Rubber composition
A rubber composition with a highly saturated diene elastomer, silica, and a specific silane coupling agent addresses the balance between wear resistance and rolling resistance in tire manufacturing, enhancing rigidity and reducing hysteresis.
Patent Information
- Application Number
- FR2022012976
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-08
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-12-08
AI Technical Summary
Existing rubber compositions used in tire manufacturing face a challenge in achieving a balance between wear resistance and low rolling resistance, as increasing tread rigidity to improve wear often leads to a significant increase in hysteretic losses and rolling resistance.
A rubber composition comprising a highly saturated diene elastomer with ethylene units exceeding 50% by mole, silica as a reinforcing filler, and a silane coupling agent of formula (G1)a(G2)aSi-Z-NH-C(O)-N=N-G4, which enhances rigidity while maintaining low hysteresis.
The composition achieves a high level of rigidity with minimal hysteresis, resulting in improved wear resistance without significantly increasing rolling resistance.
Abstract
Description
Title of the invention: Rubber composition
[0001] The field of the present invention is that of rubber compositions which comprise a silica and a highly saturated diene elastomer and which are in particular intended to be used in the manufacture of tires.
[0002] Silica-reinforced rubber compositions comprising a highly saturated diene elastomer are known, for example, from documents WO 2014114607 Al and WO 2018224776 Al. The highly saturated diene elastomer is a copolymer of ethylene and a 1,3-diene such as 1,3-butadiene and has the characteristic of containing more than 50 mol% of ethylene unit. Due to its high ethylene content and low diene unit content of less than 50 mol%, it is largely distinguished from diene elastomers that are traditionally used in rubber compositions and which generally contain more than 50 mol% of diene unit, such as polybutadienes, polyisoprenes and copolymers of 1,3-butadiene or isoprene and styrene. In particular, it has the particularity of giving a rubber composition a compromise of properties between rigidity and hysteresis which is different from that given by the diene elastomers traditionally used.
[0003] Since fuel savings and the need to preserve the environment have become a priority, it is desirable to produce mixtures having good wear resistance properties while having as low a hysteresis as possible in order to be able to implement them in the form of rubber compositions usable for the manufacture of various semi-finished products used in the composition of tires, such as for example treads, in order to obtain tires having improved wear resistance without penalizing rolling resistance.
[0004] To improve wear resistance, it is known that a certain rigidity of the tread is desirable, this stiffening of the tread being able to be obtained for example by increasing the rate of reinforcing filler in the rubber compositions constituting these treads. Unfortunately, experience shows that such stiffening of the tread penalizes in a known manner, most often in a prohibitive manner, the rolling resistance properties, being accompanied by a significant increase in the hysteretic losses of the rubber composition.
[0005] Improving stiffness performance while maintaining low rolling resistance is therefore a constant concern for tire designers. In view of the above, it is a general objective to provide com rubber positions for tires which satisfy an improved compromise of properties between stiffness and hysteresis for use in tires, particularly in treads, to improve the performance compromise between wear and rolling resistance.
[0006] The inventors have discovered a rubber composition combining both a very high level of rigidity and a very low level of hysteresis.
[0007] Thus, the invention relates to a rubber composition which comprises: - a highly saturated diene elastomer which is a copolymer of ethylene and a 1,3-diene which comprises ethylene units which represent more than 50 mol% of the monomer units of the copolymer, - a vulcanization system, - a reinforcing filler which contains silica, - and a silane coupling agent of formula (1) (Gi)3 a(G2)aSi-Z-NH-C(O)-N=N-G4 ( 1 ) in which: - Gi, identical or different, each represent a C1-C8 alkyl group, - G2, identical or different, each represent a hydroxyl group or a C1-C8 alkoxyl group, - G4 represents an aromatic group, - Z represents a C1-C8 alkanediyl group, - a is equal to 1, 2 or 3.
[0008] The invention also relates to a tire which comprises a rubber composition in accordance with the invention, preferably in its tread. Detailed description
[0009] Any interval of values designated by the expression "between a and b" represents the domain of values greater than "a" and less than "b" (i.e., limits a and b excluded) while any interval of values designated by the expression "from a to b" means the domain of values from "a" up to "b" (i.e., including the strict limits a and b
[0010] The abbreviation "pce" means parts by weight per hundred parts of elastomer (of the total elastomers if several elastomers are present).
[0011] In the present disclosure of the invention, the term a Cn-Cm group is used to designate a group having n to m carbon atoms, n being an integer greater than or equal to 1, m being an integer greater than n. For example, a Cr-C8 alkyl group designates an alkyl radical having 1 to 8 carbon atoms, a Cr-C8 alkoxyl group an alkoxy radical having 1 to 8 carbon atoms, a Cr-C8 alkanediyl group an alkanediyl radical having 1 to 8 carbon atoms, a group C6-C12 aryl an aryl radical having 6 to 12 carbon atoms.
[0012] The compounds mentioned in the description may be of fossil or bio-sourced origin. In the latter case, they may be, partially or totally, derived from biomass or obtained from renewable raw materials derived from biomass. In the same way, the compounds mentioned may also come from the recycling of materials already used, that is to say they may be, partially or totally, derived from a recycling process, or obtained from raw materials themselves derived from a recycling process.
