RECYCLABLE AND SORTED THERMOPLASTIC COMPOSITION
Incorporating lignin-based fillers into thermoplastic compositions addresses the sorting and recycling challenge by ensuring detectability in NIR systems, allowing for effective recycling while maintaining a dark color.
Patent Information
- Application Number
- FR2022010847
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-10-21
- Filing Date
- 2022-10-20
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-10-20
AI Technical Summary
Carbon black-filled polymer compositions cannot be sorted and recycled in recycling facilities due to high absorbance that masks polymer detection by near-infrared (NIR) systems.
Incorporating a lignin-based filler into thermoplastic compositions to achieve a specific color representation (L ≤ 36, a ≤ 10, b ≤ 15) and a maximum reflection intensity of ≥ 5% in the NIR wavelength range, enabling detection and sorting by NIR systems.
The lignin-based filler allows the thermoplastic composition to be distinguished and sorted from a mixture of articles, facilitating recycling and maintaining a black color similar to carbon black compositions.
Smart Images

Figure 00000025_0000 
Figure 00000025_0001 
Figure 00000026_0000
Abstract
Description
Title of the invention: RECYCLABLE AND SORTED THERMOPLASTIC COMPOSITION FIELD OF THE INVENTION
[0001] The present disclosure relates to a thermoplastic composition. The present disclosure further relates to a method of producing a thermoplastic composition comprising at least one polymer and a lignin-based filler. The present disclosure further relates to the use of a lignin-based filler. The present disclosure further relates to an article and use of the thermoplastic composition. BACKGROUND OF THE INVENTION
[0002] From a sustainability and circular economy perspective, it is desirable to recycle thermoplastic compositions or materials, such as packaging materials, in a closed loop. Carbon black is commonly used as the pigment or filler in black colored plastics. However, carbon black filled polymer compositions cannot be sorted and recycled in recycling facilities because detection of the polymer used in the thermoplastic composition with a near infrared (NIR) detection system is not possible due to the high absorbance of carbon black. The inventors have therefore recognized the need for alternative black coloring fillers or pigments, which allow sorting of the polymers in the composition and thus enable recycling of the thermoplastic composition. SUMMARY
[0003] A thermoplastic composition comprising at least one polymer and a lignin-based filler is disclosed. The color of the thermoplastic composition is represented by an L value of at most 36, an a value of at most 10 and a b value of at most 15 as determined by DIN EN ISO 11664. The thermoplastic composition has a maximum reflection intensity value, in the near infrared wavelength range of 1450 to 2450 nm of the electromagnetic spectrum, which is greater than or equal to a reflection intensity of 5% when determined by a near infrared detection system.
[0004] Further disclosed is a method of producing a thermoplastic composition comprising at least one polymer and a lignin-based filler, wherein the method comprises combining the at least one polymer and the lignin-based filler to form a thermoplastic composition, wherein
[0005] - the color of the thermoplastic composition is represented by a value L of at least plus 36, an a value of at most 10 and a b value of at most 15 as determined by DIN EN ISO 11664; and
[0006] - the thermoplastic composition has a reflection intensity value maximum, in the near-infrared wavelength range of 1450 to 2450 nm of the electromagnetic spectrum, which is greater than or equal to a reflection intensity of 5% when determined by a near-infrared detection system.
[0007] Further disclosed is the use of the lignin-based filler for the production of a thermoplastic composition comprising at least one polymer and the lignin-based filler, wherein
[0008] - the color of the thermoplastic composition is represented by a value L of at least plus 36, an a value of at most 10 and a b value of at most 15 as determined by DIN EN ISO 11664; and
[0009] - the thermoplastic composition has a reflection intensity value maximum, in the near infrared wavelength range of 1450 to 2450 nm of the electromagnetic spectrum, which is greater than or equal to a reflection intensity of 5% when determined by a near infrared detection system, and wherein the thermoplastic composition can be detected by a near infrared detection system such that the thermoplastic composition can be sorted from a mixture of articles.
[0010] An article comprising the thermoplastic composition as defined in the present description is disclosed.
[0011] The use of the thermoplastic composition as defined in the present description in a package, a housing, an automotive part, an aeronautical part, a marine part, a machine part, a sports equipment, a sports equipment part, a leisure equipment, a leisure equipment part, a tool, a part of a tool, a pipe, a membrane, a tube, a fitting, a bottle, a film, a sachet, a bag, a textile, a rope, a container, a tank, an electrical component, an electronic component, a part for energy production, a toy, a household appliance, a kitchen utensil, tableware, a floor covering, a fabric, a medical application, a food contact material, a building material, a drinking water application and / or furniture is further disclosed. Brief description of the drawings
[0012] The accompanying drawings, which are included to provide a better understanding of the embodiments and constitute a part of this description, illustrate various embodiments. In the drawings:
[0013] [Fig.1a], [Fig.1b], [Fig.2], [Fig.3a], [Fig.3b], [Fig.4], [Fig.5], [Fig.6a], [Fig.6b] and [Fig.7] disclose the results of the intensity measurements, in the near infrared, carried out in the examples. DETAILED DESCRIPTION
[0014] A thermoplastic composition comprising at least one polymer and a lignin-based filler is disclosed. The color of the thermoplastic composition is represented by an L value of at most 36, an a value of at most 10 and a b value of at most 15 as determined by DIN EN ISO 11664. The thermoplastic composition has a maximum reflection intensity value, in the near infrared wavelength range of 1450 to 2450 nm of the electromagnetic spectrum, which is greater than or equal to a reflection intensity of 5% when determined by a near infrared detection system.
