High-wear-resistance wet paper-based friction material as well as preparation method and application thereof
By simplifying the preparation process of wet paper-based friction materials, and utilizing the impregnation solution of phenolic resin and nanocellulose combined with hot-press vulcanization, the problems of complex preparation and high energy consumption in the existing technology have been solved, realizing the production of friction materials with high wear resistance and low cost, which are suitable for wet clutches and braking devices of vehicles and engineering machinery.
Patent Information
- Application Number
- CN202411069620.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-22
AI Technical Summary
The preparation steps of existing wet paper-based friction materials are complex. The high-temperature melting and drawing step requires a special high-temperature resistant device, which consumes a lot of energy, has high production costs, and lacks wear resistance.
A high-wear-resistant wet paper-based friction material is prepared by mixing natural fibers, synthetic fibers, friction modifiers and water, dehydrating and shaping the mixture, drying it, impregnating it in a phenolic resin and nanocellulose impregnation solution, and finally hot-pressing and vulcanizing it at a temperature below 230°C.
It simplifies the manufacturing process, reduces energy consumption and production costs, and improves the wear resistance and friction properties of the material, making it suitable for wet clutches and braking devices in various vehicles and engineering machinery.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of friction materials, and in particular to a highly wear-resistant wet paper-based friction material and a preparation method and application thereof. Background Art
[0002] Wet paper-based friction material is a fiber composite material that works in an oil medium. It uses cellulose fiber or synthetic fiber as reinforcing fiber, adds friction performance modifiers and fillers, is formed by papermaking process, impregnated with adhesive resin, and hot-pressed and cured. Wet paper-based friction material has the advantages of high dynamic friction coefficient, static / dynamic friction coefficient ratio close to 1, strong torque transmission ability, low friction noise, gentle and smooth bonding process, good wear resistance and designable structure shape. It is widely used in transmission and braking devices of various vehicles and engineering machinery, such as wet clutch of automobile automatic transmission, motorcycle clutch and wet brake device of heavy vehicle.
[0003] Wet paper-based friction materials must have an appropriate and stable friction coefficient and good wear resistance. Wear resistance is directly related to the safety and service life of the product, and is also an important technical indicator for measuring the durability of friction materials. The better the wear resistance, the longer its service life. Chinese patent CN107326721A discloses a method for preparing a paper-based friction material with uniform pores. First, alumina, potassium feldspar and the like are mixed and ball-milled, and the obtained ball-milled powder is filled into a mold, and mixed short fibers are obtained by high-temperature melt drawing. Then, aluminum isopropoxide powder is mixed and dispersed with glacial acetic acid solution, and then silica sol is added and mixed with tetraethylammonium hydroxide and the like to obtain a modified mixed solution. The mixed short fibers are then added to the modified mixed solution, dispersed and dried, mixed with bamboo fiber and water, and placed on a paper forming device with a screen after delamination treatment. After drying, the phenolic resin ethanol solution is immersed, and after the immersion is completed, the paper-based friction material with uniform pores is obtained. The high-temperature melt drawing needs to be preheated for 25 to 30 minutes under a nitrogen protective atmosphere at 250 to 300°C, and then heated to 1750 to 1800°C at 15°C / min, and kept melted for 1 to 2 hours. After the insulation and melting are completed, the crucible leak is wired with a glass rod. The paper-based friction material prepared by the patent has the characteristics of high friction coefficient and good controllability of the void structure, and is an ideal friction material. However, the preparation steps of the paper-based friction material of the patent are complicated, and the high-temperature melting and drawing step requires a special high-temperature resistant device, which has high energy consumption and high production cost. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a highly wear-resistant wet paper-based friction material and a preparation method and application thereof. The preparation method provided by the present invention has simple steps, does not require the use of a dedicated high-temperature resistant device, has low energy consumption, and has low production cost.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a highly wear-resistant wet paper-based friction material, comprising the following steps:
[0007] mixing natural fibers, synthetic fibers, a friction property modifier and water to obtain a slurry;
[0008] Dehydrating the slurry, forming it, and then drying it to obtain base paper;
[0009] The base paper is dipped in a dipping solution and then dried to obtain dipped paper; the dipping solution comprises phenolic resin and nanocellulose;
[0010] The impregnated paper is hot-pressed and vulcanized to obtain a wet paper-based friction material with high wear resistance; the hot-pressed and vulcanized temperature is ≤230°C.
