A component with a porous structure and its manufacturing process
Additive manufacturing techniques enable the creation of lightweight shock absorber devices with high porosity and efficient energy dissipation by forming cellular pores smaller than 14 mm, addressing the weight and energy efficiency challenges in automotive applications.
Patent Information
- Application Number
- FR2021013176
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-12-08
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-12-08
AI Technical Summary
Existing methods for manufacturing shock absorber devices with cellular structures struggle to produce pores smaller than 14 mm, which hinders the ability to reduce the weight and energy consumption of such devices, particularly in the automotive field.
A porous structure is created using additive manufacturing techniques, specifically laser powder bed fusion, to form cellular pores with an average size less than 14 mm, achieving a high wall porosity of 5-80% and cellular porosity greater than 70%, with open pores and a metallic or polymer material, allowing for lighter and more efficient energy dissipation.
The solution results in a significantly lighter shock absorber device with enhanced energy dissipation capabilities, achieving a total porosity of up to 97% and faster production times compared to traditional methods.
Smart Images

Figure 00000014_0000 
Figure 00000015_0000 
Figure 00000015_0001
Abstract
Description
Title of the invention: Part comprising a porous structure and its manufacturing method Technical field
[0001] The present invention relates to the field of porous structures comprising cellular pores, in particular intended to form all or part of a shock-absorbing device. Prior art
[0002] In order to absorb the energy of an impact, a shock-absorbing device may be in the form of a metallic or polymeric cellular structure. Such a cellular structure has a high porosity which gives it both lightness and good mechanical performance, in particular an ability to dissipate energy by sufficient plastic deformation in compression to absorb the energy of an impact.
[0003] A shock-absorbing device can be manufactured by foundry, in particular by molding. However, foundry is energy-intensive and makes it difficult, if not impossible, to obtain cellular pores with a size of less than 14 mm. It is also known to manufacture such a device by additive manufacturing, which simply allows the obtaining of specific and complex shapes as well as small cellular pores.
[0004] FR 3 033 518 A1 describes, for example, a metal or alloy part comprising cells, which can be produced by casting or by additive manufacturing.
[0005] There is a need, particularly in the automotive field, to lighten such a shock absorbing device, particularly in a constant search to reduce the energy consumption of a vehicle. Statement of the invention
[0006] The invention relates to a part comprising a porous structure comprising cellular pores and formed at least in part by the periodic repetition of an elementary pattern, each cellular pore being delimited by a wall, made of a metallic or polymer material, having a parietal porosity greater than 5% and comprising parietal pores whose average size is less than the average size of the cellular pores.
[0007] Compared to a part having an identical cellular pore structure in which the cellular pores are each delimited by a dense wall, the part according to the invention is advantageously lighter.
[0008] The “wall porosity” is equal to the ratio of the volume occupied by the pores parietal pores on the volume occupied by the walls of the porous structure. The volume occupied by the walls of the porous structure is equal to the sum of the volume of the material forming the parietal pores and the volume occupied by the parietal pores. The "parietal pores" are the pores contained in the walls.
[0009] “Cellular porosity” corresponds to the ratio of the volume occupied by the cell pores to the volume occupied by the porous structure. The volume occupied by the porous structure is equal to the sum of the volume occupied by the walls and the volume occupied by the cell pores.
[0010] The total porosity of the porous structure corresponds to the sum of the cellular porosity and the parietal porosity.
[0011] An “open” pore is delimited by a hollow wall. An open pore is thus in fluid communication with another open pore adjacent to it.
[0012] The "average" size of a pore population is the arithmetic mean of the sizes of the pore population.
[0013] The "size" of a pore, whether cellular or parietal, can be determined by the following method. The part can first be infiltrated with a resin. A slice of the part to be analyzed is cut and then polished in order to obtain a good surface condition, said polishing being carried out with a polishing paper with small grains at least grade 1200, preferably with a diamond paste. Images of the polished slice are taken using an optical microscope or an electron microscope. The magnification used is such that the width of the image is between 5 and 10 times the average pore size. A first image can be taken using a visual estimation of the average pore size.The size of the pores is determined by analyzing the images using a thresholding method followed by erosion / dilation used, for example, by image analysis software such as the ZEN CORE 2© software marketed by the company Zeiss©. The “size” of a pore corresponds, on the image, to the diameter of the smallest circle circumscribing said pore.
