Specific positive electrodes with a specific salt for an alkali metal ion battery

DE602022006852T2Active Publication Date: 2024-10-16COMMISSARIAT A LENERGIE ATOMIQUE ET AUX ENERGIES ALTERNATIVES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE602022006852
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-12-09
Filing Date
2022-11-28
Publication Date
2024-10-16
Estimated Expiration
2042-11-28

AI Technical Summary

Technical Problem

Alkaline metal-ion accumulators face significant irreversible capacity loss during the first charge due to the formation of a passivation layer on the negative electrode, which reduces their energy density, and existing solutions like prelithiation techniques and sacrificial salts generate excessive gaseous by-products or require complex setups.

Method used

A positive electrode comprising an alkali metal salt of specific formula (I) that decomposes during the first charge to form a passivation layer on the negative electrode, providing lithium ions while minimizing gaseous by-products and allowing for efficient energy storage, with the electrode also acting as an ion reserve during the accumulator's life.

Benefits of technology

The solution achieves superior theoretical and practical capacities with reduced gaseous by-products, maintaining the structural integrity of the positive electrode and minimizing unnecessary material, thus enhancing the energy density and longevity of the accumulator.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to specific positive electrodes comprising a specific salt for an alkali metal-ion type battery, alkali metal-ion type batteries comprising this type of electrodes, a method for treating such batteries and the use of said specific salt as a sacrificial salt during the first charge of these batteries.

[0002] Alkali metal-ion batteries are expected to be increasingly used as a stand-alone power source, particularly in portable electronic equipment (such as mobile phones, laptops, tools), gradually replacing nickel-cadmium (NiCd) and nickel-metal hydride (NiMH) batteries. They can also be used to provide the power supply needed for new micro-applications, such as smart cards, sensors, or other electromechanical systems.

[0003] From the point of view of their operation, these accumulators work according to the principle of insertion-deinsertion of the alkaline ion concerned (such as lithium, for lithium-ion accumulators, sodium for sodium-ion accumulators or potassium for potassium-ion accumulators).

[0004] When the battery is discharged, the alkali metal released from the negative electrode in ionic form migrates through the ion-conducting electrolyte and becomes intercalated in the crystal lattice of the active material of the positive electrode. The passage of each alkali ion in the internal circuit of the battery is exactly compensated by the passage of an electron in the external circuit, thus generating an electric current.

[0005] On the other hand, when charging the accumulator, the reactions occurring within the accumulator are the reverse reactions of the discharge, namely that: the negative electrode will insert the alkali metal in ionic form into the network of the insertion material constituting it; the positive electrode will release the alkali metal in ionic form, which will be intercalated into the insertion material of the negative electrode.

[0006] During the first charge of the accumulator, when the active material of the negative electrode is brought to an insertion potential of the alkali metal, a part of it will react with the electrolyte on the surface of the grains of active material of the negative electrode to form a passivation layer on its surface. The formation of this passivation layer consumes a significant quantity of alkali ions, which results in an irreversible loss of capacity of the accumulator (this loss being called irreversible capacity), because the reacted alkali ions are no longer available for subsequent charge / discharge cycles.

[0007] It is therefore advisable to minimize this loss as much as possible during the first charge, so that the energy density of the accumulator is as high as possible.

[0008] To do this, two types of techniques have been proposed in the prior art for lithium-ion type accumulators to overcome the aforementioned drawback: negative electrode prelithiation techniques; or positive electrode overlithiation techniques.

[0009] Concerning the negative electrode prelithiation techniques, we can cite: the so-called "techniques" in situ» consisting of depositing metallic lithium (i.e. in oxidation state “0”) on the negative electrode either in the form of a metal foil (as described in WO 1997031401) or in the form of a metallic lithium powder stabilized by a protective layer (as described in Electrochemistry Communications 13 (2011) 664-667) mixed with the ink comprising the ingredients of the negative electrode (i.e., the active material, the electronic conductors and an organic binder), the insertion of lithium being done, independently of the alternative chosen, spontaneously by a corrosion phenomenon; the techniques called “ ex situ» consisting of electrochemically prelithing the negative electrode, by placing it in a setup comprising an electrolytic bath and a counter-electrode comprising lithium, these techniques make it possible to control the quantity of lithium introduced into the negative electrode but nevertheless have the disadvantage of requiring the installation of a heavy experimental setup.

[0010] Alternatively, techniques for overlithiation of the positive electrode have also been proposed in the prior art, in particular by adding to the composition comprising the constituent ingredients of the positive electrode, a sacrificial salt which, during the first charge, will decompose and provide the necessary quantity of Li to form the passivation layer on the surface of the negative electrode.

