Preparation of a reference electrode from an electroactive material in an intermediate charge state

A method for preparing a reference electrode at an intermediate charge state using electroactive materials addresses the challenge of monitoring electrode potentials in electrochemical systems, ensuring stable operation and preventing damage by maintaining the electrochemical stability range.

FR3141562B1Active Publication Date: 2024-11-08COMMISSARIAT A LENERGIE ATOMIQUE ET AUX ENERGIES ALTERNATIVES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2022011198
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-10-27
Publication Date
2024-11-08
Estimated Expiration
2042-10-27

AI Technical Summary

Technical Problem

Existing electrochemical storage systems, such as batteries and supercapacitors, face challenges in monitoring the potential of electrodes independently and maintaining operation within the electrochemical stability range of organic solvents to prevent damage and gas production, particularly with materials like lamellar oxides that are unstable at low lithiation states.

Method used

A method to prepare a reference electrode using electroactive materials at an intermediate charge state, achieved through partial chemical oxidation or reduction, ensuring the electrode is directly functional without prior activation, using oxidizing or reducing agents to maintain a stable potential plateau, and integrating it between positive and negative electrodes.

Benefits of technology

Enables continuous monitoring of electrode potentials without prior activation, preventing operation outside the electrochemical stability range and ensuring stable performance across various charge/discharge cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000028_0000
    Figure 00000028_0000
  • Figure 00000028_0001
    Figure 00000028_0001
  • Figure 00000028_0002
    Figure 00000028_0002
Patent Text Reader

Abstract

Preparation of a reference electrode from an electro-active material in an intermediate state of charge. The present invention relates to a method for preparing a reference electrode, directly functional within a cell of an electrochemical storage system, comprising at least the steps of: (i) having at least one electro-active material whose associated redox reaction has a constant electrochemical potential in intermediate states of charge; (ii) obtaining, by chemical reaction with at least one oxidizing agent and / or at least one reducing agent, the electro-active material in an intermediate state of charge; and (iii) formulating said electro-active material obtained at the end of step (ii) within an electrode, to form said reference electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Preparation of a reference electrode from an electroactive material in an intermediate charge state Technical field

[0001] The present invention relates to the field of electrochemical storage systems, more precisely the field of electrochemical devices of the metal-ion accumulator or battery type, in particular sodium-ion, lithium-ion, potassium-ion, magnesium-ion batteries; lithium-sulfur or lithium-air batteries; and supercapacitors, for example potassium hybrid supercapacitors.

[0002] It aims more specifically to propose a new method for preparing a reference electrode which is directly functional and usable in a cell of such an electrochemical storage system, without requiring prior activation of the electrode by electrochemical means. Prior art

[0003] Electrochemical devices of the battery type, for example lithium batteries, and supercapacitors, find multiple applications, in particular in the power supply of thin embedded systems, such as credit cards, smart labels, in the power supply of mobile phones, the storage of energy from photovoltaic cells, or even in the power supply of electric vehicles.

[0004] Various electrochemical storage systems or electrochemical generators have been developed, such as metal-ion batteries, including sodium-ion, lithium-ion, potassium-ion, magnesium-ion batteries; lithium-sulfur or lithium-air batteries; and more recently supercapacitors.

[0005] These electrochemical generators, for example lithium, conventionally operate on the principle of insertion and deinsertion (or intercalation-deintercalation) of a metal, such as lithium, on at least one electrode. In particular, in a lithium-ion accumulator, the Li+ cations thus go back and forth between the electrodes, respectively positive and negative, at each charge and discharge of the accumulator. The active material of the positive electrode is capable of releasing lithium ions at the time of charging and of incorporating lithium ions at the time of discharging.

[0006] Supercapacitors are energy storage devices that provide power density and energy density that are intermediate between those provided by electrochemical batteries and conventional electrolytic capacitors. In addition, they release energy more quickly than an electrochemical battery. In standard supercapacitors, also known as "symmetrical" supercapacitors, the two electrodes (positive electrode and negative electrode) are both carbon-based. activated and the electrolyte is classically based on an ammonium salt, typically tetraethylammonium tetrafluoroborate (Et4NBF4) in acetonitrile or propylene carbonate. Supercapacitors, called "hybrid" or "asymmetric" supercapacitors, have also been developed, which are somewhere between the symmetric supercapacitors classically used based on activated carbon and batteries. One of the electrodes, classically the positive electrode, is based on activated carbon; the other electrode, classically the negative electrode, is made from a rechargeable battery material. Charge storage in a hybrid supercapacitor occurs at the negative electrode through a redox reaction, while charge storage at the positive electrode occurs through the formation of an electrochemical double layer.

[0007] It is important, for electrochemical storage systems, whether batteries or supercapacitors, to be able to know and monitor the evolution of the potential of each electrode independently and in relation to an electrode of known potential, during the operation of the electrochemical cell. In particular, for cells using electrolytes based on organic solvent(s), it is important that the cell of the electrochemical system does not operate outside the electrochemical stability range of said organic solvent(s), so as not to cause degradation and in particular the production of gas.Similarly, it is important to control, via potential limitation, the lithiation state of certain compounds such as the lamellar oxides LixM02 whose structure is unstable for x<0.5 (case of LiCoO2) or x<0.2 (LixM02 with M=Ni, Co, Mn with low Co content), or to avoid the electrodeposition of lithium in the metallic state at the negative electrode at potentials lower than 0V vs Lr7Li. In order to counter the appearance of any undesirable phenomenon, it is important to be able to know and monitor the evolution of the potential of each electrode, during the operation of the electrochemical cell.

[0008] For this, it is desirable to be able to introduce a so-called reference electrode into the electrochemical system. A reference electrode must have a stable and known potential, making it possible to know at any time the potential of each of the positive and negative electrodes of the system.

[0009] Generally speaking, as listed for example in the document Cengiz et al. [1] or proposed in the documents US 2009 / 0104510 and US 9,379,418, the reference electrodes proposed for electrochemical storage systems, in particular for metal-ion batteries, such as lithium-ion, sodium-ion, calcium-ion, lithium-ion, potassium-ion, magnesium-ion batteries, or for supercapacitors, are based on the implementation, as electrode materials: - pure metals, such as lithium, sodium or potassium, or lithium-based alloys (e.g., LixSn, LixBi, LixAu, LixIn, LixSi, LixAl, etc.), respec- primarily based on sodium, potassium, etc.; and - intercalation / insertion materials of the LiMO2 type with M representing Co, Ni or Mn; LiM'2O4 with M' representing Ni or Mn; LiM”PO4 with M” representing Fe, Co, Mn or Ni; or of the Li4Ti50i2 type.

[0010] To be suitable for use as a reference electrode, the compounds must exhibit, during the galvanostatic charge / discharge process, a potential plateau (associated redox reaction exhibiting a constant electrochemical potential), and their thermodynamic potential must be independent of the salt concentration of the electrolyte.

