaminomethylacrylamides.
[0025] The "alkyl" groups of these monomers can be linear, cyclic (substituted or not) or branched. They can be identical or not. They have a number of carbon atoms advantageously between 1 and 10, more advantageously between 1 and 8, even more advantageously between 1 and 4. It is preferably a methyl or ethyl group. Thus, the acidified or quaternized salts of ADAME and MADAME are advantageously the acidified or quaternized salts of dimethylaminoethyl acrylate and dimethylaminoethyl methacrylate.
[0026] The acidified salts are obtained by means known to those skilled in the art, and in particular by protonation. The quaternized salts are also obtained by means known to those skilled in the art, in particular by reaction with an alkyl halide, an aryl halide, for example benzyl chloride, methyl chloride (MeCl), aryl chlorides, alkyl chlorides, or dimethyl sulfate. The cationic monomer is advantageously AD AME quaternized with methyl chloride.
[0027] According to the invention, the proportion of cationic monomer used is advantageously between 1 mol% and 80 mol%, preferably between 2 mol% and 60 mol%, and even more preferably between 5 mol% and 40 mol%, relative to the total number of water-soluble monomers used.
[0028] The non-ionic monomer(s) that may be used in the context of the invention may be chosen from acrylamide, methacrylamide, N-isopropylacrylamide, N,N-dimethylacrylamide and N-methylolacrylamide. Also, N-vinylformamide, N-vinyl acetamide, N-vinylpyridine and N-vinylpyrrolidone, acryloyl morpholine (ACMO) and diacetone acrylamide may be used. A preferred non-ionic monomer is acrylamide.
[0029] According to the invention, the proportion of non-ionic monomer used is advantageously between 20 mol% and 99 mol%, preferably between 40 mol% and 98 mol%, and even more preferably between 60 mol% and 95 mol%, relative to the total number of water-soluble monomers used.
[0030] The anionic monomer(s) that can be used in the context of the invention can be chosen from a broad group. These monomers can have vinyl functionalities, in particular acrylic, maleic, fumaric, allylic and contain a carboxylate, phosphonate, phosphate, sulfate, sulfonate group, or another anionically charged group. The monomer can be acidic or in the form of a salt or corresponding alkaline earth metal, alkali metal or ammonium (advantageously quaternary ammonium) of such a monomer.Examples of suitable monomers include acrylic acid, methacrylic acid, itaconic acid, crotonic acid, maleic acid, fumaric acid, and strong acid monomers having, for example, a sulfonic acid or phosphonic acid functionality such as 2-acrylamido 2-methylpropane sulfonic acid, vinyl sulfonic acid, vinyl phosphonic acid, allyl sulfonic acid, allyl phosphonic acid, styrene sulfonic acid, and water-soluble alkali metal, alkaline earth metal, and ammonium salts of these monomers. A preferred monomer is acrylic acid.
[0031] According to the invention, the proportion of anionic monomer used is advantageously between 0 mol% and 80 mol%, preferably between 1 mol% and 60 mol%, and even more preferably between 2 mol% and 40 mol%, relative to the total number of water-soluble monomers used.
[0032] The mass ratio of water-soluble monomers / host polymer is preferably between 99 / 1 and 1 / 99, more preferably between 95 / 5 and 40 / 60.
[0033] Advantageously, the present invention uses at least two types of distinct water-soluble monomers, advantageously a non-ionic monomer and a cationic monomer, more advantageously acrylamide and a cationic monomer (for example ADAME quaternized with methyl chloride).
[0034] According to the invention, the polymer complex is advantageously obtained by inverse emulsion polymerization. Inverse emulsion polymerization also covers inverse microemulsion polymerization. This polymerization technique is well known to those skilled in the art. It consists of emulsifying, in an oil phase, an aqueous phase containing the monomer(s). This emulsification is generally carried out using a water-in-oil surfactant. After polymerization of the monomer(s), an oil-in-water surfactant is optionally added to facilitate, subsequently, the inversion of the emulsion in water.
[0035] At the end of the polymerization reaction, the resulting emulsion may be diluted or concentrated. In particular, it is possible to concentrate the emulsion, for example by distillation. Such concentration will be carried out with or without the prior introduction of an emulsifying agent of the oil-in-water (O / W) type.
[0036] Advantageously, the process for preparing the polymer complex may comprise the following steps: preparation of an aqueous phase comprising at least one host polymer and water-soluble monomers; emulsification of said aqueous solution in an oil phase; obtaining the polymer complex by polymerization of the water-soluble monomers.
[0037] Preferably, during the preparation of the complex, the host polymer is introduced into the reactor with the monomers. The polymerization is then initiated by adding the catalysts.
[0038] Preferably, the polymerization is carried out in the absence of a branching or crosslinking agent of the ethylenic polyfunctional type, for example in the absence of N,N-methylene-bis-acrylamide. It is advantageously carried out in the absence of a branching or crosslinking agent with a molecular weight of less than 200 g g / mol.