[0011] In these techniques, it should be noted that the sacrificial salt must be able to decompose at a potential located in the potential window that the positive electrode sweeps during the first charge of the formation cycle

[0012] Also, when the first charge of the formation cycle takes place, when we take lithium accumulators as an example, two simultaneous electrochemical reactions generate Li +< ions, which are the disinsertion of lithium from the positive electrode and the decomposition of the sacrificial salt.

[0013] These techniques are notably described in WO99 / 28984, which describes two families of lithium salts that can be used as sacrificial salts of lithium oxocarbons / dicarboxylates and lithium azides / oxyhydrazides, these salts being able to be decomposed by high potential oxidation (between 3V and 5V vs Li + < / Li) by generating COz and N 2 on the one hand and lithium ions available for the system on the other hand.

[0014] WO2017 / 067994 A1, WO 2017 / 067996 A1, WO 2011 / 157958 A1 and D. Shanmukaraj et al. in "Electrochemistry Communications", vol. 12, no. 10, July 18, 2010 (2010-07-18), pages 1344-1347, all disclose methods for preparing sodium-ion or lithium-ion type accumulators, comprising a positive electrode and a negative electrode arranged on either side of an electrolyte, these methods comprising a step of forming a passivation layer on the surface of the negative electrode with sodium or lithium ions resulting from the decomposition of a specific salt of the corresponding metal by applying a first charge. The specific salts used in these documents are organic salts of alkali metals, such as oxocarbons or dicarboxylates, or azides or oxyhydrazides.

[0015] US 2017 / 365882 A1 describes a lithium-ion battery comprising a positive electrode, a negative electrode, a nanoporous or mesoporous polymer separator arranged between the two electrodes, and one or more chelating agents intended to complex the transition metal ions possibly released during operation of the battery, these complexing agents possibly being present in the electrolyte solution, within the separator or on the surface of one of the electrodes of the battery. Among the chelating agents used, salts of polycarboxylic acids, such as for example lithium nitrilotriacetate (Li 3 NTA) or sodium nitrilotriacetate (Na 3 NTA), are mentioned.

[0016] In view of what already exists, the authors therefore proposed to develop new positive electrodes comprising a specific salt which can allow the efficient formation of a passivation layer on the surface of the negative electrode during the formation cycle or which can serve as an ion reserve during the life of the accumulator, in which the electrode will be incorporated. Furthermore, the specific salt used will decompose at potentials similar to those already used in the prior art but with higher theoretical and practical capacities while generating fewer gaseous by-products. STATEMENT OF THE INVENTION

[0017] Thus, the invention relates to a positive electrode for an alkali metal-ion accumulator comprising at least one organic binder and at least one alkali metal salt corresponding to the following formula (I): in which the X represents an alkaline element.

[0018] By positive electrode, we specify, classically, in what precedes and what follows, that it is the electrode which acts as cathode, when the generator delivers current (that is to say when it is in the process of discharging) and which acts as an anode when the generator is in the process of charging.

[0019] The authors of the invention were able to demonstrate that this type of salt present in a positive electrode for an alkali metal-ion accumulator, once it has been incorporated into an accumulator and the accumulator has been subjected to the first charge of the formation cycle, could act as a sacrificial salt with higher theoretical and practical capacities (therefore releasing more lithium per gram) while generating fewer gaseous by-products, the elimination of which proves to be difficult during said formation cycle compared to structurally similar salts such as those illustrated in comparative examples 1 and 2 below. Furthermore, this alkali metal salt can be used as an ion reserve during the life of the accumulator or to make the electrode work on a particular capacity range.

[0020] As mentioned above, the alkali metal salt has the following formula (I): in which the X represents an alkaline element.

[0021] The Xs may represent, in particular, the element lithium (in particular when the electrode is intended for a lithium-ion accumulator), the element sodium (in particular when the electrode is intended for a sodium-ion accumulator) or the element potassium (in particular when the electrode is intended for a potassium-ion accumulator).

[0022] The electrode also comprises at least one organic binder, preferably a polymeric binder, such as: *fluorinated (co)polymers, such as polytetrafluoroethylene (known as PTFE), polyvinylidene fluoride (known as PVDF), poly(vinylidene fluoride-co-hexafluoropropene) (known as PVDF-HFP); *elastomeric polymers, such as styrenebutadiene copolymer (known as SBR), ethylene-propylene-diene monomer copolymer (known as EPDM); *polymers of the polyvinyl alcohol family; *cellulosic polymers, such as carboxymethylcellulose (known as CMC); *polymers of the poly(meth)acrylate family, such as polymethyl methacrylate (known as PMMA); *polymers of the polyacrylic acid family (known by the abbreviation PAA); and *mixtures thereof.