[0015] A method of producing a thermoplastic composition comprising at least one polymer and a lignin-based filler is disclosed, wherein the method comprises combining the at least one polymer and the lignin-based filler to form a thermoplastic composition, wherein
[0016] - the color of the thermoplastic composition is represented by a value L of at least plus 36, an a value of at most 10 and a b value of at most 15 as determined by DIN EN ISO 11664; and
[0017] - the thermoplastic composition has a reflection intensity value maximum, in the near-infrared wavelength range of 1450 to 2450 nm of the electromagnetic spectrum, which is greater than or equal to a reflection intensity of 5% when determined by a near-infrared detection system.
[0018] The use of the lignin-based filler for the production of a thermoplastic composition comprising at least one polymer and the lignin-based filler is disclosed, wherein
[0019] - the color of the thermoplastic composition is represented by a value L of at least plus 36, an a value of at most 10 and a b value of at most 15 as determined by DIN EN ISO 11664; and
[0020] - the thermoplastic composition has a reflection intensity value maximum, in the near infrared wavelength range of 1450 to 2450 nm of the electromagnetic spectrum, which is greater than or equal to a reflection intensity of 5% when determined by a near infrared detection system, and wherein the thermoplastic composition can be detected by a near infrared detection system such that the thermoplastic composition can be sorted from a mixture of articles.
[0021] The term "mixture of articles" is to be understood in this description, unless otherwise indicated, as referring to a mixture comprising articles of different origin. Articles of different origin may be, for example, articles of different types of thermoplastic compositions. The mixture of articles may contain different types of thermoplastic compositions prepared from different polymers and fillers.
[0022] An article comprising the thermoplastic composition as defined in the present specification is further disclosed. In one embodiment, the thermoplastic composition has been formed into an article by extrusion, injection molding, compression molding, blow molding, injection blow molding, injection stretch blow molding, thermoforming, vacuum forming, melt spinning, electrospinning, melt blowing, film blowing, film casting, extrusion coating, rotational molding, coextrusion, lamination, calendering, fused deposition, or any combination thereof.
[0023] The use of the thermoplastic composition as defined in the present description in a package, a housing, an automotive part, an aeronautical part, a marine part, a machine part, a sports equipment, a sports equipment part, a leisure equipment, a leisure equipment part, a tool, a part of a tool, a pipe, a membrane, a tube, a fitting, a bottle, a film, a sachet, a bag, a textile, a rope, a container, a tank, an electrical component, an electronic component, a part for energy production, a toy, a household appliance, a kitchen utensil, tableware, a floor covering, a fabric, a medical application, a food contact material, a building material, a drinking water application and / or furniture is further disclosed.
[0024] In one embodiment, the thermoplastic composition is a recyclable and sortable thermoplastic composition. In one embodiment, the thermoplastic composition is a recyclable thermoplastic composition. In one embodiment, the method comprises producing a recyclable and sortable thermoplastic composition. In one embodiment, the method comprises producing a recyclable thermoplastic composition.
[0025] The expression: the thermoplastic composition is "sortable", should be understood in this description, unless otherwise indicated, as referring to the possibility of sorting the thermoplastic composition from the mixture of articles and thus allowing the recycling and reuse of the thermoplastic composition.
[0026] In one embodiment, the thermoplastic composition may be detected by a near-infrared detection system such that the thermo- plastic can be sorted from a mixture of items.
[0027] In one embodiment, the thermoplastic composition does not comprise carbon black.
[0028] The inventors have surprisingly discovered that by using a lignin-based material as a filler in a thermoplastic composition, in the absence of carbon black, it is possible to detect the thermoplastic composition by a near-infrared detection system and the thermoplastic composition can thus be sorted after use from a mixture of articles. The inventors have surprisingly discovered that the lignin-based filler does not mask the polymer in the thermoplastic composition as is the case when, for example, carbon black is used as a filler, which allows the use of a near-infrared detection system to recognize the thermoplastic composition.
[0029] The maximum reflection intensity value in the near-infrared wavelength range can be determined using a near-infrared measuring device. In near-infrared (NIR) spectroscopy, unique characteristics of the material or composition under study are observed by illuminating the material with a specific wavelength of infrared light. A specific pattern of this invisible light is reflected from the object, and this pattern is unique for each material, i.e., like a fingerprint. Infrared light can be detected by infrared detectors that convert the reflected radiation into an electrical signal that can be presented graphically.
[0030] Thus, the thermoplastic composition, when subjected to near-infrared illumination, can be characterized by a reflection pattern and can thus exhibit a maximum reflection intensity value in the near-infrared. From this reflection pattern, the highest peak, i.e., the maximum reflection intensity value, can be determined. The maximum reflection intensity value in the near-infrared wavelength range can thus be determined by a near-infrared measuring device. The near-infrared detection system can be a near-infrared spectroscopy device. As an example of a near-infrared measuring system, mention may be made of the one provided by trinamiX GmbH (Ludwigshafen, Germany), i.e., the trinamiX NIR Spectrometer (software package: general plastic).The near-infrared device may comprise at least one illumination source, a detector, and a software package for processing the measured signals into graphs, for example, reflection graphs in a certain wavelength region. The software package may also comprise a reference library of data for different polymers, thus enabling the software to compare the measurement results to the data in the bi . library and provide feedback on the type of polymer. This can be called "evaluation".
[0031] In one embodiment, the thermoplastic composition has a maximum reflection intensity value, in the near infrared wavelength range of 1450 to 2450 nm of the electromagnetic spectrum, that is greater than or equal to a reflection intensity of 8%, or 10%, or 15%, or 20%, or 25% when determined by a near infrared detection system. In one embodiment, the thermoplastic composition has a maximum reflection intensity value in the near infrared in the wavelength range of 1450 to 2450 nm, or in the wavelength range of 1450 to 2100 nm, or in the wavelength range of 1450 to 1800 nm, of the electromagnetic spectrum.In one embodiment, the thermoplastic composition has a near infrared peak reflection intensity value in the wavelength range of 1450 to 2450 nm, or in the wavelength range of 1450 to 2100 nm, or in the wavelength range of 1450 to 1800 nm, of the electromagnetic spectrum that is greater than or equal to a reflection intensity of 5%, or 8%, or 10%, or 15%, or 20%, or 25% when determined by a near infrared detection system.
