PtSnKCl-based dehydrogenation catalyst for paraffins and / or naphthenes on a gamma alumina support

A catalyst with optimized surface area, halogen density, and atomic ratio on gamma alumina support addresses the limitations of existing catalysts, achieving higher propylene yield and stability by minimizing coke formation and secondary reactions.

FR3147957A1Pending Publication Date: 2024-10-25IFP ENERGIES NOUVELLES
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
FR2023003932
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing dehydrogenation catalysts for paraffins and naphthenes suffer from limited activity, selectivity, and stability, particularly in the conversion of propane to propylene, due to unfavorable thermodynamic conditions and secondary reactions such as coke formation, which lead to catalyst deactivation.

Method used

A catalyst comprising a specific surface area of 175-250 m2/g, surface density of halogen between 0.75-3.5 atoms/nm2, and atomic ratio of halogen to alkaline earth element between 1.5-3, with platinum, tin, and potassium on a gamma alumina support, optimized through a controlled preparation process.

Benefits of technology

The catalyst exhibits enhanced activity, selectivity, and stability for propane dehydrogenation to propylene, with improved resistance to coke formation and reduced secondary reactions, resulting in higher propylene yield and lower benzene formation.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a catalyst comprising an active phase based on at least one metal from group VIII, at least one element M1 selected from tin, germanium, lead, gallium, indium and thallium, at least one element M2 selected from the alkali or alkaline earth elements, and at least one element X selected from the halogens, and a support comprising at least one refractory oxide, characterized in that: - the surface density of element X is between 0.75 and 3.5 atoms X / nm²; - the atomic ratio X / M2 is between 1.5 and 3; - said support comprises a specific surface area between 175 and 250 m² / g.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Paraffin and / or naphthenes dehydrogenation catalyst based on PtSnKCl on a gamma alumina support Field of the invention

[0001] The present invention relates to the field of the conversion of hydrocarbon compounds, more specifically to the dehydrogenation of a hydrocarbon feedstock comprising paraffinic compounds and / or naphthenic compounds, and more particularly to the dehydrogenation of propane in the presence of a catalyst to produce olefins and more particularly propylene. State of the art

[0002] Paraffin and / or naphthenes dehydrogenation processes are interesting routes for the dedicated production of unsaturated compounds and particularly olefins, the demand for which in global production is increasing. Indeed, among the possible routes for the production of olefins, such as thermal or catalytic cracking, metathesis as well as alcohol dehydration, paraffin and / or naphthenes dehydrogenation processes have higher yields and are very selective. The production of propylene in particular is of particular appeal in a context of increased demand for polypropylene and propylene derivatives such as acrylic acid or acrylonitrile. The need for optimization of catalysts and processes is therefore always present.

[0003] The dehydrogenation reactions of paraffins and / or naphthenes are highly endothermic and reversible. Conversion rates are limited by the conditions of thermodynamic equilibrium. In the case of propane dehydrogenation (AH = - 125 kJ / mol), a high temperature above 600°C is conventionally used and the equilibrium conversion under these conditions is of the order of 30% in industrial conditions. Since the separation of olefin from paraffin is a costly step in terms of investment and energy, it is essential to work towards maximum conversion of the feedstock to maximize the productivity of the process.

[0004] The severe conditions allowing this are thus very favorable to the secondary reactions of deep dehydrogenation, oligomerization of olefins, hydrogenolysis, cracking and coke formation. These secondary products and this coke formation are at the origin of the deactivation of the dehydrogenation catalysts and involve the regeneration of the catalyst, and in particular of the metallic phase, by at least one combustion step. The challenge is therefore to succeed in developing an active but also selective and stable catalyst for an economical process. unsustainably viable.

[0005] Among the catalysts suitable for the dehydrogenation of paraffins and more particularly for the dehydrogenation implemented in a moving bed process known as CCR (Continuing Catalytic Reforming) in English terminology, mention may in particular be made of platinum (Pt)-based catalysts and more particularly PtSnK-Cl type catalysts.

[0006] Numerous works of the prior art describe this type of dehydrogenation catalysts and the means implemented to improve their activity, selectivity and stability.

[0007] For example, US patent 4,430,517 discloses a process for the dehydrogenation of paraffins using PtSnK-Cl catalysts on an alumina support having a gamma crystallographic structure, with a specific surface area of ​​between 25 and 500 m2 / g. The halogen content is between 0.2 and 15% by weight relative to the total weight of the catalyst. The content of alkali or alkaline-earth compound is between 0.01 and 15% by weight relative to the weight of the catalyst. The atomic ratio between the alkali element and platinum is greater than 10, preferably between 15 and 25. The alkali or alkaline-earth element, preferably potassium (K), is intended to neutralize the acidity of the support and thus limit the isomerization and cracking reactions which are detrimental to selectivity. Halogen, preferably chlorine (Cl), helps limit coke formation without promoting cracking reactions, thereby increasing activity without reducing selectivity.

[0008] Patent application US2003 / 0191351A1 discloses a catalytic composition improved PtSnK-Cl on an alumina support whose crystalline phase is predominantly 0 (> 75% by weight relative to the total weight of the support) with a specific surface area of ​​between 50 and 120 m2 / g. The density of the support must be greater than 0.6 g / cm3. The halogen element content is between 0.01 and 15% by weight relative to the total weight of the catalyst, which corresponds to a surface density of chlorine of between 0.014 and 50.8 Cl atoms / nm2. The alkali element content is between 0.9 and 1.1% by weight relative to the total weight of the catalyst, which corresponds to a surface density of potassium of between 1.15 and 3.4 K7 atoms nm2. The atomic ratio between chlorine and potassium Cl / K in this specific case is therefore between 0.004 and 44.

[0009] Patent application US 2011 / 0263416 discloses a paraffin dehydrogenation catalyst using a catalyst comprising an alumina support with a specific surface area of ​​between 50 and 170 m2 / g and an active phase comprising platinum (Pt), tin (Sn), an alkali or alkaline-earth metal at a content of between 0.05 and 3% by weight and a halogen at a content of between 0.1 and 3% by weight relative to the total weight of the catalyst. In fact, in this catalyst, the surface density for chlorine is between 0.070 and 100 atoms Cl / nm2 and that for potassium is between 0.003 and 95 atoms K / nm2. The atomic ratio between chlorine and potassium Cl / K in this specific case is therefore between 0.0007 and 33333. In this patent application, the halogen, preferably chlorine, in addition to limiting the formation of coke, prevents the loss of platinum dispersion during catalyst regeneration. However, its content must not be too high to avoid platinum poisoning.

[0010] There is nevertheless still a need to develop new catalysts having improved performances in terms of activity, selectivity and stability for the dehydrogenation reactions of paraffins and / or naphthenes, and more particularly for the dehydrogenation reaction of propane to propylene.

[0011] The Applicant, in its research into improving the performance of heterogeneous catalysts for the dehydrogenation of paraffins and / or naphthenes, has surprisingly discovered that the performance of such catalysts, in terms of activity, selectivity and stability, is maximized by selecting a halogen element content within a narrow range, on a support comprising a well-defined specific surface area so that the surface density of halogen element as well as the atomic ratio between the halogen element and the alkali or alkaline-earth element are within specific ranges. Objects of the invention

[0012] The subject of the present invention is a catalyst comprising an active phase based on at least one metal from group VIII, at least one element M1 chosen from tin, germanium, lead, gallium, indium and thallium, at least one element M2 chosen from alkali or alkaline-earth elements, and at least one element X chosen from halogens, and a support comprising at least one refractory oxide, characterized in that:

[0013] - the surface density of the element X is between 0.75 and 3.5 atoms X / nm2;

[0014] - the atomic ratio X / M2 is between 1.5 and 3;

[0015] - said support comprises a specific surface area of ​​between 175 and 250 m2 / g.

[0016] According to one or more embodiments, the support is an alumina having a gamma crystal structure.