[0023] Furthermore, the electrode may comprise at least one electronically conductive additive, i.e. an additive capable of giving the electrode, in which it is incorporated, electronic conductivity, this additive being able to be, for example, chosen from carbon materials such as carbon black, carbon nanotubes, carbon fibers (in particular, carbon fibers obtained in the vapor phase known by the abbreviation VGCF), graphite in powder form, graphite fibers, graphene and mixtures thereof.

[0024] Furthermore, in addition to the other ingredients already mentioned above, the electrode may further advantageously comprise at least one active electrode material, namely a material capable of intercalating or deintercalating alkaline ions such as lithium ions, when the accumulator is a lithium-ion accumulator; sodium ions, when the accumulator is a sodium-ion accumulator; potassium ions, when the accumulator is a potassium-ion accumulator.

[0025] When the positive electrode is intended for a lithium accumulator, the active electrode material can be chosen from: metal chalcogenides of formula LiMQ 2 , in which M is at least one metallic element selected from metallic elements, such as Co, Ni, Fe, Mn, Cr, V, Al and Q is a chalcogen, such as O or S, the preferred metal chalcogenides being those of formula LiMO 2 , with M being as defined above, such as, preferably, LiCoO 2 , LiNiO 2 , LiNi x Co 1-x O 2 (with 0 <x<1), un matériau à base de lithium-nickel-manganèse-cobalt LiNi x Mn y Co z O 2 avec x+y+z=1 (connu également sous l'abréviation NMC), tel que LiNi 0 , 33 Mn 0 , 33 Co 0 , 33 O 2 , ou un matériau à base de lithium-nickel-cobalt-aluminium LiNi x Co y Al z O 2 avec x+y+z = 1 (connu également sous l'abréviation NCA), tel que LiNi 0 , 8 CO 0 , 15 Al 0 , 05 O 2 ; des chalcogénures de structure spinelle, tels que LiMn 2 O 4 ;lithiated or partially lithiated materials of formula M 1 M 2 (JO 4 ) f E 1-f , in which M 1 is lithium, which may be partially substituted by another alkali element at a substitution rate of less than 20%, M 2 is a transition metal element of oxidation state +2 selected from Fe, Mn, Ni and combinations thereof, which may be partially substituted by one or more other additional metal elements of oxidation state(s) between +1 and +5 at a substitution rate of less than 35%, JO 4 is an oxyanion in which J is selected from P, S, V, Si, Nb, Mo and combinations thereof, E is a fluoride, hydroxide or chloride anion, f is the mole fraction of the JO 4 oxyanion and is generally between 0.75 and 1 (including 0.75 and 1). ;

[0026] More specifically, lithiated or partially lithiated materials may be phosphorus-based (meaning, in other words, that the oxyanion has the formula PO 4 ) and may have an ordered or modified olivine-type structure.

[0027] The lithiated or partially lithiated materials may have the specific formula Li 3-x M' y M'' 2-y (JO 4 ) 3 , in which 0≤x≤3, 0≤y≤2, M' and M" represent identical or different metallic elements, at least one of M' and M" being a transition metallic element, JO 4 is preferably PO 4 , which may be partially substituted by another oxyanion with J being selected from S, V, Si, Nb, Mo and combinations thereof.

[0028] Lithiated or partially lithiated materials may have the formula Li(Fe x Mn 1 - x )PO 4 , where 0≤x≤1 and, preferably, x is equal to 1 (which means, in other words, that the corresponding material is LiFePO 4 ).

[0029] The positive electrodes may consist exclusively of at least one alkali metal salt of formula (I) as defined above, at least one organic binder, such as a polymeric binder and optionally at least one electronically conductive additive as defined above. Such electrodes may be used in a device of the accumulator type in order to pre-alkalize a negative electrode, this negative electrode, once the pre-alkalization operation has been carried out, being able to then be extracted from said device and incorporated into an alkali metal-ion accumulator.

[0030] The positive electrodes may also consist exclusively of at least one alkali metal salt of formula (I) as defined above, at least one organic binder, such as a polymeric binder, at least one active material as defined above and optionally at least one electronically conductive additive as defined above, in which case they may act as a permanent electrode in an accumulator and serve to form the passivation layer during the first charge applied to the accumulator.

