ELECTROCHROME GLAZING

The conductive coating structure with a silver-based metallic layer and blocking layers like nickel or titanium nitride enhances electrochemical stability, addressing the stability issues of silver-based coatings in electrochromic devices, enabling effective optical modulation and durability.

FR3140955B1Active Publication Date: 2024-10-18SAINT GOBAIN VITRAGE SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2022010517
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-10-13
Publication Date
2024-10-18
Estimated Expiration
2042-10-13

AI Technical Summary

Technical Problem

Silver-based conductive coatings in electrochromic devices suffer from low electrochemical stability, limiting their use due to redox reactions and corrosion, especially in the 1V-4V range, which affects the optical contrast and durability of the devices.

Method used

A conductive coating structure comprising a silver-based metallic functional layer with a blocking layer, such as nickel or titanium nitride, and a thick conductive oxide layer, enhances electrochemical stability, allowing operation up to 3.7V vs Li/Li+, maintaining high conductivity and transparency.

Benefits of technology

The improved electrochemical stability enables the use of silver-based coatings in electrochromic devices, providing high electrical conductivity and optical adjustability, suitable for applications requiring broad voltage ranges without degradation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000021_0000
    Figure 00000021_0000
  • Figure 00000022_0000
    Figure 00000022_0000
Patent Text Reader

Abstract

The invention relates to a material comprising a substrate coated with a first conductive coating comprising, starting from the substrate: - a first dielectric coating, - a silver-based metallic functional layer, - a blocking layer located above and immediately in contact with a silver-based metallic functional layer, chosen from metallic layers of one or more elements chosen from nickel and chromium such as Ni, Cr, NiCr, and metallic nitride layers of one or more elements chosen from titanium, nickel, chromium such as NiN, CrN, NiCrN, TiN, - a second dielectric coating comprising at least one conductive oxide layer the sum of the thicknesses of the conductive oxide layers of which is greater than 40 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: ELECTROCHROME GLAZING

[0001] The present invention relates to the field of electrochromic (EC) glazing. The invention relates in particular to an electroconductive coating for an electrochromic device comprising a silver-based metallic functional layer having improved electrochemical properties.

[0002] Electrochromic devices, and in particular electrochromic glazing, are systems capable of modulating their optical response, in the visible or in the infrared, under the action of an electrical voltage, thus making it possible to obtain electrically controlled coatings that are easily adjustable.

[0003] Electrochromic devices include, in a known manner, an electrochromic system comprising a succession of at least five layered elements essential to the operation of the device, that is, to the reversible color change following the application of an appropriate electrical supply. These five layered elements are as follows: - a first transparent electroconductive coating, - a first active layer acting as an electrode, - a layer of electrolyte, - a second active layer acting as a counter electrode, and - a second transparent electroconductive coating. At least one active layer is based on an electrochromic material. These five layered elements are generally in contact with one or two transparent substrate(s).

[0004] Electrochromic systems fall into three categories: - the inorganic technology known as "all-solid", - the so-called "hybrid" technology, - the so-called "all-polymer" technology.

[0005] In all-solid electrochromic systems, all layers are made of inorganic solid materials. These systems may comprise a single substrate. Examples of all-solid EC systems are described in patent applications EP-867 752, EP-831 360, WO 00 / 57243 and WO 00 / 71777.

[0006] Hybrid electrochromic systems comprise inorganic active layers framing an electrolyte layer based on an ionically conductive polymer. These systems traditionally comprise two substrates framing the electrochromic system. Examples of hybrid EC systems are described in patent applications EP-382,623, EP-518,754, and EP-532,408.

[0007] In "all-polymer" electrochromic systems, the active layers and the layer electrolytes are polymer-based.

[0008] The phenomenon of colouring / decolouring in the visible range or of modifications of optical properties in general, results from a transfer of charge (ions / electrons) between the two active layers.

[0009] An active layer based on an electrochromic material is capable of reversibly inserting ions. When the ions migrate to this layer, its optical properties change, and it reversibly transitions from a colorless state to a colored state. The other active layer may also be based on an electrochromic material.

[0010] Inorganic electrochromic materials are predominantly transition metal oxides, grouped into two families: cathodic color-changing oxides, such as tungsten oxide (WO3), which exhibit color in the reduced state, and anodic color-changing oxides, such as iridium oxide (IrOx) and nickel oxide (NiOx), which are colored in the oxidized state. Pairs of cathodic and anodic electrochromic materials are generally chosen, for example, a cathodic material that colors in the inserted state in association with an anodic material that is colorless in the inserted state.

[0011] The electrolyte layer must exhibit good ionic conductivity and be electronically insulating. The electrolytes of the electrochromic system ensure the passage of mobile ions within their electrochemical stability range. In theory, all monovalent ions, such as H+, Li+, Na+, K+, Ag+, divalent ions such as Zn2+, and trivalent ions such as Al3+ can be used. Lithium, alkali, or hydrogen salts are particularly suitable.