[0017] According to one or more embodiments, the group VIII metal is platinum.

[0018] According to one or more embodiments, the element Ml is tin.

[0019] According to one or more embodiments, the element M2 chosen from the elements alkali or alkaline earth is potassium.

[0020] According to one or more embodiments, the element X chosen from halogens is chlorine.

[0021] According to one or more embodiments, the surface density of the element M2 chosen from the alkali or alkaline earth elements is between 0.5 and 1.5 atoms of element M2 / nm2.

[0022] According to one or more embodiments, the content of group VIII metal is between 0.02 and 2% by elemental weight of group VIII metal relative to the total weight of the catalyst.

[0023] According to one or more embodiments, the content of element Ml is between 0.01 and 10% by elemental weight of element Ml relative to the total weight of the catalyst.

[0024] According to one or more embodiments, the surface density of the element X chosen from halogens is between 1 and 2.75 atoms X / nm2.

[0025] According to one or more embodiments, the atomic ratio X / M2 is between 1.5 and 2.5.

[0026] According to one or more embodiments, said support comprises a specific surface area of ​​between 185 and 220 m2 / g.

[0027] According to one or more embodiments, said support has a packed filling density value of between 0.50 and 0.70 g / mL.

[0028] Another subject according to the invention relates to a process for preparing a catalyst according to the invention comprising the following steps:

[0029] a) a support comprising the element Ml chosen from tin, germanium, lead, gallium, indium and thallium is prepared to obtain a first catalyst precursor;

[0030] b) the first catalyst precursor obtained in step a) is dried under a flow of a neutral gas or under a flow of a gas containing oxygen at a temperature less than or equal to 250°C, then calcined at a temperature between 350°C and 750°C to obtain a first dried and calcined catalyst precursor;

[0031] c) the first dried and calcined catalyst precursor obtained in step b) is impregnated with an impregnation solution comprising at least one precursor of at least one metal from group VIII and optionally at least one chlorine precursor to obtain a second catalyst precursor;

[0032] d) the second catalyst precursor obtained in step c) is dried under a flow of a neutral gas or under a flow of a gas containing oxygen at a temperature less than or equal to 250°C, then calcined at a temperature between 350°C and 650°C to obtain a second dried and calcined catalyst precursor;

[0033] e) the second dried and calcined catalyst precursor obtained in step d) is impregnated with an impregnation solution comprising a precursor of at least one element M2 and optionally at least one chlorine precursor to obtain a third catalyst precursor;

[0034] f) the third catalyst precursor obtained in step e) is dried under a flow of a neutral gas or under flow of a gas containing oxygen at a temperature less than or equal to 250°C, then calcined at a temperature between 350°C and 650°C;

[0035] it being understood that the chlorine precursor is supplied at least once in step c) and / or in step e).

[0036] Another subject matter according to the invention relates to a process for the dehydrogenation of a hydrocarbon feedstock comprising saturated aliphatic hydrocarbons comprising between 2 and 15 carbon atoms per molecule in which said feedstock is brought into contact with a catalyst according to the invention, or prepared according to the invention, at a pressure of between 0.1 MPa and 4 MPa, at a temperature of between 400°C and 800°C, and with a liquid volumetric space velocity of between 0.5 h 1 and 20 h 1. Detailed description of the invention 1. Definitions

[0037] In the following, the groups of chemical elements are given according to the CAS classification (CRC Handbook of Chemistry and Physics, publisher CRC press, editor-in-chief DR Lide, 81st edition, 2000-2001). For example, group VIII according to the CAS classification corresponds to the metals of columns 8, 9 and 10 according to the new IUP AC classification.

[0038] Specific surface area means the BET specific surface area (SBet in m2 / g) determined by nitrogen adsorption in accordance with standard ASTM D 3663-78 established from the BRUNAUER-EMMETT-TELLER method described in the periodical "The Journal of American Society", 1938, 60, 309.

[0039] The total pore volume of the catalyst or support used for the preparation of the catalyst is understood to mean the volume measured by intrusion with a mercury porosimeter according to standard ASTM D4284 at a maximum pressure of 4000 bars (400 MPa), using a surface tension of 484 dyne / cm and a contact angle of 140°, for example with an Autopore III model device from the Microméritics® brand.

[0040] The wetting angle was taken equal to 140° following the recommendations of the work "Techniques de l'ingénieur, traité analyse et caractérisation", pages 1050-1055, written by Jean Charpin and Bernard Rasneur. In order to obtain better precision, the value of the total pore volume corresponds to the value of the total pore volume measured by intrusion with a mercury porosimeter measured on the sample at 4000 bars (400 MPa) minus the value of the total pore volume measured by intrusion with a mercury porosimeter measured on the same sample for a pressure corresponding to 2 bars (approximately 0.2 MPa).

[0041] The packed filling density (DRT) of the support or catalyst is measured by introducing the support or catalyst into a test tube (typically of volume 100 mL) whose volume has been previously determined and then, by vibration, packing it. until a constant volume is obtained. The apparent density of the packed product is calculated by comparing the mass introduced and the volume occupied after packing. The uncertainty in the measurement is generally of the order of ± 0.01 g / mL.

[0042] The contents of metals, halogen and alkali or alkaline-earth elements are measured by X-ray fluorescence.

[0043] By paraffinic compound (also called indifferently paraffinic hydrocarbon or more simply paraffin), we mean hydrocarbon compounds of general empirical formula CnH2n+2.

[0044] By naphthenic compound (also called indifferently naphthenic hydrocarbon or more simply napthene), we mean hydrocarbon compounds comprising at least one non-aromatic saturated cycle.

[0045] Activity means the mass of converted paraffin expressed in grams of converted paraffin per gram of active metal per hour.

[0046] By selectivity is meant the mass of olefins formed relative to the mass of all the products formed by conversion of the paraffin.

[0047] Stability means the stability of the activity which is generally measured by a percentage drop in activity compared to an activity between 1 hour and 9 hours of testing.

[0048] Surface density means the quantity of element atoms per unit area expressed in square nanometers calculated from the mass content given by an X-ray fluorescence analysis and the BET specific surface area of ​​the catalyst. It is expressed in atoms / nm2.

[0049] Definition of the distribution coefficient R: the distribution profiles of the elements within the catalyst grains are obtained by Castaing microprobe. At least 30 analysis points are carried out along the diameter of the ball or the extrudate. The distribution profile c(x) is thus obtained for x € [-r; +r] with c the local mass concentration of the element, r the radius of the ball or the extrudate and x the position of the analysis point along the diameter of the grain relative to the center of this grain.

[0050] The distribution of the elements is characterized by a dimensionless distribution coefficient R weighting the local concentration by an increasing weight depending on the position on the diameter. By definition:

[0051] [Math.l] r2 Tr R = — j eÇx)dx- / I

[0052] Thus an element whose concentration is uniform has a distribution coefficient R equal to 1, an element deposited in a dome (concentration at the core greater than the concentration at the edges of the support) has a coefficient greater than 1 and an element distributed in a crust (concentration at the edges greater than the concentration at the heart of the support) has a coefficient less than 1. Castaing microprobe analysis gives the values ​​of the concentrations in a finite number of values ​​of x, R is thus evaluated numerically by integration methods well known to those skilled in the art. Preferably, R is determined by the trapezoid method. 2. Catalyst

[0053] The catalyst according to the invention comprises, preferably consists of, an active phase based on at least one metal from group VIII, at least one element M1 chosen from tin, germanium, lead, gallium, indium and thallium, at least one element M2 chosen from alkali or alkaline-earth elements, and at least one element X chosen from halogens, and a support comprising at least one refractory oxide, characterized in that:

[0054] - the surface density of the halogen is between 0.75 and 3.5 atoms X / nm2;

[0055] - the atomic ratio X / M2 is between 1.5 and 3;

[0056] - said support comprises a specific surface area of ​​between 175 and 250 m2 / g.