[0031] According to a first embodiment, the electrodes of the invention may thus be presented, from the point of their constitution, in the form of a part, for example, parallelepiped or in the form of a pellet, comprising a composite material comprising a polymer matrix constituted by one or more polymer binders (for example, one or more specific polymer binders as defined above) and comprising, as fillers, at least one alkali metal salt of formula (I) as defined above and, optionally, at least one active material, as defined above and optionally one or more electronically conductive additives, such as those defined above.A specific electrode in accordance with this first embodiment may be an electrode made of a composite material comprising a polymer matrix made of PVDF and comprising, as fillers, an alkali metal salt of formula (I) as defined above, an active material as defined above and an electronically conductive additive, such as carbon black (for example, SuperP ®< ).

[0032] According to a second embodiment, when the electrodes comprise, in addition to the other ingredients, at least one active electrode material, the electrodes of the invention may be in the form of a first part comprising a composite material comprising a polymer matrix consisting of one or more polymer binders (for example, one or more specific polymer binders as defined above) and comprising, as fillers, at least one active material and, optionally, one or more electronically conductive additives, such as those defined above and a second part, in the form of a layer deposited on the surface of the first part, said layer comprising a polymer matrix consisting of one or more polymer binders (for example, one or more specific polymer binders as defined above) and comprising, as filler, at least one alkali metal salt of formula (I) as defined above.With such an embodiment, at the end of the first charge of the formation cycle, the layer comprising the alkali metal salt decomposes, in whole or in part, to give the alkali ions necessary for the formation of the passivation layer on the negative electrode, without this disrupting the internal structure of the positive electrode, the latter, at the end of the first charge, having a structural organization similar to that of a conventional electrode, in particular without the appearance of dead volume and loss of active material.On the other hand, unlike the embodiments of the art, where the sacrificial salt is introduced directly into the precursor composition of the positive electrode and where it is necessary to include a quantity of salt greater than that necessary for the formation of the passivation layer due to the impossibility of controlling the placement of the salt grains in the structure of the electrode, the method of the invention gives the possibility of using, due to the localization of the alkali salt just at the surface of the positive electrode, only the quantity sufficient for the formation of the passivation layer on the negative electrode. In this case, there is therefore no excess salt in the positive electrode after formation of the passivation layer and therefore no unnecessary material therein.

[0033] The positive electrodes are advantageously in contact with a current collector, for example, an aluminum strip.

[0034] The positive electrodes of the invention are intended to be incorporated into an alkali metal-ion accumulator cell, which is also one of the objects of the invention and thus comprises a positive electrode as defined above, a negative electrode and an electrolyte disposed between the positive electrode and the negative electrode.

[0035] It is specified that, by negative electrode, we mean, classically, in what precedes and what follows, the electrode which acts as an anode, when the generator delivers current (that is to say when it is in the process of discharging) and which acts as cathode, when the generator is in the process of charging.

[0036] Conventionally, the negative electrode comprises, as active electrode material, a material capable of reversibly inserting alkaline ions (such as lithium ions, when the accumulator is a lithium-ion accumulator; sodium ions, when the accumulator is a sodium-ion accumulator; potassium ions, when the accumulator is a potassium-ion accumulator.

[0037] When the negative electrode is intended for a lithium accumulator, the negative electrode active material can be chosen from: carbonaceous materials, such as graphitic carbon capable of intercalating lithium which may exist, typically, in the form of a powder, flakes, fibers or spheres (for example, mesocarbon microbeads); silicon-based compounds, such as silicon carbide SiC or silicon oxide SiO x; metallic lithium; lithium alloys, such as those described in US 6203944 and / or WO 00 / 03444; lithiated titanium oxides, such as an oxide of formula Li(4-x)MxTi5O12 or Li4MyTi(5-y)O12 wherein x and y are from 0 to 0.2, M represents an element selected from Na, K, Mg, Nb, Al, Ni, Co, Zr, Cr, Mn, Fe, Cu, Zn, Si and Mo, a specific example being Li4Ti5O12, these oxides being lithium insertion materials exhibiting a low level of physical expansion after inserting lithium; non-lithiated titanium oxides, such as TiO2;oxides of formula M y Ti( 5-y )O 12 in which y ranges from 0 to 0.2 and M is an element selected from Na, K, Mg, Nb, Al, Ni, Co, Zr, Cr, Mn, Fe, Cu, Zn, Si and Mo; lithium-germanium alloys, such as those comprising crystalline phases of formula Li 4.4 Ge; or a mixture thereof, such as a mixture comprising graphite and a silicon-based compound. ;

[0038] Furthermore, in the same way as for the positive electrode, the negative electrode may comprise an organic binder, such as a polymeric binder, such as polyvinylidene fluoride (PVDF), a carboxymethylcellulose mixture with a latex of the styrene and / or butadiene type as well as possibly one or more electrically conductive additives, which may be carbon materials, such as carbon black. Furthermore, in the same way as for the positive electrode, the negative electrode may be presented, from a structural point of view, as a composite material comprising a matrix of polymeric binder(s) within which are dispersed fillers consisting of the active material (presented, for example, in particulate form) and possibly the electrically conductive additive(s), said composite material being able to be deposited on a current collector.