[0014] The average size of the parietal pores can be acquired on an image representing a transverse section of one or more walls. The average size of the cellular pores can be acquired on an image representing a transverse section of the cellular structure. Obviously, to measure the average size of the cellular pores, an image is acquired at lower magnification than to measure the average size of the parietal pores.
[0015] The method described also makes it possible to access by summation the cellular porosity and / or the parietal porosity. The cellular porosity corresponds, on the image, to the ratio of the sum of the areas occupied by the cellular pores to the area of the section of the porous structure represented on the image. The parietal porosity corresponds, on the image, to the ratio of the sum of the areas occupied by the parietal pores to the area total occupied by the walls.
[0016] The parietal porosity can be between 5% and 80%, in particular between 20% and 60%.
[0017] The average size of the parietal pores may be less than 500 pm, with preferably at least 85% of the parietal pores having a size less than 200 pm and preferably more than 50% of the parietal pores having a size less than 50 pm.
[0018] The parietal pores may be distributed irregularly, and in particular randomly, within the walls. They may be distributed in the walls homogeneously. For example, the parietal porosity does not vary by more than 20%, or even 10%, or even 5%, between two distinct zones of volume equal to 3 times the cube of the thickness of one of the walls.
[0019] The parietal pores may have an irregular shape, in particular non-spherical.
[0020] The walls may be solid, that is to say they are free from at least one parietal pore which passes through its thickness.
[0021] Alternatively, the walls are hollow. A hollow wall has at least one recess passing right through its thickness.
[0022] The walls may have a lattice shape. They may in particular be in the form of a polyhedral assembly of bars which delimit one of the recesses.
[0023] The porous structure may comprise solid walls and hollow walls.
[0024] Portions of at least one of the walls may delimit several adjacent cellular pores. The walls may comprise several flat or curved faces.
[0025] The thickness of at least one of the walls, or even of each wall, may be at least 200 μm, preferably at least 800 μm or even at least 1 mm. The thickness of a wall is the smallest distance between two opposite faces of the wall.
[0026] The porous structure may comprise open cellular pores. More than 90%, preferably more than 95%, in number of the cellular pores may be open, or even all of the cellular pores may be open.
[0027] The average size of the cellular pores may be greater than 100 μm, preferably greater than 500 μm, or even greater than 1 mm. It may be less than 14 mm, or even less than 10 mm.
[0028] The average size of the cellular pores may be at least 20 times larger, preferably at least 50 times larger, or even at least 100 times larger than the average size of the parietal pores.
[0029] The cellular porosity may be greater than 70%, preferably greater than 80%, or even greater than 90%, better still greater than 95%. It may be less than 97%, for example equal to 96%.
[0030] The porous structure is formed at least in part, or even in whole, by the periodic repetition of an elementary pattern.
[0031] The elementary pattern may be repeated periodically along one axis, or even two axes or preferably three axes different from each other, and preferably orthogonal to each other. The elementary pattern may be repeated more than five times, or even more than ten times, or even more than fifty times along each axis, in particular depending on the application for which the part is intended.
[0032] The elementary pattern may comprise, or even consist of, a cell pore and, at least in part, the wall which delimits said cell pore. The elementary pattern may comprise one or more cell pores. Alternatively, a cell pore may be defined by the repetition, at least twice, of the elementary pattern.
[0033] The elementary pattern may have a convex or concave or star shape. In particular, the elementary pattern may be a lattice, in particular convex and / or star-shaped. The elementary pattern may be any shape accessible by additive manufacturing, the repetition of which makes it possible to form cellular pores.
[0034] Preferably, the porous structure is made of a metallic material.
[0035] The porous structure may comprise, in particular for more than 95% of its mass, in particular for more than 99.0% of its mass, or even for more than 99.9% of its mass, a metal chosen from aluminum, nickel, cobalt, iron, copper, palladium, titanium, tungsten, silver, platinum and their alloys. In particular, the porous structure may be made of a stainless steel or a shape memory alloy, in particular an alloy of nickel and titanium, for example nitinol. Preferably, the porous structure is made of a stainless steel.
