A method for safely extracting lithium from an electric battery containing solid metallic lithium.
The process addresses the fire risk and inefficiency of existing lithium recovery methods by heating, orienting, and cutting electrical connections in batteries, ensuring safe and efficient lithium extraction.
Patent Information
- Application Number
- FR2021009469
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-09-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-09-09
AI Technical Summary
Current techniques for recovering solid metallic lithium from batteries pose a risk of battery fire due to the high temperatures required for melting, and there is a lack of efficient methods to manage potential short circuits during lithium recovery.
A process involving heating the battery to a temperature greater than the melting point of lithium, orienting the cells to facilitate lithium flow, and cutting electrical connections between positive electrodes to reduce reactivity and risk of fire, combined with optional steps like charging, compressing, and immersing in a dense, insulating liquid to enhance recovery.
The process safely and efficiently recovers solid metallic lithium by minimizing the risk of fire and short circuits, increasing recovery yield, and reducing the formation of pollutants during extraction.
Smart Images

Figure 00000020_0000 
Figure 00000020_0001 
Figure 00000020_0002
Abstract
Description
Title of the invention: Method for safely extracting lithium from an electric battery comprising solid metallic lithium.
[0001] The present invention relates to a method for extracting lithium from a battery comprising solid metallic lithium, in a safe manner.
[0002] The field of the invention is the field of batteries based on solid metallic lithium, and in particular Lithium-Metal-Polymer batteries, and even more particularly the field of recycling these batteries. State of the art
[0003] Batteries based on solid or quasi-solid lithium metal are known, such as, for example, Lithium-Metal-Polymer (LMP®) batteries. These batteries are increasingly used, for example, in electric vehicles or in power stations. Thus, the number of batteries based on solid or quasi-solid lithium metal has been constantly increasing for several years.
[0004] The lifespan of such batteries is not infinite and it seems necessary to recycle these batteries. However, even at the end of its life, such a battery still contains solid metallic lithium, which can be reused in other batteries or in other fields, and whose value is not negligible.
[0005] There are currently very few techniques for recovering solid metallic lithium from a battery. These rare techniques involve heating the battery to a temperature greater than or equal to the melting temperature of solid metallic lithium to recover the lithium in the liquid state. However, these techniques present a risk of battery fire.
[0006] An aim of the present invention is to remedy this drawback.
[0007] Another aim of the invention is to propose a method for recovering solid or quasi-solid metallic lithium in a battery, for all configurations where the cathode and the electrolyte are stable up to at least 181°C (or up to the melting temperature of lithium), of electrical energy storage cells in an efficient manner by limiting and controlling the effect of potential short circuits during the recovery of lithium. Statement of the invention
[0008] The invention makes it possible to achieve at least one of these aims by a method of extracting lithium from a battery, such as a solid or quasi-solid lithium electrolyte battery, comprising at least two electrical energy storage cells; each cell comprising a positive electrode, a negative electrode and solid or near-solid metallic lithium; said battery comprising a first edge from which the negative electrodes of said cells protrude and a second edge, opposite said first edge, and from which the positive electrodes protrude; said method comprising an extraction phase comprising the following steps: - positioning said battery in an orientation in which one of said first and second edges is below the other of said first and second edges, and - heating said battery to a temperature, called treatment temperature, greater than or equal to the melting temperature of said solid metallic lithium; characterized in that it further comprises a step of cutting the electrical connection between the positive electrodes of at least two, and in particular of all, the cells of said battery.
[0009] Thus, the invention proposes to recover solid metallic lithium from a battery by heating said battery to a treatment temperature greater than or equal to the melting temperature of solid metallic lithium. The metallic lithium, once melted, is evacuated, in whole or in part, naturally from each cell. Thus, the invention allows simple and uncomplicated recovery of solid metallic lithium.
[0010] Furthermore, the invention provides a specific orientation of each cell, the latter being, at a minimum, inclined. Such an orientation of each cell makes it possible to facilitate the flow of molten lithium out of the cell by gravity.
[0011] Furthermore, and above all, the invention provides for cutting the connection between the positive electrodes of at least two, preferably all, of the cells of the battery. In other words, the cutting step makes it possible to break the electrical connection between the positive electrodes of the cells of the battery. Thus, after the cutting step, the battery comprises a plurality of cells which are no longer electrically connected to each other, which reduces the reactivity of the battery, and therefore the risks of fires in the battery during the recovery of the lithium.
[0012] The first border can be characterized by the fact that it defines the side through which the lithium, once in the liquid state, must flow.
