Manufacturing process for a corrugated sheet of cold-rolled stainless steel

The manufacturing process for cold-rolled stainless steel sheets with targeted heat treatments enhances fatigue resistance by transforming martensite into fine-grained austenite, addressing the vulnerability of corrugated stainless steel membranes in liquefied natural gas tanks.

FR3135467B1Active Publication Date: 2024-09-27GAZTRANSPORT & TECHNIGAZ SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2022004482
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-05-11
Publication Date
2024-09-27
Estimated Expiration
2042-05-11

AI Technical Summary

Technical Problem

Corrugated stainless steel sheets used as primary sealing membranes for liquefied natural gas tanks face issues with fatigue resistance due to thermal contraction and mechanical stresses, leading to potential rupture at nodes under extreme conditions.

Method used

A manufacturing process involving cold-rolled stainless steel sheets with specific compositions and heat treatments to recrystallize target zones, transforming martensite into fine-grained austenite to enhance fatigue resistance.

Benefits of technology

The process significantly improves the elastic limit and fatigue resistance of the corrugated stainless steel sheets, extending their lifespan under cyclic stress conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000021_0000
    Figure 00000021_0000
  • Figure 00000021_0001
    Figure 00000021_0001
  • Figure 00000021_0002
    Figure 00000021_0002
Patent Text Reader

Abstract

The invention relates to a method for manufacturing a corrugated stainless steel sheet, comprising the following steps: Supplying (100) a stainless steel sheet; Deforming (110) the stainless steel sheet to obtain a corrugated sheet comprising target zones with a geometric deformation rate between 15% and 45%; Heat treating (120) the target zones at a temperature and heat treatment time defined according to the composition of the stainless steel, to obtain a corrugated sheet with recrystallized target zones; Cooling (130) the corrugated sheet with recrystallized target zones. Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Method for manufacturing a cold-rolled corrugated stainless steel sheet

[0001] The present invention relates to a method of manufacturing a corrugated stainless steel sheet.

[0002] This manufacturing process is more particularly intended to be implemented for the manufacture of a corrugated stainless steel sheet for application as a primary sealing membrane for the transport and / or storage of liquefied natural gas (also known by the acronym LNG) in a tank.

[0003] A sheet obtained by the manufacturing method of the invention may, by way of a preferred but non-limiting illustrative example, be used for the production of an insulating and sealed wall of a tank, integrated into a supporting structure, for example the hull of a ship.

[0004] Such tanks are, for example, those used on liquefied gas transport vessels. They must be perfectly watertight and sufficiently insulating to contain liquefied gas at low temperature and limit its evaporation.

[0005] With reference to [Fig.lA], these walls are generally made up of two successive sealing membranes, one primary 10 in contact with the product contained in the tank and the other secondary 30 arranged between the primary membrane 10 and the supporting structure 50, these two membranes being alternated with two thermally insulating barriers 20, 40. Tank walls are thus known made up of a primary insulation 20 associated with a primary membrane 10 made of stainless steel, and of a secondary insulation 40 associated with a flexible or rigid secondary membrane 30. This secondary membrane 30 comprises at least one thin continuous metal sheet, for example made of aluminum, glued in a sandwich between two glass fiber fabrics, a binder being able to ensure cohesion between the glass fabrics and the aluminum. The insulating and sealed walls of these tanks are preferably made from a set of prefabricated panels.Typically, each prefabricated panel has the general shape of a rectangular parallelepiped, the primary insulation element 20 and the secondary insulation element 40 having, respectively, seen in plan, the shape of a first rectangle and a second rectangle whose sides are substantially parallel, the lengths and / or the width of the first rectangle being less than those of the second rectangle, in order to provide a peripheral edge. The peripheral edges of the adjacent secondary insulation elements 40 and the side walls of the primary insulation elements 20 define corridors 24, which may extend over the entire length, width or height of the tank. The continuity of the primary insulation 20 is. made by inserting paving stones 25 into the corridors 24. To ensure the continuity of the secondary membrane 30, at the junction between two adjacent panels, said peripheral edges are covered, before the installation of said paving stones 25, with a strip of flexible sheet 35, comprising at least one thin continuous metal sheet. The assembly of these different panels requires very strict operating procedures and great assembly precision, in order to guarantee the thermal insulation and the sealing of the tank.

[0006] Another variant of the tank wall is partially shown in [Fig. 1B]. In this variant, the walls are also made up of two successive sealing membranes, one primary 10 in contact with the product contained in the tank and the other secondary 30 arranged between the primary membrane 10 and the supporting structure 50, these two membranes being alternated with two thermally insulating barriers 20, 40. In this variant, the secondary membrane 30 can be stretched in Invar® or in a high manganese alloy and the corrugated primary membrane 10 in stainless steel. The insulation panels of the thermally insulating barriers 20, 40 are preferably made of reinforced polyurethane foam.

