PtSnK-based dehydrogenation catalyst for paraffins and / or naphthenes on a gamma alumina support
A catalyst with specific alkaline earth elements on a gamma alumina support improves the dehydrogenation of propane to propylene, addressing activity and stability issues in existing catalysts by enhancing conversion rates and reducing secondary reactions.
Patent Information
- Application Number
- FR2023003931
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-25
AI Technical Summary
Existing dehydrogenation catalysts for paraffins and naphthenes, particularly for converting propane to propylene, suffer from limited activity, selectivity, and stability, with high temperatures leading to secondary reactions and catalyst deactivation.
A catalyst comprising a specific weight percentage content and surface density of alkaline or alkaline earth elements on a gamma alumina support, with a defined specific surface area, combined with Group VIII metals like platinum, enhances activity, selectivity, and stability.
The catalyst achieves improved conversion rates of propane to propylene with reduced secondary reactions and lower catalyst deactivation, maintaining high selectivity and stability over time.
Abstract
Description
Title of the invention: Paraffin and / or naphthenes dehydrogenation catalyst based on PtSnK on a gamma alumina support Field of the invention
[0001] The present invention relates to the field of the conversion of hydrocarbon compounds, more specifically to the dehydrogenation of a hydrocarbon feedstock comprising paraffinic compounds and / or naphthenic compounds, and more particularly to the dehydrogenation of propane in the presence of a catalyst to produce olefins and more particularly propylene. State of the art
[0002] Paraffin and / or naphthenes dehydrogenation processes are interesting routes for the dedicated production of unsaturated compounds and particularly olefins, the demand for which in global production is increasing. Indeed, among the possible routes for the production of olefins, such as thermal or catalytic cracking, metathesis as well as alcohol dehydration, paraffin and / or naphthenes dehydrogenation processes have higher yields and are very selective. The production of propylene in particular is of particular appeal in a context of increased demand for polypropylene and propylene derivatives such as acrylic acid or acrylonitrile. The need for optimization of catalysts and processes is therefore always present.
[0003] The dehydrogenation reactions of paraffins and / or naphthenes are highly endothermic and reversible. Conversion rates are limited by the conditions of thermodynamic equilibrium. In the case of propane dehydrogenation (AH = - 125 kJ / mol), a high temperature above 600°C is conventionally used and the equilibrium conversion under these conditions is of the order of 30% in industrial conditions. Since the separation of olefin from paraffin is a costly step in terms of investment and energy, it is essential to work towards maximum conversion of the feedstock to maximize the productivity of the process.
[0004] The severe conditions allowing this are thus very favorable to the secondary reactions of deep dehydrogenation, oligomerization of olefins, hydrogenolysis, cracking and coke formation. These secondary products and this coke formation are at the origin of the deactivation of the dehydrogenation catalysts and involve the regeneration of the catalyst, and in particular of the metallic phase, by at least one combustion step. The challenge is therefore to succeed in developing an active but also selective and stable catalyst for an economical process. unsustainably viable.
[0005] Among the catalysts suitable for the dehydrogenation of paraffins and more particularly for the dehydrogenation implemented in a moving bed process known as CCR (Continuing Catalytic Reforming) in English terminology, mention may in particular be made of platinum (Pt)-based catalysts and more particularly PtSnK type catalysts.
[0006] Numerous works of the prior art describe this type of dehydrogenation catalysts and the means implemented to improve their activity, selectivity and stability.
[0007] For example, US patent 4,430,517 discloses a process for the dehydrogenation of paraffins, and in particular for the dehydrogenation of isobutane to isobutylene in the presence of a catalyst based on PtSnK on a support based on alumina of gamma crystallographic nature. The content of alkali or alkaline-earth compound is between 0.01 and 15% by weight relative to the total weight of the catalyst, and the specific surface area of the support may be between 25 and 500 m2 / g, which corresponds to a surface density of potassium, which is the preferred alkali element, between 0.003 and 95 K atoms / nm2.
[0008] To adapt the catalyst to the dehydrogenation of propane, US patent 4,914,075 teaches that it is essential to carry out a high-temperature calcination, i.e. between 1000°C and 1200°C, of the alumina support containing tin in order to increase the average pore size of said support and thus promote the diffusion of heavy species and limit deactivation. This results in a reduction in the specific surface area of the support, an increase in the density and a modification of the crystalline phase of the alumina from gamma to a predominantly theta alumina (> 75% by weight relative to the total weight of the alumina). The content of alkali element or alkaline-earth element may be between 0.01 and 10% by weight for a support which may comprise a specific surface area between 50 and 120 m2 / g, which corresponds to a surface density of cesium, which is the preferred alkali element, between 0.004 and 9 Cs atoms / nm2.
[0009] Patent application US2003 / 0191351 discloses a catalytic composition based on PtSnK with a content of alkaline earth element, preferably potassium, of between 0.9 and 1.1% by weight and a support with a specific surface area which may be between 50 and 120 m2 / g, which corresponds to a surface density of potassium of between 1.15 and 3.4 atoms K / nm2. The crystalline phase of the alumina is predominantly in theta form, preferably > 75% by weight relative to the total weight of the alumina.
[0010] Patent application US2021 / 0053034 discloses a catalyst whose alumina support is obtained by a calcination step at a temperature between 900°C and 950°C. This results in a support with a reduction in specific surface area and the production of an alumina support with a predominantly delta crystallographic phase (>75%). The alkaline earth element content may be between 0.01 and 5.0% by weight, and the support may have a specific surface area of between 114 and 150 m2 / g, which corresponds to a surface density of potassium element, the preferred alkaline element, of between 0.01 and 6.75 K atoms / nm2.
[0011] Finally, US patent 8,993,474 discloses a catalyst whose alumina support containing tin is obtained by a calcination step carried out for 6 hours at 1050°C allowing the production of a support with a theta crystallinity greater than 90% by weight relative to the total weight of the alumina and having mesopore and macropore sizes respectively between 5 and 100 nm and between 0.1 and 20 pm. Such a type of catalyst has improved performance compared to those whose supports have not undergone a high-temperature calcination step. The content of alkali or alkaline-earth elements can be between 0.05 and 3.0% by weight for a support whose specific surface can be between 50 and 170 m2 / g, which corresponds to a surface density of potassium between 0.045 and 9.25 atK / nm2.
[0012] There is nevertheless still a need to develop new catalysts having improved performances in terms of activity, selectivity and stability for the dehydrogenation reactions of paraffins and / or naphthenes, and more particularly for the dehydrogenation reaction of propane to propylene.
[0013] The Applicant, in its research into improving the performance of heterogeneous catalysts for the dehydrogenation of paraffins and / or naphthenes, has surprisingly discovered that the performance of such catalysts, in terms of activity, selectivity and stability, is maximized by selecting a catalyst comprising a specific weight percentage content and surface density of alkali or alkaline-earth element, on a gamma-type alumina support comprising a well-defined specific surface area. Objects of the invention
[0014] The subject of the present invention is a catalyst comprising an active phase based on at least one metal from group VIII, at least one element M1 chosen from tin, germanium, lead, gallium, indium and thallium, at least one element M2 chosen from alkali or alkaline-earth elements and at least one element X chosen from halogens, and a support comprising at least one refractory oxide, characterized in that:
[0015] - the content of element M2, expressed in element, is between 0.4 and 8% by weight relative to the total weight of the catalyst;
[0016] - the surface density of the element M2 is between 0.5 and 1.5 atoms M2 / nm2; And
[0017] - the support is a gamma alumina comprising a specific surface area between 170 and 250 m2 / g.
[0018] According to one or more embodiments, the surface density of the alkali or alkaline-earth element is between 0.55 and 1.2 atoms of element M2 / nm2.
[0019] According to one or more embodiments, the content of group VIII metal is between 0.02 and 2% by elemental weight of group VIII metal relative to the total weight of the catalyst.
[0020] According to one or more embodiments, the content of element Ml is between 0.01 and 10% by elemental weight of element Ml relative to the total weight of the catalyst.
[0021] According to one or more embodiments, the group VIII metal is platinum.
[0022] According to one or more embodiments, the element Ml is tin.
