Polymer and its preparation process

A novel multi-step polymerization process for synthesizing a water-soluble polymer addresses the challenges of high viscosity and energy inefficiencies in producing high molecular weight PVAm, enhancing paper production efficiency and reducing environmental impact.

FR3149009A1Pending Publication Date: 2024-11-29S P C M SA
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
FR2023005149
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing methods for producing high molecular weight polyvinylamine (PVAm) for paper manufacturing face challenges such as high viscosity and difficulty in industrial scale synthesis, leading to energy inefficiencies and environmental impacts due to the use of oil, which can affect paper performance.

Method used

A water-soluble polymer is synthesized through a multi-step polymerization process involving sequential addition of monomers and compounds, followed by partial or total hydrolysis of amide groups, resulting in polymers with reduced viscosity and improved properties for paper production, including enhanced drainage and dry strength.

Benefits of technology

The new polymer process reduces energy and water requirements, lowers greenhouse gas emissions, and improves paper machine speed and productivity while maintaining or exceeding the performance of conventional polymers, with lower viscosity for easier handling and reduced water usage.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a new water-soluble polymer, its preparation process and its use, particularly for applications in the field of paper.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Polymer and its preparation process Technical field of the invention

[0001] The present invention relates to a novel water-soluble polymer, its preparation process and its use, in particular for applications in the field of paper. Prior art

[0002] During the manufacture of paper, cellulose fibers as well as mineral fillers are placed in aqueous suspension before being deposited on a forming fabric so as to eliminate the water and form a mat of wet fibers which will be pressed and dried to obtain a sheet of paper.

[0003] The retention of these fibers and fillers is an important parameter for recovering a maximum of material on the forming fabric and limiting their passage through the forming fabric.

[0004] Furthermore, the drainage capacity of the fibrous mat is also a major element in papermaking processes because an increase in the drainage capacity makes it possible to increase the speed of the paper machine, and therefore to improve its productivity but also to reduce the energy requirements during the drying of the sheet of paper or cardboard. In the laboratory, gravity drainage and vacuum drainage can be distinguished, the latter offering a better simulation of the suction boxes. This parameter is all the more important as the machines are fast.

[0005] On the other hand, there is also a search for papers and cardboards that are increasingly resistant, particularly for the packaging or tissue industry. The increase in the mechanical resistance of the paper sheet, evaluated in the dry or wet state depending on the segment of the paper industry concerned, makes it possible to offer an increased quality of paper. We can speak in particular of resistance to bursting, compression, delamination, traction in the dry or wet state.

[0006] As the paper industry is constantly seeking to improve its paper, cardboard or similar manufacturing processes, particularly with regard to cost reduction, yield, productivity or even the properties of the final product, various polymers are used to treat the pulp in order to improve, for example, retention and drainage, and to create physical properties such as the dry and wet strength of the final paper product.

[0007] Polyvinylamines (PVAm) are known and widely used in these processes, in particular to improve drainage during the formation of paper sheets and their dry strength. These polymers give better application performance, but they also make it possible to increase the speed of the paper machine and thus increase productivity.

[0008] PVAms are prepared by the polymerization of N-vinylformamide followed by the hydrolysis of some or all of the formamide groups to amines. Control of the hydrolysis reaction can vary the percentage of monomers having an amine function, which makes it possible to modulate the properties provided by this polymer according to needs and applications.

[0009] US4421602 uses partially hydrolyzed homopolymers of N-vinylformamide as a drainage aid in papermaking. From 10 to 90% of the formyl groups are hydrolyzed to amine units in an acid or base during the manufacture of this homopolymer.

[0010] PVAms often require a high molecular weight in order to develop satisfactory properties for high-performance applications. Low- to medium-molecular-weight PVAms are generally prepared by solution polymerization. However, high-molecular-weight PVAms are difficult to produce by solution polymerization because the PVAms obtained under these conditions are gels that are difficult to handle. In addition, problems related to high solution viscosity and poor heat transfer make this synthesis difficult on an industrial scale.

[0011] The following documents propose a preparation by inverse emulsion, making it possible to obtain higher molecular weights than with solution polymerization while avoiding the problems linked to the increase in viscosity: US2982749, US3278506, US3284393, US3957739, US3975341, US4078133 and US4312969. However, the use of oil is not recommended during paper manufacturing because it can lead to maintenance problems, and can impact the performance of the final paper.

[0012] The Applicant has discovered, surprisingly, that the synthesis of a polymer according to the process of the invention makes it possible to obtain polymers which, at equivalent molecular weight, have a lower viscosity. Obtaining polymers with reduced viscosity allows a reduction in the energy required when pumping them at the time of their use as well as reducing the quantity of water required for their dilution. The polymers obtained according to the process of the invention have performances at least equivalent to the polymers obtained according to a conventional process, or even improved performances in terms of dry strength, while improving drainage, thus allowing an increase in the speed of the paper machine and therefore an improvement in productivity.

[0013] The use of the polymers resulting from the invention is part of a principle of environmental awareness and of the impact of industries and humans on the planet. The energy and water required for the use of these polymers are reduced, which makes it possible to reduce the quantity of greenhouse gas emissions such as CO2.

[0014]

[0015] associated with the use of these polymers. Statement of the invention The present invention relates to a water-soluble polymer comprising: - at least one monomer A obtained by partial or total hydrolysis of the amide group -N(R2)-CO-R' of a monomer of formula (AP): [Chem.l]

[0016]

[0017] CHt \gold 1 (AP) where R1 and R2 are, independently, a hydrogen atom or an alkyl chain of 1 to 6 carbons, - at least one structuring system comprising: (i) at least one compound I chosen from: allylsulfonic acid, methallylsulfonic acid, allyl disulfonic acid, methallyl disulfonic acid, their salts and their mixtures; (ii) at least one compound II of formula (II): [Chem. 2] (II)

[0018]

[0019] R3 and R4 being, independently of each other, a hydrogen atom, a methyl group, an ethyl group, an isopropyl group or a CH2-OH group; R3 and R4 not both being hydrogen (R3^H when R4=H; R^H when R3=H), - optionally at least one hydrophilic cationic monomer B distinct from monomer A - optionally at least one monomer C chosen from hydrophilic anionic monomers distinct from compound I, hydrophilic non-ionic monomers distinct from the monomer of formula (AP) and from compound II, hydrophilic zwitterionic monomers and hydrophobic monomers. This water-soluble polymer is obtained according to the following steps: a) formation of a solution (SI) comprising at least a first fraction (Fl) containing (1) at least one monomer of formula (AP) and / or at least one of the optional monomers B and C and (2) at least one compound chosen from compounds I and II; b) polymerization 1 (PO1) of the fraction Fl to form a solution of a first prepolymer (PP1); c) adding, to the solution comprising PP1, a second fraction (F2) containing (1) at least one monomer of formula (AP) and / or at least one of the optional monomers B and C and (2) at least one compound chosen from compounds I and II; d) polymerization 2 (PO2) of fraction F2 on PP1 to form a second prepolymer (PP2); e) adding, to the solution comprising PP2, a third fraction (F3) containing (1) at least one monomer of formula (AP) and / or at least one of the optional monomers B and C and (2) at least one compound chosen from compounds I and II; f) polymerization 3 (PO3) of fraction F3 on PP2 to form a solution comprising a base polymer; g) partial or total hydrolysis of the amide group -N(R2)-CO-R* of the monomer of formula (AP) of the base polymer in order to obtain the water-soluble polymer; at least one of the fractions F1, F2 or F3 contains at least one monomer of formula (AP), at least one of the fractions F1, F2 or F3 contains at least one compound I and at least one of the fractions F1, F2 or F3 contains at least one compound II.