[0011] As for metals and alloys, they can be used directly in a three-electrode system, but exhibit potential instability over time / cycling, particularly due to their very low thermodynamic potential. Indeed, their reducing power induces strong reactivity with the electrolytes, and their potential, lower than that of the H2O / H2 or O2 / H2O pair (which allows spontaneous reactions with H2O and O2), requires control of the atmosphere during the assembly steps. In addition, the thermodynamic potential of an electrode based on pure metals is likely to vary depending on variations in the concentration of lithium ions in the electrolyte. Certainly, it can be considered that the average concentration of lithium ions in the inter-electrode space does not change.However, concentration gradients can be established, which are greater when the applied currents are high, and are therefore likely to vary the thermodynamic potential of the reference electrode. In addition, there is also a risk of variation in the potential of the reference electrode during aging, because the concentration of lithium ions in the electrolyte is likely to vary due to degradation mechanisms (drying of the liquid phase).

[0012] These disadvantages do not concern the other aforementioned electrode materials, for which the thermodynamic potential of the electrode is fixed by the number of active / inactive sites or the lithium concentration (respectively, sodium, potassium) in the alloy. Materials having a wide potential plateau as a function of the insertion rate are particularly advantageous, since they allow stability of the potential, independently of changes in the lithiation state of the material likely to occur during aging.

[0013] Insertion materials, for example Li4Ti50i2 or LiFePO4, characterized by biphasic behavior, are therefore favored. In particular, the chemical, thermal and electrochemical stability of LiFePO4 (or LFP), as well as its average oxidation-reduction potential, which is higher than the potential of the other aforementioned redox materials and constant over a wide window of lithiation rates, make LFP a material of interest for reference electrodes.

[0014] More recently, the CEA has also proposed the use, for the preparation of reference electrodes, of electroactive organic materials of type P (electron donor) or type N (electron acceptor).

[0015] However, electrodes based on the aforementioned materials (lithium insertion / intercalation materials, or P or N type materials) require prior "activation" in order to be operational as reference electrodes. Indeed, these electroactive materials only have a fixed electrochemical potential for intermediate charge states (oxidation / reduction states, or lithiation states) (from approximately 5% to 95% state of charge (SoC)), which implies prior conditioning of the electrodes in order to reach the potential plateau (generally, at approximately 50% SoC).

[0016] This step complicates the preparation and implementation of these reference electrodes. Currently, the activation of the reference electrodes is carried out exclusively electrochemically. Several methods for this electrochemical activation of the electrodes exist, the most common consisting of: (1) partially charge or discharge the reference electrode in a first two-electrode device (for example, in a half-cell with a lithium counter-electrode), then disassemble the assembly in order to recover the “activated” reference electrode, possibly rinsing it, before inserting it into the electrochemical cell for which it is intended.

[0017] However, in the context of this variant, the step of transposing the electrode from one cell to another induces a risk of deterioration of the reference electrode. (2) carrying out a partial charge or discharge of the reference electrode at the level of a three-electrode assembly, directly within the electrochemical cell for which the reference electrode is intended, by connecting, in a first stage, the reference electrode as a working electrode and then, after activation, by carrying out the three-electrode connection with the reference electrode.

[0018] This approach, although it makes it possible to avoid the disassembly step required in the first variant mentioned above, is nevertheless not without its drawbacks. In fact, the activation step has the consequence of consuming part of the cell's capacity, and controlling the state of charge of the reference electrode is delicate. In addition, this approach requires knowing the exact quantity of active material deposited or carrying out an electrochemical quantification step (charge / discharge cycle) to know the effective capacity of the electrode. Finally, since this activation step is carried out after the formation step (first charge / discharge cycle(s)) of the cells, it is not possible to have access to the information on the potentials during the formation, although this is an interesting piece of data. Statement of the invention

[0019] The present invention aims precisely to propose a new method for preparing reference electrodes, making it possible to overcome the drawbacks, discussed previously, linked to the need to activate the electrode beforehand electrochemically.

[0020] More particularly, the invention relates to a method for preparing a reference electrode, directly functional (or usable) within a cell of an electrochemical storage system, comprising at least the steps consisting of: (i) having at least one electroactive material whose associated redox reaction exhibits a constant electrochemical potential (or potential plateau) at intermediate charge states; (ii) obtaining, by chemical reaction using at least one oxidizing agent and / or at least one reducing agent, the electroactive material in an intermediate charge state; and (iii) formulating said electroactive material obtained at the end of step (ii) within an electrode, to form said reference electrode.

[0021] As mentioned above, a reference electrode is defined as being an electrode having a stable and known electrochemical potential, advantageously making it possible to serve as a reference point for independently measuring the potential of the positive and negative electrodes in an electrochemical cell.

[0022] By "directly functional" is meant that the electrode prepared according to the method of the invention is directly operational / usable as a reference electrode. It can thus be inserted into an electrochemical cell to form a three-electrode cell and be used as a reference electrode from the first charge / discharge cycle of the cell.

[0023] In particular, the electrode obtained at the end of step (iii) of the method of the invention does not require any electrochemical activation step before it can be operational as a reference electrode.

[0024] It is known to be possible to oxidize, respectively reduce, active materials using different oxidizing, respectively reducing chemical agents. For example, it is possible to decompose (oxidize) LiFePO4 using a solution of NO2BF4 in acetonitrile ([2]).

[0025] On the other hand, to the inventors' knowledge, it has never been proposed to take advantage of the possibility of oxidizing or chemically reducing active materials to obtain an electroactive material in an intermediate charge state, for the preparation of a reference electrode directly operational at the level of an electro-cell. trophic.

[0026] By "intermediate charge state", we mean according to the invention a state of partial oxidation / partial reduction (or even partial lithiation) of said electroactive compound or material or a mixture of the oxidized and reduced forms of said electroactive compound or material, corresponding to the fixed potential (potential plateau) of the redox reaction associated with the electroactive compound.

[0027] In a first embodiment variant, the starting electroactive material (i) is a material capable of being oxidized (or delithiated), step (ii) consisting of chemically obtaining said electroactive material in an intermediate oxidation state (or delithiated state).

[0028] The electroactive material in an intermediate oxidation state is preferably obtained by partial chemical oxidation using at least one oxidizing agent.

[0029] In a second embodiment, the starting electroactive material (i) is a material capable of being reduced, step (ii) consisting of chemically obtaining said electroactive material in an intermediate reduction state (or lithiation state).

[0030] The electroactive material in an intermediate reduced state is preferably obtained by partial chemical reduction using at least one reducing agent.

[0031] The method for preparing a reference electrode according to the invention can thus more particularly comprise the steps consisting of: (i) having at least one electroactive material, the associated redox reaction of which has a constant electrochemical potential in intermediate oxidation or reduction states, called “intermediate charge states”, in particular for an intermediate lithiation / delithiation state; (ii) carrying out a partial chemical oxidation or a partial chemical reduction of said electroactive material by reaction with at least one oxidizing or reducing agent, to obtain the electroactive material in an intermediate charge state; and (iii) formulating said electroactive material obtained at the end of step (ii) within an electrode, to form said reference electrode.

[0032] Advantageously, as mentioned previously, the method of the invention makes it possible to obtain a directly functional / operational electrode when it is integrated within a three-electrode electrochemical cell.