[0007] The tanks of such ships are subject to numerous constraints. Thus, cooling the tank before filling it to very low temperatures, for example of the order of -160°C for methane, or even close to -170°C, can create constraints due to the different thermal contractions of the materials constituting the walls. In addition, the ship in navigation is subject to numerous constraints such as swell, which can cause deformations of its hull and therefore of the walls of the tank by repercussion. The movements of the cargo can also create overpressure or backpressure constraints on the walls of the tank.

[0008] It should be noted that the arrangement of the insulation element(s) and the membranes is described above by way of illustration and is in no way limiting. The invention relates more specifically to the primary membrane described below.

[0009] The primary membrane 10 comprises corrugations extending over a surface of the primary membrane. These corrugations are intended to give flexibility to the primary membrane to accommodate the thermal contraction of the steel when the tank is cooled. It is thus possible to define the surface of the primary membrane by flat zones 11, waves 12 and nodes 13, as shown in [Fig. 2]. These nodes 13 are therefore the result of a deformation and are the site of a metallurgical transformation of the material from which the sheet is made. As a result, the nodes 13 form a geometrically stressed zone.

[0010] During the transport and / or storage of liquefied natural gas, the primary membrane 10 is in direct contact with the liquefied natural gas. Therefore, and as mentioned above, the nodes 13 are areas which present a risk of fatigue failure. increased when using corrugated sheet as a primary waterproofing membrane for the transport and / or storage of LNG. Indeed, the bending movements of the ship's beam fatigue the double hull of the ship and, consequently, the membrane.

[0011] The invention aims to overcome all or part of the problems cited above by proposing a method for manufacturing a corrugated stainless steel sheet having a particular heat treatment making it possible to modify the structure of the material in the target zones, giving the sheet thus obtained better fatigue resistance by improving its elastic limit.

[0012] To this end, the invention relates to a method for manufacturing a cold-rolled corrugated stainless steel sheet, comprising the following steps: - Supply of a cold-rolled stainless steel sheet having a composition comprising, the contents being expressed by mass: 0.005% < C < 0.05%, and preferably C < 0.03%; 0.1% <Si<l%; 0.5% < Mn < 2%; 4% < Ni < 10.5%; 16% < Cr < 20%; 0% < N < 0.2%; 0% < P < 0.045%; 0% < S < 0.015%; - Deformation of the stainless steel sheet, to obtain a corrugated sheet comprising target zones having a geometric deformation rate of between 15% and 45%, preferably less than 35%, or a section reduction rate in the target zones of less than 25%; - Heat treatment of the target areas of the corrugated sheet at a temperature and heat treatment time defined according to the composition of the stainless steel, to obtain a corrugated sheet with recrystallized target areas; - Cooling of the corrugated sheet with recrystallized target areas.

[0013] In one embodiment, the content of the stainless steel, expressed by mass, in nickel and nitrogen is such that: 4% < Ni < 8%, 0.05% < N < 0.2%,

[0014] and the duration of the heat treatment is defined according to the temperature of the heat treatment: temperature duration 700°C 15 to 40 minutes 750°C 5 to 20 minutes 800°C 3 to 8 minutes 850°C 30 seconds to 3 minutes

[0015]

[0016]

[0017]

[0018]

[0019]

[0020]

[0021]

[0022]

[0023]

[0024]

[0025]

[0026] In another embodiment, the content of the stainless steel, expressed by mass, in nickel and nitrogen is such that: 8% < Ni < 10.5%, 0 <N<0,l%, and the duration of the heat treatment is defined according to the temperature of the heat treatment: temperature duration 750°C 4 to 15 minutes 800°C 2 to 8 minutes 850°C 20 seconds to 2 minutes 900°C 5 to 15 seconds Advantageously, the cooling of the corrugated sheet with recrystallized target zones is carried out at a speed greater than or equal to 50°C / s. Advantageously, the heat treatment is carried out in a pass-through furnace. Advantageously, the heat treatment and / or cooling is carried out in an inert or reducing environment. Advantageously, the heat treatment is carried out in a vacuum furnace. In another embodiment of the manufacturing method according to the invention, the heat treatment can be carried out by applying heating bells to the target areas. Advantageously, the cooling of the corrugated sheet with recrystallized target zones is carried out by quenching in a quenching fluid. Advantageously, the cooling of the corrugated sheet with recrystallized target zones can be carried out by injection under pressure of a quenching fluid, preferably at room temperature. The manufacturing method according to the invention may further comprise, prior to the heat treatment, a step of cleaning the corrugated sheet. The invention also relates to a sealed and thermally insulating tank comprising at least one corrugated sheet with recrystallized target zones obtained by such a manufacturing method. The invention also relates to a cold-rolled stainless steel corrugated sheet. having a composition comprising, the contents being expressed by mass: - 0.005% < C < 0.05%, and preferably C < 0.03%; 0.1% <Si<l%; 0.5% < Mn < 2%; 4% < Ni < 10.5%; 16% < Cr < 20%; 0% < N < 0.2%; 0% < P < 0.045%; 0% < S < 0.015%; said corrugated sheet comprising corrugations defining at least one target zone having a geometric deformation rate of between 15% and 45%, preferably less than 35%, or a section reduction rate in the target zones of less than 25%, and in which the at least one target zone is recrystallized.