[0032] In one embodiment, the thermoplastic composition has a near infrared (NIR) specimen contrast that is greater than or equal to 3.0, or 5.0, or 6.0, or 9.0, in the wavelength range of 1450 to 2450 nm. The NIR specimen contrast describes the ability of spectral features such as bands or fingerprints to stand out from the background or other adjacent details and can be determined by the relationship between the highest and lowest intensity in the NIR spectrum by the following equation:
[0033] (Imax - Imin) / Imin
[0034] in which
[0035] Imax = maximum intensity (highest intensity)
[0036] Imin = minimum intensity (lowest intensity)
[0037] A thermoplastic composition, or a thermo-softenable plastic composition as it may also be called, is a plastic polymer material that becomes pliable or moldable at a certain elevated temperature and solidifies upon cooling.
[0038] The thermoplastic composition may be prepared using a polymer and a lignin-based filler. Other components or materials, such as additives, lubricants, stabilizers, antioxidants, other fillers, etc., may also be used to prepare the thermoplastic composition.
[0039] In one embodiment, the combination of the at least one polymer and the lignin-based filler comprises preparing a masterbatch and subsequently composing the masterbatch with the same or a different polymer and optionally other additives, combining the at least one polymer and the lignin-based filler comprises preparing a masterbatch and subsequently composing the masterbatch with the at least one polymer. In one embodiment, combining the at least one polymer and the lignin-based filler comprises directly composing the polymer and the lignin-based filler.
[0040] In preparing the thermoplastic composition, a so-called masterbatch may first be prepared using a polymer and the lignin-based filler. The masterbatch may be prepared by mixing the polymer and the lignin-based filler at an elevated temperature. Also other additives, lubricants, stabilizers, antioxidants, other fillers, etc. as required may also be included in the masterbatch. A masterbatch is generally considered to be a solid product (normally plastic, rubber or elastomer) in which pigments or fillers are optimally dispersed at a high concentration in a carrier material. The carrier material is compatible with the main plastic material into which it will be mixed during molding, whereby the final plastic product, i.e. the thermoplastic composition, obtains the color or properties of the masterbatch.
[0041] Alternatively, the thermoplastic composition is directly compounded at an elevated temperature from the polymer and the lignin-based filler. In addition, other additives, lubricants, stabilizers, antioxidants, other fillers, etc. as required may be directly compounded with the polymer and the lignin-based filler.
[0042] The temperature used when combining the at least one polymer and the lignin-based filler may vary depending on the type of polymer used. The appropriate temperature to be used for each polymer is readily available to those skilled in the art. In addition, polymer suppliers define appropriate processing temperatures for different polymers. Generally, temperatures ranging from, for example, 150 to 440°C, or 180 to 350°C, or 200 to 300°C, may be used.
[0043] The thermoplastic composition may contain 0.1 to 65% by weight, or 0.3 to 60% by weight, or 0.5 to 50% by weight, or 1 to 40% by weight, or 1.2 to 30% by weight, or 1.5 to 20% by weight, or 2 to 10% by weight, or 2.5 to 5% by weight, of the lignin-based filler relative to the total weight of the thermoplastic composition.
[0044] "Total weight" is to be understood in this description, unless otherwise indicated, as being the weight of all components of the thermoplastic composition, including any moisture.
[0045] The thermoplastic composition may comprise at least one polymer, for example for example, at least two different polymers, at least three different polymers, at least four different polymers, etc. The thermoplastic composition may comprise one polymer or a single polymer.
[0046] In one embodiment, the thermoplastic composition comprises a polymer and a lignin-based filler. In one embodiment, the thermoplastic composition comprises a polymer and a lignin-based filler.
[0047] The polymer may be any polymer selected from the group of thermoplastic polymers or a combination of different thermoplastic polymers. The polymer may be polyethylene, polypropylene, polystyrene, ethylene vinyl acetate (EVA), polybutylene adipate terephthalate (PBAT), polyamide, a polyacrylate, a polyester, acrylonitrile butadiene styrene (ABS), polycarbonate, polylactic acid (PLA), polyvinyl chloride (PVC), or any combination or mixture thereof. That is, one type of polymer may be used to produce the thermoplastic composition or a combination of two or more different polymers may be used.
[0048] The term "lignin-based feedstock" is to be understood in this specification, unless otherwise indicated, as referring to a feedstock that has been prepared from lignin. That is, a lignin material has been used to prepare the lignin-based feedstock. In one embodiment, the lignin-based feedstock comprises or consists of lignin. In one embodiment, the lignin-based feedstock is prepared from lignin subjected to a hydrothermal carbonization treatment.The lignin used to prepare the lignin-based feedstock may be selected from a group consisting of kraft lignin, steam explosion lignin, biorefinery lignin, supercritical separation lignin, hydrolysis lignin, flash precipitated lignin, lignin from biomass, lignin from an alkaline pulping process, lignin from the soda process, lignin from organosolv pulping, lignin from an alkali process, lignin from an enzymatic hydrolysis process, and any combination thereof. In one embodiment, the lignin is a wood-derived lignin. The lignin may be derived from softwood, hardwood, annual plants, or any combination thereof.
