LOW-FLUIDITY POLYMER COMPOSITION CONTAINING AN ABS COPOLYMER AND A TERPOLYMER AND METHOD FOR REDUCING THE FLUIDITY OF AN ABS COPOLYMER
By blending ABS copolymer with a terpolymer containing ethylene and glycidyl group units, the fluidity and impact resistance of ABS copolymers are improved, facilitating extrusion molding and producing high-quality molded articles.
Patent Information
- Application Number
- FR2021013244
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-12-09
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-12-09
AI Technical Summary
Existing ABS copolymers face issues with high melt flow index (fluidity) leading to poor processability in extrusion molding and reduced impact strength during recycling, especially when impact modifiers are added, limiting their use in various applications.
Incorporating a terpolymer with repeating units derived from ethylene and glycidyl group into the ABS copolymer to reduce melt flow index and enhance impact resistance, using a blend of ABS copolymer, terpolymer, and optionally a copolymer with methyl acrylate and ethylene units.
The resulting polymer composition achieves reduced fluidity and improved impact resistance, enabling successful extrusion molding and manufacturing of high-quality molded articles with enhanced processability.
Abstract
Description
Title of the invention: LOW FLUIDITY POLYMER COMPOSITION CONTAINING AN ABS COPOLYMER AND A TERPOLYMER AND METHOD FOR REDUCING THE FLUIDITY OF AN ABS COPOLYMER Technical field
[0001] The following disclosure relates to a low-flow polymer composition containing an acrylonitrile-butadiene-styrene copolymer and a terpolymer, and a method of reducing the flowability of an acrylonitrile-butadiene-styrene copolymer. BACKGROUND
[0002] An acrylonitrile-butadiene-styrene (ABS) copolymer has advantages such as excellent chemical resistance, dimensional stability, processability, and the like, and is used in a wide variety of fields such as washing machines, televisions, refrigerators, displays, copiers, fax machines, automobile exterior rearview mirrors, cell phone housings, toy materials, and game consoles.
[0003] There are various methods of molding an ABS copolymer, and the products listed above can be manufactured mainly by injection molding. One of the important things in the molding step is a melt flow index (MFI) which refers to the viscosity of a molten polymer, and a polymer composition having a high melt flow index, i.e., having high fluidity, is mainly used in injection molding.
[0004] Furthermore, as the interest in environmental friendliness increases, the demand for plastic recycling is increasing, and also a lot of research and development for ABS recycling is being carried out. However, when an ABS copolymer is recycled, the impact strength decreases, and especially when an injection molded article is recycled, the melt flow rate is significantly high, so that other molding methods such as extrusion molding and profile molding cannot be used.
[0005] In addition, since the ABS copolymer itself has insufficient impact strength compared with other thermoplastic polymers, an impact modifier and the like can be added to improve the impact strength of the ABS copolymer. However, when the additive is added, the viscosity decreases and the melt flow rate increases, and thus there is still a problem that the processability is deteriorated during extrusion molding and the quality of the manufactured molded article is deteriorated.
[0006] There is therefore a demand for research and development of a polymer composition having improved impact resistance and also reduced fluidity to have an advantageous melt flow index for extrusion molding. SUMMARY
[0007] One embodiment of the present disclosure relates to providing a low fluidity polymer composition containing an acrylonitrile-butadiene-styrene copolymer and a terpolymer.
[0008] Another embodiment of the present disclosure relates to providing a polymer composition which is suitable for a molding process requiring a low melt flow rate such as extrusion molding, by incorporating a terpolymer into an acrylonitrile-butadiene-styrene copolymer to impart low flow rate to the polymer composition. Yet another embodiment of the present disclosure relates to providing a high quality molded article having improved processability and processability characteristics, and improved impact resistance.
[0009] In order to solve the above problems, the present inventors have found that when a polymer composition contains an acrylonitrile-butadiene-styrene copolymer and a terpolymer containing a first repeating unit derived from ethylene and a second repeating unit containing a glycidyl group, the melt flow index of the polymer composition is effectively reduced, and also a molded article having improved impact resistance can be manufactured by using the polymer composition, and they have thus made the present disclosure.
[0010] In a general aspect, a low-flow polymer composition contains: an acrylonitrile-butadiene-styrene (ABS) copolymer and a terpolymer, wherein the terpolymer contains a first repeating unit derived from ethylene and a second repeating unit containing a glycidyl group.
[0011] According to an illustrative embodiment of the present disclosure, the terpolymer may contain a second repeating unit derived from glycidyl (meth)acrylate and a third repeating unit derived from methyl (meth)acrylate.