[0011] Preferably, the natural fiber includes one or more of hemp fiber, cotton fiber, bamboo fiber and wood pulp fiber;
[0012] The synthetic fiber includes one or more of aramid fiber, carbon fiber, glass fiber, ceramic fiber and polyimide fiber;
[0013] The mass ratio of the natural fiber to the synthetic fiber is 1:0.1-8.
[0014] Preferably, the friction performance modifier includes one or more of diatomaceous earth, silicon dioxide, feldspar, barium sulfate, graphite, aluminum oxide and organic friction powder;
[0015] The mass ratio of the natural fiber to the friction performance regulator is 1:0.1-12.
[0016] Preferably, the solid content of the slurry is 0.5-2.5%.
[0017] Preferably, the phenolic resin comprises one or more of unmodified phenolic resin, cashew nut shell oil modified phenolic resin, melamine modified phenolic resin, latex modified phenolic resin and boron modified phenolic resin;
[0018] The dry weight of the nanocellulose accounts for 0.01 to 5% of the dry weight of the phenolic resin;
[0019] The solid content of the dipping solution is 20-50%.
[0020] Preferably, the dipping time is 3 to 20 minutes.
[0021] Preferably, the temperature of the hot pressing vulcanization is 150-230° C., the pressure is 1-30 MPa, and the time is 1-30 min.
[0022] The present invention also provides a highly wear-resistant wet paper-based friction material prepared by the preparation method described in the above technical solution.
[0023] Preferably, the weight of the highly wear-resistant wet paper-based friction material is 100 to 2000 g / m 2 , thickness is 0.2~5mm.
[0024] The present invention also provides the use of the highly wear-resistant wet paper-based friction material described in the above technical solution in a wet clutch or a wet brake device.
[0025] The present invention mixes natural fiber, synthetic fiber, friction performance regulator and water, dehydrates and forms the obtained slurry, dries, immerses in glue, dries, and hot-presses and vulcanizes at a temperature below 230°C to obtain a wet paper-based friction material. The preparation method provided by the present invention has simple process and operation, the temperature in the entire preparation process does not exceed 230°C, the energy consumption is low, the reaction conditions are mild and easy to control, there is no need to use a special high-temperature resistant device, and the production cost is low. The preparation method provided by the present invention does not need to use highly flammable and toxic aluminum isopropoxide powder and flammable, toxic, and highly irritating tetraethylammonium hydroxide and di-n-propylamine chemical reagents, has high safety, and the raw materials are environmentally friendly and easy to obtain, and no organic toxic and harmful substances are discharged, and it is suitable for industrial production.
[0026] Moreover, nanocellulose is a fiber aggregate with a diameter of less than 100nm and a length of up to micrometer level obtained by treating the fiber by chemical, physical, biological or a combination of these methods. The surface contains a large number of hydroxyl groups, and has excellent mechanical properties, huge specific surface area, high crystallinity, high transparency, low density, good biodegradability and biocompatibility. Phenolic resin contains a large number of hydroxyl groups. The present invention uses a dipping solution of phenolic resin, nanocellulose and ethanol to dip the base paper. During the hot pressing vulcanization process, at least the following two chemical reactions occur: one is the polycondensation reaction between phenolic resin molecules, so that the linear small molecule phenolic resin is polymerized into a network macromolecular phenolic resin, which is the main chemical reaction in the heating and curing of conventional wet paper-based friction materials; the other is the etherification reaction between the hydroxyl groups on the surface of nanocellulose and the hydroxyl groups on the phenolic resin molecules, and the nanocellulose is introduced into the polymer to form a phenolic resin-nanocellulose-phenolic resin macromolecule, and the excellent mechanical properties of nanocellulose are used to improve the strength and flexibility of the phenolic resin, thereby increasing the wear resistance of the wet paper-based friction material and improving the friction and wear performance of the material. In addition, at the physical level, the large number of hydroxyl groups on the surface of nanocellulose form strong hydrogen bonds with the hydroxyl groups of the phenolic resin macromolecules, which can further improve the strength and wear resistance of the material. DETAILED DESCRIPTION
[0027] The present invention provides a method for preparing a highly wear-resistant wet paper-based friction material, comprising the following steps:
[0028] mixing natural fibers, synthetic fibers, a friction property modifier and water to obtain a slurry;
[0029] Dehydrating the slurry, forming it, and then drying it to obtain base paper;
[0030] The base paper is dipped in a dipping solution and then dried to obtain dipped paper; the dipping solution comprises phenolic resin and nanocellulose;
[0031] The impregnated paper is hot-pressed and vulcanized to obtain a wet paper-based friction material with high wear resistance; the hot-pressed and vulcanized temperature is ≤230°C.