[0036] Alternatively, the porous structure may comprise, in particular for more than 80% of its mass, or even for more than 90% of its mass, a polymer chosen from polyamides, polystyrenes, thermoplastic elastomers, polyaryletherketones and their mixtures, preferably from polyamides, in particular a nylon such as nylon PA12, nylon PA11 or nylon PEBA. It may comprise glass fibers, glass beads, aluminum powder and their mixtures.
[0037] The invention also relates to a shock-absorbing device formed, at least in part, from a part according to the invention, for example for the protection of objects, in particular against their falling or their transport.
[0038] The invention also relates to a device comprising a part according to the invention, the device being chosen from a vehicle, in particular a motor vehicle or railway vehicle, a porous tank, a wedge and an acoustic absorber.
[0039] The invention also relates to a method for manufacturing a part according to the invention, the method comprising the production of the porous structure by shaping a powder using an additive manufacturing technique.
[0040] Preferably, the additive manufacturing technique is a powder bed additive manufacturing technique.
[0041] Preferably, the additive manufacturing technique implements a partial or complete melting of the particles of the powder by means of a light beam or electrons, in particular a light beam. Preferably, the light beam is a laser beam.
[0042] Many powder bed additive manufacturing techniques known to those skilled in the art can be used. In particular, the additive manufacturing technique can be chosen from 3D printing techniques, notably chosen from: - printing by projection of binder onto a powder bed, known under the English name of “Binder Jetting”, - laser powder bed fusion called “LPBF” or “SLM”, English acronym for “Laser Powder Bed Fusion” and “Selective Laser Melting” respectively, - selective laser sintering called “SLS”, an English acronym for “Selective Laser Sintering”, - electron beam fusion known as “EBM”, an acronym for “Electron Beam Melting”, and - the projection of binder on powder bed “MJF”, English acronym for “Multi Jet Fusion”.
[0043] Preferably, the additive manufacturing technique is laser powder bed fusion (LPBF) or selective laser sintering (SLS), more preferably laser powder bed fusion (LPBF). Laser powder bed fusion (LPBF) is preferably implemented to form a metallic porous structure. Selective laser sintering (SLS) is preferably implemented to form a polymeric porous structure.
[0044] The technique of additive manufacturing by laser fusion on a powder bed comprises the deposition of at least one layer of powder then the partial or complete fusion of at least a part of the particles of the powder, preferably of all the particles of the layer deposited by a selective supply of energy under the action of a laser beam.
[0045] The median particle diameter of the D50 powder may be between 1 pm and 100 pm, preferably between 1 pm and 80 pm, for example between 5 pm and 45 pm. The size of the parietal pores can thus be easily controlled.
[0046] The particles may comprise, in particular for more than 95.0% of their mass, in particular for more than 99.0% of their mass, or even for more than 99.9% of their mass, a metal chosen from aluminum, nickel, cobalt, iron, copper, palladium, titanium, tungsten, silver, platinum and their alloys, in particular a stainless steel or a shape memory alloy.
[0047] The particles may comprise, in particular for more than 80% of its mass, or even for more than 90% of its mass, a polymer chosen from polyamides, poly styrenes, thermoplastic elastomers and polyaryletherketones and mixtures thereof, preferably among polyamides, in particular a nylon such as nylon PA 12, nylon PA11 or nylon PEBA.
[0048] The powder may be monodisperse.
[0049] The additive manufacturing technique may comprise the repetition, in particular more than ten times, or even more than a thousand times, of a cycle comprising the deposition of a layer of powder with a thickness of between 6 μm and 200 μm, preferably between 10 μm and 120 μm and the irradiation of at least part of the layer by the light beam, preferably a laser beam. As a variant, the cycle comprises for example the deposition of a layer of powder with a thickness of between 1 μm and 80 μm.
[0050] The additive manufacturing step may comprise the deposition of an initial layer of powder on a manufacturing plate, in particular heated to a temperature between 20°C and 250°C, in particular between 190°C and 210°C.