[0013] In the present invention, the term "tyre" means a pneumatic or non-pneumatic bandage. A pneumatic bandage usually comprises two beads intended to come into contact with a rim, a crown composed of at least one crown reinforcement and a tread, two sidewalls, the tire being reinforced by a carcass reinforcement anchored in the two beads. A non-pneumatic bandage, for its part, usually comprises a base, designed for example for mounting on a rigid rim, a crown reinforcement, ensuring the connection with a tread and a deformable structure, such as spokes, ribs or cells, this structure being arranged between the base and the crown. Such non-pneumatic bandages do not necessarily comprise a sidewall. Non-pneumatic bandages are described for example in documents WO 03 / 018332 and FR2898077.According to any one of the embodiments of the invention, the tire according to the invention is preferably a pneumatic bandage.
[0014] Unless otherwise indicated, the rates of units resulting from the insertion of a monomer into a copolymer such as the copolymer useful in the invention are expressed as a molar percentage relative to the total of the monomer units of the copolymer.
[0015] The elastomer useful for the purposes of the invention is a highly saturated diene elastomer, preferably random, which comprises ethylene units resulting from the polymerization of ethylene. In a known manner, the expression "ethylene unit" refers to the -(CH2-CH2)- unit resulting from the insertion of ethylene into the elastomer chain. The highly saturated diene elastomer is rich in ethylene units, since the ethylene units represent more than 50% by mole of all the monomer units of the elastomer.
[0016] Preferably, the highly saturated diene elastomer comprises at least 60 mol% of ethylene unit, preferably at least 65 mol% of ethylene unit. In other words, the ethylene units in the highly saturated diene elastomer preferably represent at least 60 mol% of all the monomer units of the highly saturated diene elastomer, more preferably at least 65 mol% of all the monomer units of the diene elastomer. highly saturated.
[0017] Preferably, the ethylene units in the highly saturated diene elastomer represent at most 90 mol% of all the monomer units of the highly saturated diene elastomer. More preferably, the ethylene units represent at most 85 mol% of all the monomer units of the highly saturated diene elastomer. Even more preferably, the ethylene units represent at most 80 mol% of all the monomer units of the highly saturated diene elastomer.
[0018] According to an advantageous embodiment, the highly saturated diene elastomer comprises from 60% to 90% mol of ethylene unit, particularly from 60% to 85% mol of ethylene unit, molar percentage calculated on the basis of all the monomer units of the highly saturated diene elastomer. More advantageously, the highly saturated diene elastomer comprises from 60% to 80% mol of ethylene unit, molar percentage calculated on the basis of all the monomer units of the highly saturated diene elastomer.
[0019] According to another advantageous embodiment, the highly saturated diene elastomer comprises from 65% to 90% mol of ethylene unit, particularly from 65% to 85% mol of ethylene unit, molar percentage calculated on the basis of all the monomer units of the highly saturated diene elastomer. More advantageously, the highly saturated diene elastomer comprises from 65% to 80% mol of ethylene unit, molar percentage calculated on the basis of all the monomer units of the highly saturated diene elastomer.
[0020] The highly saturated diene elastomer being a copolymer of ethylene and a 1,3-diene also comprises 1,3-diene units resulting from the polymerization of a 1,3-diene. As is known, the expression "1,3-diene unit" or "diene unit" refers to the units resulting from the insertion of the 1,3-diene by a 1,4-addition, a 1,2-addition or a 3,4-addition in the case of isoprene for example. The 1,3-diene units are those for example of a 1,3-diene having 4 to 12 carbon atoms, such as 1,3-butadiene, isoprene, 1,3-pentadiene, an aryl-1,3-butadiene. Preferably, the 1,3-diene is 1,3-butadiene or a mixture of 1,3-dienes, one of which is 1,3-butadiene. More preferably, the 1,3-diene is 1,3-butadiene, in which case the highly saturated diene elastomer is a copolymer of ethylene and 1,3-butadiene, preferably random.
[0021] The highly saturated diene elastomer can be obtained according to different synthesis methods known to those skilled in the art, in particular depending on the targeted microstructure of the highly saturated diene elastomer. Generally, it can be prepared by copolymerization of at least one 1,3-diene, preferably 1,3-butadiene, and ethylene and according to known synthesis methods, in particular in the presence of a catalytic system comprising a metallocene complex. In this respect, mention may be made of catalytic systems based on metallocene complexes, which catalytic systems are described in documents EP 1 092 731, WO 2004035639, WO 2007054223 and WO 2007054224 in the name of the Applicant. The highly saturated diene elastomer, including when it is random, can also be prepared by a process using a preformed type catalytic system such as those described in documents WO 2017093654 A1, WO 2018020122 A1 and WO 2018020123 A1. Advantageously, the diene elastomer is random and is preferably prepared according to a semi-continuous or continuous process such as described in documents WO 2017103543 A1, WO 201713544 A1, WO 2018193193 and WO 2018193194.