[0012] By way of example, for an active layer of tungsten oxide (WO3) in contact with a lithium ion-conducting electrolyte layer, there is a transfer of Li+ ions between the electrodes when a voltage is applied. The following electrochemical reaction is observed at the cathode: W6 + O2 3 (transparent) + x Li+ + xe → LUW^isW^ XO2 3 (blue).

[0013] The voltage ranges that provide the best contrast between the colored and decolorized states can be determined by voltammetry. Voltammetric cycles or curves, or voltamgrams (j = f(V)), consist of tracking the variation of the current density j over the swept potential range. The study of current density variations is significant in understanding the electrochemical behavior of materials. The color potentials (Vcoloration) and decolorization potentials (Vdecoloration) of the material, corresponding to oxidation reactions in the anodic part (j > 0) or reduction reactions in the cathodic part of the curve (j < 0), as well as the stability ranges, can be directly deduced from these curves.

[0014] If we consider an electrochromic device comprising an active layer with co cathodic loration based on tungsten oxide and an electrolyte layer including lithium ions, a coloured state is observed at 2.3 V and a colourless state at 3.2 V (vs Li / Li+).

[0015] If we consider an electrochromic device comprising an active layer with anodic coloring based on nickel oxide and an electrolyte layer comprising lithium ions, the oxidation potential associated with the disinsertion of lithium ions is approximately 4 V while the decolorization voltage can be adjusted by doping the nickel oxide between IV and 2.5 V.

[0016] If we consider the known all-polymer EC systems comprising an electrolyte layer comprising lithium ions, the voltage range between a less transparent state and a more transparent state is between 2V and 4V vs Li / Li+.

[0017] Therefore, for these EC systems, the reactions enabling coloring and decolorization occur within a potential window between IV and 4V. The materials constituting the various layer elements of the electrochromic system must have electrochemical stability ranges exceeding the potential windows required to obtain the coloring / decolorizing phenomena.

[0018] The term "voltage stability range" of a material means the potential range to which a material can be exposed without undergoing an oxidation or reduction reaction.

[0019] When a material is subjected to an electrochemical potential outside its stability range and in the presence of the corresponding ions, an oxidation-reduction reaction occurs.

[0020] In the case of electrochromic systems, the electroconductive coatings are exposed to the electrochemical potentials of the active materials with which they are in contact. This means that the electroconductive coatings of the electrochromic device must be stable in the potential range of 2 V to 4 V, or even from IV to 4 V, with respect to Li / Li+. The electroconductive coatings must therefore exhibit an electrochemical stability range relative to the Li+ / Li couple preferably between IV and 4 V. The constituent materials of these conductive coatings must not undergo redox reactions within this voltage range.

[0021] Known electroconductive coatings include conductive functional layers based on transparent conductive oxide such as indium and tin layers or fluorine-doped tin layers or metallic functional layers, particularly silver-based.

[0022] Electroconductive coatings based on a conductive oxide layer, although exhibiting excellent electrochemical stability, do not possess sufficient conductive properties at high light transmission (>80%). This results in inhomogeneous switching and / or a switching speed that decreases when the The surface area of ​​the EC system increases. Finally, in certain applications, such as automotive applications, additional processing steps like quenching or bending are sometimes necessary. These additional steps can alter conductive oxide-based coatings. Indeed, these coatings must be thick to achieve the desired resistivity values. However, these thick coatings are susceptible to cracking during heat treatment.

[0023] Conductive coatings comprising a silver-based metallic functional layer exhibit superior electrical conductivity and high transparency. However, the low electrochemical stability of the silver functional layer limits the use of this type of conductive coating in electrochromic devices. Silver-based conductive coatings undergo redox reactions with respect to the Li / Li+ couple in the 1V-4V range. At low potentials, these reactions lead to the reduction of the Ag material, the formation of a metallic alloy (such as LiAg), or the production of reduced gas (dihydrogen) for a silver-based layer. At high potentials, these reactions lead to the oxidation of the Ag+ material, the formation of an oxide (AgO), and / or the production of oxidized gas (dioxygen). In the context of high-potential reactions, one can also speak of "corrosion" of the materials.

[0024] Known electroconductive coatings of this type include: - possibly a first dielectric layer or first dielectric coating, - a silver-based metallic layer, - possibly a blocking layer, - a second dielectric layer or dielectric coating.

[0025] Cyclic voltamograms were performed to determine the voltage stability range of these electroconductive coatings using a three-electrode setup with a metallic lithium counter electrode, a metallic lithium reference electrode, and a working electrode comprising the electroconductive coating to be tested. The electrolyte is a LiClO4 / PC solution. The working electrode comprises a 2 mm glass substrate coated with a known silver-based electroconductive coating consisting, from the substrate, of the sequence (SiN / SnZnO / ZnO doped Al / Ag). The voltamogram was performed in the potential range of 2 to 4 V relative to Li / Li+ at a sweep rate of 2 mV / s.

