HYDROCONVERSION OF A PLASTIC FILLER PROMOTED BY SULFUR AND IN THE PRESENCE OF A BI-FUNCTIONAL ZEOLITHIC CATALYST
A two-step hydroconversion process using sulfur radicals and zeolitic catalysts at controlled conditions addresses energy inefficiencies and gas production in plastic waste conversion, enhancing the yield of valuable hydrocarbon products.
Patent Information
- Application Number
- FR2022010940
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-10-21
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2042-10-21
AI Technical Summary
Existing plastic waste conversion processes are energy-intensive and produce high yields of unwanted gases and coke, with limited efficiency in producing valuable liquid hydrocarbon products.
A two-step hydroconversion process involving non-catalytic and catalytic stages with sulfur radicals and a bifunctional zeolitic catalyst at controlled temperatures and pressures, minimizing energy use and gas production while maximizing liquid product yield.
The process achieves high plastic conversion to valuable hydrocarbon cuts with reduced energy consumption and optimized product selectivity, producing fuels and petrochemical raw materials efficiently.
Abstract
Description
Title of the invention: HYDROCONVERSION OF A PLASTIC CHARGE PROMOTED BY SULFUR AND IN THE PRESENCE OF A BI-FUNCTIONAL ZEOLITHIC CATALYST Technical field
[0001] The present invention relates to the field of converting solid plastic fillers into a mixture of recoverable hydrocarbons, in particular the conversion of such fillers at high pressure and temperature in the presence of hydrogen and a hydrocracking catalyst. Prior art
[0002] In a context of circular economy and waste reduction, there is particular attention paid to plastics, which are traditionally petroleum-derived products, in order to recover them.
[0003] The recovery of plastic waste may consist of transforming said plastics, by mechanical and / or chemical means, in order to allow the production of plastics or plastic-based objects again. This is the recycling of plastic waste.
[0004] This recovery of plastic waste can also follow the path of energy recovery, in particular for non-recyclable or difficult to recycle plastic waste, as an alternative, in certain cases, to landfill. Typically, the energy recovery of plastic waste consists of producing energy, in the form of electricity and / or heat. For example, it is known to subject plastics from collection and sorting channels to a pyrolysis step to produce, among other things, plastic pyrolysis oils, which are generally burned to generate electricity and / or used as fuel in industrial boilers or district heating.
[0005] Plastic waste can also be transformed by high-pressure hydrogen hydroconversion processes into hydrocarbon fractions, which can be used in particular as fuels, for example to produce gasoline or diesel, or raw materials for petrochemicals.
[0006] The French patent application registered under the Applicant's filing number 21 / 14.037 thus relates to the incorporation of a plastic fraction, typically derived from waste, into a heavy fossil hydrocarbon feedstock, in a bubbling bed or hybrid bubbling-entrained bed hydroconversion process, for the production of fuel bases and other recoverable hydrocarbons. The plastic fraction, initially solid, is introduced into the hydroconversion reactor in different ways, and the process shows overall conversion levels close to those obtained with the same type of process treating more traditional heavy loads, 100% of fossil origin.
[0007] More generally, the liquefaction of plastic waste by thermal cracking or acid catalytic cracking to produce fuels has been the subject of laboratory studies since the 1990s.
[0008] The concatenated review by Munir et al. 2018, (Munir et al., Renewable and Sustainable Energy Reviews 90, 2018, 490-515) summarizes the prior art in the hydrocracking of plastics by direct liquefaction in the absence of co-feed. The authors conclude that increasing the reaction temperature results in an increase in conversion but also in the amount of unwanted gases and coke produced. The authors recommend temperatures not exceeding 400°C in the presence of a catalyst. The authors also indicate that bifunctional catalysts with both hydrogenation-dehydrogenation and cracking capabilities are most suitable for cracking plastics. This review refers in particular to the publication by Joo and Curtis 1998 (Catalytic coprocessing of LDPE with coal and petroleum residue using different catalysts. Fuel Process Technol 1998, 53, pp. 197-214), in which a bifunctional NiMo / zeolite (presulfurized) catalyst is tested, among others, for the hydrocracking of low density polyethylene LDPE (or LDPE for "low density polyethylene" in English terminology). At 400°C the conversions obtained are less than 30%. At 430°C the conversions become more significant. At this high reaction temperature, the bifunctional catalysts with zeolite tested show better activity compared to other alumina-based catalysts. However, the quantities produced of gas and products lighter than naphtha are high. The review also refers to the publication by Walendziewski and Steininger 2001 (Thermal and catalytic conversion of waste polyolefines. Catal Today 2001, 65, p.323-330), which presents the results of hydrocracking of polyethylene (PE) waste using a commercial bifunctional catalyst NiW+10%HY. The authors conclude that the optimum temperature for liquefaction of plastics is between 410°C and 430°C or at least 390°C. At 410°C in the presence of this catalyst the quantities of gas produced are very significant.
[0009] Among the studies listed in the review by Munir et al. 2018, some have shown the potential of using sulfur in promoting the conversion of plastics.
[0010] Thus, Nakamura and Fujimoto (Development of new disposable catalyst for waste plastics treatment for high quality transportation fuel. Catalysis Today 27, 1996, p. 175-179) studied the conversion of polypropylene (PP) in an autoclave reactorbetween 380°C and 400°C, under an initial hydrogen pressure of 3 MPa, in the presence or absence of iron-based catalysts supported on activated carbon or amorphous silica-alumina and in the presence of carbon disulfide (CS2). The authors observed that, with or without catalyst, the presence of CS2 increases the yield of liquid products and reduces the yield of solid residue. The authors conclude that sulfur in the reactor is a promoter for the conversion of PP, and propose an explanatory mechanism according to which hydrocarbon radicals would be formed by thermal cracking of the CC bonds of the polymer; a majority of these radicals would recombine with each other in the absence of H2S, whereas in the presence of H2S, the latter could diffuse into the structure of the polymer, a hydrogen atom of H2S being able to be captured by a hydrocarbon radical so as to form a stable hydrocarbon and radical HS*.The lifetime of the hydrocarbon radical would thus be reduced and its recombination prevented, as well as its potential to continue thermal cracking which generally leads to unfavorable gas yields. Thermal cracking therefore makes it possible to transform enormous polymer molecules into long molecules which would not be cracked too much thanks to the stabilization of the radicals by H 2 S. These long molecules can then undergo selective catalytic cracking. Depending on the catalyst used, the yields in various cuts vary in fact, in particular the yield of gaseous product which remains high in particular with the tested catalyst based on iron supported on amorphous silica-alumina, and even higher when CS2 is associated.
[0011] Ibrahim and Seehra (Ibrahim and Seehra, Energy & Fuels 11, 1997, 926-930) studied the depolymerization temperature (Td) of a plastic mixture monitored by electron spin resonance (ESR) under an initial hydrogen pressure of 500 psig (3.45 MPa). A plastic sample composed of 5% PP, 95% high-density polyethylene (HDPE) and traces (< 3%) of polyethylene terephthalate (PET) was mixed with other compounds: elemental sulfur, or a mixture of elemental sulfur (S) and a NiMo / Al2O3 catalyst, or an HSZSM-5 zeolite. The authors found that the Td of the plastic sample decreased by 80°C when the plastic was mixed with elemental sulfur, but was not affected by the presence of HSZSM-5. Increasing the amount of elemental sulfur S introduced did not change the Td.The authors conclude that sulfur in the reactor is a promoter for the conversion of plastic during its thermal cracking by a free radical mechanism. No information on the conversion of plastics to fuels is given in their study.
[0012] Shiro et al. (Shiro et al., Energy & Fuels 16, 5, 2002, 1314-1320) studied the decomposition of low density polyethylene (LDPE) in an autoclave reactor between 300°C and 425°C under an initial hydrogen pressure of 5 MPa. Sulfur compounds, such as H2S, elemental sulfur, dimethyl disulfide (DMDS of formula (CH3S)2) etc. are added. The authors conclude that the addition of sulfur compounds has a promoting effect on the decomposition of LDPE.
[0013] The addition of sulfur or sulfur compounds is rather well known, in hydroconversion processes, to sulfurize the catalysts, and thus make them "active". Conventionally, the catalysts are advantageously subjected to a sulfurization treatment making it possible to transform, at least in part, the metallic species into sulfurized form before they are brought into contact with the feedstock to be treated. This sulfurization activation treatment is well known to those skilled in the art. The formation of the active phase of the catalyst by sulfurization can be done in situ, i.e. in the hydroconversion process after loading the catalyst or catalyst precursor, typically in the reactor, for example by adding sulfur-containing organic molecules such as DMDS, thioacetamide, etc. to the hydrocarbon feedstock to be treated, under conditions of hydrogen pressure and temperature, or can be done ex-situ, i.e. before loading the catalyst at one of the stages of the hydroconversion process, under conditions suitable for activation. For example, in the field of feedstock conversion comprising plastics, the French patent application filed under the discussed number 21 / 14.037 already mentioned above, describes the possibility of forming and activating in situ a colloidal or molecular catalyst, which is an extremely small (e.g., less than 1 μm) dispersed catalyst type (also called entrained catalyst or slurry), by the interaction of sulfur with a soluble catalyst precursor, generally at high temperature, and thus forming the metal sulfide type catalyst. A sulfur source can be H2S dissolved in the fossil hydrocarbon feedstock, or H2S contained in hydrogen recycled to the hydroconversion reactor, or originating from sulfur-containing organic molecules introduced into the fossil hydrocarbon fraction of the feedstock to be treated (e.g., injection of DMDS or thioacetamide). Patent application CA2171803, relating to the liquefaction of plastic waste mixed with a suspending agent in a pressurized container of H2 or N2, alone or in a mixture, and optionally in the presence of a solid catalyst, describes the possibility of adding a sulfur donor agent to sulfurize metals possibly present used as catalysts, in particular iron.
[0014] The problem of plastic waste management and environmental concerns being more topical than ever, there is always a search for efficient processes for converting plastic waste to make fuels or raw materials for petrochemicals, which are in particular energy-efficient and lower cost, and which can satisfy varied or changing needs in products, for example in fuels. Objectives and Summary of the Invention
[0015] In the context described above, an objective of the present invention is to provide a process for converting plastics in the presence of hydrogen to a mixture of recoverable hydrocarbons, which allows maximum conversion of the plastics while minimizing the energy required for the conversion, and while minimizing the production of gas during the conversion in order to improve the relative yield of liquid products of interest.