[0022] The highly saturated diene elastomer preferably contains units of formula (I) or units of formula (II). CH -«-“CH. -CH2-CH(CH=CH2)- (H)
[0023] The presence of saturated 6-membered cyclic unit, 1,2-cyclohexanediyl, of formula (I) in the copolymer may result from a series of very particular insertions of ethylene and 1,3-butadiene into the polymer chain during its growth. When the highly saturated diene elastomer comprises units of formula (I) or units of formula (II), the molar percentages of the units of formula (I) and the units of formula (II) in the highly saturated diene elastomer, respectively o and p, preferably satisfy the following equation (eq. 1) or equation (eq. 2), o and p being calculated on the basis of all the monomer units of the highly saturated diene elastomer. 0 < o+p < 30 (eq. 1) 0 < o+p < 25 (eq. 2)
[0024] Preferably, the highly saturated diene elastomer comprises units of formula (I) in a molar ratio greater than 0% and less than 15%, more preferably less than 10% mol, molar percentage calculated on the basis of all the monomer units of the highly saturated diene elastomer.
[0025] The rubber composition may contain, in addition to the highly saturated diene elastomer, a second diene elastomer. Diene elastomer means an elastomer consisting at least in part (i.e., a homopolymer or a copolymer) of diene monomer units (monomers carrying two carbon-carbon double bonds, conjugated or not). The second elastomer can be chosen from the group of highly unsaturated diene elastomers consisting of polybutadienes, polyisoprenes, butadiene copolymers, isoprene copolymers and their mixture. A highly unsaturated elastomer is an elastomer which contains more than 50 mol% of diene units.
[0026] Preferably, the level of the highly saturated diene elastomer in the rubber composition is at least 50 parts by weight per hundred parts of elastomer of the rubber composition (phr). More preferably, the level of the highly saturated diene elastomer in the rubber composition varies in a range from 80 to 100 phr. Even more preferably, it varies in a range from 90 to 100 phr. It is advantageously 100 phr. The highly saturated diene elastomer may be a single highly saturated diene elastomer or a mixture of several highly saturated diene elastomers which differ from each other by their microstructures or by their macrostructures.In the case where the rubber composition contains several highly saturated diene elastomers which differ from each other by their microstructures or by their macrostructures, the rate of the highly saturated diene elastomer in the rubber composition relates to the mixture of highly saturated diene elastomers.
[0027] The silica used may be any reinforcing silica known to those skilled in the art, in particular any precipitated or pyrogenic silica having a BET specific surface area and a CT AB specific surface area both less than 450 m2 / g, preferably within a range from 30 to 400 m2 / g, in particular from 60 to 300 m2 / g. In this presentation, the BET specific surface area is determined by gas adsorption using the Brunauer-Emmett-Teller method described in "The Journal of the American Chemical Society" (Vol. 60, page 309, February 1938), and more precisely according to a method adapted from the standard NF ISO 5794-1, annex E of June 2010 [multipoint volumetric method (5 points) - gas: nitrogen - vacuum degassing: one hour at 160°C - relative pressure range p / po: 0.05 to 0.17]. The CT AB specific surface area values were determined according to the standard NF ISO 5794-1, annex G of June 2010.The process is based on the adsorption of CT AB (N-hexadecyl-N,N,N-trimethylammonium bromide) on the “external” surface of the reinforcing filler.
[0028] Any type of precipitated silica may be used, in particular highly dispersible precipitated silicas (known as "HDS" for "highly dispersible" or "highly dispersible silica"). These precipitated silicas, whether highly dispersible or not, are well known to those skilled in the art. Examples that may be mentioned are the silicas described in the applications WO03 / 016215-A1 and WO03 / 016387-A1. Among the commercial HDS silicas, it is possible to use in particular the silicas “Ultrasil ® 5000GR”, “Ultrasil ® 7000GR” from the company Evonik, the silicas “Zeosil ® 1085GR”, “Zeosil® 1115 MP”, “Zeosil® 1165MP”, “Zeosil® Premium 200MP”, “Zeosil® HRS 1200 MP” from the company Solvay. As non-HDS silica, the following commercial silicas can be used: silicas “Ultrasil ® VN2GR”, “Ultrasil ® VN3GR” from Evonik, silica “Zeosil® 175GR” from Solvay, silicas “Hi-Sil EZ120G(-D)”, “Hi-Sil EZ160G(-D)”, “Hi-Sil EZ200G(-D)”, “Hi-Sil 243LD”, “Hi-Sil 210”, “Hi-Sil HDP 320G” from PPG.
[0029] The reinforcing filler may comprise any type of so-called reinforcing filler other than silica, known for its ability to reinforce a rubber composition usable in particular for the manufacture of tires, for example a carbon black. Suitable carbon blacks include all carbon blacks, in particular the blacks conventionally used in tires or their treads. Among the latter, mention will be made more particularly of reinforcing carbon blacks of the 100, 200, 300 series, or blacks of the 500, 600 or 700 series (ASTM D-1765-2017 grades), such as for example blacks NI 15, N134, N234, N326, N330, N339, N347, N375, N550, N683, N772. These carbon blacks can be used in their isolated state, as commercially available, or in any other form, for example as a carrier for some of the rubber additives used.When carbon black is used in the rubber composition, it is preferably used at a rate less than or equal to 10 phr (for example, the carbon black rate may be in a range from 1 to 10 phr). Advantageously, the carbon black rate in the rubber composition is less than or equal to 5 phr. Within the ranges indicated, the coloring (black pigmenting agent) and anti-UV properties of carbon blacks are benefited from, without otherwise penalizing the typical performance provided by silica.