[0039] Another aspect of the invention is the use of the water-soluble polymer complexes in the manufacture of paper, cardboard or the like.
[0040] The method of manufacturing paper, cardboard or the like, according to the invention, may comprise the following steps, on a paper machine: aqueous suspension of fibers, advantageously cellulose fibers; addition of the polymer complex which is the subject of the invention to the aqueous suspension of fibers; formation of a sheet of paper, cardboard or the like on the fabric of the paper machine; drying of the sheet.
[0041] The polymer complex can be added to the fiber suspension, at one or more injection points, in the dilute paste and / or in the thick paste.
[0042] In addition to the complex, other compounds known to those skilled in the art may be combined. These may include, but are not limited to, dispersants, biocides or anti-foam agents.
[0043] This method may also include the addition of polymers distinct from the complex according to the invention. Examples include coagulants, retention agents, flocculants or even starch. These additives may be polymeric or mineral in nature, for example bentonite.
[0044] Thus, the process for manufacturing paper, cardboard or the like may comprise the addition, before the formation of the sheet, of at least one additive, distinct from the polymer complex, chosen from coagulants, retention agents, flocculants and starch.
[0045] Preferably, the polymer complex is added before the mixing pump, into the thick paste.
[0046] The various stages of the process of manufacturing paper, cardboard or the like are in accordance with the techniques forming part of the knowledge of those skilled in the art.
[0047] The quantity of complex added is advantageously between 3 g of active material / tonne of fibers (dry weight in fibers, advantageously cellulosic) and 10,000 g / T, preferably between 10 g / T and 7,000 g / T and even more preferably between 30 g / T and 3,000 g / T.
[0048] The use of polymer complexes is part of a general principle of improving product performance. Reducing the quantity of product required for application therefore implicitly contributes to reducing greenhouse gas emissions such as CO2. In addition, the use of polymer complexes allows energy savings during the drying stage of the paper sheet, which requires less steam.
[0049] The following examples illustrate the invention without, however, limiting it. List of figures
[0050] There figure 1 represents a graph of UL viscosity versus monomer / polyamine ratio. The figure 2 illustrates the percentage, compared to a reference test (blank), of the improvement in drainage in thick paste and measurement of turbidity. The figure 3 illustrates the percentage, compared to a reference test (blank), of the improvement in vacuum drainage in diluted pulp and measurement of turbidity. The figure 4 illustrates the vacuum draining performance in dilute pulp and the measurement of turbidity, compared to a reference test (blank). The Figure 5 illustrates the value of dryness before pressing, compared to a reference test (blank). The figure 6 illustrates the percentage, compared to a reference test (blank), of the improvement in vacuum drainage in diluted pulp and the measurement of turbidity. figure 7 illustrates the vacuum draining performance in dilute pulp and the measurement of turbidity, compared to a reference test (blank). The figure 8 illustrates the improvement (in percentage) of vacuum drainage in dilute pulp and the measurement of turbidity compared to a reference test (blank). Examples of embodiments of the invention
[0051] In the following examples: Polyamine H-1 is a structured poly-(dimethylamine / epichlorohydrin / ethylenediamine) with a Brookfield viscosity of 850cps (Module LV2, 30 rpm -1< , 23°C) at 50% active matter by weight in water. Polyamine H-2 is a linear poly-(dimethylamine / epichlorohydrin) with a Brookfield viscosity of 30cps (Module LV1, 60 rpm -1< , 23°C) at 50% active matter by weight in water. P-3: is a linear poly-(acrylamide / acrylic acid) anionic inverse emulsion polymer with a UL viscosity of 8.16cps (Brookfield Viscosity, UL Module, 1M NaCl, 60 rpm -1< , 23°C) at 29% active matter by weight in water. P-4: is a polymer in cationic powder form, linear poly-(acrylamide / dimethylaminoethyl acrylate, MeCl), with UL viscosity = 4.1 1cps (Brookfield Viscosity, UL Module, 1M NaCl, 60 rpm -1< , 23°C) at 92% active matter by weight in water. Bentonite: Inorganic microparticle, marketed by CLARIANT under the name OPAZIL ABG. * Synthesis of an inverse emulsion polymer P1
[0052] The aqueous phase is prepared by adding 359.8g of acrylamide (50% by weight solution in water), 262.6g of dimethylaminoethyl acrylate, MeCl (80% by weight solution in water) and 90.2g of water. The pH of the solution is adjusted to between 4 and 5 with adipic acid. 100-250 ppm / MS (mass as dry monomers) of potassium bromate and 800-1500 ppm / MS of sodium diethylenetriaminepentaacetate are then added as initiators.
[0053] The organic phase is prepared by adding 234.2g of Exxsol D100S oil, 4.7g of sorbitan monooleate, 8.2g of sorbitan monooleate 3 EO (oxyethylene group), 11.1g of sorbitan monooleate 5 EO (oxyethylene group) and 4.8g of oil-in-water surfactant polymer (Rhodibloc RS) to a reactor.