[0012] According to an illustrative embodiment of the present disclosure, the second repeating unit may represent 3 to 20% by weight of the terpolymer, based on the total weight.
[0013] According to an illustrative embodiment of the present disclosure, the third repeating unit may represent 20 to 30% by weight of the terpolymer, based on the total weight.
[0014] According to an illustrative embodiment of the present disclosure, the terpolymer may be incorporated in an amount of 0.1 to 10 parts by weight, based on 100 parts by weight of the ABS copolymer.
[0015] According to an illustrative embodiment of the present disclosure, the polymer composition may further contain a copolymer containing a repeating unit derived from methyl (meth)acrylate and a repeating unit derived from ethylene.
[0016] According to an illustrative embodiment of the present disclosure, the copolymer may be incorporated in an amount of 1 to 20 parts by weight, based on 100 parts by weight of the ABS copolymer.
[0017] According to an illustrative embodiment of the present disclosure, the low-flow polymer composition may satisfy the following Equation 1:
[0018] [Equation 1] MFICOm / MFIabs <1.0
[0019] wherein MFICom is the melt flow index (g / 10 min) of the low-flow polymer composition, MFIABS is the melt flow index of a pure ABS copolymer, and the melt flow index is measured in accordance with ISO 1133-1 (2011).
[0020] According to an illustrative embodiment of the present disclosure, the low fluidity polymer composition may be intended for extrusion.
[0021] In accordance with an illustrative embodiment of the present disclosure, the low-flow polymer composition may contain substantially no polycarbonate.
[0022] In accordance with an illustrative embodiment of the present disclosure, a molded article made by using the low-flow polymer composition can satisfy the following Equation 2:
[0023] [Equation 2] ISCom / ISABs >1.0
[0024] wherein IScom is the impact strength (kJ / m2) of a molded article made by using the low-flow polymer composition, ISABS is the impact strength of a molded article made by using a pure ABS copolymer, and the impact strength is measured in accordance with ISO 179 leA.
[0025] In another general aspect, a molded article made by using the low-flow polymer composition described above can be obtained.
[0026] In yet another general aspect, a method of reducing the flowability of an ABS copolymer comprises: melt blending a polymer composition containing an acrylonitrile-butadiene-styrene (ABS) copolymer and a terpolymer using an extruder, wherein the terpolymer contains a first repeating unit derived from ethylene and a second repeating unit containing a glycidyl group.
[0027] Other features and aspects will become apparent from the detailed description, drawings, and claims which follow. DETAILED DESCRIPTION OF EMBODIMENTS
[0028] The present disclosure will be described in more detail hereinafter. However, the following examples or embodiments are only references for describing the present disclosure in detail, and the present disclosure is not limited thereto and can be implemented in various forms.
[0029] Furthermore, unless otherwise defined, all technical terms and scientific terms have the same meanings as those commonly understood by persons skilled in the art to which this disclosure relates.
[0030] The terms used herein are used only to effectively describe a certain embodiment, and are not intended to limit the present disclosure.
[0031] Further, unless otherwise specifically described, "comprising" any elements shall be understood to further imply the incorporation of other elements rather than the exclusion of any other elements.
[0032] In addition, the numerical ranges used in this specification may encompass all numerical values within the range, including the lower limit and the upper limit, logically derived increments in one form and over one scope within a defined range, all doubly limited values, and all possible combinations of the upper limit and the lower limit within the defined numerical range in different forms. Unless otherwise defined in the specification of this disclosure, values that may be outside a numerical range due to experimental error or rounding of a value are also encompassed within the defined numerical range.
[0033] A "low fluidity" described in the present disclosure refers to a characteristic having a melt flow index lower than the melt flow index of a base polymer in a polymer composition. Specifically, a polymer composition having a melt flow index lower than the melt flow index of an acrylonitrile-butadiene-styrene copolymer can be defined as a low fluidity polymer composition.
[0034] The meaning of "substantially does not contain" described in the present disclosure may be the presence of 1 part by weight or less, specifically 0.1 part by weight or less, based on 100 parts by weight of the acrylonitrile-butadiene-styrene (ABS) copolymer. For example, the meaning of a low-flow polymer composition that "substantially does not contain polycarbonate" may be the presence of 1 part by weight or less of polycarbonate, based on 100 parts by weight of the acrylonitrile-butadiene-styrene (ABS) copolymer.
[0035] The present disclosure will be described in more detail below.
