ELECTRODE NEGATIVE HYBRIDE GRAPHITE / LITHIUM

A hybrid negative electrode with graphite and solid electrolyte particles addresses inhomogeneous lithium deposition and volume expansion issues, ensuring stable and high-capacity lithium-ion battery operation.

FR3112032B1Active Publication Date: 2024-10-25SAFT GRP SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2020006745
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-26
Publication Date
2024-10-25
Estimated Expiration
2040-06-26

AI Technical Summary

Technical Problem

Existing lithium-ion batteries face challenges with inhomogeneous lithium deposition, leading to dendrite formation, mechanical degradation, and capacity reduction due to volume expansion in negative electrodes, particularly in solid electrodes.

Method used

A hybrid negative electrode comprising graphite and solid electrolyte particles, with lithium metal or lithium-rich alloys within its porosity, allowing controlled lithium deposition and minimizing volume variations through a 3D structure.

Benefits of technology

The electrode achieves homogeneous lithium deposition and significantly reduces volume changes, enhancing the electrode's capacity and stability, thereby improving battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000020_0000
    Figure 00000020_0000
  • Figure 00000021_0000
    Figure 00000021_0000
Patent Text Reader

Abstract

GRAPHITE / LITHIUM HYBRID NEGATIVE ELECTRODE The present invention relates to a mixed porous negative electrode comprising graphite and solid electrolyte particles, the structure and composition of which allow for increasing the quantity and quality of the lithium deposit while avoiding large variations in thickness. Figure for abstract: None
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: ELECTRODE HYBRID GRAPHITE / LITHIUM NEGATIVE

[0001] The present invention relates to the field of energy storage, and more specifically to accumulators, in particular of the lithium type.

[0002] Rechargeable lithium-ion accumulators offer excellent energy and volume densities and today occupy a predominant place in the market for portable electronics, electric and hybrid vehicles and stationary energy storage systems.

[0003] Solid electrolytes also offer a significant improvement in terms of safety in that they present a much lower risk of flammability than liquid electrolytes.

[0004] The operation of lithium accumulators is based on the reversible exchange of the lithium ion between a positive electrode and a negative electrode, separated by an electrolyte, the lithium being deposited at the negative electrode during charging operation. However, controlling the operating homogeneity of the negative lithium metal electrode is very delicate (growth of dendrites, degradation of mechanical properties linked to variations in the volume of the electrode, instabilities at the interfaces).

[0005] It is therefore desirable to promote the deposition of lithium and to obtain a deposit that is as homogeneous as possible.

[0006] FR2 992 478 describes a negative electrode, in particular for a lithium-ion cell, comprising lithium titanate and graphite. US 2019 / 0190012 describes a hybrid negative electrode for lithium-ion batteries comprising a hybrid electroactive material comprising graphite or silicon, and lithium titanate.

[0007] Massive electrodes make it possible to obtain high surface current densities but have the disadvantage of leading to the formation of dendrites and to inhomogeneous lithium deposition which ultimately leads to limitation of the charge.

[0008] The electrochemically active negative electrode materials for which the electrochemical capacity is the highest are generally formed from a metal capable of forming an alloy with lithium or pure lithium metal. However, these materials exhibit a high volume expansion during lithiation. This expansion will be the cause of the degradation of the Li-ion cell based on this material at the negative electrode: i) degradation of the integrity of the electrode which leads to a reduction in the capacity of the electrode, ii) fracture of the electrode-electrolyte interface (or SEI for "Solid Electrolyte Interface") which leads to the continuous formation of degradation product, iii) addition of stresses on the entire battery and degradation of other components.

[0009] It is therefore desirable to provide a negative electrode whose structure and composition make it possible to increase the volume capacity of the electrode while avoiding large variations in thickness.

[0010] The invention therefore aims in particular to provide a mixed porous negative electrode comprising graphite and solid electrolyte particles, characterized in that:

[0011] during charging, said electrode further contains: - lithium metal or in the form of a lithium-rich alloy within its porosity and - lithium in the form of lithiated graphite.

[0012] Said electrode is suitable for use in an energy storage device.

[0013] The term "negative electrode" designates when the accumulator is discharging, the electrode functioning as an anode and when the accumulator is charging, the electrode functioning as a cathode, the anode being defined as the electrode where an electrochemical oxidation reaction takes place (emission of electrons), while the cathode is the seat of the reduction.

[0014] The term negative electrode designates the electrode from which the electrons leave, and from which the cations (Li+) are released in discharge.

[0015] The term “lithium-rich alloy” means an alloy comprising at least 85 atomic% lithium.

[0016] The electrode structure according to the invention thus allows the deposition of lithium in a homogeneous manner within the porous structure while greatly limiting the volume variations of the electrode.