[0027] Advantageously, the corrugated sheet has a first corrugation in a first direction and a second corrugation in a second direction, substantially perpendicular to the first direction, at the intersection of which is a node comprising the at least one target zone.

[0028] The invention also relates to a sealed and thermally insulating tank comprising at least one such corrugated sheet.

[0029] These and other characteristics and advantages of the present invention will appear more clearly from the following description, made with reference to the accompanying drawings, given by way of non-limiting examples, and in which:

[0030] [Fig.lA] is a schematic sectional view of a prior art tank wall;

[0031] [Fig.lB] is a schematic view of another tank wall of the prior art;

[0032] [Fig.2] represents the different zones of a corrugated sheet of the prior art;

[0033] [Fig.3] represents a flowchart of the steps of the manufacturing process according to the invention;

[0034] [Fig.4] represents the detail of a node of a corrugated sheet obtained after the step of deformation of the sheet metal of the manufacturing process according to the invention;

[0035] [Fig.5] schematically represents the heat treatment step in a furnace passage and the cooling step of the manufacturing process according to the invention.

[0036] [Fig.6] represents the detail of the microstructures of a corrugated steel sheet in cold-rolled oxidizable obtained by the manufacturing process according to the invention.

[0037] [Fig.7] represents the detail of the microstructures of a corrugated steel sheet in cold-rolled oxidizable obtained by a process different from the manufacturing process according to the invention.

[0038] [Fig.8] shows results of tests carried out on different samples with and without the manufacturing method according to the invention.

[0039] [Fig.9] is a simplified illustration of a sheet metal deformation.

[0040] For the sake of clarity, the same elements will bear the same references in the different figures.

[0041] In the following, by stainless steel sheet, it is necessary to understand a piece of stainless steel obtained by cold rolling and having the shape of a rectangular parallelepiped and of thin thickness, for example between 0.15 and 5 mm. In addition, the term corrugated also means corrugated, a corrugated sheet is to be understood as a sheet having corrugations or undulations.

[0042] Preferably, in the context of the invention, the stainless steel sheet has a thickness of between 0.5 and 2 mm. Its width is preferably less than or equal to 200 cm and its length is preferably less than or equal to 400 cm. However, other dimensions can be envisaged by adapting the means implemented in carrying out the method of the invention, in particular the size of the furnace as will appear in the remainder of the description of the invention.

[0043] [Fig. 1A] is a schematic sectional view of a prior art tank wall. A sheet metal manufactured by the method of the invention could replace the primary membrane 10. This figure has already been described above.

[0044] [Fig. 1B] is a schematic view of another tank wall of the prior art. A sheet manufactured by the method of the invention could replace the primary membrane 10. This figure has already been described above.

[0045] [Fig. 2] represents the different zones of a corrugated sheet of the prior art. This figure has already been discussed previously.

[0046] [Fig. 3] represents a flowchart of the steps of the manufacturing method according to the invention. The method for manufacturing a cold-rolled stainless steel corrugated sheet according to the invention comprises a step 100 of providing a cold-rolled stainless steel sheet having a composition comprising, the contents being expressed by mass: 0.005% < C < 0.05%, and preferably C < 0.03%; 0.1% <Si<l %; 0.5% < Mn < 2%; 4% < Ni < 10.5%; 16% < Cr < 20%; 0% < N < 0.2%; 0% < P < 0.045%; 0% < S < 0.015%.

[0047] Optionally, the composition of the stainless steel of the sheet provided may comprise molybdenum in a content, expressed by mass, less than or equal to 3% (Mo < 3%) and / or copper in a content, expressed by mass, less than or equal to equal to 0.5% (Cu < 0.5%).

[0048] The remainder of the composition is made up of iron and unavoidable impurities resulting from the production of the steel. The microstructure of this stainless steel is essentially austenitic (in the form of metastable austenite). The average size of the austenite grains, also called primary austenite, is between 6 pm (micrometers) and 35 pm (micrometers).

[0049] The manufacturing method comprises a step 110 of deforming the stainless steel sheet, for example by folding or stamping, to obtain a corrugated sheet comprising corrugations defining target zones having, for a deformation carried out by folding, a geometric deformation rate of between 15% and 45% (preferably less than 35%), or having, for a deformation carried out by stamping, a section reduction rate in the target zones of less than 25%.

[0050] The section reduction rate can be seen as a ratio between the sheet sections before and after deformation. A sheet with an initial section of 5 mm2 which has a section of 4.5 mm2 after deformation (of the stamping type) has a section reduction rate of 10%.

[0051] The geometric deformation rate is a ratio representing the geometric deformation of the sheet metal in a three-dimensional manner. It can be determined by numerical calculation according to equations known to those skilled in the art. Figure 9 is a simplified illustration of a sheet metal deformation. For illustration and in a simplified manner, if we only consider one dimension, a folded sheet metal of thickness Ep (see Figure 9) so that, for a neutral fiber segment length Fn (whose length is noted 10, in thick dotted lines in Figure 9) 10 = 100mm and an outer fiber segment (whose length is noted Id with ~ fQ + , in fine dotted lines in [Fig.9]) of length Id = 110mm, the material along this outer fiber has a deformation rate of 10%, without the thickness Ep of the sheet being modified in the bending.

