METHOD FOR MANUFACTURING A PART FROM A THERMOSTATABLE MATRIX COMPOSITE MATERIAL REINFORCED BY LONG DISCONTINUOUS FIBERS

FR3141378B1Active Publication Date: 2024-10-25SAFRAN SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2022011136
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-10-26
Publication Date
2024-10-25
Estimated Expiration
2042-10-26

Smart Images

  • Figure 00000011_0000
    Figure 00000011_0000
  • Figure 00000011_0001
    Figure 00000011_0001
  • Figure 00000012_0000
    Figure 00000012_0000
Patent Text Reader

Abstract

The invention relates to a method for manufacturing a part made of a thermosetting matrix composite material reinforced with long discontinuous fibers, comprising the following steps: assembly (S2) of long discontinuous fiber webs impregnated with a thermosetting polymer in a mold at a temperature between 0°C and 60°C to form a complex preform; closing the mold (S3); applying a heating cycle (S4) to the mold to reduce the viscosity of the thermosetting polymer, the maximum temperature difference between any two points in the mold being less than or equal to 15°C; applying pressure (S5) to the mold when the viscosity of the thermosetting polymer is between 10 and 1000 Pa·s. Figure for the abstract: Fig. 3
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: METHOD FOR MANUFACTURING A PART MADE OF A COMPOSITE MATRIX MATERIAL WITH A THERMO-MATRIX HARDENABLE REINFORCED BY LONG DISCONTINUOUS FIBERS Technical field

[0001] The present disclosure relates to a method for manufacturing a part made of a thermosetting matrix composite material reinforced with long discontinuous fibers. Prior art

[0002] The manufacture by thermocompression of parts made of composite material with discontinuous long fibers or DLF (acronym known in English terminology as "Discontinuous Long Fibers") is known and generally requires heating the material and applying pressure to it in order to consolidate the material. Long fibers are generally fibers having a length ranging from 5 to 60 mm. The term DLF is used to designate composite assemblies formed from a matrix and discontinuous long fibers.

[0003] Conventionally, the material, in particular with a thermosetting matrix, is introduced into a tool which has been previously heated, in order to minimize the manufacturing cycles.

[0004] Pre-curing may also be carried out on the material before inserting it into the tool in order to minimize the viscosity of the resin during the pressurization phase in the tool and, thus, to avoid expelling the resin from the tool during this phase.

[0005] When the composite material parts to be manufactured are of complex shapes and / or have numerous folds, handling the preforms to arrange them in the manufacturing mold turns out to be a delicate operation, whether this operation is carried out manually or robotically.

[0006] In particular, the positioning in the mold of the different constituent elements of a preform is a long and delicate task since it is necessary to position the different elements precisely one after the other. When the first preform elements are placed in the mold and other preform elements are being positioned, the resin already begins to polymerize on the first elements placed in place.

[0007] This phenomenon can impact the smooth running of the thermocompression manufacturing process to the extent that, to manufacture a good quality part, the progress level (degree of polymerization) / viscosity of the resin when applying pressure must be precisely controlled.

[0008] In particular, the manufacture of parts with complex shapes and / or which include numerous folds will cause a gradient in the advancement / viscosity of the resin during manufacture in the mold. Statement of the invention

[0009] In view of the above, it would therefore be interesting to design a method making it possible to remedy at least in part the drawbacks set out above during the manufacture of a part made of composite material with a thermosetting matrix reinforced by long discontinuous fibres.

[0010] To this end, the present disclosure relates to a method for manufacturing a part made of thermosetting matrix composite material reinforced by long discontinuous fibers, comprising the following steps: - assembly of sheets of long discontinuous fibers impregnated with a thermosetting polymer in a mold at a temperature between 0°C and 60°C to form a complex preform; - closing the mold; - application of a heating cycle to the mold in order to reduce the viscosity of the thermosetting polymer, the maximum temperature difference between any two points of the mold being less than or equal to 15°C; - application of pressure in the mold when the viscosity of the thermosetting polymer is between 10 and 1000 Pa.s.