[0051] The melting of the powder particles can be controlled using a pre-established computer database. The computer database controls at each stage, by means of the execution of a computer program by a processor, a spatial displacement of the light beam relative to the deposited powder. The computer database can control: - the geometry of the porous structure, and in particular of the walls delimiting the cellular pores, by controlling the trajectory of the light beam; and - the porosity of the walls, by selecting suitable parameters for driving the additive manufacturing technique, and in particular by controlling the energy density of the light beam.
[0052] The selective melting of the powder is controlled by the selection of main additive manufacturing technique control parameters, notably chosen from the speed of movement of the light beam (V), the power of the light beam (P), the offset value between the movement vectors of the light beam (HD), the gap between two laser cords (HD) and the rotation of the cords from one layer to another.
[0053] Preferably, at least one of the additive manufacturing control parameters is chosen so as to partially coalesce the particles to bind them together. Partial coalescence makes it possible to retain part of the porosity of the powder and to form porous walls. The implementation of the additive manufacturing technique is thus different from the practice of the prior art according to which the most complete possible fusion of the particles is generally sought to form a dense metal wall.
[0054] The wall porosity can be adjusted by adapting the light beam energy density. Below a threshold energy density, the wall porosity increases with a decrease in energy density. The "threshold energy density" is the energy density above which a porous structure with dense walls is obtained. A "dense wall porous" structure has a wall porosity of less than 0.5%.
[0055] The volume energy density E, expressed in J / mm3, is defined by the following mathematical formula:
[0056] [Math.l] J7 — P L ~ V.HD.e
[0057] in which: -P is the power of the light beam, in particular the laser beam, expressed in W, - V is the speed of movement of the light beam, in particular laser, expressed in mm / s, - HD is the offset value between the displacement vectors of the light beam, in particular between two laser cords, expressed in mm, and - e is the layer thickness, expressed in mm.
[0058] Preferably, the ratio of the energy density of the light beam to the threshold energy density is between 0.3 and 0.9.
[0059] The beam displacement speed is the relative speed of the point formed by the light beam on the powder layer, relative to said layer. For a constant power P of the light beam, a constant offset value HD and a constant layer thickness e, above a threshold displacement speed, the wall porosity of the porous cellular structure increases, with an increase in the displacement speed. The “threshold displacement speed” is the displacement speed below which a porous structure with dense walls is obtained, for a constant power P of the light beam, a constant offset value HD and a constant layer thickness e. The displacement speed of the light beam may be less than 6000 mm / s.Since a high displacement speed can be implemented, the manufacturing of the part according to the invention is also faster than that of dense-walled cellular metal parts obtained by an additive manufacturing process of the prior art.
[0060] For example, for a light beam power of 275 W, a layer thickness of 50 pm, an offset value between the light beam displacement vectors of between 80 and 120 pm and a stainless steel powder having a median diameter of 36 pm, the displacement speed of the light beam is between 1500 and 6000 mm / s.
[0061] The trajectory adopted by the light beam follows displacement vectors spatially shifted two by two according to an HD shift value.
[0062] A person skilled in the art knows how to adjust the wall porosity within the porous structure, for a predetermined light beam power, light beam displacement speed and layer thickness, by adapting said offset value. For example, under these conditions, the wall porosity increases with an increase in the offset value.
[0063] The thickness of the deposited powder layer also makes it possible to adjust the wall porosity. For a predetermined light beam power, offset value and movement speed, the wall porosity increases with an increase in the thickness of the layer.
[0064] In one embodiment, prior to the production of the porous structure, the method may comprise: i) manufacturing at least one test structure with different respective light beam powers, in order to determine the threshold energy density Eseuu, the displacement speed Vo of the light beam, the offset value HD0 of the light beam and the layer thickness e0 having been predetermined and kept constant during the manufacturing of said at least one test structure, ii) selecting at least one parameter chosen from the light beam travel speed, the light beam offset value and the layer thickness so that the energy density of the light beam during the subsequent manufacturing step is less than EseuU.
