- 2024-11-08
- Estimated Expiration
- 2042-04-08
AI Technical Summary
Fused filament deposition methods produce polymeric parts with significant porosity, leading to non-gas-tight structures that cannot be effectively sealed against gases and liquids, particularly in applications requiring high pressure resistance.
A filling solution comprising an epoxy resin diluted between 50% and 80% in a solvent is used to impregnate the porosity of parts made by fused wire deposition, ensuring complete filling and maintaining waterproofness even under deformation or damage.
The process results in gas and liquid-tight parts that maintain integrity under pressures up to 4 bars, significantly reducing porosity and enhancing sealing effectiveness.
Smart Images

Figure 00000008_0000 
Figure 00000008_0001 
Figure 00000008_0002
Abstract
Description
Title of the invention: Waterproof part obtained by additive manufacturing Technical field
[0001] The invention relates to the field of parts manufactured by additive manufacturing. Prior art
[0002] Additive manufacturing methods have been widely developed in recent years because they represent a simple and rapid means of forming parts with the desired geometries and make it possible to obtain parts with complex geometries using simple processes. Additive manufacturing methods are numerous and the choice of one method or another is generally made according to the desired material and the desired characteristics of the part.
[0003] Among these manufacturing methods, fused filament fabrication (or FFF) is particularly useful for forming parts from polymeric material.
[0004] Fused filament deposition is a method that makes it possible to obtain a part directly with the desired dimensions by successively depositing a plurality of filaments made of polymeric material. To obtain a plane of the part, the filaments are arranged next to each other. It is then possible to obtain other planes of the part by depositing new filaments on those already deposited to obtain a three-dimensional part with the desired geometry. This deposition method, however, creates a part with significant porosity. Indeed, the filaments form spaces between two successive filaments in the direction parallel to the filaments, which the deposition method does not allow to be filled. The parts thus created are therefore not gas-tight.
[0005] Thus, there remains a need for a waterproof part made of polymeric material and manufactured by a fused wire deposition method. Statement of the invention
[0006] According to a first aspect, the invention aims to propose a part meeting this need.
[0007] For this, the invention relates to a part formed from a plurality of filaments composed of a polymeric material, the plurality of filaments defining a porosity in the direction parallel to the filaments, the part being characterized in that it comprises a filling solution in the porosity formed between the filaments, said filling solution comprising an epoxy resin diluted in a solvent at a dilution rate of between 50% and 80%, or even between 55% and 65%.
[0008] Such a part is gas-tight, because its porosity is filled throughout the entire thickness of the part. In addition, the tightness is maintained even during prolonged use. over time, even if the surface is damaged, for example if it is deformed or scratched.
[0009] Diluting the epoxy resin in the filling solution ensures better impregnation of the porosity of the part, and thus helps to facilitate the manufacturing process of the part.
[0010] In one embodiment, the polymeric material of the part comprises a polyetheretherketone, a polyetherimide, a polyetherketoneketone or a mixture of several polymers chosen from one or more of these families.
[0011] In one embodiment, the polymeric material may further comprise reinforcements, the reinforcements being able to be chosen from carbon fibers, glass fibers, Kevlar fibers or mixtures of several fibers from these families.
[0012] For example, the reinforcement content may be between 10% and 30% by mass.
[0013] In one embodiment, the solvent of the filling solution comprises butanone (also known as methyl ethyl ketone or MEK) pure or diluted in water. Dilution in water is particularly advantageous when the filling solution includes a water-based epoxy resin, for example an epoxy resin commercially available under the reference waterbond SR1900 ®.
[0014] In one embodiment, the porosity of the part comprising the filling solution is generally between 8% and 10%, in the case of a part deposited by fused filament deposition. Preferably more than 90% of the porosity of the part is filled by the filling solution.
[0015] In one embodiment, the epoxy resin of the filling solution may be selected from the epoxy resin available under the trade name Loctite ® EA9396, or a water-based epoxy resin, for example available under the trade name waterbond SR 1900.
[0016] In one embodiment, the part is a fuel cell end plate.
[0017] Indeed, a part such as has just been described has all the characteristics characteristics necessary for a fuel cell plate and in particular has gas and liquid tightness up to pressures of 4 bars.