[0017] According to one embodiment, the negative electrode according to the invention does not contain lithium metal before it is put into operation. However, when operating within a charging electrochemical element, it further comprises lithium metal within its porosity, said lithium being - in the form of metal and / or an alloy rich in lithium within its porosity and - in the form of lithiated graphite.

[0018] The electrode is “hybrid” in that it allows the insertion of lithium into the host material (lithiated graphite) and the deposition in metallic form and / or in a lithium-rich phase in the porosity of the electrode.

[0019] The Li is inserted into the load according to a 3D structure.

[0020] The electrode according to the invention can be described as “mixed”, in that it can be considered as a Li-ion type electrode and comprises lithium as a charge.

[0021] The negative electrode layer generally consists of a conductive support used as a current collector which is coated with the negative electrode according to the invention containing said solid electrolyte particles and said graphite particles.

[0022] Current collector means an element such as a pad, plate, sheet or other, made of conductive material, connected to the positive or negative electrode, and ensuring the conduction of the flow of electrons between the electrode and the terminals of the battery.

[0023] The current collector is preferably a two-dimensional conductive support such as a solid or perforated strip, made of metal, for example copper, nickel, steel, stainless steel or aluminum. Said collector at the negative electrode is generally in the form of a copper strip.

[0024] According to one embodiment, said electrode may further contain a binder.

[0025] The term "binder" means the materials used to give the electrode cohesion of the various components and its mechanical strength on the current collector, and / or to give the electrode a certain flexibility for its implementation in a cell. Mention may thus be made, as binders, of: polyvinylidene fluoride (PVDF) and its copolymers, polytetrafluoroethylene (PTFE) and its copolymers, polyacrylonitrile (PAN), poly(methyl)- or (butyl)methacrylate, polyvinyl chloride (PVC), poly(vinyl formalin), polyester, block polyetheramides, polymers of acrylic acid, methacrylic acid, acrylamide, itaconic acid, sulfonic acid, elastomer and cellulose compounds. The elastomer(s) that can be used as a binder can be chosen from styrene-butadiene (SBR), butadiene-acrylonitrile (NBR), hydrogenated butadiene-acrylonitrile (HNBR), and a mixture of several of these.

[0026] According to one embodiment, the lithium is not in the form of lithium titanate.

[0027] According to one embodiment, the negative electrode further contains a material " lithiophilic”. The term “lithiophilic” defines a material with an affinity for lithium, (i.e.) its ability to form alloys with lithium.

[0028] According to one embodiment, the lithiophilic element can be chosen from silicon, silver, zinc and magnesium, preferably silicon. Typically, alloys formed by these elements with lithium include LixSiy type alloys, with varying x / y atomic ratios. The lithophile element may be present in the form of particles or fibers instead of or in addition to the coating. Preferably, at least one of the characteristic dimensions of these particles or fibers is less than Ipm

[0029] This lithiophilic element can be added by adding powder of said element with graphite, during the manufacture of the electrode.

[0030] According to one embodiment, the graphite is coated with a lithiophilic element, preferably chosen from silicon, zinc, aluminum, silver, magnesium, tin, or compounds containing these elements.

[0031] The layer of lithiophilic element mentioned here coating the graphite particles typically has a thickness which can vary from a few nanometers to less than 100nm, typically approximately less than 50nm, in particular less than 20 nm, in particular less than 10 nm, more preferably from 2 to 5 nm.

[0032] This layer has several roles. It allows the nucleation energy of lithium to be reduced. It is conductive to lithium, in that it allows the transit of Li+ ions from the electrolyte layer. In addition, it can also allow homogenization of the lithium deposit by allowing the formation of local batteries: in fact, during charging, a potential difference is created in the thickness of the electrode; this potential difference can then allow electrochemical rebalancing over the thickness of the electrode by oxidation of the metallic lithium in the most positive potential zones and a reduction of Li+ in the most negative potential zones.

[0033] According to one embodiment, the coating layer consists exclusively of the lithiophilic material.

[0034] The graphite particles may be coated over all or part of their peripheral surface. According to one embodiment, the coating layer covers at least 50% of the surface of the electrode, preferably at least 75%, more preferably at least 90%, even more preferably at least 95%.

[0035] According to the invention, the negative electrode is porous:

[0036] The volume of the pores allows lithium to be accommodated in the metallic state during charging.

[0037] Here, the term “porous” according to the invention means a pore size of less than 300 nm.

[0038] The pore size corresponds to the structure of the material having an organized network of channels of very small variable pore size: typically a pore size less than Ipm, preferably less than 300 nm. This pore size gives the electrode a particularly large active surface area per unit of electrode surface area.

[0039] According to one embodiment, the electrode has a porosity of between 10 and 60%, preferably between 30 and 50%.

