A PROCESS FOR PREPARING A MATERIAL USEFUL FOR LITHIUM EXTRACTION, SAID MATERIAL AND ITS USES
A geopolymer matrix material with selective lithium adsorbents, synthesized via a sol-gel process, addresses the challenges of lithium extraction from high-salinity environments by ensuring high capacity, rapid kinetics, and mechanical stability, facilitating industrial scalability.
Patent Information
- Application Number
- FR2023005204
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-29
AI Technical Summary
Existing technologies face challenges in efficiently extracting lithium from high-salinity aqueous environments such as geothermal brines and salt lakes, as they often result in physico-chemical alteration of the brine composition, limited accessibility of adsorbent sites, and are difficult to scale up industrially due to complex synthesis processes and mechanical weaknesses.
A geopolymer matrix material is synthesized using a sol-gel process, incorporating lithium hydroxide and alumino-silicate sources, which forms a mesoporous structure with selective lithium adsorbents, allowing high lithium extraction capacity, rapid sorption kinetics, and mechanical strength suitable for fixed bed processes.
The geopolymer matrix material achieves high lithium extraction capacity, rapid sorption kinetics, and mechanical stability, enabling efficient lithium recovery from saline solutions without altering their composition, and is easily scalable for industrial use.
Smart Images

Figure 00000019_0000 
Figure 00000019_0001 
Figure 00000019_0002
Abstract
Description
Title of the invention: METHOD FOR PREPARING A MATERIAL USEFUL FOR LITHIUM EXTRACTION, SAID MATERIAL AND ITS USES technical field
[0001] The present invention relates to the field of lithium extraction and in particular to the field of lithium extraction involving solid materials.
[0002] Thus, the present invention proposes a method for preparing a solid geopolymer matrix material optionally comprising lithium-selective adsorbents, the material thus prepared, and its uses, particularly for lithium extraction. PRIOR TECHNOLOGY
[0003] Demand for lithium has increased sharply over the last decade due to the growth in the use of lithium-ion batteries. This growth stems from the electrification of transport and environmental regulations aimed at reducing the use of fossil fuels.
[0004] Today, the two primary lithium resources are rocks such as spodumene, epidolite, and petalite, and brines from salt flats found in many countries, including Argentina, Bolivia, and Chile. Geothermal waters also contain significant quantities of lithium by weight and are being studied at a pilot scale as a lithium resource. Lithium-ion battery recycling processes and manufacturing waste are also secondary lithium resources.
[0005] Regarding the "liquid" ore represented by the waters from salt flats or geothermal springs, the salinity of these environments is very high and can reach up to a hundred g / L.
[0006] One of the current challenges is therefore to develop robust and efficient technologies for extracting lithium from these aqueous media. Solid-support extraction technology is well-suited for extracting an element present in low concentrations in a saline environment. To do this, it is necessary to select a lithium-selective material or sorbent and to shape this material so that it can be used in a fixed-bed process capable of handling high flow rates (up to several m³ / h).
[0007] For the extraction of lithium contained in geothermal brines, it is envisaged to insert a lithium extraction loop onto the geothermal loop. This process must necessarily avoid the physico-chemical alteration of the flow (i.e., limiting the inputs and outputs) in order not to significantly modify the composition of the brine before its reinjection. Today, several projects exist for the recovery of lithium from geothermal brines, but none at an industrial scale to date (pre-industrial scale for Eramet). Regarding suitable solid-support extraction processes, lithium extraction from brines can be carried out using columns packed with cation-exchange microfibers, with pilot-scale trials underway. In patent application FR3087356 Al [1], Geolith uses fibers from the company Ajelis (MECALICAPT®), which are organic materials functionalized with cation-exchange organic groups. The use of organic fibers presents drawbacks when used at high temperatures, notably a risk of degradation of the organic component.
[0008] Eramet uses solid mineral materials such as lithium-loaded aluminum trioxide as precursor materials for selective lithium extraction, with a preliminary proton exchange step, in the context of salt flat mining (Argentina), and plans to use these materials for geothermal sources, and even for juices from battery recycling. While the sorption properties of these materials are effective in powder form, one of the difficulties lies in shaping them for a continuous fixed-bed process.
[0009] French patent application FR3051787 Al [2] proposes a process for preparing a solid crystalline mineral material that selectively extracts lithium in extruded form, with good mechanical strength and cohesion for column use, without the presence of fine particles. The manufacturing process uses a suspension which, after heat treatment, is extruded and then dried, resulting in a material with the formula (LiCl)x.Al(OH)3,nH2O, where n is between 0.01 and 10 and x is between 0.4 and 1. However, this process does not produce a porous material that optimizes the accessibility of the adsorbent sites to the flow through the bed, and consequently, the interior of the grains cannot be accessed, thereby reducing the extraction capacity and kinetics and thus degrading performance in fixed-bed processes.