[0023] According to one or more embodiments, the element M2 chosen from the elements alkali or alkaline earth is potassium.
[0024] According to one or more embodiments, the potassium content, expressed as an element, is between 0.5 and 3% by weight relative to the total weight of the catalyst.
[0025] According to one or more embodiments, said support comprises a specific surface area of between 185 and 220 m2 / g.
[0026] According to one or more embodiments, said support has a packed filling density value of between 0.50 and 0.70 g / mL.
[0027] According to one or more embodiments, the surface density of the element X chosen from halogens is between 1 and 2.75 atoms X / nm2.
[0028] According to one or more embodiments, the atomic ratio X / M2 is between 1.5 and 2.5.
[0029] According to one or more embodiments, the element X is chlorine.
[0030] Another object according to the invention relates to a process for preparing a catalyst according to the invention comprising the following steps:
[0031] a) a support is prepared comprising the element Ml chosen from tin, germanium, lead, gallium, indium and thallium to obtain a first catalyst precursor;
[0032] b) the first catalyst precursor obtained in step a) is dried under a flow of a neutral gas or under a flow of a gas containing oxygen at a temperature less than or equal to 250°C, then calcined at a temperature between 350°C and 750°C to obtain a first dried and calcined catalyst precursor;
[0033] c) the first dried and calcined catalyst precursor obtained in step b) is impregnated with an impregnation solution comprising at least one precursor of at least one metal from group VIII, and optionally at least one precursor of an element X, X being chosen from halogens, and optionally phosphorus, to obtain a second catalyst precursor;
[0034] d) the second catalyst precursor obtained in step c) is dried under a flow of a neutral gas or under a flow of a gas containing oxygen at a temperature less than or equal to 250°C, then calcined at a temperature between 350°C and 650°C to obtain a second dried and calcined catalyst precursor;
[0035] e) the second dried and calcined catalyst precursor obtained in step d) is impregnated with an impregnation solution comprising a precursor of at least one element M2, and optionally at least one precursor of an element X, to obtain a third catalyst precursor;
[0036] f) the third catalyst precursor obtained in step e) is dried under a flow of a neutral gas or under a flow of a gas containing oxygen at a temperature less than or equal to 250°C, then calcined at a temperature between 350°C and 650°C,
[0037] it being understood that the precursor of element X is supplied at least once in step c) and / or in step e).
[0038] Another subject according to the invention relates to a process for dehydrogenation of a hydrocarbon feedstock comprising paraffins and / or naphthenes in which said feedstock and a catalyst according to the invention, or prepared according to the invention, are brought into contact at a pressure of between 0.1 MPa and 4 MPa, at a temperature of between 200°C and 800°C, and with a liquid volumetric space velocity of between 0.5 h 1 and 50 h 1 Detailed description of the invention 1. Definitions
[0039] In the following, the groups of chemical elements are given according to the CAS classification (CRC Handbook of Chemistry and Physics, publisher CRC press, editor-in-chief DR Lide, 81st edition, 2000-2001). For example, group VIII according to the CAS classification corresponds to the metals of columns 8, 9 and 10 according to the new IUP AC classification.
[0040] Specific surface area means the BET specific surface area (SBet in m2 / g) determined by nitrogen adsorption in accordance with standard ASTM D 3663-78 established from the BRUNAUER-EMMETT-TELLER method described in the periodical "The Journal of American Society", 1938, 60, 309.
[0041] The total pore volume of the catalyst or support used for the preparation of the catalyst is understood to mean the volume measured by intrusion with a mercury porosimeter according to standard ASTM D4284 at a maximum pressure of 4000 bars (400 MPa), using a surface tension of 484 dyne / cm and a contact angle of 140°, for example with an Autopore III model device from the Microméritics® brand.
[0042] The wetting angle was taken equal to 140° following the recommendations of the work "Techniques de l'ingénieur, traité analyse et caractérisation", pages 1050-1055, written by Jean Charpin and Bernard Rasneur. In order to obtain better precision, the value of the total pore volume corresponds to the value of the total pore volume measured by intrusion with a mercury porosimeter measured on the sample at 4000 bars (400 MPa) minus the value of the total pore volume measured by intrusion with a mercury porosimeter measured on the same sample for a pressure corresponding to 2 bars (0.2 MPa).
[0043] The packed filling density (DRT) of the support or catalyst is measured by introducing the support or catalyst into a test tube (typically of volume 100 mL) whose volume has been previously determined and then, by vibration, packing it until a constant volume is obtained. The apparent density of the packed product is calculated by dividing the mass introduced by the volume occupied after packing. The uncertainty in the measurement is generally of the order of ± 0.01 g / mL.
[0044] The contents of metals, halogen and alkali or alkaline-earth elements are measured by X-ray fluorescence.
[0045] By paraffinic compound (also called indifferently paraffinic hydrocarbon or more simply paraffin), we mean hydrocarbon compounds of general empirical formula CnH2n+2-
[0046] By naphthenic compound (also called indifferently naphthenic hydrocarbon or more simply napthene), we mean hydrocarbon compounds comprising at least one non-aromatic saturated cycle.
[0047] Activity means the mass of converted paraffin expressed in grams of converted paraffin per gram of active metal per hour.
[0048] By selectivity is meant the mass of olefins formed relative to the mass of all the products formed by conversion of the paraffin.
[0049] Stability means the stability of the activity which is generally measured by a percentage drop in activity compared to an activity between 1 hour and at least 9 hours of testing.
[0050] Surface density means the quantity of element atoms per unit area expressed in square nanometers calculated from the mass content given by an X-ray fluorescence analysis and the BET specific surface area of the catalyst. It is expressed in atoms / nm2.
[0051] Definition of the distribution coefficient R: the distribution profiles of the elements within the catalyst grains are obtained by Castaing microprobe. At least 30 analysis points are carried out along the diameter of the ball or the extrudate. The distribution profile c(x) is thus obtained for x € [-r ; +r] with c the local mass concentration of the element, r the radius of the ball or the extrudate and x the position of the analysis point along the grain diameter relative to the center of that grain.
[0052] The distribution of the elements is characterized by a dimensionless distribution coefficient R weighting the local concentration by an increasing weight depending on the position on the diameter. By definition:
[0053] [Math.l] fi = —| c(x)dx / | c(x)x2dx 3 jF_r Z
[0054] Thus, an element whose concentration is uniform has a distribution coefficient R equal to 1, an element deposited in a dome (concentration at the core greater than the concentration at the edges of the support) has a coefficient greater than 1 and an element distributed in a crust (concentration at the edges greater than the concentration at the core of the support) has a coefficient less than 1. Analysis by Castaing microprobe gives the values of the concentrations in a finite number of values of x, R is thus evaluated numerically by integration methods well known to those skilled in the art. Preferably, R is determined by the trapezoid method. 2. Catalyst
[0055] The catalyst according to the invention comprises, preferably consists of, an active phase based on at least one metal from group VIII, at least one element M1 chosen from tin, germanium, lead, gallium, indium and thallium, at least one element M2 chosen from alkali or alkaline-earth elements and at least one element X chosen from halogens, and a support comprising at least one refractory oxide, characterized in that:
[0056] - the content of element M2, expressed in element, is between 0.4 and 8% by weight relative to the total weight of the catalyst;
[0057] - the surface density of the element M2 is between 0.5 and 1.5 atoms M2 / nm2; And
[0058] - the support is a gamma alumina comprising a specific surface area between 170 and 250 m2 / g.
[0059] Thanks to the combination of these very specific characteristics, namely a content and a surface density of alkali or alkaline-earth element and a gamma alumina support comprising a well-defined specific surface, the catalyst according to the invention has improved performance, both in terms of activity, selectivity and stability, for the dehydrogenation of paraffins and / or naphthenes and more particularly for the dehydrogenation of propane.
[0060] Advantageously, the content of metal from group VIII, expressed as an element, is between 0.02 and 2% by weight relative to the total weight of the catalyst, preferably between 0.05 and 1.5% by weight, even more preferably between 0.1 and 0.8% by weight.
[0061] Advantageously, the metal from group VIII is chosen from platinum (Pt) or palladium (Pd), preferably platinum.