[0033] Advantageously, the method according to the invention thus makes it possible to dispense with any electrochemical step, prior to the use of the electrode as a reference electrode, which would be likely, as discussed previously, to damage the reference electrode or to disrupt the operation of the electrochemical system.

[0034] Thus, the method for preparing a reference electrode according to the invention does not include any electrochemical activation step, prior to the operation of the reference electrode within a three-electrode cell, whether within of an electrochemical cell separate from that in which the reference electrode is intended to be implemented or within the cell of the electrochemical system in which it will be used.

[0035] Furthermore, the method of the invention makes it possible to obtain good control of the state of charge of the reference electrode material.

[0036] The functional reference electrode prepared according to the method of the invention can be implemented for various electrochemical storage systems or electrochemical generators, and in particular for metal-ion batteries, for example sodium-ion, lithium-ion, potassium-ion, magnesium-ion batteries; lithium-sulfur or lithium-air batteries, and supercapacitors, for example potassium hybrid supercapacitors.

[0037] It can thus be directly integrated into a cell of such an electrochemical storage system or electrochemical generator, to form a cell with three electrodes: a positive electrode, a negative electrode and the reference electrode prepared according to the invention.

[0038] The integration of a reference electrode obtained according to the method of the invention within at least one of the cells of an electrochemical storage system or electrochemical generator, advantageously makes it possible to access the potentials of each of the positive and negative electrodes, and this from the first charge / discharge cycle of the cell. Knowledge and monitoring of the potentials of the positive and negative electrodes makes it possible to detect, where appropriate, potential defects in their operation.

[0039] Monitoring the potentials of the positive and negative electrodes during operation of the electrochemical storage system, by means of the reference electrode prepared according to the invention, advantageously allows optimized use of said electrochemical system, in particular use at its maximum capacity, without being exposed to risks of malfunction, and thus allows improved safety in the use of said electrochemical system.

[0040] Other characteristics, variants and advantages of the method for preparing a reference electrode according to the invention and of its implementation at the level of a cell of an electrochemical storage system will become more apparent upon reading the description, examples and figures which follow, given by way of illustration and not limitation of the invention. Brief description of the drawings

[0041] [Fig.l] shows, schematically, in cross-section, an example of assembly 100 of the different elements, including the reference electrode prepared according to the invention, within a cell of an electrochemical storage system;

[0042] [Fig.2] shows the diffractogram obtained by DRX analysis (ray diffraction) X) powder prepared in example 1.1. by partial delithiation of LiFePO4;

[0043] [Fig.3] shows the evolution of the current (in A) and the potential (in V) during the charge / discharge cycles carried out according to example 1.2., with the reference electrode assembled in half-cell;

[0044] [Fig.4] shows the evolution of the potential (in V vs Li+ / Li) as a function of the capacity specific mass (in mAh / g) during the two charge / discharge cycles carried out according to example 1.2., with the reference electrode assembled in half-cell;

[0045] [Fig.5] shows, schematically, the welding of an electrode on a aluminum connecting tab as made in example 1;

[0046] [Fig.6] shows, schematically, the lithium-ion cell, in pouch format- cell, prepared in Example 2, comprising a reference electrode prepared according to the invention;

[0047] [Fig.7] shows the evolution curves of the cell voltage of the lithium- ion, and the potentials of the positive and negative electrodes, as a function of the capacity, obtained using a reference electrode prepared according to the invention, and using a conventional reference electrode (requiring activation) for a first discharge at C / 10, a first charge at C / 2 and a discharge at C / 2, as described in example 2;

[0048] [Fig.8] shows the evolution curves of the cell voltage of the lithium- ion, in galvanostatic charge and discharge, at different regimes, obtained using a reference electrode prepared according to the invention and a conventional reference electrode, as described in example 2.

[0049] It should be noted that, for reasons of clarity, the various elements in Figures 1, 5 and 6 are shown in free scale, the actual dimensions of the various parts not being respected.

[0050] In the rest of the text, the expressions “between ... and ...”, “ranging from ... to ...” and “varying from ... to ...” are equivalent and are intended to mean that the limits are included, unless otherwise stated. Detailed description Step (i): Electroactive material

[0051] As indicated previously, the method of the invention uses one or more electroactive materials whose electrochemical oxidation-reduction reaction, also called redox reaction, associated with the reversible passage from a reduced state of the electroactive material to an oxidized state, has the particularity of presenting a constant electrochemical potential or electrochemical potential plateau.

[0052] The potential plateau, associated with an electroactive material, can be identified by a cycling test of an electrode based on said electroactive material, assembled in a half-cell or a complete cell, for example in the form of a button cell, by operating a charge or a discharge in galvanostatic mode. The constant electrochemical potential corresponds to the potential plateau observed at the level of the charge / discharge curves at constant current (for example, curves of variation of the potential E as a function of time or as a function of the absolute or specific mass capacity during cycling in galvanostatic mode). Note that in a complete cell (this is always the case in a half-cell with a lithium counter-electrode), this potential plateau is only observable if the counter-electrode used (which then acts as a reference) also has a potential plateau during its charge / discharge at constant current.

[0053] The potential plateau is thus reached for intermediate charge states, which can generally range from 5% to 95% of the complete charge (oxidation or reduction).

[0054] Of course, the value of the potential plateau depends on the redox couple associated with the electroactive material used.

[0055] As indicated previously, by "intermediate charge state" is meant according to the invention a state of partial oxidation / partial reduction (or even partial lithiation) of said electroactive compound or material or a mixture of the oxidized and reduced forms of said electroactive compound or material, corresponding to the fixed potential (potential plateau) of the redox reaction associated with the electroactive compound.

[0056] The electroactive material(s) from which a reference electrode according to the invention is prepared may be chosen from the materials usually used to form electrochemically activated reference electrodes, as mentioned above.

[0057] According to a first variant embodiment, the electroactive material used to prepare a reference electrode according to the method of the invention is a material capable of being oxidized (in particular, capable of being delithiated), and thus capable of exhibiting an intermediate oxidation state (in particular delithiated) corresponding in galvanostatic cycling to the potential plateau.

[0058] Such materials may for example be chosen from intercalation (or insertion) materials of the LiM02 type with M representing Co, Ni or Mn; LiM' 2O4 with M' representing Ni or Mn; and LiM”PO4 with M” representing Fe, Co, Mn or Ni;

[0059] It may also be a question of electroactive organic materials of type P whose associated redox reaction has a constant electrochemical potential.

[0060] By material, also called “organic” compound, we mean a compound, in particular of a molecular, oligomeric or polymeric nature, of carbon chemistry, comprising carbon and hydrogen atoms, and one or more heteroatoms chosen from oxygen, nitrogen, sulfur, phosphorus, these atoms and heteroatoms being linked only by covalent bonds, this compound possibly being in the form of a salt, for example a metal salt.

[0061] By “P-type” or “electron donor” electroactive material is meant an organic material which can undergo, due to the nature of its electroactive functions or redox functions, a reversible oxidation from the neutral state to a positively charged state, with anionic charge compensation.