[0049] In this specification, unless otherwise indicated, the term "kraft lignin" means lignin that is derived from kraft black liquor. Black liquor is an aqueous alkaline solution of lignin residues, hemicellulose, and inorganic chemicals used in a kraft pulping process. Black liquor from the pulping process includes components from different softwood and hardwood species in various proportions. Lignin can be separated from black liquor by various techniques, including, for example, preci pitation and filtration. Lignin generally begins to precipitate at pH values below 11 - 12. Different pH values can be used to precipitate lignin fractions with different properties. These lignin fractions differ from each other in molecular weight distribution, e.g., Mw and Mn, polydispersity, hemicellulose and extractive contents. The molar mass of lignin precipitated at a higher pH value is higher than the molar mass of lignin precipitated at a lower pH value. In addition, the molecular weight distribution of the lignin fraction precipitated at a lower pH value is broader than that of the lignin fraction precipitated at a higher pH value. Precipitated lignin can be purified from inorganic impurities, hemicellulose and wood extractives using acid washing steps.Further purification can be achieved by filtration.
[0050] The term "flash-precipitated lignin" is to be understood in this specification as lignin that has been precipitated from black liquor in a continuous process by decreasing the pH of a black liquor stream, under the influence of an overpressure ranging from 200 to 1000 kPa, to the lignin precipitation level using a carbon dioxide acidifying agent, preferably carbon dioxide, and abruptly releasing the pressure to precipitate the lignin. The process for producing flash-precipitated lignin is disclosed in patent application FI 20106073. The residence time in the above process is less than 300 s. Flash-precipitated lignin particles, having a particle diameter of less than 2 μm, form agglomerates, which can be separated from the black liquor using, for example, filtration.The advantage of flash-precipitated lignin is its greater reactivity compared to normal kraft lignin. Flash-precipitated lignin can be purified and / or activated if necessary for further processing.
[0051] Lignin can be derived from an alkali process. The alkali process can begin with the liquefaction of biomass with a strong alkali followed by a neutralization process. After the alkali treatment, the lignin can be precipitated in a manner similar to that presented above.
[0052] Lignin can be derived from steam explosion. Steam explosion is a pulping and extraction technique that can be applied to wood and other fibrous organic material.
[0053] In this specification, unless otherwise indicated, "biorefinery lignin" means lignin that can be recovered from a refining facility or process where biomass is converted into fuel, chemicals, and other materials.
[0054] In this specification, unless otherwise indicated, the term "supercritical separation lignin" means lignin that can be recovered from biomass using a supercritical fluid separation or extraction technique. Supercritical conditions correspond to the temperature and pressure above the critical point for a given substance. Under supercritical conditions, separate liquid and gas phases do not exist. Supercritical water or liquid extraction is a process for breaking down and converting biomass into cellulosic sugar using water or a liquid under supercritical conditions. The water or liquid, acting as a solvent, extracts the sugars from the cellulosic plant material and the lignin remains as a solid particle.
[0055] Lignin may be derived from a hydrolysis process. Lignin derived from the hydrolysis process may be recovered from chemical processes on paper pulp or wood.
[0056] Lignin can be derived from an organosolv process. Organosolv is a pulping technique that uses an organic solvent to solubilize lignin and hemicellulose.
[0057] In one embodiment, the lignin-based feedstock comprises or consists of lignin. In one embodiment, the lignin-based feedstock is prepared from lignin subjected to a hydrothermal carbonization (HTC) treatment. Hydrothermal carbonization treatment of lignin refers to a process for thermochemical conversion of a lignin-containing material in an aqueous suspension. The hydrothermal carbonization treatment of lignin produces lignin derivatives having a high carbon content and functional groups.
[0058] In one embodiment, the lignin-based feedstock is prepared from lignin derived from an enzymatic hydrolysis process and / or a Kraft process.
[0059] In one embodiment, the lignin-based feedstock is prepared from lignin derived from an enzymatic hydrolysis process and / or a Kraft process and subjected to the hydrothermal carbonization treatment. In one embodiment, the lignin-based feedstock is prepared from lignin derived from an enzymatic hydrolysis process and subjected to the hydrothermal carbonization treatment. In one embodiment, the lignin-based feedstock is prepared from lignin derived from a Kraft process and subjected to the hydrothermal carbonization treatment.
[0060] In one embodiment, the enzymatic hydrolysis process comprises enzymatically hydrolyzing a plant-derived feedstock, such as a wood-based feedstock. In one embodiment, the enzymatic hydrolysis process comprises enzymatically hydrolyzing cellulose. In one embodiment, the lignin-based feedstock is prepared from lignin derived from wood pulping, e.g., kraft lignin.
[0061] The paste suspension comprising a lignin-based feedstock as disclosed in the present specification may be prepared as described below. The lignin to be used may be derived, for example, from a process in which lignin is formed upon enzymatic hydrolysis of a lignocellulosic feedstock or the lignin may be derived from a Kraft process. Other sources of lignin may also be used.
[0062] The derived lignin may be dissolved in an alkaline solution, such as NaOH. Dissolution may be accomplished by heating the mixture of lignin and alkaline solution to about 80°C, adjusting the pH to a value above 7, such as 9 to 11, and mixing the mixture of lignin and alkaline solution for a predetermined time. Mixing may be continued for about 2 to 3 hours. The exact pH value is determined based on the target product quality.
[0063] The dissolved lignin can then be subjected to a hydrothermal carbonization (HTC) treatment.
[0064] The hydrothermal carbonization treatment may take place in one reactor (HTC reactor), or if necessary, in several parallel reactors, operating discontinuously. The dissolved lignin may be preheated before being introduced into the HTC reactor(s). The temperature in the HTC reactor(s) may be between 150 and 250°C and the pressure may be between 20 and 30 bar. The residence time in the HTC reactor(s) may be between about three and six hours. In the HTC reactor, the lignin is carbonized, whereby a stabilized lignin derivative with a high specific surface area may be precipitated. The formed pasty suspension comprising the carbonized lignin may then be removed and cooled.