[0036] The present disclosure provides a low-carbon polymer composition fluidity containing: an acrylonitrile-butadiene-styrene (ABS) copolymer and a terpolymer, wherein the terpolymer contains a first repeating unit derived from ethylene and a second repeating unit containing a glycidyl group.
[0037] The acrylonitrile-butadiene-styrene copolymer (hereinafter referred to as ABS copolymer) may be an acrylonitrile-butadiene-styrene copolymer in which butadiene, styrene and acrylonitrile are polymerized by a common or known method. For example, it may be a polymer polymerized by an emulsion polymerization method or a suspension polymerization method, and a commercially available product may be used without limitation.
[0038] By way of non-limiting example, a repeating unit derived from butadiene may be contained in an amount of 5 to 50 wt%, specifically 20 to 40 wt%, a repeating unit derived from styrene may be contained in an amount of 20 to 70 wt%, specifically 25 to 60 wt%, and a repeating unit derived from acrylonitrile may be contained in an amount of 5 to 40 wt%, specifically 10 to 35 wt%, based on the total weight of the ABS copolymer. The weight average molecular weight (Mw) of the ABS copolymer may be 10,000 to 500,000 g / mol, 50,000 to 300,000 g / mol, or 80,000 to 250,000 g / mol. In addition, the glass transition temperature (Tg) of the ABS copolymer may be 70 to 150°C or 80 to 130°C, and the melting point (Tm) of the ABS copolymer may be 150 to 300°C or 180 to 250°C. The melt flow index (MFI) of the ABS copolymer may be 1 to 100 g / 10 min, 1 to 50 g / 10 min, or 5 to 30 g / 10 min, but is not limited thereto.
[0039] According to an illustrative embodiment, the terpolymer may contain a first repeating unit derived from ethylene, a second repeating unit derived from glycidyl (meth)acrylate, and a third repeating unit derived from methyl (meth)acrylate. Specifically, the terpolymer may contain a first repeating unit derived from ethylene, a second repeating unit derived from glycidyl methacrylate, and a third repeating unit derived from methyl acrylate.
[0040] The terpolymer may be a terpolymer in which ethylene, glycidyl (meth)acrylate, and methyl (meth)acrylate are polymerized by a common or known method, or a commercially available product may be used without limitation.
[0041] Specifically, the second repeating unit may be contained in an amount of 0.1 to 50 wt%, specifically 1 to 30 wt%, and more specifically 3 to 20 wt%, based on the total weight of the terpolymer. In addition, the third repeating unit may be included in an amount of 0.1 to 50 wt%, specifically 5 to 40 wt%, and more specifically 20 to 30 wt%, based on the total weight of the terpolymer. The weight average molecular weight (Mw) of the terpolymer may be 10,000 to 500,000 g / mol or 50,000 to 250,000 g / mol, and the melt flow index (MFI, 190°C / 2.16 kg) of the terpolymer may be 1 to 100 g / 10 min, 1 to 40 g / 10 min, or 1 to 30 g / 10 min, but is not limited to. The polymer composition containing the terpolymer satisfying the above ranges has an effectively reduced melt flow index (MFI) to improve the processability in extrusion molding and also improve the impact resistance of the molded article produced.
[0042] According to an illustrative embodiment, the terpolymer may be included in an amount of 0.1 to 20 parts by weight or 0.1 to 10 parts by weight, specifically 0.5 to 7 parts by weight, and more specifically 1 to 5 parts by weight, based on 100 parts by weight of the ABS copolymer. When the above ranges are satisfied, the melt flow index (MFI) of the polymer composition can be adjusted more easily, and a molded article having a further improved impact resistance can be manufactured. In addition, the content of the terpolymer can be adjusted appropriately to easily apply the melt flow index (MFI) of the polymer composition to a target value and the impact resistance of the manufactured molded article.
[0043] According to an illustrative embodiment, the polymer composition may further contain a copolymer containing a repeating unit derived from methyl (meth)acrylate and a repeating unit derived from ethylene. Specifically, a copolymer in which methyl (meth)acrylate and ethylene are polymerized by a common or known method may be used, or a commercially available product may be used without limitation. Specifically, the copolymer may be poly(ethylene-co-methyl methacrylate) or poly(ethylene-co-methyl acrylate).