[0016] The present invention thus proposes, according to a first aspect, a process for hydroconversion of a plastic filler comprising the following steps: (a1) a step of non-catalytic hydroconversion of said filler in the presence of hydrogen, in contact with a source of radicals, said source comprising sulfur and being introduced in such a way that the sulfur content is between 3% and 20% by weight relative to the weight of the plastic filler, to produce first conversion products; (a2) a step of catalytic hydroconversion of the first conversion products in the presence of hydrogen, in contact with at least one hydroconversion catalyst, said hydroconversion catalyst comprising at least one hydro-dehydrogenating element chosen from the group formed by the non-noble elements of group VIB and group VIII of the periodic table, taken alone or as a mixture, and a porous support comprising a porous mineral matrix and at least one zeolite, said steps (a1) and (a2) being carried out at an absolute pressure of between 1 MPa and 38 MPa, at a temperature greater than or equal to 200°C and less than 400°C, at an hourly space velocity relative to each hydroconversion reactor of between 0.05 h 1 and 10 h1, and with a quantity of hydrogen of between 50 Nm3 / m3 and 5000 Nm3 / m3.
[0017] Compared to other plastic conversion technologies, in particular pyrolysis, the method according to the present invention has the advantage, among others, of being more economical in terms of energy and operating and investment costs, thanks to its operation at a lower temperature than pyrolysis.
[0018] The process according to the present invention can also make it possible to vary the composition of the products obtained, in particular thanks to the selectivity provided by the catalyst during the second catalytic hydroconversion stage, which can be chosen according to the targeted recovery (e.g. kerosene for the aeronautical sector, diesel or gasoline for the automobile sector, naphtha for steam cracking, etc.).
[0019] According to one or more implementations of the invention, steps (a1) and (a2) are carried out within the same reactor, preferably within the same ebullated bed reactor.
[0020] According to one or more implementations of the invention, steps (a1) and (a2) are carried out in two separate reactors, preferably steps (a1) and (a2) being carried out in two separate ebullated bed reactors or step (a1) being carried out in one ebullated bed reactor and step (a2) being carried out in one fixed bed reactor.
[0021] According to one or more implementations of the invention, said at least one zeolite of the support of the hydroconversion catalyst is chosen from the list consisting of zeolites of FAU groups, preferably zeolites of FAU group chosen from zeolites X, Y, USY, Y having undergone a dealumination treatment, BEA, ISV, IWR, IWW, MEI, UWY, MEL, MTW, MTT, MSE, FER and MFI, and preferably, said at least one zeolite is chosen from zeolites of the FAU or BEA groups.
[0022] According to one or more implementations of the invention, the catalyst support comprises a USY zeolite and / or a Beta zeolite.
[0023] According to one or more implementations of the invention, the support of the hydroconversion catalyst comprises at least one zeolite chosen from the group formed by the zeolites ZSM-12, IZM-2, ZSM-22, ZSM-23, SAPO-11, ZSM-48, and ZBM-30.
[0024] According to one or more implementations of the invention, the hydroconversion catalyst comprises:
[0025] - between 0.1% and 50% by weight of said at least one hydro-dehydrogenating element of the group formed by the non-noble elements of group VIB and group VIII, expressed as weight of oxide relative to the total weight of said catalyst; - between 0.1 and 99.9% by weight of a porous support relative to the total weight of said catalyst, said support comprising between 0.1% and 80% by weight of zeolite relative to the total weight of said support, and between 0.1% and 99.9% by weight of a porous mineral matrix expressed as weight of oxide relative to the total weight of said support; - between 0 and 20% by weight, and preferably between 0.1% and 20% by weight, of at least one element chosen from the group formed by phosphorus, boron, and silicon, expressed as weight of oxide relative to the total weight of said catalyst; - between 0 and 20% by weight of at least one element from group VIIA, preferably 0.1 to 20%; - between 0 and 20% by weight of at least one element from group VIIB, preferably 0.1 to 20%, 0 to 60% by weight of at least one element from group VB, preferably 0.1 to 60%; the percentages being expressed as a percentage by weight relative to the total mass of catalyst, the sum of the percentages of the elements constituting said catalyst being equal to 100%.
[0026] According to one or more implementations of the invention, the hydroconversion catalyst comprises a porous mineral matrix consisting of at least one refractory oxide chosen from the group formed by alumina, silica-alumina, clay, titanium oxide, boron oxide and zirconia, taken alone or in a mixture, and preferably the porous mineral matrix is alumina.
[0027] According to one or more implementations of the invention, the hydroconversion catalyst comprises, as hydro-dehydrogenating elements, at least one non-noble group VIII metal chosen from nickel and cobalt, preferably nickel, and at least one group VIB metal chosen from molybdenum and tungsten, preferably molybdenum.
[0028] According to one or more implementations of the invention, the source of radicals comprising sulfur is chosen from the list consisting of H2S, elemental sulfur, carbon disulfide (CS2), dimethyl sulfide (DMS), dimethyl sulfoxide (DMSO), diethyl sulfide (DES), dimethyl disulfide (DMDS of formula (CH3S)2), mercaptans, polysulfides such as di-tert-nonyl polysulfide, taken alone or as a mixture, and is preferably chosen from H2S, DMS, DMDS, and DES.
[0029] According to one or more implementations of the invention, the sulfur content in step (a1) is between 3% and 15% by weight relative to the weight of the plastic filler, preferably between 3% and 10% by weight of the filler.
[0030] According to one or more implementations of the invention, the method further comprises: (aO) a prior step of conditioning said feedstock for its introduction into a reactor in which at least the first step (a1) is carried out, said step (aO) comprising: - sending the plastic charge in the form of solid particles into an extruder, preferably with a plastic diluent, in which it is gradually heated to a temperature higher than the melting temperature of said plastic charge, and put under the pressure of the first hydroconversion reactor, during conveying, and - the introduction of the extruded plastic charge into said reactor.
[0031] According to one or more implementations of the invention, the plastic filler is in solid form and comprises one or more polymers chosen from the list consisting of alkene polymers, diene polymers, vinyl polymers, and styrenic polymers, polyesters, and polyamides, and preferably said plastic filler comprises at least 50% by weight of polyolefins relative to the total weight of the plastic filler, said polyolefins preferably being chosen from the list consisting of polyethylene, polypropylene and / or copolymers of ethylene and propylene.
[0032] According to one or more implementations of the invention, steps (a1) and (a2) are carried out at an absolute pressure of between 2 MPa and 25 MPa, and at a temperature temperature greater than or equal to 300°C and less than 400°C.
[0033] Other objects and advantages of the invention will appear on reading the following description of particular examples of embodiment of the invention, given as non-limiting examples. Detailed description of the invention
[0034] In the following detailed description, numerous specific details are set forth in order to provide a more thorough understanding of the method. However, it will be apparent to those skilled in the art that the method may be practiced without necessarily all of these specific details. In other instances, well-known features have not been described in detail to avoid unnecessarily complicating the description.
[0035] Some definitions are given below for a better understanding of the invention.
[0036] In this description, the term "comprise" is synonymous with (means the same as) "include" and "contain", and is inclusive or open and does not exclude other elements that are not mentioned. It is understood that the term "comprise" includes the exclusive and closed term "consist".
[0037] In the present description, the expression "between ... and ..." means that the limit values of the interval are included in the range of values described, unless otherwise specified.
[0038] In the present invention, the different ranges of values of given parameters may be used alone or in combination. For example, a preferred range of pressure values may be combined with a more preferred range of temperature values, or a preferred range of values of one chemical compound or element may be combined with a more preferred range of values of another chemical compound or element.
[0039] Within the meaning of the present invention, the various embodiments presented can be used alone or in combination with each other, without limitation of combination.
[0040] In the present description, the groups of chemical elements are given according to the CAS classification (CRC Handbook of Chemistry and Physics, publisher CRC press, editor-in-chief DR Lide, 81st edition, 2000-2001). For example, group VIII according to the CAS classification corresponds to the metals of columns 8, 9 and 10 according to the new IUP AC classification, and group VIB to the metals of column 6.
[0041] The term "hydroconversion" refers to a process whose primary purpose is to reduce the boiling point range of a hydrocarbon feedstock, and in which a substantial portion of the feedstock is converted to products having boiling point ranges lower boiling points than those of the original feedstock. Hydroconversion generally involves the fragmentation of molecules, typically hydrocarbons, into smaller molecular fragments with a lower number of carbon atoms and a higher hydrogen to carbon ratio (H / C). The reactions carried out during hydroconversion reduce the size of hydrocarbon molecules, primarily by cleavage of carbon-carbon bonds, in the presence of hydrogen to saturate the cleaved bonds and aromatic rings. The mechanism by which hydroconversion typically occurs involves the formation of free radicals, commonly hydrocarbons, during fragmentation primarily by thermal cracking, followed by capping of the free radical ends or fragments with hydrogen in the presence of active catalyst sites.Of course, during a hydroconversion process, other reactions typically associated with hydrotreatment may occur, such as, among others, the removal of sulfur or nitrogen from the feedstock, or the saturation of olefins, and as more broadly defined below. In French terminology, the term hydroconversion is rather reserved for processes that treat heavy petroleum feedstocks such as atmospheric residues and vacuum residues (but not only), while the term hydrocracking is rather reserved for processes that treat lighter feedstocks such as vacuum distillates and gas oils. In English terminology, the terms hydroconversion and hydrocracking are often used interchangeably. In this description, the terms hydrocracking and hydroconversion are synonymous, the feedstock treated being of the plastic type.
[0042] The term "hydrotreating", commonly referred to as "HDT", refers to a milder operation whose primary purpose is to remove impurities such as sulfur, nitrogen, oxygen, halides, and trace metals from the feedstock, and to saturate olefins and / or stabilize free radicals, typically hydrocarbons, by reacting them with hydrogen rather than allowing them to react with themselves. The primary purpose is not to change the boiling point range of the feedstock. Thus, hydrotreatment includes in particular hydrodesulfurization reactions (commonly called "HDS"), hydrodenitrogenation reactions (commonly called "HDN") and hydrodemetalation reactions (commonly called "HDM"), accompanied by hydrogenation, hydrodeoxygenation, hydrodearomatization, hydroisomerization, hydrodealkylation, hydrocracking, hydrodeasphalting and Conradson carbon reduction reactions.Hydroprocessing is most commonly carried out using a fixed bed reactor, although other reactors can also be used for hydroprocessing, for example an ebullated bed hydroprocessing reactor.
[0043] The terms "porous supported catalyst", "solid supported catalyst", and "supported catalyst" refer to catalysts that are typically used in conventional ebullated bed and fixed bed hydroconversion systems, including catalysts designed primarily for hydrocracking or hydrodemetallization and catalysts designed primarily for hydroprocessing. Such catalysts typically comprise (i) a catalyst support having a large surface area and numerous interconnected channels or pores and (ii) fine particles of an active catalyst such as sulfides of cobalt, nickel, tungsten, molybdenum, or mixed sulfides of these elements (e.g., NiMo, CoMo, etc.), dispersed within the pores. Supported catalysts are commonly produced as cylindrical extrudates ("pellets") or spherical solids, although other shapes are possible.
[0044] In the present description, according to the IUP AC convention, "micropores" means pores whose diameter is less than 2 nm; "mesopores" means pores whose diameter is greater than 2 nm and less than 50 nm; and "macropores" means pores whose diameter is greater than or equal to 50 nm.