[0062] The group VIII metal may be present in the final catalyst in oxide, sulfide, halide, oxyhalide form, in chemical combination with one or more of the other components of the catalyst or in elemental metal form.
[0063] Advantageously, the content of element Ml, chosen from tin, germanium, lead, gallium, indium and thallium, expressed as an element, in the catalyst according to the invention is between 0.01 and 10% by weight relative to the total weight of the catalyst, more preferably between 0.05 and 5% by weight and very preferably between 0.1 and 1% by weight.
[0064] Preferably, the element Ml is tin (Sn).
[0065] The element Ml can exist in the catalyst in oxide, sulfide, halide, oxyhalide form, in chemical combination with one or more of the other components of the catalyst or even in elemental metal form.
[0066] Advantageously, the content of element M2, chosen from alkali or alkaline-earth elements, expressed as an element, in the catalyst according to the invention is between 0.4 and 8% by weight relative to the total weight of the catalyst, more preferably between 0.45 and 6.0% by weight, and very preferably between 0.5 and 3% by weight.
[0067] Preferably, the element M2 is potassium (K) or cesium (Cs), and more preferably potassium.
[0068] When the element M2 is potassium, the potassium content, expressed as an element, in the catalyst according to the invention is advantageously between 0.5 and 3% by weight relative to the total weight of the catalyst, more preferably between 0.5 and 2.5% by weight, and very preferably between 0.5 and 2.25% by weight, and even more preferably between 0.65 and 0.95% by weight.
[0069] Advantageously, the surface density of element M2 in the catalyst according to the invention is between 0.5 and 1.5 atoms of element M2 / nm2, more preferably between 0.55 and 1.2 atoms of element M2 / nm2 and very preferably between 0.65 and 1 atom of element M2 / nm2.
[0070] The catalyst according to the invention further comprises a halogen element (hereinafter referred to as X). The halogen content is advantageously between 0.75 and 5.5% by weight of halogen element relative to the total weight of the catalyst, more preferably between 0.85 and 4% by weight and very preferably between 1 and 3.5% by weight.
[0071] Preferably, the halogen element is selected from the group consisting of fluorine, chlorine, bromine and iodine. Preferably, the halogen element is chlorine (Cl).
[0072] Advantageously, the surface density of halogen element in the catalyst is between 0.75 and 3.5 atoms of element X / nm2 by weight, preferably between 1 and 2.75 atoms of element X / nm2, more preferably between 0.85 and 2.75 atoms of element X / nm2 and very preferably between 1 and 2.45 atoms of element X / nm2.
[0073] Advantageously, the atomic ratio between the halogen element and the element M2 chosen from alkali or alkaline-earth compounds is between 1.5 and 3, and preferably between 1.5 and 2.5. Preferably, the halogen is chlorine and the alkali or alkaline-earth is potassium.
[0074] In one embodiment according to the invention, the catalyst may further comprise phosphorus. The phosphorus may be present in the final catalyst as an oxide or mixed oxide compound, phosphate, polyphosphate, sulfide, halide, oxyhalide, hydride, in chemical combination with one or more of the other components of the catalyst.
[0075] In this embodiment, the phosphorus content, expressed as an element, in the catalyst is between 0.4 and 1% by weight relative to the total weight of the catalyst, preferably between 0.4 and 0.8% by weight.
[0076] All the elements (the metal of group VIII, element M1, element M2, element X, optionally phosphorus) are preferably distributed uniformly in the support. This distribution is characterized by a Castaing microprobe analysis by determining a distribution coefficient of between 0.8 and 1.1 for all the elements and preferably between 0.9 and 1.0 for all the elements.
[0077] The specific surface area of the catalyst according to the invention is between 170 m2 / g and 250 m2 / g, preferably between 180 m2 / g and 220 m2 / g, preferentially between 185 m2 / g and 220 m2 / g, more preferentially between 185 m2 / g and 210 m2 / g, and even more preferentially between 185 m2 / g and 195 m2 / g.
[0078] The catalyst advantageously has a total pore volume measured by mercury porosimetry of between 0.1 cmVg and 1.5 cmVg, preferably between 0.4 cmVg and 0.8 cmVg, and very preferably between 0.4 cmVg and 0.7 cmVg.
[0079] Advantageously, the catalyst has a packed filling density (DRT) value of between 0.50 and 0.70 g / mL, preferably between 0.60 and 0.65 g / mL. 3. Support
[0080] The catalyst support according to the invention comprises at least one refractory oxide, specifically the support comprises a gamma alumina.
[0081] The specific surface area of the support is between 170 m2 / g and 250 m2 / g, preferably between 180 m2 / g and 220 m2 / g, preferentially between 185 m2 / g and 220 m2 / g, more preferentially between 185 m2 / g and 210 m2 / g, and even more preferentially between 185 m2 / g and 195 m2 / g.
[0082] The support advantageously has a total pore volume measured by mercury porosimetry of between 0.1 cmVg and 1.5 cmVg, preferably between 0.4 cmVg and 0.8 cm3 / g, and very preferably between 0.4 cmVg and 0.7 cmVg.
[0083] Advantageously, the support has a packed filling density (DRT) value of between 0.50 and 0.70 g / mL, preferably between 0.60 and 0.65 g / mL.
[0084] The support is advantageously in the form of beads, extrudates, pellets or powder. Preferably, the support is in the form of beads. When the support is in the form of beads, its diameter is generally between 0.5 mm and 5 mm, preferably between 1 mm and 2 mm. When the support is in the form of extrudates, the diameter of the extrudates is between 0.5 mm and 5 mm, preferably with a length-to-diameter ratio of 1:1 to 5:1.
[0085] The support can be obtained by any technique known to those skilled in the art. The shaping can be carried out for example by extrusion, by pelletizing, by the drop coagulation method (“oil-drop” according to English terminology), by granulation on a rotating plate or by any other method well known to those skilled in the art. 4. Process for preparing the catalyst
[0086] The catalyst according to the invention can be prepared using any technique known to those skilled in the art. Group VIII metal
[0087] Advantageously, the group VIII metal is supplied to the support in any suitable manner, such as coprecipitation, ion exchange or impregnation. Preferably, it is introduced by impregnation of the support, for example by excess or dry impregnation (the volume of solution containing the element to be introduced corresponding to the pore volume of the support), and preferably by excess impregnation. For this, the support is impregnated with an impregnation solution, aqueous or organic or consisting of a mixture of water and at least one organic solvent, comprising at least one precursor of the group VIII metal.
[0088] In general, hydrogen chloride or another similar acid may also be added to the impregnation solution to further facilitate the incorporation or attachment to the surface of the support of the Group VIII metal and promote uniform distribution of the Group VIII metal in the support.
[0089] When the group VIII metal is platinum, the platinum precursors are part of the following group, without this list being exhaustive: hexachloroplatinic acid, bromoplatinic acid, ammonium chloroplatinate, platinum chlorides, such as PtCl2 or PtCl4, platinum dichlorocarbonyl dichloride, platinum tetraamine chloride or even dihydroxyplatinediammine. Organic platinum complexes, such as platinum (II) diacetyl acetonate can also be used. These precursors can be used alone or in a mixture. Preferably, the precursor used is hexachloroplatinic acid. Element Ml
[0090] The element Ml selected from tin, germanium, lead, gallium, indium and thallium can be supplied in any suitable manner, such as coprecipitation, ion exchange or impregnation, at any stage of the catalyst preparation process.
[0091] According to a first variant, the element Ml can be introduced into the support, for example during the synthesis of the support or during the shaping of the support. Without being exhaustive, the techniques of addition before or during the dissolution of the oxide precursors of the support during the synthesis of the support, with or without ripening, may be suitable. The introduction can therefore be simultaneous or successive to the mixing of the precursors of the support. The element Ml can be introduced during the synthesis of the support according to a sol-gel type technique or even be added to an alumina sol. The element Ml can also be introduced during the implementation of the support according to the techniques of the prior art for shaping the support such as the shaping procedures by extrusion or by drop coagulation (oil-drop according to the English terminology).