[0011] Such a method makes it possible to produce by thermocompression parts of complex shapes which are difficult to demould, without there being a thermal gradient in the preform of these parts during the moulding. In particular, the manufacture begins with a complex preform (the shape of the preform is complex in the sense that it is a preform which cannot be inserted into an already hot tool in a limited number of operations or in a limited time; it is generally not a simple geometric shape in three dimensions such as a sphere, a cube, a parallelepiped, etc.) in a cold mould. It will be noted that a complex preform can, for example, be composed of several independent parts or a preform whose shape with respect to the mould would prevent its insertion in a single block.The manufacturing process continues with a rise in temperature of the mold in order to reduce the viscosity of the thermosetting polymer, thus making it possible to control the pressure of the material in the mold according to the rheokinetic profile. In other words, the application of pressure is carried out from a predetermined viscosity value, which leads to controlled fine-tuning of the material in the mold, allowing . thus obtaining homogeneous material properties throughout the thickness of the material and by area and which are stable. The advantage of discontinuous fibers is their ability to flow in the tooling. A precise preform is therefore not necessary. However, the finishing can be controlled by applying pressure to the material when the latter has the right level of viscosity so as not to shear the material or separate the fibers from the resin (thermosetting polymer). It should be noted that it is possible to have preform elements assembled outside the tooling and then introduced into the tooling to form the preform.

[0012] According to other possible characteristics, taken individually or in combination: - the pressure is applied when the viscosity of the thermosetting polymer is less than or equal to 500 Pa.s, preferably less than or equal to 100 Pa.s; -the method comprises a step of pre-polymerization of the thermosetting polymer in order to increase the minimum viscosity of the thermosetting polymer; - the sheets of long discontinuous fibers comprise fibers with a length greater than or equal to 10 mm; - the sheets of long discontinuous fibers are carbon, glass or aramid fibers; - the thermosetting polymer is chosen from an epoxy, polyurethane, polyester, phenolic, BMI (polybismaleimide) resin; - the maximum temperature of the heating cycle is greater than or equal to 150°C, preferably greater than or equal to 180°C; - the applied pressure ranges from 20 to 200 bars; -the complex preform comprises an assembly in the mold of several elements which each result from the prior assembly outside the mold of sheets of long discontinuous fibers impregnated with a thermosetting polymer. Brief description of the drawings

[0013] Other characteristics and advantages of the subject of the present disclosure will emerge from the following description of embodiments, given as non-limiting examples, with reference to the appended figures.

[0014] [Fig-1] [Fig.l] is a general perspective view of an example of a part of complex shape which can be produced by a manufacturing method according to an embodiment of the invention;

[0015] [Fig.2A] [Fig.2A] is a schematic general view of an installation for manufacturing a part made of composite material of complex shape according to one embodiment of the invention;

[0016] [Fig.2B] [Fig.2B] is a schematic general view similar to that of [Fig.2A] and showing a different means of applying differentiated pressure;

[0017] [Fig.2C] [Fig.2C] is a schematic general view similar to that of [Fig.2A] and showing another different means of applying differentiated pressure;

[0018] [Fig.3] [Fig.3] is a flowchart representing the steps of a fa process fabrication of a part made of composite material of complex shape according to an embodiment of the invention;

[0019] [Fig.4] [Fig.4] is a graph illustrating the evolution with temperature of the viscosity of an epoxy resin with and without pre-curing. Detailed description

[0020] The invention finds a particularly interesting application in the manufacture by thermocompression of parts made of composite material of complex shapes with a thermosetting matrix reinforced by long discontinuous fibers.

[0021] Such parts can be applied in many industrial sectors such as aeronautics, automobiles, railways, etc. More particularly, the parts that can be manufactured can be applied to aircraft engines, landing gear or nacelles and can, for example, be flow straighteners, cowlings, thrust reverser grilles, acoustic panels, structural panels, etc.