[0032] Unless otherwise specified, the materials and equipment used in the present invention are all commercially available products in the art.
[0033] The invention mixes natural fiber, synthetic fiber, friction performance regulator and water to obtain slurry.
[0034] In the present invention, the natural fiber preferably includes one or more of hemp fiber, cotton fiber, bamboo fiber and wood pulp fiber, more preferably cotton fiber or hemp fiber-cotton fiber mixture, and the mass ratio of hemp fiber to cotton fiber in the hemp fiber-cotton fiber mixture is preferably 1:1. In the present invention, the diameter of the natural fiber is preferably 1-50 μm, more preferably 10-40 μm; the length of the natural fiber is preferably 0.2-10 mm, more preferably 0.5-5 mm.
[0035] In the present invention, the synthetic fiber preferably includes one or more of aramid fiber, carbon fiber, glass fiber, ceramic fiber and polyimide fiber. In the present invention, the diameter of the synthetic fiber is preferably 1 to 30 μm, more preferably 3 to 20 μm; the length of the synthetic fiber is preferably 0.1 to 10 mm, more preferably 0.3 to 5 mm. In the present invention, the synthetic fiber preferably includes a mixture of aramid fiber and carbon fiber, and the mass ratio of aramid fiber to carbon fiber in the mixture is preferably 8 to 13:7 to 8, more preferably 1:1 or 13:7.
[0036] In the present invention, the mass ratio of the natural fiber to the synthetic fiber is preferably 1:0.1-8, more preferably 1:1-6, further preferably 1:2-4, and specifically preferably 1:0.1, 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5 or 1:8.
[0037] In the present invention, the friction performance modifier preferably includes one or more of diatomite, silica, feldspar, barium sulfate, graphite, alumina and organic friction powder; the feldspar preferably includes one or more of sodium feldspar, calcium feldspar, potassium feldspar and barium feldspar; the organic friction powder preferably includes one or more of rubber powder, cashew nut shell oil friction powder, tire powder and amino ester powder. In the present invention, the friction performance modifier is more preferably the first composite friction performance modifier or the second composite friction performance modifier in terms of mass fraction; the first composite friction performance modifier preferably includes a mixture of diatomite, feldspar, graphite, rubber powder and cashew nut shell oil friction powder in a mass ratio of 15:5:6:30:20; the second composite friction performance modifier preferably includes a mixture of diatomite, feldspar, alumina, graphite and rubber powder in a mass ratio of 23:10:2:15:10. In the present invention, the particle size of the friction performance modifier is preferably 10-800 mesh, more preferably 20-350 mesh.
[0038] In the present invention, the mass ratio of the natural fiber to the friction performance regulator is preferably 1:0.1-12, more preferably 1:1-10, further preferably 1:2-8, and specifically preferably 1:0.1, 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5, 1:8, 1:8.5, 1:9, 1:9.5, 1:10, 1:10.5, 1:11, 1:11.5 or 1:12.
[0039] The present invention has no special limitation on the mixing, and a mixing method well known to those skilled in the art may be adopted, such as stirring and mixing.
[0040] In the present invention, the solid content of the slurry is preferably 0.5-2.5%, more preferably 1-2%, and further preferably 1.5%.
[0041] After obtaining the slurry, the present invention dehydrates the slurry, forms it, and then dries it to obtain base paper.
[0042] In the present invention, the dehydration forming preferably includes: pouring the slurry into a former or a sheet maker, vacuum dehydrating the slurry after it is evenly dispersed to obtain a first wet paper web, and pressing and dehydrating the first wet paper web to obtain a second wet paper web.
[0043] In the present invention, the vacuum degree of the vacuum dehydration is preferably 0.01 to 0.06 MPa, more preferably 0.02 to 0.05 MPa, and further preferably 0.03 to 0.04 MPa; the present invention has no special limitation on the time of the vacuum dehydration, and the solid content of the first wet paper web obtained by vacuum dehydration can be 10 to 25%, and the solid content is more preferably 15 to 20%. The time of the vacuum dehydration is specifically 3 to 300 s.