[0045] The term "specific surface area" of zeolites, supports or catalysts means the BET specific surface area determined by nitrogen adsorption in accordance with ASTM D 3663-78 established from the BRUNAUER-EMMETT-TELLER method described in the periodical "The Journal of American Society", 60, 309, (1938).
[0046] The quantitative analysis of microporosity (pores with a diameter of less than 2 nm) is carried out using the "t" method (Lippens-De Boer method, 1965) which corresponds to a transform of the initial nitrogen adsorption isotherm as described in the book "Adsorption by powders and porous solids. Principles, methodology and applications" written by F. Rouquérol, J. Rouquérol and K. Sing, Academie Press, 1999. Eight pressure points are used, P / P0 = 0.075, 0.100, 0.125, 0.150, 0.175, 0.200, 0.250 and 0.300
[0047] Similarly, the term "total pore volume" of zeolites, supports or catalysts means the volume measured by nitrogen adsorption for P / P0 = 0.99, pressure for which it is assumed that the nitrogen has filled all the pores.
[0048] The term “mesoporous volume” of zeolites means the difference between the total pore volume described above and the microporous volume.
[0049] The method according to the invention and its operation are described in more detail below.
[0050] The object of the invention is to propose a process for hydroconversion of a plastic charge comprising the following steps: (al) a non-catalytic hydroconversion step of said feedstock in the presence of hydrogen, in contact with a source of radicals, said source comprising sulfur and being introduced so that the sulfur content is between 3% and 20% by weight relative to the weight of the plastic charge, to produce first conversion products; (a2) a step of catalytic hydroconversion of the first conversion products in the presence of hydrogen, in contact with at least one hydroconversion catalyst, said hydroconversion catalyst comprising at least one hydro-dehydrogenating element chosen from the group formed by the non-noble elements of group VIB and group VIII of the periodic table, taken alone or as a mixture, and a porous support comprising a porous mineral matrix and at least one zeolite, said steps (a1) and (a2) being carried out at an absolute pressure of between 1 MPa and 38 MPa, at a temperature greater than or equal to 200°C and less than 400°C, at an hourly space velocity relative to each hydroconversion reactor of between 0.05 h 1 and 10 h 1, and with a quantity of hydrogen of between 50 Nm3 / m3 and 5000 NmVm3. The charge
[0051] The feedstock treated in the hydroconversion process according to the invention is a plastic feedstock.
[0052] The plastic filler of the method according to the invention comprises plastics which themselves more particularly comprise polymers.
[0053] Plastics or plastic materials are generally polymers which are most often mixed with additives, in order to constitute, after shaping, various materials and objects (injection-molded parts, tubes, films, fibers, fabrics, mastics, coatings, etc.). The additives used in plastics can be organic compounds or inorganic compounds. These are, for example, fillers, colorants, pigments, plasticizers, property modifiers, flame retardants, etc.
[0054] Thus, by plastic filler, we mean a solid filler of plastics comprising one or more polymers, and which may contain other compounds, such as additives of organic or inorganic origin and / or usage impurities, in particular from the life cycle of plastic materials and objects, and / or from the waste collection and sorting circuit. For example, usage impurities may be metallic, organic or mineral; they may be packaging residues, food residues or compostable residues (biomass). Usage impurities may also include glass, wood, cardboard, paper, aluminum, iron, metals, tires, rubber, silicones, rigid polymers, thermosetting polymers, household, chemical or cosmetic products, used oils, water.
[0055] In the present description, the term “plastic impurities” refers to all compounds initially contained in the plastic filler which are not polymers and which are not capable of being converted during the process step(s). For example, certain organic additives can be at least partly converted in the process according to the invention, in the same way as polymers. These are therefore not considered as impurities of the plastics. On the other hand, some of the inorganic additives can be eliminated during the process, for example those containing metals, and / or sulfur, and / or nitrogen, and / or oxygen, and / or other heteroatoms (Cl, Br, etc.). They are considered as impurities of the plastics.
[0056] The plastics included in the plastic feedstock of the process according to the invention are generally production scrap and / or waste, in particular household waste, building waste or waste from electrical and electronic equipment. Preferably, the plastic waste comes from collection and sorting channels.
[0057] The plastic filler of the process according to the invention therefore comprises polymers, and in particular thermoplastics. The polymers included in the plastic fraction of the filler may be alkene polymers, diene polymers, vinyl polymers, styrenic polymers (e.g. polystyrene “PS”), polyesters, and / or polyamides. Preferably, the polymers included in the plastic filler of the invention are alkene polymers, diene polymers, vinyl polymers and / or styrenic polymers (e.g. polystyrene “PS”). Preferably, the polymers included in the plastic filler are polyolefins (alkene polymers), such as polyethylene (PE), polypropylene (PP) and / or copolymers of ethylene and propylene. For example, the plastic filler of the filler comprises at least 50% by weight, preferably at least 80% by weight, more preferably at least 90% by weight, and most preferably at least 94% by weight, of polyolefins relative to the total weight of the plastic filler.
[0058] The plastic filler may comprise mixtures of polymers, in particular mixtures of thermoplastics and / or mixtures of thermoplastics and other polymers, and compounds other than these thermoplastics and polymers, in particular the additives advantageously used to formulate the plastic material and generally usage impurities resulting from the life cycle of the plastic materials and objects, and / or resulting from the waste collection and sorting circuit. The plastic filler of the method according to the invention generally comprises less than 50% by weight of these additives and usage impurities, preferably less than 20% by weight, and more preferably less than 10% by weight.
[0059] The plastic filler may advantageously be pretreated upstream of the process so as to at least eliminate all or part of the so-called coarse usage impurities, that is to say usage impurities in the form of particles of a size greater than or equal to 10 mm, preferably greater than or equal to 5 mm, or even greater than or equal to 1 mm, for example usage impurities of the wood, paper, biomass, iron, aluminum, glass, etc. type, and to shape it generally in the form of particles (divided solids) so as to facilitate treatment in the process. This pretreatment may comprise a grinding step, a washing step at atmospheric pressure and / or a drying step. This pretreatment may be carried out on a different site, for example in a waste collection and sorting center, or on the same site where the treatment method according to the invention is implemented.Preferably, this pretreatment makes it possible to reduce the content of usual impurities to less than 6% by weight. At the end of the pretreatment, the plastic filler is generally stored in the form of particles, for example in the form of ground material or powder, so as to facilitate handling and transport to the process.
[0060] (aO) Optional step of conditioning the feedstock for its injection into the first hydroconversion reactor
[0061] The method according to the invention may comprise a step (aO) of conditioning the plastic charge for its injection into the first hydroconversion reactor.
[0062] In the present description, the term "first hydroconversion reactor" refers to the reactor in which at least step (a1) is carried out, i.e. when step (a1) is carried out or in which the two steps (a1) and (a2) are carried out if they are carried out in the same reactor. Thus, if the two steps are carried out in separate reactors, the hydroconversion reactor of step (a2) is not the first hydroconversion reactor.
[0063] By conditioning the feedstock is meant its conditioning for the following step (a1) of hydroconversion of the feedstock once introduced into the first hydroconversion reactor, i.e. its placing in a state and at temperature and pressure conditions suitable for hydroconversion in the first hydroconversion reactor.
[0064] The plastic charge initially in solid form can be conditioned before being sent to the first hydroconversion reactor, in particular to adapt to the type of hydroconversion reactor used and facilitate its conversion.
[0065] According to one or more embodiments, the plastic filler in the form of solid particles is sent into an extruder, preferably with a plastic diluent, in which it is gradually heated to a temperature above the melting temperature of said plastic filler, and put under the pressure of the first hydroconversion reactor, during conveying preferably for a duration less than 15 minutes, and the extruded plastic charge is introduced into the reactor.
[0066] According to these embodiments, the plastic filler introduced into the first hydroconversion reactor by extrusion is in an essentially liquid form.
[0067] Extrusion is classically a process that allows the injection or shaping of a polymer initially in a solid state. According to an extrusion process, the material is transported via one or more screws, kneaded and heated, which allows it to melt. And at the same time, the screw(s) convey the material and cause it to increase in pressure, which allows it to be injected into a die or into a mold.
[0068] According to these embodiments of the invention, the extrusion of the plastic feedstock is a means of introducing the plastic feedstock which is solid at room temperature into the first hydroconversion reactor operating under high pressure and temperature. The extrusion therefore makes it possible to heat, in order to liquefy, and to pressurize the plastic feedstock at the operating conditions of the reactor described below.
[0069] The material is not injected into a die or a mold as in a conventional extrusion process, thus not constituting a shaping process, but it is injected directly into the reactor.
[0070] The "plastic diluent" is for example formed by a hydrocarbon or a mixture of light liquid hydrocarbons. For example, the plastic diluent is a hydrocarbon oil composed of hydrocarbons of which at least 50% by weight, and preferably at least 80% by weight, relative to the weight of the plastic diluent, have a boiling point below 300°C. Examples of suitable hydrocarbon diluents include, but are not limited to, light liquid hydrocarbons, typically C5+ hydrocarbons, i.e. hydrocarbons which may have 5 or more carbon atoms per molecule, for example xylene, toluene, gasoline, mixtures thereof, etc. The plastic diluent may have a function as a solvent for the plastic fraction, in particular for the polymer(s) of the plastic filler.
[0071] During extrusion, the plastic filler is preferably gradually heated to a temperature above its melting temperature so as to melt. Advantageously, at least 80% by weight of the plastic fraction is in liquid (molten) form at the end of the extrusion, very advantageously at least 90% by weight, preferably at least 95% by weight, or even 98% by weight. As described above, the plastic fraction generally contains compounds other than polymers, in particular plastic impurities. Some of these non-polymeric compounds, including plastic impurities, may be insoluble and / or have a higher melting point than the polymer(s) of the plastic fraction. Even if all of the polymer(s) melt, a portion of the liquid fraction, taking into account the non-polymeric compounds, may therefore remain in a solid form. This is true for all the steps described below in which heating results in the total or almost total liquefaction of the plastic fraction.
[0072] The extrusion temperature depends on the polymer composition(s) of the plastic filler (nature and proportion(s) of the polymer(s)).
[0073] Preferably, the extruder is operated at a temperature between a temperature 25°C lower than the melting temperature of the plastic filler and a temperature 25°C higher than the melting temperature of the plastic filler.
[0074] In the case where the plastic filler comprises a mixture of polymers, the extruder is operated at a temperature between a temperature of 25°C lower than the melting temperature of the least refractory polymer (i.e. which has the lowest melting temperature) of the plastic filler and a temperature of 25°C higher than the melting temperature of the most refractory polymer (i.e. which has the highest melting temperature) of the plastic filler.
[0075] Advantageously, the plastic filler is preferably gradually heated in the extruder to a temperature above the melting temperature of the polymer which has the highest melting point.
[0076] As an indication, the melting temperature of polypropylene (PP) is approximately 170°C, the melting temperature of polyethylene (PE) is between approximately 85°C and 140°C, and the melting temperature of polystyrene (PS) is between approximately 240°C and 270°C.