[0057] Thanks to the combination of these very specific characteristics, the catalyst according to the invention has improved performance in terms of activity, selectivity and stability for the dehydrogenation of paraffins and / or naphthenes and more particularly for the dehydrogenation of propane.

[0058] Advantageously, the content of metal from group VIII, expressed as an element, is between 0.02 and 2% by weight relative to the total weight of the catalyst, preferably between 0.05 and 1.5% by weight, even more preferably between 0.1 and 0.8% by weight.

[0059] Advantageously, the metal from group VIII is chosen from platinum (Pt) or palladium (Pd), preferably platinum.

[0060] The group VIII metal may be present in the final catalyst in oxide, sulfide, halide, oxyhalide form, in chemical combination with one or more of the other components of the catalyst or in elemental metal form.

[0061] Advantageously, the content of element Ml chosen from tin, germanium, lead, gallium, indium and thallium, expressed as an element, in the catalyst according to the invention is between 0.01 and 10% by weight relative to the total weight of the catalyst, more preferably between 0.05 and 5% by weight and very preferably between 0.1 and 1% by weight.

[0062] Preferably, the element Ml is tin (Sn).

[0063] The element Ml can exist in the catalyst in oxide, sulfide, halide, oxyhalide form, in chemical combination with one or more of the other components of the catalyst or in elemental metal form.

[0064] Advantageously, the content of element M2 chosen from alkali or alkaline-earth elements, expressed as an element, in the catalyst according to the invention is between 0.5 and 2.5% by weight, more preferably between 0.6 and 2.0% by weight and very preferably between 0.75 and 1.7% by weight.

[0065] Preferably, the element M2 is potassium (K) or cesium (Cs), and more preferably potassium.

[0066] Advantageously, the surface density of element M2 in the catalyst according to the invention is between 0.5 and 1.5 atoms of element M2 / nm2, more preferably between 0.60 and 1.2 atoms of element M2 / nm2 and very preferably between 0.65 and 1 atom of element M2 / nm2.

[0067] Advantageously, the content of element X chosen from halogens in the catalyst according to the invention is between 0.75 and 5.5% by weight, more preferably between 0.85 and 4% by weight and very preferably between 1 and 3.5% by weight.

[0068] Preferably, element X is selected from the group consisting of fluorine, chlorine, bromine and iodine. Preferably, element X is chlorine (Cl).

[0069] According to the invention, the surface density of element X in the catalyst is between 0.75 and 3.5 atoms of element X / nm2 by weight, more preferably between 0.85 and 2.75 atoms of element X / nm2, more preferably between 1 and 2.75 atoms of element X / nm2, and very preferably between 1 and 2.45 atoms of element X / nm2. Preferably, the halogenated compound is chlorine.

[0070] An essential parameter of the catalyst according to the invention is that the atomic ratio between the element X chosen from halogens and the element M2 chosen from alkali or alkaline-earth compounds is between 1.5 and 3, and preferably between 1.5 and 2.5. Preferably, the halogen is chlorine and the alkali or alkaline-earth is potassium.

[0071] In one embodiment according to the invention, the catalyst may further comprise phosphorus. The phosphorus may be present in the final catalyst as an oxide or mixed oxide compound, phosphate, polyphosphate, sulfide, halide, oxy-halide, hydride, in chemical combination with one or more of the other components of the catalyst.

[0072] In this embodiment, the phosphorus content, expressed as an element, in the catalyst is between 0.4 and 1% by weight relative to the total weight of the catalyst, preferably between 0.4 and 0.8% by weight.

[0073] All the elements (the metal of group VIII, element M1, element M2, element X, optionally phosphorus) are preferably distributed uniformly in the support. This distribution is characterized by a Castaing microprobe analysis by determining a distribution coefficient between 0.8 and 1.1 for all the elements and preferably between 0.9 and 1.0 for all the elements.

[0074] The specific surface area of ​​the catalyst according to the invention is between 175 m2 / g and 250 m2 / g, preferably between 180 m2 / g and 220 m2 / g, preferentially between 185 and 220 m2 / g, more preferably between 185 m2 / g and 210 m2 / g, and even more preferably between 185 m2 / g and 195 m2 / g.

[0075] The catalyst advantageously has a total pore volume measured by mercury porosimetry of between 0.1 cmVg and 1.5 cmVg, preferably between 0.4 cmVg and 0.8 cmVg, and very preferably between 0.4 cmVg and 0.7 cmVg.

[0076] Advantageously, the catalyst has a packed filling density (DRT) value of between 0.50 and 0.70 g / mL, preferably between 0.60 and 0.65 g / mL. 3. Support

[0077] The support generally comprises at least one oxide selected from the group consisting of magnesium, titanium, zirconium, aluminum, silicon oxides. Preferably, the support comprises silica, alumina or silica-alumina, and very preferably alumina. Preferably, the support comprises alumina, and preferably the support is made of alumina. Preferably, the support is a gamma alumina.

[0078] The specific surface area of ​​the support is between 175 m2 / g and 250 m2 / g, preferably between 180 m2 / g and 220 m2 / g, preferentially between 185 and 220 m2 / g, more preferentially between 185 m2 / g and 210 m2 / g, and even more preferentially between 185 m2 / g and 195 m2 / g.

[0079] The support advantageously has a total pore volume measured by mercury porosimetry of between 0.1 cmVg and 1.5 cmVg, preferably between 0.4 cmVg and 0.8 cmVg, and very preferably between 0.4 cmVg and 0.7 cmVg.

[0080] Advantageously, the support has a packed filling density (DRT) value of between 0.50 and 0.70 g / mL, preferably between 0.60 and 0.65 g / mL.

[0081] The support is advantageously in the form of beads, extrudates, pellets or powder. Preferably, the support is in the form of beads. When the support is in the form of beads, its diameter is generally between 0.5 mm and 5 mm, preferably between 1 mm and 2 mm. When the support is in the form of extrudates, the diameter of the extrudates is between 0.5 mm and 5 mm, preferably with a length-to-diameter ratio of 1:1 to 5:1.

[0082] The support can be obtained by any technique known to those skilled in the art. The shaping can be carried out for example by extrusion, by pelletizing, by the drop coagulation method (“oil-drop” according to English terminology), by granulation on a rotating plate or by any other method well known to those skilled in the art. 4. Process for preparing the catalyst

[0083] The catalyst according to the invention can be prepared using any technique known to those skilled in the art. Group VIII metal

[0084] Advantageously, the group VIII metal is supplied to the support in any suitable manner, such as coprecipitation, ion exchange or impregnation. Preferably, it is introduced by impregnation of the support, for example by excess or dry impregnation (the volume of solution containing the element to be introduced corresponding to the pore volume of the support), and preferably by excess impregnation. For this, the support is impregnated with an impregnation solution, aqueous or organic or consisting of a mixture of water and at least one organic solvent, comprising at least one precursor of the group VIII metal.

[0085] In general, hydrogen chloride or another similar acid may also be added to the impregnation solution to further facilitate the incorporation or attachment to the surface of the support of the Group VIII metal and promote uniform distribution of the Group VIII metal in the support.

[0086] When the group VIII metal is platinum, the platinum precursors are part of the following group without this list being limiting: hexachloroplatinic acid, bromoplatinic acid, ammonium chloroplatinate, platinum chlorides, platinum dichlorocarbonyl dichloride, platinum tetraamine chloride or even dihydroxyplatin-diammine. Organic platinum complexes, such as platinum (II) diacetyl acetonate, can also be used. These precursors can be used alone or in a mixture. Preferably, the precursor used is hexachloroplatinic acid. Element Ml

[0087] The element Ml selected from tin, germanium, lead, gallium, indium and thallium can be supplied in any suitable manner, such as coprecipitation, ion exchange or impregnation, at any stage of the catalyst preparation process.