[0044] In the present invention, the squeezing dehydration is preferably performed on a press. In the present invention, the moisture content of the second wet paper web is preferably 25 to 50%, more preferably 30 to 45%, and further preferably 35 to 40%.
[0045] In the present invention, the drying temperature is preferably 70 to 110°C, more preferably 80 to 100°C, and further preferably 90 to 95°C; the drying time is preferably 3 to 600s, more preferably 50 to 500s, and further preferably 100 to 300s; the drying is preferably carried out in a drying cylinder, a vacuum dryer or an oven.
[0046] After the base paper is obtained, the base paper is dipped in a dipping solution and then dried to obtain the dipped paper; the dipping solution comprises phenolic resin and nanocellulose.
[0047] In the present invention, the phenolic resin preferably includes one or more of unmodified phenolic resin (pure phenolic resin), cashew nut shell oil modified phenolic resin, melamine modified phenolic resin, latex modified phenolic resin and boron modified phenolic resin; the present invention has no special limitation on the phenolic resin, and the phenolic resin is prepared by a commercial product well known to those skilled in the art or a preparation method well known to those skilled in the art. In a specific embodiment of the present invention, the phenolic resin is purchased from Shengquan Group.
[0048] In the present invention, the diameter of the nanocellulose is preferably <100nm, and the length is preferably micrometer-level, more preferably 10-100μm. In the present invention, the nanocellulose is preferably used in the form of nanocellulose dry powder or nanocellulose aqueous dispersion, and the solid content of the nanocellulose aqueous dispersion is preferably 1-6%, more preferably 2-5%, and further preferably 3-4%. In the present invention, the dry weight of the nanocellulose preferably accounts for 0.01-5% of the dry weight of the phenolic resin, more preferably 0.1-4.5%, further preferably 1-2%, and specifically preferably 0.01%, 0.05%, 0.1%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%.
[0049] The invention adds nanocellulose to the dipping solution, and during the subsequent hot pressing vulcanization, the nanocellulose reacts chemically with the phenolic resin to generate network composite macromolecules, thereby improving the strength and toughness of the phenolic resin, thereby improving the wear resistance of the wet paper-based friction material and improving the friction and wear performance of the wet paper-based friction material.
[0050] In the present invention, the solid content of the dipping solution is preferably 20-50%, more preferably 25-45%, further preferably 30-40%, and most preferably 35%. In the present invention, the solvent in the dipping solution is preferably ethanol.
[0051] In the present invention, the dipping solution is preferably obtained by mixing phenolic resin, nanocellulose and ethanol. In the present invention, the mixing temperature is preferably room temperature, the mixing time is preferably 5 to 90 minutes, more preferably 10 to 60 minutes, more preferably 15 to 45 minutes; the mixing method preferably includes stirring mixing and / or ultrasonic mixing, more preferably stirring mixing, or ultrasonic mixing first and then stirring mixing.
[0052] In the present invention, the dipping temperature is preferably room temperature, and the dipping time is preferably 3 to 20 minutes, more preferably 3 to 20 minutes, and further preferably 3 to 20 minutes.
[0053] In the present invention, the glue content of the dipstick is preferably 20-40%, more preferably 30-35%, specifically preferably 30.3%, 30.5%, 32.3% or 32.4%; wherein, glue content = (mass of wet paper-based friction material - mass of base paper) / mass of wet paper-based friction material × 100%.
[0054] After obtaining the impregnated paper, the present invention performs hot pressing vulcanization on the impregnated paper to obtain a wet paper-based friction material with high wear resistance; the temperature of the hot pressing vulcanization is ≤230°C.
[0055] In the present invention, the temperature of the hot press vulcanization is preferably 150 to 230° C., more preferably 180 to 220° C., and further preferably 200 to 210° C.; the pressure of the hot press vulcanization is preferably 1 to 30 MPa, more preferably 1.5 to 10 MPa, and further preferably 2 to 5 MPa; the time of the hot press vulcanization is preferably 1 to 30 min, more preferably 3 to 20 min, and further preferably 5 to 10 min; the hot press vulcanization is preferably carried out in a vulcanizer.
[0056] The present invention provides a highly wear-resistant wet paper-based friction material prepared by the preparation method described in the above technical solution.