[0077] Preferably, the extruder is operated at a temperature between 60°C and 295°C, more preferably between 60°C and 195°C.
[0078] Advantageously, the extruder is operated at a temperature between 60°C and 165°C, so as to melt a plastic filler mainly comprising PE as polymer.
[0079] Advantageously, the extruder is operated at a temperature between 145°C and 195°C, so as to melt a plastic filler mainly comprising PP as polymer.
[0080] Advantageously, the extruder is operated at a temperature between 215°C and 295°C, so as to melt a plastic filler mainly comprising PS as polymer.
[0081] The operating temperature of the extruder is advantageously adapted according to the composition of the plastic charge.
[0082] Advantageously, the extruder comprises at least one screw conveying section, called the extrusion section, fed with the plastic fraction.
[0083] The residence time in this extrusion section (volume of said section divided by the volume flow rate of plastic fraction) is advantageously less than 15 minutes, preferably less than 10 minutes, and more preferably less than 2 minutes.
[0084] Said extrusion section is advantageously connected to a vacuum extraction system so as to remove impurities such as dissolved gases, light organic compounds and / or moisture which may be present in the plastic fraction.
[0085] Said extrusion section may also advantageously comprise a filtration system for removing solid particles of undesirable size, for example of a size greater than 200 μm, and preferably of a size greater than 40 μm, such as sand particles. If a diluent is used, the viscosity being able to decrease, it is possible to filter particles of smaller size, for example of a size greater than 3 μm.
[0086] According to one or more other embodiments, the plastic filler in the form of solid particles is mixed with a plastic diluent in a mixing section and heated in a heating section to a temperature above the melting temperature of said plastic filler, preferably between 60°C and 295°C, before its introduction into the first hydroconversion reactor, the heating step being able to be carried out before or after mixing with the plastic diluent, and preferably after mixing with the plastic diluent.
[0087] These embodiments thus correspond to a direct injection of the plastic filler in an essentially liquid form, after said plastic filler has been mixed with a plastic diluent to form a slurry then heated so as to obtain an essentially liquid plastic filler.
[0088] By plastic filler in an essentially liquid form is meant that at least 80% by weight of the polymer(s) of the plastic filler are in a liquid form, preferably at least 90% by weight, more preferably at least 95% by weight, and even more preferably at least 98% by weight. By polymers of the plastic fraction in a liquid form is meant polymers which are not in a solid form, the latter being generally considered to correspond to the crystalline, semi-crystalline and amorphous states of a polymer.
[0089] By slurry is meant a mixture of substances in the form of a suspension, which usually corresponds to a system formed of solid particles dispersed in a liquid (liquid dispersion). More specifically, a plastic filler in the form of a suspension corresponds to a system comprising solid plastic particles dispersed in a liquid, for example a system comprising between 1% by weight and 50% by weight of solid plastic particles dispersed in a liquid, or even between 1% by weight and 30% by weight or even between 5% by weight and 20% by weight. The liquid continuous phase in which the solid plastic particles are dispersed may be a diluent.
[0090] These embodiments have the particular advantage of implementing simple and inexpensive equipment.
[0091] The plastic filler in the form of solid particles may be premixed with a plastic diluent in a mixing section to form a suspension, then the suspension may be sent to a heating section to be heated to a temperature above the melting temperature of said plastic fraction, so that the solid particles of the suspended plastic filler melt, and said heated plastic filler may then be introduced into the first hydroconversion reactor. The mixing of the plastic diluent and the plastic filler in the form of particles in the mixing section is preferably carried out at atmospheric pressure or a pressure close to atmospheric pressure.
[0092] Preferably, during the mixing step in the mixing section, the temperature is such that the suspension has a kinematic viscosity of less than 0.3.10-3 m2 / s, corresponding to the viscosity of a pumpable fluid. The temperature at this step is preferably lower than the temperature operated in the heating step described below, in the case where the mixing step is dissociated and precedes the heating step.
[0093] The mixing section may comprise a mixing tank having dynamic stirring means for suspension, for example an agitator and / or a recirculation pump.
[0094] After heating the suspension, the plastic filler is essentially in liquid form.
[0095] What has been described for the temperature conditions of the extruder of the other embodiments described above applies to the heating of the suspension, and is therefore not repeated here.
[0096] The heating temperature may also depend on the plastic diluent used, such a plastic diluent being able in particular, depending on its nature, to allow the suspended plastic charge to melt at a lower temperature.
[0097] The heating section comprises any heating means known to a person skilled in the art capable of heating a suspended plastic charge, and for example comprising a furnace comprising at least one heating compartment, and / or tubes in which the suspension flows, any type of suitable heat exchanger, etc.
[0098] The mixing section and the heating section may be part of the same device configured to carry out the mixing and then the heating consecutively.
[0099] Before its introduction into the first hydroconversion reactor, the heated plastic charge may undergo a pressurization step to be adapted to the pressure operated in the first hydroconversion reactor, for example using a suitable pump. It can also be subjected to a filtration step aimed, for example, at eliminating solid particles from the plastic load which may be part of the impurities in plastics, such as sand, glass, metals, certain additives called "fillers" in English, etc.
[0100] According to another variant, a direct injection of the plastic feedstock in an essentially liquid form can be carried out after said plastic feedstock has been heated so as to obtain an essentially liquid plastic fraction, then mixed with a plastic diluent to form a diluted plastic feedstock introduced into the first hydroconversion reactor.
[0101] According to yet another variant, the mixing step and the heating step are carried out simultaneously, the mixing and heating sections then forming part of the same device configured to implement the mixing and heating simultaneously.
[0102] According to one or more other embodiments, a direct injection of the plastic filler in suspension is carried out into the first hydroconversion reactor: the plastic filler in the form of solid particles is first sent into a mixer to be mixed with a plastic diluent and form a suspension, preferably at a temperature greater than or equal to ambient temperature and lower than the melting temperature of said plastic filler, and said plastic filler in the form of a suspension is introduced into the first hydroconversion reactor.
[0103] These embodiments also have the advantage of implementing simple and inexpensive equipment.
[0104] According to these embodiments, the plastic filler in the form of solid particles is first sent to a mixer to be mixed with a plastic diluent and form a suspension, then said plastic filler in the form of suspension is introduced into the first hydroconversion reactor.
[0105] The mixing of the plastic diluent and the plastic filler in the mixer is preferably carried out at a temperature greater than or equal to room temperature, e.g. 15°C, and lower than the melting temperature of said plastic filler (or lower than the melting temperature of the polymer which has the lowest melting point if said plastic filler comprises a mixture of polymers). A temperature slightly lower than the melting temperature of the plastic filler may constitute the upper limit for the temperature of the mixture, because the plastic diluent used, depending on its nature, has an influence on the temperature at which the plastic filler can be dissolved (in the case where the plastic diluent has a solvent function).
[0106] According to one configuration, the mixing can be carried out at a temperature greater than or equal to 50°C or even 75°C and less than 170°C, for example well suited to the use of a VGO as a plastic diluent and a plastic filler comprising mainly PP as the polymer, or at a temperature greater than or equal to 150°C and less than 170°C, for example well suited to the use of a vacuum residue as a plastic diluent and a plastic filler comprising mainly PP as the polymer.
[0107] According to one configuration, the mixture can be carried out at a temperature greater than or equal to 50°C or even 75°C and less than 140°C, or else carried out at a temperature greater than or equal to 50°C or even 75°C and less than 85°C, for example well suited to the use of a VGO as a plastic diluent and to a plastic filler mainly comprising PE as a polymer.
[0108] According to one configuration, the mixture may be carried out at a temperature greater than or equal to 50°C or even 75°C and less than 270°C, or else carried out at a temperature greater than or equal to 50°C or even 75°C and less than 240°C, for example well suited to the use of a VGO as a plastic diluent and a plastic filler mainly comprising PS as a polymer, or else at a temperature greater than or equal to 150°C and less than 270°C, or even less than 240°C, for example well suited to the use of a vacuum residue as a plastic diluent and a plastic filler mainly comprising PS as a polymer.
[0109] The mixing may or may not be active. Examples of active mixing devices that may be used include, but are not limited to, high shear mixing such as mixing created in a pump with a propeller or turbine rotor, multiple static in-line mixers, multiple static in-line mixers in combination with high shear in-line mixers, multiple static in-line mixers in combination with high shear in-line mixers, multiple static in-line mixers in combination with high shear in-line mixers followed by recirculation pumping into the surge tank, combinations of the above devices followed by one or more multi-stage centrifugal pumps.
[0110] Before their introduction into the first hydroconversion reactor, the suspended plastic charge can undergo a pressurization step to be adapted to the pressure operated in the first hydroconversion reactor.
[0111] (al) sulfur-promoted thermal conversion step
[0112] According to the invention, the process comprises a first step (al) of non-catalytic hydroconversion of the plastic filler in the presence of hydrogen in contact with a source of radicals, to produce first conversion products.
[0113] By non-catalytic, it is meant that the hydroconversion step (a1) is carried out without involving catalytic reactions by means of a catalyst, i.e. a hydroconversion catalyst as is known to be used during a conventional hydroconversion, typically a porous supported catalyst or an entrained catalyst as well. called "slurry" (very small catalyst, e.g. less than 1 pm in diameter, dispersed in the reaction medium, distributed uniformly in the reactor, and carried along with the products leaving the reactor) formed for example from a soluble catalyst precursor of the metallic or organometallic type.
[0114] No catalyst of this type (porous support or slurry) participates in the reactions in step (al) of the process according to the invention.
[0115] The radical source comprises sulfur, and may be referred to as a sulfur radical source throughout the remainder of the description.
[0116] The source of sulfur radicals is introduced so that the sulfur content (elemental sulfur S) is between 3% and 20% by weight relative to the weight of the feedstock, preferably between 3% and 15% by weight, preferably between 3% and 10% by weight.
[0117] According to one or more embodiments of the invention, the source of sulfur radicals is chosen from the non-exhaustive list of the following compounds: H2S, elemental S, carbon disulfide (CS2), dimethyl sulfide (DMS), dimethyl sulfoxide (DMSO), diethyl sulfide (DES), dimethyl disulfide (DMDS of formula (CH3 S)2), mercaptans, polysulfides (for example of general formula RrS-S-R2 or RSS-SH, with R, Riet R2 possibly being an H, an alkyl or an aryl) such as for example di-tert-nonyl polysulfide, taken alone or in a mixture. Preferably, the source of sulfur radicals is chosen from the list consisting of H2S, DMS, DMDS, DES, and preferably is DMDS or H2S.
[0118] The operating conditions are described in more detail below, at the same time as those of the hydroconversion step (a2).
[0119] Without being bound by any theory, a radical mechanism involving H2S and HS* radicals such as that demonstrated in the prior art and described above, could explain at least in part the promotion of the conversion of the plastic charge at this stage (al) of the process according to the invention.