[0054] The aqueous phase is then transferred into the organic phase and then emulsified, for example using Ultra-Turax, at 8000 rpm for 1 minute in order to obtain a uniform inverse emulsion.
[0055] The inverse emulsion is deoxygenated with nitrogen bubbling for 30 min. Polymerization is initiated by the addition of sodium bisulfite and the temperature is maintained at 55°C for approximately 1.5 hours. The reaction medium is finally treated with an excess of sodium bisulfite to reduce the free monomers.
[0056] Once the inverse emulsion is made, the Brookfield viscosity is measured (UL Module, 1M NaCl, 60 rpm -1< , 23°C). A UL viscosity of 4.21 cps is obtained for an active ingredient of 39% by weight. * Synthesis of inverse emulsion polymer P2
[0057] The aqueous phase is prepared by adding 491.3g of acrylamide (50% by weight solution in water), 92.9g of dimethylaminoethyl acrylate, MeCl (80% by weight solution in water) and 149.2g of water. The pH of the solution is adjusted between 4 and 5 with adipic acid. 100-250 ppm / MS of potassium bromate and 800-1500 ppm / MS of sodium diethylenetriaminepentaacetate are then added as initiators.
[0058] The organic phase is prepared by adding 213.2g of Exxsol D100S oil, 26g of sorbitan monooleate and 3.8g of surfactant polymer (Rhodibloc RS) to a reactor.
[0059] The aqueous phase is then transferred into the organic phase and then emulsified, for example using Ultra-Turax, at 8000 rpm for 1 minute in order to obtain a uniform inverse emulsion.
[0060] The inverse emulsion is deoxygenated with nitrogen bubbling for 30 min. Polymerization is initiated by the addition of sodium bisulfite and the temperature is maintained at 55°C for approximately 1.5 hours. The reaction medium is finally treated with an excess of sodium bisulfite to reduce the free monomers.
[0061] Once the inverse emulsion is made, the Brookfield viscosity is measured (UL Module, 1M NaCl, 60 rpm -1< , 23°C). A UL viscosity of 4.26 cps is obtained for an active ingredient of 32% by weight. * Synthesis of an inverse emulsion complex according to the invention (I-1)
[0062] The aqueous phase is prepared by adding 369.1g of acrylamide (50% by weight solution in water), 256.8g of dimethylaminoethyl acrylate, MeCl (80% by weight solution in water), 2.2g of water and 82.5g of polyamine H-1. The pH of the solution is adjusted between 4 and 5 with adipic acid. 100-250 ppm / MS of potassium bromate and 800-1500 ppm / MS of sodium diethylenetriaminepentaacetate are then added as initiators.
[0063] The organic phase is prepared by adding 234.2g of Exxsol D100S oil, 4.7g of sorbitan monooleate, 8.2g of sorbitan monooleate 3 EO (oxyethylene group), 11.1g of sorbitan monooleate 5 EO (oxyethylene group) and 4.8g of surfactant polymer (Rhodibloc RS) to a reactor.
[0064] The aqueous phase is then transferred into the organic phase and then emulsified, for example using Ultra-Turax, at 8000 rpm for 1 minute in order to obtain a uniform inverse emulsion.
[0065] The inverse emulsion is deoxygenated with nitrogen bubbling for 30 min. Polymerization is initiated by the addition of sodium bisulfite and the temperature is maintained at 55°C for approximately 1.5 hours. The reaction medium is finally treated with an excess of sodium bisulfite to reduce the free monomers.
[0066] Once the inverse emulsion is made, the Brookfield viscosity is measured (UL Module, 1M NaCl, 60 rpm -1< , 23°C). A UL viscosity of 3.81 cps is obtained for an active ingredient of 43.1% by weight. * Synthesis of an inverse emulsion complex according to the invention (1-2)
[0067] The aqueous phase is prepared by adding 290.6g of acrylamide (50% by weight solution in water), 212.1g of dimethylaminoethyl acrylate, MeCl (80% by weight solution in water), 1g of water and 213.4g of polyamine H-1. The pH of the solution is adjusted between 4 and 5 with adipic acid. 100-250 ppm / MS of potassium bromate and 800-1500 ppm / MS of sodium diethylenetriaminepentaacetate are then added as initiators.
[0068] The organic phase is prepared by adding 234.2g of Exxsol D100S oil, 4.7g of sorbitan monooleate, 8.2g of sorbitan monooleate 3 EO (oxyethylene group), 11.1g of sorbitan monooleate 5 EO (oxyethylene group) and 4.8g of surfactant polymer (Rhodibloc RS) to a reactor.
[0069] The aqueous phase is then transferred into the organic phase and then emulsified, for example using Ultra-Turax, at 8000 rpm for 1 minute in order to obtain a uniform inverse emulsion.