[0010] French patent application FR3015458 Al [3] has the same objective of shaping a material suitable for a column process and describes the use of an alumina-type binder followed by extrusion and a drying phase with a synthesis process similar to that described in French patent application FR3051787 Al [2]. In this case as well, the porosity of the material is limited, meaning that only the outer part of the extrudates is used when in contact with the column flow, which can reduce the material's performance. Finally, in both of these patent applications, the shape obtained is difficult to control during the drying step, and shaping is limited to the formation of extrudates.
[0011] Geopolymer-based materials have also been proposed for the separation of metal ions or metalloids such as metal or metalloid cations, from a liquid medium containing them.
[0012] Thus, international application WO 2016 / 173950 A1 describes the functionalization of monolithic geopolymer foam for the catalysis or decontamination of effluents in fixed-bed treatment processes [4]. The synthesis is carried out in two steps: the foam is first prepared, and then its functionalization takes place in a second step. This complicates the overall synthesis of the material, which can make its scaling up to industrial production difficult. Furthermore, with such a synthesis, the amount of adsorbent that can be introduced into the material is limited. Indeed, the selective adsorbents are only present on the surface of the foam's macropores and not within its mesoporous walls, which can limit the contact surface with the effluent and therefore the overall capacity of the material.Furthermore, the functionalization method described in this application [4] only applies to CN-bonded metal-coordinate polymer nanoparticles, which are not suitable for lithium extraction. Moreover, this synthesis route aims to utilize the foams in their monolithic form, specifically directly as a "straight" decontamination column.
[0013] International application WO 2021 / 152248 A1 finally describes the synthesis of a selective adsorbent-geopolymer composite comprising an interconnected macroporous network [5]. To create the macroporous network, the synthesis involves the formulation of an emulsion containing precursors of the material and the removal of the oily phase once the material has hardened. The synthesis process remains complex, making it difficult to industrialize. Furthermore, this synthesis route leads to the formation of macropores with walls that are sometimes thin and have sharp junctions. These walls thus exhibit weakened mechanical strength, particularly during the passage of an effluent, which can lead to their degradation and the formation of fine particles capable of clogging a column.
[0014] Given the increasing demand for lithium, the inventors aimed to develop a lithium-selective mineral adsorbent suitable for use in a fixed bed, exhibiting good properties in terms of capacity, flow rate (kinetics), and optimized accessibility to the sorbent sites. Furthermore, this material must be prepared using an efficient, simple, and easily industrialized process. Description of the invention
[0015] The present invention makes it possible to achieve the goal set by the inventors, since they propose to prepare a geopolymer matrix material in which this matrix serves as a lithium extractor in order to have a high capacity but can also serve as a mesoporous binder to incorporate a more selective lithium adsorbent.
[0016] Indeed, when synthesized in the presence of lithium, the structure of the geopolymer matrix material is adapted to be partially selective for lithium and allows for a high lithium extraction capacity. Furthermore, the possible addition of an ion exchanger, i.e., a lithium-selective adsorbent, within this geopolymer matrix material provides increased selectivity for lithium under the specific effluent conditions to be treated, particularly highly saline effluents. The mesoporous structure of the geopolymer matrix allows accessibility to the adsorbent particles dispersed within it, resulting in extremely rapid sorption kinetics and optimized performance. Moreover, the mechanical strength of the geopolymer matrix is suitable for use in a fixed bed.The size of the ion exchangers, their dispersion in the geopolymer matrix, and the mesoporosity of the latter therefore make it possible to significantly improve the kinetic properties of ion exchange and thus the shape of the breakthrough curves.
[0017] Finally, it should be noted that the process for preparing the geopolymer matrix material according to the invention is a conventional sol-gel process, easy to implement and industrialize. Furthermore, the geopolymer matrix material according to the invention can be easily shaped in various ways such as 3D printing, foaming, extrusion, and grinding with sieving to make it suitable for a column process.
[0018] Thus, the present invention relates to a process for preparing a material suitable for extracting lithium, comprising the steps of:
[0019] a) prepare a geopolymer mixture by mixing together (i) an activation solution comprising at least lithium hydroxide and (ii) an alumino-silicate source;
[0020] b) allow said geopolymer mixture prepared in step a) to harden, thereby obtaining a geopolymer matrix material;
[0021] c) washing the geopolymer matrix material obtained in step b) by which at least part of the lithium (Li+) cations comprising the geopolymer matrix material are removed and a material suitable for extracting lithium is obtained.
[0022] In the context of the present invention, the term "geopolymer matrix" or "geopolymer" refers to a solid, inorganic, and porous material in its dry state, obtained by hardening a mixture containing finely ground materials (i.e., the alumino-silicate source) and a saline solution (i.e., the activation solution). This mixture is capable of setting and hardening over time. This mixture may be referred to as a "geopolymer mixture," "geopolymer blend," "geopolymer composition," or "geopolymer composition." The hardening of the geopolymer results from the dissolution / polycondensation of the finely ground materials of the geopolymer mixture in saline solution such as a high pH saline solution (i.e. the activation solution).