[0057] In the present invention, the weight of the highly wear-resistant wet paper-based friction material is preferably 100 to 2000 g / m 2, more preferably 200 to 1500 g / m 2 , more preferably 300 to 1000 g / m 2 , preferably 342g / m 2 , 345g / m 2 , 407g / m 2 or 408g / m 2 The thickness of the highly wear-resistant wet paper-based friction material is preferably 0.2-5 mm, more preferably 0.25-2 mm, further preferably 0.3-1 mm, most preferably 0.35-0.5 mm, and specifically preferably 0.379 mm, 0.392 mm, 0.398 mm or 0.423 mm; the dynamic friction coefficient of the highly wear-resistant wet paper-based friction material is preferably ≥0.093, more preferably 0.093-0.110, specifically preferably 0.093, 0.104, 0.108 or 0.110; the static friction coefficient of the highly wear-resistant wet paper-based friction material is preferably ≥0.124, more preferably 0.124-0.142, specifically preferably 0.124, 0.133 or 0.142; the wear rate of the highly wear-resistant wet paper-based friction material is specifically preferably ≤3×10 -7 cm 2 / J, preferably 7×10 -8 cm 2 / J, 1×10 - 7 cm 2 / J or 3×10 -7 cm 2 / J.
[0058] The present invention provides the application of the highly wear-resistant wet paper-based friction material described in the above technical solution in a wet clutch or wet brake device. In the present invention, the highly wear-resistant wet paper-based friction material is preferably used in wet clutches or wet brake devices of various vehicles or engineering machinery, and is more preferably used in wet clutches of automobile automatic transmissions, motorcycle clutches or wet brake devices of heavy vehicles; the highly wear-resistant wet paper-based friction material preferably works in an oil medium. The present invention adds nanocellulose to the phenolic resin impregnation solution, and during the subsequent hot pressing vulcanization, the nanocellulose reacts chemically with the phenolic resin to produce a network composite macromolecule, thereby improving the strength and toughness of the phenolic resin, thereby improving the wear resistance of the wet paper-based friction material, and improving the friction and wear performance of the wet paper-based friction material, and has a good application prospect in wet clutches or wet brake devices of various vehicles or engineering machinery.
[0059] In order to further illustrate the present invention, a highly wear-resistant wet paper-based friction material provided by the present invention, a preparation method thereof and an application thereof are described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0060] In the following examples and comparative examples, the feldspar is potassium feldspar; the phenolic resin is the phenolic resin used for friction materials of Shengquan Group; the rubber powder is purchased from Cardolite Corporation; the diameter of the nanocellulose is <100 nm and the length is in the micron level.
[0061] Comparative Example 1
[0062] In terms of mass, 8 parts of cotton fiber, 8 parts of aramid fiber, 8 parts of carbon fiber, 15 parts of diatomaceous earth, 5 parts of feldspar, 6 parts of graphite, 30 parts of rubber powder, and 20 parts of cashew nut shell oil friction powder are uniformly dispersed with water to obtain a slurry with a solid content of 1.5%. The slurry is poured into a former, the slurry is uniformly dispersed, and vacuum dehydrated to a solid content of 10-25% under a vacuum degree of 0.01-0.06MPa, and then further dehydrated with a press to obtain a wet paper web with a moisture content of 40%, which is placed in a 95°C vacuum dryer for drying to obtain base paper. The base paper is placed in a phenolic resin ethanol solution with a solid content of 30%, dipped in glue at room temperature for 10 minutes, taken out, and dried at 105°C for 10 minutes to obtain dipped paper with a glue content of 29.7%. The dipped paper is hot-pressed and vulcanized on a vulcanizer at 200°C and 2MPa for 5 minutes to obtain a highly wear-resistant wet paper-based friction material. High wear resistance wet paper-based friction material with a basis weight of 408g / m 2 , thickness is 389μm.
[0063] The friction and wear properties of the wet paper-based friction material were tested using an MM2000 friction performance tester. Under the conditions of a speed of 2000 r / min and a pressure of 0.4 MPa, the dynamic friction coefficient of the wet paper-based friction material was 0.084 and the static friction coefficient was 0.095. After 2000 tests, the wear rate was 5×10 -7 cm 2 / J, meets the requirements of Class 2 and Class 3 products in the national standard GB / T37208-2018 non-metallic paper-based wet friction materials.