[0030] The silica preferably represents more than 50% by mass of the reinforcing filler. In other words, the proportion of silica in the reinforcing filler is greater than 50% by weight of the total weight of the reinforcing filler. More preferably, the silica represents more than 85% by mass of the reinforcing filler.
[0031] The total rate of reinforcing filler may vary over a wide range, for example from 30 phr to 150 phr. According to a first embodiment, the total rate of reinforcing filler varies over a range from 30 phr to 60 phr. According to a second embodiment, the total rate of reinforcing filler varies over a range from more than 60 phr to 150 phr. The first embodiment is preferred over the second embodiment for use of the rubber composition in a tread having very low rolling resistance. Any of these rate ranges total reinforcing filler may be applied to any of the embodiments of the invention.
[0032] The rubber composition in accordance with the invention has the essential characteristic of comprising a silane of formula (1) (Gûs a(G2)aSi-Z-NH-C(O)-N=N-G4 (1) in which: - Gi, identical or different, each represent a CrC8 alkyl group, - G2, identical or different, each represent a hydroxyl group or a CrC8 alkoxyl group, - G4 represents an aromatic group, - Z represents a CrC8 alkanediyl group, - a is equal to 1, 2 or 3.
[0033] The silane of formula (1) is a coupling agent (or bonding agent) intended to ensure a sufficient connection, of a chemical and / or physical nature, between the silica and the diene elastomer.
[0034] Preferably G2, identical or different, each represent a C1-C4 alkoxyl group. More preferably G2, identical or different, each represent a methoxyl or ethoxyl group.
[0035] Preferably Gi, identical or different, each represent a methyl or ethyl group.
[0036] G4 is an aromatic hydrocarbon group or an aromatic group containing a heteroatom such as a nitrogen, oxygen or sulfur atom. Preferably G4 is a C6-C12 aryl group, more preferably G4 represents a phenyl or tolyl group.
[0037] Preferably Z represents a C1-C4 alkanediyl group. More preferably Z represents a 1,3-propanediyl group.
[0038] According to any one of the embodiments of the invention, a is preferably equal to 3.
[0039] Advantageously, the silane coupling agent of formula (1) is a compound in which G2 each represents an ethoxyl group, Gi each represents a methyl group, G4 represents a phenyl group, Z represents a 1,3-propanediyl group and a is equal to 1, 2 or 3. More advantageously, the silane coupling agent of formula (1) is a compound in which G2 each represents an ethoxyl group, G4 represents a phenyl group, Z represents a 1,3-propanediyl group and a is equal to 3.
[0040] The silane coupling agent of formula (1) can be prepared according to the synthesis methods described in patent application WO2015162053A1.
[0041] In the rubber composition according to the invention, the level of the silane coupling agent of formula (1) is adjusted by a person skilled in the art according to the surface area specific to the silica used in the rubber composition and according to the silica content in the rubber composition. According to any one of the embodiments of the invention, it preferably varies from 1 to 15 phr, more preferably from 1.5 to 10 phr, even more preferably from 2 to 5 phr.
[0042] The rubber composition according to the invention has the further essential characteristic of containing a vulcanization system, that is to say a sulfur-based crosslinking system. The sulfur is typically provided in the form of molecular sulfur or a sulfur-donating agent, preferably in molecular form. Sulfur in molecular form is also referred to as molecular sulfur. The term “sulfur donor” means any compound which releases sulfur atoms, combined or not in the form of a polysulfide chain, capable of being inserted into the polysulfide chains formed during vulcanization and bridging the elastomer chains. In addition to the vulcanization system, various known secondary accelerators or vulcanization activators such as zinc oxide, stearic acid, etc. are incorporated during the first non-productive phase and / or during the productive phase.The sulfur content is preferably between 0.5 and 4 pce, that of the primary accelerator is preferably between 0.5 and 5 pce. These preferential rates can apply to any of the embodiments of the invention.
[0043] Any compound capable of acting as a vulcanization accelerator (primary or secondary) may be used which is capable of acting as a vulcanization accelerator for diene elastomers in the presence of sulfur, in particular accelerators of the thiazole type and their derivatives, accelerators of the sulfenamide type for primary accelerators, and accelerators of the thiuram, dithiocarbamate, dithiophosphate, thiourea and xanthate type for secondary accelerators. Examples of primary accelerators include, in particular, sulfenamide compounds such as N-cyclohexyl-2-benzothiazyl sulfenamide ("CBS"), N,N-dicyclohexyl-2-benzothiazyl sulfenamide ("DCBS"), N-tert-butyl-2-benzothiazyl sulfenamide ("TBBS"), and mixtures of these compounds. The primary accelerator is preferably a sulfenamide, more preferably N-cyclohexyl-2-benzothiazyl sulfenamide.Examples of secondary accelerators include thiuram disulfides such as tetraethylthiuram disulfide, tetrabutylthiuram disulfide ("TBTD"), tetrabenzylthiuram disulfide ("TBZTD") and mixtures of these compounds. The secondary accelerator is preferably a thiuram disulfide, more preferably tetrabenzylthiuram disulfide.
[0044] The vulcanization is carried out in a known manner at a temperature generally between 130°C and 200°C, for a sufficient time which may vary by example between 5 and 90 min depending in particular on the cooking temperature, the vulcanization system adopted and the vulcanization kinetics of the composition considered.