[0065] The parameters described above can be adjusted according to the composition of the powder used. Brief description of the drawings
[0066] The invention may be better understood by reading the detailed description which follows of the example and the attached drawing in which:
[0067] [Fig-1] [Fig.l] includes a photograph of an example of a part according to the invention, as well as a photograph by optical microscopy of a wall of the part,
[0068] [Fig.2] [Fig.2] schematically represents different examples of elementary pattern to form by repetition a porous structure according to the invention and
[0069] [Fig.3] [Fig.3] schematically illustrates an example of implementation of an additive manufacturing process on a powder bed using a laser beam (A), in a configuration without (B) and with (C) overlap. Detailed description
[0070] An example of part 10 according to the invention is shown in [Fig.l].
[0071] The part is cubic in shape with dimensions of 50x50x50 mm3. It has a porous structure 15 comprising open cellular pores 20 and me- metals 30 which each delimit one or more cellular pores and form a partition between adjacent cellular pores.
[0072] The cellular pores 20 have a substantially spherical shape with a diameter of 5.6x5.6 mm2. They are arranged periodically along three orthogonal axes.
[0073] The walls 30 are hollow, i.e. they comprise recesses which pass right through them in their thickness so as to fluidly connect adjacent cellular pores.
[0074] As illustrated in the photograph which represents an enlargement of a wall 30, a wall 30 comprises parietal pores 31 which are delimited by dense metallic zones 32.
[0075] Thus, the part has a cellular porosity which is formed by the cellular pores and a parietal porosity which is formed by the parietal pores.
[0076] In [Fig. 2], different examples of elementary patterns 50 have been illustrated, which by periodic repetition result in the formation of a porous structure. Of course, other elementary patterns than those shown can result in the formation of a porous structure.
[0077] The elementary patterns have for example a lattice shape, which can be cubic, octahedral, dodecahedral, octagonal gyrobicupola, cu-boctahedron, truncated octahedron, large icosahedron and icosahedron.
[0078] A cellular pore may be delimited by an elementary pattern, for example cubic 51 or octahedral 52. Such a cellular pore 20 is then delimited by a wall 30 comprising several faces, each face being provided with a through recess 53. The wall of such a cellular pore then has the shape of a polyhedral lattice.
[0079] Alternatively, a cellular pore may be delimited by the repetition of the elementary motif in at least one direction, as is the case, for example, with the elementary star motif illustrated in [Fig.2].
[0080] Figure 3A illustrates the trajectory of a laser beam 100 during the manufacture of a porous structure by laser additive manufacturing on a powder bed. The spot of the laser beam is moved according to displacement vectors spaced apart by an offset value HD, on a layer of powder 110 to be melted of thickness e which has been deposited on layers previously deposited and bonded together 120 under the effect of the laser beam. As illustrated in Figures 3B and 3C, the areas impacted by the laser beam, and therefore partially melted, extend over the entire thickness of the layer to be melted as well as over a portion of the lower layer on which the layer to be melted rests. The areas impacted by the laser beam during its movement may be non-overlapped (Figure 3B) or partially overlapped (Figure 3C). Thus, an offset value HD can avoid a partial overlap of the impacted areas and facilitate the formation of parietal porosity. Furthermore, a high speed of movement of the laser spot induces a lower local heating of the area impacted by the laser beam, which facilitates the formation of parietal porosity. Examples Example 1
[0081] The part illustrated in [Fig.l] was manufactured in the following manner.
[0082] A 316L stainless steel particle powder, having a median diameter D50 of 36 pm, was used in an LPBF type additive manufacturing machine marketed by SLM Solutions. The machine is equipped with a laser source emitting at a wavelength of 1040 nm.
[0083] The part was manufactured with the additive manufacturing machine on a 316L stainless steel manufacturing plate heated to a temperature of 200°C with the following parameters: - layer thickness: 30 pm, - laser power: 225 W, - laser beam movement speed: 4771 mm / s, - offset value: 100 pm, - laser beam energy density: 15.71 J / mm3.
[0084] The implementation of these specific driving parameters made it possible to obtain a porous structure having a specific parietal porosity. Example 2
[0085] A 316L stainless steel powder, having a median diameter D50 of 36 pm, was used in an LPBF machine marketed by SLM Solutions. The machine is equipped with a laser source emitting at a wavelength of 1040 nm.