[0013] In the present application, by “electrical energy storage cell”, or “cell”, is meant an assembly comprising, at least: - a negative electrode formed by, or comprising, a layer of solid metallic lithium; - a positive electrode, - a solid electrolyte, in particular comprising lithium salt, arranged between the positive electrode and the negative electrode, and - a current collector on the positive electrode side.
[0014] In the present application, “solid or quasi-solid metallic lithium” may comprise: - pure metallic lithium; or - a combination of at least one metallic lithium alloy; or - a combination of pure metallic lithium and at least one lithium alloy metallic.
[0015] When the “solid or near-solid metallic lithium” comprises a combination of different forms of lithium, such as those indicated above, having different melting temperatures, then the heating step involves heating the battery to a processing temperature greater than or equal to: - the lowest of said different melting temperatures; and - preferably, the highest of said different melting temperatures.
[0016] According to a non-limiting example embodiment, the treatment temperature is greater than or equal to 180.5°C.
[0017] According to an exemplary embodiment, the treatment temperature is less than or equal to a maximum temperature, for example 300°C.
[0018] The battery may comprise a number of cells greater than or equal to 2.
[0019] The battery may comprise several cells assembled, or in particular stacked, in an assembly direction. The assembly direction may be perpendicular to the plane formed by each cell.
[0020] In particular, the battery may correspond to a battery in which the cells are connected in series.
[0021] According to one embodiment, the cutting step can perform a cutting of connection wires between the positive electrodes along a cutting line located at the level, and in particular at the limit, of the second border, on the side of said electrical connection wires.
[0022] This embodiment makes it possible to retain, or not to remove, solid metallic lithium from the battery, when cutting the electrical connections, which makes it possible to improve the lithium recovery efficiency.
[0023] In this embodiment, the cutting of the connection wires must be sufficiently close to the second edge so that after cutting there is no longer any contact between the different positive electrodes.
[0024] According to another embodiment, the cutting step can cut the cells along a cutting line located at the level, and in particular at the limit, of the second border, on the side of said cells.
[0025] In this embodiment, in order to reduce the amount of lithium lost, the cutout must be in the immediate vicinity of the second edge.
[0026] For example, the cut can be made at a distance “d” from the second border less than or equal to 2mm, or less than or equal to 1% of the cell dimension between the first and second borders of the battery.
[0027] The cutting step can be carried out by trimming.
[0028] In this case, the battery is inserted into a cutter of suitable size and power.
[0029] According to embodiments, the cutting step can be carried out before the start of the heating step.
[0030] According to embodiments, the cutting step can be carried out after the start of the heating step. In this case, preferably, the cutting step can be carried out before the solid metallic lithium begins to melt.
[0031] According to embodiments, the cutting step can be carried out before the positioning step.
[0032] According to embodiments, the cutting step can be carried out after the positioning step.
[0033] According to embodiments, the cutting step can be carried out during the positioning step.
[0034] According to a particularly advantageous characteristic, the method according to the invention can further comprise, before the extraction phase, a step of electrically charging the battery, said extraction phase being applied to said charged battery.
[0035] Electrically charging the battery, and carrying out the extraction phase on the electrically charged cells, makes it possible to increase the lithium extraction efficiency. Indeed, electrically charging a cell makes it possible to move the lithium ions towards the negative electrode, which makes it possible to increase the quantity of recoverable lithium.
[0036] Each cell can be charged individually, or by electrically charging the battery.
[0037] According to a particularly advantageous embodiment, the extraction phase can further comprise a step of compressing the battery.
[0038] Thus, the molten lithium is forced out of each cell, which increases the amount of lithium recovered.
[0039] The compression step can be carried out continuously throughout the extraction phase. In this case, each cell is subjected to compression, in part or in full, throughout the duration of the extraction phase.
[0040] Alternatively, the compression step may be performed discretely, one or more times, during the extraction phase. In this case, the extraction phase includes times when the battery is not subjected to compression.
[0041] Advantageously, the compression step can apply compression to the surface of the battery by sweeping the surface of said battery from the second edge towards the first edge. Thus, the molten lithium is gradually brought / guided towards the first edge from which the negative electrodes protrude, which increases the quantity of lithium recovered and reduces the risk of contact between the lithium and the positive electrodes.
[0042] For example, the compression step can be carried out by passing the battery between two rollers.
[0043] According to another example, the compression step can be carried out by a compression roller compressing the battery against a support surface.
[0044] Compression may be applied in successive passes, each pass sweeping the surface of the battery starting from the second edge towards the first edge.