[0092] According to a second variant, the element Ml can be introduced onto the support, for example by impregnation of the previously shaped support. The impregnation of the support with a solution, aqueous or organic or consisting of a mixture of water and at least one organic solvent, comprising one or more precursors of elements Ml can be carried out by excess solution or dry. The impregnation of the support with a solution containing one or more precursors of element Ml can be carried out before, after or at the same time as the impregnation of the group VIII metal. The impregnation can be carried out in the presence of species acting on the interaction between the precursor of element Ml and the support.These species may be, for example, and without being limiting, mineral acids (HCl, HNO3) or organic acids (carboxylic or polycarboxylic acid types), and organic compounds of the complexing type, as described for example in patents US 6,872,300 and US 6,291,394. Preferably, the impregnation is carried out according to any technique known to those skilled in the art making it possible to obtain a homogeneous distribution of the element Ml within the support.
[0093] According to a third variant, the element M1 can also be introduced partly during the synthesis or shaping of the support and partly by deposition on the shaped support.
[0094] Preferably, the element M1 is introduced into the support, i.e. during the synthesis of the support or during the shaping of the support. In the case of an alumina-based support in the form of beads prepared by the draining technique, the precursor of the element Ml is introduced into the suspension to be drained.
[0095] The precursors of the element Ml may be inorganic or of organometallic type, optionally of water-soluble organometallic type. The precursor of the element Ml may be chosen from the group formed by halogenated compounds, hydroxides, carbonates, carboxylates, sulfates, tartrates and nitrates. These forms of the element Ml may be introduced into the catalyst preparation medium as such or generated in situ (for example by introduction of tin and carboxylic acid). When the element Ml is tin, the tin-based organometallic precursors may be chosen, for example, from the following list: SnR4, where R represents an alkyl group, for example the butyl group, Me3SnCl, Me2SnCl2, Et3SnCl, Et2 SnCl2, EtSnCl3, iPrSnCl2 and the hydroxides Me3SnOH, Me2Sn(OH)2, Et3SnOH, Et2 Sn(OH)2, the oxides (Bu3Sn)2O, the acetate Bu3SnOC(O)Me. Preferably, halogenated species of tin, in particular chlorinated, are used.Even more preferably, the precursor of element Ml is SnCl2 or SnCl4. Element M2
[0096] The element M2 chosen from the alkali or alkaline-earth elements can be supplied in any suitable manner, such as coprecipitation, ion exchange or impregnation and this at any stage of the catalyst preparation process. It can in particular be introduced according to the three variants described in the case of the element ML. Preferably, it is introduced by impregnation, dry or in excess, preferably in excess and particularly preferably it is introduced after having introduced the metal of group VIII as described above.
[0097] The precursor(s) of element M2 chosen from alkali or alkaline-earth elements may be chosen from hydroxides, halides, nitrates, carbonates. When element M2 is potassium, the precursors may be chosen from KOH, KC1, KN03, K2CO3, or K2PtCl6. Element X
[0098] The element X chosen from halogens can be supplied in any suitable manner, such as coprecipitation, ion exchange or impregnation and this at any stage of the catalyst preparation process. It can in particular be introduced according to the three variants described in the case of the element ML
[0099] In a preferred embodiment, the element X is chlorine. The chlorine is introduced by impregnation, and particularly preferably it is introduced by impregnation at the same time as the Group VIII metal or before the impregnation of the Group VIII metal. As a possible counter-anion of the compounds comprising element Ml, group VIII metal and element M2, chlorine can also be introduced simultaneously with these elements, for example by using precursors of the type H2PtCl6, SnCl2 or KC1 or by treatment of the support at one of the preparation steps with hydrochloric acid. Chlorine can also be supplied in the preparation process by an additional oxychlorination step. Phosphorus (optional)
[0100] The phosphorus can be supplied in any suitable manner, such as coprecipitation, ion exchange or by impregnation and this at any stage of the catalyst preparation process. It can in particular be introduced according to the three variants described in the case of the element ML
[0101] According to a variant, the phosphorus is introduced into the support, that is to say during its shaping, for example simultaneously with the ML element
[0102] According to another variant, the phosphorus is introduced by impregnation, and particularly preferably it is introduced by impregnation at the same time as the group VIII metal. In this case, the impregnation solution contains the precursor of the group VIII metal and the precursor of the phosphorus.
[0103] The phosphorus precursors may be acids or salts, and may be chosen from the following compounds: H3PO4, H3PO3, H3PO2, NH4H2PO4, or (NH4)2 HPO4. Order of introduction of precursors
[0104] As described above, the process for preparing the catalyst according to the invention comprises several embodiments which are distinguished in particular by the order of introduction of the metal from group VIII, the element M1, the element M2, the element X and optionally the phosphorus onto the shaped support and / or into the support, i.e. during the synthesis of the support or during the shaping of the support. The process for preparing the catalyst comprises the introduction, simultaneously or successively, in any order, of the metal from group VIII, the element M1, the element M2, and optionally the phosphorus and / or the element X onto the shaped support and / or into the support.
[0105] When the element M1 and / or the element M2 and / or optionally the phosphorus and / or the element X are introduced into the support, i.e. during the synthesis of the support or during the shaping of the support, the preparation process generally comprises a drying step and a calcination step before the deposition of the group VIII metal. The drying is generally carried out at a temperature less than or equal to 250°C, preferably between 50°C and 250°C, more preferably between 70°C and 200°C, in air or under an inert atmosphere. The calcination is preferably carried out at a temperature between 350°C and 750°C and preferably between 400°C and 600°C and even more preferably between 400°C and 550°C. The temperature rise may be regular or include intermediate temperature stages, these stages being reached with fixed or variable temperature rise rates. These temperature rises may therefore be identical or differ in their speed (in degrees per minute or per hour). The gas atmosphere used during calcination contains oxygen. Air may therefore also be used during this calcination step. The calcination gas may optionally contain water.
[0106] When one or more elements from the metal of group VIII, the element M1, the element M2, the element X and / or optionally phosphorus, are introduced onto the shaped support, preferably by dry or excess impregnation, the introduction of said elements can be simultaneous by a single impregnation solution or take place separately by several impregnation solutions containing one or more of the components and this in any order.
[0107] Any impregnation solution described in the present invention may comprise any polar solvent known to those skilled in the art. Said polar solvent used is advantageously chosen from the group formed by methanol, ethanol, water, phenol, cyclohexanol, taken alone or as a mixture. Said polar solvent may also be advantageously chosen from the group formed by propylene carbonate, DMSO (dimethylsulfoxide), N-methylpyrrolidone (NMP) or sulfolane, taken alone or as a mixture. Preferably, a polar protic solvent is used. A list of common polar solvents and their dielectric constant can be found in the book "Solvents and Solvent Effects in Organic Chemistry", C. Reichardt, Wiley-VCH, 3rd edition, 2003, pages 472-474. Very preferably, the solvent used is water or ethanol, and particularly preferably, the solvent is water.
[0108] After each impregnation step, the catalyst precursor obtained is preferably dried in order to remove all or part of the solvent introduced during the impregnation, preferably at a temperature below 250°C, more preferably between 50°C and 250°C, and more preferably between 70°C and 200°C. The drying is advantageously carried out for a period of between 1 and 24 hours, preferably between 1 and 20 hours. The drying is carried out in air, or under an inert atmosphere (nitrogen for example). After the drying step, the catalyst is preferably calcined, generally in air. The calcination temperature is generally between 350°C and 650°C and preferably between 400°C and 650°C, and even more preferably between 450°C and 550°C. The temperature ramp may optionally contain temperature steps. The calcination time is generally between 0.5 hours and 16 hours, preferably between 1 hour and 5 hours.The gas atmosphere used during calcination contains oxygen. Air can . therefore also be used during this calcination step. The calcination gas may possibly contain water.