[0088] According to a first variant, the element Ml can be introduced into the support, for example during the synthesis of the support or during the shaping of the support. Without being exhaustive, the techniques of addition before or during the dissolution of the oxide precursors of the support during the synthesis of the support, with or without ripening, may be suitable. The introduction can therefore be simultaneous or successive to the mixing of the precursors of the support. The element Ml can be introduced during the synthesis of the support according to a sol-gel type technique or even be added to an alumina sol. The element Ml can also be introduced during the implementation of the support according to prior art techniques for shaping the support such as shaping procedures by extrusion or by drop coagulation (oil-drop according to Anglo-Saxon terminology).

[0089] According to a second variant, the element Ml can be introduced onto the support, for example by impregnation of the previously shaped support. The impregnation of the support with a solution, aqueous or organic or consisting of a mixture of water and at least one organic solvent, comprising one or more precursors of elements Ml can be carried out by excess solution or dry. The impregnation of the support with a solution containing one or more precursors of element Ml can be carried out before, after or at the same time as the impregnation of the group VIII metal. The impregnation can be carried out in the presence of species acting on the interaction between the precursor of element Ml and the support.These species may be, for example, and without being limiting, mineral acids (HCl, HNO3) or organic acids (carboxylic or polycarboxylic acid types), and organic compounds of the complexing type, as described for example in patents US 6,872,300 and US 6,291,394. Preferably, the impregnation is carried out according to any technique known to those skilled in the art making it possible to obtain a homogeneous distribution of the element Ml within the catalyst.

[0090] According to a third variant, the element M1 can also be introduced partly during the synthesis or shaping of the support and partly by deposition on the shaped support.

[0091] Preferably, the element Ml is introduced into the support, i.e. during the synthesis of the support or during the shaping of the support. In the case of an alumina-based support in the form of beads prepared by the draining technique, the precursor of the element Ml is introduced into the suspension to be drained.

[0092] The precursors of the element Ml may be inorganic or of organometallic type, optionally of water-soluble organometallic type. The precursor of the element Ml may be chosen from the group formed by halogenated compounds, hydroxides, carbonates, carboxylates, sulfates, tartrates and nitrates. These forms of the element Ml may be introduced into the catalyst preparation medium as such or generated in situ (for example by introduction of tin and carboxylic acid). When the element Ml is tin, the tin-based organometallic precursors may be chosen, for example, from the following list: SnR4, where R represents an alkyl group, for example the butyl group, Me3SnCl, Me2SnCl2, Et3SnCl, Et2 SnCl2, EtSnCl3, iPrSnCl2 and the hydroxides Me3SnOH, Me2Sn(OH)2, Et3SnOH, Et2 Sn(OH)2, the oxides (Bu3Sn)2O, the acetate Bu3SnOC(O)Me. Preferably, halogenated species of tin, in particular chlorinated, are used.Even more preferably, the precursor of element Ml is SnCl2 or SnCl4. Element M2

[0093] The element M2 chosen from the alkali or alkaline-earth elements can be supplied in any suitable manner, such as coprecipitation, ion exchange or impregnation and this at any stage of the catalyst preparation process. It can in particular be introduced according to the three variants described in the case of the element M1. Preferably, it is introduced by impregnation, dry or in excess, preferably in excess and particularly preferably it is introduced after having introduced the metal of group VIII as described above.

[0094] The precursor(s) of element M2 chosen from alkali or alkaline-earth elements may be chosen from hydroxides, halides, nitrates, carbonates. When element M2 is potassium, the precursors may be chosen from KOH, KC1, KNO3, K2CO3, or K2PtCl6. Element X

[0095] The element X chosen from halogens can be supplied in any suitable manner, such as coprecipitation, ion exchange or impregnation and this at any stage of the catalyst preparation process. It can in particular be introduced according to the three variants described in the case of the element ML

[0096] In a preferred embodiment, the element X is chlorine. The chlorine is introduced by impregnation, and particularly preferably it is introduced by impregnation at the same time as the group VIII metal or before the impregnation of the group VIII metal. As a possible counter-anion of the compounds comprising the element M1, the group VIII metal and the element M2, chlorine can also be introduced simultaneously with these elements, for example by the use of precursors of the type H2PtCl6, SnCl2 or KC1 or by treatment of the support in one of the preparation steps with hydrochloric acid. Chlorine can also be supplied in the preparation process by an additional oxychlorination step. Phosphorus (optional)

[0097] The phosphorus can be supplied in any suitable manner, such as coprecipitation, ion exchange or by impregnation and this at any stage of the catalyst preparation process. It can in particular be introduced according to the three variants described in the case of the element ML

[0098] According to a variant, the phosphorus is introduced into the support, i.e. during its shaping, for example simultaneously with the ML element

[0099] According to another variant, the phosphorus is introduced by impregnation, and particularly preferably it is introduced by impregnation at the same time as the group VIII metal. In this case, the impregnation solution contains the precursor of the group VIII metal and the precursor of the phosphorus.

[0100] The phosphorus precursors may be acids or salts, and may be chosen from the following compounds: H3PO4, H3PO3, H3PO2, NH4H2PO4, or (NH4)2 HPO4. Order of introduction of precursors

[0101] As described above, the process for preparing the catalyst according to the invention comprises several embodiments which are distinguished in particular by the order of introduction of the metal from group VIII, the element M1, the element M2, the element X and optionally the phosphorus onto the shaped support and / or into the support, i.e. during the synthesis of the support or during the shaping of the support. The process for preparing the catalyst comprises the introduction, simultaneously or successively, in any order, of the metal from group VIII, the element M1, the element M2, the element X and optionally the phosphorus onto the shaped support and / or into the support.

[0102] When the element M1 and / or the element M2 and / or the element X and / or optionally phosphorus are introduced into the support, i.e. during the synthesis of the support or during the shaping of the support, the preparation process generally comprises a drying step and a calcination step before the deposition of the group VIII metal. The drying is generally carried out at a temperature less than or equal to 250°C, preferably between 50°C and 250°C, more preferably between 70°C and 200°C, in air or under an inert atmosphere. The calcination is preferably carried out at a temperature between 350°C and 750°C and preferably between 400°C and 600°C and even more preferably between 400°C and 550°C. The temperature rise may be steady or include intermediate temperature stages, these stages being reached with fixed or variable temperature rise rates.These temperature increases can therefore be identical or differ in their speed (in degrees per minute or per hour). The gas atmosphere used during calcination contains oxygen. Air can therefore also be used during this calcination stage. The calcination gas may possibly contain water.

[0103] When one or more elements from the metal of group VIII, the element M1, the element M2, and / or the element X, optionally phosphorus, are introduced onto the shaped support, preferably by dry or excess impregnation, the introduction of said elements can be simultaneous by a single impregnation solution or take place separately by several impregnation solutions containing one or more of the components and this in any order.

[0104] Any impregnation solution described in the present invention may comprise any polar solvent known to those skilled in the art. Said polar solvent used is advantageously chosen from the group formed by methanol, ethanol, water, phenol, cyclohexanol, taken alone or in a mixture. Said polar solvent can also be advantageously chosen from the group formed by propylene carbonate, DMSO (dimethyl sulfoxide), N-methylpyrrolidone (NMP) or sulfolane, taken alone or in a mixture. Preferably, a polar protic solvent is used. A list of common polar solvents and their dielectric constant can be found in the book "Solvents and Solvent Effects in Organic Chemistry", C. Reichardt, Wiley-VCH, 3rd edition, 2003, pages 472-474. Very preferably, the solvent used is water or ethanol, and particularly preferably, the solvent is water.