[0044] By way of non-limiting example, the repeating unit derived from methyl (meth)acrylate may be included in an amount of 1 to 50% by weight, specifically 15 to 35% by weight, and the repeating unit derived from ethylene may be included in an amount of 50 to 99% by weight, specifically 65 to 85% by weight, based on the total weight of the copolymer. The weight average molecular weight (Mw) of the copolymer may be 10,000 to 500,000 g / mol or 50,000 to 250,000 g / mol and the melt flow index (MFI, 190°C / 2.16 kg) of the copolymer may be 1 to 800 g / 10 min, 1 to 50 g / 10 min, or 1 to 45 g / 10 min, but is not limited thereto.
[0045] The copolymer may be included in an amount of 0.1 to 30 parts by weight, 1 to 20 parts by weight, or 1 to 15 parts by weight, based on 100 parts by weight of the ABS copolymer. The weight ratio of the terpolymer to the copolymer may be 1:0.1 to 50 or 1:0.5 to 10, but is not limited thereto. In addition, the polymer composition can easily apply the melt flow index (MFI) of the polymer composition to a target value and the impact strength of the molded article manufactured by appropriately adjusting the content of the copolymer.
[0046] According to an illustrative embodiment, the low-flow polymer composition may further contain a thermoplastic polymer, in addition to the acrylonitrile-butadiene-styrene polymer. The non-limiting example of the polymer The thermoplastic polymer may be one selected from the group consisting of polyvinyl chloride (PVC), polypropylene (PP), polyacrylate, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polymethyl methacrylate (PMMA), polyamide, styrene-acrylonitrile copolymer (SAN), acrylonitrile-styrene-acrylate (ASA), and the like, or a mixture thereof. The thermoplastic polymer may be included in an amount of 0.1 to 200 parts by weight, 1 to 100 parts by weight, or 1 to 50 parts by weight, based on 100 parts by weight of the ABS copolymer, but is not limited thereto, and for manufacturing a molded article having physical properties to be targeted, the content of the composition may be adjusted.However, when a polycarbonate (PC) is included in the polymer composition, the viscosity of the polymer composition is rather significantly reduced so that it is difficult to implement low fluidity, which may therefore not be preferred.
[0047] According to an illustrative embodiment, the low-flow polymer composition may further contain an additive that is commonly used in the art, depending on the purpose and use. For example, a UV stabilizer, a UV absorber, an antioxidant, a viscosity modifier, a plasticizer, a heat stabilizer, a colorant, a pigment, a dye, a mold release agent, an antistatic agent, an antibacterial agent, a processing aid, a metal deactivator, a flame retardant, an anti-friction agent, a wear resistance imparting agent, a lubricant, and the like may be further included. Here, the additives may be included at a suitable content within a range that does not adversely affect the physical properties desired in the present disclosure.
[0048] In accordance with an illustrative embodiment of the present disclosure, the low-flow polymer composition may satisfy the following Equation 1, and specifically the following Equation 3:
[0049] [Equation 1] MFICom / MFIABs <1.0
[0050] [Equation 3] MFICom / MFIAbs < 0.8
[0051] in which MFICom is the melt flow index (g / 10 min) of the polymer composition, MFIABs is the melt flow index of a pure ABS copolymer, and the melt flow index is measured in accordance with ISO 1133-1 (2011).
[0052] When Equation 1, specifically Equation 3, is satisfied, the polymer composition may have low fluidity, and the polymer composition may have a more advantageous melt flow rate during extrusion molding to improve processability.
[0053] The present disclosure can provide a molded article manufactured by using the low-flow polymer composition described above. Any method for processing the molded article can be used without much limitation as long as it is commonly used or known in the art and, for example, a method such as injection molding, extrusion, profile extrusion, calendering, and direct blowing can be used, and in particular, since the low-flow polymer composition contains the ABS copolymer and the terpolymer described above, the composition has a reduced melt flow index (MFI) upon extrusion molding, and therefore, when the low-flow polymer composition is used for extrusion, the processability can be further improved, and a high-quality molded article can be manufactured.
[0054] According to an illustrative embodiment of the present disclosure, the molded article made by using the low-flow polymer composition may satisfy the following Equation 2, specifically the following Equation 4. The molded article may include known molded articles such as a film and a sheet without limitation. Specifically, the molded article of the following Equations 2 and 4 may be a sheet:
[0055] [Equation 2] ISCom / ISABs >1.0
[0056] [Equation 4] ISCom / ISABs> 1.2
[0057] in which ISCom is the impact strength (kJ / m2) of a molded article manufactured by using the low-flow polymer composition and ISABs is the impact strength of a molded article manufactured by using a pure ABS copolymer, and the impact strength is measured in accordance with ISO 179 leA.