[0062] The electrochemical mechanism associated with a P-type material can be schematized as follows:

[0063] [Chem.l] RRR .> L \ ; * A',<L>. . * HAS ; 3 sec. V ................y. 4' ' ... | " -¾ ® " .-¾ ' | R' ' R'

[0064] The P-type electroactive organic materials considered according to the invention can be chosen from organic materials, molecules, oligomers or organic polymers, already proposed as active materials for organic electrodes, for example for batteries. Such materials are documented in the literature [3].

[0065] In particular, such electroactive organic materials of type P may be chosen from compounds, in particular molecules, oligomers or polymers, carrying redox functions chosen from: - stable radicals O', N' or NO', in particular nitroxide (NO') or phenoxy (PhO') functions; Such polymers may be chosen, for example, from polymers having a linear skeleton chosen from poly(meth)acrylates, polythiophenes, polyfluorenes, polycarbazoles, polyanilines, polyphenylenes, polyisothionaphthenes, polyacetylenes, polyphenylenevinylenes, and their copolymers; and bearing at least side groups having at least one stable radical of type O', N' or NO', in particular having at least one nitroxide and / or phenoxy function, in particular at least one nitroxide function. These may be, for example, polymers carrying side groups of 2,2,6,6-tetramethylpiperidinyl-N-oxy (TEMPO) structure, such as a poly(2,2,6,6-tetramethylpiperidinyloxy-4-yl methacrylate), denoted PTMA. - conjugated ether (-O-) or thioether (-S-) functions; such as thianthrene, phenothiazine, and their oligomeric or polymeric derivatives; ir-conjugated conductive polymers of polythiophene (PT) type, for example poly(3,4-ethylenedioxythiophene), better known as “PEDOT”; - conjugated amine functions, in particular aromatic or heteroaryl amine groups, such as dianiline, triphenylamine, polyaniline or polypyrrole, molecules of the viologen or carbazole type, polyviologens and polycarbazoles; and other ir-conjugated conductive polymers, such as polythiophenes, polyanilines and polypyrroles, e.g. polyacetylenes.

[0066] The P-type organic material may be in different forms, provided that they allow the partial chemical oxidation of said P-type organic material so as to achieve the desired intermediate charge state. In particular, the P-type material may be in a form such that it does not degrade, in particular does not dissolve in the electrolyte of the electrochemical cell in which the reference electrode will be implemented.

[0067] Several strategies are known to insolubilize redox organic compounds.

[0068] As mentioned above, one of the most commonly used strategies is to prepare the organic redox compound in the form of polymers or copolymers, crosslinked or not, with pendant or intramolecular redox functions.

[0069] Another strategy for insolubilizing electroactive organic compounds consists of producing composite structures by physisorption, with an inorganic substrate, for example silica, alumina, carbon, within which weak bonds are created (hydrogen, ji-ji interactions, Van der Waals), making it possible to limit, or even prevent, the dissolution of the redox organic compound.

[0070] It is also possible to graft the electroactive organic compound onto an inorganic solid (silica, alumina, carbon, etc.) via ionic or covalent bonds, for example by acid-base reaction with the hydroxyls of the silica surface or by reaction of diazonium salts with the carbon surface, in order to form an insoluble organic / inorganic hybrid compound.

[0071] Another strategy consists of adding ionic functions to the electroactive organic compound, for example of the carboxylate, sulfonate, alcoholate, imide, enolate type, etc., making it possible to limit the dissolution of the compound in an organic medium.

[0072] In a particularly preferred embodiment, the electroactive material used for the preparation of a reference electrode according to the invention is chosen from insertion materials of the LiM”PO4 type with M” representing Fe, Co, Mn or Ni. Advantageously, it may be LiFePO4 (or LFP) whose associated redox reaction LiFePO4 / FePO4 has a potential plateau at approximately 3.424 V.

[0073] According to another variant embodiment, the electroactive material used to prepare a reference electrode according to the method of the invention is a material capable of being reduced, and capable of exhibiting a corresponding intermediate reduction state in galvanostatic cycling at a constant potential (potential plateau).

[0074] Such materials are for example chosen from intercalation / insertion materials of the Li4Ti50i2 type.

[0075] It may also be a question of electroactive organic materials of type N whose associated redox reaction presents a constant electrochemical potential.

[0076] By “N-type” or “electron acceptor” electroactive material is meant an organic material which can undergo, due to the nature of its electroactive functions, a reversible reduction from the neutral state to a negatively charged state, with cationic charge compensation.

[0077] The electrochemical mechanism associated with an N-type material can be schematized as follows:

[0078] [Chem.2]

[0079] The N-type electroactive organic materials considered according to the invention can be chosen from organic materials, molecules, oligomers or organic polymers, already proposed as active materials for organic electrodes, for example for batteries, as described in publication [3].

[0080] In particular, such electroactive organic materials of type N can be chosen from compounds, in particular molecules, oligomers or polymers, carrying redox functions chosen from: - conjugated azo functions (-N=N-) such as azobenzene or one of its derivatives, - disulfide functions (-SS-) such as diphenyl disulfides, tetrathionap-thalene, poly(2,5-dimercapto-1,3,4-thiadiazole), poly(5,8-dihydro-1H,4H-2,3,6,7-tetrathia-anthracene); and - conjugated carbonyl functions, in particular contained within quinonoid structures, such as anthraquinone; anhydride structures such as pyromellitic anhydride, dimide structures such as perylene dimide; or carboxylate structures such as perylene tetracarboxylate.

[0081] For example, an N-type electroactive organic material may be based, for example, on perylene tetracarboxylate, also known as PTCLi4.

[0082] As mentioned previously concerning P-type organic materials, said N-type organic compound(s), carrying redox units as considered above, may be in different forms, as indicated above, provided that they allow the partial chemical reduction of said N-type organic material in the presence of a reducing agent so as to obtain the desired intermediate charge state.

[0083] In a particularly preferred embodiment, the electroactive material used for the preparation of a reference electrode according to the invention is Li4Ti5O 12 (or LTO), the associated redox reaction of which has a potential plateau at approximately 1.5 V.

[0084] The electroactive material in step (i) of the process of the invention is preferably in the form of a powder. Step (ii): Chemical oxidation / reduction

[0085] As indicated previously, the method of the invention comprises a step (ii) of obtaining, by chemical synthesis using oxidizing and / or reducing agent(s), said electroactive material in an intermediate charge state.

[0086] Preferably, step (ii) proceeds, for an electroactive material capable of being oxidized (respectively, capable of being reduced), to a partial chemical oxidation (respectively, to a partial chemical reduction) of said starting electroactive material, using at least one chemical oxidizing agent (respectively using at least one chemical reducing agent).

[0087] Of course, the nature of the oxidizing agent (respectively, of the reducing agent), as well as the conditions of the oxidation reaction (respectively, of the reduction), are adjusted with regard to the nature of the electroactive material which one seeks to partially oxidize (respectively, to reduce).