[0064] Comparative Example 2
[0065] In terms of mass, 10 parts of cotton fiber, 10 parts of hemp fiber, 13 parts of aramid fiber, 7 parts of carbon fiber, 23 parts of diatomaceous earth, 10 parts of feldspar, 2 parts of alumina, 15 parts of graphite, and 10 parts of rubber powder are uniformly dispersed with water to obtain a slurry with a solid content of 1.7%. The slurry is poured into a sheet maker, and after the slurry is uniformly dispersed, it is vacuum dehydrated under 0.01-0.06MPa to a solid content of 10-25%, and then further dehydrated with a press to obtain a wet paper web with a moisture content of 40%, which is placed in a 105°C drying cylinder to obtain base paper. The base paper is placed in a phenolic resin ethanol solution with a solid content of 34%, dipped in glue at room temperature for 15 minutes, taken out, and dried at 100°C for 30 minutes to obtain dipped paper with a glue content of 32.3%. The dipped paper is hot-pressed and vulcanized on a vulcanizer at 200°C and 4MPa for 3 minutes to obtain a highly wear-resistant wet paper-based friction material. High wear resistance wet paper-based friction material with a basis weight of 338g / m 2 , thickness is 391μm.
[0066] The friction and wear properties of the wet paper-based friction material were tested using an MM2000 friction performance tester. Under the conditions of a speed of 2000 r / min and a pressure of 0.4 MPa, the dynamic friction coefficient of the wet paper-based friction material was 0.095 and the static friction coefficient was 0.106. After 2000 tests, the wear rate was 2×10 -7 cm 2 / J, meets the requirements of Class 2 and Class 3 products in the national standard GB / T37208-2018 non-metallic paper-based wet friction materials.
[0067] Example 1
[0068] In terms of mass, 8 parts of cotton fiber, 8 parts of aramid fiber, 8 parts of carbon fiber, 15 parts of diatomaceous earth, 5 parts of feldspar, 6 parts of graphite, 30 parts of rubber powder, and 20 parts of cashew nut shell oil friction powder are uniformly dispersed with water to obtain a slurry with a solid content of 1.5%. The slurry is poured into a sheet maker, and after the slurry is uniformly dispersed, it is vacuum dehydrated to a solid content of 10-25% under 0.01-0.06MPa, and then further dehydrated with a press to obtain a wet paper web with a moisture content of 40%, which is placed in a 95°C vacuum dryer for drying to obtain base paper. A nanocellulose aqueous dispersion with a solid content of 4% is added to a phenolic resin ethanol solution with a solid content of 30%, and mechanically stirred at room temperature for 15 minutes to obtain a dipping solution. The base paper is dipped in the above dipping solution for 10 minutes at room temperature, taken out, and dried at 105°C for 10 minutes to obtain a dipped paper with a glue content of 30.3%. The impregnated paper was hot-pressed and vulcanized on a vulcanizer at 200°C and 2MPa for 5 minutes to obtain a highly wear-resistant wet paper-based friction material. The quantitative weight of the highly wear-resistant wet paper-based friction material is 407g / m 2, with a thickness of 398 μm. The dry weight of nanocellulose accounts for 0.5% of the dry weight of phenolic resin.
[0069] The friction and wear properties of the high wear-resistant wet paper-based friction material were tested by using an MM2000 friction performance tester. Under the conditions of a rotation speed of 2000 r / min and a pressure of 0.4 MPa, the dynamic friction coefficient of the high wear-resistant wet paper-based friction material was 0.093, which was 10.7% higher than that of comparative example 1; the static friction coefficient was 0.124, which was 30.5% higher than that of comparative example 1; after 2000 tests, the wear rate was 3×10 -7 cm 2 / J, which is 40% lower than that of comparative example 1. It meets the requirements of Class 2 and Class 3 products in the national standard GB / T37208-2018 non-metallic paper-based wet friction materials.