[0020] The present invention also relates to the process for preparing this water-soluble polymer.

[0021] The present invention also relates to a method for manufacturing paper or cardboard using this water-soluble polymer.

[0022] The present invention also relates to the use of this water-soluble polymer in the recovery of hydrocarbons (oil and / or gas); in the drilling or cementing of wells (in particular hydrocarbon wells); in the stimulation of hydrocarbon wells (oil and / or gas), for example hydraulic fracturing, conformation, diversion; in the treatment of water in open, closed or semi-closed circuits; in the treatment of fermentation musts; in the treatment of sludge; in construction; in the treatment of wood; in the treatment of hydraulic composition (concrete, cement, mortar and aggregates); in the mining industry; in the formulation of cosmetic products; in the formulation of detergents; in the manufacture of textiles; in geothermal energy; in the manufacture of hygienic diapers; or in agriculture.

[0023] The invention also relates to the use of the polymer according to the invention as a flocculant, coagulant, binding agent, fixing agent, viscosity reducing agent, thickening agent, absorbent agent, friction reducing agent, drainage agent, filler retention agent, dehydrating agent, conditioning agent, stabilizing agent, fixing agent, film-forming agent, sizing agent, superplasticizing agent, clay inhibitor or dispersant. Description of the invention

[0024] By "polymer" is meant a polymer comprising at least one monomer A and optionally at least one monomer of formula (AP), a structuring system comprising at least one compound I and at least one compound II and optionally at least one monomer B or C. When the water-soluble polymer of the invention consists solely of identical monomers A and a structuring system comprising at least one compound I and at least one compound II, it is then referred to as a homopolymer.

[0025] By “hydrophilic monomer” is meant a monomer which has an octanol / water partition coefficient, Kow, less than or equal to 1, in which the partition coefficient Kow is determined at 25°C in an octanol / water mixture having a volume ratio of 1 / 1, at a pH between 6 and 8.

[0026] By "hydrophobic monomer" is meant a monomer which has an octanol / water partition coefficient, Kow, greater than 1, in which the partition coefficient Kow is determined at 25°C in an octanol / water mixture having a volume ratio of 1 / 1, at a pH between 6 and 8.

[0027] The octanol / water partition coefficient, Kow, represents the ratio of concentrations (g / L) of a monomer between the octanol phase and the aqueous phase. It is defined as follows:

[0028] [Math.l] JL'' __ J ftckvwl “ r ' i monomer 1 J water

[0029] By "water-soluble polymer" is meant a polymer which gives an aqueous solution without insoluble particles when dissolved under stirring at 25°C and with a concentration of 10 gL 1 in deionized water.

[0030] Throughout the description, the viscosities are measured with a Brookfield viscometer, at 25°C in aqueous solution.

[0031] In the present description, it is considered that a person skilled in the art is able to determine the modulus and speed of the Brookfield viscometer adapted according to the viscosity range to be measured. This type of measurement is in fact part of the general knowledge of a person skilled in the art.

[0032] By “X and / or Y” is meant “X”, or “Y”, or “X and Y”.

[0033] Also part of the invention are all possible combinations between the different embodiments disclosed, whether preferred embodiments or given by way of example. Furthermore, when ranges of values ​​are indicated, the bounds are part of these ranges. The disclosure also includes all combinations between the bounds of these value ranges. For example, the value ranges “1-20, preferably 5-15”, imply the disclosure of the ranges “1-5”, “1-15”, “5-20” and “15-20” and the values ​​1, 5, 15 and 20.

[0034] In the description, a base polymer designates the water-soluble polymer obtained according to the process of the invention before it undergoes the hydrolysis reaction according to step g). Water-soluble polymer

[0035] The present invention relates to a water-soluble polymer comprising: - at least one monomer A obtained by partial or total hydrolysis of the amide group -N(R2)-CO-R' of a monomer of formula (AP):

[0036] [Chem.l]

[0037] where R1 and R2 are, independently, a hydrogen atom or an alkyl chain of 1 to 6 carbons, - at least one structuring system comprising: (i) at least one compound I chosen from: allylsulfonic acid, methallylsulfonic acid, allyl disulfonic acid, methallyl disulfonic acid, their salts and their mixtures; (ii) at least one compound II and of formula (II):

[0038] [Chem.2] (II)

[0039] R3 and R4 being, independently of one another, a hydrogen atom, a methyl group, an ethyl group, an isopropyl group or a CH2-OH group; R3 and R4 not both being hydrogen (R3^H when R4=H; R^H when R3=H), - optionally at least one hydrophilic cationic monomer B distinct from monomer A - optionally at least one monomer C chosen from hydrophilic anionic monomers distinct from compound I, hydrophilic nonionic monomers distinct from monomer AP and compound II, hydrophilic zwitterionic monomers and hydrophobic monomers, at least one of the fractions F1, F2 or F3 contains at least one monomer of formula (AP), at least one of the fractions F1, F2 or F3 contains at least one compound I and at least one of the fractions F1, F2 or F3 contains at least one compound II. Monomeric composition Monomer A

[0040] The water-soluble polymer according to the invention is a synthetic polymer. It may further comprise one or more hydrophilic cationic monomers B.

[0041] Monomer A is advantageously a vinylamine obtained by hydrolysis of a monomer of formula (AP).

[0042] Advantageously, the monomer(s) of formula (AP) may be chosen, in particular, from N-vinylformamide, N-vinyl-N-methylformamide, N-vinylacetamide, N-vinyl-N-methylacetamide, N-vinyl-N-ethylacetamide, N-vinyl-propianamide, N-vinyl-N-methylpropianamide and N-vinylbutyramide. Preferably, it is N-vinylformamide.

[0043] The water-soluble polymer advantageously comprises between 1 and 100 mol% of cationic monomer(s) A, preferably at least 30 mol%, more preferably at least 50 mol%, even more preferably at least 70 mol%. Hydrophilic cationic monomer B

[0044] The water-soluble polymer may optionally comprise one or more hydrophilic cationic monomers B distinct from monomer A.

[0045] Advantageously, the hydrophilic cationic monomer(s) B which can be used in the context of the invention are chosen from monomers derived from vinyl type units (advantageously acrylamide, acrylic, allyl or maleic), these monomers having a phosphonium or quaternary ammonium function.Mention may be made, in particular and without limitation, of diallyldialkyl ammonium salts such as diallyl dimethyl ammonium chloride (DADMAC); acidified or quaternized salts of dialkylaminoalkylacrylamides; acidified or quaternized salts of dialkylaminoalkylmethacrylamides, such as for example methacrylamidopropyl trimethyl ammonium chloride (MAPTAC), acrylamidopropyl trimethyl ammonium chloride (APTAC), acidified or quaternized salts of dialkyl aminoalkyl acrylate such as quaternized or salified dimethylaminoethyl acrylate (ADAME), acidified or quaternized salts of dialkyl aminoalkyl methacrylate such as quaternized dimethylaminoethyl methacrylate (MADAME). or salified and mixtures thereof. Advantageously, the alkyl groups are C1-C3. Preferably, monomer B is a diallyldialkyl ammonium salt, more preferably it is diallyl dimethyl ammonium chloride.

[0046] A person skilled in the art will know how to prepare the quaternized monomers, for example using a quaternizing agent of type RX, R being an alkyl group and X being a halogen or a sulfate. The quaternizing agent may be chosen from dialkyl sulfates comprising from 1 to 6 carbon atoms or alkyl halides comprising from 1 to 6 carbon atoms. Preferably, the quaternizing agent is chosen from methyl chloride, benzyl chloride, dimethyl sulfate or diethyl sulfate. In addition, the present invention also covers monomers of type DADMAC, APTAC and MAPTAC whose counterion is a sulfate, a fluoride, a bromide or an iodide instead of the chloride.