[0105] After each impregnation step, the catalyst precursor obtained is preferably dried in order to remove all or part of the solvent introduced during the impregnation, preferably at a temperature below 250°C, more preferably between 50°C and 250°C, and more preferably between 70°C and 200°C. The drying is advantageously carried out for a period of between 1 and 24 hours, preferably between 1 and 20 hours. The drying is carried out in air, or under an inert atmosphere (nitrogen for example). After the drying step, the catalyst is preferably calcined, generally in air. The calcination temperature is generally between 350°C and 650°C and preferably between 400°C and 650°C, and even more preferably between 450°C and 550°C. The temperature ramp may optionally contain temperature steps. The calcination time is generally between 0.5 hours and 16 hours, preferably between 1 hour and 5 hours.The gas atmosphere used during calcination contains oxygen. Air can therefore also be used during this calcination step. The calcination gas may optionally contain water.

[0106] In a particular embodiment, the catalyst according to the invention is prepared according to a preparation process comprising the following successive steps:

[0107] a) a support is prepared comprising the element Ml chosen from tin, germanium, lead, gallium, indium and thallium to obtain a first catalyst precursor;

[0108] b) the first catalyst precursor obtained in step a) is dried under a flow of a neutral gas or under a flow of a gas containing oxygen at a temperature less than or equal to 250°C, then calcined at a temperature between 350°C and 750°C to obtain a first dried and calcined catalyst precursor;

[0109] c) the first dried and calcined catalyst precursor obtained in step b) is impregnated with an impregnation solution comprising at least one precursor of at least one metal from group VIII and optionally at least one chlorine precursor to obtain a second catalyst precursor;

[0110] d) the second catalyst precursor obtained in step c) is dried under a flow of a neutral gas or under a flow of a gas containing oxygen at a lower temperature or equal to 250°C, then calcined at a temperature between 350°C and 650°C to obtain a second dried and calcined catalyst precursor;

[0111] e) the second dried and calcined catalyst precursor obtained in step d) is impregnated with an impregnation solution comprising a precursor of at least one element M2 and optionally at least one chlorine precursor to obtain a third catalyst precursor;

[0112] f) the third catalyst precursor obtained in step e) is dried under a flow of a neutral gas or under a flow of a gas containing oxygen at a temperature less than or equal to 250°C, then calcined at a temperature between 350°C and 650°C;

[0113] g) optionally, an oxychlorination step is carried out at a temperature between 350°C and 550°C and under a pressure between 0.1 and 1.5 MPa, then calcination is carried out at a temperature between 350°C and 650°C;

[0114] it being understood that the chlorine precursor is supplied at least once either in step c) and / or in step e), or possibly in step g).

[0115] Preferably, the introduction of the element M2 chosen from the alkali or alkaline-earth elements, and more particularly potassium, is carried out on a catalyst precursor comprising the metal of group VIII, more particularly platinum, previously dried and calcined. Indeed, the fact of introducing the potassium after the platinum makes it possible to avoid a leaching effect of the platinum during the impregnation of the metal of group VIII.

[0116] In step a), a support is prepared comprising the element Ml, preferably tin. The element Ml, preferably tin, can be introduced at any time during the preparation of the support, and preferably during shaping, or by impregnation on an already formed support. Preferably, the element Ml is introduced during the shaping of the support.

[0117] Similarly, the phosphorus can be introduced at any time during the preparation of the support, and preferably during shaping, or by impregnation on an already formed support. According to one variant, the phosphorus is introduced into the support, i.e. during the shaping of the support, preferably with the element M1, preferably tin. According to another variant, the phosphorus is introduced by impregnation, and particularly preferably it is introduced by impregnation at the same time as the group VIII metal.

[0118] The introduction of the group VIII metal can advantageously be carried out by one or more excess impregnations of solution on the support, or by one or more dry impregnations, and, preferably, by a single excess impregnation of said support (preferably containing the element Ml, preferably tin, and optionally phosphorus), using solution(s), preferably aqueous, containing the precursor of the group VIII metal and preferably the phosphorus precursor (when the support does not contain or partially contains phosphorus).

[0119] In step e) the second dried and calcined catalyst precursor obtained in step d) is impregnated with an impregnation solution comprising at least one precursor of an element M2 chosen from alkali or alkaline-earth elements. The introduction of the alkali or alkaline-earth element(s) may advantageously be carried out by one or more excess solution impregnations on the support, or by one or more dry impregnations, and, preferably, by a single dry or excess impregnation of said precursor, using solution(s), preferably aqueous, containing at least one precursor of the alkali or alkaline-earth element, and preferably at least one potassium precursor.

[0120] In optional step g), the chlorine is supplied by means of an oxychlorination treatment. Such a treatment may for example be carried out at a temperature between 350°C and 550°C and under a pressure between 0.1 MPa and 1.5 MPa, for a duration preferably between 30 minutes and 10 hours, and under a flow of air containing the desired quantity of chlorine and possibly containing water.

[0121] According to another variant, the catalyst according to the invention can be prepared by preparing a support comprising tin by introducing the tin precursor during the shaping of the support, followed by one or more excess solution impregnations on the support, or by one or more dry impregnations, using solution(s), preferably aqueous, containing a precursor of a metal from group VIII, a phosphorus precursor and a precursor of an alkali or alkaline-earth element and preferably a potassium precursor, alone or in a mixture, then drying and calcining under the conditions described above.

[0122] When the various precursors used in the preparation of the catalyst according to the invention do not contain halogen or contain halogen in insufficient quantity, it may be necessary to add a halogenated compound during the preparation. Any compound known to those skilled in the art may be used and incorporated into any of the steps of preparation of the catalyst according to the invention. In particular, it is possible to use organic compounds such as methyl or ethyl halides, for example dichloromethane, dichloroethane, dichloropropane, chloroform, methylchloroform or carbon tetrachloride.

[0123] The halogen can also be added by means of impregnation with an aqueous solution of the corresponding acid, for example hydrochloric acid, at any time during the preparation. A typical protocol consists of impregnating the solid so as to introduce the desired quantity of halogen. The catalyst is kept in contact with the aqueous solution for a time long enough to deposit this quantity of halogen. Additional reduction step (optional)

[0124] In an embodiment according to the invention, prior to the use of the catalyst in the catalytic reactor and the implementation of a dehydrogenation process, a reducing treatment step is carried out in the presence of a reducing gas so as to obtain a catalyst comprising said metal from group VIII and said element M1 at least partially in metallic form. This step is advantageously carried out in situ, that is to say after the loading of the catalyst into a dehydrogenation reactor. Carrying out the reducing treatment of the catalyst in situ makes it possible to dispense with an additional step of passivation of the catalyst by an oxygenated compound or by CO2, which is necessarily the case when the catalyst is prepared by carrying out a reducing treatment ex situ, that is to say outside the reactor used for the dehydrogenation.Indeed, when the reducing treatment is carried out ex-situ, it is necessary to carry out a passivation step in order to preserve the metallic phase of the catalyst in the presence of air (during the operations of transporting and loading the catalyst into the hydrogenation reactor), then to carry out a new step of reducing the catalyst.

[0125] The reducing gas is preferably hydrogen. Hydrogen can be used pure or in a mixture (for example a hydrogen / nitrogen, hydrogen / argon, hydrogen / methane mixture). In the case where hydrogen is used in a mixture, all proportions are possible.

[0126] Preferably, said reducing treatment is carried out at a temperature between 100°C and 600°C, and preferably between 200°C and 580°C, under a stream of hydrogen, pure or diluted, up to the maximum reduction temperature, followed by maintenance for example for 30 minutes to 6 hours at this temperature. The rise in temperature up to the desired reduction temperature is generally slow, for example set between 0.1 and 10°C / min, preferably between 0.3 and 7°C / min.

[0127] The hydrogen flow rate, expressed in L / hour / gram of catalyst precursor, is between 0.01 and 100 L / hour / gram of catalyst, preferably between 0.05 and 10 L / hour / gram of catalyst precursor, even more preferably between 0.1 and 5 L / hour / gram of catalyst precursor. Passivation step (optional)

[0128] The process according to the invention may advantageously comprise a step of passivation by a sulfur compound which makes it possible to improve the selectivity of the catalysts and to avoid thermal runaways during the start-up of new catalysts ("run-away" according to English terminology). The passivation step is carried out by implementing methods known to those skilled in the art.