[0039] The electrolyte disposed between the positive electrode and the negative electrode may be a liquid electrolyte conducting alkali ions, which may comprise (or even consist of) at least one organic solvent and at least one metal salt and possibly a compound from the family of vinyl compounds.

[0040] The organic solvent(s) may be carbonate solvents and, more specifically: cyclic carbonate solvents, such as ethylene carbonate (symbolized by the abbreviation EC), propylene carbonate (symbolized by the abbreviation PC), butylene carbonate, vinylene carbonate, fluoroethylene carbonate, fluoropropylene carbonate and mixtures thereof; linear carbonate solvents, such as diethyl carbonate (symbolized by the abbreviation DEC), dimethyl carbonate (symbolized by the abbreviation DMC), ethylmethyl carbonate (symbolized by the abbreviation EMC) and mixtures thereof.

[0041] The organic solvent(s) may also be ester solvents (such as ethyl propionate, n-propyl propionate), nitrile solvents (such as acetonitrile) or ether solvents (such as dimethyl ether, 1,2-dimethoxyethane).

[0042] The metal salt(s) may be chosen from salts of the following formulae: Mel, Me(PF 6 ) n , Me(BF 4 )n, Me(ClO 4 ) n , Me(bis(oxalato)borate) n (which may be designated by the abbreviation Me(BOB) n ), MeCF 3 SO 3 , Me[N(FSO 2 ) 2 ] n , Me[N(CF 3 SO 2 ) 2 ] n , Me[N(C 2 F 5 SO 2 ) 2 ] n , Me[N(CF 3 SO 2 )(RF SO 2 )] n , in which RF is a group -C 2 F 5 , -C 4 F 9 or -CF 3 OCF 2 CF 3 , Me(AsF 6 ) n , Me[C(CF 3 SO 2 ) 3 ] n , Me 2 S n , Me(C 6 F 3 N 4 ) (C 6 F 3 N 4 corresponding to 4,5-dicyano-2-(trifluoromethyl)imidazole and, when Me is Li, the salt corresponds to lithium 4,5-dicyano-2-(trifluoromethyl)imidazole, this salt being known by the abbreviation LiTDI), in which Me is a metallic element and, preferably, a metallic transition element, an alkali element or an alkaline-earth element and, more preferably, Me is Li (in particular, when the accumulator of the invention is a lithium-ion or lithium-air accumulator), Na (in particular,when the accumulator is a sodium-ion accumulator), K (in particular, when the accumulator is a potassium-ion accumulator).,

[0043] When Me is Li, the salt is preferably LiPF 6 .

[0044] The concentration of the metal salt in the liquid electrolyte is advantageously at least 0.01 M, preferably at least 0.025 M and more preferably at least 0.05 M and advantageously at most 5 M, preferably at most 2 M and more preferably at most 1 M.

[0045] A liquid electrolyte that can be used in the accumulators of the invention, in particular when it is a lithium-ion accumulator, is an electrolyte comprising a mixture of carbonate solvents (for example, a mixture of cyclic carbonate solvents, such as a mixture of ethylene carbonate and propylene carbonate and present, for example, in identical volume), a lithium salt, for example, LiPF 6 (for example, 1M).

[0046] The liquid electrolyte may be included within a separator disposed between the positive electrode and the negative electrode, said separator being able to consist of a porous polymeric membrane, such as a polyolefin membrane(s).

[0047] Finally, the invention relates to a method for treating the accumulator cell as defined above comprising a step of forming a passivation layer on the surface of the negative electrode with the X ions resulting from the decomposition of the alkali metal salt of formula (I) as defined above by applying a first charge to the aforementioned cell. It is understood that the X ions are alkali ions resulting directly from the X of the alkali metal salt of formula (I).

[0048] In other words, the first charge is applied under potential conditions necessary for the decomposition of the alkali metal salt present at the positive electrode, this decomposition resulting in a release of alkali ions, which will contribute to the formation of the passivation layer on the surface of the negative electrode. Because the alkali salt provides the alkali ions necessary for the formation of the passivation layer, this salt can thus be called a "sacrificial salt".