[0018] Furthermore, obtaining such a plate is greatly simplified by using a fused wire deposition process. End plates according to this embodiment are less expensive alternatives and require less machining than the end plates of the prior art.
[0019] According to another of its aspects, the invention also relates to a method of manufacturing a part, the method comprising at least the following steps: - A step of manufacturing the part by depositing a plurality of filaments formed from a polymer using a fused filament deposition method; - a step of impregnating the porosity of the part thus manufactured with a filling solution, the filling solution comprising an epoxy resin diluted in a solvent at a dilution rate of between 50% and 80% or even between 55% and 65%, this impregnation step further comprising the application of reduced pressure to the porosity of the part.
[0020] The part thus obtained is impregnated throughout its porosity with the filling solution. Impregnation throughout the porosity of the part makes it possible to obtain parts whose advantages have been described above. In particular, impregnation to the heart of the porosity of the parts allows excellent sealing of the parts. For example, the remaining porosity of a part thus obtained may be less than 5%. Such porosity represents a reduction of approximately 50% of the porosity of a part obtained by fused filament deposition.
[0021] As demonstrated in the examples at the end of this application, the filling of all the porosity of the parts with the filling solution is enabled by the chosen specific dilution rate of the epoxy resin and the application of the reduced pressure to the porosity during the impregnation with the resin.
[0022] If the viscosity of the filling solution is too high, that is to say if the dilution rate is too low, the capillarity does not allow good impregnation to the core of the parts, even under reduced pressure.
[0023] Too high a dilution rate is also not satisfactory, because the quantity of filling solution retained inside the porosity is too low to allow good sealing.
[0024] In one embodiment, the porosity of the part during the impregnation step is at a pressure less than or equal to 900 mbar.
[0025] This reduced pressure allows very good impregnation of the internal porosity of the part by the filling solution.
[0026] In one embodiment, the impregnation of the part with the impregnation solution is carried out by at least partial immersion of the part in a bath comprising the filling solution. Brief description of the drawings
[0027] [Fig-1] [Fig.l] schematically represents a process for manufacturing a part by a fused deposition process.
[0028] [Fig.2] [Fig.2] represents a sectional view of a part conforming to part 1 of the example.
[0029] [Fig.3] [Fig.3] represents a sectional view of a part conforming to part 2 of the example.
[0030] [Fig.4] [Fig.4] represents a sectional view of a part conforming to part 3 of the example. Description of the embodiments
[0031] The invention is now described by means of figures and examples illustrating particular embodiments, which are only present to aid understanding of the invention and which should not be interpreted in a limiting manner.
[0032] [Fig. 1] very schematically represents a method of manufacturing a part 10 by a fused wire deposition method.
[0033] The part 10 is obtained by depositing filaments of a polymeric material 11 by means of a print head 13.
[0034] As shown in [Fig.l], in a part 10 obtained by molten filament deposition, the filaments 11 are deposited next to each other to form a part with the desired geometry, or even on top of each other to form a part of a certain thickness.
[0035] [Fig.l] represents a part 10 in the process of being manufactured and shows a filament 14 being deposited by the print head 13.
[0036] As indicated previously, a part obtained by this manufacturing method comprises a plurality of filaments of a polymeric material 11. These filaments have porosity between them. This porosity takes the form of channels 12, due to the geometry of the filaments 11.
[0037] In a part of the invention, the porosity is open, that is to say that it is possible to access the interior of the porosity from the outside without having to cross any material.
[0038] In the application, when a part is referred to as being sealed, this is to be understood as being sealed against gases and liquids. For example, sealing against gases and liquids encountered in a fuel cell, for example water, oxygen and hydrogen.
[0039] For example, a part will be said to be gas-tight if it can withstand a pressure of 2 bars, better still 4 bars, applied for at least 5 minutes. Examples
[0040] Three pieces were prepared, two according to a method outside the invention for comparison purposes, and the third according to the invention.
[0041] All three parts are made of polymeric material, obtained by a fused deposition process. The filaments used are made of polyetherimide, available under the trade name Ultem 1010™. The machine used for additive manufacturing is available under the trade name Stratasys ®.
[0042] The first part corresponds to a part directly obtained after the additive manufacturing step by fused wire deposition, without an additional process step.