[0045] The rubber composition in accordance with the invention may also comprise all or part of the usual additives normally used in elastomer compositions intended for the manufacture of tires, in particular pigments, protective agents such as anti-ozone waxes, chemical anti-ozonants, antioxidants, plasticizers such as plasticizing oils or resins.
[0046] The rubber composition, before vulcanization, can be manufactured in suitable mixers, using two successive preparation phases according to a procedure well known to those skilled in the art: a first thermo-mechanical working or kneading phase (sometimes referred to as a "non-productive" phase) at high temperature, up to a maximum temperature of between 110°C and 190°C, preferably between 130°C and 180°C, followed by a second mechanical working phase (sometimes referred to as a "productive" phase) at a lower temperature, typically below 110°C, for example between 40°C and 100°C, a finishing phase during which the sulfur or sulfur donor and the vulcanization accelerator are incorporated.
[0047] For example, the first (non-productive) phase is carried out in a single thermomechanical step during which all the necessary constituents, any additional processing agents and other various additives, with the exception of the vulcanization system, are introduced into a suitable mixer such as a conventional internal mixer. The total mixing time in this non-productive phase is preferably between 1 and 15 min. After cooling the mixture thus obtained during the first non-productive phase, the vulcanization system is then incorporated at low temperature, generally in an external mixer such as a roller mixer, and the whole is then mixed (productive phase) for a few minutes, for example between 2 and 15 min.
[0048] The rubber composition may be calendered or extruded in the form of a sheet or plate, in particular for laboratory characterization, or in the form of a semi-finished (or profiled) rubber usable in a tire. The composition may be either in the raw state (before crosslinking or vulcanization), or in the cured state (after crosslinking or vulcanization). It may constitute all or part of a semi-finished article, in particular intended to be used in a pneumatic or non-pneumatic tire which comprises a tread, in particular in the tread of the tire.
[0049] In summary, the invention is advantageously implemented according to any one of the following embodiments 1 to 29:
[0050] Mode 1: Rubber composition which comprises: - a highly saturated diene elastomer which is a copolymer of ethylene and a 1,3-diene which comprises ethylene units which represent more than 50 mol% of the monomer units of the copolymer, - a vulcanization system, - a reinforcing filler which contains silica, - and a silane coupling agent of formula (1) (GJs a(G2)aSi-Z-NH-C(O)-N=N-G4 (1) in which: - Gi, identical or different, each represent a CrC8 alkyl group, - G2, identical or different, each represent a hydroxyl group or a CrC8 alkoxyl group, - G4 represents an aromatic or heteroaromatic group, - Z represents a CrC8 alkanediyl group, - a is equal to 1, 2 or 3.
[0051] Mode 2: Rubber composition according to mode 1 in which the 1,3-diene is 1,3-butadiene or a mixture of 1,3-dienes, one of which is 1,3-butadiene.
[0052] Mode 3: Rubber composition according to mode 1 or 2 in which the 1,3-diene is 1,3-butadiene.
[0053] Mode 4: Rubber composition according to any one of modes 1 to 3 in which the ethylene units in the highly saturated diene elastomer represent at least 60 mol% of all the monomer units of the highly saturated diene elastomer.
[0054] Mode 5: Rubber composition according to any one of modes 1 to 4 in which the ethylene units in the highly saturated diene elastomer represent at least 65 mol% of all the monomer units of the highly saturated diene elastomer.
[0055] Mode 6: Rubber composition according to any one of modes 1 to 5 in which the ethylene units in the highly saturated diene elastomer represent at least 70 mol% of all the monomer units of the highly saturated diene elastomer.
[0056] Mode 7: Rubber composition according to any one of modes 1 to 6 in which the ethylene units in the highly saturated diene elastomer represent at most 90 mol% of all the monomer units of the highly saturated diene elastomer.
[0057] Mode 8: Rubber composition according to any one of modes 1 to 7 in which the ethylene units in the highly saturated diene elastomer represent at most 85 mol% of all the monomer units of the diene elastomer highly saturated.
[0058] Mode 9: Rubber composition according to any one of modes 1 to 8 in which the ethylene units in the highly saturated diene elastomer represent at most 80 mol% of all the monomer units of the highly saturated diene elastomer.
[0059] Mode 10: Rubber composition according to any one of modes 1 to 9 in which the highly saturated diene elastomer contains units of formula (I) or units of formula (II). -CH2-CH(CH=CHs)- (H)
[0060] Mode 11: Rubber composition according to any one of modes 1 to 10 in which the highly saturated diene elastomer comprises units of formula (I) in a molar ratio greater than 0% and less than 15%, molar percentage calculated on the basis of all the monomer units of the highly saturated diene elastomer. ch2—ch2 CH2 / \:H2 CH— CH (O
[0061] Mode 12: Rubber composition according to any one of modes 1 to 11 in which the highly saturated diene elastomer comprises units of formula (I) in a molar ratio greater than 0% and less than 10% mol, molar percentage calculated on the basis of all the monomer units of the highly saturated diene elastomer.
[0062] Mode 13: Rubber composition according to any one of modes 1 to 12 in which the highly saturated diene elastomer is a random copolymer.
[0063] Mode 14: Rubber composition according to any one of modes 1 to 13 in which the level of the highly saturated diene elastomer is at least 50 parts by weight per hundred parts of elastomer of the rubber composition (pce).