[0049] Also, when the positive electrode further comprises at least one active electrode material, the alkali ions necessary for the formation of the passivation layer do not come from said active material of the positive electrode. The alkali ions of the active material of the positive electrode are therefore not lost for the formation of this layer during the first charge and therefore the loss of capacity of the accumulator is reduced or even zero.

[0050] The cell according to the invention is subjected, in accordance with the method of the invention, to a first charging step under potential conditions necessary for the decomposition of the alkali metal salt included in the positive electrode, the decomposition materializing by the release of alkali ions, which will participate in the formation of the passivation layer.

[0051] Also, from a practical point of view, it is understood that the alkali metal salt must be able to decompose within a potential window that the positive electrode can withstand during the first charge.

[0052] Thus, when the first charge is carried out, in addition to the accumulator cell being charged, a decomposition reaction of the alkali metal salt also takes place. During this reaction, the alkali metal salt produces alkali ions which pass into the electrolyte and react with it to form the passivation layer on the active material particles of the negative electrode. In addition to the release of alkali ions, the decomposition of the salt results in the production of a small amount of gaseous compounds. These may be soluble in the electrolyte and can, if necessary, be removed during a degassing step.

[0053] Finally, the invention relates to the use of a salt of the following formula (I): wherein X represents an alkali element as a sacrificial salt for the formation of a passivation layer on the surface of a negative electrode of an alkali metal-ion accumulator, which further comprises a positive electrode comprising said salt and an electrolyte disposed between the positive electrode and the negative electrode.

[0054] Other characteristics and advantages of the invention will appear from the additional description which follows and which relates to particular embodiments.

[0055] Of course, this additional description is given only as an illustration of the invention and in no way constitutes a limitation thereof. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] [ Fig. 1] is a graph illustrating the evolution of the voltage U (in V vs Li +< / Li) as a function of the specific capacity C (in mAh / g), curve a) being representative of the battery obtained with the composite electrode comprising the salt of example 1, curve b) being representative of the battery obtained with the composite electrode comprising the salt of comparative example 1 and curve c) being representative of the battery obtained with the composite electrode comprising the salt of comparative example 2. [ Fig. 2] is a graph illustrating, for a cell obtained with the electrode comprising the salt of example 1, the evolution of the voltage U (in V vs Li +< / Li) as a function of the specific capacity C (in mAh / g) with curve a) being representative of the electrode comprising the salt of example 1 during the first charge, curve b) being representative of the counter-electrode based on Li4Ti5O 12 during the first charge and curve c) being representative of the counter-electrode based on Li 4 Ti 5 O 12 during the second discharge. DETAILED DESCRIPTION OF SPECIFIC EMBODIMENTS EXAMPLE 1

[0057] This example illustrates the preparation of a lithium salt which can be used for the preparation of a positive electrode in accordance with the invention, this lithium salt corresponding to the following formula:

[0058] Nitriloacetic acid (1 g) is dispersed in 50 mL of ultrapure water before adding lithium hydroxide (3 equivalents, 0.65 g). After 24 hours of stirring at room temperature, the water is evaporated using a rotary evaporator. The resulting compound is then quantitatively characterized by X-ray diffraction (XRD) and infrared spectroscopy. The purity and water content of the hydrated structures are determined by elemental and thermogravimetric analysis. The compound is then desolvated under vacuum at 250 °C. This compound has a theoretical capacity of 384 mAh / g and a measured capacity of 550 mAh / g and a theoretical volume of gas released of 2.5 eq mol. COMPARATIVE EXAMPLE 1

[0059] This example illustrates the preparation of a lithium salt which can be used for the preparation of a positive electrode not in accordance with the invention, this lithium salt corresponding to the following formula:

[0060] Ethylenediaminetetraacetic acid (1 g) is dispersed in 50 mL of ultrapure water before adding lithium hydroxide (4 equivalents, 0.57 g). After 24 hours of stirring at room temperature, the water is evaporated using a rotary evaporator. The resulting compound is then quantitatively characterized by X-ray diffraction (XRD) and infrared spectroscopy. The purity and water content of the hydrated structures are determined by elemental and thermogravimetric analysis. The compound is then desolvated under vacuum at 250 °C. This compound has a theoretical capacity of 339 mAh / g and a measured capacity of 424 mAh / g and a theoretical volume of gas released of 3 eq mol. COMPARATIVE EXAMPLE 2