[0070] Example 2
[0071] In terms of mass fraction, 8 parts of cotton fiber, 8 parts of aramid fiber, 8 parts of carbon fiber, 15 parts of diatomaceous earth, 5 parts of feldspar, 6 parts of graphite, 30 parts of rubber powder, and 20 parts of cashew nut shell oil friction powder are uniformly dispersed with water to obtain a slurry with a solid content of 1.7%. The slurry is poured into a sheet maker, and after the slurry is uniformly dispersed, it is dehydrated to a solid content of 10-25% under a small vacuum condition of 0.01-0.06MPa, and then further dehydrated with a press to obtain a wet paper web with a moisture content of 40%, which is placed in a 95°C vacuum dryer for drying to obtain base paper. A nanocellulose aqueous dispersion with a solid content of 4% is added to a phenolic resin ethanol solution with a solid content of 30%, and mechanically stirred at room temperature for 30 minutes to obtain a dipping solution. The base paper is dipped in the above dipping solution for 10 minutes at room temperature, taken out, and dried at 105°C for 10 minutes to obtain a dipped paper with a glue content of 30.5%. The impregnated paper was hot-pressed and vulcanized on a vulcanizer at 200°C and 2MPa for 5 minutes to obtain a highly wear-resistant wet paper-based friction material. The quantitative weight of the highly wear-resistant wet paper-based friction material is 408g / m 2 , with a thickness of 423 μm. The dry weight of nanocellulose accounts for 1% of the dry weight of phenolic resin.
[0072] The friction and wear properties of the high wear-resistant wet paper-based friction material were tested using an MM2000 friction performance tester. Under the conditions of a rotation speed of 2000 r / min and a pressure of 0.4 MPa, the dynamic friction coefficient of the high wear-resistant wet paper-based friction material was 0.104, which was 23.9% higher than that of comparative example 1; the static friction coefficient was 0.133, which was 40% higher than that of comparative example 1; after 2000 tests, the wear rate was 1×10 -7 cm 2 / J, which is reduced by 80% compared with comparative example 1. It meets the requirements of Class 2 and Class 3 products in the national standard GB / T37208-2018 non-metallic paper-based wet friction materials.
[0073] Example 3
[0074] In terms of mass, 10 parts of cotton fiber, 10 parts of hemp fiber, 13 parts of aramid fiber, 7 parts of carbon fiber, 23 parts of diatomaceous earth, 10 parts of feldspar, 2 parts of alumina, 15 parts of graphite, and 10 parts of rubber powder are uniformly dispersed with water to obtain a slurry with a solid content of 1.9%. The slurry is poured into a sheet maker, and after the slurry is uniformly dispersed, it is vacuum dehydrated under 0.01-0.06MPa to a solid content of 10-25%, and then further dehydrated with a press to obtain a wet paper web with a moisture content of 42%, which is placed in a 105°C drying cylinder for drying to obtain base paper. A nanocellulose aqueous dispersion with a solid content of 4% is added to a phenolic resin ethanol solution with a solid content of 34%, and mechanically stirred at room temperature for 30 minutes to obtain a dipping solution. The base paper is dipped in the above dipping solution for 15 minutes at room temperature, taken out, and dried at 100°C for 30 minutes to obtain a dipped paper with a glue content of 32.4%. The impregnated paper was hot-pressed and vulcanized on a vulcanizer at 200°C and 4MPa for 3 minutes to obtain a highly wear-resistant wet paper-based friction material. The quantitative weight of the highly wear-resistant wet paper-based friction material is 342g / m 2 , with a thickness of 392 μm. The dry weight of nanocellulose accounts for 0.05% of the dry weight of phenolic resin.
[0075] The friction and wear properties of the high wear-resistant wet paper-based friction material were tested by using an MM2000 friction performance tester. Under the conditions of a rotation speed of 2000 r / min and a pressure of 0.4 MPa, the dynamic friction coefficient of the high wear-resistant wet paper-based friction material was 0.108, which was 13.7% higher than that of comparative example 2; the static friction coefficient was 0.133, which was 25.5% higher than that of comparative example 2; after 2000 tests, the wear rate was 1×10 -7 cm 2 / J, which is 50% lower than that of comparative example 2. It meets the requirements of Class 2 and Class 3 products in the national standard GB / T37208-2018 non-metallic paper-based wet friction materials.