[0070] The inverse emulsion is deoxygenated with nitrogen bubbling for 30 min. Polymerization is initiated by the addition of sodium bisulfite and the temperature is maintained at 55°C for approximately 1.5 hours. The reaction medium is finally treated with an excess of sodium bisulfite to reduce the free monomers.
[0071] Once the inverse emulsion is made, the Brookfield viscosity is measured (UL Module, 1M NaCl, 60 rpm -1< , 23°C). A UL viscosity of 3.71 cps is obtained for an active ingredient of 42.1% by weight. * Synthesis of an inverse emulsion complex according to the invention (1-3)
[0072] The aqueous phase is prepared by adding 287.8g of acrylamide (50% by weight solution in water), 210.1g of dimethylaminoethyl acrylate, MeCl (80% by weight solution in water), 0.7g of water and 237.5g of polyamine H-1. The pH of the solution is adjusted between 4 and 5 with adipic acid. 100-250 ppm / MS of potassium bromate and 800-1500 ppm / MS of sodium diethylenetriaminepentaacetate are then added as initiators.
[0073] The organic phase is prepared by adding 214.2g of Exxsol D100S oil, 4.7g of sorbitan monooleate, 8.2g of sorbitan monooleate 3 EO (oxyethylene group), 11.1g of sorbitan monooleate 5 EO (oxyethylene group) and 4.8g of surfactant polymer (Rhodibloc RS) to a reactor.
[0074] The aqueous phase is then transferred into the organic phase and then emulsified, for example using Ultra-Turax, at 8000 rpm for 1 minute in order to obtain a uniform inverse emulsion.
[0075] The inverse emulsion is deoxygenated with nitrogen bubbling for 30 min. Polymerization is initiated by the addition of sodium bisulfite and the temperature is maintained at 55°C for approximately 1.5 hours. The reaction medium is finally treated with an excess of sodium bisulfite to reduce the free monomers.
[0076] Once the inverse emulsion is made, the Brookfield viscosity is measured (UL Module, 1M NaCl, 60 rpm -1< , 23°C). A UL viscosity of 3.46 cps is obtained for an active ingredient of 43.1% by weight. * Synthesis of an inverse emulsion complex according to the invention (1-4)
[0077] The aqueous phase is prepared by adding 250.9g of acrylamide (50% by weight solution in water), 183.1g of dimethylaminoethyl acrylate, MeCl (80% by weight solution in water), 0.9g of water and 280.1g of polyamine H-1. The pH of the solution is adjusted between 4 and 5 with adipic acid. 100-250 ppm / MS of potassium bromate and 800-1500 ppm / MS of sodium diethylenetriaminepentaacetate are then added as initiators.
[0078] The organic phase is prepared by adding 234.2g of Exxsol D100S oil, 4.7g of sorbitan monooleate, 8.2g of sorbitan monooleate 3 EO (oxyethylene group), 11.1g of sorbitan monooleate 5 EO (oxyethylene group) and 4.8g of surfactant polymer (Rhodibloc RS) to a reactor.
[0079] The aqueous phase is then transferred into the organic phase and then emulsified, for example using Ultra-Turax, at 8000 rpm for 1 minute in order to obtain a uniform inverse emulsion.
[0080] The inverse emulsion is deoxygenated with nitrogen bubbling for 30 min. Polymerization is initiated by the addition of sodium bisulfite and the temperature is maintained at 55°C for approximately 1.5 hours. The reaction medium is finally treated with an excess of sodium bisulfite to reduce the free monomers.
[0081] Once the inverse emulsion is made, the Brookfield viscosity is measured (UL Module, 1M NaCl, 60 rpm -1< , 23°C). A UL viscosity of 3.01 cps is obtained for an active ingredient of 41.2% by weight. * Synthesis of an inverse emulsion complex according to the invention (1-5)
[0082] The aqueous phase is prepared by adding 184.5g of acrylamide (50% by weight solution in water), 134.7g of dimethylaminoethyl acrylate, MeCl (80% by weight solution in water), 0.5g of water and 396g of polyamine H-1. The pH of the solution is adjusted between 4 and 5 with adipic acid. 100-250 ppm / MS of potassium bromate and 800-1500 ppm / MS of sodium diethylenetriaminepentaacetate are then added as initiators.
[0083] The organic phase is prepared by adding 234.2g of Exxsol D100S oil, 4.7g of sorbitan monooleate, 8.2g of sorbitan monooleate 3 EO (oxyethylene group), 11.1g of sorbitan monooleate 5 EO (oxyethylene group) and 4.8g of surfactant polymer (Rhodibloc RS) to a reactor.
[0084] The aqueous phase is then transferred into the organic phase and then emulsified, for example using Ultra-Turax, at 8000 rpm for 1 minute in order to obtain a uniform inverse emulsion.