[0120] During this hydroconversion step, a maximum of plastic feedstock is converted. In particular, the process according to the invention advantageously makes it possible to convert more than 50% by weight of the solid plastic feedstock into non-solid conversion products, i.e. liquid and gaseous, preferably more than 65% by weight, even more preferably more than 80% by weight, and even more preferably more than 90% by weight.
[0121] The first conversion products are hydrocarbons which can be characterized by boiling point ranges. Conventionally, a hydrocarbon fraction is defined by an initial boiling point greater than or equal to a first temperature, and a final boiling point lower than a second temperature greater than the first temperature. For simplification, the expression "boiling range from ... to ...." can be used to express these initial (included in the range) and final (not included in the range) boiling points.
[0122] The first conversion products include hydrocarbon cuts lighter than naphtha (typical boiling range from PI to 80°C, PI being the initial point of the distillation curve), naphtha type (typical boiling range from 80°C to 150°C), kerosene (typical boiling range from 150°C to 250°C), diesel (typical boiling range from 250°C to 370°C), heavy cuts (typical boiling range from 370°C to 540°C), very heavy (typical boiling range from 540°C to 740°C) and extra heavy (typical boiling range above 740°C).
[0123] The first conversion products may also comprise small quantities of gaseous products, typically gases such as C1 to C6 hydrocarbons (i.e. having between 1 and 6 carbon atoms). (a2) catalytic hydroconversion step
[0124] According to the invention, the process comprises a second step (a2) of catalytic hydroconversion of the first conversion products in the presence of hydrogen, in contact with at least one hydroconversion catalyst.
[0125] This second step (a2) of catalytic hydroconversion forms second conversion products.
[0126] These second conversion products are a mixture of recoverable hydrocarbons, in particular hydrocarbon fractions which can in particular be characterized as described for the first hydroconversion products, by boiling point ranges. These fractions can serve as fuel bases or raw materials for petrochemistry (light hydrocarbons, distillates intended for a steam cracker in particular for the production of recycled polyolefins, bases for the production of bitumens, lubricants, etc.), in particular directly after fractionation or after fractionation followed by one or more subsequent treatments in step (a2), for example a hydrotreatment aimed at removing residual sulfur or other possible contaminants such as for example nitrogen, chlorine, silicon or metals.
[0127] The second conversion products include hydrocarbon cuts lighter than naphtha (typical boiling range of PI to 80°C), naphtha type (typical boiling range of 80°C to 150°C), kerosene (typical boiling range of 150°C to 250°C), diesel (typical boiling range of 250°C to 370°C), heavy cuts (typical boiling range of 370°C to 540°C), very heavy (typical boiling range of 540°C to 740°C) and extra heavy (typical boiling range above 740°C).
[0128] The second conversion products may also comprise small amounts of gaseous products, typically gases such as C1 to C6 hydrocarbons. Preferably, less than 30% of gas is produced during step (a1), more preferably less than 20% by weight, and even more preferably less than 15% by weight relative to the feedstock.
[0129] The association of the first hydroconversion step (al) promoted by sulfur, without catalyst and the catalytic hydroconversion step (a2) based in particular on a catalyst suitable for low-temperature operation, thio-resistant, and selective, makes it possible to maximize the conversion of the plastic feedstock while minimizing the energy required for the conversion, and while minimizing the production of gas during the conversion in order to improve the relative yield of liquid products of interest.
[0130] Indeed, the inventors have demonstrated that with the combination of these two steps (a1) and (a2), it was surprisingly possible to minimize the yield of gaseous hydrocarbons at the end of the hydroconversion, i.e. C1 to C6 hydrocarbons, relative to the liquid products obtained.
[0131] The choice of catalyst in step (a2), and in particular the selectivity provided by the catalyst, also makes it possible to modify the composition of the liquid products obtained, depending on the intended recovery. For example, it may be advantageous to maximize a naphtha cut for a steam cracking application, or a kerosene cut for the aeronautical sector, or even a very heavy cut for the production of bitumens, for example by choosing a catalyst that is more selective in one or other of these cuts.
[0132] The catalyst
[0133] The hydroconversion catalyst used in the process according to the invention is a bifunctional hydrocracking catalyst combining an acid function with a hydro-dehydrogenating function and at least one binding matrix. Such catalysts are well known in the field of hydrocracking. Such hydrocracking catalysts are generally classified on the basis of the nature of their acid function, in particular catalysts comprising an amorphous acid function of the silica-alumina type and catalysts comprising a zeolitic cracking function such as zeolite Y or zeolite beta. Hydrocracking catalysts can also be classified according to the major product obtained when they are used in a hydrocracking process (the two main products generally being middle distillates and naphtha in conventional hydrocracking processes dealing with a feedstock of the vacuum distillates or gas oils type).
[0134] The hydroconversion catalyst used in the process according to the invention comprises at least one hydro-dehydrogenating element chosen from the group formed by the non-noble elements of group VIB and group VIII of the periodic table, taken alone or as a mixture, and a porous support which comprises, and is preferably constituted by, a porous mineral matrix and at least one zeolite.
[0135] The hydroconversion catalyst is thio-resistant, at least by the nature of the hydro-dehydrogenating element(s) that it contains. It can thus withstand the presence of sulfur radicals, in particular in the case where steps (a1) and (a2) are implemented in the same reactor.
[0136] Depending on the choice of catalyst, it may be possible to promote hydrotreatment reactions of the heteroatoms contained in the feedstock.
[0137] The hydroconversion catalyst advantageously comprises: - between 0.1% and 50% by weight of said at least one hydro-dehydrogenating element from the group formed by the non-noble elements of group VIB and group VIII, expressed as weight of oxide relative to the total weight of said catalyst; - between 0.1% and 99.9% by weight of a porous support relative to the total weight of said catalyst, said support comprising between 0.1% and 80% by weight of zeolite(s) relative to the total weight of said support, preferably between 2% and 70% by weight, and very preferably between 3 and 60% by weight, and between 0.1% and 99.9% by weight of porous mineral matrix (binder), expressed as weight of oxide relative to the total weight of said support; - between 0 and 20% by weight, and preferably between 0.1% and 20% by weight, of at least one element chosen from the group formed by phosphorus, boron, and silicon, expressed as weight of oxide relative to the total weight of said catalyst (as weight of oxide P2O5 for phosphorus, as weight of oxide B2O3 for boron, and as weight of oxide SiO2 for silicon); - between 0 and 20% by weight of at least one element from group VIIA, preferably between 0.1% and 20%; - between 0 and 20% by weight of at least one element from group VIIB, preferably between 0.1% and 20%, - between 0 and 60% by weight of at least one element from group VB, preferably between 0.1% and 60%, the percentages being expressed as a percentage by weight relative to the total mass of catalyst, the sum of the percentages of the elements constituting said catalyst being equal to 100%.
[0138] The hydro-dehydrogenating function
[0139] The hydroconversion catalyst in step (a2) comprises at least one hydro-dehydrogenating element chosen from the group formed by the non-noble elements of group VIB and group VIII of the periodic table, taken alone or as a mixture.
[0140] Advantageously, the hydroconversion catalyst of the process according to the invention does not contain noble metals, which can make the catalyst sensitive to certain compounds such as sulfur compounds, and harm its activity.
[0141] Preferably, the non-noble elements of group VIII are chosen from iron, cobalt, and nickel, taken alone or in a mixture, and preferably from nickel and cobalt.
[0142] Preferably, the elements of group VIB are chosen from chromium, tungsten and molybdenum, taken alone or in a mixture, and preferably from molybdenum and tungsten.
[0143] The following combinations of metals are preferred: nickel-molybdenum (NiMo), nickel-molybdenum-tungsten (NiMoW), and nickel-tungsten (NiW), and most preferably nickel-molybdenum (NiMo).
[0144] The content of the catalyst in non-noble group VIII element is advantageously between 0 and 20% by weight of oxide relative to the total weight of said catalyst, preferably between 0.5% and 10% by weight of oxide and very preferably between 1% and 8% by weight of oxide.
[0145] The content of the catalyst in group VIB element is advantageously between 1% and 50% by weight of oxide relative to the total weight of said catalyst, preferably between 5% and 40% by weight of oxide, and more preferably between 10% and 35% by weight of oxide.
[0146] Preferably, the hydroconversion catalyst used in the process according to the invention also contains a promoter element chosen from phosphorus, boron, silicon, very preferably phosphorus.
[0147] According to one or more preferred embodiments, the hydroconversion catalyst comprises nickel and molybdenum, and optionally phosphorus.
[0148] When the catalyst contains phosphorus, the phosphorus content is generally less than 15% by weight of P2O5 oxide relative to the total weight of said catalyst, preferably between 0.1% and 10% by weight of P2O5 oxide, and more preferably between 0.2% and 6% by weight of P2O5 oxide.
[0149] The hydroconversion catalyst may also contain at least one element from group VIIA, preferably chosen from chlorine and fluorine.
[0150] The hydroconversion catalyst may further contain at least one element from group VIIB, preferably manganese.
[0151] The hydroconversion catalyst may also contain at least one element from group VB, preferably niobium.
[0152] The catalyst support
[0153] The hydroconversion catalyst in step (a2) comprises a porous support which comprises and is preferably constituted by at least one porous mineral matrix and at least one zeolite.
[0154] Preferably, said zeolite is chosen from 10MR zeolites (zeolite having channels whose opening is defined by a ring with 10 oxygen atoms) or 12MR (zeolite having channels whose opening is defined by a ring with 12 oxygen atoms).
[0155] According to one or more preferred embodiments, the support of the hydroconversion catalyst comprises at least one zeolite chosen from zeolites belonging to the FAU groups (including zeolites X, Y, USY and any other de designation of Y zeolites having undergone a dealumination treatment), BEA, ISV, IWR, IWW, MEI, UWY, MEL, MTW, MTT, MSE, FER or MFI, and preferably, among the zeolites of the FAU or BEA groups. Some examples of zeolites from the preceding families, without restricting the list of possible choices, are cited below: ZSM-5 (MFI), ZSM-11 (MEL), ZSM-12 (MTW), ZSM-23 (MTT), ZSM-35 (FER), ZSM-48 (MRE), CP841E, CP814C, CP811C-300, HSZB25, HSZB30, HSZB150, HSZ931, HSZ940, HSZ980 (BEA), or Y82, Y84, CP300-56, CBV712, CBV720, CBV760, CBV780, CBV500, HSZ320, HSZ330, HSZ331, HSZ385, HSZ350, HSZ360, HSZ390, HSZ341, or HSZ371 (FAU, or USY).
[0156] Preferably the support comprises a USY zeolite and / or a Beta zeolite, alone or as a mixture, and preferably, it comprises and preferably consists of a USY zeolite. All methods of preparing zeolites are capable of being applied to obtaining the zeolites used in the preparation of the catalyst.
[0157] According to one or more embodiments, the support of the hydroconversion catalyst comprises a USY zeolite and a Beta zeolite.
[0158] According to one or more embodiments, the support of the hydroconversion catalyst comprises at least one zeolite chosen from the group formed by the zeolites ZSM-12, IZM-2, ZSM-22, ZSM-23, SAPO-11, ZSM-48, and ZBM-30.