[0065] Therefore, a pasty suspension comprising a lignin-based filler is formed.
[0066] The pasty suspension comprising a lignin-based feedstock may be introduced into a separation unit, where the precipitated lignin may be separated from the pasty suspension. The separated lignin-based feedstock may be dried and recovered. Before drying, the lignin-based feedstock may be, if necessary, washed. The recovered lignin-based feedstock may be further processed, for example, crushed, further dried, ground, etc., before being used as a lignin-based feedstock.
[0067] During the process described above, lignin polymers are linked together. Thus, the lignin-based feedstock can be considered to comprise or consist of lignin polymers that are linked together. Lignin polymers that are linked or linked together may no longer be soluble. However, smaller chains of lignin polymers remain soluble and can therefore be subjected to standard analytical techniques such as size exclusion chromatography or nuclear magnetic resonance spectroscopy. (NMR spectroscopy), which require the analyte to be dissolved in a solvent. Thus, different properties of the soluble fraction of the lignin-based filler can be determined.
[0068] In one embodiment, the starting material for preparing the lignin-based feedstock is lignin derived from an enzymatic hydrolysis process. Enzymatic hydrolysis is a process in which an enzyme(s) helps cleave bonds in molecules with the addition of water elements. In one embodiment, the enzymatic hydrolysis comprises the enzymatic hydrolysis of cellulose.
[0069] In one embodiment, the lignin-based feedstock is prepared from lignin derived from an enzymatic hydrolysis process which is subjected to a hydrothermal carbonization treatment.
[0070] In one embodiment, the lignin-based filler comprises ash in a total amount ranging from 0.1 to 2.8% by weight, or from 0.2 to 2.5% by weight, or from 0.3 to 1.5% by weight, or from 0.4 to 1.0% by weight. The ash content can be determined according to DIN 51719.
[0071] The inventors have surprisingly discovered that when, for example, lignin from the enzymatic hydrolysis process is used to produce the lignin-based feedstock, it is possible to reduce the ash content of the lignin-based feedstock. The lower ash content has the additional advantage of, for example, higher purity of the lignin-based feedstock.
[0072] The lignin-based filler may comprise carbon in a total amount ranging from 59 to 70% by weight. In one embodiment, the lignin-based filler comprises carbon in a total amount ranging from 59 to 70% by weight, or from 62 to 70% by weight, or from 63 to 69% by weight, or from 64 to 68% by weight. The amount of carbon in the lignin-based filler may be determined according to DIN 51732(1997).
[0073] In one embodiment, the solubility of the lignin-based filler in 0.1 M NaOH is between 1 and 45 wt%, or 3 and 35 wt%, or 5 and 30 wt%. The solubility can be measured as follows: first, a sample is dried at a temperature of 60°C for four hours. A sample mass of 0.5 grams is weighed and suspended in 50 ml of 0.1 M NaOH at a concentration of 1% having a temperature of 22°C. Mixing is continued for 1 hour, after which the sample is placed on a glass microfiber paper (1.6 qm) and the filter paper with the sample is dried at a temperature of 60°C for 2 hours. The portion of the sample that has dissolved can be determined gravimetrically.
[0074] In one embodiment, the lignin-based filler has a weight average molecular weight (Mw) ranging from 1000 to 4000 Da, or from 1300 to 3700 Da, or from 1700 to 3200 Da, or 2500 to 3000 Da, or 2600 to 2900 Da, or 2650 Da to 2850 Da, when determined based on the soluble fraction of the lignin-based filler. The weight-average molecular weight can be determined by size exclusion chromatography (SEC) using 0.1 M NaOH as the eluent and a sample amount of approximately 1 mg / ml, which is dissolved in 0.1 M NaOH. Molecular weights are measured relative to polystyrene sulfonate standards. A UV detector at a wavelength of 280 nm is used.
[0075] The polydispersity index (PDI) of the lignin-based filler may be between 1.5 and 5.0, or 1.8 and 4.5, or 1.9 and 4.3, or 2.1 and 4.0, or 2.4 and 3.5, or 2.6 and 3.2, when determined based on the soluble fraction of the lignin-based filler. The polydispersity index may be determined by size exclusion chromatography (SEC). The PDI is a measure of the molecular weight distribution in a given polymer sample. The PDI is calculated as the weight average molecular weight (Mw) divided by the number average molecular weight (Mn). The PDI indicates the distribution of individual molecular weights in a batch of polymers.
[0076] The lignin-based filler may have an STS A value ranging from 3 to 150 m2 / g, or from 5 to 100 m2 / g, or from 7 to 60 m2 / g, or from 20 to 30 m2 / g. The STSA value may be determined according to ASTM D6556.
[0077] In one embodiment, the lignin-based filler has a density of at most 1.5 g / cm3. In one embodiment, the lignin-based filler has a density ranging from 1.0 to 1.5 g / cm3, or from 1.1 to 1.4 g / cm3. The density can be determined according to ISO 21687.
[0078] The lignin-based filler has the additional advantage of imparting a black color to the thermoplastic composition which otherwise resembles the color of the thermoplastic composition prepared using carbon black as the filler.
[0079] In one embodiment, the color of the thermoplastic composition is represented by an L value of at most 36, an a value of at most 10 and a b value of at most 15 as determined by DIN EN ISO 11664.