[0052] The step 110 of deformation of the sheet metal allows the formation of corrugations, or undulations, on the sheet metal. These corrugations 15 are visible in [Fig.4]. These corrugations aim to provide flexibility to the sheet metal with a view to its use for the transport and / or storage of liquefied gas.

[0053] [Fig. 4] represents the detail of a node 13 of a corrugated sheet obtained after the step 110 of deformation of the sheet. In [Fig. 4], after the deformation step, the corrugated sheet has a first corrugation 15 in a first direction and a second corrugation 16 in a second direction substantially perpendicular to the first direction. At the intersection of the first corrugation 15 and the second corrugation 16 is node 13. It comprises target zones 14 having a deformation rate of between 15% and 45%, preferably less than 35%, or a section reduction rate in the target zones of less than 25%. This deformation / reduction rate is inherent to the deformation step and can be determined by calculation methods known to those skilled in the art. These deformation rates lead to the appearance of martensite, in higher content in the target zones 14 of node 13.

[0054] The step 110 of deformation of the sheet generates, in the target zones 14, a change at the microstructural level of the stainless steel. The metastable austenite of the stainless steel, initially present in the form of grains of average size between 6 and 35 micrometers, transforms into a mixture of austenite and martensite. The martensite is present in the form of lamellae of smaller dimensions than that of the primary austenite grains of the steel sheet before deformation.

[0055] The transformation of primary austenite into martensite is partial. After deformation, the ratio between austenite and martensite depends on several factors, and in particular on the initial composition of the stainless steel and the level of deformation / section reduction of the sheet. In other words, for identical deformation, the ratio between austenite and martensite will be different for two stainless steel sheets of different composition. In the same way, for a given initial steel composition, the ratio between austenite and martensite will be different depending on the location of the sheet considered (target zone, wave or flat zone) due to the difference in the rate of deformation / section reduction undergone depending on the location of the sheet.

[0056] The target zones 14 have a geometric deformation rate of between 15% and 45% or a section reduction rate locally in the target zones of less than 25%. Geometric deformation rate is used for target zones obtained following a bending deformation step. Section reduction rate is used for target zones obtained following a stamping deformation step. As mentioned previously, it is these target zones 14 which form a geometrically stressed zone, and therefore present an increased risk of fatigue failure. In the target zones 14, the austenite grains have transformed, at least partially, into martensite lamellae during the deformation step 110.

[0057] The steps of the manufacturing method according to the invention described below make it possible to improve the fatigue resistance of the target zones 14 without deteriorating the mechanical properties of the zones adjacent to the target zones 14.

[0058] The manufacturing method according to the invention comprises, after step 110 of deformation of the sheet, a step 120 of heat treatment of the corrugated sheet comprising the target zones 14, at a temperature and a heat treatment duration defined according to the composition of the stainless steel, to obtain a sheet

[0059]

[0060]

[0061]

[0062] corrugated with recrystallized target areas. The recrystallization of the target areas is explained below. In the context of the invention, the recrystallization temperature is between 700 and 900 °C and the heat treatment time is between 5 seconds and 40 minutes. In the context of the invention, the heat treatment 120 of a part means the heating and maintaining the temperature of said part. More precisely, for a content of stainless steel, expressed in mass, in nickel and nitrogen such that: 4% < Ni < 8% 0.05% < N < 0.2%, the duration of heat treatment 120 is defined according to the heat treatment temperature as follows: temperature duration 700°C 15 to 40 minutes 750°C 5 to 20 minutes 800°C 3 to 8 minutes 850°C 30 seconds to 3 minutes In other words, the duration of the heat treatment is directly related to the heat treatment temperature. For this nickel and nitrogen content of the steel in question, for a temperature of 700°C, the heat treatment duration is between 15 and 40 minutes. For a temperature of 750°C, the heat treatment duration is between 5 and 20 minutes, etc. Furthermore, for a content of stainless steel, expressed in mass, in nickel and nitrogen such that: 8% < Ni < 10.5% 0 <N<0,l%, the duration of heat treatment 120 is defined according to the heat treatment temperature as follows: temperature duration 750°C 4 to 15 minutes 800°C 2 to 8 minutes 850°C 20 seconds to 2 minutes 900°C 5 to 15 seconds

[0063] It will appear more generally to those skilled in the art that various modifications can be made to the embodiments described above, in light of the teaching disclosed to them herein. The invention is defined by ranges of heat treatment duration according to a heat treatment temperature, for example 750°C or 800°C. However, the invention applies in a similar manner for heat treatment temperatures between the indicated limits. For example, for a heat treatment temperature of 775°C (i.e. between the indicated temperatures of 750 and 800°C), those skilled in the art know on the basis of the description of the invention that the duration of the heat treatment will have to be adapted between 4 and 8 minutes.