[0064] Mode 15: Rubber composition according to any one of modes 1 to 14 in which the content of the highly saturated diene elastomer varies in a range from 80 to 100 pce.
[0065] Mode 16: Rubber composition according to any one of modes 1 to 15 in which the total level of reinforcing filler varies in a range from 30 to 150 pce.
[0066] Mode 17: Rubber composition according to any one of modes 1 to 16 in which the total rate of reinforcing filler varies in a range from 30 pce to 60 pce.
[0067] Mode 18: Rubber composition according to any one of modes 1 to 17 in which the silica represents more than 50% by mass of the reinforcing filler.
[0068] Mode 19: Rubber composition according to any one of modes 1 to 18 in which the silica represents more than 85% by mass of the reinforcing filler.
[0069] Mode 20: Rubber composition according to any one of modes 1 to 19 in which G2, identical or different, each represents a CrC4 alkoxyl group.
[0070] Mode 21: Rubber composition according to any one of modes 1 to 20 in which G2, identical or different, each represent a methoxyl or ethoxyl group.
[0071] Mode 22: Rubber composition according to any one of modes 1 to 21 in which Gb, identical or different, each represents a methyl or ethyl group.
[0072] Mode 23: Rubber composition according to any one of modes 1 to 22 in which G4 is a C6-C12 aryl group.
[0073] Mode 24: Rubber composition according to any one of modes 1 to 23 in which G4 represents a phenyl or tolyl group.
[0074] Mode 25: Rubber composition according to any one of modes 1 to 24 in which Z represents a CrC4 alkanediyl group.
[0075] Mode 26: Rubber composition according to any one of modes 1 to 25 in which Z represents a 1,3-propanediyl group.
[0076] Mode 27: Rubber composition according to any one of modes 1 to 26 in which a is equal to 3.
[0077] Mode 28: A tire which comprises a rubber composition defined in any one of modes 1 to 27.
[0078] Mode 29: Tire which comprises a rubber composition defined at one any of modes 1 to 27 in its tread.
[0079] The above-mentioned characteristics of the present invention, as well as others, will be better understood upon reading the following description of several exemplary embodiments of the invention, given for illustrative and non-limiting purposes. Examples
[0080] Dynamic properties The dynamic properties G* and tan(ô)max are measured on a viscoanalyzer (Metravib VA4000), according to the ASTM D 5992-96 standard. The response of a sample of vulcanized composition (cylindrical specimen 4 mm thick and 400 mm2 in cross-section) is recorded, subjected to sinusoidal stress in alternating simple shear, at a frequency of 10 Hz, under normal temperature conditions (23°C) according to the ASTM D 1349-99 standard. A strain amplitude sweep is carried out from 0.1% to 100% (forward cycle), then from 100% to 0.1% (return cycle). The results used are the complex dynamic shear modulus (G*), the loss factor tan(ô) and the modulus difference AG* between the values at 0.1 and 50% strain (Payne effect). For the return cycle, we indicate the maximum value of tan(ô) observed, noted tan(ô)max.
[0081] The results used are the complex shear modulus G*, the loss factor tan(ô) and the difference in modulus AG* between the values at 0.1 and 50% deformation (Payne effect). For the return cycle, the maximum value of tan(ô) observed is indicated, noted tan(ô)max. The complex modulus G* at 50% deformation, noted G*, the difference in modulus AG* between the values 0.1 and 50% deformation (Payne effect) and the value of tan(ô)max are given on the basis of 100, the value 100 being attributed to the control composition (T).
[0082] The response of the vulcanized composition sample (cylindrical specimen 4 mm thick and 400 mm2 in cross-section) is also recorded, subjected to sinusoidal stress in alternating simple shear at an imposed stress of 0.7 MPa and at a frequency of 10 Hz, during a temperature sweep, from a minimum temperature lower than the Tg of the elastomers of the compositions up to a maximum temperature higher than 100°C. The results used are the complex dynamic shear modulus (G*); the values of G* are taken at a temperature of 60°C.
[0083] The stiffness (G*) and hysteresis (tan(ô)max and AG*) results are expressed on a base of 100 relative to a control taken as a reference. A value lower than 100 indicates a lower value than that of the control. The lower the value of AG*, the lower the non-linearity which is a source of hysteresis. The lower the value of tan(ô)max, the lower the hysteresis of the rubber composition. The lower the value of G*, the lower the stiffness of the composition.