[0109] In a particular embodiment, the catalyst according to the invention is prepared according to a preparation process comprising the following successive steps:
[0110] a) a support is prepared comprising the element Ml chosen from tin, germanium, lead, gallium, indium and thallium to obtain a first catalyst precursor;
[0111] b) the first catalyst precursor obtained in step a) is dried under a flow of a neutral gas or under a flow of a gas containing oxygen at a temperature less than or equal to 250°C, then calcined at a temperature between 350°C and 750°C to obtain a first dried and calcined catalyst precursor;
[0112] c) the first dried and calcined catalyst precursor obtained in step b) is impregnated with an impregnation solution comprising at least one precursor of at least one metal from group VIII, and optionally at least one precursor of an element X, and optionally phosphorus to obtain a second catalyst precursor;
[0113] d) the second catalyst precursor obtained in step c) is dried under a flow of a neutral gas or under a flow of a gas containing oxygen at a temperature less than or equal to 250°C, then calcined at a temperature between 350°C and 650°C to obtain a second dried and calcined catalyst precursor;
[0114] e) the second dried and calcined catalyst precursor obtained in step d) is impregnated with an impregnation solution comprising a precursor of at least one element M2, and optionally at least one precursor of an element X, to obtain a third catalyst precursor;
[0115] f) the third catalyst precursor obtained in step e) is dried under a flow of a neutral gas or under a flow of a gas containing oxygen at a temperature less than or equal to 250°C, then calcined at a temperature between 350°C and 650°C;
[0116] g) optionally, an oxychlorination step is carried out at a temperature between 350°C and 550°C and under a pressure between 0.1 MPa and 1.5 MPa, then calcination is carried out at a temperature between 350°C and 650°C;
[0117] it being understood that the element X is supplied at least once in step c) and / or in step e), or possibly in step g).
[0118] In one embodiment according to the invention, when element X is chlorine, said chlorine element is supplied at least once either in step c) and / or in step e), and / or in step g).
[0119] Preferably, the introduction of the element M2 chosen from the alkali or alkaline-earth elements, and more particularly potassium, is carried out on a catalyst precursor comprising the metal of group VIII, more particularly platinum, previously dried and calcined. Indeed, the fact of introducing the potassium after the platinum prevents a leaching effect of platinum during impregnation of the group VIII metal.
[0120] In step a), a support is prepared comprising the element Ml, preferably tin. The element Ml, preferably tin, can be introduced at any time during the preparation of the support, and preferably during shaping, or by impregnation on an already formed support. Preferably, the element Ml is introduced during the shaping of the support.
[0121] Similarly, the phosphorus can be introduced at any time during the preparation of the support, and preferably during shaping, or by impregnation on an already formed support. According to one variant, the phosphorus is introduced into the support, i.e. during the shaping of the support, preferably with the element M1, preferably tin. According to another variant, the phosphorus is introduced by impregnation, and particularly preferably it is introduced by impregnation at the same time as the group VIII metal.
[0122] The introduction of the group VIII metal can advantageously be carried out by one or more excess impregnations of solution on the support, or by one or more dry impregnations, and, preferably, by a single excess impregnation of said support (preferably containing the element Ml, preferably tin, and optionally phosphorus), using solution(s), preferably aqueous, containing the precursor of the group VIII metal and preferably the phosphorus precursor (when the support does not contain or partially contains phosphorus).
[0123] In step e) the second dried and calcined catalyst precursor obtained in step d) is impregnated with an impregnation solution comprising at least one precursor of an element M2 chosen from alkali or alkaline-earth elements. The introduction of the alkali or alkaline-earth element(s) may advantageously be carried out by one or more excess solution impregnations on the support, or by one or more dry impregnations, and, preferably, by a single dry or excess impregnation of said precursor, using solution(s), preferably aqueous, containing at least one precursor of the alkali or alkaline-earth element, and preferably at least one potassium precursor.
[0124] In optional step g), the chlorine is supplied by means of an oxychlorination treatment. Such a treatment may for example be carried out at a temperature between 350°C and 550°C and under a pressure between 0.1 MPa and 1.5 MPa, for a duration preferably between 30 minutes and 10 hours, and under a flow of air containing the desired quantity of chlorine and possibly containing water.
[0125] According to another variant, the catalyst according to the invention can be prepared by preparing a support comprising tin by introducing the tin precursor during shaping the support, followed by one or more excess solution impregnations on the support, or by one or more dry impregnations, using solution(s), preferably aqueous, containing a precursor of a metal from group VIII, a precursor of phosphorus and a precursor of an alkali or alkaline-earth element and preferably a precursor of potassium, alone or in a mixture, then drying and calcining under the conditions described above.
[0126] When the various precursors used in the preparation of the catalyst according to the invention do not contain halogen or contain halogen in insufficient quantity, it may be necessary to add a halogenated compound during the preparation. Any compound known to those skilled in the art may be used and incorporated into any of the steps of preparation of the catalyst according to the invention. In particular, it is possible to use organic compounds such as methyl or ethyl halides, for example dichloromethane, dichloroethane, dichloropropane, chloroform, methylchloroform or carbon tetrachloride.
[0127] The halogen can also be added by means of impregnation with an aqueous solution of the corresponding acid, for example hydrochloric acid, at any time during the preparation. A typical protocol consists of impregnating the solid so as to introduce the desired quantity of halogen. The catalyst is kept in contact with the aqueous solution for a time long enough to deposit this quantity of halogen. Additional reduction step (optional)
[0128] In one embodiment according to the invention, prior to the use of the catalyst in the catalytic reactor and the implementation of a dehydrogenation process, a reducing treatment step is carried out in the presence of a reducing gas so as to obtain a catalyst comprising said metal from group VIII and said element M1 at least partially in metallic form. This step is advantageously carried out in situ, that is to say after the loading of the catalyst into a dehydrogenation reactor. Carrying out the reducing treatment of the catalyst in situ makes it possible to dispense with an additional step of passivation of the catalyst by an oxygenated compound or by CO2, which is necessarily the case when the catalyst is prepared by carrying out a reducing treatment ex situ, that is to say outside the reactor used for the dehydrogenation.Indeed, when the reducing treatment is carried out ex-situ, it is necessary to carry out a passivation step in order to preserve the metallic phase of the catalyst in the presence of air (during the operations of transporting and loading the catalyst into the hydrogenation reactor), then to carry out a new step of reducing the catalyst.
[0129] The reducing gas is preferably hydrogen. Hydrogen can be used pure or as a mixture (for example a hydrogen / nitrogen, hydrogen / argon, hydrogen / methane). In the case where hydrogen is used in a mixture, all proportions are possible.
[0130] Preferably, said reducing treatment is carried out at a temperature between 100°C and 600°C, and preferably between 200°C and 580°C, under a stream of hydrogen, pure or diluted, up to the maximum reduction temperature, followed by maintenance for example for 30 minutes to 6 hours at this temperature. The rise in temperature up to the desired reduction temperature is generally slow, for example set between 0.1 and 10°C / min, preferably between 0.3 and 7°C / min.
[0131] The hydrogen flow rate, expressed in L / hour / gram of catalyst precursor, is between 0.01 and 100 L / hour / gram of catalyst, preferably between 0.05 and 10 L / hour / gram of catalyst precursor, even more preferably between 0.1 and 5 L / hour / gram of catalyst precursor. Passivation step (optional)
[0132] The process according to the invention may advantageously comprise a step of passivation by a sulfur compound which makes it possible to improve the selectivity of the catalysts and to avoid thermal runaways during the start-up of new catalysts ("run-away" according to English terminology). The passivation step is carried out by implementing methods known to those skilled in the art.
[0133] The step of passivation by a sulfur compound is generally carried out at a temperature between 20 and 350°C, preferably between 40 and 200°C, for 10 minutes to 240 minutes. The sulfur compound is for example chosen from the following compounds: thiophene, thiophane, alkylmonosulfides such as dimethylsulfide, diethylsulfide, dipropylsulfide and propylmethylsulfide or an organic disulfide of formula HO-Ri-SS-R2-OH such as dithiodiethanol of formula HO-C2H4-SSC 2H4-OH (often called DEODS). The sulfur content is generally between 0.1 and 2% by weight of said element relative to the total weight of the catalyst.
[0134] 5. Process for the dehydrogenation of paraffins and / or naphthenes
[0135] The invention also relates to a process for dehydrogenation of a hydrocarbon feedstock comprising paraffinic and / or naphthenic compounds in the presence of the catalyst according to the invention.