[0026] No oxidation reaction is observed between 2 V and 3.4 V. A slight increase in current density is observed around 3.4 V vs. Li / Li+, followed by a sharp increase around 3.7 V vs. Li / Li+. This sharp increase is attributable to The oxidation of metallic Ag to Ag+ ions, which dissolve in the electrolyte, demonstrates that such conductive coatings cannot be used in electrochromic devices except by limiting the accessible contrast of the EC device by imposing potentials below 3.7 V. In this case, no complete decolorization or coloring is achieved.

[0027] In order to be able to benefit in electrochromic devices from the improved optical and conductive properties of silver-based electroconductive coatings, it is necessary to expand their electrochemical stability range.

[0028] The present invention relates to an electroconductive coating comprising a silver-based metallic functional layer exhibiting improved electrochemical stability. The coating of the invention is particularly suitable for use in electrochromic devices.

[0029] The applicant has discovered that the use of certain blocking layers in combination with a thick conductive oxide layer results in improved electrochemical stability, particularly around 3.7V vs. Li / Li+. This improved electrochemical stability makes the agent-based conductive coating suitable for EC applications.

[0030] The invention relates to a material comprising a substrate coated with a first conductive coating comprising, starting from the substrate:

[0031] - a first dielectric coating,

[0032] - a silver-based metallic functional layer, - a blocking layer located above and immediately in contact with a functional silver-based metallic layer, selected from metallic layers of one or more elements selected from nickel and chromium such as Ni, Cr, NiCr, and metallic nitride layers of one or more elements selected from titanium, nickel, chromium such as NiN, CrN, NiCrN, TiN,

[0033] - a second dielectric coating comprising at least one oxide layer conductor whose sum of the thicknesses of the conductive oxide layers is greater than 40 nm, preferably 50 nm.

[0034] The invention makes it possible to increase the stability range of the silver-based electroconductive coating above 3.7 V compared to Li / Li+.

[0035] The invention also relates to a conductive coating comprising a silver-based metallic functional layer, preferably transparent, electrochemically stable in the 2 to 4 V potential window relative to Li / Li+. The conductive coating comprises:

[0036] - a silver-based metallic functional layer, - a blocking layer located above and immediately in contact with a functional silver-based metallic layer, selected from the metallic layers of one or several elements chosen from nickel and chromium such as Ni, Cr, NiCr, and metallic nitride layers of one or more elements chosen from titanium, nickel, chromium such as NiN, CrN, NiCrN, TiN.

[0037] Thanks to this particular coating structure, it is possible to obtain a transparent conductive coating exhibiting electrochemical stability compatible with EC systems while having high electrical conductivity properties.

[0038] The invention also relates to a material having the following characteristic(s): - the blocking layer has a thickness between 0.1 and 5.0 nm, - the blocking layer is chosen from a titanium nitride layer, metallic layers based on nickel and / or chromium, - the blocking layer is chosen from nickel-based metallic layers comprising at least 20% nickel by mass relative to the mass of the nickel-based metallic layer, - the second dielectric coating comprises a conductive oxide layer selected from mixed tin and indium oxide or zinc oxide doped with aluminum and / or gallium, - the second dielectric coating comprises a conductive oxide layer based on aluminum-doped zinc oxide with a thickness greater than 50 nm, - the first dielectric coating comprises at least one crystalline dielectric layer, notably based on zinc oxide, possibly doped with at least one other element, such as aluminium, - the first dielectric coating comprises a layer based on aluminum and / or zirconium silicon nitride or oxynitride, and / or a layer based on zinc and tin oxide, - the substrate is made of glass, particularly soda-lime silico-glass, or of polymeric organic matter, - the material further comprises a first active layer comprising an electrochromic material located in contact with the electroconductive coating, - the material further comprises an electrolyte layer located in contact with the first active layer comprising an electrochromic material, preferably the electrolyte is a lithium ionic conduction electrolyte, - the material further comprises a second active layer located in contact with the electrolyte layer, - the material further comprises a second electroconductive coating located in contact with the electrolyte layer.

[0039] The invention also relates to an electrochromic system comprising: - a material according to the invention, - a first active layer comprising an electrochromic material, - an electrolyte layer, - a second active layer and - a second transparent electroconductive coating, - possibly a substrate.

[0040] The electrochromic material of the active layers may be based on a mineral material such as tungsten oxide, nickel oxide, iridium oxide, cerium oxide, or on an organic material such as electronically conductive polymers like polyaniline or poly(3,4-ethylenedioxythiophene) (PEDOT) or Prussian blue. These materials may incorporate cations, in particular protons or lithium ions.

[0041] The electrochromic material of the first active layer may be based on an oxide of an element selected from tungsten, nickel, iridium, chromium, iron, cobalt, rhodium, or on a mixed oxide of at least two of these elements, in particular a mixed oxide of nickel and tungsten. It is preferably based on tungsten oxide.