[0129] The passivation step by a sulfur compound is generally carried out at a temperature temperature between 20 and 350°C, preferably between 40 and 200°C, for 10 minutes to 240 minutes. The sulfur compound is for example chosen from the following compounds: thiophene, thiophane, alkylmonosulfides such as dimethylsulfide, diethylsulfide, dipropylsulfide and propylmethylsulfide or an organic disulfide of formula HO-Ri-SS-R2-OH such as di-thio-di-ethanol of formula HO-C2H4-SSC 2H4-OH (often called DEODS). The sulfur content is generally between 0.1 and 2% by weight of said element relative to the total weight of the catalyst.

[0130] 5. Process for the dehydrogenation of paraffins and / or naphthenes

[0131] The invention also relates to a process for dehydrogenation of a hydrocarbon feedstock comprising paraffinic and / or naphthenic compounds in the presence of the catalyst according to the invention.

[0132] The processes for dehydrogenating paraffins and / or naphthenes make it possible to selectively produce olefins and contribute to the production of significant quantities of hydrogen essential for the hydrogenation and hydrotreatment processes of a petrochemical complex or a refinery.

[0133] The hydrocarbon feedstock generally comprises paraffinic and / or naphthenic compounds containing from 2 to 30 carbon atoms per molecule, taken alone or in a mixture. More particularly, the hydrocarbon feedstock comprises paraffinic and / or naphthenic compounds comprising 2 to 15 carbon atoms per molecule, preferably paraffinic compounds comprising 2 to 5 carbon atoms per molecule, such as propane, n-butane, n-pentane, isomers of butane and pentane or their mixture, and / or preferably naphthenic compounds comprising from 5 to 12 carbon atoms such as cyclohexane, methylcyclohexane, decalin or their mixture. The feedstock may also comprise unsaturated hydrocarbons comprising 2 to 15 carbon atoms per molecule.

[0134] Typically, the dehydrogenation catalyst is loaded into a unit and previously subjected to a reduction treatment as described above. It can be implemented in any manner known to those skilled in the art. It can, for example, be implemented in a fixed bed or in a moving bed, preferably in a moving bed. According to a variant of the invention, the dehydrogenation catalyst is implemented in several reactors installed in series.

[0135] The various processes for dehydrogenation of paraffins and naphthenes are differentiated by the choice of operating conditions and the composition of the feedstock. The adjustment of the operating conditions, depending on the nature of the feedstock to be treated, is done in such a way as to obtain the best pressure-temperature-yield and activity match in a manner known to those skilled in the art.

[0136] Generally, the process for dehydrogenating a hydrocarbon feedstock comprising paraffins and / or naphthenes is carried out at a pressure of between 0.1 MPa and 4 MPa, at a temperature between 200°C and 800°C and with a liquid volumetric space velocity between 0.5 h 1 and 50 h1.

[0137] More particularly, the paraffin dehydrogenation reaction is carried out at a pressure of between 0.1 MPa and 4 MPa and more preferably between 0.25 MPa and 3.0 MPa and at a temperature of between 400 and 800°C depending on the nature of the feedstock, the temperature being advantageously between 560 and 700°C for a feedstock comprising mainly propane, between 450 and 600°C for a feedstock comprising mainly isobutane, and between 400 and 550°C for a feedstock comprising mainly isopentane. It may be advantageous to use hydrogen as a diluent. The hydrogen / hydrocarbon molar ratio of the feedstock is generally between 0.1 and 10, preferably between 0.5 and 8.The liquid volumetric space velocity of the hydrocarbon feedstock (LHSV or Liquid Hourly Space Velocity according to English terminology), the unit of which is in liters of hydrocarbon feedstock per liter of catalyst and per hour, is preferably between 0.5 and 50 h1, more preferably between 1.5 and 15 h1.

[0138] More particularly, the naphthenes dehydrogenation reaction is carried out at a pressure of between 0.1 and 2 MPa, preferably between 0.1 and 1 MPa, and at a temperature of between 200 and 400°C. The mass flow rate of treated feedstock per unit mass of catalyst is generally between 0.5 and 50 h1.

[0139] The catalyst according to the invention can be regenerated by at least one combustion step in an oxidizing medium.

[0140] The regeneration of the catalyst is carried out in a cyclic or continuous system. It can consist of a simple combustion of the coke deposits. This combustion operation is usually carried out by injecting air into an inert mixture. The oxygen content in the gas at the regeneration inlet is preferably between 0.1 and 2% by volume. The combustion is usually carried out at a temperature between 350 and 550°C and under pressure between 0.1 and 1.5 MPa.

[0141] Combustion may optionally be preceded by an operation of stripping the sulfur contained in the catalyst in the case where the catalyst comprises sulfur introduced by injection of DMDS for example.

[0142] The regeneration may also include, at the end of the coke combustion step, a catalyst oxyhalogenation step, preferably oxychlorination. For this, the oxygen content in the gas at the regeneration inlet is increased by at least 10% compared to the value of the previous combustion step. At least one halogenated derivative, i.e. at least one halogen and / or one halogenated compound, is introduced simultaneously. Chlorine and / or a chlorinated compound is preferably used. The proportion of halogen and / or halogenated compound used is such that 0.2 to 1.5% by weight of a halogenated alumina derivative can be formed relative to the catalyst. subjected to regeneration. Oxyhalogenation is carried out at a temperature between 350 and 550°C and under a pressure between 0.1 MPa and 1.5 MPa. A catalyst calcination step is generally carried out after oxyhalogenation, during which the oxygen content in the gas at the regeneration inlet is between 3 and 20% by volume, the average temperature is between 350 and 550°C and the pressure is between 0.1 MPa and 1.5 MPa.

[0143] Before subjecting the regenerated catalyst to the reaction conditions, it undergoes a preliminary reduction under a gas containing hydrogen, preferably under pure hydrogen. This reduction can be carried out in the regeneration chamber if this is separate from the reaction chamber, in the reaction chamber itself or in an intermediate zone separate from the regeneration and reaction zones. This reduction, if it has not been carried out prior to the reaction, can also occur in the reaction chamber after the reaction has started: the first stages of the reaction then serve to transform the catalyst into a catalytically active form for dehydrogenation. The reduction is carried out under a stream of gas containing hydrogen, preferably under pure hydrogen, at a temperature between 330 and 600°C and at a pressure between 0.2 and 2.5 MPa, preferably between 0.4 and 1.5 MPa.

[0144] Possible sulfurization of the catalyst can follow this reduction step and therefore precede the dehydrogenation reaction itself.

[0145] All or part of the hydrogen produced can be recycled to the inlet of the dehydrogenation reactor. All or part of the unconverted propane can be recycled to the inlet of the dehydrogenation reactor. Examples

[0146] The following examples illustrate the invention without limiting its scope.

[0147] Support 1: In examples 1, 2, 4, 5 and 6, a gamma alumina is used having the following properties: SBet = 190 m2 / g, Total pore volume = 0.65 cm3 / g, support density (DRT) = 0.63 g / cm3, tin content 0.30% by weight.

[0148] Support 2 (non-compliant): In example 3, a predominantly theta alumina is used with the following properties: SBet = 80 m2 / g, Total pore volume = 0.57 cm3 / g, support density (DRT) = 0.70 g / cm3, tin content 0.30% by weight.

[0149] Example 1: Catalyst A PtSnKCl / Al2O3 (comparative)

[0150] A catalyst A is prepared on support 1 aiming for a deposition of 0.3% by weight of platinum element, 0.25 Cl atoms / nm2 (non-compliant) and 1.00 K atoms / nm2 on the final catalyst.

[0151] To 100 g of alumina support containing tin, 400 cm3 of an aqueous solution of hexachloroplatinic acid at 37.75 g / L and hydrochloric acid at 6.95 g / L are added. by excess impregnation. Leave in contact for 4 hours then drain. Dry at 120°C in an oven for 15 hours and calcine in a crossed bed at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.