[0022] [Fig. 1] is a general schematic perspective view from above of a thrust reverser grid 10 of an aircraft reactor capable of being manufactured by a manufacturing method according to an embodiment of the invention which will be described below.

[0023] The grid G ​​generally comprises a plurality of parallel spars L, spaced apart from each other and connected to each other by vanes or fins A which each extend transversely between two consecutive spars. The fins are spaced longitudinally from each other between two consecutive spars so as to provide, in the space formed between the spars and the fins, cavities through which a flow of thrust reversing air can flow when the grid is put into operation. The grid comprises two upstream flanges B1 and downstream B2 respectively arranged at its two opposite longitudinal ends and used to mount the grid on the nacelle of the reactor.

[0024] As shown in [Fig.2A] and designated by the general reference 10, an installation for manufacturing composite material parts of complex shapes according to an embodiment of the invention will now be described. For reasons of simplicity, the part which will be manufactured in the installation according to the aforementioned method has a complex shape but which is however simpler than that of the grid G ​​of [Fig.l]. A preform shape is complex in the sense that it is a preform which cannot be inserted into an already hot tool in a limited number of operations or in a limited time as already mentioned above. Generally speaking, it is a shape which, by definition, is not a simple geometric shape such as a sphere, a cube, a parallelepiped, etc. On the contrary, a complex shape is a shape whose projection in at least one plane includes, for example, at least one concavity or re-entrant portion (re-entrant angle) in the surface formed by its contour. The part may also have such a projection in several planes. It should be noted that the descriptions of the installation and the process which follow obviously apply to any part of complex shape.

[0025] The installation 10 comprises a mold comprising two parts, namely an upper tool or cover 12 and a lower tool or cover 14 (for a tool used to produce a grid like that of [Fig. 1], the tool further comprises two parts movable in the plane of the grid). Each of the tools comprises an internal surface which is shaped in a suitable manner so that, when the two tools are brought against each other as in [Fig. 2A] and the mold is thus closed, the two internal surfaces facing the two tool parts which each have a relief form, together, the contour or the envelope of a closed cavity 15 internal to the mold and which will house the part to be manufactured. The contour of the cavity defines the external contour of the future part.

[0026] In the example illustrated in [Fig.2A], the part has a section along a view in a plane X, Z which has the general appearance of a lying T whose bar 16 is arranged substantially vertically (along the Z axis) and whose leg 18 is arranged substantially horizontally. It will be noted that the leg 18 is not, however, rectilinear and is slightly curved with its free end 18a raised upwards (in the direction of the tool 12) and a central part 18b directed downwards (in the direction of the tool 14). The part also extends along a third direction Y perpendicular to the plane of [Fig.2A] while retaining, for example, the general shape of the section illustrated in [Fig.2A]. However, the appearance of the part along the Y direction can also adopt a complex shape.

[0027] The two mold parts (upper and lower tools) are arranged here along a vertical axis Z, one above the other. However, other spatial arrangements can be envisaged and, for example, an arrangement in which the two mold parts are arranged along a horizontal axis (the arrangement of [Fig.2A] is rotated by 90°).

[0028] The installation 10 also comprises two heating elements 20 and 22 which are in the form of heating plates, one upper 20 arranged above the upper tool 12 and in contact with the latter in order to optimize the heat transfer between these two elements, and the other lower 22, arranged below the lower tool 14 and in contact with the latter for the same reasons. The di dimensions along the longitudinal axis X of the heating plates are here greater than the dimensions of the tools because the heating plates are generally those of the press used for compression.

[0029] A compression device along the Z axis which is conventionally used in this type of installation is part of the installation 10 (press mentioned above and of which the heating plates are part) and is used to apply, at the appropriate moment, an axial pressure to the material present in the cavity 15. Other compression devices along other axes can also be used. Figures 2B and 2C respectively illustrate different means of applying differentiated pressure: in [Fig.2B] the axes along which the pressures are applied are different (here perpendicular to each other) whereas in [Fig.2C] the compression axes are parallel.