[0085] The inverse emulsion is deoxygenated with nitrogen bubbling for 30 min. Polymerization is initiated by the addition of sodium bisulfite and the temperature is maintained at 55°C for approximately 1.5 hours. The reaction medium is finally treated with an excess of sodium bisulfite to reduce the free monomers.
[0086] Once the inverse emulsion is made, the Brookfield viscosity is measured (UL Module, 1M NaCl, 60 rpm -1< , 23°C). A UL viscosity of 2.51 cps is obtained for an active ingredient of 39.8% by weight. * Synthesis of an inverse emulsion complex according to the invention (1-6)
[0087] The aqueous phase is prepared by adding 439.1g of acrylamide (50% by weight solution in water), 83.1g of dimethylaminoethyl acrylate, MeCl (80% by weight solution in water), 0.2g of water and 214g of polyamine H-1. The pH of the solution is adjusted between 4 and 5 with adipic acid. 100-250 ppm / MS of potassium bromate and 800-1500 ppm / MS of sodium diethylenetriaminepentaacetate are then added as initiators.
[0088] The organic phase is prepared by adding 213.2g of Exxsol D100S oil, 26g of sorbitan monooleate and 3.8g of surfactant polymer (Rhodibloc RS) to a reactor.
[0089] The aqueous phase is then transferred into the organic phase and then emulsified, for example using Ultra-Turax, at 8000 rpm for 1 minute in order to obtain a uniform inverse emulsion.
[0090] The inverse emulsion is deoxygenated with nitrogen bubbling for 30 min. Polymerization is initiated by the addition of sodium bisulfite and the temperature is maintained at 55°C for approximately 1.5 hours. The reaction medium is finally treated with an excess of sodium bisulfite to reduce the free monomers.
[0091] Once the inverse emulsion is made, the Brookfield viscosity is measured (UL Module, 1M NaCl, 60 rpm -1< , 23°C). A UL viscosity of 3.61 cps is obtained for an active ingredient of 39.3% by weight. * Synthesis of an inverse emulsion complex according to the invention (1-7)
[0092] The aqueous phase is prepared by adding 287.8g of acrylamide 50% by weight in water, 210.1g of dimethylaminoethyl acrylate, MeCl 80% by weight in water, 0.7g of water and 237.5g of polyamine H-2. The pH of the solution is adjusted between 4 and 5 with adipic acid. 100-250 ppm / MS of potassium bromate and 800-1500 ppm / MS of sodium diethylenetriaminepentaacetate are then added as initiators.
[0093] The organic phase is prepared by adding 214.2g of Exxsol D100S oil, 4.7g of sorbitan monooleate, 8.2g of sorbitan monooleate 3 EO (oxyethylene group), 11.1g of sorbitan monooleate 5 EO (oxyethylene group) and 4.8g of surfactant polymer (Rhodibloc RS) to a reactor.
[0094] The aqueous phase is then transferred into the organic phase and then emulsified, for example using Ultra-Turax, at 8000 rpm for 1 minute in order to obtain a uniform inverse emulsion.
[0095] The inverse emulsion is deoxygenated with nitrogen bubbling for 30 min. Polymerization is initiated by adding sodium bisulfite using a syringe pump. The temperature is raised and then maintained at 55°C for approximately 1.5 hours. The reaction medium is finally treated with an excess of sodium bisulfite to reduce the free monomers.
[0096] Once the inverse emulsion is made, the Brookfield viscosity is measured (UL Module, 1M NaCl, 60 rpm -1< , 23°C). A UL viscosity of 3.31 cps is obtained for an active ingredient of 43.1% by weight. * Synthesis of a reverse emulsion complex according to the invention (1-8)
[0097] The aqueous phase is prepared by adding 537.3g of acrylamide 50% by weight in water, 101.7g of dimethylaminoethyl acrylate, MeCl 80% by weight in water, 0.7g of water and 73g of polyamine H-1. The pH of the solution is adjusted between 4 and 5 with adipic acid. 100-250 ppm / MS of potassium bromate and 800-1500 ppm / MS of sodium diethylenetriaminepentaacetate are then added as initiators.
[0098] The organic phase is prepared by adding 210.3g of Exxsol D100S oil, 25.9g of sorbitan monooleate and 3.7g of surfactant polymer (Rhodibloc RS) to a reactor.
[0099] The aqueous phase is then transferred into the organic phase and then emulsified, for example using Ultra-Turax, at 8000 rpm for 1 minute in order to obtain a uniform inverse emulsion.
[0100] The inverse emulsion is deoxygenated with nitrogen bubbling for 30 min. Polymerization is initiated by adding sodium bisulfite using a syringe pump. The temperature is raised and then maintained at 55°C for approximately 1.5 hours. The reaction medium is finally treated with an excess of sodium bisulfite to reduce the free monomers.