[0136] The processes for dehydrogenating paraffins and / or naphthenes make it possible to selectively produce olefins and contribute to the production of significant quantities of hydrogen essential for the hydrogenation and hydrotreatment processes of a petrochemical complex or a refinery.
[0137] The hydrocarbon feedstock generally comprises paraffinic and / or naphthenic compounds containing from 2 to 30 carbon atoms per molecule, taken alone or in a mixture. More particularly, the hydrocarbon feedstock comprises paraffinic and / or naphthenic compounds containing from 2 to 15 carbon atoms per molecule, preferably paraffinic compounds having 2 to 5 carbon atoms per molecule, such as propane, n-butane, n-pentane, isomers of butane and pentane or their mixture, and / or preferably naphthenic compounds having 5 to 12 carbon atoms such as cyclohexane, methylcyclohexane, decalin or their mixture. The feedstock may also comprise unsaturated hydrocarbons having 2 to 15 carbon atoms per molecule.
[0138] Typically, the dehydrogenation catalyst is loaded into a unit and previously subjected to a reduction treatment as described above. It can be implemented in any manner known to those skilled in the art. It can, for example, be implemented in a fixed bed or in a moving bed, preferably in a moving bed. According to a variant of the invention, the dehydrogenation catalyst is implemented in several reactors installed in series.
[0139] The various processes for dehydrogenation of paraffins and naphthenes are differentiated by the choice of operating conditions and the composition of the feedstock. The adjustment of the operating conditions, depending on the nature of the feedstock to be treated, is done in such a way as to obtain the best pressure-temperature-yield and activity match in a manner known to those skilled in the art.
[0140] Generally, the process for dehydrogenating a hydrocarbon feedstock comprising paraffins and / or naphthenes is carried out at a pressure of between 0.1 MPa and 4 MPa, at a temperature of between 200°C and 800°C and with a liquid volumetric space velocity of between 0.5 h 1 and 50 h 1.
[0141] More particularly, the paraffin dehydrogenation reaction is carried out at a pressure of between 0.1 MPa and 4 MPa and more preferably between 0.25 MPa and 3.0 MPa and at a temperature of between 400 and 800°C depending on the nature of the feedstock, the temperature being advantageously between 560 and 700°C for a feedstock comprising mainly propane, between 450 and 600°C for a feedstock comprising mainly isobutane, and between 400 and 550°C for a feedstock comprising mainly isopentane. It may be advantageous to use hydrogen as a diluent. The hydrogen / hydrocarbon molar ratio of the feedstock is generally between 0.1 and 10, preferably between 0.5 and 8.The liquid volumetric space velocity of the hydrocarbon feedstock (LHSV or Liquid Hourly Space Velocity according to English terminology), the unit of which is in liters of hydrocarbon feedstock per liter of catalyst and per hour, is preferably between 0.5 and 50 h1, more preferably between 1.5 and 15 h1.
[0142] More particularly, the naphthenes dehydrogenation reaction is carried out at a pressure of between 0.1 and 2 MPa, preferably between 0.1 and 1 MPa, and at a temperature of between 200 and 400°C. The mass flow rate of treated feedstock per unit mass of catalyst is generally between 0.5 and 50 h1.
[0143] The catalyst according to the invention can be regenerated by at least one combustion step in an oxidizing medium.
[0144] The regeneration of the catalyst is carried out in a cyclic or continuous system. It can consist of a simple combustion of the coke deposits. This combustion operation is usually carried out by injecting air into an inert mixture. The oxygen content in the gas at the regeneration inlet is preferably between 0.1 and 2% by volume. The combustion is usually carried out at a temperature between 350 and 550°C and under pressure between 0.1 and 1.5 MPa.
[0145] Combustion may optionally be preceded by an operation of stripping the sulfur contained in the catalyst in the case where the catalyst comprises sulfur introduced by injection of DMDS for example.
[0146] The regeneration may also include, at the end of the coke combustion step, a catalyst oxyhalogenation step, preferably an oxychlorination. For this, the oxygen content in the gas at the regeneration inlet is increased by at least 10% compared to the value of the previous combustion step. At least one halogenated derivative, i.e. at least one halogen and / or one halogenated compound, is introduced simultaneously. Chlorine and / or a chlorinated compound are preferably used. The proportion of halogen and / or halogenated compound used is such that 0.2 to 3.5% by weight of a halogenated alumina derivative can be formed relative to the catalyst subjected to regeneration. The oxyhalogenation is carried out at a temperature of between 350 and 550°C and under a pressure of between 0.1 MPa and 1.5 MPa.A catalyst calcination step is generally carried out after oxyhalogenation during which the oxygen content in the gas at the regeneration inlet is between 3 and 20% by volume, the average temperature is between 350 and 550°C and the pressure is between 0.1 MPa and 1.5 MPa.
[0147] Before subjecting the regenerated catalyst to the reaction conditions, it undergoes a preliminary reduction under a gas containing hydrogen, preferably under pure hydrogen. This reduction can be carried out in the regeneration chamber if this is separate from the reaction chamber, in the reaction chamber itself or in an intermediate zone separate from the regeneration and reaction zones. This reduction, if it has not been carried out prior to the reaction, can also occur in the reaction chamber after the reaction has started: the first stages of the reaction then serve to transform the catalyst into a catalytically active form for dehydrogenation. The reduction is carried out under a stream of gas containing hydrogen, preferably under pure hydrogen, at a temperature between 330 and 600°C and at a pressure between 0.2 and 2.5 MPa, preferably between 0.4 and 1.5 MPa.
[0148] Possible sulfurization of the catalyst can follow this reduction step and therefore precede the dehydrogenation reaction itself.
[0149] All or part of the hydrogen produced can be recycled to the inlet of the dehydrogenation reactor. All or part of the unconverted propane can be recycled to the inlet of the dehydrogenation reactor. Examples
[0150] The following examples illustrate the invention without limiting its scope.
[0151] Support 1: In examples 1, 2, 5, 6 and 7, a gamma alumina is used having the following properties: SBet = 190 m2 / g, Total pore volume = 0.65 cm3 / g, support density (DRT) = 0.63 g / cm3, tin content 0.30% by weight.
[0152] Support 2: In examples 3 and 4, a predominantly theta alumina is used with the following properties: SBet = 80 m2 / g, Total pore volume = 0.59 cm3 / g, support density (DRT) = 0.62 g / cm3, tin content 0.30% by weight.
[0153] Example 1: Catalyst A PtSnK / Al2O3-Cl (comparative)
[0154] A catalyst A is prepared on support 1, aiming for a deposition of 0.3% by weight of platinum element, 1.2% by weight of chlorine element, 0.18% by weight of potassium element relative to the total weight of the catalyst (non-compliant), and a surface density of potassium of 0.15 atoms K / nm2 (non-compliant).
[0155] To 100 g of support 1, 400 cm3 of an aqueous solution of hexachloroplatinic acid at 37.75 g / L and hydrochloric acid at 6.95 g / L are added by excess impregnation. The mixture is left in contact for 4 hours and then drained. It is dried at 120°C in a ventilated oven for 15 hours and then calcined in a crossed bed at 500°C under an air flow rate of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.
[0156] To 100 g of this calcined solid, 75 cm3 of a potassium carbonate solution at a concentration of 4.7 g / L is added by dry impregnation. It is left to mature, dried at 120°C in a ventilated oven for 15 hours and then calcined in a crossed bed at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.
[0157] Catalyst A obtained after calcination contains 0.30% by weight of platinum element, 0.29% by weight of tin element, 1.2% by weight of chlorine element and 0.18% by weight of potassium element relative to the total weight of the catalyst (non-compliant), i.e. a surface density of 0.14 atoms K / nm2 (non-compliant).
[0158] Example 2: Catalyst B PtSnK / Al2O3-Cl (comparative)
[0159] A catalyst B is prepared on the support prepared in example 1, aiming for a deposition of 0.3% by weight of platinum element, 1.2% by weight of chlorine element, 3.1% by weight of potassium element relative to the total weight of the catalyst, i.e. a surface density of 2.50 atoms K / nm2 (non-compliant).