[0023] More specifically, a geopolymer or geopolymer matrix is an amorphous inorganic alumino-silicate polymer. This polymer is obtained from a reactive material containing essentially silica and aluminum (i.e., the alumino-silicate source), activated by a strongly alkaline solution, with a low solid / solution mass ratio in the formulation. The structure of a geopolymer consists of a Si-O-Al network formed of silicate (SiO4) and aluminate (AlO4) tetrahedra linked at their vertices by sharing oxygen atoms. The substitution of a silicon atom (valence +IV) by an aluminum atom (valence +III) results in a charge deficit compensated by one or more charge-compensating cations, also called compensating cations, which offset the negative charge of the AlO4 complex. Compensating cations are generally alkali metal cations and typically Na+ and K+ cations.
[0024] The high pH saline solution, also known in the field of geopolymerization as "activation solution", is a strongly alkaline aqueous solution that may optionally contain silicate components, in particular selected from the group consisting of silica, colloidal silica and vitreous silica.
[0025] The expressions "activation solution", "high pH saline solution" and "strongly alkaline solution" are, in the present invention, similar and can be used interchangeably.
[0026] The activation solution implemented within the framework of the invention is an aqueous solution, meaning that the solvent it contains is water. For the purposes of this invention, "water" means tap water, deionized water (or demineralized water), distilled water, ultrapure water (18.2 MQ), or a mixture thereof.
[0027] By "strongly alkaline" or "high pH" is meant a solution whose pH is greater than 9, in particular greater than 10, in particular greater than 11 and, more particularly, greater than 12. In other words, the activation solution has an OH concentration greater than 0.01 M, in particular greater than 0.1 M, in particular greater than 1 M and, more particularly, between 5 and 20 M.
[0028] In addition, the activation solution includes the compensating cation or the mixture of compensating cations in the form of an ionic solution or a salt.
[0029] In the context of the present invention, since the activation solution used contains lithium hydroxide (LiOH), all or part of the compensating cations are lithium cations (Li+). Typically, the amount of LiOH in the activation solution is between 3% and 6% by mass, in particular between 4% and 5% by mass, and especially on the order of 4.6% (i.e., 4.6% ± 0.1%) by mass relative to the total mass of the activation solution.
[0030] Furthermore, the activation solution implemented within the framework of the invention may also contain one or more elements selected from the group consisting of sodium silicate (Na2SiO3), potassium silicate (K2SiO2), sodium hydroxide (NaOH), potassium hydroxide (KOH), calcium hydroxide (Ca(OH)2), cesium hydroxide (CsOH), sodium oxide (Na2O), lithium oxide (Li2O), and mixtures thereof. In a particular embodiment, the activation solution implemented within the framework of the invention contains sodium oxide (Na2O) and lithium oxide (Li2O). In a further specific embodiment, the activation solution is an aqueous solution containing silica (SiO2), sodium oxide (Na2O), lithium oxide (Li2O), and lithium hydroxide (LiOH). The experimental section below provides an example of an activation solution belonging to such an embodiment.
[0031] The expressions "alumino-silicate source" and "reactive material containing essentially silica and aluminum" are, in the present invention, similar and can be used interchangeably.
[0032] The reactive material containing essentially silica and aluminum, usable for preparing the geopolymer matrix implemented within the framework of the invention, is advantageously a solid source containing amorphous aluminosilicates. These amorphous aluminosilicates are notably selected from natural aluminosilicate minerals such as illite, stilbite, kaolinite, pyrophyllite, andalusite, bentonite, kyanite, milanite, grovenite, amesite, cordierite, feldspar, allophane, etc.; calcined natural aluminosilicate minerals such as metakaolin; synthetic glasses based on pure aluminosilicates; aluminous cement; pumice; calcined by-products or residues from industrial operations such as fly ash and blast furnace slag obtained respectively from the combustion of coal and during the transformation of iron ore into pig iron in a blast furnace; and mixtures thereof.In one particular embodiment, the alumino-silicate source used is metakaolin.
[0033] Taking into account any silicate components that the activation solution may contain, the quantity of alumino-silicate source(s) is such that the SiO2 / Al2O3 molar ratio in the geopolymer matrix of the material obtained in step b), and therefore of the lithium-trapping material prepared according to the process of the invention, is between 2.3 and 4.3, in particular between 3.0 and 3.6, and especially on the order of 3.3 (i.e., 3.3 ± 0.1). This molar ratio can be obtained by dissolving the geopolymer matrix material in hydrofluoric acid.
[0034] With such a SiO2 / Al2O3 molar ratio, it is possible to have a quantity of charge-compensating cations (Li+) allowing an intrinsic capacity of Optimal lithium trapping for the material prepared according to the process of the invention.
[0035] Furthermore, the amount of water in the activation solution is between 65% and 80% by mass, in particular between 70% and 75% by mass, and specifically, on the order of 72% (i.e., 72% ± 1%) by mass relative to the total mass of the activation solution.
[0036] It should be noted that the combination of such an amount of water and the SiO2 / Al2O3 molar ratio as previously defined makes it possible to obtain a geopolymer matrix material with an optimal mesopore size for lithium trapping.
[0037] As a reminder, a geopolymer or geopolymer matrix has an intrinsic mesoporous porosity of approximately 5 to 30% by volume relative to the total volume of the geopolymer. The latter may also exhibit unconnected macropores, this porosity resulting primarily from the geopolymerization process. In other words, a geopolymer, due to its preparation process, exhibits connected mesopores and possibly unconnected macropores.