[0058] Since the low-flow polymer composition contains the above-described ABS copolymer and terpolymer, the molded article manufactured by using the composition can satisfy Equation 2, specifically Equation 4, to implement excellent impact resistance.
[0059] More specifically, the low-flow polymer composition can satisfy both Equations 1 and 2, specifically both Equations 3 and 4. In this case, the low-flow polymer composition having a reduced melt flow index (MFI) can be used to manufacture a molded article having even further improved impact resistance.
[0060] The present disclosure may provide a method for reducing the fluidity of an ABS copolymer comprising: melt blending a polymer composition containing an acrylonitrile-butadiene-styrene (ABS) copolymer and a terpolymer using an extruder, wherein the terpolymer contains a first repeating unit derived from ethylene and a second repeating unit containing a glycidyl group.
[0061] Detailed descriptions for the acrylonitrile-butadiene-styrene (ABS) copolymer and the terpolymer are as described above, and will therefore be omitted.
[0062] The method of reducing the fluidity of an ABS copolymer can be implemented to provide more advantageous viscosity conditions in the ABS molding step, and specifically the method of reducing the fluidity of an ABS copolymer can be used to obtain a reduced melt index in the ABS extrusion molding process.
[0063] According to an illustrative embodiment, the method for reducing the fluidity of an ABS copolymer may comprise a step of melt-mixing the polymer composition by means of an extruder. Any melt-mixing method may be used without much limitation as long as it is a common method for melt-mixing a thermoplastic resin, and as a non-limiting example thereof, the melt-mixing method may be carried out at a temperature of 200 to 260°C by using a twin-screw melt-mixing extruder, but is not limited thereto. Then, the polymer composition is melt-mixed to produce a pellet for molding by an extruder, and the produced pellet for molding may be used for manufacturing a molded article, but the present disclosure is not limited thereto.
[0064] According to an illustrative embodiment, the polymer composition can contain both the ABS copolymer and the terpolymer to easily achieve low fluidity, thereby being applied to a molding process requiring low fluidity such as extrusion molding for better processability, and a molded article having improved impact resistance and high quality can be manufactured.
[0065] Hereinafter the present disclosure will be described in more detail with reference to examples and comparative examples. However, the following examples and comparative examples are only examples to describe the present disclosure in more detail, and do not limit the present disclosure in any way.
[0066] The physical properties of the following examples and comparative examples of the present disclosure were measured by the following methods.
[0067] [Physical property evaluation method]
[0068] 1. Melt Flow Index (MFI) [g / 10 min]
[0069] The melt flow index (MFI) is measured at a temperature of 220°C under conditions of a 10 kg load in accordance with ISO 1133-1 (2011). The measured values are listed in Table 1, and when the measured MFI value satisfies Equation 1, it is determined that the composition has low flowability.
[0070] [Equation 1] MFICom / MFIAbs <1.0
[0071] wherein MFICom is the melt flow index of a polymer composition according to the examples and comparative examples, and MFIAbs is the melt flow index of a pure ABS copolymer.
[0072] 2. Impact resistance [kJ / m2]
[0073] The Charpy impact strength on notched bar is measured in accordance with ISO 179 leA. The measured values are listed in Table 1.
[0074] 3. Flexural modulus [MPa]
[0075] The flexural modulus is measured in accordance with ISO 178. The measured values are listed in Table 1.
[0076] [Examples 1 to 5, and Comparative Examples 1 and 2]
[0077] An acrylonitrile-butadiene-styrene copolymer (Terluran® GP22), an ethylene-methyl acrylate-glycidyl methacrylate terpolymer (Lotader® AX8900), and an ethylene-methyl acrylate copolymer (Lotryl® 29MA03T) were blended according to the raw material proportions described in Table 1 below to prepare polymer compositions. Specifically, the raw materials listed in Table 1 were dry blended and continuously quantitatively fed into a feeding unit of a twin-screw extruder for melt blending and production of a molding pellet. The produced pellet was sufficiently dried, and a sample suitable for the specification described in [Physical Property Evaluation Method] was prepared for physical property measurement.
[0078] [Tableauxl] Polymer Composition (parts by weight) MFI Impact Strength Flexural Modulus Terluran® G P22 Lotader® A X8900 Lotryl® 29 MA03T Example 1 99 1 - 9.9 24 2041 Example 2 97 3 - 7.2 27 1984 Example 3 95 5 - 6.8 30 1910 Example 4 94 1 5 10.6 31 1839 Example 5 94 3 3 7.9 29 1784 Comparative Example 1 100 - - 14.2 22 2171 Comparative Example 2 95 - 5 16 37 1975
[0079] As shown in Table 1 above, when Comparative Example 1 for a pure ABS copolymer and Examples 1 to 3 for a polymer composition containing the ABS copolymer and the terpolymer described above are compared, it is confirmed that the MFI of the examples is effectively reduced, and also better impact resistance is observed.