[0080] In one embodiment, the color of the thermoplastic composition is represented by an L value of at most 36, or at most 35, or at most 30, or at most 25, or at most 20, or at most 15, or at most 10. In one embodiment, the color of the thermoplastic composition is represented by an a value of at most 10, at most 9, or at most 8, or at most 7, or at most 6, or at most 5, or at most 4.8, or at most 4.5, or at most 4.3. In one embodiment, the color of the thermoplastic composition is represented by a b value of at most 15, or at most 13, or at most 12, or at most 10, or at most 8, or at most 7, or at most 6.5, or at most 6.3 or at most 6.1.
[0081] In one embodiment, the color of the thermoplastic composition is represented by an L value of at most 36, or at most 35, or at most 30, or at most 25, or at most 20, or at most 15, or at most 10; and an a value of at most 10, at most 9, or at most 8, or at most 7, or at most 6, or at most 5, or at most 4.8, or at most 4.5, or at most 4.3; and a b value of at most 15, or at most 13, or at most 12, or at most 10, or at most 8, or at most 7, or at most 6.5, or at most 6.3 or at most 6.1.
[0082] In one embodiment, the color of the thermoplastic composition is represented by an L value of at least 2, or at least 4. In one embodiment, the color of the thermoplastic composition is represented by an a value of at least 1, or at least 2. In one embodiment, the color of the thermoplastic composition is represented by a b value of at least 4, or at least 6, or at least 8, or at least 10.
[0083] In one embodiment, the color of the thermoplastic composition is represented by an L value of at least 2, or at least 4; and the color of the thermoplastic composition is represented by an a value of at least 1, or at least 2; and the color of the thermoplastic composition is represented by a b value of at least 4, or at least 6, or at least 8, or at least 10.
[0084] The values L, a and b indicate values for the color of the thermoplastic composition. These values can be determined by DIN EN ISO 11664 and can be measured by any device that allows the measurement of the CIELab color space. The inventors of the current application surprisingly discovered that the use of the lignin-based filler made it possible to obtain a dark black thermoplastic composition.
[0085] In one embodiment, the thermoplastic composition has an opacity of at least 90%, or at least 95%, or at least 98%. The opacity shows how transparent or translucent the thermoplastic composition is. The opacity can be measured by the BYK Spectro-guide 45 / 0 apparatus. The reference value is 100%.
[0086] The use of the lignin-based filler has the additional advantage of making the thermoplastic composition sortable by NIR techniques and therefore recyclable because it does not mask the NIR reflectance of the polymer in the thermoplastic composition and thus allows the thermoplastic composition to be sorted from a mixture of articles and thus makes it possible to recycle the thermoplastic composition. Furthermore, the thermoplastic composition as disclosed in the present description has the additional advantage of having a black color rather similar to that provided by carbon black. EXAMPLES
[0087] Reference will now be made in detail to various embodiments.
[0088] The description below discloses certain embodiments in sufficient detail that a person skilled in the art will be able to use the embodiments based on the disclosure. Not all steps or features of the embodiments are discussed in detail, as many steps or features will be obvious to those skilled in the art based on this description.
[0089] Example 1 - Preparation of thermoplastic compositions and testing thereof
[0090] In this example, the aim was to evaluate whether the sorting of the prepared thermoplastic compositions into different fractions can be achieved using a near-infrared detection system.
[0091] The effect of different lignin-based fillers in different amounts in thermoplastic compositions was tested. In addition, comparative examples were prepared using carbon black (CB) in thermoplastic compositions instead of the lignin-based filler.
[0092] Two different types of lignin-based fillers were tested. The lignin-based filler, which is designated LBF in this example, was prepared following the description provided above in this specification using lignin material derived from an enzymatic wood hydrolysis process and subjected to a hydrothermal carbonization treatment. Other thermoplastic compositions were prepared using virgin lignin (PL) as the lignin-based filler. The virgin lignin was derived from the same enzymatic wood hydrolysis process as the LBF lignin, but it was not subjected to the hydrothermal carbonization treatment. The carbon black (CB) used in the comparative examples was MONARCH®800 supplied by Cabot. The properties of the lignin-based filler and virgin lignin were measured and are shown in the table below:
[0093] [Tables 1] Measured value Measurement method Unit LBF PL STSA ASTM D6556 m2 / g 49.3 9.3 Density ISO 21687 g / cm3 1.3-1.4 1.3-1.4 C content DIN51732 % 65.93 60.3 H content DIN51732 % 5.57 5.90 N content DIN51732 % 0.11 0.76 S content DIN51732 % 0.03 <0.05 Ash content DIN51719 % 2.3 0.4 Solubility in 0.1 M NaOH As described in this specification % 26.2 40.8 PH ASTMD1512 - 8.4 6-7 Moisture content ASTM DI509 % 0.7 2.4
[0094] Properties of lignin-based fillers called LBF and PL
[0095] The carbon content of the carbon black was > 95% and the density was 1.8 g / cm3.
[0096] First, the following masterbatches were prepared:
[0097] [Tables2] Filler Type Polypropylene Polystyrene Polyethylene Polyamide Ethylene-vinyl acetate 40% by weight of carbon black XXXXX 40% by weight of virgin lignin XXXXX 40% by weight of lignin-based filler XXXXX
[0098] Prepared masterbatches
[0099] The masterbatches therefore contained: 40% by weight of filler, 52% by weight of the polymer and in total 8% by weight of a set of additives (consisting of 2% of Ca stearate (lubricant), 2% of the antioxidant Irganox 1010, 4% of polyethylene wax (lubricant)).