[0030] The method of manufacturing the part according to an embodiment of the invention is shown in [Fig. 3] in the form of a flowchart and begins with a first step S1 of opening the mold. In practice, one of the tools, in particular the upper tool 12, is moved away from the lower tool 14 along the Z axis to allow access to the bottom of the cavity which is arranged here in the lower tool 14.

[0031] During this step the mold is "cold" in the sense that it is only at a temperature lower than the temperature permitted for manual handling and which does not cause rapid evolution of the resin (polymerization). In the present case, it is for example heated and the temperature of the mold is, for example, limited to 60°C.

[0032] During the following step S2, long discontinuous fibers, for example carbon (alternatively glass or aramid), impregnated with a thermosetting polymer such as a thermosetting resin, for example an epoxy resin, are positioned inside the cavity 15 of the mold so as to line the bottom of the cavity by matching the walls (internal surfaces of the tools) of the latter which form its contour. During this step, in practice, an assembly is carried out in the mold, in one or more layers, of sheets of these impregnated long discontinuous fibers to form a complex preform. These sheets are for example obtained by cutting from a roll of impregnated long discontinuous fibers.Given the mold temperature (0-60°C), the thermosetting polymer of the first layers placed in the mold is not likely to start to polymerize during this stage while all the layers have not yet been assembled. It should be noted that the materials in the layer have a certain mechanical strength. It is therefore possible to arrange the tooling blocks around the preform, particularly above it. The assembly is introduced under a press plate which positions the assembly.

[0033] It is also possible to have a simplified preform on one of the faces (the face su upper) and rely on the flow of the material to conform the shapes on the upper part

[0034] Alternatively, elements or parts of the preform can be shaped or assembled outside the mold (each element or part is previously formed by assembling outside the mold sheets of long discontinuous fibers impregnated with a thermosetting polymer) and then introduced therein in order to consolidate / assemble these elements or parts together and thus constitute the desired preform.

[0035] When this step is completed, the upper tool 12 can come into contact with the lower tool 14 (by descending according to an appropriate descent command) along a predefined joint plane in order to close the mold (step S3). In Figure 2, the mold is in the closed position.

[0036] During the following step S4, a heating cycle is applied to the mold via the heating plates 20, 22 in order to reduce the viscosity of the thermosetting polymer to a desired value. A predetermined temperature rise profile (temperature rise ramp in °C per minute) which may include one or more stages is applied to heat the tools 12, 14 and the internal cavity 15 in a suitable manner. The temperature profile and the temperature values ​​applied are predetermined (knowing the shape of the part to be manufactured, the temperature rise profiles and the temperature values ​​are obtained empirically by prior tests carried out on parts of different shapes) and the heating profile can be stopped or modified; for example the heating temperature can be maintained at a stage value.Alternatively, it is possible to introduce into the heating process a temperature setpoint higher than the expected temperature, for example a setpoint of 200°C for 180°C for an example of resin illustrated in [Fig.4] and the setpoint is reset to the value of 180°C when the thermocouple(s) used in the installation approach this value.

[0037] Alternatively, a self-heating mold can be used instead of heating plates. Such a mold can use a heat transfer fluid, induction technology (for example from the company Roctool), or pulsed air technology (for example PTFS type from the company Surface Génération).

[0038] When the temperature of the resin in the cavity 15 reaches the desired temperature, the resin is softened but nevertheless remains sufficiently viscous to be subjected to external pressure and to flow in a controlled manner inside the cavity without risking being forced out of the cavity under the effect of this pressure.

[0039] For example, the viscosity of the resin is between 10 and 1000 Pa.s so that it can be subjected in a controlled manner to external pressure. Preferably, the viscosity of the resin is less than 500 Pa.s, or even less than 100 Pa.s.