[0047] By “quaternizing agent” we mean a molecule capable of alkylating a tertiary amine.

[0048] The water-soluble polymer advantageously comprises between 0 and 99 mol% of hydrophilic cationic monomer(s) B, preferably between 0 and 50 mol%, more preferably between 0 and 30 mol%. Monomer C

[0049] The water-soluble polymer according to the invention may optionally comprise at least one monomer C chosen from hydrophilic anionic monomers distinct from compound I, hydrophilic non-ionic monomers distinct from monomer A and compound II, hydrophilic zwitterionic monomers and hydrophobic monomers.

[0050] Hydrophilic anionic monomers distinct from compound I

[0051] Advantageously, the hydrophilic anionic monomer(s) that can be used in the context of the invention can be chosen from a broad group. The monomers can have vinyl functions (advantageously acrylic, maleic, fumaric, malonic, itaconic, or allylic) and contain a carboxylate, phosphonate, phosphate, sulfate, sulfonate group, or another group with anionic charge.Examples of suitable monomers include acrylic acid; methacrylic acid; dimethylacrylic acid; itaconic acid; crotonic acid; maleic acid; fumaric acid; acrylamido undecanoic acid; 3-acrylamido 3-methylbutanoic acid; maleic anhydride; strong acid monomers having, for example, a sulfonic acid or phosphonic acid function such as vinylsulfonic acid, vinylphosphonic acid, 2-methylidenepropane-1,3-disulfonic acid, 2-sulfoethylmethacrylate, sulfopropylmethacrylate, sulfopropylacrylate, allylphosphonic acid, styrenesulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid (ATBS), acid. 2-acrylamido-2-methylpropane disulfonic acid; water-soluble salts of these monomers such as their alkali metal, alkaline earth metal, or ammonium salts; and mixtures thereof. Preferably, it is acrylic acid and / or 2-acrylamido-2-methylpropane sulfonic acid (ATBS), more preferably it is acrylic acid.

[0052] In a particular embodiment, the hydrophilic anionic monomer(s) may be partially or totally salified.

[0053] By salified is meant the substitution of a proton of at least one acid function of the type -R(=O)-OH (with R= P, S or C) of the anionic monomer by a metal or ammonium cation to form a salt of the type -R(=O)-OX (X being a metal or ammonium cation). In other words, the non-salified form corresponds to the acid form of the monomer, for example RC(=O)-OH in the case of the carboxylic acid function, whereas the salified form of the monomer corresponds to the form RC(=O)-0 X+, X+ corresponding to an alkali or ammonium cation. The salification of the acid functions of the water-soluble polymer may be partial or total.

[0054] The salified form advantageously corresponds to the salts of alkali metals (Li, Na, K, etc.), alkaline earth metals (Ca, Mg, etc.) or ammonium (for example the ammonium ion or a tertiary ammonium), or their mixtures. The preferred salts are the sodium salts.

[0055] Salification can be done, partially or totally, before, during or after polymerization.

[0056] Advantageously between 0 and 100 mol% of the hydrophilic anionic monomer(s) are in salified form, preferably between 10 and 90 mol%.

[0057] The water-soluble polymer according to the invention advantageously comprises between 0 and 30 mol% of hydrophilic anionic monomers, preferably less than 20 mol%, more preferably less than 10 mol%.

[0058] In a preferred embodiment, the water-soluble polymer does not comprise anionic monomers other than compound I.

[0059] In a particular embodiment, when at least one hydrophilic anionic monomer is 2-acrylamido-2-methylpropane sulfonic acid, it may be at least partially in its hydrated form. The hydrated form of 2-acrylamido-2-methylpropane sulfonic acid is a particular form of 2-acrylamido-2-methylpropane sulfonic acid that can be obtained by controlled crystallization of the 2-acrylamido-2-methylpropane sulfonic acid monomer. US 10,759,746 describes how to obtain the hydrated form of 2-acrylamido-2-methylpropane sulfonic acid.

[0060] In a preferred embodiment, the water-soluble polymer does not comprise a hydrophilic anionic monomer.

[0061] Hydrophilic non-ionic monomers distinct from the monomer AP and from compound II

[0062] Advantageously, the hydrophilic non-ionic monomer(s) which can be used in the context of the invention are chosen from the group comprising water-soluble vinyl monomers, such as acrylamide, methacrylamide, N-alkylacrylamides, N-alkylmethacrylamides, alkoxylated esters of acrylic acid, alkoxylated esters of methacrylic acid, N-vinylpyrrolidone, N-methylolacrylamide, N-vinyl acetamide, N-vinyl imidazole, N-vinyl suc-cinimide, acryloyl morpholine (ACMO), acryloyl chloride, glycidyl methacrylate, glyceryl methacrylate, diacetone acrylamide, hydroxyalkyl (meth)acrylates, thioalkyl (meth)acrylate, hydroxyalkylacrylates, hydroxyalkyl methacrylates, and mixtures thereof. Among these non-ionic monomers, the alkyl groups are advantageously C1-C5, more advantageously C1-C3.These are preferably linear alkyls. Preferably, the non-ionic monomer is acrylamide.

[0063] The water-soluble polymer according to the invention advantageously comprises between 0 and 30 mol% of hydrophilic non-ionic monomers, preferably less than 20 mol%, more preferably less than 10 mol%.

[0064] In a preferred embodiment, the water-soluble polymer does not comprise non-ionic monomers other than the compound(s) II.

[0065] The water-soluble polymer can be post-hydrolyzed. Post-hydrolysis is the reaction of the polymer after polymerization. This step consists of the reaction of hydrolyzable functional groups of advantageously non-ionic monomers, more advantageously the amide or ester functions, with a hydrolysis agent. This hydrolysis agent can be an enzyme, an ion exchange resin, or an alkali metal. Preferably, the hydrolysis agent is a Brpnsted base. During this post-hydrolysis step of the water-soluble polymer, the number of carboxylic acid functions increases. Indeed, the reaction between the base and the amide or ester functions present in the water-soluble polymer produces carboxylate groups.

[0066] Hydrophilic zwitterionic monomers

[0067] Advantageously, the hydrophilic zwitterionic monomer(s) which may be used in the context of the invention are chosen, in particular, from derivatives of a vinyl-type unit (advantageously acrylamide, acrylic, allyl or maleic), this monomer having an amine or quaternary ammonium function and an acid function of carboxylic (or carboxylate), sulfonic (or sulfonate) or phosphoric (or phosphate) type. Preferably, this monomer comprises an amine or quaternary ammonium function and an acid function of carboxylic (or carboxylate), sulfonic (or sulfonate) or phosphoric (or phosphate) type. Dimethylaminoethyl acrylate derivatives, such as 2-((2-9 (acryloyloxy) ethyl) dimethyl- lammonio) ethane-l-sulfonate, may be mentioned in particular and in a non-limiting manner, 3 - ((2- (acryloyloxy) ethyl) dimethylammonio) propane-1-sulfonate, 4 - ((2- (acryloyloxy) ethyl) dimethylammonio) butane-1-sulfonate, [2-(acryloyloxy) ethyl] (dimethylammonio) acetate, derivatives of dhné-thylaminoethyl methacrylate such as 2 - ((2- (methacryloyloxy) ethyl) dimethylammonio) ethane-l-sulfonate, 3 - ((2- (methacryloyloxy) ethyl) dimethylammonio) propane-1-sulfonate, 4 - ((2 - (methacryloyloxy) ethyl) dimethylammonio) butane-1-sulfonate, [2- (methacryloyloxy) ethyl] (dimethylammonio) acetate, dimethylamino propylacrylamide derivatives such as 2 - ((3-acrylamidopropyl) dimethylammonio) ethane-1-sulfonate, 3 - ((3-acrylamidopropyl) dimethylammonio) propane-1-sulfonate, 4 - ((3-acrylamidopropyl) dimethylammonio) butane -1-sulfonate, [3- (acryloyl) oxy) propyl] (dimethylammonio) acetate, dimethylamino propyl methylacrylamide,or derivatives such as 2 -((3-methacrylamidopropyl) dimethylammonio) ethane-1-sulfonate, 3 - ((3-me dimethylammonio) propane-1-sulfonate 4 - ((3-methacrylamidopropyl) dimethylammonio) butane-1-sulfonate and propyl [3- (methacryloyloxy)] (dimethylammonio) acetate and mixtures thereof.