[0042] The electrochromic material of the second active layer or counter electrode is preferably based on an oxide of an element selected from tungsten, nickel, iridium, chromium, iron, cobalt, rhodium, or on a mixed oxide of at least two of these elements, in particular a mixed oxide of nickel and tungsten. It is preferably based on nickel oxide or iridium oxide (anodic electrochromic material).

[0043] If the electrochromic material of the first active layer is tungsten oxide, i.e., a cathodic electrochromic material whose colored state corresponds to the most reduced state, an anodic electrochromic material based on nickel or iridium oxide can, for example, be used for the counter electrode. This could, in particular, be a layer of mixed vanadium and tungsten oxide or mixed nickel and tungsten oxide.

[0044] The thickness of the active layers is generally between 50 nm and 600 nm, in particular between 150 nm and 250 nm.

[0045] The thickness of the electrolyte layer can be between 1 nm and 1 mm. When the electrolyte layer is made of an inorganic material, its thickness is preferably between 1 and 300 nm, between 1 and 50 nm, or between 1 and 10 nm. When the electrolyte layer is made of a polymeric material, its thickness is preferably between 100 and 800 pm or between 100 and 500 pm.

[0046] The two electroconductive coatings must be connected to respective power supply connectors. These connectors, for example bus bar and wires, are respectively brought into contact with the transparent conductive coatings to supply the appropriate power supply.

[0047] The invention also relates to an electrochromic system comprising two substrates joined together by means of a chassis or frame.

[0048] Throughout this description, the substrate according to the invention is considered to be horizontally positioned. The electroconductive coating is deposited on top of the substrate. The meanings of the terms "above" and "below," and "lower" and "upper," are to be understood with respect to this orientation. Unless otherwise specified, the terms "above" and "below" do not necessarily mean that two layers and / or coatings are in contact with each other. When it is specified that a layer is deposited "in contact" with another layer or coating, this means that there cannot be one (or more) layer(s) interposed between these two layers (or layer and coating).

[0049] All the luminous characteristics described are obtained according to the principles and methods of the European standard EN 410 relating to the determination of the luminous and solar characteristics of glazing used in glass for construction.

[0050] The preferred characteristics that appear in the following description are applicable both to the material according to the invention and, where applicable, to the glazing or system according to the invention.

[0051] The electroconductive coating is deposited by magnetic field-assisted sputtering (magnetron process). According to this advantageous embodiment, all layers of the coating are deposited by magnetic field-assisted sputtering.

[0052] Unless otherwise stated, the thicknesses referred to in this document are physical thicknesses.

[0053] The present invention is suitable for single-layer functional silver-based coatings. The solution of the invention is also suitable for multi-layer functional silver-based coatings, in particular two- or three-layer functional coatings. The coating comprises at least one or a single functional silver-based metallic layer.

[0054] The silver-based functional metallic layer, before or after heat treatment, comprises at least 95.0%, preferably at least 96.5% and better still at least 98.0% by mass of silver relative to the mass of the functional layer.

[0055] Preferably, the silver-based functional metal layer before heat treatment comprises less than 1.0% by mass of metals other than silver relative to the mass of the silver-based functional metal layer.

[0056] The term "metallic layer" means a layer comprising no more than 30%, 20% or 10% oxygen and / or nitrogen as an atomic percentage in the layer.

[0057] The blocking layers are intended to improve the electrochemical properties of the silver layers.

[0058] When these blocking layers are deposited in metallic or nitrided form, these layers can undergo partial or total oxidation depending on their thickness and the nature of the layers surrounding them, for example, at the time of deposition of the next layer or by oxidation in contact with the underlying layer.

[0059] Advantageously, the blocking layers are nickel-based metallic layers. The nickel-based metallic blocking layers may comprise, (before heat treatment), at least 20%, at least 30%, at least 40%, at least 50%, at least 60%, at least 70%, at least 80%, at least 90%, at least 95%, at least 96%, at least 97%, at least 98%, at least 99% or 100% by mass of nickel relative to the mass of the nickel-based metallic layer.

[0060] Nickel-based metallic layers can be selected from: - the metallic nickel layers, - doped nickel metallic layers, - metallic layers based on nickel alloy.

[0061] Nickel alloy-based metallic layers can be nickel and chromium alloy-based.

[0062] The blocking layers can also advantageously be titanium nitride layers.

[0063] Each blocking layer has a thickness between 0.1 and 5.0 nm. The thickness of these blocking layers can be: - of at least 0.1 nm, of at least 0.2 nm, of at least 0.5 nm and / or - at most 5.0 nm, at most 4.0 nm, at most 3.0 nm, at most 2.0 nm.

[0064] The electroconductive coating comprises at least one functional layer and at least two dielectric coatings comprising at least one dielectric layer, such that each functional layer is disposed between two dielectric coatings.