[0045] The space between the compression rollers, respectively between the compression roller and the bearing surface, may correspond to the thickness of the battery minus the thickness of the solid metallic lithium layers. This allows compression to be applied, as long as there is still solid lithium in the battery.
[0046] The space between the two compression rollers, respectively between the compression roller and the support surface, can be reduced with successive passes, so as to always apply compression to the battery.
[0047] The speed of passage between the compression rollers, respectively of the compression roller, and more generally the scanning speed, can be between a few mm to a few tens of mm, per second.
[0048] Furthermore, the method according to the invention may comprise, before the extraction phase, a step of removing at least one electrical connector from the battery, also called a “crimp” in English.
[0049] This makes it easier to process the battery.
[0050] Furthermore, the method according to the invention may comprise, before the extraction phase, a step of removing the overflow of material at the level of at least one, and particularly each, edge of the battery.
[0051] According to a first version, the positioning step can carry out a positioning of the battery in an orientation in which the first edge of said battery is located below the second edge of said battery.
[0052] Such an orientation of the battery, and therefore of each cell of the battery, makes it possible on the one hand to facilitate the flow of the molten lithium out of the cell by gravity, and on the other hand to avoid contact between the molten lithium and the positive electrodes or the current collector of the positive electrode, such contact being able to cause an electrical short circuit or an electric arc, such a short circuit being able to cause a fire.
[0053] According to a preferred embodiment of this first version, the positioning step can bring about a vertical positioning of the battery, in which the first edge is located downwards.
[0054] Thus, the flow of molten lithium out of each cell, by gravity, is improved.
[0055] In addition, the risk of contact between the molten lithium and the positive electrode(s) is reduced, or even zero.
[0056] Preferably, in this first version, the step of heating the battery can be carried out under inert gas.
[0057] Thus, the method according to the invention reduces the risk of accidents, in particular the risk of fire.
[0058] Furthermore, the method according to the invention makes it possible to avoid the formation of polluting compounds which can be generated by unwanted, or even uncontrolled, physicochemical reactions during the extraction of lithium.
[0059] According to a non-limiting exemplary embodiment, the inert gas may be, or comprise, any of the following gases: helium (He), neon (Ne), argon (Ar), krypton (Kr), xenon (Xe) and radon (Rn).
[0060] According to another embodiment of this first version, the step of heating the battery can be carried out under vacuum.
[0061] According to a second version, the positioning step can carry out a positioning of the battery in an orientation in which the first edge of said battery is located above the second edge of said battery. In this case, the extraction phase further comprises, before the heating step, a step of immersing the battery in a liquid, called a treatment liquid, denser than liquid lithium and electrically insulating.
[0062] This second version proposes a specific orientation of each cell, the latter being at least inclined, so that the first edge from which the negative electrodes protrude is above the level of the second edge, opposite the first edge, from which the positive electrodes protrude. Such an orientation of each cell makes it possible, on the one hand, to facilitate the flow of molten lithium out of the cell by difference in density, and on the other hand to avoid contact between the molten lithium and the positive electrodes or the current collectors of the positive electrodes, such contact being able to cause an electrical short circuit, such a short circuit being able to cause a fire. In addition, immersing the assembly of cell(s) in a liquid makes it possible to improve the dissipation of calories from the cell, in particular during a short circuit and therefore to greatly limit its effect.
[0063] In the present application, by "density" is meant the ratio between the density of the liquid considered and the density of water.
[0064] According to a preferred embodiment of this second version, the positioning step can bring about a vertical positioning of the battery, in which the second edge is located downwards.
[0065] Thus, the flow of molten lithium out of each cell, due to the difference in density, is improved.
[0066] In addition, the risk of contact between the molten lithium and the positive electrodes is reduced, or even zero.
[0067] Preferably, the immersion step can be carried out by immersing the battery completely in the treatment liquid.
[0068] The liquid may be a natural or synthetic oil, having the following physicochemical properties: - hydrophobic and non-reactive towards lithium, - electrical insulator, - having a density greater than that of lithium, - thermally stable beyond the melting temperature of lithium, i.e. 180.5°C, - a flash point, as well as an auto-ignition point, as high as possible.