[0061] This example illustrates the preparation of a lithium salt which can be used for the preparation of a positive electrode not in accordance with the invention, this lithium salt corresponding to the following formula:

[0062] Diethylenediaminepentaacetic acid (1 g) is dispersed in 50 mL of ultrapure water before adding lithium hydroxide (5 equivalents, 0.53 g). After 24 hours of stirring at room temperature, the water is evaporated using a rotary evaporator. The resulting compound is then quantitatively characterized by X-ray diffraction (XRD) and infrared spectroscopy. The purity and water content of the hydrated structures are determined by elemental and thermogravimetric analysis. The compound is then desolvated under vacuum at 250 °C. This compound has a theoretical capacity of 316 mAh / g and a measured capacity of 407 mAh / g and a theoretical volume of gas released of 3.3 eq mol. EXAMPLE 2

[0063] This example illustrates the preparation of test electrodes comprising the salts prepared in the previous examples, these electrodes being intended just to analyze the electrochemical decomposition of said salts in a button cell context facing a metallic lithium electrode or in a configuration of " Pouch Cell » compared to an electrode comprising Li4Ti 5 O 12 . In this respect, they do not include active electrode material in addition to the salts, unlike what should be the case for electrodes intended to operate in a real battery context.

[0064] Three types of these electrodes are prepared: an electrode comprising the lithium salt of Example 1; an electrode comprising the lithium salt of Comparative Example 1; and an electrode comprising the lithium salt of Comparative Example 2.

[0065] The protocol for preparing these electrodes is as follows.

[0066] The appropriate salt is mixed with SuperP ® carbon black in a mortar and then the whole is dispersed in a solution comprising PVDF in NMP (N-methylpyrrolidinone), in order to obtain an ink, the dry extract of which is composed of 60% by mass of salt, 30% by mass of carbon black and 10% by mass of PVDF. This ink is coated on an aluminum strip having a thickness of 100 µm wet and, after drying at 55°C, the deposit obtained is cut into a disc of 14 mm in diameter, calendered at a pressure of 10 tonnes and dried under vacuum. EXAMPLE 3

[0067] In this example, the electrodes prepared in Example 2 are each assembled facing a lithium metal counter-electrode with a polyolefin separator soaked in an organic electrolyte (1M LiPF 6 solution in a mixture of ethylene carbonate / propylene carbonate / dimethylcarbonate in proportions 1 / 1 / 3 by volume) within a button cell battery. The 3 batteries thus formed are subjected to a charge / discharge cycle at a C / 20 rate.

[0068] The results of this cycle are reported on the figure 1, which illustrates the evolution of the voltage U (in V vs Li +< / Li) as a function of the specific capacity C (in mAh / g), curve a) being representative of the battery obtained with the composite electrode comprising the salt of example 1, curve b) being representative of the battery obtained with the composite electrode comprising the salt of comparative example 1 and curve c) being representative of the battery obtained with the composite electrode comprising the salt of comparative example 2.

[0069] It is clear from this figure that with the battery obtained with the composite electrode comprising the salt of Example 1, the decomposition takes place at approximately 4.1 V vs Li + < / Li, that it is totally irreversible (no reduction phenomenon) and that it corresponds to 550 mAh / g of equivalent of lithium ions released, which is a substantial improvement compared to the batteries obtained with the salts of Comparative Examples 1 and 2. EXAMPLE 4

[0070] In this example, an electrode according to example 2 (the electrode comprising the salt of example 1) is assembled facing a counter-electrode based on Li 4 Ti 5 O 12 (LTO) with a polyolefin separator soaked in an organic electrolyte (solution of LiPF 6 1M in a mixture of ethylene carbonate / propylene carbonate / dimethyl carbonate in proportions 1 / 1 / 3 by volume) within a single-sided cell of the type " Pouch Cell » comprising a third metallic lithium electrode serving as a reference electrode.

[0071] The cell obtained is subjected to a charge / discharge cycle carried out at a C / 20 regime by controlling the potential of the electrodes relative to the reference electrode. The results are reported on the figure 2, which illustrates the evolution of the voltage U (in V vs Li +< / Li) as a function of the specific capacity C (in mAh / g) with curve a) being representative of the electrode comprising the salt of example 1 during the first charge, curve b) being representative of the counter-electrode based on Li 4 Ti 5 O 12 during the first charge and curve c) being representative of the counter-electrode based on Li 4 Ti 5 O 12 during the first discharge.

[0072] This experiment demonstrates that the lithium released by the decomposition of the salt is indeed available and inserted into the LTO counter-electrode and that it is possible to remove it during discharge.