[0065] For the purposes of this invention, "dielectric coating" means that there may be a single layer or several layers of different materials within the coating. A "dielectric coating" according to the invention comprises primarily dielectric layers. However, according to the invention, these coatings may also comprise layers of other types, in particular absorbent layers, for example, metallic layers.

[0066] A "same" dielectric coating is considered to be located: - between the substrate and the first functional layer, - between each silver-based functional metallic layer, - above the last functional layer (the one furthest from the substrate).

[0067] For the purposes of this invention, "dielectric layer" means that, from the point of view of its nature, the material is "non-metallic", that is to say, it is not a metal. In the context of the invention, this term refers to a material having an n / k ratio over the entire visible wavelength range (from 380 nm to 780 nm) equal to or greater than 5. n denotes the real refractive index of the material at a given wavelength and k represents the imaginary part of the refractive index at a given wavelength; the n / k ratio being calculated at a given wavelength identical for n and for k.

[0068] The thickness of a dielectric coating corresponds to the sum of the thicknesses of the layers constituting it.

[0069] The coatings have a thickness greater than 15 nm, preferably between 15 and 200 nm.

[0070] The dielectric layers of the coatings have the following characteristics, alone or in combination: - They are deposited by magnetic field-assisted sputtering, - They are chosen from oxides or nitrides of one or more elements chosen from titanium, silicon, aluminum, zirconium, tin, indium and zinc, - they have a thickness greater than 2 nm, preferably between 2 and 100 nm.

[0071] The dielectric coating located above the silver-based metallic functional layer must be sufficiently conductive so that the electroconductive coating retains its electrode function.

[0072] The dielectric coating located above the silver-based metallic functional layer comprises at least one conductive oxide layer. The conductive oxide layers are selected from indium oxide, mixed tin and indium oxide, tin-doped indium oxide (ITO “Indium Tin Oxide”), tin oxide, doped tin oxide, zinc oxide, doped zinc oxide such as zinc oxide doped in particular with aluminium (AZO) and / or gallium, ruthenium oxide, doped ruthenium oxide and fluorine-doped tin oxide (SnO2:F).

[0073] Preferably, mixed tin and indium oxide (ITO) or zinc oxide doped with aluminium and / or gallium is used.

[0074] The sum of the thicknesses of all the conductive oxide layers located in the dielectric coating directly above the silver-based functional layer is greater than 50 nm or greater than 60 nm.

[0075] The sum of the thicknesses of all the conductive oxide layers located in the dielectric coating directly above the silver-based functional layer is less than 150 nm, less than 100 nm or less than 80 nm.

[0076] Preferably, the dielectric coating located directly above the silver-based functional layer comprises at least one conductive oxide layer with a thickness greater than 50 nm or 60 nm.

[0077] Preferably, the dielectric coating located directly above the silver-based functional layer comprises at least one conductive oxide layer based on aluminum-doped zinc oxide with a thickness greater than 50 nm or 60 nm. The combination of a blocking layer according to the invention with a thick conductive oxide layer based on doped zinc oxide gives the best results in terms of electrochemical stability.

[0078] According to one embodiment, the dielectric coating may comprise at least two layers, an aluminum-doped zinc oxide layer and a mixed indium tin oxide (ITO) layer.

[0079] According to the invention, indium tin oxide (or tin-doped indium oxide, or ITO) is understood to be a mixed oxide or mixture obtained from indium(III) (In₂O₃) and tin(IV) (SnO₂) oxides, preferably in mass proportions of between 70 and 95% for the former and 5 to 20% for the latter. A typical mass proportion is approximately 90% In₂O₃ to approximately 10% SnO₂.

[0080] According to the invention, the conductive zinc oxide-based layers may comprise at least 50%, at least 60%, at least 70%, at least 80%, at least 90%, or at least 95% by mass of zinc relative to the total mass of all the elements constituting the zinc oxide-based layer, excluding oxygen and nitrogen. To be sufficiently conductive, the zinc oxide-based layers are doped with at least one other element, referred to as the "dopant element." The zinc oxide-based layers may therefore comprise one or more dopant elements selected from aluminum, titanium, niobium, zirconium, magnesium, copper, silver, gold, silicon, molybdenum, nickel, chromium, platinum, indium, tin, and hafnium, preferably aluminum.

[0081] Conductive layers based on doped zinc oxide may include: - at least 1%, at least 2% or at least 5%, and / or - at most 15% or at most 10%, in mass of doping elements relative to the total mass of all elements constituting the zinc oxide-based layer excluding oxygen and nitrogen.

[0082] The dielectric coating located beneath the silver-based metallic functional layer need not necessarily be conductive. Advantageously, it may comprise a crystalline layer, also called a stabilizing or wetting layer. A stabilizing layer is defined as a layer made of a material capable of stabilizing the interface with the functional layer. These layers are generally zinc oxide-based.