[0080] When Example 3 and Comparative Example 2 containing the methyl acrylate-ethylene copolymer are compared, they have the same amount of ABS copolymer, but their MFIs conflict, and since the content of the terpolymer was increased in Examples 1 to 3, the MFI was further reduced. It is therefore confirmed that the polymer composition according to an illustrative embodiment of the present disclosure can effectively realize low fluidity by incorporating the ABS copolymer and the terpolymer.
[0081] The present disclosure can provide a low-flow polymer composition containing an acrylonitrile-butadiene-styrene copolymer and a terpolymer. Specifically, the low-flow polymer composition can impart an advantageous melt flow index in extrusion molding requiring low flowability by an interaction of the terpolymer and the acrylonitrile-butadiene-styrene copolymer, and also a molded article having improved impact resistance can be manufactured by using the composition. Therefore, when the low-flow polymer composition is used, it is easy to adjust the viscosity of the composition, the processability in a polymer molding step is improved, and a molded article having excellent impact resistance can be manufactured in various shapes.
[0082] Although the present disclosure has been described above by specified objects and specific illustrative embodiments, these have been presented only to facilitate the overall understanding of the present disclosure. Therefore, the present disclosure is not limited to the illustrative embodiments by the specific features, and various changes and modifications may be made by those skilled in the art concerned by the present disclosure from this description.
[0083] Accordingly, the spirit of the present disclosure should not be limited to the illustrative embodiments described above, and the following claims, as well as anything modified equally or equivalently to the claims, are intended to fall within the scope and spirit of the disclosure.
Claims
Claims
1. A low-flow polymer composition comprising an acrylonitrile-butadiene-styrene (ABS) copolymer and a terpolymer, wherein the terpolymer contains a first repeating unit derived from ethylene, a second repeating unit derived from glycidyl (meth)acrylate, and a third repeating unit derived from methyl (meth)acrylate, which low-flow polymer composition satisfies the following Equation 1: [Equation 1] MFIcom / MFIABs <1.0 wherein MFICom is the melt flow index (g / 10 min) of the low-flow polymer composition, MFIAbs is the melt flow index of a neat ABS copolymer, and the melt flow index is measured in accordance with ISO 1133-1 (2011).
2. A low-flow polymer composition according to claim 1, wherein the second repeating unit is included in an amount of 3 to 20% by weight, based on the total weight of the terpolymer.
3. A low-flow polymer composition according to claim 1, wherein the third repeating unit is included in an amount of 20 to 30% by weight, based on the total weight of the terpolymer.
4. A low-flow polymer composition according to claim 1, wherein the terpolymer is included in an amount of 0.1 to 10 parts by weight based on 100 parts by weight of the ABS copolymer.
5. A low-flow polymer composition according to claim 1, further comprising a copolymer containing a repeating unit derived from methyl (meth)acrylate and a repeating unit derived from ethylene.
6. A low-flow polymer composition according to claim 5, wherein the copolymer is included in an amount of 1 to 20 parts by weight, based on 100 parts by weight of the ABS copolymer.
7. The low-flow polymer composition of claim 1, which low-flow polymer composition contains 1 part by weight or less of polycarbonate, based on 100 parts by weight of the acrylonitrile-butadiene-styrene (ABS) copolymer.
8. Use of a low fluidity polymer composition according to any one of claims 1 to 7, for extrusion.
9. A molded article made by using the low-flow polymer composition of any one of claims 1 to 7.
10. A molded article according to claim 9, which satisfies the following Equation 2: [Equation 2] ISCOm / ISAbs > 1.0 wherein IScom is the impact strength (kJ / m2) of the molded article, ISabs is the impact strength of a molded article manufactured by using a pure ABS copolymer, and the impact strength is measured in accordance with ISO 179 leA.
11. A method of reducing the fluidity of an acrylonitrile-butadiene-styrene (ABS) copolymer, the method comprising: melt blending a polymer composition containing an ABS copolymer and a terpolymer using an extruder, wherein the terpolymer contains a first repeating unit derived from ethylene and a second repeating unit derived from glycidyl (meth)acrylate and a third repeating unit derived from methyl (meth)acrylate.