[0160] To 100 g of support 1, 400 cm3 of an aqueous solution of hexachloroplatinic acid at 37.75 g / L and hydrochloric acid at 6.95 g / L are added by excess impregnation. The mixture is left in contact for 4 hours and then drained. It is dried at 120°C for 15 h and then calcined at 500°C under an air flow rate of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.
[0161] To 100 g of this calcined solid, 75 cm3 of a potassium carbonate solution at a concentration of 78.3 g / L is added by dry impregnation. It is left to mature, dried at 120°C in a ventilated oven for 15 hours and then calcined in a crossed bed at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.
[0162] Catalyst B obtained after calcination contains 0.30% by weight of platinum element, 0.29% by weight of tin element, 1.2% by weight of chlorine element and 3.1% by weight of potassium element relative to the total weight of the catalyst, i.e. a surface density of 2.51 atoms K / nm2 (non-compliant).
[0163] Example 3: Catalyst C PtSnKCl / Al2O3 (comparative)
[0164] A catalyst C is prepared on support 2 (non-compliant), aiming for a deposit of 0.3% by weight of platinum element, 0.8% by weight of chlorine element, 0.28% by weight of potassium element (non-compliant) and 0.54 atoms K / nm2.
[0165] To 100 g of support 2, 400 cm3 of an aqueous solution of hexachloroplatinic acid at 37.75 g / L and hydrochloric acid at 6.95 g / L are added by excess impregnation. The mixture is left in contact for 4 hours and then drained. It is dried at 120°C in a ventilated oven for 15 hours and then calcined in a crossed bed at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.
[0166] To 100 g of this calcined solid, 70 cm3 of a potassium carbonate solution at a concentration of 6.8 g / L is added by dry impregnation. It is left to mature, dried at 120°C in a ventilated oven for 15 hours and then calcined in a crossed bed at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.
[0167] Catalyst C obtained after calcination contains 0.30% by weight of platinum element, 0.29% by weight of tin element, 0.8% by weight of chlorine element and 0.27% by weight of potassium element relative to the total weight of the catalyst (non-compliant), i.e. a surface density of 0.52 atoms K / nm2.
[0168] Example 4: Catalyst D PtSnKCl / Al2O3 (comparative)
[0169] A catalyst D is prepared on support 2 (non-compliant), aiming for a deposition of 0.3% by weight of platinum element, 0.8% by weight of chlorine element, 1% by weight of potassium element and 1.93 K atoms / nm2 (non-compliant).
[0170] To 100 g of support 2, 400 cm3 of an aqueous solution of hexachloro- acid are added. platinum at 37.75 g / L and hydrochloric acid at 6.95 g / L by excess impregnation. Leave in contact for 4 hours then spin. Dry at 120°C in a ventilated oven for 15 hours then calcine in a crossed bed at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.
[0171] To 100 g of this calcined solid, 75 cm3 of a potassium carbonate solution at a concentration of 25.2 g / L is added by dry impregnation. It is left to mature, dried at 120°C in a ventilated oven for 15 hours and then calcined in a crossed bed at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.
[0172] Catalyst D obtained after calcination contains 0.30% by weight of platinum element, 0.29% by weight of tin element, 0.8% by weight of chlorine element and 1% by weight of potassium element relative to the total weight of the catalyst, i.e. a surface density of 1.93 atoms K / nm2 (non-compliant).
[0173] Example 5: Catalyst E PtSnKCl / Al2O3 (according to the invention)
[0174] A catalyst E is prepared on the support 1, aiming for a deposition of 0.3% by weight of platinum element, 1.2% by weight of chlorine element, 0.68% by weight of potassium element relative to the total weight of the catalyst and 0.55 atoms K / nm2.
[0175] To 100 g of support 1, 400 cm3 of an aqueous solution of hexachloroplatinic acid at 37.75 g / L and hydrochloric acid at 6.95 g / L are added by excess impregnation. The mixture is left in contact for 4 hours and then drained. It is dried at 120°C in a ventilated oven for 15 hours and then calcined in a crossed bed at 500°C under an air flow rate of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.
[0176] To 100 g of this calcined solid, 75 cm3 of a potassium carbonate solution at a concentration of 17.2 g / L is added by dry impregnation. It is left to mature, dried at 120°C in a ventilated oven for 15 hours and then calcined in a crossed bed at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.
[0177] Catalyst E obtained after calcination contains 0.30% by weight of platinum element, 0.29% by weight of tin element, 1.2% by weight of chlorine element and 0.7% by weight of potassium element relative to the total weight of the catalyst, i.e. a surface density of 0.57 atoms K / nm2.
[0178] Example 6: Catalyst F PtSnKCl / Al2O3 (according to the invention)
[0179] A catalyst F is prepared on support 1, aiming for a deposition of 0.3% by weight of platinum element, 1.2% by weight of chlorine element, 0.92% by weight of potassium element and 0.75 atoms K / nm2.
[0180] To 100 g of support 1, 400 cm3 of an aqueous solution of hexachloro- platinum at 37.75 g / L and hydrochloric acid at 6.95 g / L by excess impregnation. Leave in contact for 4 hours then spin. Dry at 120°C in a ventilated oven for 15 hours then calcine in a crossed bed at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.
[0181] To 100 g of this calcined solid, 75 cm3 of a potassium carbonate solution at a concentration of 21.9 g / L is added by dry impregnation. It is left to mature, dried at 120°C in a ventilated oven for 15 hours and then calcined in a crossed bed at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.
[0182] The catalyst F obtained after calcination contains 0.30% by weight of platinum element, 0.29% by weight of tin element, 1.2% by weight of chlorine element and 0.95% by weight of potassium element relative to the total weight of the catalyst, i.e. a surface density of 0.77 atoms K / nm2.
[0183] Example 7: Catalyst G PtSnKCl / Al2O3 (according to the invention)
[0184] A catalyst G is prepared on the support 1, aiming for a deposition of 0.3% by weight of platinum element, 1.2% by weight of chlorine element, 1.23% by weight of potassium element relative to the total weight of the catalyst and 1.00 atoms K / nm2.
[0185] To 100 g of support 1, 400 cm3 of an aqueous solution of hexachloroplatinic acid at 37.75 g / L and hydrochloric acid at 6.95 g / L are added by excess impregnation. The mixture is left in contact for 4 hours and then drained. It is dried at 120°C in a ventilated oven for 15 hours and then calcined in a crossed bed at 500°C under an air flow rate of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.
[0186] To 100 g of this calcined solid, 75 cm3 of a potassium carbonate solution at a concentration of 26.3 g / L is added by dry impregnation. It is left to mature, dried at 120°C in a ventilated oven for 15 hours and then calcined in a crossed bed at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.
[0187] Catalyst G obtained after calcination contains 0.30% by weight of platinum element, 0.29% by weight of tin element, 1.2% by weight of chlorine element and 1.3% by weight of potassium element relative to the total weight of the catalyst, i.e. a surface density of 1.05 K atoms / nm2.
[0188] Example 8: Process for the dehydrogenation of propane using catalysts A to G
[0189] 10 cm3 of catalyst are introduced into a reactor provided with a shell electric heater. The gas flows are sent in a downward current ("downflow" according to Anglo-Saxon terminology), that is to say from top to bottom compared to the catalytic bed.
[0190] The reduction step is carried out with the following protocol: the catalyst is heated under inert gas to 150°C with a ramp of 5°C / min then maintained at 150°C for 1h30. The inert gas is replaced by hydrogen and the temperature is raised to 635°C with a ramp of 5°C / min then maintained at 635°C for 9h30. The reduction step is then completed and the hydrogen flow rate is set at 28 L / h.
[0191] The propane flow rate is in turn set to 28 L / h, i.e. a LHSV of 10.8 h1. The setting of this flow rate corresponds to the initial reaction time. The gaseous effluent is analyzed by gas chromatography by calculating the volume and mass proportions of each compound. The major products formed participating in the calculation of the selectivity are methane, ethane, ethylene, propylene and benzene.
[0192] The conversion is calculated by making the ratio of the mass quantity of products formed analyzed in the effluent to the mass quantity of propane injected.