[0101] Once the inverse emulsion is made, the Brookfield viscosity is measured (UL Module, 1M NaCl, 60 rpm -1< , 23°C). A UL viscosity of 4.01 cps is obtained for an active ingredient of 38.6% by weight. * Synthesis of an inverse emulsion complex according to the invention (1-9)
[0102] The aqueous phase is prepared by adding 280.5g of acrylamide (50% by weight solution in water), 204.7g of dimethylaminoethyl acrylate, MeCl (80% by weight solution in water), 0.7g of water and 227.5g of polyamine H-1. The pH of the solution is adjusted between 4 and 5 with adipic acid. 2-25ppm / MS of sodium hypophosphite are added as a limiting agent and 2-25ppm / MS of methylene bis acrylamide as a crosslinking agent. 100-250 ppm / MS of potassium bromate and 800-1500 ppm / MS of sodium diethylenetriaminepentaacetate are then added as initiators.
[0103] The organic phase is prepared by adding 211.2g of Exxsol D100S oil, 4.7g of sorbitan monooleate, 8.2g of sorbitan monooleate 3 EO (oxyethylene group), 11.1g of sorbitan monooleate 5 EO (oxyethylene group) and 4.8g of surfactant polymer (Rhodibloc RS) to a reactor.
[0104] The aqueous phase is then transferred into the organic phase and then emulsified using Ultra-Turax at 8000 rpm for 1 minute to obtain a uniform inverse emulsion.
[0105] The inverse emulsion is deoxygenated with nitrogen bubbling for 30 min. Polymerization is initiated by the addition of sodium bisulfite and the temperature is maintained at 55°C for approximately 1.5 hours. The reaction medium is finally treated with an excess of sodium bisulfite to reduce the free monomers.
[0106] Once the inverse emulsion is made, the Brookfield viscosity is measured (UL Module, 1M NaCl, 60 rpm -1< , 23°C). A UL viscosity of 2.31 cps is obtained for an active ingredient of 41.8%.
[0107] Concerning the stability of the inverse emulsions according to the invention (I-1 to I-9), we do not observe any phase shift after several weeks of storage at room temperature. * Synthesis of a mixture of polymers in inverse emulsion (M-1)
[0108] In a beaker of IL, 767.8g of emulsion P2 is weighed and stirred using a half-moon type stirring blade. 205.2g of polyamine H-1 is added slowly and the mixture is left stirring for 10 minutes to ensure homogeneity. The mixture has an active ingredient of 35.8% by weight. A phase separation of the mixture is observed after one week of storage at room temperature. * Synthesis of a mixture of polymers in inverse emulsion (M-2)
[0109] In a beaker of IL, 571.8g of emulsion P1 is weighed and stirred using a half-moon type stirring blade. 300g of polyamine H-1 is added slowly and the mixture is left stirring for 10 minutes to ensure homogeneity. The mixture has an active ingredient of 38.2% by weight. A phase separation of the mixture is observed after one week of storage at room temperature. * Synthesis of a mixture of polymers in inverse emulsion (M-3)
[0110] In a beaker of IL, 759.9g of the P2 emulsion is weighed and stirred using a half-moon type stirring blade. 54g of polyamine H-1 is slowly added and the mixture is left stirring for 10 minutes to ensure homogeneity. The mixture has an active ingredient of 33.2% by weight. A phase separation of the mixture is observed after one week of storage at room temperature. * Synthesis of a polymer in powder form (C-1)
[0111] In a polymerization reactor, 748.7g of 50% acrylamide, 126.2g of dimethylaminoethyl acrylate, 80% MeCl, 431.5g of water and 95g of polyamine H-1 are charged. The pH of the solution is adjusted between 3 and 4 with adipic acid. The solution is cooled to a temperature between 0 and 2°C and then deoxygenated with a nitrogen sparge for 15 minutes. 1-15 ppm / MS of sodium persulfate and 1-15 ppm / MS of Mohr's salt are then added as initiators.
[0112] The reaction temperature increases from 0 to 90°C and the polymer is obtained in gel form. This gel is cut, chopped, dried for 45 minutes at a temperature of 75°C, ground and finally sieved. This produces a polymer in powder form with a particle size less than or equal to 1mm.