[0069] According to another aspect of the same invention, there is provided an installation for extracting lithium from a battery, with solid or quasi-solid lithium electrolyte, comprising at least two electrical energy storage cells; each cell comprising a positive electrode, a negative electrode and solid or quasi-solid metallic lithium; said battery comprising a first edge from which the negative electrodes of said cells protrude and a second edge, opposite said first edge, and from which the positive electrodes protrude; said installation comprising: - means for positioning said battery in an orientation in which one of said first and second edges is below the other of said first and second edges; and - a heating means configured to heat said battery to a temperature, called treatment temperature, greater than or equal to the melting temperature of said solid metallic lithium; characterized in that it further comprises a means for cutting the electrical connection between the positive electrodes of at least two, and in particular of all, the cells of said battery.
[0070] Generally, the installation may comprise means configured to implement any combination of at least one of the characteristics described above, and which are not repeated here in detail for the sake of brevity.
[0071] For example, the cutting means may comprise a paper cutter.
[0072] In particular, the heating means may comprise an oven.
[0073] Advantageously, the oven can be filled with an inert gas, or be placed under vacuum, or even be filled with a treatment liquid denser than liquid lithium.
[0074] The installation according to the invention may further comprise a means for compressing the battery.
[0075] The compression means may comprise at least one roller.
[0076] In particular, the compression means may comprise a single roller compressing the battery against a bearing surface. The bearing surface may be heated to accelerate the temperature rise of the battery.
[0077] Alternatively, the compression means may comprise two rollers between which the battery is passed.
[0078] Generally, the compression means may be configured to apply continuous compression throughout the extraction phase.
[0079] Alternatively, the compression means may be configured to apply compression discretely over time, one or more times, during the extraction phase. In this case, the extraction phase includes times when the battery is not subjected to compression.
[0080] Advantageously, the compression means may be configured to apply compression, of constant or variable value, progressively or by sweeping over the surface of the battery, from the second edge towards the first edge. Thus, the molten lithium is gradually brought / guided towards the first edge in the lower position, which increases the quantity of lithium recovered and reduces the risk of contact between the lithium and the positive electrodes.
[0081] In the case of using one or two compression rollers, the compression can be applied to the battery in successive passes. Each pass applies a sweeping compression over the surface of the battery, from the second edge towards the first edge. At the end of each pass, the compression can be stopped, by moving the rollers apart or by moving the roller away from the support surface, to return to the second edge in order to start a new pass.
[0082] The distance between the rollers, respectively between the compression roller and the support surface, can be reduced as the passes progress, and in particular between two successive passes.
[0083] The invention can be implemented to treat several batteries, in particular several batteries forming a battery pack and connected to each other in parallel within said battery pack.
[0084] At least two batteries can be aligned side by side, without overlapping, by example in a direction parallel to the first border.
[0085] In this case, the compression can be applied to at least two batteries by the same compression means, namely a set of rollers, or a roller cooperating with a support surface. Description of figures and embodiments
[0086] Other advantages and characteristics will appear on examining the detailed description of non-limiting embodiments, and the appended drawings in which: - [Fig.l] is a schematic representation of a non-limiting exemplary embodiment of a cell within the meaning of the present invention; - [Fig.2] is a schematic representation of a non-limiting exemplary embodiment of a battery within the meaning of the present invention; - [Fig.3] is a schematic representation of a first non-limiting example of embodiment of a method according to the invention; - [Fig.4] is a schematic representation of a second example of embodiment of a method according to the invention; - [Fig.5] is a schematic representation of a third example of embodiment of a method according to the invention; - [Fig.6] is a schematic representation of a first non-limiting example of an installation according to the invention; - [Fig.7] is a schematic representation of a second non-limiting example of an installation according to the invention; and - FIGURES 8a and 8b are schematic representations of examples of electrical connection breaking between the positive electrodes of the battery cells, which can be implemented in the present invention.
[0087] It is understood that the embodiments which will be described below are in no way limiting. In particular, it will be possible to imagine variants of the invention comprising only a selection of characteristics described below, isolated from the other characteristics described, if this selection of characteristics is sufficient to confer a technical advantage or to differentiate the invention compared to the state of the prior art. This selection includes at least one preferably functional characteristic without structural detail, or with only a part of the structural details if this part is only sufficient to confer a technical advantage or to differentiate the invention compared to the state of the prior art.
[0088] In the figures, the elements common to several figures retain the same reference.
[0089] [Fig.l] is a schematic representation of an exemplary embodiment not limiting of a cell within the meaning of the present invention.
[0090] The cell 100, shown in [Fig.l], comprises a negative electrode 102 formed by, or comprising, a layer of solid metallic lithium.
[0091] The cell 100 further comprises a positive electrode 104.
[0092] A layer 106 of solid electrolyte is arranged between the negative electrode 102 and the positive electrode 104. This layer of solid electrolyte 106 may for example comprise lithium salt.