[0038] By "mesopores", we mean pores or voids having an average diameter of between 2 and 50 nm and in particular between 2 and 20 nm. In the context of the present invention, the optimal mesopore size for lithium trapping is typically between 2 and 10 nm and in particular centered around 5 nm.
[0039] Step a) of the process according to the invention is a conventional step in the preparation of geopolymers. Typically, it comprises the following substeps:
[0040] i) prepare an activation solution comprising at least lithium hydroxide as previously defined,
[0041] ii) add to the solution obtained in substep i) at least one alumino-silicate source and mix the whole, thereby obtaining a geopolymer mixture comprising at least lithium hydroxide.
[0042] In substep ii), the alumino-silicate source(s) is / are added to the activation solution comprising at least lithium hydroxide, either all at once or in several additions. Once the alumino-silicate source(s) has / are added to the activation solution, the resulting solution or dispersion is mixed using a mixer, a magnetic stirrer, a magnetic stir bar, an ultrasonic bath, or a homogenizer. The mixing / kneading in substep ii) of the process according to the invention is carried out manually or mechanically at a sustained speed. For the purposes of this invention, "sustained speed" means a rotational speed of the mixer or magnetic stirrer rotor greater than or equal to 1000 rpm, in particular greater than or equal to 1500 rpm, and, in particular, greater than or equal to 2000 rpm. Advantageously, this agitation is achieved using a magnetic stirrer or a mixer.Any mixer known to a person skilled in the art can be used within the scope of the present invention. By way of non-limiting examples, one may mention a NAUTA® mixer, a HOBART® mixer, a HENSCHEL® mixer and a . HEIDOLPH® mixer.
[0043] The experimental section below gives, by way of illustration, an example of the preparation of such a geopolymer mixture.
[0044] Typically, step a) of the process and in particular substeps i) and ii) which it comprises are carried out at a temperature between 10°C and 40°C, advantageously between 15°C and 30°C and, more particularly, at room temperature (i.e. 23°C ± 5°C) for a period of more than 1 min, in particular between 2 min and 15 min and, in particular, between 3 min and 5 min.
[0045] Step b) of the process according to the invention consists of subjecting the geopolymer mixture obtained in step a) to conditions enabling its hardening.
[0046] Any technique known to a person skilled in the art for hardening a geopolymer mixture can be used during the hardening step of the process.
[0047] The conditions enabling hardening in step b) of the process according to the invention advantageously include a curing step optionally followed by a drying step. The curing step can be carried out at a temperature between 10°C and 80°C, in particular between 20°C and 60°C and, in particular, between 30°C and 40°C, and can last between 1 and 40 days, or even longer. Alternatively, the conditions enabling hardening in step b) can include a curing step at a temperature below 30°C and, in particular, at room temperature, and can last between 18 hours and 150 days, in particular between 24 hours and 120 days, and, in particular, on the order of 3 months (i.e., 3 months ± 5 days).Regardless of the temperature at which the curing stage is carried out, it can be done in open air, underwater, in various airtight molds, by humidifying the atmosphere surrounding the geopolymer mixture, or by applying a waterproof coating to said geopolymer mixture.
[0048] Step c) of the process according to the invention is implemented to eliminate at least some of the compensating cations and in particular at least some of the lithium (Li+) cations included in the geopolymer matrix material.
[0049] In a first embodiment, step c) may consist of bringing the geopolymer matrix material into contact with a washing solution and agitating the mixture for a period of between 10 seconds and 5 minutes, in particular between 20 seconds and 3 minutes, and especially for approximately 30 seconds (i.e., 30 seconds ± 5 seconds). After removing the washing solution containing compensating cations, the step of contacting the material with a new washing solution and agitating it can be repeated at least once, twice, five, ten, or even fifteen times. The washing solution may have the same or different composition for two consecutive washes. In this first embodiment, the concentration of Li+ in the washing solution recovered after the Contact with the geopolymer matrix material and agitation allows assessment of the washing progress and the need to repeat the contact with a new washing solution. In a second implementation, step c) may consist of placing the geopolymer matrix material in a column and circulating a washing solution through this column. This circulation is typically continuous. By monitoring the Li+ concentration at the column outlet, the washing progress can be assessed.
[0050] Typically, the washing solution usable for both the first and second embodiments as defined above can be a neutral or acidic aqueous solution, optionally concentrated in sodium. An acidic aqueous solution usable within the scope of the invention is an aqueous solution having a pH between 4 and 6. A concentrated sodium aqueous solution usable within the scope of the invention comprises a concentration of [Na+] greater than or equal to 0.01 M. In a particular embodiment, the washing solution is water as previously defined, and in particular deionized water.
[0051] Advantageously, following this washing step and before any use of the material suitable for extracting the lithium thus obtained, the latter is subjected to drying. This drying can be carried out at a temperature between 40°C and 90°C, in particular between 50°C and 85°C and, in particular, between 60°C and 80°C, and can last between 4 hours and 5 days, in particular between 8 hours and 2 days and, in particular, between 10 hours and 15 hours.