[0040] This porosity makes it possible in particular, on the one hand, to accommodate the lithium metal in the porosity and, on the other hand, to maintain the mechanical strength of the electrode.

[0041] Graphite particles are not limited in their morphology. Examples include spherical or ovoidal particles, platelets, etc.

[0042] Typically, the graphite particles have a diameter between 1 and 30 pm nominal (or equivalent)

[0043] A mixture of several particle sizes and several graphite morphologies can also be used.

[0044] The electrolyte may be solid or non-solid, preferably solid.

[0045] According to one embodiment, the solid electrolyte is of the sulfide type.

[0046] Typically, said sulfide electrolyte can be chosen from: - the set of phases [(Li2S)y (Li2O)t(P2S5)i_y_t](i_z)(LiX)z with X representing a halogen element; 0 <y<l ; 0<z<l ; 0<t< 1 - argyrodites such as Li6PS5X, with X=C1, Br, I, or Li7P3Sn; - sulfide electrolytes having the crystallographic structure equivalent to compound LiioGeP2Si2; Li3PS4.

[0047] According to another object, the present invention also relates to a method for preparing an electrode according to the invention, said method comprises the step of mixing graphite, optionally previously coated, solid electrolyte particles and a porophoric agent, then a treatment making it possible to remove the porophoric agent, such as a heat treatment of the mixture obtained.

[0048] It is understood that the mixture may also comprise lithiophilic element powder according to the embodiment discussed above. As a blowing agent, mention may in particular be made of polypropylene carbonate. Typically, the content of the blowing agent in the mixture is between 10 and 50% by weight.

[0049] The creation of porosity can then be carried out by a treatment allowing the removal of the porophoric agent, by application or adaptation of known methods, generally depending on the nature of the porophoric agent used. Typically, this can be carried out by heat treatment, at a temperature generally above 150°C.

[0050] The prior coating of the graphite particles with a lithiophilic element can be carried out by any method allowing the deposition of a thin layer, such as: - chemical deposition: sol-gel, spin-coating, vapor deposition, atomic layer deposition (ALD), molecular layer deposition (MLD), or by controlled oxidation; and - physical vapor deposition (PVD): vacuum evaporation, cathode sputtering, pulsed laser deposition, electrohydrodynamic deposition.

[0051] Typically, the coating layer can be deposited by ALD or PVD.

[0052] ALD consists of exposing the surface of the carbon particles successively to different chemical precursors in order to obtain ultra-thin layers.

[0053] The deposition can generally be carried out by ALD, PVD. Typically, the PVD treatment is carried out on a fluidized bed to allow homogeneous deposition, (i.e.) treatment of the particles in all directions.

[0054] According to another object, the present invention also relates to an all-solid electrochemical element comprising a porous negative electrode according to the invention, and a positive electrode, such that the ratio k = Cnegative material / CpOsitiVe is between 0.2 and 0.95, preferably between 0.5 and 0.9,

[0055] where Cnegative material represents the sum of the capacity of the graphite and a part of the capacity of all the lithiable materials present at the negative electrode in the discharged state. The part of capacity considered is that whose potential, measured during a discharge at C / 100, is greater than 0.2V vs Li7Li°. The capacities are equal to the products of the mass of each active material multiplied by the mass capacity (the masses being expressed in g / cm2 and the mass capacities in mAh / g, the active materials of the negative electrode comprising graphite as well as the other lithiable materials), and where

[0056] CpOsitiVe represents the capacity of the positive electrode in mAh / cm2.

[0057] According to one embodiment, the porosity of the negative electrode in the discharged state (expressed as a percentage) is equal to 100*R* (lk)*Cpositive*4.85 / e where:

[0058] CpositiVe represents the capacity of the positive electrode in mAh / cm2

[0059] e represents the thickness of the negative electrode in the discharged state expressed in pm

[0060] R represents a number between 0.6 and 3, preferably between 1.1 and 1.7 and

[0061] k is as defined above.

[0062] According to one embodiment, the electrochemical element comprises an intermediate layer between the negative electrode and the solid electrolyte layer used as a separator; this layer mainly contains fine amorphous carbon powder as well as a lithiophilic element forming alloys with lithium. The carbon powder and the powder of the lithiophilic element are preferably of nanometric size (between 20 and 100 nm). The lithiophilic element may be different from that used in the negative electrode.

[0063] The term "electrochemical element" means an elementary electrochemical cell consisting of the positive electrode / electrolyte / negative electrode assembly, making it possible to store the electrical energy supplied by a chemical reaction and to restore it in the form of current.

[0064] Typically such an electrochemical element comprises a negative electrode layer, a positive electrode layer and an electrolytic separation layer, such that said solid electrolyte particles are present within the three layers.