[0068] The water-soluble polymer according to the invention advantageously comprises between 0 and 30 mol% of hydrophilic zwitterionic monomers, preferably less than 20 mol%, more preferably less than 10 mol%.

[0069] In a preferred embodiment, the water-soluble polymer does not comprise a zwitterionic monomer.

[0070] Hydrophobic monomers

[0071] Advantageously, the monomer(s) having a hydrophobic character which can be used in the context of the invention can be chosen, in particular, from (meth)acrylic acid esters with an alkyl, arylalkyl and / or ethoxylated and / or propoxylated chain; (meth)acrylamide derivatives with an alkyl, arylalkyl or dialkyl and / or ethoxylated and / or propoxylated chain; cationic allyl derivatives having an alkyl, arylalkyl or dialkyl chain and / or an ethoxylated and / or propoxylated chain; anionic or cationic hydrophobic derivatives of (meth)acryloyl; and anionic or cationic monomeric derivatives of (meth)acrylamide carrying a hydrophobic chain. The hydrophobic monomers can comprise halogen atoms, for example chlorine.

[0072] Among these hydrophobic monomers: - the alkyl groups are preferably C3-C20, more preferably C3-C8. The C6-C20 alkyls are preferably linear alkyls while the C3-C5 alkyls are preferably branched, - the arylalkyl groups are preferably C7-C25, more preferably C7-C15, - the ethoxylated chains preferably comprise 6 to 100 -CH2-CH2-O- groups, more preferably 10 to 40, - the propoxylated chains preferably comprise 1 to 50 -CH2-CH2-CH2 -O- groups, more preferably 1 to 20.

[0073] Preferred monomers belonging to these classes are, for example: - n-hexyl (meth)acrylate, n-octyl (meth)acrylate, octyl (meth)acrylamide, lauryl (meth)acrylate, lauryl (meth)acrylamide, myristyl (meth)acrylate, myristyl (meth)acrylamide, pentadecyl (meth)acrylate, pentadecyl (meth)acrylamide, cetyl (meth)acrylate, cetyl (meth)acrylamide, oleyl (meth)acrylate, oleyl (meth)acrylamide, erucyl (meth)acrylate, erucyl (meth)acrylamide, and combinations thereof. - cationic allyl derivatives having a formula (III) or (IV):

[0074] [Chem.3] (IV)

[0075] where, R5: independently an alkyl chain containing 1 to 4 carbons; R6: an alkyl or arylalkyl chain comprising 8 to 30 carbons; X: a halide selected from the group consisting of bromides, chlorides, iodides, fluorides and any negatively charged counterion; and, preferably, hydrophobic cationic derivatives of the methacryloyl type corresponding to the formula (V):

[0076] [Chem.4] (V)

[0077] in which A: O or N-R9 (preferably A=N-R9), R7, R8, R9, Rio, Ru: independently a hydrogen or an alkyl chain containing 1 to 4 carbons, Q: an alkyl chain comprising 1 to 8 carbons, R12: an alkyl or arylalkyl chain comprising 8 to 30 carbons, X: a halide selected from the group consisting of bromides, chlorides, iodides, fluorides, and any negatively charged counterion.

[0078] The water-soluble polymer according to the invention generally comprises less than 3 mol% of hydrophobic monomers.

[0079] When the water-soluble polymer according to the invention comprises hydrophobic monomers, they are present in such an amount that the polymer remains soluble in water.

[0080] In a preferred embodiment according to the invention, the hydrophilic cationic polymer does not comprise a hydrophobic monomer.

[0081] The quantities of the different monomers will be adjusted by a person skilled in the art so as not to exceed 100 mol% during the preparation of the water-soluble polymer. Preferably, monomers A and B represent 100 mol% of the monomers of the water-soluble polymer. Structuring system

[0082] The water-soluble polymer structuring system comprises: (i) at least one compound I; (ii) at least one compound II.

[0083] This structuring system allows the production of a structured water-soluble polymer.

[0084] By “structured polymer” is meant a non-linear polymer which has side chains. This structuring comes from the presence of the compound(s) I and IL

[0085] The compound I used in the context of the invention is advantageously chosen from: allylsulfonic acid, methallylsulfonic acid, allyl disulfonic acid, methallyl disulfonic acid, their salts and their mixtures, preferably it is methallylsulfonic acid, for example sodium methallylsulfonate.

[0086] The salified form advantageously corresponds to the salts of alkali metals (Li, Na, K, etc.), alkaline earth metals (Ca, Mg, etc.) or ammonium (for example the ammonium ion or a tertiary ammonium). The preferred salts are the sodium salts.

[0087] The water-soluble polymer advantageously comprises between 500 and 50,000 ppm of compound I relative to the total weight of the monomers of formula (AP) (+ optionally monomers B and C) of the water-soluble polymer, preferably between 800 and 20,000 ppm, more preferably between 1,000 and 10,000 ppm.

[0088] Compound II used in the context of the invention is of formula (II):

[0089] [Chem.2]

[0090] R3 and R4 being, independently of one another, a hydrogen atom, a methyl group, an ethyl group, an isopropyl group or a CH2-OH group; R3 and R4 not both being hydrogen (R3^H when R4=H; R^H when R3=H).

[0091] Compound II used in the context of the invention is advantageously chosen from: N,N-dimethylacrylamide, N,N-diethylacrylamide, N,N-isopropylacrylamide, N-methylolacrylamide and mixtures thereof. Preferably, it is N,N-dimethylacrylamide.

[0092] The water-soluble polymer according to the invention advantageously comprises between 500 and 50,000 ppm of compound II relative to the total weight of the monomers of formula (AP) (+ optionally monomers B and C) of the water-soluble polymer, preferably between 1,000 and 30,000 ppm, more preferably between 2,000 and 20,000 ppm.

[0093] In the water-soluble polymer, the mass ratio between compound I and compound II is advantageously between 0.01 and 100, preferably between 0.1 and 10.

[0094] In a preferred embodiment according to the invention, the quantity of compound I is greater than the quantity of compound II. Thus, the mass ratio between compound I and compound II is advantageously greater than 1 and less than or equal to 100, preferably greater than 1 and less than or equal to 10. Optional

[0095] The water-soluble polymer may further comprise at least one crosslinking agent. This crosslinking agent may be chosen from monomers with polyethylene unsaturation (having at least two unsaturated functions), such as, for example, vinyl functions, in particular allylic, acrylic, or from monomers having at least two epoxy functions. Examples that may be mentioned are methylene bis acrylamide (MBA), triallyamine, tetraallylammonium chloride, 1,2 dihydroxyethylene bis-(N-acrylamide) and mixtures thereof. Preferably, it is methylene bis acrylamide (MBA).

[0096] The amount of crosslinking agent in the water-soluble polymer is advantageously between 5 and 5,000 ppm, relative to the total weight of the monomers of formula (AP) (+ optionally monomers B and C) of the water-soluble polymer, more preferably between 50 and 3,000 ppm.

[0097] In a particular embodiment according to the invention, the water-soluble polymer does not comprise a crosslinking agent.