[0052] As previously mentioned, the geopolymer matrix material prepared according to the process of the invention can easily be shaped. This shaping can take place before and / or after obtaining this geopolymer matrix material, i.e., before and / or after step b) of the process according to the invention.
[0053] In a first embodiment, the geopolymer matrix material prepared according to the process of the invention is in the form of a macroporous monolith with interconnected macropores. In other words, the shaping used in this first embodiment aims to obtain a monolithic geopolymer matrix material in which the geopolymer matrix is mesoporous and macroporous, with interconnected macropores. By "macropores," we mean pores or voids having an average diameter greater than 50 nm and, in particular, greater than 70 nm. The mesopores in the geopolymer matrix of the material obtained following this first embodiment are as previously defined.
[0054] A person skilled in the art is aware of various techniques for obtaining a geopolymer matrix material in the form of a macroporous monolith with interconnected macropores. Illustrative and non-limiting examples of such techniques include additive manufacturing such as extrusion or 3D printing, foaming, and the use of sacrificial templates (emulsion, beads, etc.). polymers, fibers, molds, etc.).
[0055] In a second embodiment, the geopolymer matrix material prepared according to the process of the invention is in the form of objects with a size ranging from 100 µm to 10 mm. Such objects are usable in packed columns and may be in particular in the form of powders, beads or extrudates.
[0056] A person skilled in the art is aware of various techniques for obtaining a geopolymer matrix material in the form of objects ranging in size from 100 µm to 10 mm. By way of illustrative and non-limiting examples, one may mention grinding possibly combined with sieving, extrusion, granulation or compounding.
[0057] In a particular embodiment of this second embodiment, the geopolymer matrix material is in the form of a micron-sized powder, ideal for a column processing method. In other words, the material obtained by this embodiment is in the form of grains whose size is typically between 100 µm and 700 µm and, in particular, between 200 µm and 500 µm.
[0058] In this embodiment, the geopolymer matrix material obtained following step b) of the process according to the invention is subjected to grinding followed by sieving. Similarly, step c) of washing, performed on the geopolymer matrix material in the form of a micron-sized powder, allows, in addition to the removal of at least some of the compensating cations, the removal of particles resulting from the grinding and adhering to the grains of geopolymer matrix material.
[0059] As previously mentioned, the lithium-extracting material prepared according to the process of the invention can be used pure or can incorporate a lithium-selective adsorbent. Indeed, the lithium-extracting material can be the geopolymer itself, the formulation of which intrinsically confers upon it a property of selective lithium extraction. This geopolymer can also be used as a mesoporous and possibly macroporous binder that can incorporate one or more lithium-selective adsorbents. The lithium-extracting material is then in the form of a composite comprising a geopolymer matrix in which the lithium-selective adsorbent(s) are dispersed, coated, and / or incorporated.Typically, in this composite material, lithium-selective adsorbents are present on the surface, particularly on the surface of pores and voids such as mesopores and possibly macropores in the mesoporous geopolymer matrix. The integration of selective adsorbents thus significantly increases the selectivity of the entire composite. Indeed, the composite then possesses several selective sorption sites: one on the geopolymer matrix (or phase) and another, highly selective one, at the level of the lithium-selective adsorbents.
[0060] To prepare such a composite material capable of extracting lithium, the geopolymer mixture prepared in step a) further comprises at least one selective lithium extractor. This selective lithium extractor(s) may be added to the activation solution comprising at least lithium hydroxide, mixed with the aluminosilicate source, and / or added to the fresh geopolymer mixture.
[0061] In the context of the present invention, the expressions "selective lithium extractor" and "selective lithium ion exchanger" are equivalent and may be used interchangeably.
[0062] The selective lithium extractant(s) used in the present invention must be compatible with the composition of a geopolymer. In other words, they must be stable in a strongly basic environment.
[0063] Advantageously, the selective lithium extractant(s) implemented within the framework of the invention can be chosen from the group consisting of a double-lamellar lithium-aluminium hydroxide (LiX-2Al(OH)3) with X representing a hydroxide or a chloride, manganese oxide, titanium oxide, tin oxide, tin antimoniate, antimony oxide, tantalum oxide, niobium oxide, iron phosphate and zirconium phosphate.
[0064] Furthermore, the size and shape of this / these selective lithium extractant(s) must be chosen such that its / their incorporation within the geopolymer matrix does not impact the extraction kinetics of the latter, i.e., it does not influence the formation of mesopores in the matrix, does not block access to the center of the matrix, particularly when the latter is in granular form, and is easily dispersible. To satisfy these various conditions, at least one selective lithium extractant is typically in the form of a powder with an advantageously spherical and submicron morphology. In particular, the grain size of the selective lithium extractant used in the invention is between 2 nm and 50 pm, particularly between 10 nm and 10 pm, and especially between 20 nm and 1 pm.
[0065] The present invention also relates to a material suitable for extracting lithium prepared by a process as previously defined.