[0113] Once the polymer is in powder form, the Brookfield viscosity is measured (UL Module, 1M NaCl, 60 rpm -1< , 23°C). A UL viscosity of 3.76 cps is obtained for an active material of 92.8% by weight in water. Table 1: Summary of examples and counter-examples (PA = polyamine, %MA = percentage of active ingredient by weight) Name Shape Cationic monomer (mol%) Type PA % mass monomers / polyamine %MY UL (cps) P-1 Emulsion 30 N / A 100 / 0 39 4.21 P-2 Emulsion 10 N / A 100 / 0 32 4.26 H-1 Liquid N / A H-1 0 / 100 50 N / A H-2 Liquid N / A H-2 0 / 100 50 N / A I-1 Emulsion 30 H-1 90 / 10 43 3.81 I-2 Emulsion 30 H-1 75 / 25 42 3.71 I-3 Emulsion 30 H-1 70 / 30 43 3.46 I-4 Emulsion 30 H-1 66 / 34 41 3.01 I-5 Emulsion 30 H-1 50 / 50 40 2.51 I-6 Emulsion 10 H-1 70 / 30 39 3.61 I-7 Emulsion 30 H-2 70 / 30 43 3.31 I-8 Emulsion 10 H-1 90 / 10 39 4.01 I-9 Emulsion 30 H-1 70 / 30 42 2.31 M-1 Blend 10 H-1 70 / 30 36 4.26 M-2 Blend 30 H-1 70 / 30 38 4.21 M-3 Blend 10 H-1 90 / 10 33 4.26 C-1 Powder 10 H-1 90 / 10 93 3.76 P-3 Emulsions 30* N / A 100 / 0 29 8,16 P-4 Powder 10 N / A 100 / 0 92 4,11 *molar percentage of anionic monomer
[0114] The trials in Table 2 are analyzed by group: [2-4], [5-6], [7-8-9], [10-11-12], and [13-14-15]. * Assessment Test Procedures * Recycled fiber pulp :
[0115] Wet pulp is obtained by disintegrating dry pulp to obtain a final aqueous concentration of 4% by mass in water to produce the thick pulp, which is diluted in water to 1% by mass to obtain the diluted pulp. It is a neutral pH pulp composed of 100% recycled cardboard fibers. * UL viscosity measurement:
[0116] 500 mg of polymer (resulting from the polymerization of the monomers, according to the invention or not) are added to 490 ml of deionized water. After complete dissolution, 29.25 grams of NaCl are added.
[0117] Viscosity is measured using a Brookfield digital DVII+ viscometer at a rotation speed of 60 rpm at 25°C (UL module). * Drainage Performance Assessment (DDA) :
[0118] The DDA (Dynamic Drainage Analyzer) allows to automatically determine the time (in seconds) required to drain a fibrous suspension under vacuum. The polymers are added to the wet paste (0.6 liters of paste at 1.0% by mass) in the DDA cylinder while stirring at 1000 rpm: According to the following sequence for the evaluation of a single polymer: T=0s: stirring of the paste T=10s: addition of the cationic drainage agent (350 g / t) T=30s: stopping of the stirring and draining under vacuum at 200 mBar for 60s According to the following sequence for the evaluation of a combination of polymers: T=0s: stirring of the paste T=5s: addition of the cationic drainage agent (350 g / t) T=10s: addition of the cationic polymer (250 g / t) T=20s: addition of the anionic polymer (150 g / t) and / or bentonite (1.5 kg / t) T=30s: stopping of the stirring and draining under vacuum at 200 mBar for 60s
[0119] The dosages are expressed in grams of active ingredient / tonne of fibers (dry weight in fibers, advantageously cellulosic).
[0120] The pressure under the fabric is recorded as a function of time. When all the water is evacuated from the fibrous mat, the air passes through it, causing a break in slope to appear on the curve representing the pressure under the fabric as a function of time. The time, expressed in seconds, recorded at this break in slope corresponds to the drainage time. The shorter the time, the better the vacuum drainage.
[0121] In addition, the turbidity of the white water from the DDA measurement is measured. The lower the turbidity value, the greater the retention of solid particles in the fibrous mat. * Dryness:
[0122] The DDA test allows the free water to be drained from the fibrous suspension under vacuum. The purpose of the dryness test is to measure the amount of water bound in the fibrous mat. To do this, the resulting fibrous mat cake is recovered from the DDA test and its mass is measured before and after drying in an oven at 105°C for 2 hours. The ratio of the two masses is used to obtain the dryness. The higher this value, the more the drainage polymer eliminates bound water. * Evaluation of thick paste drainage performance :
[0123] In a beaker, 500ml of thick paste at 4% in water is processed, subjected to a low shear rate (stirring speed of 300 rpm). The polymer is added to this fibrous suspension with a contact time T=1min.
[0124] This treated paste is transferred to the Canadian Standard Freeness Tester.
[0125] The volume of water released over time is recorded. The greater the amount of water released, the better the drainage of the thick paste. * Turbidity :
[0126] Turbidity refers to the content of suspended matter that clouds the fluid. It is measured using a HANNA spectrophotometer, which measures the decrease in the intensity of the light beam at an angle of 90°, at a wavelength of 860 nm and expressed in NTU.
[0127] According to the figure 1 , we see that, all things being equal, the UL viscosity decreases when the monomer / polyamine ratio falls. We therefore conclude that the polyamine plays the role of transfer agent to the polymer.
[0128] According to the figures 2 And 3, whatever the products of the invention (I-1 to I-5) compared to the polymer alone (P-1) and compared to the polyamine alone (H-1), a synergistic effect is observed concerning the improvement of the drainage of the thick paste, the vacuum drainage of the diluted paste (DDA) as well as the turbidity. In this case, the monomer / polyamine mass ratio 70 / 30 (I-3) makes it possible to obtain the most favorable combination of thick paste drainage gain / vacuum drainage of the diluted paste (DDA) / turbidity.