[0193] The activity is calculated by determining the mass quantity of propane converted per gram of platinum per hour.
[0194] Propylene selectivity is calculated by dividing the mass quantity of propylene formed by the sum of the mass quantities of all the reaction products at a propane conversion level of 28%.
[0195] The benzene selectivity is calculated by taking the ratio of the mass quantity of benzene formed to the sum of the mass quantities of all the reaction products at a propane conversion level of 28%. The benzene selectivity is particularly informative as to the propensity of the catalyst to produce coke and to deactivate: the higher this selectivity, the more easily the catalyst will coke.
[0196] Stability is determined by comparing the initial activity of the catalyst with the activity at 9 hours of TOS (Time on Stream): % loss of activity = ((activity at 1 hour of TOS) - (activity at 9 hours of TOS)) / (activity at 1 hour of TOS).
[0197] Table 1 below reports the activities after 1 hour and 9 hours of “Time On Stream”, the percentage of loss of activity between 1 hour and 9 hours of TOS and the maximum selectivities obtained in propylene and benzene.
[0198] [Tableauxl] Catalyst Sbet (m2 / g ) K content (% wt) Surface density eK (K atoms / nm2) Activity at 1 hour of TOS gC3 / gPt / h Activity at 9 hours of TOS gC3 / gPt / h % loss of activity Selectivity Propylene % wt Selectivity Benzene % wt A (comparati 0 190 0.18 0.14 920 650 29.3 91.2 0.7 B (comparati 0 190 3.10 2.51 250 240 4.0 86.4 0.0 C (comparati 0 80 0.27 0.52 660 510 22.7 92.8 0.6 D (comparati 0 80 1.00 1.93 320 305 4.7 88.5 0.0 E (compliant) 190 0.70 0.57 900 780 13.3 96.0 0.4 F (compliant) 190 0.95 0.77 900 780 13.3 96.5 0.3 G (compliant) 190 1.30 1.05 850 750 11.7 96.7 0.2
[0199] The performance of non-compliant catalyst A having a potassium content of less than 0.40% by weight and a potassium surface density of less than 0.5 atoms K / nm2 clearly shows a deficit in propylene selectivity and a high value of benzene selectivity compared to the catalysts according to the invention. The deactivation of this catalyst is also increased compared to the catalysts according to the invention.
[0200] The performance of non-compliant catalyst B having a surface density of potassium greater than 1.5 K atoms / nm2 clearly show a deficit in catalyst activity and a lower selectivity in propylene compared to the catalysts according to the invention.
[0201] The performance of non-compliant catalyst C having a specific surface area of less than 170 m2 / g and a potassium content of less than 0.40% by weight clearly shows a deficit in activity and propylene selectivity compared to the catalysts according to the invention. The deactivation of this catalyst is also increased compared to the catalysts according to the invention.
[0202] The performance of non-compliant catalyst D having a specific surface area of less than 170 m2 / g and a potassium surface density of greater than 1.5 K atoms / nm2 clearly shows a deficit in activity and propylene selectivity compared to the catalysts according to the invention.
[0203] The performances of catalysts E, F and G according to the invention present the best results both in terms of activity and propylene selectivity. At comparable activity at 1 hour of TOS as is the case for catalyst A, catalysts E, F and G present increased stability with a loss of activity more than 2 times lower as well as a benzene selectivity 1.5 to more than 3 times lower.
[0204] The performances of catalysts E, F and G according to the invention comprising a specific surface area of between 170 and 250 m2 / g, a potassium content of between 0.4 and 8% by weight of potassium element relative to the total weight of the catalyst, and a surface density of potassium of between 0.5 and 1.5 atoms K / nm2 are the best in terms of activity and propylene selectivity while keeping the benzene selectivity and the deactivation speed at low levels.
Claims
Claims
1. Catalyst comprising an active phase based on at least one metal from group VIII, at least one element M1 chosen from tin, germanium, lead, gallium, indium and thallium, at least one element M2 chosen from alkali or alkaline-earth elements and at least one element X chosen from halogens, and a support comprising at least one refractory oxide, characterized in that: - the content of element M2, expressed as an element, is between 0.4 and 8% by weight relative to the total weight of the catalyst; - the surface density of element M2 is between 0.5 and 1.5 atoms M2 / nm2; and - the support is a gamma alumina comprising a specific surface area between 170 and 250 m2 / g.
2. Catalyst according to claim 1, characterized in that the surface density of the alkali or alkaline-earth element is between 0.55 and 1.2 atoms of element M2 / nm2.
3. Catalyst according to one of claims 1 or 2, characterized in that the content of group VIII metal is between 0.02 and 2% by elemental weight of group VIII metal relative to the total weight of the catalyst.
4. Catalyst according to any one of the preceding claims, characterized in that the content of element Ml is between 0.01 and 10% by elemental weight of element Ml relative to the total weight of the catalyst.
5. Catalyst according to any one of the preceding claims, characterized in that the group VIII metal is platinum.
6. Catalyst according to any one of the preceding claims, characterized in that the element Ml is tin.
7. Catalyst according to any one of the preceding claims, characterized in that the element M2 chosen from the alkali or alkaline-earth elements is potassium.
8. Catalyst according to claim 7, characterized in that the potassium content, expressed as an element, is between 0.5 and 3% by weight relative to the total weight of the catalyst.
9. Catalyst according to any one of the preceding claims, characterized in that said support comprises a specific surface area of between 185 and 220 m2 / g.
10.
11.
12.
13.
14. Catalyst according to any one of the preceding claims, characterized in that said support has a packed filling density value of between 0.50 and 0.70 g / mL. Catalyst according to any one of the preceding claims, characterized in that the surface density of the element X chosen from halogens is between 1 and 2.75 atoms X / nm2. Catalyst according to any one of the preceding claims, characterized in that the atomic ratio X / M2 is between 1.5 and 2.
5. Catalyst according to any one of the preceding claims, characterized in that the element X is chlorine. A process for preparing a catalyst according to any one of claims 1 to 13 comprising the following steps: a) a support comprising the element Ml chosen from tin, germanium, lead, gallium, indium and thallium is prepared to obtain a first catalyst precursor; b) the first catalyst precursor obtained in step a) is dried under a flow of a neutral gas or under a flow of a gas containing oxygen at a temperature less than or equal to 250°C, then calcined at a temperature between 350°C and 750°C to obtain a first dried and calcined catalyst precursor; c) the first dried and calcined catalyst precursor obtained in step b) is impregnated with an impregnation solution comprising at least one precursor of at least one metal from group VIII, and optionally at least one precursor of an element X, X being chosen from halogens, and optionally phosphorus, to obtain a second catalyst precursor; d) the second catalyst precursor obtained in step c) is dried under a flow of a neutral gas or under a flow of a gas containing oxygen at a temperature less than or equal to 250°C, then calcined at a temperature between 350°C and 650°C to obtain a second dried and calcined catalyst precursor; e) impregnating the second dried and calcined catalyst precursor obtained in step d) with an impregnation solution comprising a precursor of at least one element M2, and optionally at least one precursor of an element X, to obtain a third catalyst precursor; f) the third catalyst precursor obtained in step e) is dried under a flow of a neutral gas or under a flow of a gas containing oxygen at a temperature less than or equal to 250°C, then calcined at a temperature between 350°C and 650°C, it being understood that the precursor of element X is supplied at least once in step c) and / or in step e).
15. Process for the dehydrogenation of a hydrocarbon feedstock comprising paraffins and / or naphthenes in which said feedstock is brought into contact with a catalyst according to any one of claims 1 to 13, or prepared according to claim 14, at a pressure of between 0.1 MPa and 4 MPa, at a temperature of between 200°C and 800°C, and with a liquid volumetric space velocity of between 0.5 h 1 and 50 h 1.
Citation Information
Patent Citations
Dehydrogenation catalyst composition
US20030191351A1
Dehydrogenation catalyst composition
US20210053034A1
Dehydrogenation catalyst composition
US4914075A
Process for improving catalysts
US6291394B1
Reforming catalyst with chelated promotor
US6872300B1