[0098] The water-soluble polymer according to the invention may further comprise at least one transfer agent, for example, chosen from methanol, isopropyl alcohol, sodium hypophosphite, 2-mercaptoethanol and their mixture. We may also cite transfer agents of the xanthate, dithiocarbonate, dithiocarbamate and trithiocarbonate type and their mixtures, preferably it is sodium hypophosphite.

[0099] The amount of transfer agent in the water-soluble polymer is advantageously between 10 and 10,000 ppm, relative to the total weight of the monomers of formula (AP) (+ optionally monomers B and C) of the water-soluble polymer, more preferably between 50 and 5,000 ppm.

[0100] In a particular embodiment according to the invention, the water-soluble polymer does not comprise a transfer agent. Physical characteristics of the base polymer

[0101] The base polymer has a weight average molecular weight advantageously between 50,000 and 25,000,000 g / mol, preferably between 75,000 and 15,000,000 g / mol, more preferably between 100,000 and 10,000,000 g / mol. This is the weight average molecular weight.

[0102] The weight average molecular weight is preferably measured by gel permeation chromatography coupled with a Malls detector.

[0103] The base polymer is obtained and used in liquid form.

[0104] The viscosity of the solution comprising the base polymer is advantageously between 100 and 50,000 cps, preferably between 1,000 and 20,000 cps.

[0105] Physical characteristics of the water-soluble polymer

[0106] The water-soluble polymer has a weight-average molecular weight advantageously between 50,000 and 25,000,000 g / mol, preferably between 75,000 and 15,000,000 g / mol, more preferably between 100,000 and 10,000,000 g / mol. This is the weight-average molecular weight.

[0107] The weight average molecular weight is preferably measured by gel permeation chromatography coupled with a Malls detector.

[0108] The water-soluble polymer is obtained and used in liquid form.

[0109] The viscosity of the solution comprising the water-soluble polymer is advantageously between 20 and 2,000 cps, preferably between 50 and 1,500 cps.

[0110] The concentration of water-soluble polymer in the solution resulting from step g) is advantageously between 5 and 30% by weight relative to the total weight of the solution comprising the water-soluble polymer, preferably between 8 and 25% by weight, more preferably between 10 and 20% by weight. Gradient

[0111] The water-soluble polymer according to the invention is a gradient polymer.

[0112] Polymers having a gradient structure are polymers composed of at least two monomers in which the change in composition of the monomers is gradual, unlike block polymers, which have an abrupt change in composition, and random polymers, which do not have a continuous change in composition. In the gradient polymer, due to the gradual change in composition along the length of the polymer chain, less intra-chain and inter-chain repulsion is observed.

[0113] The gradient can be formed by a spontaneous or forced gradient. Spontaneous gradient polymerization is due to a difference in reactivity of the monomers. Forced gradient polymerization involves varying the composition of monomers introduced throughout the polymerization time.

[0114] A forced gradient process comprises (1) introducing a first fraction of monomers into a reactor, (2) adding at least one additional fraction of monomers, advantageously different from the first, and (3) polymerizing the monomers introduced into the reactor. Polymerization of the monomers is initiated upon introduction of the first fraction.

[0115] The addition of the additional monomer fraction may be carried out in parallel with the introduction of the first monomer fraction into the reactor (the introduction of the fractions may therefore begin and end at the same time). Alternatively, the start of the first monomer feed (first fraction) into the reactor may precede the start of the addition of a second monomer fraction. Alternatively, a first and a second fraction may be introduced simultaneously, but the duration of addition of the second fraction may be greater than the duration of introduction of the first fraction into the reactor. This embodiment is also applicable to processes using at least 3 monomer fractions.

[0116] According to the process of the invention, the water-soluble polymer obtained is formed by the sequenced addition of the monomers, in other words it is a forced gradient process.

[0117] The process according to the invention comprises a first fraction (F1) and at least two additional fractions (F2 and F3). At least one of the fractions F1, F2 and F3 of the process is different from the other fractions. Preferably, the fractions F1, F2 and F3 are different. By different fraction is meant a fraction having a different monomer composition (ratio and / or nature of the monomers) and / or compounds I and II. (ratio and / or nature of compounds I and II).

[0118] Preferably, at least two of the fractions of the process comprise a monomer of a different nature. Polymerization process

[0119] The process for the sequential polymerization of the water-soluble polymer according to the invention comprises the following steps: a) formation of a solution (SI) comprising at least a first fraction (Fl) containing (1) at least one monomer of formula (AP) or at least one of the optional monomers B and C and (2) at least one compound chosen from compounds I and II; b) polymerization 1 (PO1) of the fraction Fl to form a solution of a first prepolymer (PP1); c) adding, to the solution comprising PP1, a second fraction (F2) containing (1) at least one monomer of formula (AP) or at least one of the optional monomers B and C and (2) at least one compound chosen from compounds I and II; d) polymerization 2 (PO2) of fraction F2 on PP1 to form a second prepolymer (PP2); e) adding, to the solution comprising PP2, a third fraction (F3) containing (1) at least one monomer of formula (AP) or at least one of the optional monomers B and C and (2) at least one compound chosen from compounds I and II; f) polymerization 3 (PO3) of fraction F3 on PP2 to form a solution comprising a base polymer; g) partial or total hydrolysis of the amide group -N(R2)-CO-R* of the monomer of formula (AP) of the base polymer in order to obtain the water-soluble polymer; at least one of the fractions F1, F2 or F3 contains at least one monomer of formula (AP), at least one of the fractions F1, F2 or F3 contains at least one compound I and at least one of the fractions F1, F2 or F3 contains at least one compound II.

[0120] This process may comprise the addition of additional fractions, but none after step g) of hydrolysis of the base polymer.

[0121] It is possible that the improved performance of the polymers obtained according to the process of the invention is due to the fact that the polymerization is carried out sequentially and continuously, that is to say without interruption.

[0122] By "sequentially" is meant that the polymerization of the monomers of the base polymer is carried out in several fractions while not being interrupted, that is to say that the addition of the fractions is carried out continuously and that the polymerization does not stop. The different steps a) to f) are therefore carried out successively. In other words, a first fraction of monomers can be added in casting and polymerizes so as to form a first prepolymer PP1 which continues to polymerize with the fraction F2 to form the prepolymer PP2, which itself continues to polymerize with the F3 fraction to obtain, at the end of polymerization, the base polymer. At least one of the fractions F1, F2 and F3 of the process is different from the other fractions. Preferably, the fractions F1, F2 and F3 are different. The addition of different fractions during the polymerization process made it possible to obtain a gradient in the composition of the base polymer.

[0123] Step g) is carried out on the base polymer once the polymerization is complete. It can be carried out consecutively to the end of the polymerization or at another later time. Preferably, it is carried out consecutively to PO3. In other words, the base polymer used for step g) no longer continues to polymerize. On the other hand, it undergoes a post-treatment which modifies its chemical structure. Step g) is advantageously carried out in a reactor other than the polymerization because it requires dilution of the solution comprising the base polymer. The dilution of the base polymer is advantageously carried out in water.

[0124] The hydrolysis of step g) is advantageously carried out on polymers having monomers of formula (AP).

[0125] In the polymerization process according to the invention, the total sum of the molar percentages of the monomers of the different fractions is equal to the total sum of the molar percentages of the monomers of the water-soluble polymer.

[0126] Step a), formation of a solution (SI) comprising a first fraction (Fl) Solution (SI)

[0127] The SI solution is generally composed of: - a solvent; - a primer; - of a first FL fraction

[0128] The solvent is advantageously water, or a solvent in which the monomers and the water-soluble polymer are soluble. Preferably, the solvent is water.