[0083] The zinc oxide-based layers may comprise at least 50%, at least 60%, at least 70%, at least 80%, at least 90%, at least 95%, at least 96% at least 97%, at least 98%, at least 99% or 100% by mass of zinc relative to the total mass of all elements constituting the zinc oxide-based layer excluding oxygen and nitrogen.

[0084] To be properly crystallized by sputtering deposition, zinc oxide-based layers advantageously comprise at least 80%, or even at least 90% by mass of zinc relative to the total mass of all the elements constituting the zinc oxide-based layer, excluding oxygen and nitrogen.

[0085] Zinc oxide-based layers may comprise one or more elements selected from aluminium, titanium, niobium, zirconium, magnesium, copper, silver, gold, silicon, molybdenum, nickel, chromium, platinum, indium, tin and hafnium, preferably aluminium.

[0086] Zinc oxide-based layers can optionally be doped with at least one other element, such as aluminium.

[0087] The zinc oxide-based layer comprises, in order of increasing preference, at least 80%, at least 90%, at least 95%, at least 98%, at least 100%, by mass of oxygen relative to the total mass of oxygen and nitrogen.

[0088] Preferably, the dielectric coating located directly below the functional silver-based metallic layer comprises at least one crystalline dielectric layer, in particular based on zinc oxide, optionally doped with at least one other element, such as aluminum.

[0089] These zinc oxide layers have a thickness: - of at least 1.0 nm, of at least 2.0 nm, of at least 3.0 nm, of at least 4.0 nm, of at least 5.0 nm, and / or - at most 25 nm, at most 10 nm, at most 8.0 nm.

[0090] Preferably, the dielectric coating located directly below the silver-based functional metal layer comprises at least one barrier dielectric layer. A barrier dielectric layer (hereinafter referred to as a barrier layer) is defined as a layer made of a material capable of blocking the diffusion of oxygen and water at high temperatures from the ambient atmosphere or the transparent substrate to the functional layer. Such dielectric layers are selected from the following: - based on silicon and / or aluminum and / or zirconium compounds selected from oxides such as SiO2, nitrides such as silicon nitride Si3N4 and aluminum nitrides AIN, and oxynitrides SiOxNy, possibly doped with at least one other element, - based on zinc and tin oxide, - based on titanium oxide.

[0091] Preferably, the first dielectric coating comprises at least one di electric base: - of an aluminium and / or silicon and / or zirconium nitride or oxynitride or - of a mixed zinc and tin oxide, or - of a titanium oxide.

[0092] Preferably, the first dielectric coating comprises: - a layer based on an aluminum nitride or oxynitride and / or silicon and / or zirconium, and / or - a layer based on a mixed zinc and tin oxide, and / or - a layer based on an aluminium and / or silicon and / or zirconium nitride or oxynitride and a dielectric layer based on a mixed zinc and tin oxide located above, preferably in contact with, the layer based on an aluminium and / or silicon and / or zirconium nitride or oxynitride.

[0093] The zinc and tin oxide-based layer is located below, preferably in contact with, the zinc oxide-based layer.

[0094] These dielectric barrier layers have, in increasing order of preference, a thickness: - less than or equal to 40 nm, less than or equal to 30 nm, less than or equal to 25 nm, and / or - greater than or equal to 5 nm, greater than or equal to 10 nm or greater than or equal to 15 nm.

[0095] The substrate coated with the electroconductive coating, or the coating alone, may not have undergone heat treatment. The present invention relates to the unheat-treated material or the heat-treated material.

[0096] The electroconductive coating may not have undergone heat treatment at a temperature above 500 °C, preferably 300 °C.

[0097] The coating may have undergone heat treatment at a temperature above 300 °C, preferably 500 °C. In this case, the heat treatments are selected from annealing, for example by rapid thermal annealing such as laser or flash lamp annealing, quenching, and / or bending. Rapid thermal annealing is described, for example, in application WO2008 / 096089. The heat treatment temperature (at the coating) is above 300 °C, preferably above 400 °C, and even better above 500 °C.

[0098] The substrate coated with the coating can be curved or tempered glass.

[0099] The transparent substrates according to the invention are preferably made of a rigid mineral material, such as glass, or organic polymer-based (or polymer).

[0100] The transparent organic substrates according to the invention may also be made of polymer, rigid or flexible. Examples of suitable polymers according to the invention include, in particular: - polyethylene, - polyesters such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN); - polyacrylates such as polymethyl methacrylate (PMMA); - polycarbonates; - polyurethanes; - polyamides; - polyimides; - fluorinated polymers such as fluoroesters like ethylene tetrafluoroethylene (ETFE), polyvinylidene fluoride (PVDF), polychlorotrifluoroethylene (PCTFE), ethylene chlorotrifluoroethylene (ECTFE), fluorinated ethylene-propylene copolymers (FEP); - photocurable and / or photopolymerizable resins, such as thiolene, polyurethane, urethane-acrylate, polyester-acrylate resins and - polythiourethanes.

[0101] The substrate is preferably a sheet of glass or glass-ceramic.