[0152] To 100 g of this calcined solid, 440 cm3 of a potassium carbonate solution at a concentration of 26.3 g / L is added by excess impregnation. Drying is carried out at 120°C for 15 hours and then calcined at 500°C under an air flow rate of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.

[0153] Catalyst A obtained after calcination contains 0.29% by weight of platinum element, 0.29% by weight of tin element, 0.26% by weight of chlorine element relative to the total weight of the catalyst, i.e. a density of 0.23 Cl atoms / nm2 (non-compliant), and a content of 2.3% by weight of potassium element, i.e. a density of 1.86 K atoms / nm2, and therefore a Cl / K atomic ratio of 0.12 (non-compliant).

[0154] Example 2: Catalyst B PtSnKCl / Al2O3 (comparative)

[0155] A catalyst B is prepared on support 1, aiming for a deposition of 0.3% by weight of platinum element, 0.61 Cl atoms / nm2 (non-compliant) and 0.61 K atoms / nm2 on the final catalyst.

[0156] To 100 g of alumina support containing tin, 400 cm3 of an aqueous solution of hexachloroplatinic acid and hydrochloric acid are added by impregnation in excess hexachloroplatinic acid at 37.75 g / L and hydrochloric acid at 6.95 g / L by impregnation in excess ès. The mixture is left in contact for 4 hours and then drained. It is dried at 120°C for 15 h and then calcined at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.

[0157] To 100 g of this calcined solid, 75 cm3 of a potassium carbonate solution at a concentration of 12.7 g / L is added by dry impregnation. It is left to mature, dried at 120°C in an oven for 15 hours and then calcined in a crossed bed at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.

[0158] Catalyst B obtained after calcination contains 0.30% of platinum element, 0.29% by weight of tin element, 0.9% by weight of chlorine element, i.e. a density of 0.61 Cl atoms / nm2 (non-compliant), and 0.48% by weight of potassium element, i.e. a density of 0.39 K atoms / nm2, and therefore a Cl / K atomic ratio of 1.55.

[0159] Example 3: Catalyst C PtSnKCl / Al2O3 (comparative)

[0160] A catalyst C is prepared on support 2 (non-compliant), aiming for a deposition of 0.3% by weight of platinum element, 1.70 atoms Cl / nm2 and 1.00 atoms K / nm2 on the final catalyst.

[0161] To 100 g of alumina support containing tin, 400 cm3 of an aqueous solution of hexachloroplatinic acid at 37.75 g / L and hydrochloric acid at 6.95 g / L are added. by excess impregnation. Leave in contact for 4 hours then wring. Dry at 120°C for 15 hours then calcine at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.

[0162] To 100 g of this calcined solid, 50 cm3 of a potassium carbonate solution at a concentration of 15.9 g / L are added by dry impregnation. The mixture is left to mature, dried at 120°C for 15 hours and then calcined at 500°C under an air flow rate of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.

[0163] Catalyst C obtained after calcination contains 0.30% by weight of platinum element, 0.29% by weight of tin element, 0.9% by weight of chlorine element, i.e. a density of 1.70 Cl atoms / nm2, and 0.6% by weight of potassium element, i.e. a density of 1.03 K atoms / nm2, and therefore a Cl / K atomic ratio of 1.71.

[0164] Example 4: Catalyst D PtSnKCl / Al2O3 (non-compliant)

[0165] A catalyst D is prepared on support 1, aiming for a deposition of 0.3% by weight of platinum element, 1.15 Cl atoms / nm2 and 2.0 K atoms / nm2 on the final catalyst.

[0166] To 100 g of alumina support containing tin, 400 cm3 of an aqueous solution of hexachloroplatinic acid at 37.75 g / L and hydrochloric acid at 6.95 g / L are added by excess impregnation. The mixture is left in contact for 4 hours and then drained. It is dried at 120°C for 15 h and then calcined at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.

[0167] To 100 g of this calcined solid, 75 cm3 of a potassium carbonate solution at a concentration of 57.4 g / L are added by dry impregnation. It is left to mature, dried at 120°C for 15 h and then calcined at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.

[0168] Catalyst D obtained after calcination contains 0.30% by weight of platinum element, 0.29% by weight of tin element, 1.27% by weight of chlorine element, i.e. a density of 1.13 Cl atoms / nm2, and a content of 2.50% by weight of potassium element, i.e. a density of 2.03 K atoms / nm2, and therefore a Cl / K atomic ratio of 0.56 (non-compliant).

[0169] Example 5: Catalyst E PtSnKCl / Al2O3 (according to the invention)

[0170] A catalyst E is prepared on support 1, aiming for a deposition of 0.3% by weight of platinum element, 1.15 Cl atoms / nm2 and 0.75 K atoms / nm2 on the final catalyst.

[0171] To 100 g of alumina support containing tin, 400 cm3 of an aqueous solution of hexachloroplatinic acid at 37.75 g / L and hydrochloric acid at 6.95 g / L are added by excess impregnation. The mixture is left in contact for 4 hours and then drained. It is dried at 120°C for 15 h and then calcined at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.

[0172] To 100 g of this calcined solid is added 75 cm3 of a solution of carbonate of potassium at a concentration of 21.9 g / L by dry impregnation. Allow to mature, dry at 120°C for 15 hours and then calcine at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.

[0173] The catalyst E obtained after calcination contains 0.30% by weight of platinum element, 0.29% by weight of tin element, 1.27% by weight of chlorine element, i.e. a density of 1.13 Cl atoms / nm2, and 1.39% by weight of potassium element, i.e. a density of 0.75 K atoms / nm2, and therefore a Cl / K atomic ratio of 1.51.

[0174] Example 6: Catalyst F PtSnKCl / Al2O3 (according to the invention)

[0175] A catalyst F is prepared on support 1, aiming for a deposition of 0.3% by weight of platinum element, 2.30 Cl atoms / nm2 and 1.00 K atoms / nm2 on the final catalyst.

[0176] To 100 g of alumina support containing tin, 400 cm3 of an aqueous solution of hexachloroplatinic acid at 37.75 g / L and hydrochloric acid at 6.95 g / L are added by excess impregnation. The mixture is left in contact for 4 hours and then drained. It is dried at 120°C for 15 h and then calcined at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.

[0177] To 100 g of this calcined solid, 430 cm3 of a potassium chloride solution at a concentration of 29.5 g / L is added by excess impregnation. It is left to mature, dried in an oven at 120°C for 15 hours and then calcined in a crossed bed at 500°C under an air flow of 100 liters per hour for 3 hours, with a temperature rise rate of 7°C per minute.

[0178] The catalyst F obtained after calcination contains 0.30% by weight of platinum element, 0.29% by weight of tin element, 2.52% by weight of chlorine element, i.e. a density of 2.25 Cl atoms / nm2, and a content of 1.30% by weight of potassium element, i.e. a density of 1.05 K atoms / nm2, and therefore a Cl / K atomic ratio of 2.14.

[0179] Example 7: Process for the dehydrogenation of propane using catalysts A to F

[0180] 10 cm3 of catalyst are introduced into a reactor provided with a shell electric heating. The gas flows are sent in a downward current, that is, from top to bottom relative to the catalytic bed.

[0181] The reduction step is carried out with the following protocol: the catalyst is heated under inert gas to 150°C with a ramp of 5°C / min then maintained at 150°C for 1h30. The inert gas is replaced by hydrogen and the temperature is raised to 635°C with a ramp of 5°C / min then maintained at 635°C for 9h30. The reduction step is then completed and the hydrogen flow rate is set at 28 L / h.

[0182] The propane flow rate is in turn set to 28 L / h, i.e. a LHSV of 10.8 h1. The time of flow rate adjustment corresponds to the initial reaction time. The pressure is maintained at atmospheric. The gaseous effluent is analyzed by chromatography gaseous by calculating the volume and mass proportions of each compound. The major products formed participating in the calculation of selectivity are methane, ethane, ethylene, propylene and benzene.