[0129] The polymerization initiators used can be any compounds that dissociate into radicals under polymerization conditions, for example: organic peroxides, hydroperoxides, hydrogen peroxide, persulfates, azo compounds and redox couples. The use of water-soluble initiators is preferred. In some cases, it is advantageous to use mixtures of various polymerization initiators, for example mixtures of redox catalysts and azo compounds. Preferably, these are persulfates or azo compounds.

[0130] In a particular embodiment, the SI solution is formed by mixing in a polymerization tank the solvent, the initiator and the FL fraction

[0131] In this particular mode, the fraction Fl can be added all at once, in several times or by pouring, that is to say drop by drop into the solvent / initiator mixture. Preferred Initially, the Fl fraction is added all at once to the polymerization tank.

[0132] In a particular embodiment, the initiator and the fraction F1 are added by casting into a polymerization tank comprising the solvent. They can be added separately or premixed. Preferably, they are added separately.

[0133] In a preferred embodiment, the initiator is added continuously throughout the polymerization process. In this case, the initiator is advantageously added in parallel with the different fractions, during the different polymerization steps and during any aging steps of the different prepolymers (PP1 and PP2) and the base polymer.

[0134] In this preferred embodiment of the invention, the duration of the initiator casting is between 50 minutes and 560 minutes, preferably between 130 minutes and 430 minutes. First fraction (F1)

[0135] Advantageously, the fraction F1 comprises between 10 and 65% by weight of monomer (formula (AP) + optionally monomers B and C) relative to the total weight of monomer (A + optionally monomers B and C) of the water-soluble polymer, preferably between 15 and 60% by weight.

[0136] The fraction F1 advantageously comprises between 0 and 100 mol% of monomers of formula (AP), preferably between 5 and 90 mol%, more preferably between 10 and 85 mol% relative to the total number of moles of monomers in the fraction F1.

[0137] When the water-soluble polymer comprises a hydrophilic cationic monomer B, the fraction F1 advantageously comprises between 0 and 100 mol% of hydrophilic cationic monomers B, preferably between 10 and 95 mol%, more preferably between 15 and 90 mol% relative to the total number of moles of monomers in the fraction F1.

[0138] Fraction F1 advantageously comprises between 250 and 30,000 ppm of compounds I relative to the total weight of monomers of formula (AP) (+ optionally monomers B and C) of the water-soluble polymer, preferably between 350 and 10,000 ppm, more preferably between 500 and 7,000 ppm.

[0139] Fraction F1 advantageously comprises between 5 and 30,000 ppm of compounds II relative to the total weight of monomers of formula (AP) (+ optionally monomers B and C) of the water-soluble polymer, preferably between 500 and 20,000 ppm, more preferably between 1,000 and 15,000 ppm.

[0140] The various monomers and compounds comprising F1 are advantageously added in the form of solutions. These solutions can be added separately or as a mixture in the polymer tank, all at once, in several times or by pouring, i.e. drop by drop, to form the solution SL. Preferably, the addition is done as a mixture and all at once.

[0141] When the fraction Fl is added during casting, the casting advantageously lasts between 10 minutes and 80 minutes, preferably between 40 minutes and 70 minutes.

[0142] In a preferred embodiment, the fraction F1 is prepared in the reactor (polymerization tank) before the addition of initiator.

[0143] In a particular embodiment, the fraction F1 comprises at least one monomer of formula (AP), at least one compound I and at least one compound II.

[0144] In a particular embodiment, the fraction F1 comprises at least one monomer of formula (AP), at least one hydrophilic cationic monomer B, at least one compound I and at least one compound II.

[0145] In a particular embodiment, the fraction F1 comprises at least one hydrophilic cationic monomer B, at least one compound I and at least one compound II.

[0146] The pH of the fraction Fl is advantageously adjusted between 4 and 9, preferably between 5 and 8, more preferably between 6 and 7.

[0147] The pH of the fraction F1 can be adjusted using acid or base depending on the initial pH of the fraction F1. As acid, by way of example and in a non-limiting manner, mention may be made in particular of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid. As base, by way of example and in a non-limiting manner, mention may be made in particular of sodium hydroxide, potassium hydroxide, ammonia.

[0148] Step b), polymerization of the F1 fraction to form a first prepolymer (PP1) Polymerization 1 (PO1)

[0149] Prior to the polymerization PO1, the atmosphere of the polymerization tank can be replaced by an inert gas such as for example nitrogen or argon.

[0150] PO1 polymerization is generally a radical polymerization. Polymerization initiators may be used, in particular initiators which dissociate into radicals under the polymerization conditions.

[0151] The PO1 polymerization is generally initiated at a temperature between 70 and 90°C, preferably between 75 and 85°C, the polymerization temperature is then controlled using cooling means so as not to exceed 95°C.

[0152] The PO1 polymerization generally lasts between 10 minutes and 80 minutes, preferably between 40 minutes and 70 minutes.

[0153] The polymerization advantageously begins at the moment when the first monomers, the solvent and the initiator are in contact, in other words, the polymerization time PO1 advantageously corresponds to the duration of the casting of the fraction FL. Advantageously, the polymerization time corresponds to the casting time when the fraction Fl is cast. Prepolymer (PP1)

[0154] At the end of the polymerization PO1, a prepolymer PPL is obtained.

[0155] In a particular embodiment according to the invention, the PP1 link is left to age for between 5 minutes and 60 minutes, preferably between 10 minutes and 30 minutes.

[0156] By "left to age" we mean that the temperature of the medium is maintained between 80 and 90°C after the end of the polymerization to allow an increase in viscosity by internal branching phenomena of the polymer. This definition of aging concerns all stages of the polymerization process.

[0157] Step c), addition of a second fraction (F2) to the solution comprising PP1 Second fraction F2

[0158] Advantageously, fraction F2 comprises between 10 and 80% by weight of monomer (formula (AP) + optionally monomers B and C) relative to the total weight of monomer (formula (AP) + optionally monomers B and C) of the water-soluble polymer, preferably between 15 and 70%.

[0159] Fraction F2 advantageously comprises between 0 and 100 mol% of monomers of formula (AP), preferably between 5 and 90 mol%, more preferably between 10 and 85 mol% relative to the total number of moles of monomers in fraction F2.

[0160] When the water-soluble polymer comprises a hydrophilic cationic monomer B, the fraction F2 advantageously comprises between 0 and 100 mol% of hydrophilic cationic monomers B, preferably between 10 and 95 mol%, more preferably between 15 and 90 mol% relative to the total number of moles of monomers in the fraction F2.

[0161] Fraction F2 advantageously comprises between 250 and 30,000 ppm of compounds I relative to the total weight of monomers of formula (AP) (+ optionally monomers B and C) of the water-soluble polymer, preferably between 350 and 10,000 ppm, more preferably between 500 and 5,000 ppm.

[0162] Fraction F2 advantageously comprises between 250 and 30,000 ppm of compounds II relative to the total weight of monomers of formula (AP) (+ optionally monomers B and C) of the water-soluble polymer, preferably between 500 and 20,000 ppm, more preferably between 1,000 and 15,000 ppm.

[0163] The various monomers and compounds comprising F2 are advantageously added in the form of solutions. These solutions can be added separately or as a mixture in the polymer tank, all at once, in several times or by pouring. Preferably, the addition is done by mixing and by pouring.

[0164] When fraction F2 is added during casting, the casting advantageously lasts between 10 minutes and 100 minutes, preferably between 30 minutes and 90 minutes.

[0165] In a preferred embodiment, fraction F2 comprises at least one monomer of formula (AP) and / or B, at least one compound I and at least one compound IL.