[0066] In a first embodiment, the material suitable for extracting lithium prepared by a process as defined above is a geopolymer in which the lithium content is at least 2% by mass relative to the total mass of said geopolymer. This embodiment corresponds to the case where no additional selective lithium extractor is used.
[0067] In a second embodiment, the material suitable for extracting lithium prepared by a process as defined above is a composite material comprising at least one selective lithium extractor in a geopolymer matrix in which the lithium content is at least 2% by mass relative to the total mass of said geopolymer matrix.
[0068] As previously explained, the lithium-extracting material according to the invention is synthesized in the presence of lithium supplied primarily in the form of lithium hydroxide (LiOH) in the activation solution. Lithium in the form of the Li+ cation acts as a compensating cation, possibly with one or more other types of compensating cations, particularly Na+ and K+ cations, in the material during its synthesis. Even if the material is washed to remove at least some of the compensating cations, especially the Li+ cations, lithium remains in its structure, a signature of this synthesis in the presence of lithium. For this reason, the geopolymer and the geopolymer matrix according to the invention can be defined respectively as the "lithium geopolymer" and the "lithium geopolymer matrix."
[0069] The lithium content in the lithium-extracting material according to the invention is in particular between 2% and 6% by mass, in particular between 2.5% and 5.5% by mass, more particularly between 3% and 5% by mass, and, most particularly, on the order of 4% by mass (4% ± 0.5% by mass) relative to the total mass of said geopolymer matrix. The lithium content of the material according to the invention is understood to be after the washing step, i.e., step c) as defined above, and before any contact with a liquid likely to contain lithium. This lithium content can be obtained after analysis by inductively coupled plasma atomic emission spectrometry (ICP-AES) or inductively coupled plasma mass spectrometry (ICP-MS) of the material according to the invention dissolved in an acid such as hydrofluoric acid.
[0070] In the material according to the invention, the size of the mesopores of the geopolymer or geopolymer matrix is between 2 nm and 50 nm and is centered around 5 nm. The porosity of the material according to the invention can be measured by nitrogen adsorption-desorption or by mercury intrusion.
[0071] As previously mentioned, the material can be easily shaped in various ways as described above to be adapted to a column process. Thus, the material according to the invention can be in the form of a powder, and in particular a powder with a particle size between 100 µm and 700 µm and, in particular, 200 µm and 500 µm, an extrudate, a geopolymer foam, or even a macroporous monolith.
[0072] It is evident that the powder, beads, extrudates, geopolymer foam and macroporous monolith according to the present invention may or may not comprise at least one selective lithium extractant as previously defined.
[0073] In the experimental part below, the material according to the invention does not include No selective lithium extractant is capable of adsorbing at least 4 mg of lithium per gram of dry material, and in particular between 4 mg and 8.4 mg of lithium per gram of dry material. Furthermore, the present invention relates to the use of a material as previously defined for extracting lithium from a solution containing it.
[0074] In other words, the present invention relates to a method for extracting lithium from a solution containing it, consisting of contacting a material such as previously described or a material prepared by a preparation process as previously defined with a solution containing lithium. At the end of this contacting step, a lithium-charged material is obtained.
[0075] The solution containing lithium, typically in the form of a lithium salt from which lithium is to be extracted, is a natural saline solution, concentrated or obtained from a lithium extraction or processing method. More particularly, said solution is advantageously a saline solution selected from the group consisting of brines from salt lakes or geothermal springs, brines from salt lakes or geothermal springs concentrated in lithium following evaporation, seawater, effluents from cathode production plants, effluents from lithium chloride or lithium hydroxide production plants, effluents from lithium extraction processes from minerals or a mixture thereof.Depending on its nature, the solution used in the invention may also contain one or more species selected from sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), fluorine (F), chlorine (Cl), bromine (Br), iodine (I), sulfates (SO4), carbonates (CO3), nitrates (NO3), and bicarbonates (HCO3). Typically, the amount of lithium in the solution used in the extraction process according to the invention is between 0.005 M and 0.5 M, and in particular between 0.05 M and 0.3 M.
[0076] In the extraction process according to the invention, the material as previously defined is placed in a column, and contact between the lithium-containing solution and the material is achieved by passing the solution over the material in the column. In this case, the extraction process according to the invention is a column process.
[0077] Alternatively, the extraction process according to the invention can be a batch process, i.e. a process involving contact between the material as previously defined and the lithium-containing solution and agitation of the whole.
[0078] The extraction process according to the invention may, in addition, include a preliminary step of preparing the material according to the preparation process as previously defined and / or a subsequent step of recovering lithium from the lithium-loaded material obtained.
[0079] This final recovery step corresponds to a lithium desorption step carried out by contacting the lithium-loaded material with an aqueous solution to obtain an eluate containing at least lithium, which can then be concentrated by evaporation. The contact, possibly carried out under stirring, lasts between 30 seconds and 15 minutes, specifically between 1 and 10 minutes, and, for example, 2 minutes. Furthermore, this recovery step can be repeated at least once, twice, three times, five times, ten times, fifteen times, or even twenty times. Typically, the aqueous solution used for lithium desorption can be a neutral or acidic aqueous solution, possibly concentrated in alkali ions, particularly Na+ ions. Everything previously described for the washing solution used in step c) applies mutatis mutandis to the aqueous solution used for lithium desorption. By "concentrated in alkali ions," we mean a solution in which the concentration of alkali ions is greater than or equal to 0.01 M.In one particular embodiment, the aqueous solution used for lithium desorption is ultrapure water.