[0065] It is understood that the solid electrolyte particles present in the different layers may be identical or different.

[0066] Within the scope of the present invention, the positive electrode of the positive electrode layer may be of any known type.

[0067] The term positive electrode designates the electrode where the electrons enter, and where the cations (Li+) arrive in discharge.

[0068] The positive electrode layer generally consists of a conductive support used as a current collector which is coated with the positive electrode containing the positive electrode active material, solid electrolyte particles and a carbon additive.

[0069] This carbon additive is distributed in the electrode so as to form an electronic percolating network between all of the particles of active material and the current collector.

[0070] Typically the positive electrode may also comprise a binder, such as those previously mentioned for the negative electrode.

[0071] The active material of the positive electrode is not particularly limited. It may be selected from the following groups or mixtures thereof:

[0072] - a compound (a) of formula LixMi_y_z_wM'yM”zM'”w02 (LM02) where M, M', M” and M”' are selected from the group consisting of B, Mg, Al, Si, Ca, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, W and Mo provided that at least M or M' or M'' or M”' is selected from Mn, Co, Ni, or Fe; M, M', M” and M”' being different from each other; and 0.8 <x<l,4 ; 0<y<0,5 ; 0<z<0,5 ; 0<w<0,2 et x+y+z+w<2,l ;

[0073] - a compound (b) of formula LixMn2_y_zM'yM"zO4 (LMO), where M' and M" are chosen in the group consisting of B, Mg, Al, Si, Ca, Ti, V, Cr, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb and Mo; M' and M" being different from each other, and 1 <x<1,4 ; 0<y<0,6 ; 0<z<0,2 ;

[0074] - a compound (c) of formula LixFei yMyPO4(LFMP) where M is chosen from the group consisting of B, Mg, Al, Si, Ca, Ti, V, Cr, Mn, Co, Ni, Cu, Zn, Y, Zr, Nb and Mo; and 0.8 <x<l,2 ; 0<y<0,6 ;

[0075] - a compound (d) of formula LixMni y zM'yM”zP04 (LMP), where M' and M” are different from each other and are selected from the group consisting of B, Mg, Al, Si, Ca, Ti, V, Cr, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb and Mo, with 0.8 <x<l,2 ; 0<y<0,6 ; 0<z<0,2 ;

[0076] - a compound (e) of formula xLi2MnO3; (lx)LiM02 where M is at least one element chosen from Ni, Co and Mn and x <l.

[0077] - a compound (f) of formula Lii+XMO2 yFy of cubic structure where M represents at least one element selected from the group consisting of Na, K, Mg, Ca, B, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Al, Y, Zr, Nb, Mo, Ru, Ag, Sn, Sb, Ta, W, Bi, La, Pr, Eu, Nd and Sm and where 0 < x < 0.5 and 0 < y < 1;

[0078] - Graphite

[0079] - Silicon

[0080] - a titanium and niobium oxide TNO having the formula (g):

[0081] LixTia_yMyNbb- ZM'ZO( (X+4a+5b) / 2)-c- dXc

[0082] where0 <x<5;0<y<l;0<z<2;l<a<5;l<b<25; 0,25 <a / b<2;0<c< 2 and 0 < d < 2; ay > 0; bz > 0;

[0083] M and M' each represent at least one element selected from the group consisting of Li, Na, K, Mg, Ca, B, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Al, Y, Zr, Nb, Mo, Ru, Ag, Sn, Sb, Ta, W, Bi, La, Pr, Eu, Nd and Sm;

[0084] X represents at least one element selected from the group consisting of S, F, Cl and Br.

[0085] The index d represents an oxygen vacancy. The index d can be less than or equal to 0.5.

[0086] Said at least one titanium and niobium oxide may be chosen from TiNb2O7, Ti2 Nb2O9 and Ti2Nbi0O29.

[0087] - a lithiated titanium oxide or a titanium oxide capable of being lithiated. LTO is chosen among the following oxides:

[0088] h) Lix.aMaTiy.bM'bO4.c.dXc in which 0 <x<3 ; l<y<2,5 ; 0<a<l ; 0<b<l ; 0<c<2 et -2,5<d<2,5 ;

[0089] M represents at least one element selected from the group consisting of Na, K, Mg, Ca, B, Mn, Fe, Co, Cr, Ni, Al, Cu, Ag, Pr, Y and La;

[0090] M' represents at least one element selected from the group consisting of B, Mo, Mn, Ce, Sn, Zr, Si, W, V, Ta, Sb, Nb, Ru, Ag, Fe, Co, Ni, Zn, Al, Cr, La, Pr, Bi, Sc, Eu, Sm, Gd, Ti, Ce, Y and Eu;

[0091] X represents at least one element selected from the group consisting of S, F, Cl and Br;

[0092] The index d represents an oxygen vacancy. The index d can be less than or equal to 0.5.