[0084] Microstructure of elastomers by nuclear magnetic resonance analysis (NMR): The microstructure of the elastomers is determined by 'H NMR analysis, supplemented by 13C NMR analysis when the resolution of the 'H NMR spectra does not allow the attribution and quantification of all species. The measurements are carried out using a BRUKER 500MHz NMR spectrometer at frequencies of 500.43 MHz for proton observation and 125.83MHz for carbon observation. For non-soluble elastomers that have the ability to swell in a solvent, a 4mm z-grad HRMAS probe is used to observe the proton and carbon in proton-decoupled mode. Spectra are acquired at rotation speeds of 4000Hz to 5000Hz. For measurements on soluble elastomers, a liquid NMR probe is used to observe the proton and carbon in proton-decoupled mode. The preparation of insoluble samples is carried out in rotors filled with the analyzed material and a deuterated solvent allowing swelling, generally deuterated chloroform (CDCl3). The solvent used must always be deuterated and its chemical nature can be adapted by the person skilled in the art. The quantities of material used are adjusted so as to obtain spectra with sufficient sensitivity and resolution. Soluble samples are dissolved in a deuterated solvent (approximately 25 mg of elastomer in 1 ml), generally deuterated chloroform (CDCl3). The solvent or solvent blend used must always be deuterated and its chemical nature can be adapted by those skilled in the art. In both cases (soluble sample or swollen sample): For proton NMR, a single 30° pulse sequence is used. The spectral window is adjusted to observe all the resonance lines belonging to the analyzed molecules. The accumulation number is adjusted to obtain a sufficient signal-to-noise ratio for the quantification of each pattern. The recycling time between each pulse is adapted to obtain a quantitative measurement. For carbon NMR, a single 30° pulse sequence is used with proton decoupling only during acquisition to avoid “Nuclear Overhauser” (NOE) effects and to remain quantitative. The spectral window is adjusted to observe all the resonance lines belonging to the analyzed molecules. The accumulation number is adjusted to obtain a sufficient signal-to-noise ratio for the quantification of each pattern. The recycling delay between each pulse is adapted to obtain a quantitative measurement. NMR measurements are performed at 25°C.
[0085] Glass transition temperature: The glass transition temperatures, Tg, of polymers are measured using a differential scanning calorimeter. The analysis is performed according to the requirements of ASTM D3418-08.
[0086] Moonev Viscosity: The Mooney viscosity is measured using an oscillating consistometer as described in ASTM D1646 (1999). The measurement is carried out according to the following principle: the sample analyzed in the raw state (i.e., before curing) is molded (shaped) in a cylindrical enclosure heated to a given temperature (100°C). After 1 minute of preheating, the rotor rotates within the test piece at 2 revolutions / minute and the torque used to maintain this movement is measured after 4 minutes of rotation. The Mooney viscosity (ML) is expressed in "Mooney units" (MU, with 1 MU = 0.83 Newton.meters).
[0087] Preparation of rubber compositions: Two rubber compositions are prepared. The manufacturing of these compositions is carried out as follows: The elastomer, then the silica, the silane coupling agent, and the various other ingredients, with the exception of the vulcanization system, are introduced into an internal mixer (final filling rate: approximately 70% by volume), whose initial tank temperature is approximately 80°C. Thermomechanical work (non-productive phase) is then carried out in one step, lasting approximately 5 to 6 minutes, until a maximum "fall" temperature of 160°C is reached. The mixture thus obtained is recovered, cooled, and then sulfur and a sulfenamide-type accelerator are incorporated into a mixer (homo-finisher) at 23°C, mixing everything (productive phase) for an appropriate time (for example, between 5 and 12 minutes).
[0088] The compositions thus obtained are then calendered, either in the form of plates (with a thickness ranging from 2 to 3 mm) or thin sheets of rubber, for the measurement of their physical or mechanical properties after vulcanization at 150°C (cooked state), or in the form of profiles which can be used directly, after cutting and / or assembling to the desired dimensions, for example as semi-finished products for tires.
[0089] The formulations (in pce) of the rubber compositions are described in Table 2 (Table 2).
[0090] The rubber compositions all contain a highly saturated diene elastomer, elastomer E1, a vulcanization system, and a silica. The rubber composition T1 is a control composition since it contains a silane coupling agent, TESPT, conventionally used in diene rubber compositions reinforced with a silica and intended for use in a tire. The composition C1, which contains an azosilane coupling agent corresponding to formula (1), is in accordance with the invention. The azosilane is the compound of formula (EtO)3Si(CH2)3 - NH-C(=O)-N=N-Ph in which the symbol Ph denotes a phenyl group. It is prepared according to the procedure described in document WO2015162053A1.
[0091] The formulations (in pce) of the rubber compositions Tl and Cl are described in Table 1 (Table 1). The total sulfur content is identical for each of the rubber compositions, knowing that in the case of the rubber composition Tl, the coupling agent “Si69” releases free sulfur during its reaction with Telastomer, which represents a source of sulfur available for vulcanization, i.e. 0.3 pce. The coupling agents are introduced into the rubber compositions at iso rate of alkoxysilane function.