[0166] Step d), polymerization of fraction F2 on PP1 to form a second prepolymer (PP2) Polymerization (PO2)

[0167] The PO2 polymerization is carried out in the continuity of the PO1 polymerization, it is carried out under the same time and temperature conditions (advantageously 70 to 90°C for 10 minutes to 100 minutes, preferably between 30 minutes and 90 minutes).

[0168] The PO1 polymerization advantageously lasts between 10 minutes and 100 minutes, preferably between 30 minutes and 90 minutes.

[0169] PO2 polymerization begins with the addition of the first monomers of fraction F2.

[0170] Advantageously, the polymerization time PO2 corresponds to the duration of the casting of the fraction F2. Prepolymer (PP2)

[0171] At the end of the PO2 polymerization, a PP2 prepolymer is obtained.

[0172] In a particular embodiment according to the invention, the PP2 prepolymer is left to age for between 5 and 60 min, preferably between 10 and 30 min.

[0173] Step e), addition of a third fraction (F3) to the solution comprising PP2 Fraction F3

[0174] Advantageously, fraction F3 comprises between 5 and 40% by weight of monomer (formula (AP) + optionally monomers B and C) relative to the total weight of monomer (formula (AP) + optionally monomers B and C) of the water-soluble polymer, preferably between 10 and 30%.

[0175] Fraction F3 advantageously comprises between 0 and 100 mol% of monomers of formula (AP), preferably between 5 and 90 mol%, more preferably between 10 and 85 mol% relative to the total number of moles of monomers in fraction F3.

[0176] When the water-soluble polymer comprises a hydrophilic cationic monomer B, the fraction F3 advantageously comprises between 0 and 100 mol% of hydrophilic cationic monomers B, preferably between 10 and 95 mol%, more preferably between 15 and 90 mol% relative to the total number of moles of monomers in the fraction F3.

[0177] Fraction F3 advantageously comprises between 0 and 10,000 ppm of compounds I relative to the total weight of monomers of formula (AP) (+ optionally monomers B and C) of the water-soluble polymer, preferably between 10 and 5000 ppm, more preferably between 20 and 1500 ppm.

[0178] Fraction F3 advantageously comprises between 0 and 10,000 ppm of compounds II relative to the total weight of monomers of formula (AP) (+ optionally monomers B and C) of the water-soluble polymer, preferably between 0 and 1,000 ppm.

[0179] The various monomers and compounds making up F3 are advantageously added in the form of solutions. These solutions can be added separately or as a mixture to the polymer tank, all at once, in several batches or by pouring (i.e. drop by drop). Preferably, the addition is done by mixing and drop by drop.

[0180] When fraction F3 is added during casting, the casting advantageously lasts between 10 minutes and 100 minutes, preferably between 30 minutes and 90 minutes.

[0181] In a particular embodiment, the fraction F3 comprises at least one monomer of formula (AP) and at least one compound I.

[0182] Step f), polymerization of fraction F3 on PP2 to form the water-soluble polymer Polymerization (PO3)

[0183] The PO3 polymerization is carried out in the continuity of the PO2 polymerization, it is carried out under the same time and temperature conditions as PO2 (advantageously 70 to 90°C for 10 minutes to 100 minutes, preferably between 30 minutes and 90 minutes).

[0184] PO3 polymerization begins with the addition of the first monomers of the F3 fraction.

[0185] Advantageously, the polymerization time PO3 corresponds to the duration of the casting of the fraction F3.

[0186] At the end of the PO3 polymerization, the base polymer is obtained.

[0187] The reaction is considered to be completed advantageously 60 minutes after obtaining the base polymer, the optional aging time of the base polymer not being included in these 60 minutes, preferably 90 minutes after, more preferably 120 minutes after. The reaction can also be stopped by adding an excess of initiator and / or water, this step is used to eliminate any residual monomers present in the solution comprising the base polymer, once the base polymer is obtained, advantageously after the optional aging step when it is present. Optional step(s)

[0188] The method according to the invention may further comprise additional steps and is not limited to the steps described previously.

[0189] In a particular embodiment according to the invention, the polymerization process according to the invention may comprise the addition of additional fractions constituting the base polymer.

[0190] In a preferred embodiment according to the invention, the base polymer is left to age for between 10 minutes and 180 minutes after step f) of PO3 polymerization and prior to step g), preferably between 30 minutes and 150 minutes. In the case of the addition of additional fractions, aging is carried out after the last polymerization step and prior to step g).

[0191] In a particular embodiment according to the invention, a crosslinking agent and / or a transfer agent is added during at least one of the steps described previously.

[0192] In a particular embodiment according to the invention, a crosslinking agent is added to the fraction F1 and / or to the fraction F2.

[0193] When a crosslinking agent is added, it is advantageously chosen from the crosslinking agents previously mentioned.

[0194] When a crosslinking agent is added, its quantity is advantageously between 5 and 5,000 ppm relative to the total weight of the water-soluble polymer (monomers of formula (AP), and optionally monomers B and C), preferably between 50 and 3,000 ppm.

[0195] In a particular embodiment according to the invention, a transfer agent is added to the fraction F1 and / or to the fraction F2.

[0196] When a transfer agent is added, it is advantageously chosen from the transfer agents previously mentioned.

[0197] When a transfer agent is added, its quantity is advantageously between 10 and 10,000 ppm relative to the total weight of the water-soluble polymer (monomers of formula (AP) and optionally monomers B and C), preferably between 50 and 5,000 ppm.

[0198] Step g), partial or total hydrolysis of the amide group -N(R2)-CO-RX of the monomer of formula (AP) of the base polymer in order to obtain the water-soluble polymer

[0199] Hydrolysis can be carried out by the action of acid (acid hydrolysis) or base (basic hydrolysis). Preferably, it is basic hydrolysis.

[0200] The acid hydrolysis can be carried out using any acid known to those skilled in the art, by way of example and in a non-limiting manner, mention may in particular be made of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid.

[0201] The acid hydrolysis is advantageously carried out at a pH between 0 and 2, preferably between 0 and 1.

[0202] The acid hydrolysis is advantageously carried out at a temperature between 60 and 100°C, preferably between 70 and 90°C, more preferably between 75 and 85°C.

[0203] The duration of the acid hydrolysis step is advantageously between 120 minutes and 720 minutes, preferably between 180 hours and 600 hours, more preferably between 300 minutes and 540 minutes.

[0204] The basic hydrolysis can be carried out using any base known to those skilled in the art, by way of example and in a non-limiting manner, mention may be made of including sodium hydroxide, potassium hydroxide, ammonia.

[0205] The basic hydrolysis is advantageously carried out at a pH between 8 and 14, preferably between 8 and 13, more preferably between 9 and 12.

[0206] The basic hydrolysis is advantageously carried out at a temperature between 60 and 100°C, preferably between 70 and 90°C, more preferably between 75 and 85°C.

[0207] The duration of the basic hydrolysis step is advantageously between 60 minutes and 480 minutes, preferably between 120 minutes and 420 minutes, more preferably between 240 minutes and 360 minutes.

[0208] Depending on the amount of acid or base added, the monomers of formula (AP) are partially or completely converted into monomer A.

[0209] Advantageously between 1 and 100 mol% of monomer of formula (AP) are hydrolyzed, preferably at least 30 mol%, more preferably at least 50 mol%, even more preferably at least 70 mol%.

[0210] Once the hydrolysis reaction is complete, the pH is advantageously adjusted between 6 and 9.

[0211] Although prepared in solution, the water-soluble polymer of the invention can also be used in solid form. The main solid / liquid isolation techniques then used are those of atomization or spray drying (which consists of creating a cloud of fine droplets in a hot gas stream for a controlled period), drum drying, fluidized bed dryers, etc. Papermaking process

[0212] The present invention also relates to a process for manufacturing paper or cardboard comprising (1) the addition of a water-soluble polymer according to the invention into an aqueous suspension of fibers and (2) the formation of a sheet of paper or cardboard. Thus, the invention relates to the use of a water-soluble polymer in a papermaking process.