[0080] Other features and advantages of the present invention will become apparent to those skilled in the art upon reading the examples given below, which are given by way of illustration and not limitation, with reference to the accompanying figures. Brief description of the drawings
[0081] [Fig-1] is a photograph of the monolith formed after setting the geopolymer (part (a)) as well as grains obtained at the end of synthesis and which can be used in fixed bed lithium extraction processes (part (b)).
[0082] [Fig.2] shows the diffractogram of the lithium geopolymer synthesized in Example 1.
[0083] [Fig.3] shows the nitrogen adsorption / desorption isotherm carried out on the geo lithium polymer synthesized in example 1.
[0084] [Fig.4] shows the mesopore size distribution of the lithium geopolymer summarized in example 1.
[0085] [Fig.5] shows the lithium concentration in successive batches of the injection contact depending on the total volume of water used.
[0086] DETAILED DESCRIPTION OF PARTICULAR EMBODIMENTS
[0087] Example 1: Synthesis of lithium geopolymer grains
[0088] 7.536 g of a commercial Betolin Li24 solution (Wöllner, composed of 23% by mass SiO2, 3% by mass Na2O, 5% by mass Li2O and 69.2% by mass H2O) is mixed with 2.0 g of ultrapure water and 0.46 g of LiOH. The solution is then homogenized manually.
[0089] In a second step, 5.332 g of clay powder (Metakaolin Metamax from BASF) are finally added and the whole is once again homogenized manually.
[0090] After 3 months of rest at room temperature, a monolithic material is obtained (part (a) of [Fig. 1]). This material is then ground and the resulting grains are sieved to obtain grains with a size distribution between 300 and 500 µm (part (b) of [Fig. 1]), which is the particle size best suited for use in column processing.
[0091] Finally, a washing step is carried out (see example 4).
[0092] This step is necessary to eliminate the presence of fine particles adhering to the grains after grinding (which could clog the column) and to remove some of the cations (Na+ and especially Li+) present in the material. To do this, 3 g of material are stirred manually for 30 seconds in the presence of 100 mL of demineralized water. This step is repeated 15 times, changing the water between each test.
[0093] The materials are finally dried at 80°C overnight.
[0094] Example 2: Characterization of the lithium geopolymer
[0095] The chemical composition of the lithium geopolymer of Example 1 was analyzed after dissolving it in hydrofluoric acid. This composition is as follows: 3.3 SiO2 : 1 Al2O3 : 1 Li2O : 17.5 H2O.
[0096] The lithium content of this material is on the order of 4% by mass.
[0097] The material synthesized in Example 1 was characterized by ray diffraction X. The diffractogram is shown [Fig.2].
[0098] The diffractogram is characteristic of an amorphous geopolymer with a broad hump between 20 and 30°. The observed peaks correspond to the presence of residual TiO2 initially present in trace amounts in the metakaolin used as a precursor of the material.
[0099] The material synthesized in Example 1 was characterized by nitrogen adsorption / desorption to evaluate its porous structure. The isotherm obtained is shown in [Fig. 3].
[0100] This material exhibits an isotherm characteristic of a mesoporous material. It has a total pore volume of approximately 0.1 cm3.g 1 and a specific surface area of 81 m 2.gA As observed in [Fig.4], it has a pore size distribution between 2 and 10 nm, centered around 5 nm.
[0101] This pore size distribution and specific surface area are sufficient to improve the accessibility of lithium adsorption sites, particularly those located inside the grain, and to allow rapid sorption kinetics.
[0102] Example 3: Extraction of Lithium from an aqueous solution by the lithium geopolymer
[0103] The material from Example 1 was contacted with a lithium-containing solution to evaluate its lithium extraction capacity. For this purpose, between 20 and 50 mg of the material from Example 1 were contacted with 10 mL of a solution containing 200 mg / L of Li (as chloride), 11 g / L of Na (as chloride) and 1.3 g / L of magnesium (as chloride). Under these highly saline conditions, the material from Example 1 captures between 0.58 and 1.22 mmol (i.e., between 4 and 8.4 mg) of lithium per gram of material.
[0104] Example 4: Extraction of Lithium present in the lithium geopolymer
[0105] This example shows the feasibility of extracting the lithium present in the material of example 1 by means of a step of contacting it with an aqueous solution.
[0106] For this example, 3 g of the material from Example 1 in the form of grains ground to 300-500 pm are brought into contact with 30 mL of ultrapure water solution for 2 min under stirring and then the solid is allowed to settle.
[0107] After recovery of the solution, the lithium concentration in it is analyzed. This step is performed 20 times. Figure 5 shows the evolution of the Li concentration measured in each of the successive batches as a function of the cumulative volume of water used for contact (30 mL multiplied by the number of batches).