Claims

1. Positive electrode for alkali metal-ion accumulator comprising at least one organic binder and at least one alkali metal salt of the following formula (I): wherein the X represent an alkali element.

2. Positive electrode according to claim 1, wherein, for the formula (I), the X represent the lithium element, the sodium element or the potassium element.

3. Positive electrode according to claim 1 or 2, wherein, for the formula (I), the X represent the lithium element.

4. Positive electrode according to any one of the preceding claims, wherein the organic binder is a polymeric binder.

5. Positive electrode according to claim any one of the preceding claims, further comprising at least one electrode active material.

6. Positive electrode according to claim 5, wherein, when the positive electrode is intended for a lithium accumulator, the electrode active material is selected from: - metal chalcogenides of formula LiMQ2, wherein M is at least one metal element selected from the metal elements, such as Co, Ni, Fe, Mn, Cr, V, Al and Q is a chalcogen; - chalcogenides of spinel structure, such as LiMn2O4; - lithiated or partially lithiated materials of formula M1M2(JO4)fE1-f, wherein M1 is lithium, optionally partially substituted with another alkali element up to a substitution level of less than 20%, M2 is a transition metal element of oxidation state +2 selected from Fe, Mn, Ni and combinations thereof, optionally partially substituted with one or more other additional metal elements of oxidation state(s) between +1 and +5 up to a substitution level of less than 35%, JO4 is an oxyanion wherein J is selected from P, S, V, Si, Nb, Mo and combinations thereof, E is a fluoride, hydroxide or chloride anion, f is the mole fraction of the oxyanion JO4 and is, generally, between 0.75 and 1 (including 0.75 and 1).

7. Positive electrode according to claim any one of the preceding claims, further comprising at least one electronically conductive additive.

8. Positive electrode according to claim any one of the preceding claims, said electrode being in the form of a part comprising a composite material comprising a polymer matrix consisting of one or more polymeric binders and comprising, as charges, at least one alkali metal salt of formula (I) such as defined in claim 1 and, optionally, at least one electrode active material and, optionally, one or more electronically conductive additives.

9. Positive electrode according to any one of claims 1 to 7, said electrode being in the form of a first part comprising a composite material comprising a polymer matrix consisting of one or more polymeric binders and comprising, as charges, at least one active material and, optionally, one or more electronically conductive additives and comprising a second part, in the form of a layer deposited on the surface of the first part, said layer comprising a polymer matrix consisting of one or more polymeric binders and comprising, as charges, at least one alkali metal salt of formula (I) such as defined in claim 1.

10. Alkali metal-ion accumulator cell comprising a positive electrode such as defined according to any one of claims 1 to 9, a negative electrode and an electrolyte disposed between the positive electrode and the negative electrode.

11. Alkali metal-ion accumulator cell according to claim 10, wherein the negative electrode comprises, as electrode active material, an active material selected from: - carbon materials, such as graphitic carbon capable of intercalating lithium; - silicon-based compounds, such as silicon carbide SiC or silicon oxide SiOx; - metallic lithium; - lithium alloys; - lithiated titanium oxides, such as an oxide of formula Li(4-x)MxTi5O12 or Li4MyTi(5-y)O12 wherein x and y range from 0 to 0.2, M represents an element selected from Na, K, Mg, Nb, Al, Ni, Co, Zr, Cr, Mn, Fe, Cu, Zn, Si and Mo; - non-lithiated titanium oxides, such as TiO2; - oxides of formula MyTi(5-y)O12 wherein y ranges from 0 to 0.2 and M is an element selected from Na, K, Mg, Nb, Al, Ni, Co, Zr, Cr, Mn, Fe, Cu, Zn, Si and Mo; - lithium-germanium alloys; or - a mixture thereof.

12. Alkali metal-ion accumulator cell according to claim 10 or 11, wherein the electrolyte is a liquid electrolyte conducting alkali ions comprising at least one organic solvent and at least one metallic salt.

13. Method for treating the accumulator cell such as defined according to any one of claims 10 to 12, comprising a step of forming a passivation layer at the surface of the negative electrode with the X ions resulting from the decomposition of the alkali metal salt of formula (I) such as defined in claim 1 by applying a first charge to the abovementioned cell.

14. Use of a salt of following formula (I): wherein the X represent an alkali element as sacrificial salt for the formation of a passivation layer at the surface of a negative electrode of an alkali metal-ion accumulator, which further comprises a positive electrode comprising said salt and an electrolyte disposed between the positive electrode and the negative electrode.