[0043] The second part corresponds to a part obtained by a manufacturing step additive, like the first part but the process for obtaining the second part includes a step of applying an epoxy resin to its external surfaces.
[0044] The epoxy resin used is commercially available under the name Loctite ® EA9396. The epoxy resin is diluted to 50% by mass in butanone and is applied with a brush.
[0045] The third part is obtained like the first part by an additive manufacturing step. It is then placed in a bath of the same epoxy resin, Loctite ® EA9396, diluted to 50% by mass in butanone, and its porosity is placed under vacuum, at a pressure of 900 mbar for at least 10 minutes.
[0046] The part is then left to rest at room temperature for a period of at least 2 hours and then undergoes a resin polymerization cycle at 160°C for one hour.
[0047] It can be noted that the third part is according to the invention, and is moreover obtained by a method of the invention.
[0048] Leak tests are carried out on the three parts obtained. For this, the parts obtained are placed in a tank of water. One side of the part is placed under a given pressure of compressed air. If the compressed gas manages to pass through the part, bubbles are observed in the tank and the part is considered to be non-leaktight. Otherwise, that is to say if no leak is observed, the pressure applied to the part is increased.
[0049] The pressure applied to the parts is 0.25 bar, then 1.8 bar, and finally 4 bar, this pressure being maintained for up to 5 minutes if no leak is observed.
[0050] The table below describes the results obtained, and indicates for each part whether a leak is observed or not. If a leak is observed, the part is not tested at higher pressures and "—" indicates that the part has not been tested.
[0051] [Tables 1] Applied pressure 0.25 bar 1.8 bar 4 bar Part 1 (outside the invention) leak — — Part 2 (outside the invention) no leak leak — Part 3 (sebn the invention) no leak no leak no leak
[0052] As indicated in the table, part 1 corresponding to the part obtained directly after the deposition of molten wire shows leaks from the lowest pressures applied.
[0053] Part 2, corresponding to the part coated on the surface with diluted epoxy resin, remains watertight if low pressures are applied. However, leaks are observed from an applied pressure of 1.8 bars, and treating the surface of the part with a diluted resin therefore does not allow a watertight part to be obtained.
[0054] Only part 3, which is obtained by a process of the invention, makes it possible to obtain a sealed part which resists a pressure of 4 bars applied for at least 5 minutes.
[0055] Comparison of the behavior of these three parts clearly demonstrates that putting the porosity of the part under reduced pressure during impregnation with the diluted resin makes it possible to obtain a part which remains watertight at higher pressures than parts which are not obtained by a process of the invention.
[0056] [Fig. 2] and respectively figures 3 and 4, represents a tomography obtained for a section of part 1 of the example, and respectively part 2 and part 3.
[0057] In Figures 2 to 4, a porous portion of the part appears black, while a non-porous portion appears lighter.
[0058] [Fig.2], representing part 1, clearly shows the porosity channels characteristic of a part obtained by deposition of fused wire.
[0059] [Fig.3], representing part 2, shows fewer porous channels, some being filled by the applied surface treatment.
[0060] [Fig.4], representing part 3, shows even less porosity, indicating even better sealing.
Claims
Claims
1. A method of manufacturing a fuel cell terminal plate, the method comprising at least the following steps: - a step of manufacturing the fuel cell terminal plate by depositing a plurality of filaments (11) formed of a polymer by means of a fused deposition method; - a step of impregnating the porosity of the part thus manufactured with a filling solution, the filling solution comprising an epoxy resin diluted in a solvent at a dilution rate of between 50% and 80%, this step further comprising the application of a pressure less than or equal to 900 mbar to the porosity of the part; and - a step of polymerizing the epoxy resin.
2. A manufacturing method according to claim 1, wherein the polymeric material comprises a polyetheretherketone, a polyetherimide, a polyetherketoneketone or a mixture of several polymers chosen from one or more of these families.
3. Manufacturing method according to claim 1 or 2, in which the polymeric material further comprises reinforcements, the reinforcements being able to be chosen from carbon fibers, glass fibers, Kevlar fibers or mixtures of several fibers from these families.
4. A manufacturing method according to any one of claims 1 to 3, wherein the solvent of the filling solution comprises pure butanone or diluted in water.