[0108] Thus, it is observed that lithium can be extracted from the geopolymer by contacting it with an aqueous solution. After a first contact step, approximately 20% of the mass of Li present in the material is recovered. This percentage increases to 40% after 20 successive contact steps.
[0109] In this way, the lithium captured during the extraction step (described in Example 3) by a geopolymer material as described in Example 1 can be re-extracted through steps of contact with an aqueous solution. References
[0110] [1] Patent application FR3087356 Al [YES] [2] Patent application FR3051787 Al
[0112] [3] Patent application FR3015458 Al
[0113] [4] International Application WO 2016 / 173950 Al
[0114] [5] International Application WO 2021 / 152248 Al
Claims
Claims
1. A method for preparing a material capable of extracting lithium, comprising the steps of: a) preparing a geopolymeric mixture by mixing together (i) an activation solution comprising at least lithium hydroxide and (ii) an aluminosilicate source; b) allowing said geopolymeric mixture prepared in step a) to harden, whereby a geopolymeric matrix material is obtained; c) washing the geopolymeric matrix material obtained in step b) whereby at least a portion of the lithium cations (Li+) comprised in the geopolymeric matrix material are removed and a material capable of extracting lithium is obtained.
2. Preparation process according to claim 1, characterized in that the quantity of LiOH in said activation solution is between 3% and 6% by mass, in particular between 4% and 5% by mass and, in particular, of the order of 4.6% (i.e. 4.6% ±0.1%) by mass relative to the total mass of said activation solution.
3. Preparation process according to claim 1 or 2, characterized in that the SiO2 / Al2O3 molar ratio in the geopolymer matrix of the material obtained in said step b) is between 2.3 and 4.3, in particular between 3.0 and 3.6 and, in particular, of the order of 3.3 (i.e. 3.3 ± 0.1).
4. Preparation process according to any one of claims 1 to 3, characterized in that the quantity of water in said activation solution is between 65% and 80% by mass, in particular between 70% and 75% by mass and, in particular, of the order of 72% (i.e. 72% ± 1%) by mass relative to the total mass of the activation solution.
5. Preparation process according to any one of claims 1 to 4, characterized in that the geopolymeric mixture prepared in said step a) further comprises at least one selective lithium extractant.
6. Preparation process according to claim 5, characterized in that said at least one selective lithium extractant is chosen from the group consisting of a lamellar double hydroxide of lithium-aluminium (LiX-2Al(OH)3) with X representing a hydroxide or a chloride, manganese oxide, titanium oxide, tin oxide, tin antimonate, antimony oxide, tantalum oxide, niobium oxide, iron phosphate and zirconium phosphate.
7. Material capable of extracting lithium prepared by a process as defined
8.
9.
10.
11.
12.
13.
14.
15. to any one of claims 1 to 4, said material being a geopolymer in which the lithium content is at least 2% by mass relative to the total mass of said geopolymer. Material capable of extracting lithium prepared by a process as defined in claim 5 or 6, said material being a composite material comprising at least one selective lithium extractant in a geopolymer matrix in which the lithium content is at least 2% by mass relative to the total mass of said geopolymer matrix. Material according to claim 7 or 8, characterized in that the size of the mesopores of said geopolymer or of said geopolymeric matrix is between 2 nm and 50 nm. Material according to any one of claims 7 to 9, characterized in that said material is in the form of a macroporous monolith with connected macropores. Material according to any one of claims 7 to 9, characterized in that said material is in the form of objects whose size is between 100 μm and 10 mm. Use of a material according to any one of claims 7 to 11 for extracting lithium from a solution containing it. A method of extracting lithium from a solution containing it, comprising contacting a material according to any one of claims 7 to 11 with a solution containing lithium. Extraction method according to claim 13, characterized in that said method is a column method or a batch method. Method according to claim 13 or 14, characterized in that the solution is a saline solution chosen from the group consisting of brines from salt lakes or geothermal sources, brines from salt lakes or geothermal sources, concentrated in lithium following evaporation, sea water, effluents from cathode production plants, effluents from lithium chloride or hydroxide production plants, effluents from processes for extracting lithium from minerals or a mixture thereof.
Citation Information
Patent Citations
A METHOD FOR PREPARING A SHAPED ADSORBENT MATERIAL COMPRISING A SHAPING STEP IN THE PRESENCE OF A MINERAL BINDER AND A METHOD FOR EXTRACTING LITHIUM FROM SALINE SOLUTIONS USING SAID MATERIAL
FR3015458A1
process FOR PREPARING AN ADSORBENT MATERIAL AND PROCESS FOR EXTRACTING LITHIUM USING SAID MATERIAL
FR3051787A1
INSTALLATION AND METHOD FOR SEPARATION OF AT LEAST ONE IONIC SPECIES FROM A SOLUTION COMPRISING AT LEAST SAID IONIC SPECIES AND LITHIUM
FR3087356A1
Method for producing a functionalised geopolymer foam, said functionalised foam, and the uses thereof
WO2016173950A1
Process for obtaining synthetic geopolymers and synthetic geopolymers