[0076] Example 4
[0077] In terms of mass, 10 parts of cotton fiber, 10 parts of hemp fiber, 13 parts of aramid fiber, 7 parts of carbon fiber, 23 parts of diatomaceous earth, 10 parts of feldspar, 2 parts of alumina, 15 parts of graphite, and 10 parts of rubber powder are uniformly dispersed with water to obtain a slurry with a solid content of 1.8%. The slurry is poured into a sheet maker, and after the slurry is uniformly dispersed, it is vacuum dehydrated under 0.01-0.06MPa to a solid content of 10-25%, and then further dehydrated with a press to obtain a wet paper web with a moisture content of 41%, which is placed in a 105°C drying cylinder to obtain base paper. Nanocellulose powder is added to a phenolic resin ethanol solution with a solid content of 34%, first ultrasonically treated for 15 minutes, and then mechanically stirred for 30 minutes to obtain a dipping solution. The base paper is dipped in the above dipping solution at room temperature for 15 minutes, taken out, and dried at 100°C for 30 minutes to obtain a dipped paper with a glue content of 32.3%. The impregnated paper was hot-pressed and vulcanized on a vulcanizer at 200°C and 4MPa for 3 minutes to obtain a highly wear-resistant wet paper-based friction material. The quantitative weight of the highly wear-resistant wet paper-based friction material is 345g / m 2 , with a thickness of 379 μm. The dry weight of nanocellulose accounts for 0.1% of the dry weight of phenolic resin.
[0078] The friction and wear properties of the high wear-resistant wet paper-based friction material were tested by using an MM2000 friction performance tester. Under the conditions of a rotation speed of 2000 r / min and a pressure of 0.4 MPa, the dynamic friction coefficient of the high wear-resistant wet paper-based friction material was 0.110, which was 15.8% higher than that of comparative example 2; the static friction coefficient was 0.142, which was 34% higher than that of comparative example 2; after 2000 tests, the wear rate was 7×10 -8 cm 2 / J, which is 65% lower than that of comparative example 2. It meets the requirements of Class 2 and Class 3 products in the national standard GB / T37208-2018 non-metallic paper-based wet friction materials.
[0079] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a highly wear-resistant wet paper-based friction material, comprising the following steps: mixing natural fibers, synthetic fibers, a friction modifier, and water to obtain a slurry; Dehydrating the slurry to obtain base paper after forming it into a shape and drying it; The base paper is impregnated in an impregnation solution and then dried to obtain impregnated paper; the impregnation solution comprises phenolic resin and nanocellulose; The impregnated paper is hot-pressed and vulcanized to obtain a wet paper-based friction material with high wear resistance; the hot-pressed and vulcanized temperature is ≤230°C.
2. The highly wear-resistant wet paper-based friction material according to claim 1, characterized in that: The natural fibers include one or more of hemp fibers, cotton fibers, bamboo fibers and wood pulp fibers; The synthetic fiber includes one or more of aramid fiber, carbon fiber, glass fiber, ceramic fiber and polyimide fiber; The mass ratio of the natural fiber to the synthetic fiber is 1:0.1-8.
3. The preparation method according to claim 1, characterized in that The friction performance modifier includes one or more of diatomaceous earth, silicon dioxide, feldspar, barium sulfate, graphite, aluminum oxide and organic friction powder; The mass ratio of the natural fiber to the friction performance regulator is 1:0.1-12.
4. The preparation method according to any one of claims 1 to 3, characterized in that The solid content of the slurry is 0.5-2.5%.
5. The preparation method according to claim 1, characterized in that The phenolic resin includes one or more of unmodified phenolic resin, cashew nut shell liquid modified phenolic resin, melamine modified phenolic resin, latex modified phenolic resin and boron modified phenolic resin; The dry weight of the nanocellulose accounts for 0.01 to 5% of the dry weight of the phenolic resin; The solid content of the dipping solution is 20-50%.
6. The preparation method according to claim 1, characterized in that The dipping time is 3 to 20 minutes.
7. The preparation method according to claim 1, characterized in that The temperature of the hot pressing vulcanization is 150-230° C., the pressure is 1-30 MPa, and the time is 1-30 minutes.
8. A highly wear-resistant wet paper-based friction material prepared by the preparation method according to any one of claims 1 to 7.
9. The preparation method according to claim 8, characterized in that The quantitative weight of the highly wear-resistant wet paper-based friction material is 100 to 2000 g / m 2 , thickness is 0.2~5mm.
10. Use of the highly wear-resistant wet paper-based friction material according to claim 8 or 9 in a wet clutch or wet brake device.
Citation Information
Patent Citations
Wet type paper-based friction material as well as preparation method and application thereof
CN102002883A
Phenol resin composite material and method for producing the same
JP2008248092A
Cited By
Production process of nanofiber composite impregnated paper
CN120486164A
A production process of nanofiber composite impregnated paper
CN120486164B