[0159] Said zeolites are advantageously defined in the classification “Atlas of Zeolite Framework Types, 6th revised edition”, Ch. Baerlocher, LB Mc Cusker, DH Oison, 6th Edition, Elsevier, 2007, Elsevier".
[0160] These designations USY, Beta, ZSM-12 etc. are frequent in the literature but they do not restrict the characteristics of the zeolites used in the process of the present invention to such a designation.
[0161] The USY zeolite which can be used in the catalyst support of the process according to the invention advantageously has at least one of the following characteristics:
[0162] - a specific surface area measured by nitrogen physisorption according to the BET method greater than 500 m2 / g, preferably between 600 m2 / g and 1100 m2 / g, even more preferably between 750 m2 / g and 1000 m2 / g,
[0163] - a mesoporous volume of between 0.05 mL / g and 0.9 mL / g, preferably between 0.08 mL / g and 0.7 mL / g and even more preferably between 0.1 mL / g and 0.6 mL / g,
[0164] - has a mesh parameter (which can be measured by X-ray Diffraction according to ASTM 03942-80) between 24.10 Â and 24.70 Â, preferably between 24.15 Â and 24.60 Â, even more preferably between 24.20 Â and 24.56 Â,
[0165] - a Si / Al molar ratio of between 2 and 300, preferably between 2.5 and 150, even more preferably between 2.5 and 100 (characterization possible by semiquantitative X-ray fluorescence for the Si content) and ICP (Induced Coupled Plasma)).
[0166] The Beta zeolite which can be used in the catalyst support of the process according to the invention advantageously has a Si / Al molar atomic ratio of between 5 and 300, preferably between 6 and 200, and more preferably between 6 and 100.
[0167] The Beta zeolite used may also have a specific surface area measured by nitrogen physisorption according to the BET method greater than 500 m2 / g, preferably between 550 m2 / g and 900 m2 / g, even more preferably between 550 m2 / g and 800 m2 / g, and a mesoporous volume between 0.05 mL / g and 0.9 mL / g, preferably between 0.1 mL / g and 0.9 mL / g and even more preferably between 0.15 mL / g and 0.85 mL / g.
[0168] Preferably, the total weight content of zeolite(s) in the support is between 0.1% and 80% by weight relative to the weight of the support of said catalyst, preferably between 2% and 70% by weight and more preferably between 3% and 60% by weight.
[0169] When the support comprises a mixture of a US Y zeolite and a Beta zeolite, the weight ratio of USY relative to Beta is preferably between 1 and 20, more preferably between 1.5 and 18, and even more preferably between 2 and 15.
[0170] The porous mineral matrix used in the catalyst support, also called binder matrix or binder, is advantageously composed of at least one refractory oxide, preferably chosen from the group formed by alumina, silica-alumina, clay, titanium oxide, boron oxide and zirconia, taken alone or as a mixture. Preferably, the porous mineral matrix is chosen from alumina and silica-alumina, taken alone or as a mixture. Even more preferably, the porous mineral matrix is alumina. Alumina can advantageously be in all its forms, known to those skilled in the art. For example, the alumina is selected from the group consisting of alpha, rho, chi, kappa, eta, gamma, theta and delta aluminas, preferably selected from gamma, theta and delta aluminas, and even more preferably is gamma alumina, for example boehmite. In the case where the support comprises alumina, the weight content of alumina in the catalyst support may be between 1% and 99.9% by weight relative to the total weight of said support, preferably between 30% and 98% by weight and even more preferably between 40% and 97% by weight.
[0171] According to one or more embodiments, the support of the hydroconversion catalyst also comprises an amorphous silica-alumina. Such a catalyst support is called a “composite”. These composite supports are known as supports consisting of a mixture of highly acidic zeolite(s), for example USY zeolite, and a moderately acidic amorphous matrix, for example a silica-alumina, and as having intermediate activity and selectivity. The acid function of the catalyst is mainly based on the mixture of zeolite(s) and amorphous silica-alumina of the support. The weight content of amorphous silica-alumina in the support may be between 1% and 99.9% by weight relative to the total weight of said support, preferably between 30% and 98% by weight, and more preferably between 40% and 97% by weight. In the case of the use of such a catalyst with a composite support, the support may also comprise a binder, other than amorphous silica-alumina, and which may be chosen from the group formed by alumina, clay, titanium oxide, boron oxide and zirconia, taken alone or as a mixture, and preferably be alumina. The alumina may advantageously be in all its forms known to those skilled in the art.Very preferably, the alumina is chosen from the group consisting of alpha, rho, chi, kappa, eta, gamma, theta and delta aluminas, preferably chosen from gamma, theta and delta aluminas. In the case where said support comprises alumina, the weight content of alumina in the catalyst support may be between 1% and 70% by weight relative to the total weight of said support, preferably between 2% and 60% by weight and even more preferably between 5% and 50% by weight.
[0172] Preferably, the porous support comprising at least one zeolite advantageously has a total pore volume of between 0.15 cm3.g 'and 1.2 cm3.g', preferably between 0.18 cm3.g 1 and 1.1 cm3.g', and very preferably between 0.2 cm3.g 1 and 1.0 cm3.g'.
[0173] The BET surface area of the support comprising at least one zeolite is advantageously greater than 150 m2.g', preferably between 150 m2.g' and 900 m2.g', very preferably between 180 m2.g' and 850 m2.g', and even more preferably between 200 m2.g' and 800 m2.g'.
[0174] The support is advantageously in the form of irregular and non-spherical beads, extrudates, pellets or agglomerates whose specific shape may result from a crushing step. The support is conventionally of millimetric size, preferably a size between 0.4 mm and 4.4 mm.
[0175] The catalyst may also further comprise at least one organic compound containing oxygen and / or nitrogen and / or sulfur before sulfurization. Such additives are known to those skilled in the art. Generally, the organic compound is chosen from a compound comprising one or more chemical functions chosen from a carboxylic function, alcohol, thiol, thioether, sulfone, sulfoxide, ether, aldehyde, ketone, ester, carbonate, amine, nitrile, imide, oxime, urea and amide or compounds including a furan cycle or sugars.
[0176] The content of organic compound(s) containing oxygen and / or nitrogen and / or sulfur on the catalyst is between 1 and 30% by weight, preferably between 1.5 and 25% by weight, and more preferably between 2 and 20% by weight relative to the weight total catalyst.
[0177] The preparation of the catalyst is known to those skilled in the art and generally comprises a step of impregnation of the metals of group VIII and / or group VIB and optionally of the phosphorus and / or of the organic compound on the support comprising at least one zeolite, followed by drying, then by an optional calcination making it possible to obtain the metals in their oxide forms. Before its use in a process for hydrocracking hydrocarbon fractions, the catalyst is generally subjected to sulfurization in order to obtain the metals in their sulfurized or partially sulfurized forms.
[0178] When an organic compound is present, the catalyst preferably does not undergo calcination during its preparation, i.e. the impregnated catalytic precursor has not been subjected to a heat treatment step at a temperature above 200°C under an inert atmosphere or under an atmosphere containing oxygen, in the presence of water or not.
[0179] The catalyst may alternatively undergo a calcination step during its preparation, i.e. the impregnated catalytic precursor has been subjected to a heat treatment step at a temperature of between 200°C and 1000°C and preferably between 250°C and 750°C, for a duration typically of between 15 minutes and 10 hours, under an inert atmosphere or under an atmosphere containing oxygen, in the presence of water or not.
[0180] An example of a catalyst used in step (a2) comprises, and preferably consists of, at least one group VI metal and at least one non-noble group VIII metal, a USY zeolite and an alumina binder.
[0181] Another example of catalyst used in step (a2) comprises, and is preferably constituted by, nickel, molybdenum, a USY zeolite, optionally in admixture with a Beta zeolite, alumina, and optionally phosphorus. Operation of steps (a1) and (a2)
[0182] Equipment
[0183] Steps (a1) and (a2) can be carried out within the same reactor, or carried out in two separate reactors.
[0184] Preferably, steps (a1) and (a2) are carried out within the same reactor.
[0185] According to one or more embodiments, steps (a1) and (a2) are carried out within the same ebullated bed reactor.
[0186] According to one or more embodiments in which steps (a1) and (a2) are carried out in two separate reactors, steps (a1) and (a2) are carried out in two separate ebullated bed reactors.
[0187] According to one or more embodiments in which steps (a1) and (a2) are carried out in two separate reactors, step (a1) is carried out in a bed reactor bubbling and step (a2) is carried out in a fixed bed reactor.
[0188] Several reactors, arranged in series or in parallel, can be implemented for carrying out step (a1) and / or step (a2).
[0189] When steps (a1) and (a2) are carried out in the same reactor, the hydroconversion is carried out “one pot”, that is to say that the hydroconversion reactions of steps (a1) and (a2) take place concomitantly, in the same reaction medium. Carrying out steps (a1) and (a2) in the same reactor makes it possible in particular to limit the number of pieces of equipment required for the hydroconversion and simplified operation.
[0190] Depending on the embodiment(s) in which steps (a1) and (a2) are carried out in separate reactors, it is possible to use reactors of different technologies, for example for step (a1) a two-phase reactor (gas and liquid) or a three-phase reactor (gas, liquid and solid) of the bubbling bed or slurry type in which the solid phase is not a catalyst but the plastic feedstock, and a three-phase reactor of the fixed bed type for step (a2). In this way, the process has in particular more flexibility as regards the introduction of the plastic feedstock into the first hydroconversion reactor.
[0191] Carrying out steps (a1) and (a2) in two separate reactors also allows more flexibility with respect to the operating conditions, such as the possibility of operating at different pressures, for example with a higher pressure in step (a1) than in step (a2), or at different or differently controlled temperatures, for example with an ebullated bed reactor in step (a1) and a fixed bed reactor in step (a2).
[0192] When steps (a1) and (a2) are carried out in separate reactors, it is possible to provide an intermediate gas / liquid separation between the two steps (a1) and (a2). This separation may have the advantage of using a second reactor, that for step (a2), which is smaller, or operating with a longer residence time. This also has the advantage of being able to use less catalyst, particularly in the case of an ebullated bed reactor.
[0193] Steps (a1) and (a2) of the process according to the invention use reactors, which may be hydroconversion reactors.
[0194] The term "hydroconversion reactor" refers to any vessel in which the hydroconversion of a feedstock is the primary purpose, e.g., cracking the feedstock (i.e., reducing the boiling point range), in the presence of hydrogen and a hydroconversion catalyst. Hydroconversion reactors typically include at least one inlet through which the feedstock and hydrogen may be introduced and at least one outlet from which an upgraded material may be withdrawn. Specifically, hydroconversion reactors are also characterized by possessing sufficient thermal energy to cause the fragmentation of larger molecules into smaller molecules by thermal decomposition. Typically hydroconversion reactors include, but are not limited to, entrained bed reactors, also known as slurry reactors (three-phase reactors - liquid, gas, solid - in which the solid and liquid phases can behave as one homogeneous phase), ebullated bed reactors (three-phase fluidized reactors), moving bed reactors (three-phase reactors with downward movement of solid catalyst and upward or downward flow of liquid and gas), and fixed bed reactors (three-phase reactors with downward flow of liquid feedstock over a fixed bed of supported catalyst with hydrogen typically flowing simultaneously with the liquid, but possibly countercurrently in some cases).