[0183] The conversion is calculated by making the ratio of the mass quantity of products formed analyzed in the effluent to the mass quantity of propane injected.

[0184] The activity is calculated by determining the mass quantity of propane converted per gram of platinum per hour.

[0185] Propylene selectivity is calculated by dividing the mass quantity of propylene formed by the sum of the mass quantities of all the reaction products at a propane conversion level of 28%.

[0186] The benzene selectivity is calculated by taking the ratio of the mass quantity of benzene formed to the sum of the mass quantities of all the reaction products at a propane conversion level of 28%. The benzene selectivity is particularly informative as to the propensity of the catalyst to produce coke and to deactivate: the higher this selectivity, the more easily the catalyst will coke.

[0187] Stability is determined by comparing the initial activity of the catalyst with the activity at 9 hours of TOS (Time on Stream): % loss of activity = ((activity at 1 hour of TOS) - (activity at 9 hours of TOS)) / (activity at 1 hour of TOS).

[0188] Table 1 below reports the activities after 1 hour and 9 hours of “Time On Stream”, the percentage of loss of activity between 1 hour and 9 hours of TOS and the maximum selectivities obtained in propylene and benzene.

[0189] [Tables 1] Catalyst Surface density Cl (Cl atoms / nm2) Cl / K ratio Sbet (m2 / g ) Activity at 1 h of TOS gC3 / gPt / h Activity at 9 h of TOS gC3 / gPt / h % loss of activity Selectivity Propylene %wt Selectivity Benzene %wt A (comparati 0 0.23 0.12 190 172 162 6.0 87.0 0.00 B (comparati 0 0.61 1.55 190 650 430 33.8 94.1 0.75 C (comparati 0 1.70 1.71 80 820 590 28.1 94.3 0.60 D (non-compliant) 1.13 0.56 190 250 225 10.0 94.3 0.60 E (compliant) 1.13 1.51 190 900 780 13.3 96.9 0.25 F (compliant) 2.25 2.14 190 1050 990 5.7 98.5 0.20

[0190] The performance of non-compliant catalyst A comprising a surface density of chlorine of less than 0.75 atoms K / nm2 and a Cl / K ratio of less than 1.5 shows a deficit in activity and propylene selectivity compared to the catalysts according to the invention.

[0191] The performance of non-compliant catalyst B comprising a surface density of chlorine of less than 0.75 atoms K / nm2 shows a deficit in activity and propylene selectivity as well as a high value of benzene selectivity and deactivation rate compared to the catalysts according to the invention.

[0192] The performance of non-compliant catalyst C with a surface area of ​​less than 175 m2 / g shows a deficit in activity and propylene selectivity as well as a high value of benzene selectivity and deactivation rate compared to the catalysts according to the invention.

[0193] The performance of non-compliant catalyst D with a Cl / K ratio of less than 1.5 shows a deficit in propylene activity and selectivity as well as a high benzene selectivity value compared to the catalysts according to the invention.

[0194] The performances of catalysts E and F according to the invention comprising a top surface area between 175 and 250 m2 / g, a Cl / K ratio between 1.5 and 3, and a surface density of chlorine between 0.75 and 3.5 Cl atoms / nm2 present the best results in terms of activity and propylene selectivity while keeping the benzene selectivity and the deactivation rate at low levels.

Claims

Claims

1. Catalyst comprising an active phase based on at least one metal from group VIII, at least one element M1 chosen from tin, germanium, lead, gallium, indium and thallium, at least one element M2 chosen from alkali or alkaline-earth elements, and at least one element X chosen from halogens, and a support comprising at least one refractory oxide, characterized in that: - the surface density of element X is between 0.75 and 3.5 atoms X / nm2; - the atomic ratio X / M2 is between 1.5 and 3; - said support comprises a specific surface area of ​​between 175 and 250 m2 / g.

2. Catalyst according to claim 1, characterized in that the support is an alumina having a gamma crystalline structure.

3. Catalyst according to one of claims 1 or 2, characterized in that the metal of group VIII is platinum.

4. Catalyst according to any one of the preceding claims, characterized in that the element Ml is tin.

5. Catalyst according to any one of the preceding claims, characterized in that the element M2 chosen from the alkali or alkaline-earth elements is potassium.

6. Catalyst according to any one of the preceding claims, characterized in that the element X chosen from halogens is chlorine.

7. Catalyst according to any one of the preceding claims, characterized in that the surface density of the element M2 chosen from the alkali or alkaline-earth elements is between 0.5 and 1.5 atoms of element M2 / nm2.

8. Catalyst according to any one of the preceding claims, characterized in that the content of group VIII metal is between 0.02 and 2% by elemental weight of group VIII metal relative to the total weight of the catalyst.

9. Catalyst according to any one of the preceding claims, characterized in that the content of element Ml is between 0.01 and 10% by elemental weight of element Ml relative to the total weight of the catalyst.

10. Catalyst according to any one of the preceding claims, characterized in that the surface density of the element X chosen from the halogens is between 1 and 2.75 X atoms / nm2.

11. Catalyst according to any one of the preceding claims, characterized in that the atomic ratio X / M2 is between 1.5 and 2.

5.

12. Catalyst according to any one of the preceding claims, characterized in that said support comprises a specific surface area of ​​between 185 and 220 m2 / g.

13. Catalyst according to any one of the preceding claims, characterized in that said support has a packed filling density value of between 0.50 and 0.70 g / mL.

14. A process for preparing a catalyst according to any one of claims 1 to 13 comprising the following steps: a) a support comprising the element Ml chosen from tin, germanium, lead, gallium, indium and thallium is prepared to obtain a first catalyst precursor; b) the first catalyst precursor obtained in step a) is dried under a flow of a neutral gas or under a flow of a gas containing oxygen at a temperature less than or equal to 250°C, then calcined at a temperature between 350°C and 750°C to obtain a first dried and calcined catalyst precursor; c) the first dried and calcined catalyst precursor obtained in step b) is impregnated with an impregnation solution comprising at least one precursor of at least one metal from group VIII and optionally at least one chlorine precursor to obtain a second catalyst precursor;d) the second catalyst precursor obtained in step c) is dried under a flow of a neutral gas or under a flow of a gas containing oxygen at a temperature less than or equal to 250°C, then calcined at a temperature between 350°C and 650°C to obtain a second dried and calcined catalyst precursor; e) the second dried and calcined catalyst precursor obtained in step d) is impregnated with an impregnation solution comprising a precursor of at least one element M2 and optionally at least one chlorine precursor to obtain a third catalyst precursor; f) the third catalyst precursor obtained in step e) is dried under a flow of a neutral gas or under a flow of a gas containing oxygen at a temperature less than or equal to 250°C, then calcined at a temperature between 350°C and 650°C; it being understood that the chlorine precursor is supplied at least; once at step c) and / or step e).

15. A process for the dehydrogenation of a hydrocarbon feedstock comprising saturated aliphatic hydrocarbons comprising between 2 and 15 carbon atoms per molecule, in which said feedstock is brought into contact with a catalyst according to any one of claims 1 to 13, or prepared according to claim 14, at a pressure of between 0.1 MPa and 4 MPa, at a temperature of between 400°C and 800°C, and with a liquid volumetric space velocity of between 0.5 h 1 and 20 h 1.

Citation Information

Patent Citations

  • Dehydrogenation catalyst composition

    US20030191351A1

  • Dehydrogenation catalyst

    US20110263416A1

  • Process for improving catalysts

    US6291394B1

  • Reforming catalyst with chelated promotor

    US6872300B1

  • A catalyst with increased selectivity for n-butene and 1,3-butadiene in dehydrogenation and dehydroisomerization of n-butane and a method for producing a mixture of n-butane, 1,3-butadiene and iso-butene in high yield using the same

    KR101440695B1