[0088] Examples of oxidizing agents include: nitronium tetrafluoroborate (NO2BF4), nitrosyl tetrafluoroborate (NOBF4), potassium persulfate (K2S2O8), sodium nitrate (NaNO3), nitrile trifluoromethanesulfonate (NO2CF3SO3), potassium permanganate (KMnO4), nitric acid (HNO3), sulfuric acid (H2SO4), peroxydisulfuric acid (H2S2O8), peroxymonosulfuric acid (H2SO5), “Magic Blue” (Tris(4-bromophenyl)aminium hexachloridoantimonate), hydrogen peroxide (H2O2), lead dioxide (PbO2), organic peracids such as metachloroperbenzoic acid (mCPBA), metal cations such as Ce4+, Ag+, Cu2+, gases such as O2, O3, N2O, etc.

[0089] Examples of reducing agents include: alkali metals such as lithium, sodium, potassium; hydrides such as lithium hydride (LiH) and sodium borohydride (NaBH4), hydrogen, carbon, salts such as sodium sulfite (Na2SO3), sodium hydrosulfite (Na2S2O4), sodium thiosulfate (Na2S2O3), hydrazine (N2H4), lithium iodide (LiI).

[0090] The implementation conditions for carrying out the partial chemical oxidation or reduction are of course adjusted with regard to the electroactive material and the agent oxidizing or reducing agent brought into contact.

[0091] The oxidation or reduction reaction can be carried out in bulk (in the absence of solvent) or by wet method (in the presence of one or more solvents).

[0092] For example, in the case where the electroactive material is LiFePO4, step (ii) can be carried out by partial chemical oxidation of the material using an oxidizing agent, preferably with NO2BF4, to obtain a Lii xFePO4 powder, with 0.30 < x < 0.70, in particular 0.50 < x < 0.60. The partial oxidation of LiFePO4 is more particularly carried out in a solvent medium, preferably in acetonitrile. Such an oxidation reaction is for example described in publication [2].

[0093] Obtaining the partially oxidized (or partially reduced) form of the electroactive material can be controlled by adjusting the molar proportions of electroactive material and oxidizing agent (respectively, reducing agent) used.

[0094] Generally, the molar ratio between said oxidizing or reducing agent and said electroactive material to be oxidized or reduced is between 0.1 and 0.9, in particular between 0.4 and 0.6.

[0095] By way of example, in the case of an electroactive intercalation / insertion material of the LiM02; LiM'2O4 or LiM”PO4 type described previously, for example of the LiFePO4 type, the oxidation conditions are adjusted to obtain the material in an intermediate charge state (oxidation state), corresponding to an intermediate delithiation state, in particular with a delithiation rate ranging from 30% to 70%, in particular from 50% to 60%.

[0096] Thus, according to a particular embodiment, in the case where said electroactive material in step (i) is an electroactive intercalation material of the LiM02; LiM'2O4 or LiM”PO4 type, step (ii) can carry out a partial oxidation of said material to obtain said material in an intermediate delithiation state, in particular with a delithiation rate ranging from 30% to 70% and more particularly from 50% to 60%.

[0097] In other words, the electroactive material in an intermediate charge state obtained at the end of step (ii) may more particularly be of composition Lii XMO2; LibxM'2 O4 or Lii XM”PO4, for example Lii xFePO4, with 0.30 < x < 0.70, in particular 0.50 < x < 0.60.

[0098] The formation in step (ii) of the material at an intermediate charge state corresponding to the potential plateau can be verified by a cycling test (charge / discharge) of an electrode based on said material obtained, assembled in a half-cell or complete cell, for example in a half-battery, as illustrated in the examples.

[0099] As illustrated in the examples, in the case of LiFePO4, the material in an intermediate charge state is characterized by a two-phase behavior, with the coexistence of two different crystallographic phases (fully lithiated and completely delithiated) identifiable for example by X-ray diffraction analysis (XRD).

[0100] In the case of a LiM02 type material, this intermediate charge state results in a solid solution phenomenon, with the metal M present in mixed oxidation states (M(III) and M(IV)) in the crystals.

[0101] It is understood that the reaction of said electroactive material with said oxidizing or reducing agent(s) may be followed by one or more steps of removing the solvent(s) and / or washing the material obtained.

[0102] Preferably, the electroactive material in an intermediate charge state is obtained in step (ii) in the form of a powder, preferably with a particle size suitable for easy implementation during the formulation of the ink based on said electroactive material for the preparation of the electrode in step (iii).

[0103] In a particular embodiment, step (ii) may thus comprise a step of grinding the electroactive material obtained, dry or wet, making it possible to obtain the electroactive material in the form of a powder.

[0104] In a particular embodiment, the method of the invention is implemented to prepare a reference electrode from LiFePO4, and more particularly comprises the steps consisting of: (i) have a LiFePO4 powder, (ii) carrying out a partial chemical oxidation of said LiFePO4 powder, in particular by reaction with NO2BF4 as oxidizing agent in acetonitrile, to obtain a Lii xFePO4 powder, with 0.30 < x < 0.70, in particular 0.50 < x < 0.60; and (iii) formulating said Lii xFePO4 powder obtained in step (ii) within an electrode, to form said directly functional reference electrode.

[0105] It is understood that chemical synthesis variants, other than the variants described above, may be considered to obtain in step (ii) the material in an intermediate charge state. For example, in the case of implementing the method of the invention from an electroactive material capable of being oxidized, for example LiFePO4, step (ii) may proceed in a first step of total chemical oxidation (total delithiation) of the material using at least one oxidizing agent, for example by NO2BF4 (obtaining FePO4), followed by a partial reduction using at least one reducing agent to reach the intermediate charge state (Liy FePO4 with 0.30 < y < 0.70, in particular 0.40 < y < 0.50).

[0106] Step (iii): Formulation of the electroactive material in an intermediate charge state within an electrode

[0107] As indicated previously, the method of the invention comprises a step (iii) of integrating the electroactive material into an intermediate charge state, obtained at the outcome of step (ü), preferably in the form of a powder, within an electrode.

[0108] The integration of the electroactive material at the level of an electrode can be carried out by any conventional method of preparing electrodes.

[0109] The formulation of said electroactive material at the level of an electrode can thus comprise at least the following steps: - preparation of a dispersion, more commonly called “ink”, comprising, in one or more aqueous and / or organic solvents, said electroactive material in an intermediate charge state obtained at the end of step (ii); one or more binders and optionally one or more electronically conductive additives; - depositing ink on the surface of a current collector; - evaporation of said solvent(s) from the ink to form the electrode film; and preferably - calendering of the electrode.

[0110] The ink solvent may comprise water and / or one or more organic solvents, for example N-methyl-2-pyrrolidone.

[0111] Electronically conductive additives are used to improve the electronic conductivity of the electrode. They can be chosen, for example, from carbon fibers, carbon black, carbon nanotubes and mixtures thereof.

[0112] Said electronically conductive additive(s), when present, may preferably be implemented in a content ranging from 1 to 10% by mass, in particular from 2 to 8% by mass, relative to the mass of the electrode. It is understood that the total mass of the electrode does not include the mass of the current collector.

[0113] The binders are used to ensure the mechanical strength of the electrode on the current collector, the cohesion of the different components of the electrode or even its flexibility properties. They can be chosen from polymer binders, in particular chosen from fluorinated polymers, for example from polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polymers derived from carboxymethylcellulose (CMC), polysaccharides and latexes, in particular of the styrene-butadiene rubber (BR) type or in English "stryrene-butadiene rubber" (SBR)).