[0195] Step (a1), if carried out in a reactor separate from step (a2), can be carried out in any type of reactor corresponding to the above definition of a hydroconversion reactor, but without catalyst.
[0196] According to one or more embodiments of the invention, the plastic feedstock is introduced into the first hydroconversion reactor by extrusion, and therefore in a substantially liquid form, as described above for the optional step (aO). In these cases, hydroconversion reactors of the fixed bed, moving bed, or bubbling bed type, as mentioned above, can be implemented.
[0197] According to one or more embodiments, step (a2) is carried out in at least one ebullated bed hydroconversion reactor. When steps (a1) and (a2) are carried out in the same reactor, such an ebullated bed reactor is suitable for introducing the plastic filler in substantially liquid form, for example at the end of an extrusion as already mentioned, and is even better suited to cases where the plastic filler is introduced in the form of solid particles, possibly in suspension in a liquid, such as for example described above also for the optional step (a0).
[0198] The ebullated bed hydroconversion reactor comprises the hydroconversion catalyst which is maintained in the reactor. According to one or more embodiments of the invention, one or more hydroconversion reactors, which may be in series and / or in parallel, operating in an ebullated bed, may be used as for the H-Oil™ process, as described, for example, in patents US4521295 or US4495060 or US4457831 or US4354852, in the article Aiche, March 19-23, 1995, Houston, Texas, article number 46d, "Second generation ebullated bed technology", or in chapter 3.5 "Hydroprocessing and Hydroconversion of Residue Fractions" of the book "Catalysis by Transition Metal Sulphides", Technip Editions, 2013. According to these implementations, the reactor is operated in a fluidized bed called a fluidized bed. bubbling. The reactor advantageously comprises a recirculation pump which makes it possible to maintain the porous supported solid hydroconversion catalyst in a bubbling bed by continuously recycling at least a portion of a liquid fraction withdrawn from the upper part of the reactor and reinjected into the lower part of the reactor. The ebullated bed reactor preferably comprises at least one inlet located at or near the bottom of the reactor through which the plastic feedstock is introduced together with the hydrogen, and at least one outlet at or near the top of the reactor through which the conversion products are withdrawn. The reactor preferably further comprises an inlet and an outlet for the supported catalyst in connection with means for injecting and withdrawing the supported catalyst. The bubbling bed reactor further includes an expanded catalyst zone comprising the porous supported catalyst. The bubbling bed reactor also includes a lower supported catalyst-free zone located below the expanded catalyst zone, and an upper supported catalyst-free zone located above the expanded catalyst zone. The feed in the bubbling bed reactor continuously recirculates from the upper supported catalyst-free zone to the lower supported catalyst-free zone by means of a recycle conduit in communication with a boiling pump. At the top of the recycle conduit is preferably a funnel-shaped recycle cup through which the feed is drawn from the upper supported catalyst-free zone. The internal recycled feed is mixed with "fresh" feed and additional hydrogen gas. The catalyst injection and withdrawal means allow for continuous replacement of the supported catalyst, which is one of the advantages of ebullated bed technology, compared to other types of reactors, for example fixed bed, for which a reactor shutdown may be required to replace the spent catalyst (deactivated mainly by deposition of metals contained in the feedstock, for example in the form of vanadium sulfide and nickel sulfide, and by coke deposition). The spent catalyst, withdrawn from the reactor, can be sent to a regeneration zone in which the carbon and sulfur it contains are removed. It is also possible to send the spent catalyst withdrawn from the reactor to a rejuvenation zone in which the majority of the deposited metals are removed, before sending the spent and rejuvenated catalyst to a regeneration zone in which the carbon and sulfur it contains are removed.The regenerated or rejuvenated catalyst can then be reintroduced into the reactor, possibly in association with fresh catalyst, by the catalyst injection means. This withdrawal and this addition of catalyst. can be done for example on a daily basis. Typically, the means for injecting and withdrawing the supported catalyst comprise at least one conduit opening into the supported catalyst expansion zone of the reactor for the introduction of fresh (and / or regenerated and / or rejuvenated) supported catalyst into the supported catalyst expansion zone of the reactor and the withdrawal of spent catalyst from said zone. The introduction and withdrawal can be done with the same conduit, or via separate conduits, then requiring at least two conduits, an injection conduit for the injection of supported catalyst into the reactor and a conduit for the withdrawal of spent catalyst. By this continuous replacement of the catalyst, the ebullated bed technology ultimately makes it possible to increase the time between two shutdowns of the conversion process.
[0199] The ebullated bed hydroconversion reactor, because the supported catalyst is kept stirring by significant liquid recycling, has a pressure drop across the reactor which remains low and constant, and the reaction exotherms are quickly averaged over the catalytic bed, which is therefore almost isothermal and does not require the injection of cooling flows ("quenches" in English).
[0200] Operating conditions
[0201] The hydroconversion process according to the invention is carried out in each reactor or in the single reactor at an absolute pressure of between 1 MPa and 38 MPa, at a temperature greater than or equal to 200°C and less than 400°C, at an hourly space velocity (“WH” for hourly volume velocity, commonly called “LHSV” for “Liquid Hourly Space Velocity” in English) relative to each reactor, of between 0.05 h 1 and 10 h 1, and with a quantity of hydrogen of between 50 NmVm3 and 5000 NmVm3.
[0202] It is understood that the temperature at these steps is the temperature at the start of the operation, also called the “start of run” (in English terminology), when an implementation comprising a fixed bed is operated. In the case of other types of reactor, for example a bubbling bed reactor, there is no notion of start of run temperature, because the temperature is substantially constant during the operation. However, it can be considered that the operating temperature given for these steps (a1) and (a2) is in all cases the temperature at the start of the operation, which for example in the case of the bubbling bed reactor remains the same during the operation.
[0203] In the case of a fixed bed reactor, the WH is generally expressed as the ratio of the volume flow rate of feedstock, preferably liquid, to the volume of catalyst loaded into the reactor, taken under standard conditions of temperature and pressure. In the case of an ebullated bed reactor, the WH is generally expressed as the ratio of the volume flow rate of feedstock, preferably liquid, to the volume of the reactor, taken under standard conditions of temperature and pressure.
[0204] The two steps (a1) and (a2) are therefore implemented under the conditions mentioned above.
[0205] According to one or more embodiments, steps (a1) and (a2) are implemented: - at an absolute pressure between 2 MPa and 25 MPa, preferably between 3 and 20 MPa, - at a temperature greater than or equal to 250°C and less than 400°C, preferably greater than or equal to 300°C and less than 400°C, more preferably greater than or equal to 320°C and less than 400°C, more preferably greater than or equal to 330°C and less than 390°C, for example 380°C, - at an hourly space velocity relative to each reactor of between 0.1 h 1 and 10 h 1, preferably between 0.1 h 1 and 5 h 1, - with a quantity of hydrogen between 50 NmVm3 and 5000 Nm3 / m3, preferably between 100 Nm3 / m3 and 2000 Nm3 / m3 and very preferably between 200 Nm3 / m3 and 1000 Nm3 / m3.
[0206] According to one or more other embodiments, at least one ebullated bed reactor is used to implement step (a1) or steps (a1) and (a2), operated at an hourly space velocity, relative to the volume of each reactor, of between 0.15 h 1 and 2 h *, and even more preferably between 0.15 h 1 and 1 h 1
[0207] According to one or more other embodiments, at least one ebullated bed reactor is used to implement step (a1) or steps (a1) and (a2), and the overall WH, i.e. the liquid feed flow rate in step (a1) taken under standard temperature and pressure conditions, relative to the total volume of the reactors of steps (a1) and (a2), is between 0.05 h 1 and 0.09 h 1.
[0208] The relatively low temperature operation, below 400°C, allows the process to be economical in terms of energy and operating and investment costs, particularly in comparison with other higher temperature hydroconversion processes or other technologies such as pyrolysis. Examples
[0209] The examples below aim to show certain performances of the method according to the invention, in comparison with methods according to the prior art.
[0210] Examples 1 to 4 are not in accordance with the invention. Examples 5 and 6 are in accordance with the invention.
[0211] In the examples below, a plastic filler of polypropylene (Weight mo average molecular mass by weight Mw=456000 Da and average molecular mass by number Mn=76800 Da) is introduced in the form of solid particles into an autoclave reactor, also called below “batch” reactor.
[0212] The operating conditions are as follows:
[0213] reaction temperature 380°C,
[0214] partial pressure H2: 7 MPa,
[0215] test duration: 150 minutes,
[0216] stirring speed: 1400 rpm
[0217] Procedure for all the examples below: the batch reactor is loaded with the plastic feedstock, the catalyst previously activated by a sulfurization procedure as known to those skilled in the art, and the DMDS, when they are used. The reactor is closed, purged with nitrogen and purged with hydrogen, then pressurized with hydrogen to a pressure of approximately 3 MPa. The reactor is then heated to the test temperature. Stirring is activated from 300°C. When the reaction temperature is reached, the pressure in the reactor is instantly adjusted to the target value by adding H2. At this time, the reaction time is counted. At the end of the experiment duration, the reactor is cooled rapidly to stop the reaction and stirring is stopped. The liquid and gaseous effluents are recovered and separated from any unconverted solid products.
[0218] The results regarding the conversion products and hydroconversion performances are summarized in Table 1 below.
[0219] Example 1: Hydroconversion process without a source of sulfur radicals and without a catalyst (non-compliant)
[0220] Without the addition of a source of sulfur radicals or catalyst, no conversion of the plastic load is observed: 100% of the plastic load is solid at the end of the test.
[0221] Example 2: Hydroconversion process with a 4% weight S sulfur radical source and without catalyst (non-compliant)
[0222] In this example 2, the source of sulfur radicals which is DMDS, is added in the proportion of 4% by weight of sulfur relative to the weight of the plastic filler. A conversion of the plastic filler of 93.5% relative to the filler (yield in non-solid products) is observed, with a yield in liquid products of 93% by weight relative to the filler.
[0223] The product yield and composition of the liquid products are given in Table 1.
[0224] Example 3: Hydroconversion process without a source of sulfur radicals and with a Cl catalyst (non-compliant)
[0225] Catalyst Cl is in a mass proportion of 10% catalyst relative to the charge. Catalyst Cl is a catalyst composed of 16.2% by weight of MoO3 and 2.9% weight of NiO relative to the catalyst on a support comprising 30% by weight of a USY zeolite with a mesh parameter of 24.37 Å in an alumina matrix, relative to the support.
[0226] We obtain a conversion of the plastic charge of 7% compared to the charge, with in addition all of the liquid products belonging to an extra heavy cut with an initial boiling point greater than or equal to 740°C.