[0086] The part was manufactured with the additive manufacturing machine on a 316L stainless steel manufacturing plate heated to a temperature of 200°C with the following parameters: - layer thickness: 50 pm, - laser power: 275 W, - laser beam movement speed: 3501 mm / s, - offset value: 120 pm.
[0087] The energy density of the laser beam is lower than the threshold energy density. The porous structure has a cellular porosity of 85% and its metal walls have a parietal porosity of 35.7%, measured by optical microscopy and image processing. Thus, the total porosity of the part is 94.6%.
[0088] The invention is obviously not limited to the examples of production of the part and to the examples of implementation of the method, described for illustrative purposes and not limiting.
[0089] For example, the part according to the invention is a heat exchanger, a filtration body or a structural part. Such a part could thus be implemented in the field of health, the mining industry, or construction.
Claims
Claims
1. Part (10) comprising a porous structure (15) comprising cellular pores (20) and formed at least in part by the periodic repetition of an elementary pattern (50), each cellular pore being delimited by a wall (30), made of a metallic or polymer material, having a parietal porosity greater than 5% and comprising parietal pores (31) whose average size is less than the average size of the cellular pores.
2. Part according to claim 1, the average size of the cellular pores being at least 20 times larger, preferably at least 50 times larger, or even at least 100 times larger than the average size of the parietal pores.
3. Part according to any one of claims 1 and 2, the average size of the parietal pores being less than 500 pm, with preferably at least 85% of the parietal pores having a size less than 200 pm and preferably more than 50% of the parietal pores having a size less than 50 pm.
4. Part according to any one of the preceding claims, the porous structure being made of a metallic material.
5. Part according to any one of the preceding claims, the porous structure comprising, in particular for more than 95% of its mass, a metal chosen from aluminum, nickel, cobalt, iron, copper, palladium, titanium, tungsten, silver, platinum and their alloys, the porous structure being in particular made of a stainless steel or a shape memory alloy, in particular an alloy of nickel and titanium, for example nitinol.
6. Part according to any one of the preceding claims, the parietal porosity being between 5% and 80%, in particular between 20% and 60%.
7. Part according to any one of the preceding claims, the cellular porosity being greater than 70%, preferably greater than 80%, or even greater than 90%, better still greater than 95% and / or less than 97%.
8. A method of manufacturing a part according to any one of the preceding claims, the method comprising producing the porous structure by shaping a powder using an additive manufacturing technique.
9. Method according to the preceding claim, the additive manufacturing technique being a powder bed additive manufacturing technique.
10. Method according to the preceding claim, the additive manufacturing technique implementing a partial or complete melting of the particles of the powder by means of a light beam or an electron beam, in particular a light beam, preferably a laser beam.
11. A method according to claim 10, the ratio of the energy density of the light beam to the threshold energy density being between 0.3 and 0.9, the threshold energy density being the energy density above which a porous structure with dense walls is obtained.
12. A method according to any one of claims 8 to 11, the median particle diameter of the powder being between 1 pm and 100 pm, preferably between 1 pm and 80 pm.
13. Method according to any one of claims 10 to 12, the additive manufacturing technique comprising the repetition, in particular more than ten times, or even more than a thousand times, of a cycle comprising the deposition of a layer of the powder with a thickness (e) of between 6 pm and 200 pm, preferably of between 10 pm and 120 pm, and the irradiation of at least part of the layer by the light beam, preferably a laser beam.
14. Method according to any one of claims 10 to 13, comprising prior to the production of the porous structure: i) manufacturing at least one test structure with different respective light beam powers, in order to determine the threshold energy density EseuU above which a porous structure with dense walls is obtained, the speed of movement Vo of the light beam, the offset value HD0 of the light beam and the layer thickness e0 having been predetermined and kept constant during the manufacture of said at least one test structure, ii) selecting at least one parameter chosen from the speed of movement of the light beam, the offset value of the light beam and the layer thickness so that the energy density of the light beam during the subsequent manufacturing step is less than ESeuib