[0064] During the heat treatment step 120, the martensite lamellae present in the corrugated sheet divide to transform into austenite grains of a size smaller than the size of the martensite lamellae (and therefore much smaller than the initial size of the austenite grains in the steel of the sheet before deformation). In other words, thanks to the heat treatment, the martensite in the target zones is mainly transformed into fine-grained austenite. Typically, the residual martensite content after heat treatment is less than or equal to 4%. These are then referred to as recrystallized target zones. In other words, a target zone is recrystallized as soon as its martensite-type microstructure is transformed into a fine-grained austenite microstructure, called secondary.The production of these austenite nanograins, or more generally the refinement of a microstructure into smaller austenite grains, makes it possible to obtain better performance in terms of the elastic limit of the material. The improvement of this elastic limit has a beneficial effect on the fatigue resistance of the target areas concerned.

[0065] Finally, the manufacturing method according to the invention comprises a step 130 of cooling the corrugated sheet with recrystallized target zones. The step 130 of cooling the corrugated sheet with recrystallized target zones stops the growth of the grains throughout the sheet and aims to freeze the microstructure in the form of austenite nano-grains obtained by the heat treatment 120.

[0066] [Fig.5] schematically represents the heat treatment step in a furnace passage and the cooling step of the manufacturing process according to the invention.

[0067] In an embodiment shown in [Fig. 5], the heat treatment 120 is carried out in a pass-through furnace 20. Advantageously, the heat treatment step 120 and the cooling step 130 take place in an environment that is protective against surface contamination. It may be noted that the heat treatment 120 can alternatively be carried out in a vacuum furnace. These specific environments are intended to prevent the formation of scale or any other contamination on the surface of the corrugated sheet. These surface contaminations are to be avoided to avoid a stripping step (mechanical, chemical or other) after the heat treatment. However, the method according to the invention may also comprise a stripping step after the heat treatment 120, in particular in the case where the heat treatment environment is not protective against surface contamination.

[0068] Advantageously, the manufacturing method according to the invention may further comprise, prior to the heat treatment 120, a step 115 of cleaning the corrugated sheet. The cleaning step 115 aims to eliminate all traces of pollutants present on the corrugated sheet, in particular fatty substances or metal shavings.

[0069] As illustrated in [Fig.5], the corrugated sheet is placed on a movable sole 21, for example a belt or a set of rollers, which passes through the furnace 20 from one side to the other. By setting the sole 21 in motion in the direction 22, the corrugated sheet moves inside 20 in a first zone 23 called the entry zone. The entry zone 23 is a zone without heating. On the other hand, in the case of a controlled environment, the entry zone 23 is under a controlled environment. Thus, without breaking the environment, by translation of the sole in the direction 22, the corrugated sheet is then transferred into a second zone 24 called the heating zone. The heat treatment step 120 takes place in the heating zone 24, a zone in which the corrugated sheet is exposed to the target temperature for an adequate duration.For example, for a corrugated sheet of stainless steel with a content, expressed by mass, of nickel and nitrogen of 6% and 0.15% respectively and a heating zone 24 set at 800°C, the exposure time is between 5 and 10 minutes, for example 8 minutes. For a given temperature and a given composition of the stainless steel of the corrugated sheet, tests were carried out by the Applicant to determine the exposure time ranges mentioned above.

[0070] The speed of advance of the hearth through the passage furnace 20 is calculated as a function of the length of the heating zone 24 in order to obtain the desired exposure time. For example, for a passage furnace having a heating zone 10m long and for an exposure target of 5 minutes at 800°C, the speed of the hearth is fixed at 2m / min.

[0071] Alternatively, depending on the dimensions of the corrugated sheets, a step-by-step advancement of the sole can also be envisaged, to limit the durations during which the corrugated sheet is present simultaneously in two stages.

[0072] Note that in this example, the sole is movable in translation. However, the same principle applies to other types of movement, in particular rotation with a rotary rack furnace, and preferably for parts of small dimensions, for example of the order of 30 cm x 50 cm (or more depending on the size of the furnace). The invention is based on a heat treatment at a predefined temperature and duration in a heating zone.

[0073] At the end of the exposure time in the heating zone 24, the corrugated sheet undergoes rapid cooling, for example hyperquenching type cooling.

[0074] The heat treatment step 120 and / or the cooling step 130 are preferably carried out in an inert or reducing environment in order to avoid the formation of oxide on the surface of the sheet. For the cooling step 130, the quenching fluid is then chosen from fluids that protect against oxidation. In both cases (heat treatment step 120 and cooling step 130), hydrogenated nitrogen, argon, helium, or possibly pure hydrogen may be noted. Alternatively, if the cooling does not take place in an inert or reducing environment, or in addition, the corrugated sheet with recrystallized target zones may be subjected, after the cooling step 130, to a pickling step in order to eliminate any unwanted residue that may be present on the surface of the sheet.