[0093] The positive electrode 104 is generally formed by a layer of composite based on polymer and active material. The cell 100 may further comprise a current collector 108 on the side of the positive electrode 104 and forming part of, or associated with, the positive electrode 104. The current collector 108 is generally made of aluminum.
[0094] Conventionally, the negative electrode 102 of the cell 100 protrudes beyond the other elements of the cell 100 on the side of a first edge 110 of the cell 100, here towards the right of the figure. The positive electrode 104 with current collector 108 protrudes beyond the other elements of the cell 100 on the side of a second edge 112, opposite the first edge 110. In the example shown, only the collector 108 protrudes over the second edge 112, here towards the left of the figure. In other examples, the protrusion could relate to only the positive electrode 104 or also to the positive electrode 104 and the collector 108.
[0095] Of course, the cell 100 shown in [Fig. 1] is a very simplified embodiment, given by way of illustration and in no way limiting. The cell within the meaning of the present invention may comprise layers other than those indicated, or more numerous layers, or layers whose composition is different from the composition given here by way of non-limiting example.
[0096] [Fig.2] is a schematic representation of a non-limiting exemplary embodiment of a battery comprising several cells.
[0097] The battery 200, shown in [Fig.2], comprises several identical cells 100r100n, assembled in a direction 202 perpendicular to the plane of the layers of each cell 100;.
[0098] Each cell 100; may be identical to cell 100 of [Fig.l].
[0099] The battery 200 comprises wires / tracks / connection lines 202 of the positive electrodes of all the cells 100r100n to each other. These connection lines 202 are connected to a connector 204 of the battery 200 forming the positive terminal of the battery 200. This connector 204 is also called a “crimp” in English.
[0100] The battery 200 comprises wires / tracks / connecting lines (not shown) of the negative electrodes of all the cells 100i-100n to each other. These connecting lines are connected to a connector (not shown) of the battery 200 forming the negative terminal of battery 200.
[0101] [Fig.3] is a schematic representation of a non-limiting exemplary embodiment of a method according to the invention.
[0102] The method 300, shown in [Fig. 3], comprises a first step 302, optional, during which the electrical connectors, and in particular the current concentrators also called “crimps” in English, of the battery, are removed.
[0103] During an optional step 304, overflows of material, and in particular of solid metallic lithium, at each lateral edge of the battery are removed.
[0104] Next, the method 300 comprises a phase 306 of extracting the metallic lithium from the battery cells.
[0105] The extraction phase 306 comprises a step 308 of positioning the battery in an orientation in which the first edge from which the negative electrodes protrude is at a lower level than the second edge from which the positive electrodes and / or the collectors protrude. In particular, step 308 positions the battery in a vertical orientation, i.e. parallel to the gravity vector, with the first edge from which the negative electrodes protrude downwards. Preferably, but in no way limiting, the battery is maintained in this orientation throughout the extraction phase 306.
[0106] The extraction phase 306 further comprises a step 310 of heating the battery to a treatment temperature greater than or equal to the melting temperature of the solid metallic lithium present in the battery, for example 180.5°C. This temperature will cause the melting of the solid metallic lithium and its extraction from each cell by natural flow under the effect of gravity. Preferably, but in no way limiting, the battery is maintained at this temperature throughout the extraction phase 306.
[0107] Advantageously, the heating step is carried out in a closed enclosure filled with inert gas.
[0108] The extraction phase 306 may further comprise an optional step 312 of compressing the battery in order to expel the molten lithium from each cell of the battery. The compression may be carried out continuously during all, or part, of the extraction phase 306. Alternatively, the compression step 312 may be repeated discretely several times during the extraction phase 306. Preferably, the compression step 312 applies the compression progressively, or by sweeping, over the surface of the battery, starting with the second edge from which the positive electrodes protrude and going towards the first edge from which the negative electrodes protrude.
[0109] In particular, the method 300 comprises a step 314 of cutting the electrical connection between the positive electrodes / current collectors of at least two, and in particular of all, the cells of the battery. Such a cutting step 314 makes it possible to cut the electrical connection between the positive electrodes of the cells of the battery, which makes it possible to reduce the reactivity of the battery. Thus, the risks of fire in the battery during the extraction phase are reduced, so that the recovery of the solid metallic lithium can be carried out in a safer and less risky manner.
[0110] In the example shown, the step 314 of cutting the electrical connections is carried out before the extraction phase 306. Alternatively, the step 314 of cutting can be carried out during the extraction phase 306, before, during or after the positioning step 308, or before, during or after the heating step 310.