[0093] i) HxTiyO4 in which 0 <x<l ; 0<y<2, et

[0094] j) a mixture of compounds h) to i).

[0095] Examples of lithiated titanium oxides belonging to group h) are spinel Li4 Ti50i2, Li2TiO3jlaramsdellite Li2Ti3O7,LiTi2O4, LixTi2O4, with 0 <x<2 et Li2Na2Ti60i4.

[0096] A preferred LTO compound has the formula Li4_aMaTi5_bM'bO4j, for example Li4Ti50i2 which is also written Li4 / 3Ti5 / 3O4.

[0097] The positive electrode electronic conductive material is generally chosen from graphite, carbon black, acetylene black, soot, graphene, carbon nanotubes or a mixture thereof.

[0098] The current collector of the positive electrode layer is typically made of aluminum.

[0099] The electrolytic layer (or separator) contains an electrolytic composition, which may comprise one or more electrolytic constituents. As solid electrolyte constituents, mention may in particular be made of sulfur compounds alone or in a mixture with other constituents, such as polymers or gels. can thus cite partially or completely crystallized sulfides as well as amorphous ones. Examples of these materials can be selected from sulfides of composition A Li2S - B P2S5 (with 0 <A<l,0<B<l et A+B = 1) et leurs dérivés (par exemple avec dopage Lil, LiBr, LiCl, ...) ; les sulfures de structure argyrodite ; ou ayant une structure crystallographique similaire au composé LGPS (Lii0GeP2Si2 ), et ses dérivés. Les matériaux électrolytiques pourront également comprendre des oxysulfures, des oxydes (grenat, phosphate, anti-perovskite, ...), des hydrures, des polymères, des gels ou des liquides ioniques conducteurs des ions lithium.

[0100] Examples of sulfide electrolyte compositions are described in particular in Park, K.H., Bai, Q. Kim, D.H., Oh, D.Y., Zhu, Y., Mo, Y., & Jung, Y.S. (2018). Design Strategies, Practical Considerations, and New Solution Processes of Sulfide Solid Electrolytes for All-Solid-State Batteries. Advanced Energy Materials, 1800035.

[0101] In all-solid-state elements, the electrolytic compounds may be included in the electrolytic layer, but may also be included partly within the electrodes.

[0102] Typically, the electrochemical element according to the invention is a “lithium free” type battery.

[0103] It is understood that the term "lithium free" defines the fact that the battery does not contain lithium metal when the accumulator is assembled, but that lithium is deposited in metallic form and then consumed in a controlled and reversible manner in situ during operation of the battery. Typically, lithium is deposited within the negative electrode during charging and consumed during discharging.

[0104] According to another object, the present invention also relates to an electrochemical module comprising the stack of at least two elements according to the invention, each element being electrically connected with one or more other element(s).

[0105] The term “module” therefore designates here the assembly of several electrochemical elements, said assemblies being able to be in series and / or parallel.

[0106] Another object of the invention is still a battery comprising one or more modules according to the invention.

[0107] The term “battery” or accumulator means the assembly of several modules according to the invention.

[0108] According to one embodiment, the batteries according to the invention are accumulators whose capacity is greater than 100 mAh, typically 1 to 100 Ah. Figures

[0109] [Fig. 1] [Fig. 1] schematically represents the ratio between the capacity of the negative electrode (N on the left), and the positive electrode (P on the right). Such that this is represented, the capacity of the negative electrode in the charged state is the sum of the capacity of the lithium metal (CLi) accumulated during charging, and the sum of the capacity of the graphite and the part of the capacity of all the lithiable materials present at the negative electrode in the discharged state whose potential during discharge is greater than 0.2V (Cg). This total capacity in the charged state is equal to the capacity of the positive electrode. In other words, the capacity of the negative electrode can increase during charging by the addition of lithium, until it reaches the capacity of the positive electrode.

[0110] [Fig.2] [Fig.2] shows a schematic representation of the structure of a electrochemical element according to the invention in the discharged state. Said element comprises a negative electrode layer (1), a positive electrode layer (3), separated by an electrolytic layer (2).

[0111] The negative electrode layer (1) comprises a current collector (4) on which the negative electrode material according to the invention is deposited, consisting of solid electrolyte particles (5) and graphite particles (6).

[0112] It is understood that according to embodiments not shown here, the particles (6) may be covered with a lithiophilic metal.

[0113] The electrolyte particles (5) and graphite particles (6) create a porosity within which lithium metal can be deposited during charging (not shown here). The separation layer (2) consists of solid electrolyte particles (7). These particles (7) may be identical to the particles (5).