[0075] In the case of the passage furnace 20 illustrated in [Fig. 5], the cooling 130 is carried out by transferring the corrugated sheet with recrystallized target zones into a quenching zone 25 adjacent to the heating zone 24 in the direction 22 of advancement of the hearth.

[0076] Advantageously, the cooling step 130 is carried out very quickly, for example at a speed greater than or equal to 50°C / s.

[0077] The heat treatment 120 and / or the cooling 130 is preferably carried out in an inert or reducing environment for the reasons explained previously.

[0078] In the case of a heat treatment 120 in a vacuum furnace or controlled environment, the cooling 130 is carried out by pressurized injection of the quenching fluid at room temperature.

[0079] In another embodiment, the heat treatment 120 can be carried out by applying local heating means, for example heating bells, to the target areas. For this, the heating bells are positioned on the nodes, matching the shape of the corrugated sheet. It is also possible to envisage induction or convection type heating means, in particular for short-term heat treatments.

[0080] As previously stated, since the heat treatment is carried out on thin sheets (typically between 0.5 and 2 mm thick), it is estimated that the core heating time is close to the skin heating time. Thus, it is considered that the core heating time is low compared to the exposure times defined in the manufacturing method of the invention.

[0081] In the case where the heating means of the heating zone of the oven does not allow a When placing the sheet to be treated in a heating zone already heated to the target temperature (e.g. vacuum furnace), the impact of the temperature rise slope is taken into account by reducing the holding time at the target temperature. This reduction is all the more significant when the heat treatment temperature is high and the temperature rise rate slow. Note that for heat treatment times of less than 5 minutes, a gradual temperature rise to the target temperature is not possible.

[0082] The manufacturing method may also comprise a step 125 of regulating the speed of advance of the sole as a function of the temperature in the heating zone 24 in order to properly control the duration of the heat treatment and possibly take into account the temperature rise slope. For example, for a part of greater thickness, the speed of advance of the sole is regulated so as to be lower than the speed of advance for a part of thinner thickness.

[0083] Thus, the manufacturing method according to the invention is based on a heat treatment optimized according to the chemical composition of the steel of the sheet. The parameters of duration and temperature of the heat treatment are chosen to obtain a satisfactory reversion of martensite to austenite in the target zones of the node, while limiting the growth of primary austenite grains (i.e. in the undeformed zones of the node) and secondary austenite grains (in the deformed zones).

[0084] The manufacturing method of the invention is based on a heat treatment specific to the target zones, zones weakened due to deformation to obtain the corrugations essential to the envisaged application of transport / storage of liquefied gas. The heat treatment of the invention allows the transformation of the martensite present in the target zones into secondary austenite with a smaller grain size. This results in better mechanical properties of the target zones. In other words, the invention takes advantage of the partial transformation at the level of the microstructures of the target zones by means of the martensite formed to obtain, after heat treatment, austenite grains of a size smaller than those of the martensite lamellae and the austenite grains initially present in the stainless steel.

[0085] The corrugated sheet with recrystallized target zones manufactured by the manufacturing method according to the invention can be used as a component in the manufacture of a sealing membrane (primary membrane 10) for the transport and / or storage of liquefied gas at cryogenic temperatures.

[0086] [Fig.6] shows the detail of the microstructures of a corrugated steel sheet in cold-rolled oxidizable sheet obtained by the manufacturing process according to the invention. On this magnification (x 1000), we can see the delimitation of the austenite grains 60 initially present in the cold-rolled stainless steel sheet. These grains have at least partially transformed into martensite, in the form of lamellae 61. With the heat treatment adapted to the manufacturing process according to the invention, the lamellae 61 are transformed into so-called secondary austenite, in the form of fine grains 62, or nano-grains. It is the refinement of the grains 60 of primary austenite into nano-grains 62 of secondary austenite which makes it possible to obtain better mechanical performance by improving the elastic limit of the sheet thus manufactured. The average size of the secondary austenite grains is between 0.2 pm (micrometers) and 2 pm (micrometers), and may even be less than 0.2 pm.

[0087] [Fig. 7] shows the detail of the microstructures of a cold-rolled stainless steel corrugated sheet obtained by a process different from the manufacturing process according to the invention. In this example, the corrugated sheet was subjected to too long a heat treatment, i.e. the duration of which exceeded the heat treatment duration of the process of the invention. In other words, the corrugated sheet whose detail is shown in [Fig. 7] was not obtained with the manufacturing process according to the invention.

[0088] On this magnification (x 500), we can see the delimitation of the austenite grains 60, of dimensions similar to those initially present in the cold-rolled stainless steel sheet. Traces of martensite lamellae 61 are faintly visible. As can be seen, an excessive heat treatment time did not lead to the formation of secondary austenite nano-grains. On the contrary, the heat treatment annealed the material. The microstructure obtained comprises a mixture of primary austenite grains and secondary austenite grains having grown significantly to a size close to that of the primary austenite grains.