[0111] Non-limiting examples of embodiments of a step of cutting the electrical connections between the positive electrodes of cells, which can be implemented in the present invention, are given in more detail with reference to FIGURES 8a and 8b.
[0112] [Fig.4] is a schematic representation of another non-limiting example of embodiment of a method according to the invention.
[0113] The method 400, shown in [Fig.4], comprises, like the method 300 of [Fig.3], the optional steps 302 of removing the electrical connectors from the battery and 304 of removing the overflows of solid lithium metal on each edge of the battery.
[0114] The method 400 then comprises the step 314 of cutting the electrical connections between the positive electrodes of the battery cells.
[0115] Next, the method 400 comprises a phase 406 of extracting metallic lithium from the cells.
[0116] The extraction phase 406 comprises a step 408 of positioning the battery in an orientation in which the first edge 110 from which the negative electrodes 102 protrude is at a higher level, in a vertical direction, than the second edge 112 from which the positive electrodes 104 and the collectors protrude. In particular, step 408 positions the battery in a vertical orientation, that is to say parallel to the gravity vector, with the first edge 110 from which the negative electrodes protrude upwards. Preferably, but in no way limiting, the battery is maintained in this orientation throughout the extraction phase 406.
[0117] The extraction phase 406 comprises a step 410 of immersing the battery in a treatment liquid, neutral, and denser than liquid lithium. For example, the treatment liquid may be a natural or synthetic oil, for example a paraffin oil, having the following physicochemical properties: - hydrophobic and non-reactive with respect to lithium, - electrical insulator, - a density higher than that of lithium, - thermally stable beyond the melting temperature of lithium, i.e. 180.5°C, and - a flash point, as well as an auto-ignition point, as high as possible, for example a temperature above 600°C, and at least higher than the cell treatment temperature.
[0118] The immersion step 410 is performed by immersing the battery in the treatment liquid such that said treatment liquid completely covers the battery.
[0119] This immersion step 410 is particularly advantageous in promoting significant heat exchange between the battery and the treatment liquid, which limits the risks of overheating of the battery and the evacuation of calories generated during a short circuit and improves the heating kinetics.
[0120] The extraction phase 406 further comprises the heating step 310 described above, and may optionally comprise the compression step 312 described above.
[0121] During the heating step, the treatment temperature must not exceed a degradation temperature of the treatment liquid, beyond which the treatment liquid degrades. In other words, the treatment liquid, by exceeding a threshold temperature, would change its property so that the properties stated above are no longer satisfied. Ideally, the degradation temperature of the treatment liquid must be +40°C higher, and for example between +20°C and +60°C, compared to the melting temperature of lithium.
[0122] [Fig.5] is a schematic representation of another non-limiting example of embodiment of a method according to the invention.
[0123] The method 500, shown in [Fig.5], comprises all the steps of the method 300 of [Fig.3], respectively of the method 400 of [Fig.4].
[0124] The method 500 further comprises, prior to the steps of the method 300, respectively of the method 400, a step 502 carrying out an electrical recharging of at least one cell of the battery.
[0125] Said at least one cell can be partially or totally recharged.
[0126] Electrically charging a cell increases the amount of lithium available for extraction because electrical recharging causes lithium ions to migrate toward the negative electrode of said cell.
[0127] [Fig.6] is a schematic representation of a non-limiting example embodiment of an installation according to the invention.
[0128] The installation 600, shown in [Fig. 6], can be used to implement the method according to the invention, and in particular the methods 300 and 500 of FIGURES 3 and 5.
[0129] The installation 600 makes it possible to extract and recover part or all of the lithium from the cells of a battery comprising solid metallic lithium, such as for example the battery 200 of [Fig.2].
[0130] The installation 600 comprises an oven 602, filled with an inert gas or placed under vacuum, configured to heat the battery to a treatment temperature, greater than or equal to the melting temperature of the solid metallic lithium present in the cells, for example 180.5°C or 181°C.
[0131] The installation 600 comprises a pair of clamps 604 for holding the battery 200 in a vertical, or at least inclined, position, in which the first edge 110 is positioned below the level of the second edge 112. Each clamp 604 is movably mounted on a vertical rail 606 so as to move the battery 200 vertically.
[0132] The installation 600 further comprises a pair of rollers 608, having between them a spacing corresponding to the thickness of the battery 200 minus the thickness of the solid layers of metallic lithium. The pair of rollers 608 is positioned so that, when the clamps 604 are moved upwards, the battery 200 passes between the rollers 608 starting with the second edge 112. Thus, the rollers apply compression to the battery 200, progressively starting with the second edge 112 and going towards the first edge 110.