[0100] 3 kg of each type of masterbatch was prepared, and this was done at a loading of 40% by weight of filler. The masterbatches produced were then physically dry blended to 3% by weight. The following compositions were prepared:
[0101] - Polypropylene (PP) as a masterbatch in polypropylene (PP) (PP thermoplastic composition)
[0102] - Polystyrene (PS) as a masterbatch in acrylonitrile butadiene styrene (ABS) (ABS thermoplastic composition)
[0103] - Polyethylene (PE) as a masterbatch in high-density polyethylene density (HDPE) (thermoplastic composition HDPE)
[0104] - Polyamide (PA) as a masterbatch in polyamide (PA 12) (thermoplastic composition PA 12)
[0105] - Ethylene vinyl acetate (EVA) as a masterbatch for poly- vinyl chloride PVC (thermoplastic PVC composition)
[0106] The prepared thermoplastic compositions each contained the amount of the different fillers shown in Tables 3 to 9.
[0107] Different thermoplastic compositions were prepared using different polymers and fillers and varying the amount of filler. Some of the samples were prepared as flat plates and others as granules.
[0108] The granules were prepared as follows:
[0109] Sample compounding was carried out on Leistritz ZSE27 with a submerged granulator. The extruder that was used for sample compounding was Leistritz ZSE 27 MAXX. It is a high-speed co-rotating twin-screw extruder with a screw diameter of 27 mm and an L / D ratio of 48. It contains an atmospheric and vacuum degassing port, a side feeder for fillers and can be equipped with a melt pump and gas injection units for foaming. The plant was equipped with a Gala PLU submerged granulation system for granulating the extruded materials into pellets.
[0110] The flat plates were prepared as follows:
[0111] The granular samples prepared above were injection molded on ARBURG 420 M allrounder 1000-350. The machine was equipped with a quick-change mold for ISO-certified test specimens. Plates were prepared in this way for other thermoplastic compositions than for that prepared with PVC.
[0112] For the thermoplastic composition prepared with PVC, the pellet samples prepared above were extruded on a Weber CE5.2 conical twin-screw extruder with a vent port. At its maximum RPM of 30, the extruder had a throughput of approximately 80 kg / h. The sample strips were made with a 70 mm x 5 mm die and then machined into T-bars with a tabletop CNC milling machine.
[0113] The prepared samples were analyzed by subjecting the samples to measurements carried out with a portable near-infrared (NIR) spectroscopy device from trinamiX GmbH (Ludwigshafen, Germany), i.e., a trinamiX NIR Spectrometer (software package: general plastic).
[0114] The various samples prepared and their properties and measurement results are presented in the tables below and in Figures 1 to 7. The “evaluation” in the tables indicates the results given by the measuring equipment. “ND” means “not detectable”.
[0115] [T ableaux3 ] Polymer PP PP PP PP PP PP PP PP Amount of CB - 1.2% - - - - 0.2% Amount of PL - - 1.2% - - - - Amount of LBF - - - 1.2% 2.0% 4.0% 1.0% Maximum Reflection Intensity 19.3% 1.4% 19.2% 20.4% 21.8% 23.2% 1.8% Minimum Reflection Intensity 0.7% 0.8% 0.7% 0.8% 0.8% 0.8% 0.8% Specimen Contrast NIR 26.6 0.8 26.4 24.5 26.3 28.0 1.3 L 67.74 7.5 21.15 12.93 9.77 8.28 8.01 a -1.12 0.42 9.63 4.67 4.43 4 0.41 b -1.05 1.37 13.49 6.58 5.72 4.94 1.42 Opacity 54% 101% 91% 101% 102% 104% 101% Rating - Material PP ND PP PP PP PP ND
[0116] Thermoplastic composition samples prepared with polypropylene (PP) as the polymer and the sample type being a plate.
[0117] The results are presented in Figures 1a and 1b.
[0118] [Tables4] Polymer PP PP PP PP Amount of CB - 40.0% - - Amount of PL - - 40.0% - Amount of LBF - - - 40.0% Maximum Reflection Intensity 20.2% 3.3% 33.1% 43.5% Minimum Reflection Intensity 1.8% 1.9% 3.4% 7.2% Specimen Contrast NIR 10.2 0.7 8.7 5.0 Evaluation - Material PP ND PP PP
[0119] Thermoplastic composition samples prepared with polypropylene (PP) as polymer and the sample type being a granule
[0120] The results are shown in [Fig.2].
[0121] [Tables5] Polymer HDPE HDPE HDPE HDPE CB - 1.2% - - PL - - 1.2% - LBF - - - 1.2% Maximum Reflection Intensity 35.6% 1.2% 31.6% 31.3% Minimum Reflection Intensity 0.6% 0.4% 0.6% 0.5% Specimen Contrast NIR 58.3 2.0 51.7 61.6 L 75.42 7.86 17.9 10.24 a -1.17 -0.59 9.72 3.95 b -2.2 -1.35 11.52 4.94 Opacity 52% 100% 85% 100% Evaluation - Material HDPE ND HDPE HDPE
[0122] Thermoplastic composition samples prepared with polyethylene (high density polyethylene HDPE) as polymer and the sample type being a plate
[0123] The results are shown in Figures 3a and 3b.
[0124] [Tableauxô] Polymer HDPE HDPE HDPE HDPE CB - 40.0% - - PL - - 40.0% - LBF - - - 40.0% Maximum Reflection Intensity 24.3% 2.8% 30.6% 19.1% Minimum Reflection Intensity 1.6% 1.5% 3.3% 2.1% Specimen Contrast NIR 14.2 0.9 8.3 8.1 Evaluation - Material HDPE ND HDPE HDPE
[0125] Thermoplastic composition samples prepared with polyethylene (high density polyethylene HDPE) as polymer and the sample type being a granule
[0126] The results are shown in [Fig.4].