[0114] The positive electrode layer (3) comprises a current collector (4') on which is deposited a mixture comprising solid electrolyte particles (9), conductive carbon (8), and active material particles (10).

[0115] It is understood that layers (1) and (3) may further comprise binders, which are not shown in [Fig.l]. Examples:

[0116] 1- Preparation of the negative electrodes:

[0117] The electrolytes used to illustrate the invention are sulfide type compounds of composition Li3PS4, (Li3PS4)os(LiI)o.2 and Li6PS5Cl. The graphite powder is of platelet type (for example SFG15 from Imerys). The conductive additive used in the examples is carbon black (of type C65 from Imerys). The solid electrolyte and the carbon are mixed with a binder (1% PTFE), a lithiophilic material such as Zn, Ag, Mg and Si and a porophoric agent (polypropylene carbonate) whose quantity is calculated to have the desired porosity after the thermal treatment of decomposition of the agent. The mixing of the powders is carried out manually in a glove box in an agate mortar by mixing with a pestle 500 mg of mixture for 10 min. A quantity of this mixture is placed in a pelletizing mold whose matrix has an internal diameter of 1 cm; the mass of the mixture is equal to the grammage of the electrode multiplied by the internal surface of the matrix. The whole is compressed at a pressure between 1 and 5 t / cm2. The lithiophilic material can be used in several forms: either in the form of fine powder (particles of size between 30 nm and 200 nm), or the material has been deposited on the electrolyte powder or on the carbon powder by PVD. The process used is cathodic sputtering with a rotating enclosure allowing movement of the particles and thus obtaining a more homogeneous deposition on the surface of the particles.

[0118] 2- Production of the accumulator:

[0119] The positive electrode used in the examples consists of an active material NMC (composition: Li(Ni0.6oMno. 2oCo0 2o)02), sulfide electrolyte of composition (Li3PS4)o.8(LiI)o.2 and PTFE. The respective proportions are 74.5%, 25% and 0.5%. The constituents are mixed for 5 min in an agate mortar in a glove box.

[0120] The mass of mixture in mg for the production of the electrode is equal to the desired surface capacity in mAh / cm2 multiplied by the surface area of ​​the electrode and divided by 190 mAh / g.

[0121] In the pellet mold containing the negative electrode pellet, 50 mg of electrolyte (Li3PS4)o.8(LiI)o.2 are added to make the electrolytic layer to ensure electronic insulation between the 2 electrodes. The assembly is then compressed at 5 t / cm2. The mass of positive electrode mixture is then added to the surface of the electrolyte layer, then a new compression of the assembly is carried out at 5 t / cm2.

[0122] The pellet thus obtained is then heat treated at 260°C under argon for 15 min to remove the blowing agent.

[0123] The assembly is then placed in a sealed electrochemical cell allowing electrical connection with the positive and negative electrodes, while maintaining a mechanical pressure of approximately 50 bar. The cell is then charged at C / 20 up to a voltage of 4.3V. The total capacity of the positive electrode considered in Tables 1 and 2 corresponds to the charged capacity of the 1st charge divided by the surface area of ​​the electrode.

[0124] Due to partial irreversibility of the positive electrode capacity, the total capacity cannot be measured during subsequent cycles.

[0125] One way to measure the total capacity after the 1st cycle is to charge the accumulator to the maximum nominal voltage of the accumulator (in our example 4.3V) at a slow rate (typically C / 20), then to dismantle the accumulator in a glove box, recover a sample of known surface area (if the electrode is double-sided, the surface area considered is to be multiplied by 2). Still in a glove box, the electrode sample is placed in a sealed cell of known volume equipped with pressure and temperature sensors as well as a septum. Using a syringe filled with water, water is introduced into the cell on the electrode (the electrode must be completely impregnated). The lithium in the metallic state in the electrode will thus react with the water to form hydrogen. Once the cell pressure has stabilized, the number of moles of hydrogen formed (nH2) can be calculated from the pressure, temperature and volume of the cell. The total surface capacity of the positive electrode in mAh / cm2 is equal to nH2*53600 / S, S being the negative electrode surface area previously considered expressed in cm2.

[0126] The porosity of the negative electrode is estimated as follows: a negative electrode is prepared under the conditions described in paragraph 1. Then a heat treatment is applied at 260°C for 15 min under argon. The porosity is then conventionally calculated from the thickness, the mass of the treated electrode and the composition of the electrode and the density of the components.