[0133] The installation further comprises a receptacle 610 for recovering the molten metallic lithium which flows out of each cell under the effect of gravity. The receptacle 610 must be inert with respect to lithium.
[0134] Advantageously, the installation 600 further comprises a means 612 for cutting the electrical connections between the positive electrodes of the battery.
[0135] In the example shown, the cutting means 612 is arranged in the oven 602. Alternatively, the cutting means 612 can be arranged outside the oven 602. For example, the cutting means 612 can be arranged above the oven 602 or on the side of the oven or even at a distance from the oven 602.
[0136] In the example shown, the cutting means 612 is a cutter provided for cutting the electrical connections. The battery 200 is arranged between the jaws of the cutter on the side of its second edge, for example by means of the clamps 604. The cutter 612 is then actuated to cut the electrical connections between the positive electrodes of the battery cells.
[0137] Alternatively, the cutting means 612 may be shears, a grinder, a laser cutting means, and more generally any suitable cutting means.
[0138] [Fig.7] is a schematic representation of another non-limiting example of an installation according to the invention.
[0139] The installation 700, shown in [Fig.7], can be used to implement the method according to the invention, and in particular the methods 400 and 500 of FIGURES 4 and 5.
[0140] The installation 700 includes all the elements of the installation 600 of [Fig. 6], except for the differences indicated below.
[0141] In the installation 700, the clamps 604 are configured to orient the battery 200, in an inclined manner and preferably vertically, with the first edge 110 of the battery 200 above the second edge 112.
[0142] In addition, the oven 602 does not include a recovery receptacle 610.
[0143] Further, the pair of rollers 608 is positioned above the battery 200 to apply compression from the second edge 112 of the battery 200 toward the first edge 110 of the battery 200.
[0144] Furthermore, the oven 602 is filled with a treatment liquid 702 completely covering the battery 200. The treatment liquid 702 is electrically insulating and inert with respect to lithium, and above all denser than the molten lithium. This treatment liquid 702, denser than lithium, makes it possible to guide the molten lithium towards the first edge 110 so that the molten lithium leaves the battery and ends up at the surface of the treatment liquid 702, and is recovered there.
[0145] In the present invention, the cutting of the electrical connections between the positive electrodes of the battery cells can be carried out in different ways.
[0146] [Fig.8a] gives a first example of the embodiment of a cutting of the electrical connections between the positive electrodes of the battery which can be implemented in the present invention.
[0147] In the example shown, the cutting is carried out along a cutting line 802 located at the level, and in particular at the limit, of the second edge 112, on the side of the cells 100r100n of the battery 200. In other words, in this example, the cells forming the battery are cut at the level of the second edge of the battery.
[0148] In order to reduce the quantity of lithium lost, the cutting can be carried out in the immediate vicinity of the second edge 112. For example, the cutting can be carried out at a distance from the second edge 112 less than or equal to 2 mm, or less than or equal to 1% of the dimension of the cells between the first edge 110 and the second edge 112 of the battery 200.
[0149] [Fig.8b] gives another example of the embodiment of a cutting of the electrical connections between the positive electrodes of the battery which can be implemented in the present invention.
[0150] In the example shown, the cutting is carried out along a cutting line 804 located at the level, and in particular at the limit, of the second border 112, on the side of the electrical connection wires 202. In other words, in this example, the cells forming the battery are not cut.
[0151] This exemplary embodiment makes it possible to retain, or not to remove, solid metallic lithium from the battery when cutting the electrical connections between the positive electrodes of the cells, which makes it possible to improve the lithium recovery efficiency.
[0152] In this exemplary embodiment, the cutting of the connection wires 202 must be sufficiently close to the second edge 112 so that after the cutting, there is no longer any contact between the positive electrodes.
[0153] Of course, the invention is not limited to the examples detailed above.
[0154] For example, the composition of each cell may be different from that indicated in [Fig.l],
[0155] Furthermore, the installation according to the invention may comprise devices other than those shown in FIGURES 6 or 7, such as for example means for cutting the electrical connectors of the battery, means for cutting the overhangs on one, or on each, of the edges.
[0156] Alternatively to what is described, the clamps 604 can be fixed, and it is the rollers 608, respectively the cutter 612, which can be movable.
[0157] Furthermore, the invention is not limited to the embodiments described above, but can be applied to solid or quasi-solid electrolyte batteries not comprising a polymer at the cathode. The invention can be applied to any battery having a solid or quasi-solid electrolyte and a cathode stable up to the temperature of the melting point of the solid or quasi-solid electrolyte component.