[0102] The substrate is preferably transparent, colorless (in which case it is clear glass or extra clear) or colored, for example in blue, gray or bronze. The glass is preferably of the soda-lime silicate type, but it can also be of the borosilicate or aluminoborosilicate type.

[0103] According to a preferred embodiment, the substrate is made of glass, in particular soda-lime silico-glass or of polymeric organic matter.

[0104] The substrate advantageously has at least a dimension greater than or equal to 1 m, or even 2 m and even 3 m.

[0105] The substrate thickness generally varies between 0.05 mm and 19 mm. When the substrate is mineral, its thickness is preferably between 0.7 and 9 mm, particularly between 2 and 8 mm, or even between 4 and 6 mm. The substrate may be flat or convex, or even flexible. When the substrate is organic, its thickness is preferably between 1 and 2 mm. Examples I. Electroconductive Coatings

[0106] Electroconductive coatings were deposited by sputtering onto a transparent glass substrate. The glass substrates are 2.1 mm thick aluminosilicate glass substrates. Functional layers (F) are silver-based metallic layers. Dielectric coatings include: - silicon nitride-based layers, - layers based on zinc and tin oxide, - layers of aluminum-doped zinc, - layers of indium and tin. The blocking layers are chosen from titanium, titanium nitride, nickel and chromium, and zinc layers. The conditions for the deposition of the layers, which were deposited by sputtering (so-called "magnetron cathode sputtering"), are summarized in Table 1.

[0107] [Tables] Target Layer Used Pressure Pa Gas ITO In2O3 90%, SnO2 10% wt. 0.2 Ar / (Ar + O2) at 99% Zn Zn 0.2 Ar at 100% NiCr Ni:Cr at 80%:20% by wt. 0.2 Ar at 100% TiN Ti 0.1 to 1 Ar 85% - N2 15% Ti Ti 0.1 to 1 Ar at 100% Ag Ag 0.1 to 1 Ar at 100% SnZnO Zn:Sn at 64:36% at. 0.1 to 1 Ar / (Ar + O2) at 50% Si3N4 Si:Al at 92:8% by wt. 0.32 Ar / (Ar + N2) at 55%

[0108] Table 2 lists the materials of each layer or coating that constitutes the coatings according to their position with respect to the substrate bearing the stack (last line at the bottom of the table).

[0109] [Tables2] Rev. 1 Rev. 2 Rev. 3 Rev. 4 Rev. 5 Rev. 6 Rev. 7 extra RDs ITO - 60 35 35 35 - - AZO 60 - 60 60 60 60 60 Zn - - - - - - - CB Ti 0.5 0.5 1 - - - - TiN - - - 1 - - - NiCr - - - - 1 1 - Zn - - - - - - 2 CF Ag 10 10 10 10 10 10 10 RD lower. AZO 5 5 5 5 5 5 5 SnZnO 5 5 5 5 5 5 5 Si3N4 20 20 20 20 20 20 20 Glass substrate 2 mm 2 mm 2 mm 2 mm 2 mm 2 mm 2 mm

[0110] The first dielectric coatings include a SiN / SnZnO / ZnO sequence to prevent the diffusion of chemical species from the substrate and to decrease surface roughness and optimize the quality of the silver. The coatings have not undergone high-temperature heat treatment. II. Determination of electrochemical properties

[0111] In order to determine the electrochemical properties of conductive coatings by In relation to the mobile species of the electrolyte such as Li / Li+, voltammetric cycles were performed. For this, the current response resulting from a continuous variation of the potential of the electroconductive coating (used as a working electrode) on which the electrochemical reaction under study takes place is measured. The figures represent voltammetric cycles performed using a three-electrode setup with a metallic lithium counter electrode, a metallic lithium reference electrode, and a working electrode incorporating various electroconductive coatings. The electrolyte consists of a LiClO4 / PC solution. The voltamograms are performed in the potential window of 2 to 4 V relative to Li / Li+ at a sweep rate of 2 mV / s.

[0112] 1. Nature of dielectric layers of the upper dielectric coating

[0113] The electroconductive coatings Rev. 1, Rev. 2 and Rev. 3 differ in the choice of the conductive oxide layer(s) constituting the dielectric coating superior. The electroconductive coatings tested in [Fig. 1] have not undergone heat treatment. This graph shows coating degradation with an oxidation peak and a reduction peak, as well as a current increase above 3.4 V vs. Li / Li+. However, this phenomenon is less pronounced when using a conductive oxide layer based on aluminum-doped zinc oxide. This is reflected in particular by a less pronounced peak in the case of Rev.1 than in Rev.2 or Rev.3. Consequently, the electroconductive coating of the invention preferably comprises at least one layer of aluminum-doped zinc oxide with a thickness greater than 40 nm or greater than 50 nm. 2. Nature of the blocking layers 1. Absence of heat treatment

[0114] Rev.4 and Rev.5 differ from Rev.3 in the nature of the blocking layer (TiN and NiCr respectively versus Ti). [Fig.2] shows the voltamogram cycles of these 3 coatings in the absence of heat treatment.