[0129] According to the figures 4 And 5 , it is observed that the products of the invention (I-3 and I-6) are much more efficient in vacuum draining of the diluted paste, in turbidity, as well as in dryness before pressing compared to the corresponding mixtures (M-1 and M-2) as well as compared to the products alone (H-1, P-1 and P-2).
[0130] According to the figure 6, whatever the products of the invention (I-3 and I-7) compared to the products alone (P-1, H-1, H-2) we observe a synergistic effect concerning the improvement of the vacuum drainage of the diluted paste (DDA) as well as the turbidity. In this specific case, we note that the structure of the polyamine has a positive impact on the application performance compared to a linear polyamine.
[0131] According to the figure 7 , we observe that the polymerization in the form of inverse emulsion (I-8) remains much more efficient compared to the powder form (C-1) and the corresponding mixture (M-3). In addition, the polymerization in the form of inverse emulsion, with a polyamine, makes it possible to resolve the problem of stability of the simple mixture.
[0132] According to the figure 8, in tests 2 to 15, the products of the invention I-3 and I-6, tested comparatively and respectively to the products P-1 and P-2 (table 2; test 4 vs 2 and 3, test 6 vs 2 and 5, test 9 vs 7 and 8, test 12 vs 10 and 11, and test 15 vs 13 and 14), in combination with a retention system (single or multi-component), provide better performances in terms of improvement of the vacuum drainage of the diluted pulp (DDA) as well as reduction of turbidity.
Claims
1. A polymer complex obtained by inverse emulsion polymerization of water-soluble monomers: in the presence of a cationic water-soluble host polymer comprising amine functions, characterized in that the host polymer is chosen from poly-(dimethylamine (co)epichlorohydrin) and poly(dimethylamine-co-epichlorohydrin-co-ethylenediamine).
2. The polymer complex according to claim 1, characterized in that the host polymer is poly(dimethylamine-co-epichlorohydrin-co-ethylenediamine).
3. The polymer complex according to any one of claims 1 to 2, characterized in that the mass ratio between the water-soluble monomers and the host polymer is between 99 / 1 and 1 / 99, preferably between 95 / 5 and 40 / 60.
4. The polymer complex according to any one of the preceding claims, characterized in that the water-soluble monomers are chosen from the group comprising: - quaternary ammonium salts of dimethylaminoethyl acrylate (ADAME); quaternary ammonium salts of dimethylaminoethyl methacrylate (MADAME); dimethyldiallylammonium chloride (DADMAC); acrylamido propyltrimethyl ammonium chloride (APTAC); methacrylamido propyltrimethyl ammonium chloride (MAPTAC); - acrylamide; N-isopropylacrylamide; N,N-dimethylacrylamide; N-vinylformamide; N-vinylpyrrolidone; - acrylic acid; methacrylic acid; itaconic acid; crotonic acid; maleic acid; fumaric acid; 2-acrylamido 2-methylpropane sulfonic acid; vinylsulfonic acid; vinyl phosphonic acid; allylsulfonic acid; allylphosphonic acid; styrene sulfonic acid; water-soluble alkali metal, alkaline earth metal, or ammonium salts of these monomers.
5. A process for preparing the polymer complex object of any one of claims 1 to 4, comprising the following steps: - preparing of an aqueous phase comprising at least one host polymer and water-soluble monomers; - emulsifying said aqueous solution in an oil phase; - obtaining the polymer complex by polymerization of the water-soluble monomers.
6. The process according to claim 5, characterized in that the polymerization is carried out in the absence of a branching agent or crosslinking agent of polyfunctional ethylenic type.
7. A process for the manufacture of paper, cardboard or the like, wherein, before forming said sheet, a polymer complex according to one of claims 1 to 4 is added to a suspension of fibers at one or more injection points.
8. The process according to claim 7, characterized in that the amount of polymer complex added is, by dry weight, between 3 g / ton of fibers, advantageously cellulosic, and 10,000 g / ton of fibers, preferably between 10 g / ton of fibers and 7000 g / ton of fibers, and, even more preferably, between 30 g / ton of fibers and 3000 g / ton of fibers.
9. A process for the manufacture of paper, cardboard or the like, comprising the following steps, on a paper machine: - placing fibers, advantageously cellulosic fibers, in an aqueous suspension; - adding the polymer complex, object of any one of claims 1 to 4; - forming a sheet of paper, cardboard or the like on the wire surface of the paper machine; - drying the sheet.
10. The process according to any one of claims 7 to 9, characterized in that the process comprises the addition, before forming said sheet, the addition of at least an additive, other than the complex according to any one of claims 1 to 4, chosen among coagulants, retention agents, flocculants and starch.