[0127] For the calculation of the quantities Cnegative material and k, it is necessary to measure the mass capacity of the materials forming lithium alloys used in the examples. This can be determined as follows: - an electrode based on the material considered is produced by mixing the active material with carbon (10% for example) and a binder (5% for example) according to the classic processes for preparing lithium-ion accumulators - an accumulator is assembled with this electrode, a counter electrode made of metallic lithium, a membrane-type separator and an electrolyte based on carbonate solvent and LiPF6 - after having carried out a lithiation (*) of the material considered up to a battery voltage of 0V at a regime of C / 50, a delithiation is carried out at a regime of C / 100 up to a potential of 2V. Given that the lithium counter electrode has a potential equal to 0 at rest, the measurement of the battery voltage is approximately equal to that of the potential of the electrode containing the material considered when the regime is low (for example C / 100) - the mass capacity of the material is equal to the discharged capacity between 0.2V and 2V divided by the mass of the material considered

[0128] (*) lithiation corresponds to the mechanism occurring during the charging of the negative electrode in the accumulator in the configuration of the invention, that is to say by using a counter electrode with a high potential (typically greater than 3 V); similarly, delithiation corresponds to the discharge of the negative electrode in the configuration of the invention.

[0129] For the thickness measurement necessary for calculating the swelling of the negative electrode: the electrochemical cell is disassembled in the charged state and then the assembly is placed in a scanning electron microscope with which it is possible to measure the thickness of the negative electrode.

[0130] The examples of the invention and the results obtained are gathered in Tables 1 and 2. The comparative examples of Tables 4-6 were prepared with the same procedure as that used for the examples of the invention.

[0131] The results of the examples of the invention are presented in Table 3 and those of the comparative examples in Table 6.

[0132] The examples of the invention exhibit low swelling of the negative electrode in the charged state. Indeed, the variation in thickness between the charged and discharged states is less than 15% (between 5% and 11%). In addition, the volume capacity of the negative electrodes of the examples of the invention is high, greater than 710 mAh / cm3

[0133] Comparative examples 1 and 2 do not contain lithium metal in the charged state, which corresponds to a value of k equal to 1. The volume capacity of these electrodes is significantly lower (less than 600 mAh / cm3).

[0134] Comparative example 3 has a value of k <1 (k=0.5) with a high value of R (>7). It is also noted that the volume capacity of the electrode is low (472 mAh / cm3)

[0135] Comparative example 4 has a value of k > 1 (k=0.5) with a low value of R (R=0.3). In this case, we see that the capacity is high (737mAh / cm 3) but that the swelling under load is very high: 66%, which is detrimental to the operation of the accumulator.

[0136] Therefore, unlike the comparative examples, the examples of the invention make it possible to achieve high negative electrode volume capacities while avoiding strong swelling of the negative electrode under load.

[0137] Description of examples of the invention:

[0138] [Tables 1] No. Example Molar composition of the electrolyte % mass of electrolyte in the electrode before TT diameter of electrolyte particles (pm) material forming lithium alloys % material forming lithium alloys % carbon black Exl Li3PS4 30 1 Si 2 2 Ex2 Li3PS4 30 3 Si 3 2 Ex3 Li3PS4 30 5 Si 1 2 Ex4 Li3PS4 30 3 Si 5 2 Ex5 Li3PS4 30 0.5 Si 3 2 Ex6 Li3PS4 30 3 Si 3 2 Ex7 Li3PS4 40 3 Si 3 2 Ex8 Li3PS4 30 3 Si 3 2 Ex9 (Li3PS4)0.8(LiI)o.2 50 3 Ag 3 2 ExlO Li6PS5Cl 35 3 Zn 3 5 Exile Li3PS4 55 3 Si 3 2

[0139] [Tables2] No. Example final porosity (%) total capacity of the positive electrode (mA h / cm2) % graphite weight of lithiabl es materials (Gr+NC+alloy) (mg / cm2) k=Cmat negative act / Cp ositive R 100*R(lk)C+*4.85 / e Exl 30 4 61 4.184 0.50 1.4 30 Ex2 40 4 64 3.043 0.40 1.2 40 Ex3 25 4 66 5.746 0.60 1.7 25 Ex4 10 4 62 5.048 0.80 1.0 10 Ex5 30 4 64 3.804 0.50 1.2 30 Ex6 35 4 64 3.804 0.50 1.5 35 Ex7 40 4 54 3.622 0.50 2.1 40 Ex8 44 4 64 3.804 0.50 2.1 44 Ex9 30 4 44 3.393 0.50 1.5 30 ExlO 15 4 56 5.637 0.50 0.8 15 Exile 25 4 39 2.605 0.40 0.8 25

[0140] Results relating to the examples:

[0141] [Tables3] No. Example Minimum swelling of the negative electrode (%) Volume capacity in the charged state (mAh / c m3) Exl 6 851 Ex2 6 1072 Ex3 6 711 Ex4 11 926 Ex5 7 992 Ex6 6 925 Ex7 5 763 Ex8 5 804 Ex9 5 796 Exl0 11 731 Exil 11 919