[0115] Replacing the metallic blocking layer of Ti with TiN or NiCr significantly impacts the electrochemical window of silver. The current rise above 3.4V vs. Li / Li+ is much lower, and the oxidation or reduction peaks around 3.6-3.7V vs. Li / Li+ are no longer observed. The electrode coating is compatible with EC devices operating in the 2-4V vs. Li / Li+ range. The NiCr and TiN layers effectively act as a shield against any degradation of the silver layer that may occur during the deposition of a subsequent layer (sputtering deposition), high-temperature annealing and / or subsequent electrochemical reaction.

[0116] Rev.6, Rev.7 and Rev.1 differ in the nature of the blocking layer (respectively NiCr, Zn and Ti). [Fig.3] shows the voltamogram cycles of these 3 coatings. No heat treatment was carried out.

[0117] The presence of a zinc- or titanium-based metallic blocking layer near the silver layer does not show any positive effect. The presence of redox peaks indicates electrode degradation. Rev.6 according to the invention exhibits good electrochemical stability. A very slight current increase is observed above 3.4 V, and no redox peaks are observed. The invention allows the use of the silver-based coating in a high-contrast electro-chromic device operating in the 2-4V vs Li / Li+ range. 2. After heat treatment

[0118] After heat treatment at 600°C for 8 minutes, redox peaks are observed for Rev.1, Rev.7 and Rev.6. [Fig.4] shows the voltamogram cycles of these 3 coatings after heat treatment.

[0119] For rev.7 comprising a blocking layer based on metallic zinc, this phenomenon is particularly significant. An increase in current above 3.4 V is observed, as well as redox peaks at 3.6 and 3.7 V. After heat treatment, the presence of a metallic zinc layer alone does not improve the electrochemical stability of silver.

[0120] For Rev.6 comprising a NiCr-based blocking layer, the positive impact of This layer is weaker when subjected to heat treatment.

Claims

Claims

1. Material comprising a substrate coated with a first conductive coating comprising, starting from the substrate: - a first dielectric coating, - a silver-based metal functional layer, - a blocking layer located above and immediately in contact with the silver-based metal functional layer, chosen from metal layers of one or more elements chosen from nickel and chromium such as Ni, Cr, NiCr, and metal nitride layers of one or more elements chosen from titanium, nickel, chromium such as NiN, CrN, NiCrN, TiN, - a second dielectric coating comprising at least one conductive oxide layer, the sum of the thicknesses of the conductive oxide layers chosen from mixed tin and indium oxide, tin-doped indium oxide, doped zinc oxide, doped ruthenium oxide and fluorine-doped tin oxide (SnO2:F) in the second dielectric coating of which is greater than 40 nm.

2. Material according to claim 1, characterized in that the blocking layer has a thickness of between 0.1 and 5.0 nm.

3. Material according to any one of the preceding claims, characterized in that the blocking layer is chosen from a layer of titanium nitride, metal layers based on nickel and / or chromium.

4. Material according to any one of the preceding claims, characterized in that the second dielectric coating comprises a layer of conductive oxide chosen from mixed tin and indium oxide or zinc oxide doped with aluminum and / or gallium.

5. Material according to any one of the preceding claims, characterized in that the second dielectric coating comprises a layer of conductive oxide based on aluminum-doped zinc oxide with a thickness greater than 50 nm.

6. Material according to any one of the preceding claims, characterized in that the first dielectric coating comprises at least one crystallized dielectric layer, in particular based on zinc oxide, optionally doped with at least one other element, such as aluminum.

7. Material according to the preceding claim, characterized in that the crystallized dielectric layer, notably based on zinc oxide, has a thickness of 2 to 15 nm.

8. Material according to any one of the preceding claims, characterized in that the first dielectric coating comprises: - a layer based on silicon nitride or oxynitride of aluminum and / or zirconium, and / or - a layer based on zinc and tin oxide.

9. Material according to any one of the preceding claims, characterized in that the substrate is made of glass, in particular soda-lime-silica or polymeric organic material.

10. Electrochromic system comprising: - a material comprising a substrate coated with a first conductive coating comprising, starting from the substrate: - a first dielectric coating, - a silver-based metallic functional layer, - a blocking layer located above and immediately in contact with the silver-based metallic functional layer, chosen from metallic layers of one or more elements chosen from nickel and chromium such as Ni, Cr, NiCr, and metallic nitride layers of one or more elements chosen from titanium, nickel, chromium such as NiN, CrN, NiCrN, TiN, - a second dielectric coating comprising at least one conductive oxide layer, the sum of the thicknesses of the conductive oxide layers is greater than 40 nm, - a first active layer comprising an electrochromic material, - an electrolyte layer,- a second active layer and - a second transparent electrically conductive coating, - possibly a substrate.,