[0089] The microstructures presented in Figures 6 and 7 highlight the crucial importance of step 120 of the heat treatment. Indeed, on the one hand, the chemical composition of the steel used must be taken into account, and on the other hand, the duration of the heat treatment must be adapted to the exposure temperature. If the duration of the heat treatment is less than the duration of the process of the invention, a significant proportion of the martensite lamellae does not have time to transform into austenite nano-grains. And if the duration of the heat treatment is greater than the duration of the process of the invention, the material is annealed, the martensite lamellae are transformed back into large austenite grains.

[0090] [Fig.8] shows results of tests carried out on different samples with the manufacturing method according to the invention and without the manufacturing method according to the invention. The abscissa axis represents the number of cycles to failure (N). The ordinate axis represents the cyclic elongation. In this case, the cyclic elongation (Ec) is 0.55 mm. This factor is identical for all the tests presented below. A sample is a portion of cold-rolled corrugated sheet metal deformed according to step 110, comprising a complete node. Each sample was subjected to cyclic elongation, and the number of cycles until the sample ruptured was observed. The rupture can for example result in cracks in the target area.

[0091] Two samples of cold-rolled and then deformed stainless steel sheet (i.e. having undergone the deformation step 110), as illustrated in [Fig.4], were tested with a heat treatment step and a cooling step: - 304L of composition (in mass percentage) as follows: 0.0159% C, 0.57% Si, 1.135% Mn, 0.0243% P, 0.0027% S, 18.272% Cr, 9.310% Ni, 0.116% Cu, 0.039% Mo and 0.0175% N. - 301LN with the following composition (in mass percentage): 0.025% C, 0.52% Si, 1.70% Mn, 0.033% P, 0.003% S, 17.32% Cr, 6.63% Ni, 0.25% Cu and 0.108% N

[0092] These samples underwent various heat treatments in a protective environment. This gives the average service lives at iso-stress (in number of cycles): - 304L without any heat treatment (“Raw 304L”): 155,147 cycles; - 304L with a heat treatment of 800°C for 6 minutes (depending on the process of the invention): 470,467 cycles; - 304L with a heat treatment of 800°C for 10 minutes (beyond the range): 134,400 cycles; - 301LN without heat treatment (“Raw 301LN”): 1,896,400 cycles; - 301LN with a heat treatment of 800°C for 5 minutes (in the range): 2,000,000 cycles without observed breakage (tests stopped at 2,000,000 cycles).

[0093] It may be noted that the numbers of cycles indicated are averages obtained from several tests carried out for a given condition.

[0094] The raw 304L sample constitutes a reference sample, comprising the target zones 14. Its lifetime is 155147 cycles.

[0095] An identical sample was subjected to the process of the invention, with a heat treatment step of 800°C for 6 minutes (sample 304L 800°C / 6 mins). Its lifetime increases to 470467 cycles (i.e. 3 times greater than that of the reference sample).

[0096] An identical sample was subjected to a heat treatment not corresponding to the method of the invention, with a heat treatment step of 800°C for 10 minutes (sample 304L 800°C / 10 mins). Its lifetime increases to 134,400 cycles. In other words, its lifetime decreases compared to the reference sample. Not only does too long a heat treatment not improve the elastic limit of the sample, but it can also have a negative effect on the lifetime of the sample.

[0097] The raw 301LN sample constitutes another reference sample, comprising the target areas 14. Its lifetime is 1,896,400 cycles.

[0098] An identical sample was subjected to the process of the invention, with a heat treatment step of 800°C for 5 minutes (301LN 800°C / 5 mins). Its lifetime is 2,000,000 cycles without crack detection (i.e. at least 1.05 times greater than that of the reference sample).

[0099] Another test was carried out on a higher loading level (“high load level” with a cyclic elongation (Ec) of 0.7 mm) with one test per condition. This resulted in an average service life at iso-stressing (in number of cycles) as follows: - 301LN without heat treatment (“Raw 301LN”): 367,200 cycles; - 301LN with a heat treatment of 750°C for 10 minutes (in the duration range corresponding to the method of the invention): 2,000,000 cycles without observed breakage (tests stopped at 2,000,000 cycles).

[0100] The raw 301LN sample constitutes another reference sample, comprising the target areas 14. Its lifetime at the high load level is 367,200 cycles.

[0101] An identical sample was subjected to the method of the invention, with a heat treatment step of 750°C for 10 minutes (301LN 750°C / 10mins). Its lifetime at the high load level is 2,000,000 cycles without crack detection (i.e. at least 5.44 times greater than that of the reference sample). The tests carried out on different samples with and without the manufacturing method according to the invention clearly show the improvement in the fatigue resistance of the samples tested thanks to the method of the invention. Microscopic observations highlight the effects of the heat treatment on the formation of microstructures, and therefore on the resulting elastic limit performances.

[0102] The invention also relates to a cold-rolled corrugated stainless steel sheet having a composition comprising, the contents being expressed by mass: - 0.005% < C < 0.05%, and preferably C < 0.03%; 0.1% <Si<l%; 0.5% < Mn < 2%; 4% < Ni < 10.5%; 16% < Cr < 20%; 0% < N < 0.2%; 0% < P < 0.045%; 0% < S < 0.015%; said corrugated sheet comprising corrugations defining at least one target zone 14 having a geometric deformation rate of between 15% and 45%, preferably less than 35%, or a section reduction rate in the target zones less than 25%, and in which the at least one target zone is recrystallized.