[0142] Description of comparative examples:

[0143] [Tables4] No. Example Molar composition of electrolyte % mass electrolyte In Electrode before TT Electrolyte particle diameter (pm) lithium alloy forming material % lithium alloy forming material % carbon black Ex Co mp 1 Li3PS4 30 1 none 0 2 Ex Co mp 2 Li3PS4 30 1 Si 5 2 Ex Co mp 3 Li3PS4 30 1 Si 2 2 Ex Co mp 4 Li3PS4 30 1 Si 2 2

[0144] [Tables5] N° Exe porosity capacity to % grap grammage ma k=Cmat R 100*R(lk mple final ( size of the el hite teriaux lithiab act nega )C+*4.85 / e %) electrode po positive (mA h / cm2) es (Gr+NC+alloy) (mg / cm2) tive / Cp ositive Ex Co mp 1 30 4 67 10.989 1.00 Ex Co mp 2 30 4 62 6.304 1.00 Ex Co mp 3 70 4 65 4.240 0.50 7.1 70 Ex Co mp 4 10 4 65 4.240 0.50 0.3 10

[0145] Results relating to comparative examples:

[0146] [Tableauxô] No. Example minimum swelling of the negative electrode (%) volume capacity in the charged state (mAh / cm3) Ex Comp 1 5,351 Ex Comp 2 8,589 Ex Comp 3 3,397 Ex Comp 4 66,737

Claims

Claims

1. Mixed porous negative electrode comprising graphite and solid electrolyte particles, characterized in that: during charging, said electrode further contains: - lithium metal or a lithium-rich phase within its porosity and - lithium in the form of lithiated graphite, such that the porosity is between 10 and 60%

2. Electrode according to claim 1 such that it further contains a material which forms lithium alloys, preferably silicon.

3. Electrode according to any one of the preceding claims, such that the graphite is coated with an element forming lithium alloys, preferably chosen from silicon, zinc, aluminum, silver, magnesium, tin, or compounds containing these elements.

4. Electrode according to any one of the preceding claims such that the solid electrolyte is of the sulfide type.

5. Electrode according to claim 4, such that said sulfide electrolyte is chosen from: - the set of phases [(Li2S)y (Li2O)t(P2S5)i_y_t](i_Z)(LiX)z with X representing a halogen element; 0 <y<l ; 0<z<l ; 0<t<l - les argyrodites tels que Li6PS5X, avec X=C1, Br, I, ou Li7P3 Su; - les électrolytes sulfures ayant la structure cristallographique équivalente au composé Lii0GeP2Si2 ; Li3PS4.

6. An electrode according to any preceding claim, such that the electrode has a porosity of between 30 and 50%.

7. An electrode according to any preceding claim, such that the electrode has a pore size of less than 300 nm.

8. A method of preparing an electrode according to any one of the preceding claims comprising the step of mixing optionally pre-coated graphite particles solid electrolyte and a blowing agent, followed by treatment to remove the blowing agent.

9. All-solid electrochemical element comprising a porous negative electrode according to any one of claims 1 to 7, and a positive electrode, such that the ratio k = Cnegative material / CpOsitiVe is between 0.2 and 0.95, preferably between 0.5 and 0.9, where Cnegative material represents the sum of the capacity of the graphite and a part of the capacity of all the lithiable materials present at the negative electrode in the discharged state. The part of capacity considered is that whose potential, measured during a discharge at C / 100, is greater than 0.2V vs Li7Li°, the capacities are equal to the products of the mass of each active material multiplied by the mass capacity (the masses being expressed in g / cm2 and the mass capacities in mAh / g, the active materials of the negative electrode including graphite as well as other lithiable materials), and where CpOsitiVe represents the capacity of the positive electrode in mAh /

10. uni . Electrochemical element according to claim 9, such that the porosity of the electrode in the discharged state expressed in % is equal to 100* R.(lk).CpOsitiVe*4.85 / e where: CpOSitive represents the capacity of the positive electrode in mAh / cm2 e represents the thickness of the negative electrode in the discharged state expressed in pm R represents a number between 0.6 and 3, preferably between 1.1 and 1.7 and k is as defined in claim 9.

11. All-solid electrochemical element comprising a porous negative electrode according to any one of claims 1 to 7 comprising an intermediate layer between the negative electrode and a layer of solid electrolyte, this layer containing mainly fine amorphous carbon powder as well as a compound forming alloys with lithium.

12. Electrochemical module comprising the stack of at least two elements as defined according to claim 9, each 19 element being electrically connected with one or more other element(s).

13. A battery comprising one or more modules according to claim 12.