[0040] The heating cycle implemented is such that the maximum temperature difference between any two points of the mold is less than or equal to 15°C. This allows pressure to be applied to a resin in a controlled state of progress / viscosity and therefore similar in each zone in which the pressure is applied. If this value is exceeded, it would be possible to obtain points with a viscous resin.

[0041] During the following step S5, pressure is applied to the material present in the mold, via the aforementioned pressurizing device when the viscosity of the thermosetting polymer is between 10 and 1000 Pa.s. The application of the pressure is dependent on the thermal properties of the tooling via the rheokinetic profile. The pressure is applied for viscosities, preferably, less than 500 Pa.s, or even less than 1000 Pa.s in the descent or rise of the minimum viscosity.

[0042] If the pressure is applied before reaching the minimum viscosity, it is preferable to carry out a pre-curing (pre-polymerization) in order to increase the value of the minimum viscosity and to make the material (fibers + resin) flow into the cavity. If the viscosity of the resin drops too much after the pressure has been applied, there is a risk of expelling the resin and thus having areas too rich in fibers.

[0043] [Fig.4] represents two viscosity curves of the same epoxy resin (e.g. HexMC® material from Hexcel with an 8552 resin), one C1 without pre-curing of the resin and the other C2 with pre-curing for 10 minutes at a temperature of 180°C (maximum 190°C). As an example, a temperature rise profile of 10°C / min is applied.

[0044] Since the rise in the viscosity value is relatively rapid after passing the viscosity minimum, it is useful to reduce the ramp by modifying the temperature (for example using an intermediate level or by controlling the heating plates).

[0045] In practice, the pressure application device is controlled by the heating plates 20 and 22 so that the application of pressure by the device is controlled when the temperature rise profile of the heating plates reaches a predetermined value.

[0046] Although the present disclosure has been described with reference to a specific exemplary embodiment, it is obvious that various modifications and changes may be made to these examples without departing from the general scope of the invention as defined by the claims. Furthermore, individual features of the various embodiments recited may be combined in additional embodiments. Therefore, the description and drawings should be considered in an illustrative rather than restrictive sense.

Claims

Claims

1. Method for manufacturing a part made of a composite material with a thermosetting matrix reinforced by long discontinuous fibers, comprising the following steps: - Assembling (S2) sheets of long discontinuous fibers impregnated with a thermosetting polymer in a mold at a temperature between 0°C and 60°C to form a complex preform; - closing the mold (S3); - applying a heating cycle (S4) to the mold in order to reduce the viscosity of the thermosetting polymer, the maximum temperature difference between any two points of the mold being less than or equal to 15°C; - applying a pressure (S5) in the mold when the viscosity of the thermosetting polymer is between 10 and 1000 Pa.s.

2. Method according to claim 1, wherein the pressure is applied when the viscosity of the thermosetting polymer is less than or equal to 500 Pa.s, preferably less than or equal to 100 Pa.s.

3. A method according to claim 1 or 2, comprising a step of prepolymerizing the thermosetting polymer in order to increase the minimum viscosity of the thermosetting polymer.

4. A method according to any one of claims 1 to 3, wherein the webs of long discontinuous fibers comprise fibers of a length greater than or equal to 10 mm.

5. The method of claim 4, wherein the webs of long discontinuous fibers are carbon, glass or aramid fibers.

6. Method according to any one of claims 1 to 5, in which the thermosetting polymer is chosen from an epoxy, polyurethane, polyester, phenolic, BMI resin.

7. Method according to any one of claims 1 to 6, in which the maximum temperature of the heating cycle is greater than or equal to 150°C, preferably greater than or equal to 180°C.

8. A method according to any one of claims 1 to 7, wherein the applied pressure ranges from 20 to 200 bars.

9. A method according to any one of claims 1 to 8, wherein the complex preform comprises an assembly in the mold of several elements which each result from the prior assembly outside the mold of sheets of long discontinuous fibers impregnated with a thermoset polymer.