Claims
Claims
1. Method (300;400;500) for extracting lithium from a battery (200), with solid or quasi-solid lithium electrolyte comprising at least two cells (100) for storing electrical energy; each cell comprising a negative electrode (102), a positive electrode (104;108) and solid (106) or quasi-solid metallic lithium; said battery comprising a first edge (110) from which the negative electrodes (102) of said cells protrude and a second edge (112), opposite (112) to said first edge (110), and from which the positive electrodes (104) protrude; said method (300;400;500) comprising an extraction phase (306;406) comprising the following steps: - positioning (308;408) of said battery (200) in an orientation in which one (110;112) of said first and second edges is located below the other (112;110) of said first and second edges, and - heating (310) of said battery (200) to a temperature, called treatment temperature, greater than or equal to the melting temperature of said solid metallic lithium; characterized in that it further comprises a step (314) of cutting the electrical connection between the positive electrodes of at least two, and in particular of all, the cells (100) of said battery (200): - before the start of the heating step (310), or - after the start of the heating step (310), before solid metallic lithium begins to melt.;
2. Method (300;400;500) according to the preceding claim, characterized in that the cutting step (314) cuts connection wires between the positive electrodes along a cutting line (802) located at the level, and in particular at the limit, of the second edge (112), on the side of said electrical connection wires.
3. Method (300;400;500) according to any one of the preceding claims, characterized in that the cutting step carries out a cutting of the cells along a cutting line (804) located at the level, and in particular at the limit of the second border (112), on the side of said cells.
4. Method (300;400;500) according to any one of the preceding claims, characterized in that the cutting step (314) is carried out by trimming.
5. Method (500) according to any one of the preceding claims, characterized in that it further comprises, before the extraction phase (306;406), a step (502) of electrically charging the battery (200), said extraction phase (306;406) being applied to said charged battery (200).
6. Method (300;400;500) according to any one of the preceding claims, characterized in that the extraction phase (306;406) further comprises a step (312) of compressing the battery (200).
7. Method (300; 400; 500) according to any one of the preceding claims, characterized in that it comprises, before the extraction phase (306; 406), a step (302) of removing at least one electrical connector from the battery (100).
8. Method (300;500) according to any one of the preceding claims, characterized in that the positioning step (308) performs a positioning of the battery (200) in an orientation in which the first edge (110) of said battery is located below the second edge (112) of said battery (200).
9. Method (300; 500) according to the preceding claim, characterized in that the positioning step (308) places the battery (200) in a vertical position, in which the first edge (110) is located downwards.
10. Method (300; 500) according to any one of claims 8 or 9, characterized in that the step of heating (310) the battery (200) is carried out under inert gas or under vacuum.
11. Method (400; 500) according to any one of claims 1 to 7, characterized in that the positioning step (408) performs a positioning of the battery (200) in an orientation in which the first edge (110) of said battery is located above the second edge (112) of said battery, and in that the extraction phase (406) further comprises, before the heating step (310), a step (410) of immersing the battery (200) in a liquid (702), called treatment liquid, denser than liquid lithium and electrically insulating.
12. Installation (600;700) for extracting lithium from a battery (200),
13.
14.
15. solid or quasi-solid lithium electrolyte, comprising at least two electrical energy storage cells (100); each cell comprising a negative electrode (102), a positive electrode (104;108) and solid (106) or quasi-solid metallic lithium; said battery comprising a first edge (110) from which the negative electrodes (102) of said cells protrude and a second edge (112), opposite (112) to said first edge (110), and from which the positive electrodes (104) protrude; said installation (600;700) comprising: - means (604) for positioning said battery (200) in an orientation in which one (110; 112) of said first and second edges is below the other (112; 110) of said first and second edges; and - a heating means (602) configured to heat said battery (200) to a temperature, called treatment temperature, greater than or equal to the melting temperature of said solid metallic lithium; characterized in that it further comprises means (612) for cutting the electrical connection between the positive electrodes of at least two, and in particular of all, the cells (100) of said battery (200): - before the start of the heating step (310), or - after the start of the heating step (310) before lithium solid metal begins to melt. Installation (600; 700) according to the preceding claim, characterized in that the cutting means (612) comprises a cutter. Installation (600; 700) according to any one of claims 12 or 13, characterized in that the heating means comprises an oven (502). Installation (500) according to any one of claims 12 to 14, characterized in that it comprises a means of compression (508) of the battery (200).