[0103] Advantageously, the corrugated sheet has a first corrugation 15 in a first direction and a second corrugation 16 in a second direction, substantially perpendicular to the first direction 15, at the intersection of which is a node 13 comprising the at least one target zone 14.

[0104] The invention also relates to a sealed and thermally insulating tank comprising at least one such corrugated sheet.

[0105] It will more generally appear to those skilled in the art that various modifications can be made to the embodiments described above, in light of the teaching which has just been disclosed to them. In the following claims, the terms used should not be interpreted as limiting the claims to the embodiments set out in the present description, but should be interpreted to include all equivalents which the claims are intended to cover by virtue of their wording and the prediction of which is within the reach of those skilled in the art based on their general knowledge.

Claims

Claims

1. A method of manufacturing a cold-rolled stainless steel corrugated sheet, comprising the following steps: - Supply (100) of a cold-rolled stainless steel sheet having a composition comprising, the contents being expressed by mass: 0.005% < C < 0.05%, and preferably C < 0.03%; 0.1% <Si<l%; 0.5% < Mn < 2%; 4% < Ni < 10.5%; 16% < Cr < 20%; 0% < N < 0.2%; 0% < P < 0.045%; 0% < S < 0.015%; the remainder being iron and residual elements resulting from the elaboration; - Deformation (110) of the stainless steel sheet, to obtain a corrugated sheet comprising target zones having a geometric deformation rate of between 15% and 45%, preferably less than 35%, or a section reduction rate in the target zones of less than 25%; - Heat treatment (120) of the target areas of the corrugated sheet at a temperature and heat treatment duration defined according to the composition of the stainless steel, to obtain a corrugated sheet with recrystallized target areas; - Cooling (130) of the corrugated sheet with recrystallized target zones, the manufacturing process being characterized in that, for a content of stainless steel, expressed by mass, in nickel and nitrogen such that: 4% < Ni < 8% 0.05% < N < 0.2% the duration of the heat treatment (120) is defined according to the temperature heat treatment: temperature duration 700°C 15 to 40 minutes 750°C 5 to 20 minutes 800°C 3 to 8 minutes 850°C 30 seconds to 3 minutes and, for a content of stainless steel, expressed in mass, in nickel and nitrogen such that: 8% < Ni < 10.5% 0 <N<0,l% the duration of the heat treatment (120) is defined according to the temperature of the heat treatment: temperature duration 750°C 4 to 15 minutes 800°C 2 to 8 minutes 850°C 20 seconds to 2 minutes 900°C 5 to 15 seconds

2.

3.

4.

5.

6. Manufacturing method according to claim 1, wherein the cooling (130) of the corrugated sheet with recrystallized target zones is carried out at a speed greater than or equal to 50°C / s. Manufacturing method according to any one of claims 1 or 2, wherein the heat treatment (120) is carried out in a pass-through furnace. Manufacturing method according to any one of claims 1 to 3, wherein the heat treatment (120) and / or the cooling (130) is carried out in an inert or reducing environment. Manufacturing method according to any one of claims 1 or 2, wherein the heat treatment (120) is carried out in a vacuum furnace. Manufacturing method according to any one of claims 1 or 2, wherein the heat treatment (120) is carried out by applying heating bells to the target areas.

7. Manufacturing method according to any one of claims 1 to 6, wherein the cooling (130) of the corrugated sheet with recrystallized target zones is carried out by quenching in a quenching fluid.

8. Manufacturing method according to any one of claims 1 to 6, in which the cooling (130) of the corrugated sheet with recrystallized target zones is carried out by injection under pressure of a quenching fluid, preferably at room temperature.

9. Manufacturing method according to any one of claims 1 to 8, further comprising, prior to the heat treatment (120), a step (115) of cleaning the corrugated sheet.

10. Corrugated sheet of cold-rolled stainless steel having a composition comprising, the contents being expressed by mass: 0.005% < C < 0.05%, and preferably C < 0.03%; 0.1% < Si < 1%; 0.5% < Mn < 2%; 4% < Ni < 10.5%; 16% < Cr < 20%; 0% < N < 0.2%; 0% < P < 0.045%; 0% < S < 0.015%; the remainder being iron and residual elements resulting from the production; said corrugated sheet comprising corrugations defining at least one target zone (14) having a geometric deformation rate of between 15% and 45%, preferably less than 35%, or a section reduction rate in the target zones of less than 25%, and in which the at least one target zone is recrystallized.

11. Corrugated sheet according to claim 10, in which the corrugated sheet has a first corrugation (15) in a first direction and a second corrugation (16) in a second direction, substantially perpendicular to the first direction (15), at the intersection of which is a node (13) comprising the at least one target zone (14).

12. A sealed and thermally insulating tank comprising at least one corrugated sheet according to any one of claims 10 or 11.