[0114] A particularly preferred binder is poly(vinylidene fluoride) (PVDF).

[0115] Said binder(s) may be present in an amount less than or equal to 20% by mass, relative to the total mass of the electrode, in particular less than or equal to 10% by mass, in particular between 1 and 10% by mass, relative to the total mass of the electrode. It is understood that the total mass of the electrode does not include the mass of the current collector.

[0116] The ink can be homogenized before spreading.

[0117] The deposition of the ink on the surface of the current collector can be carried out by any technique known to those skilled in the art, for example by coating, by a printing technique, by extrusion or by co-lamination.

[0118] The current collector may be solid, for example in the form of a strip or in the form of a grid.

[0119] The current collector may be made of a metallic material chosen from copper, aluminum, nickel or stainless steel potentially coated with carbon.

[0120] The evaporation of the solvent(s) from the ink may be carried out by drying, for example in an oven, at a temperature of between 20 and 150°C, in particular between 50 and 80°C, in particular for a period of between 1 and 15 hours.

[0121] Preferably, the ink drying step is followed by a calendering step.

[0122] Said active material(s) in an intermediate charge state may represent from 5 to 98% by mass, in particular at least 30% by mass, in particular at least 50% by mass and more particularly from 70 to 96% by mass, relative to the total mass of the electrode, excluding the mass of the current collector.

[0123] The grammage of the electrode, in other words the mass of electroactive material in an intermediate charge state implemented according to the invention, per unit area, can be adjusted by controlling the rate of active material and the thickness of deposition, in particular coating, of the ink formulated on the current collector. Preferably, the grammage of the electrode is between 0.1 mg / cm2 and 50 mg / cm2, in particular between 1 mg / cm2 and 30 mg / cm2, and more particularly between 3 mg / cm2 and 10 mg / cm2. ELECTROCHEMICAL STORAGE SYSTEM

[0124] As indicated previously, the electrode obtained at the end of step (iii) is directly functional as a reference electrode. In other words, it can be used as a reference electrode, without a prior step, within a cell of an electrochemical storage system or electrochemical generator.

[0125] In particular, the method for preparing a reference electrode according to the invention does not comprise any step of electrochemical activation of the electrode obtained at the end of step (iii), prior to its operation as a reference electrode.

[0126] The electrochemical storage systems, in which a reference electrode obtained according to the invention can be incorporated, can be diverse. It can be a metal-ion battery, in particular sodium, lithium, potassium, magnesium batteries; a lithium-sulfur or lithium-air battery.

[0127] It may also be a supercapacitor, in particular a “standard” supercapacitor or a so-called “hybrid” supercapacitor, in particular a potassium hybrid supercapacitor.

[0128] The cell of the electrochemical storage system may typically comprise a positive electrode, a negative electrode and an electrolyte, in particular impregnating a porous membrane separating said electrodes.

[0129] It may also be a cell based on a ceramic electrolyte membrane, or based on a solid electrolyte, for example a solid polymer electrolyte or hybrid solid electrolyte.

[0130] The reference electrode prepared according to the method of the invention is thus integrated as a third electrode at the cell level of the electrochemical storage system.

[0131] The invention thus relates, according to another of its aspects, to a method for preparing a cell of an electrochemical storage system, for example a lithium battery, comprising a step of preparing a reference electrode according to the method as described previously, followed by a step of integrating said reference electrode at the level of a cell of an electrochemical storage system to obtain a cell with three electrodes.

[0132] A cell of an electrochemical storage system, within which a reference electrode obtained according to the invention is used, is thus a three-electrode system, comprising more particularly: - a positive electrode; - a negative electrode; and - said reference electrode prepared according to the method of the invention as described previously.

[0133] The nature of the elements constituting the cell of the electrochemical storage system, in particular the positive and negative electrodes and the electrolyte, of course depends on the type of device considered, depending on whether it is a metal-ion battery, a lithium-sulfur battery, a lithium-air battery, a supercapacitor, etc.

[0134] Said active material(s) of the negative electrode may in particular be chosen from activated carbon, carbonaceous materials for intercalation of an alkaline element such as graphite; silicon; conversion materials of the MO2 type with M representing for example Sn (SnO2), Si (SiO2), or of the M3O4 type with M representing for example Co (Co3O4), Mn (Mn3O4) etc., metals (Li, Na, K, Mg, Ca) and alloys based on these metals, titanium oxides of the Li4Ti50i2 type.

[0135] Said active material(s) of the positive electrode may in particular be chosen from activated carbon, LiMO2 or LiM2O4 with M representing Mn, Co, Ni or one of their combinations, for example LiNiO,6MnOj2CoO>2O2; LiMPO4 with M representing Fe, Mn or one of their combinations.

[0136] The following example, with reference to the implementation of a reference electrode prepared according to the method of the invention at the level of a cell of a lithium-ion battery, is thus given solely by way of illustration of the invention, it being understood that the use of a reference electrode obtained according to the invention is in no way limited to this particular mode of implementation.

[0137] Thus, as an example of implementation, a reference electrode prepared according to the method of the invention is introduced into a lithium battery, in particular a lithium-ion battery.

[0138] A reference electrode prepared according to the invention can for example be implemented at the level of a cell of a lithium-ion battery further comprising: - a positive electrode comprising a positive active material, for example LiNi0>6 Mno,2Coo202; - a negative electrode comprising a negative active material, for example based on graphite; and - an electrolyte comprising at least one lithium salt, for example LiPF6, in one or more organic solvents, for example chosen from carbonate solvents, such as ethylene carbonate (EC), diethyl carbonate (DEC) and / or dimethyl carbonate (DMC).

[0139] It is understood that the different elements are assembled within the cell of the electrochemical storage system, for example the battery or the supercapacitor, so as, on the one hand, to allow efficient use of the reference electrode, for example for the purpose of knowing the potentials of the positive and negative electrodes and, on the other hand, so that the presence of this third electrode does not interfere negatively with the operation of the cell of said electrochemical storage system.

[0140] In particular, the reference electrode can be used when the cell of said electrochemical storage system is subjected to cycling for currents ranging from C / 100 to 100C, in particular from C / 50 to 100C, and more particularly from C / 50 to 5C, in particular from C / 2 to 5C, at temperatures ranging from -40°C to 100°C.

[0141] Generally speaking, the different electrodes of the cell of the electrochemical storage system are separated from each other by a porous membrane, also called a “separator”, impregnated with the electrolyte.

[0142] Such porous separators can be, for example, made of polyethylene or polypropylene.

[0143] The cell of the electrochemical storage system may advantageously have a configuration of superimposed layers. In other words, the assembly of the cell may be carried out by stacking the different elements in the form of layers.

[0144] Each of the electrodes of a cell of the electrochemical storage system may be in the form of a layer of the electrode material, deposited on at least one of the faces or on both faces of a current collector in the form of a thin film, for example in the form of a metal strip.

[0145] According to an alternative embodiment, in the case of an architecture of the cell of the electrochemical storage system in the form of a stack of the different elements, the reference electrode can be positioned between the positive and negative electrodes.