[0227] The product yield and composition of the liquid products are given in Table 1.
[0228] Example 4: Hydroconversion process with a 1% weight S sulfur radical source and a Cl catalyst (non-compliant)
[0229] The catalyst Cl is in a mass proportion of 10% catalyst relative to the charge.
[0230] In this example 4, the source of sulfur radicals which is DMDS, is added in the proportion of 1% by weight of sulfur relative to the weight of the plastic filler.
[0231] A conversion of the plastic charge is observed with a low yield of liquid products, of 58% by weight relative to the charge, with in addition all of the products belonging to an extra heavy cut with an initial boiling point greater than or equal to 740°C.
[0232] The product yield and composition of the liquid products are given in Table 1.
[0233] Example 5: Hydroconversion process with a 4% weight S sulfur radical source and a Cl catalyst (compliant)
[0234] The catalyst Cl is in a mass proportion of 10% catalyst relative to the charge.
[0235] In this example 5, the source of sulfur radicals which is DMDS, is added in the proportion of 4% by weight of sulfur relative to the weight of the plastic filler.
[0236] A conversion of the plastic charge is observed with a yield of non-solid products of 96% by weight relative to the charge, including a yield of liquid products of 93% by weight and a yield of gaseous products of 3% by weight.
[0237] Compared to example 2 with the same source of sulfur radicals, in the same proportion, but without catalyst, the following differences are noted on the following cuts: -16 percentage points of heavy products (370°C-740°C), +3 percentage points of diesel cut (250°C-370°C), +9 percentage points in kerosene (150°C-250°C), +4 percentage points in naphtha (80°C-150°C), showing more selectivity towards the diesel, kerosene and naphtha cuts, which can be more easily recovered.
[0238] Compared to example 3 without a source of sulfur radicals but with catalyst Cl, we note a much higher conversion and the following differences on the sections following: -76 percentage points of extra-heavy products with an initial boiling point greater than or equal to 740°C and +76 percentage points of products with a final boiling point less than 740°C (including recoverable cuts).
[0239] The product yield and composition of the liquid products are given in Table 1.
[0240] Example 6: Hydroconversion process with a 4% weight S sulfur radical source and a C2 catalyst (compliant)
[0241] Catalyst C2 is in a mass proportion of 10% catalyst relative to the charge.
[0242] Catalyst C2 is a catalyst composed of 20% by weight of MoO3 and 3.8% by weight of NiO by mass relative to the catalyst on a support comprising 16% by weight of a US Y zeolite with a mesh parameter of 24.37 Å and 6% by weight of a beta zeolite with a Si / Al molar ratio of 27 in an alumina matrix, relative to the support.
[0243] In this example 6, the source of sulfur radicals which is DMDS, is added in the proportion of 4% by weight of sulfur relative to the weight of the plastic filler.
[0244] A conversion of the plastic charge is observed with a yield of non-solid products of 98% by weight relative to the charge, including a yield of liquid products of 86% by weight and a yield of gaseous products of 12% by weight.
[0245] Compared to example 2 with the same source of sulfur radicals, in the same proportion, but without catalyst, the following differences are noted on the following cuts: -44 percentage points of very heavy products (540°C+), -2 percentage points in heavy products (370°C-540°C), +6 percentage points of diesel cut (250°C-370°C), +16 percentage points in kerosene (150°C-250°C), +13 percentage points in naphtha (80°C-150°C), showing more selectivity towards the kerosene and naphtha cuts, which can be more easily recovered.
[0246] Compared to Example 5 with the same source of sulfur radicals, in the same proportion, but with a different catalyst, it is noted that the conversion into non-solid products is just as good, that the quantity of gas produced, although greater, remains acceptable compared to the liquid products, and that the selectivity is greater in light cuts (540°C-), in particular in kerosene cuts (150°C-250°C) and naphtha (80°C-150°C).
[0247] The product yield and composition of the liquid products are given in Table 1.
[0248] Table 1 below presents a summary of the main data, including the product yield and the composition of the liquid products of the examples described.
[0249] [Tables 1] Ex.l Ex.2 Ex. 3 Ex. 4 Ex. 5 Ex. 6 Sulfur radical source - DMD S - DMD S DMD S DMD S S content relative to the charge (% mass) - 4 - 1 4 4 Catalyst - - Cl Cl Cl C2 Catalyst ratio relative to the charge (% mass) - - 10 10 10 10 Product yield (% mass) gas - 0.5 3 4 3 12 liquid - 93 5 58 93 86 solid 100 6.5 92 38 4 2 Composition of liquid products by boiling point range in °C (% mass) PI-80 - 1 - - 2 8 80-150 - 3 - - 7 16 150-250 - 4 - - 13 20 250-370 - 6 - - 9 12 370-540 - 18 - - 11 20 540-740 - 46 - - 35 8 740+ - 22 100 100 24 16
Claims
Claims
1. A process for hydroconversion of a plastic filler comprising the following steps: (al) a step of non-catalytic hydroconversion of said filler in the presence of hydrogen, in contact with a source of radicals, said source comprising sulfur and being introduced in such a way that the sulfur content is between 3% and 20% by weight relative to the weight of the plastic filler, to produce first conversion products;(a2) a step of catalytic hydroconversion of the first conversion products in the presence of hydrogen, in contact with at least one hydroconversion catalyst, said hydroconversion catalyst comprising at least one hydro-dehydrogenating element chosen from the group formed by the non-noble elements of group VIB and group VIII of the periodic table, taken alone or as a mixture, and a porous support comprising a porous mineral matrix and at least one zeolite, said steps (a1) and (a2) being carried out at an absolute pressure of between 1 MPa and 38 MPa, at a temperature greater than or equal to 200°C and less than 400°C, at an hourly space velocity relative to each hydroconversion reactor of between 0.05 h 1 and 10 h 1, and with a quantity of hydrogen of between 50 NmVm3 and 5000 Nm3 / m3;
2. 111. Hydroconversion process according to claim 1, in which steps (a1) and (a2) are carried out within the same reactor.
3. Hydroconversion process according to claim 2, in which steps (a1) and (a2) are carried out within the same ebullated bed reactor.
4. A hydroconversion process according to claim 1, wherein steps (a1) and (a2) are carried out in two separate reactors, preferably steps (a1) and (a2) being carried out in two separate ebullated bed reactors or step (a1) being carried out in one ebullated bed reactor and step (a2) being carried out in one fixed bed reactor.
5. Hydroconversion process according to any one of the preceding claims, in which said at least one zeolite of the support of the hydroconversion catalyst is chosen from the list consisting of zeolites of FAU groups, preferably zeolites of FAU group chosen from zeolites X, Y, USY, Y having undergone a treatment of dealumination, BEA, ISV, IWR, IWW, MEI, UWY, MEL, MTW, MTT, MSE, FER and MFI, and preferably, said at least one zeolite is chosen from zeolites of the FAU or BEA groups.
6. A hydroconversion process according to any preceding claim, wherein the catalyst support comprises a USY zeolite and / or a Beta zeolite.
7. A hydroconversion process according to any one of the preceding claims, wherein the hydroconversion catalyst support comprises at least one zeolite selected from the group consisting of zeolites ZSM-12, IZM-2, ZSM-22, ZSM-23, SAPO-11, ZSM-48, and ZBM-30.
8. Hydroconversion process according to any one of the preceding claims, in which the hydroconversion catalyst comprises: - between 0.1% and 50% by weight of said at least one hydro-dehydrogenating element from the group formed by the non-noble elements of group VIB and group VIII, expressed as weight of oxide relative to the total weight of said catalyst; - between 0.1 and 99.9% by weight of a porous support relative to the total weight of said catalyst, said support comprising between 0.1% and 80% by weight of zeolite relative to the total weight of said support, and between 0.1% and 99.9% by weight of a porous mineral matrix expressed as weight of oxide relative to the total weight of said support; - between 0 and 20% by weight, and preferably between 0.1% and 20% by weight, of at least one element chosen from the group formed by phosphorus, boron, and silicon, expressed as weight of oxide relative to the total weight of said catalyst;- between 0 and 20% by weight of at least one element from group VIIA, preferably 0.1 to 20%; - between 0 and 20% by weight of at least one element from group VIIB, preferably 0.1 to 20%, 0 to 60% by weight of at least one element from group VB, preferably 0.1 to 60%; the percentages being expressed as a percentage by weight relative to the total mass of catalyst, the sum of the percentages of the elements constituting said catalyst being equal to 100%.;
9. A hydroconversion process according to any one of the preceding claims, wherein the hydroconversion catalyst comprises a porous mineral matrix consisting of at least one refractory oxide selected from the group consisting of alumina, silica-alumina, clay, titanium oxide, boron oxide and zirconia, taken alone or in mixture, and preferably the porous mineral matrix is alumina.
10. A hydroconversion process according to any one of the preceding claims, wherein the hydroconversion catalyst comprises, as hydro-dehydrogenating elements, at least one non-noble group VIII metal selected from nickel and cobalt, preferably nickel, and at least one group VIB metal selected from molybdenum and tungsten, preferably molybdenum.
11. A hydroconversion process according to any one of the preceding claims, wherein the source of radicals comprising sulfur is selected from the list consisting of H2S, elemental sulfur, carbon disulfide (CS2), dimethyl sulfide (DMS), dimethyl sulfoxide (DMSO), diethyl sulfide (DES), dimethyl disulfide (DMDS of formula (CH3S)2), mercaptans, polysulfides such as di-tert-nonyl polysulfide, taken alone or as a mixture, and preferably is selected from H2S, DMS, DMDS, and DES.
12. Hydroconversion process according to any one of the preceding claims, wherein the sulfur content in step (al) is between 3% and 15% by weight relative to the weight of the plastic feedstock, preferably between 3% and 10% by weight of the feedstock.
13. Hydroconversion process according to any one of the preceding claims, further comprising: (aO) a prior step of conditioning said feedstock for its introduction into a reactor in which at least the first step (a1) is carried out, said step (aO) comprising: - sending the plastic feedstock in the form of solid particles into an extruder, preferably with a plastic diluent, in which it is gradually heated to a temperature above the melting temperature of said plastic feedstock, and put under the pressure of the first hydroconversion reactor, during conveying, and - introducing the extruded plastic feedstock into said reactor.
14. A hydroconversion process according to any one of the preceding claims, wherein the plastic filler is in solid form and comprises one or more polymers selected from the list consisting of alkene polymers, diene polymers, vinyl polymers, and styrenic polymers, polyesters, and polyamides, and preferably said plastic filler comprises at least 50% by weight of polyolefins relative to the total weight of the plastic filler, said polyolefins preferably being chosen from the list consisting of polyethylene, polypropylene and / or copolymers of ethylene and propylene.
15. A hydroconversion process according to any one of the preceding claims, wherein said steps (a1) and (a2) are carried out at an absolute pressure of between 2 MPa and 25 MPa, and at a temperature greater than or equal to 300°C and less than 400°C.