[0092] Elastomer El is a copolymer of ethylene and 1,3-butadiene prepared according to the following procedure: In a 70 L reactor containing methylcyclohexane (64 L), ethylene (5600 g) and 1,3-butadiene (2948 g), butyloctylmagnesium (BOMAG) dissolved in methylcyclohexane and the catalytic system is added. The Mg / Nd ratio is 6.2. The volume of the solution of the catalytic system introduced is 840 mL, the concentration of the catalytic system solution in Nd being 0.0065 M. The reaction temperature is regulated at a temperature of 80 ° C and the polymerization reaction starts. The polymerization reaction proceeds at a constant pressure of 8.3 bar. The reactor is supplied throughout the polymerization with ethylene and 1,3-butadiene in the molar proportions 73 / 27. The polymerization reaction is stopped by cooling, degassing the reactor and adding ethanol. An antioxidant is added to the polymer solution. The copolymer is recovered after steam stripping and drying to constant mass.The polymerization time is 225 minutes. The weighted mass (6.206 kg) allows the average catalytic activity of the catalytic system to be determined, expressed in kilograms of synthesized polymer per mole of neodymium metal per hour (kg / mol.h). The copolymer has an ML value of 62. The catalytic system is a preformed catalytic system. It is prepared in methylcyclohexane from a metallocene, [Me2Si(Flu)2Nd(q-BH4)2Li(THF)] at 0.0065 mol / L, a co-catalyst, butyloctylmagnesium (BOMAG) whose BOMAG / Nd molar ratio is equal to 2.2, and a preformed monomer, 1,3-butadiene whose 1,3-butadiene / Nd molar ratio is equal to 90. The medium is heated to 80°C for a period of 5 hours. It is prepared according to a preparation method in accordance with paragraph II. 1 of patent application WO 2017093654 AL
[0093] The results of the properties after curing of the rubber compositions are recorded in Table 2. Compared to composition Tl, composition Cl has a higher rigidity without the hysteresis being increased, even the hysteresis is greatly decreased. [Tables 1] Compositions (in pce) Tl Cl EBR(l) 100 100 Silica (2) 38 38 Coupling agent Si69 (3) 3.1 Azosilane coupling agent (4) 4.3 Wax Ozone (5) 1 1 Antioxidant (6) 2 2 Stearic acid (7) 2 2 ZnO (8) 2.4 2.4 Sulphur 1 1.3 CBS (9) 1 1 (1) Copolymer of ethylene and 1,3-butadiene containing 73.8 mol% of ethylene, 11.9 mol% of 1,2-butadiene units, 6.7 mol% of 1,4-butadiene units and 7.6 mol% of 1,2-cyclohexane rings, of ML 62 (2) “Zeosil 1165 MP” from Solvay-Rhodia in the form of microbeads (3) Liquid silane triethoxysilylpropyltetrasulfide (TESPT) “Si69” from Evonik (4) Silane azosilane (EtO)3Si(CH2)3-NH-C(=O)-N=N-Ph (5) Anti-ozone wax “VARAZON 4959” from the company Sasol Wax (6) N-(l,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine “Santoflex 6PPD” from Flexys (7) Stearic acid “Pristerene 4931” from Uniqema (8) Industrial grade Zinc Oxide from Umicore (9) N-cyclohexyl-2-benzothiazol-sulfenamide “Santocure CBS” from Flexsys [Tables 2] Composition Tl Cl AG 23°C 100 65 Tanô max return 23° 100 75 G* 60°C 100 127
Claims
Claims
1. A rubber composition which comprises: - a highly saturated diene elastomer which is a copolymer of ethylene and a 1,3-diene which comprises ethylene units which represent more than 50 mol% of the monomer units of the copolymer, - a vulcanization system, - a reinforcing filler which contains a silica, - and a silane coupling agent of formula (1) (Gi)3_a(G2)aSi-Z-NH-C(O)-N=N-G4(l) in which: - Gi, which may be identical or different, each represent a C i-C8 alkyl group, - G2, which may be identical or different, each represent a hydroxyl group or a CrC8 alkoxyl group, - G4 represents an aromatic group, - Z represents a CrC8 alkanediyl group, - a is equal to 1, 2 or 3.
2. A rubber composition according to claim 1 wherein the 1,3-diene is 1,3-butadiene or a mixture of 1,3-dienes one of which is 1,3-butadiene, preferably 1,3-butadiene.
3. A rubber composition according to any one of claims 1 to 2 wherein the ethylene units in the highly saturated diene elastomer represent at least 60 mol% of all the monomer units of the highly saturated diene elastomer, preferably at least 65 mol% of all the monomer units of the highly saturated diene elastomer.
4. A rubber composition according to any one of claims 1 to 3 wherein the ethylene units in the highly saturated diene elastomer represent at most 90 mol% of all the monomer units of the highly saturated diene elastomer, preferably at most 85 mol% of all the monomer units of the highly saturated diene elastomer.
5. A rubber composition according to any one of claims 1 to 4 wherein the ethylene units in the highly saturated diene elastomer represent at most 80 mol% of all the monomer units of the highly saturated diene elastomer.
6. A rubber composition according to any one of claims 1
7.
8.
9.
10.
11.
12.
13.
14.
15. to 5 in which the highly saturated diene elastomer is a random copolymer. Rubber composition according to any one of claims 1 to 6 in which the silica represents more than 50% by mass of the reinforcing filler, preferably more than 85% by mass of the reinforcing filler. Rubber composition according to any one of claims 1 to 7 in which G2, identical or different, each represents a C1-C4 alkoxyl group. Rubber composition according to any one of claims 1 to 8 in which G2, identical or different, each represents a methoxyl or ethoxyl group. Rubber composition according to any one of claims 1 to 9 in which Gi, identical or different, each represents a methyl or ethyl group. A rubber composition according to any one of claims 1 to 10 wherein G4 represents a phenyl or tolyl group. A rubber composition according to any one of claims 1 to 11 wherein Z represents a C1-C4 alkanediyl group. A rubber composition according to any one of claims 1 to 12 wherein Z represents a 1,3-propanediyl group. A rubber composition according to any one of claims 1 to 13 wherein a is equal to 3. Tire which comprises a rubber composition defined in any one of claims 1 to 14, preferably in its tread.