[0146] [Fig.l] schematically represents, in cross-section, an example of assembly 100 of the different elements, integrating a reference electrode prepared according to the invention, within a cell of an electrochemical storage system, for example like the cell of a metal-ion battery.

[0147] As shown in this figure, in an alternative embodiment, a cell of an electrochemical storage system, for example a metal-ion battery, in which a reference electrode prepared according to the invention is incorporated, may comprise the assembly 100 of the following different elements, in this stacking order: - a positive electrode 22, in particular formed from a layer of active material 220 on a current collector 221, for example made of aluminum; - a porous separator 24, for example made of polypropylene, intended to be impregnated with the electrolyte; - said reference electrode 21, prepared as described above, formed of a layer 211 of the electrode material incorporating said electroactive material in an intermediate charge state, at the level of a current collector 212, for example made of aluminum;

[0148] - a porous separator 24, for example made of polypropylene, intended to be impregnated by the electrolyte; and - a negative electrode 23, in particular formed from a layer of active material 231 on a current collector 232, for example made of aluminum.

[0149] Within the cell of the electrochemical system, the assembly is soaked with an electrolyte comprising at least one alkali or alkaline-earth metal salt, for example a lithium salt in the case of a lithium battery, in one or more aqueous or organic solvents.

[0150] Porous separators provide electronic insulation between the electrodes, while allowing easy passage of ions from the electrolyte. Of course, other configurations are possible. For example, it is possible to enclose the reference electrode in a separator folded back on itself.

[0151] The reference electrode 21 prepared according to the invention, inserted within the assembly between the positive 22 and negative 23 electrodes, advantageously has a surface in a plane orthogonal to the stacking direction of the different elements (electrodes and separators), reduced compared to the surfaces of the positive and negative electrodes in this same plane. Preferably, Make projected from the reference electrode in a plane orthogonal to the stacking direction, does not exceed 10%, in particular 5%, of the projected area in this same plane of the positive and negative electrodes.

[0152] The invention is not limited to the arrangement shown in [Fig.l]. Other assemblies may be considered, provided that they allow both the operation of the cell of the electrochemical storage system and the use of the reference electrode. Examples of configuration of cells with three electrodes are for example described in document US 9,379,418.

[0153] A reference electrode prepared according to the invention can advantageously be used in the manufacture of all-solid-state batteries (“all-solid-state” batteries).

[0154] Advantageously, a reference electrode prepared according to the invention can be implemented in cells of various formats: wound or stacked cells, in rigid or flexible packaging, in prismatic or cylindrical format, etc.

[0155] In a particular embodiment, a reference electrode prepared according to the invention can be integrated into a cell of an electrochemical storage system packaged in a prismatic format, and in particular in the form of a “pouch cell” as illustrated in the examples. Such a “pouch cell” notably has a flexible aluminum-plastic packaging.

[0156] Advantageously, the integration of a reference electrode at the level of at least one of the cells of the electrochemical storage system makes it possible to monitor the potentials of the positive and negative electrodes, simultaneously or not, continuously, periodically, randomly or at predetermined times, during the operation of the electrochemical storage system.

[0157] Thus, the potential difference between the positive electrode (respectively, the negative electrode) and the reference electrode makes it possible to measure and monitor the potential of the positive electrode (respectively, the negative electrode) relative to a known potential value, during operation of the supercapacitor.

[0158] The connections and electrical circuits external to the assembly are not shown in the figures.

[0159] The external circuit between the positive electrode (respectively, the negative electrode) and the reference electrode may be electrically connected to a voltage monitor to enable the potential of the positive electrode (respectively, the negative electrode) to be indicated or recorded.

[0160] The invention will now be described by means of the following figures and examples, given of course for illustrative and non-limiting purposes of the invention. EXAMPLE 1

[0161] Preparation according to the method of the invention of a reference electrode

[0162] 1.1. Partial chemical delithiation of LiFePO4

[0163] 5.12 g of LiFePO4 material are dispersed under an argon atmosphere in 100 mL of acetonitrile. 1.06 g of NO2BF4 (0.25 eq) is added, then the reaction medium is stirred for 48 hours, at room temperature.

[0164] The suspension is then filtered, then the powder is washed with 4 x 100 mL of acetonitrile before being dried at 60°C for 12 hours. 4.9 g of black powder are obtained.

[0165] The powder thus prepared was characterized by DRX ([Fig.2]).

[0166] The diffractogram obtained shows the coexistence of the LiFePO4 and FePO4 phases.

[0167] 1.2. Preparation of a reference electrode deposited on an aluminum collector

[0168] An ink composed of 90.5% of the material prepared in step 1.1.; 5% of VGCF (“vapor grown carbon fiber”) carbon fibers and 4.5% of polyvinylidene fluoride (PVDF) binder was prepared in N-methylpyrrolidone and coated onto an aluminum collector.

[0169] After drying and pressing at 10 tons, the electrode was assembled into a half-cell with a metallic lithium counter-electrode. Two charge / discharge cycles were carried out at a C / 10 regime.

[0170] [Fig.3] shows the evolution of voltage and current over time. [Fig.4] shows the evolution of potential (V vs Li+ / Li) with specific capacity (mAh / g), during the first two cycles.

[0171] This test shows that the starting potential of the electrode is 3.5V vs Lr7Li, and therefore well on the potential plateau, and that the state of charge of the electrode is 50%.

[0172] The composition of the electrode material is therefore Li0j5FePO4.

[0173] 1.3. Preparation of a reference electrode on an aluminum grid

[0174] An ink composed of 90.5% of the material prepared in step 1.1; 5% VGCF carbon fibers and 4.5% PVDF binder was prepared in N-methylpyrrolidone and coated onto an aluminum grid.

[0175] After drying, the coated grids are calendered until they reach a thickness of approximately 50 μm.

[0176] After calendering the coated aluminum grids, the reference electrodes are then cut.

[0177] The cut electrodes are ultrasonically welded onto aluminum connecting tabs, as shown schematically in [Fig.5]. EXAMPLE 2

[0178] Implementation of the reference electrode at the level of a battery cell

[0179] The reference electrode is introduced at the level of a lithium-ion battery cell.

[0180] The assembly is carried out in “pouch cell” format, from the following electrodes: - the reference electrode prepared according to example 1.3 above, ready for use; - a positive electrode based on LiNioj6Mno,2Cooj202 (2.9 mAh / cm2); - a negative electrode based on graphite (3.2 mAh / cm2).

[0181] The electrodes are separated by two Celgard® separators, and the assembly is impregnated with an electrolyte based on ethylene carbonate (EC) / ethyl methyl carbonate (EMC) (EC:EMC 3:7 (vol)), LiPF6 salt (1 M) and 2% by mass of vinylene carbonate (VC).

[0182] [Fig.6] schematically represents the pouch-cell format cell thus obtained.

[0183] The performance of the cell is compared with that of similar cells incorporating a conventional reference electrode based on LiFePO4 and requiring prior activation.