[0127] [Tables?] Polymer PA12 PA12 CB 2.0% - PL - - LBF - 2.0% Maximum reflection intensity 1.4% 27.0% Minimum reflection intensity 0.7% 1.0% Specimen contrast NIR 1.0 26.0 L 3.69 8.32 a -0.24 3.02 b -1.33 3.53 Opacity 104% 104% Evaluation - Material ND PA
[0128] Thermoplastic composition samples prepared with polyamide (PA) as polymer and the sample type being a plate
[0129] The results are shown in [Fig.5].
[0130] [Tables8] Polymer ABS ABS ABS ABS CB - 1.2% - - PL - - 1.2% - LBF - - - 1.2% Maximum Reflection Intensity 21.5% 1.4% 20.6% 20.8% Minimum Reflection Intensity 0.8% 0.6% 0.9% 0.9% Specimen Contrast NIR 25.9 1.3 21.9 22.1 L 82.78 11.46 35.78 23.09 a -2.82 -0.52 5.74 4.63 b 3.2 -0.68 7.18 5.84 Opacity 75% 100% 100% 100% Evaluation - Material ABS ND ABS ABS
[0131] Thermoplastic composition samples prepared with an acrylonitrile-butadiene-styrene (ABS) copolymer as the polymer and the sample type being a plate
[0132] The results are shown in Figures 6a and 6b.
[0133] [Tables9] Polymer PVC PVC PVC PVC CB - 1.2% - - PL - - 1.2% - LBF - - - 1.2% Maximum Reflection Intensity 15.8% 1.4% 14.1% 15.1% Minimum Reflection Intensity 1.0% 0.7% 0.9% 0.8% Specimen Contrast NIR 14.8 1.0 14.7 17.9 L 66.53 11.57 23.04 16.51 a 1.44 -0.27 7.35 2.27 b 16.83 -0.66 9.63 2.36 Opacity 98% 100% 98% 100% Evaluation - Material PVC ND PVC PVC
[0134] Thermoplastic composition samples prepared with polyvinyl chloride (PVC) as the polymer and the sample type being a plate
[0135] The results are shown in [Fig.7].
[0136] From the above results and Figures 1 to 7, it can be seen that in all cases where the thermoplastic composition was prepared with a lignin-based filler (LBF or PL) to form a black-colored thermoplastic composition, the near-infrared reflectance of the thermoplastic composition is not masked by the filler as is the case when using carbon black. Therefore, the polymer type can be checked and detection and sorting of the thermoplastic composition is possible unlike the situation when using carbon black as the filler. From the above results, it can be seen that when using carbon black, the polymer is masked and cannot be detected (not detected (ND)).
[0137] It will be apparent to those skilled in the art that with advances in technology, the basic idea can be implemented in various ways. The embodiments are therefore not limited to the examples described above; rather, they may vary within the scope of the claims.
[0138] The embodiments described above may be used in any combination with each other. Several of the embodiments may be combined together to form another embodiment. A thermoplastic composition, method, or use disclosed herein may include at least one of the embodiments described above. It will be understood that the benefits and advantages described above may relate to one embodiment or may relate to several embodiments. Embodiments are not limited to those that solve any or all of the stated problems or those that exhibit any or all of the stated benefits and advantages.The term "comprising" is used in this description to mean the inclusion of the following feature(s) or act(s), without excluding the presence of one or more additional features or acts.
Claims
Claims
1. Use of a lignin-based filler in a thermoplastic composition comprising at least one polymer and the lignin-based filler to be able to detect the thermoplastic composition by a near-infrared detection system so that the thermoplastic composition can be sorted from a mixture of articles, wherein - the thermoplastic composition contains 0.3 to 65% by weight of the lignin-based filler relative to the total weight of the thermoplastic composition, - the color of the thermoplastic composition is represented by an L value of at most 36, an a value of at most 10 and a b value of at most 15 as determined by DIN EN ISO 11664;- the thermoplastic composition has a maximum reflection intensity value, in the near infrared wavelength range of 1450 to 2450 nm of the electromagnetic spectrum, that is greater than or equal to a reflection intensity of 5% when determined by a near infrared detection system; and - the thermoplastic composition has a near infrared specimen contrast that is greater than or equal to 3.0 in the wavelength range of 1450 to 2450 nm.;
2. The use of claim 1, wherein the lignin-based filler comprises or consists of lignin.
3. The use of claim 1, wherein the lignin-based filler is prepared from lignin subjected to a hydrothermal carbonization treatment.
4. Use of any one of the preceding claims, wherein the thermoplastic composition is a recyclable and sortable thermoplastic composition.
5. Use of any one of the preceding claims, wherein the thermoplastic composition has a maximum reflection intensity value, in the near infrared wavelength range of 1450 to 2450 nm of the electromagnetic spectrum, which is greater than or equal to a reflection intensity of 8%, or 10%, or 15%, or 20%, or 25% when determined by a near infrared detection system.
6. Use of any one of the preceding claims, in wherein the thermoplastic composition exhibits a near infrared specimen contrast that is greater than or equal to 5.0, or 6.0, or 9.0, in the wavelength range of 1450 to 2450 nm.
7. Use of any one of the preceding claims, wherein the thermoplastic composition contains 0.3 to 60% by weight, or 0.5 to 50% by weight, or 1 to 40% by weight, or 1.2 to 30% by weight, or 1.5 to 20% by weight, or 2 to 10% by weight, or 2.5 to 5% by weight of the lignin-based filler relative to the total weight of the thermoplastic composition.
8. Use of any one of the preceding claims, wherein the polymer is polyethylene, polypropylene, polystyrene, ethylene vinyl acetate, polybutylene adipate terephthalate, polyamide, polyacrylate, polyester, acrylonitrile butadiene styrene, polycarbonate, polylactic acid or polyvinyl chloride, or any combination or mixture thereof.
9.