[0184] This reference electrode is an LFP reference electrode with the same ink and coating parameters as that of the invention, the only difference being that the LFP is incorporated in its initial state, without a prior chemical delithiation step. After fabrication, the cell was charged to C / 10, then the reference electrode was electrochemically activated.

[0185] The cell integrating a reference electrode formed according to the invention and the cell integrating a conventional reference electrode are subjected to the same electrochemical tests at 25°C, namely: - Training step (for the non-activated comparative electrode) - Galvanostatic discharge at different regimes - Galvanostatic charging at different speeds.

[0186] Figures 7 and 8 show the curves of evolution of the potential (V) with the capacity (mAh.h) for a first discharge at C / 10, a first charge at C / 2 and a last discharge at C / 2, as well as for different charge and discharge regimes.

[0187] These tests show that the results obtained are comparable between the cells integrating the conventional reference electrodes and the cell integrating the reference electrode prepared according to the invention.

[0188] On the other hand, the reference electrode does not need to be activated before being usable, unlike conventional reference electrodes.

[0189] Thus, the data can be obtained from the first charge called the “formation step” in the case of conventional electrodes. On the other hand, in the case of a conventional reference electrode, which needs to be activated beforehand within the cell in which it is implemented, the cell first undergoes a first charge or “formation step”, during which the reference electrode cannot be used. References

[0190] [1] Cengiz et al., J. Electrochem. Soc. 2021;

[0191] [2] Yamada et al. Electrochem. Solid State Lett., 2005;

[0192] [3] Poizot et al., Chem. Rev. https: / / dx.doi.org / 10.1021 / acs.chemrev.9b00482.

Claims

Claims

1. Method for preparing a reference electrode, directly functional within a cell of an electrochemical storage system, said method comprising at least the steps consisting of: (i) providing at least one electroactive material whose associated redox reaction has a constant electrochemical potential at intermediate charge states; (ii) obtaining, by chemical reaction using at least one oxidizing agent and / or at least one reducing agent, the electroactive material in an intermediate charge state; and (iii) formulating said electroactive material obtained at the end of step (ii) within an electrode, to form said reference electrode.

2. Method according to the preceding claim, in which said electroactive material in step (i) is a material capable of being oxidized, in particular is chosen from: • intercalation materials of the LiMO2 type with M representing Co, Ni or Mn; LiM'2O4 with M' representing Ni or Mn; LiM”PO4 with M” representing Fe, Co, Mn or Ni; and • electroactive organic materials of the P type whose associated redox reaction has a constant electrochemical potential, in particular chosen from compounds, in particular molecules, oligomers or polymers, carrying redox functions chosen from: - stable radicals 0', N' or NO', in particular nitroxide (N0') or phenoxy (Ph0') functions; such as for example polymers carrying side groups of 2,2,6,6-tetramethylpiperidinyl-N-oxy (TEMPO) structure; - conjugated ether (-0-) or thioether (-S-) functions;such as thianthrene, phenothiazine, and their oligomeric or polymeric derivatives; ir-conjugated conductive polymers of poly-thiophene (PT) type, for example poly(3,4-ethylenedioxythiophene); - conjugated amine functions, in particular aromatic or heteroaryl amine groups, such as dianiline, triphenylamine, polyaniline or polypyrrole, molecules of viologen or carbazole type, polyviologens and polycarbazoles; and other ir-conjugated conductive polymers, such as poly-acetylenes.;

3. A method according to any preceding claim, in wherein said electroactive material in step (i) is an insertion material of the LiM”PO4 type with M” representing Fe, Co, Mn or Ni, in particular said electroactive material in step (i) is LiFePO4.

4. A method according to claim 2 or 3, wherein step (ii) carries out a partial chemical oxidation of said electroactive material using at least one chemical oxidizing agent, in particular chosen from nitronium tetrafluoroborate (NO2BF4), nitrosyl tetrafluoroborate (NOBF4), potassium persulfate (K2S2O8), sodium nitrate (NaNO3), nitrile trifluoromethanesulfonate (NO2CF3SO3), potassium permanganate (KMnO4), nitric acid (HNO3), sulfuric acid (H2SO4), peroxydisulfuric acid (H2S2O8), peroxymonosulfuric acid (H2SO5), Magic Blue (Tris(4-bromophenyl)aminium hexachloridoantimonate), hydrogen peroxide (H2O2), lead dioxide (PbO2), organic peracids such as metachloroperbenzoic acid (mCPBA), metal cations such as Ce4+, Ag+, Cu2+, gases such as O2, O3, N2O.

5. Method according to any one of claims 2 to 4, wherein said electroactive material in step (i) is an electroactive intercalation material of the LiMO2; LiM'2O4 or LiM”PO4 type, step (ii) carrying out a partial oxidation of said material to obtain said material in an intermediate delithiation state, in particular with a delithiation rate ranging from 30% to 70% and more particularly from 50% to 60%.

6. Method according to claim 1, in which said electroactive material in step (i) is a material capable of being reduced, in particular is chosen from: • intercalation materials of the Li4Ti50i2 type; and • electroactive organic materials of the N type whose associated redox reaction has a constant electrochemical potential, in particular chosen from compounds, in particular molecules, oligomers or polymers, carrying redox functions chosen from: - conjugated azo functions (-N=N-) such as azobenzene or one of its derivatives, - disulfide functions (-SS-) such as diphenyldisulfides, tetrathionapphthalene, poly(2,5-dimercapto-1,3,4-thiadiazole), poly(5,8-dihydro-1H,4H-2,3,6,7-tetrathia-anthracene); and - conjugated carbonyl functions, in particular contained within quinonoid structures, such as for example anthraquinone; anhydride structures such as pyromellitic anhydride, dimide structures such as perylene dimide; or carboxylate structures such as perylene tetracarboxylate.

7. Method according to the preceding claim, in which step (ii) carries out a partial chemical reduction of said electroactive material using at least one reducing chemical agent, in particular chosen from alkali metals such as lithium, sodium, potassium; hydrides such as lithium hydride (LiH) and sodium borohydride (NaBH4), hydrogen, carbon, salts such as sodium sulfite (Na2SO3), sodium hydrosulfite (Na2S2O4), sodium thiosulfate (Na2S2O3), hydrazine (N2H4), lithium iodide (LiI).

8. A method according to any one of claims 1 to 5, wherein said material in step (i) is LiFePO4, step (ii) being carried out by partial chemical oxidation using an oxidizing agent, in particular by reaction with NO2BF4 as oxidizing agent in acetonitrile, to obtain a Lii xFePO4 powder, with 0.30 < x < 0.70, in particular 0.50 < x < 0.

60.

9. A method according to any one of the preceding claims, wherein said material in an intermediate charge state obtained at the end of step (ii) is in the form of a powder.

10. Method according to any one of the preceding claims, in which step (iii) of formulating said electroactive material at an electrode comprises at least the following steps: - preparation of a dispersion, called "ink", comprising, in one or more aqueous and / or organic solvents, said electroactive material obtained at the end of step (ii); one or more binders and optionally one or more electronically conductive additives; - deposition of the ink on the surface of a current collector; and - evaporation of said solvent(s) from the ink to form the electrode film; and preferably - calendering of the electrode.