[0213] The different stages of the process for manufacturing paper, cardboard or the like are known and conform to the techniques calling upon the knowledge of the person skilled in the art; it is not necessary to describe them in more detail because they remain known and conventional to the person skilled in the art; if necessary, he may refer to the document: Handbook for Pulp & Paper Technologists, 4th Edition, GASmook.

[0214] According to the invention, the water-soluble polymer is added in the papermaking process, before or after formation of the sheet of paper, cardboard or the like. Thus, the contacting of the cellulosic material with the polymer of the invention can be carried out in different ways and in particular according to typical methods known to those skilled in the art.

[0215] The water-soluble polymer may be added to the cellulosic material in the form of dilute or undiluted aqueous solution. It can be applied by an impregnation technique, or can be directly added into the fiber suspension at any point in the papermaking process where dry strength agents are usually introduced.

[0216] Thus, the polymer according to the invention can be introduced into the thick stock or into the thin stock. It can be added at the mixing pump, before the headbox or the filter screen. Preferably, the polymer is introduced before the headbox.

[0217] Preferably, the polymer according to the invention is injected industrially into the fibrous suspension, i.e. before its dilution with white water (thick paste). The consistency of the paste is of the order of 1 to 5% by mass of cellulose fibers.

[0218] The papermaking process according to the invention can be implemented with any type of paper pulp, such as for example virgin fiber pulps (Kraft, Bisulfite), recycled fiber pulps, deinked pulps, mechanical and thermomechanical pulps.

[0219] The water-soluble polymer is advantageously added before the formation of the sheet, directly to the fibrous suspension.

[0220] It can be added at a single point or at two injection points.

[0221] The papermaking process according to the invention may also comprise the addition of other additives and / or polymers depending on the needs, by way of example and in a non-limiting manner, mention may be made of: biocides, coagulants, retention agents, flocculants, starch. Use

[0222] The present invention also relates to the use of the water-soluble polymer in the recovery of hydrocarbons (oil and / or gas); in the drilling or cementing of wells; in the stimulation of hydrocarbon wells (oil and / or gas), for example hydraulic fracturing, conforming, diversion; in the treatment of water in open, closed or semi-closed circuit; in the treatment of fermentation musts; in the treatment of sludge; in construction; in the treatment of wood; in the treatment of hydraulic composition (concrete, cement, mortar and aggregates); in the mining industry; in the formulation of cosmetic products; in the formulation of detergents; in the manufacture of textiles; in geothermal energy; in the manufacture of hygienic diapers; or in agriculture.

[0223] The present invention also relates to the use of the water-soluble polymer as a flocculant, coagulant, binding agent, fixing agent, viscosity reducing agent, thickening agent, absorbent agent, friction reducing agent, drainage agent, charge retention agent, dehydrating agent, conditioning agent, stabilizing agent, fixing agent, film-forming agent, sizing agent, superplasticizing agent, clay inhibitor or dispersant.

[0224] The invention and the advantages arising therefrom will become more apparent from the following examples given to illustrate the invention, and not in a limiting manner. Examples

[0225] List of abbreviations: DADMAC: Dimethyldiallyl ammonium (monomer B) NVF: N-Vinylformamide (monomer of formula (AP)) DM AM: Dimethylacrylamide (compound II) SMS: Sodium methallyl sulfonate (compound I) SPS: Sodium persulfate (polymerization initiator) V-50: 2,2'-Azobis(2-methylpropionamidine)dihydrochloride (polymerization initiator) MBA: Methylene bis acrylamide (crosslinking agent)

[0226] Description of GPC-Malls molecular weight characterization

[0227] Gel permeation chromatography is a method for separating macromolecules according to their hydrodynamic volume. It is coupled with a Malls detector, allowing the measurement of light scattering at several angles.

[0228] The synthesized polymers are analyzed under the following conditions: - Instrument: GPC-2 - Columns: Shodex SB-806-HQ & SB-805 Custom - Method : * Temperature: 30°C * Mobile phase: 0.4 M NaNO3, 100 ppm NaN3 + TFA (pH 3.5) * Injection: 100 pL * Flow rate: 0.3 mL / min * Detection: (i) Light Scattering Detector (MALLS): Absolute Molar Mass (ii) Refractometry (RI): Concentration

[0229] The viscosity is measured using a Brookfield viscometer, at 25°C with a Brookfield module chosen from: LV1 speed 12 rpm, LV2 speed 12 rpm, LV4 speed 6 or 12 rpm. The Brookfield module chosen depends on the viscosity of the solution measured. The person skilled in the art knows and is accustomed to adjusting the module according to the viscosity of the solution to be measured, which is part of his general knowledge.

[0230] Preparation of polymers 1 to 3 according to the invention (P1-P3 (INV)) Polymer 1 (PI)

[0231] First sequence: Prepolymer PP1 In a 1 liter reactor equipped with a mechanical stirrer, a thermometer, a Using a refrigerant and a nitrogen gas immersion tube, a first fraction Fl composed of 530.4 g of water, 55.6 g of N-vinylformamide (99% by weight in water), 1.56 g of dimethylacrylamide and 0.330 g of sodium methallyl sulfonate is introduced into the tank base. The pH is adjusted between 6.2 and 6.8 with 1.96 g of phosphoric acid (75% by weight in water) and 2.48 g of sodium hydroxide (30% by weight in water). The medium is heated and maintained at a temperature between 78 and 82 °C using a water bath. An addition of 2 g of V-50 (13% by weight in water) allows this tank base to be initiated and the polymerization of the monomers (PO1) to be initiated to form a first prepolymer PPL

[0232] Second sequence: PP2 prepolymer When the exotherm is over, casting begins: an initiator (30.6 g of V-50 at 3.0% by weight in water) for 180 minutes, and simultaneously a second fraction F2, composed of 75.9 g of water, 111.2 g of N-Vinylformamide (99% by weight in water), 1.56 g of dimethylacrylamide and 0.20 g of sodium methallyl sulfonate, in 60 minutes. Once the fraction F2 is cast, the PP2 prepolymer is left to age for 10 minutes (PO2 polymerization to form the PP2 prepolymer takes place during the casting of the fraction F2 and during aging).

[0233] Third sequence: Polymer base Then, a third fraction F3, consisting of 76.9 g of water, 55.6 g of N-vinylformamide (99% by weight in water), 0.128 g of sodium methallyl sulfonate, is poured in over 50 minutes. At the end of the addition of fraction F3, the polymer is left to age for 120 minutes (PO3 polymerization to form the polymer takes place during the casting of fraction F3 and during aging). Once aging is complete, 10 g of V-50 (39% by weight in water) are added.

[0234] Polymer base 1 The solution comprising the base polymer 1 obtained has a pH of 6.9, an active material of 23.2% by weight, a viscosity of 11,500 cps and a molecular weight obtained by GPC-Malls of 200,000 g / mol.

[0235] Hydrolysis of the base polymer 1 to obtain the polymer 1 according to the invention PI In a 1 liter reactor equipped with a mechanical stirrer, a thermometer, and a condenser, 250 g of polymer base 1 is introduced to carry out the hydrolysis. The polymer is heated to 80 °C. 11.5 g of sodium bisulfite (35% by weight in water) and 50 g of water are added. After 45 minutes, 129.4 g of sodium hydroxide (30% by weight in water) are poured in over 20 minutes. The hydrolysis time is 270 minutes. The polymer is cooled to 35 °C. 73 g of hydrochloric acid (33% by weight in water) is added to adjust the pH to 7, and the water-soluble polymer PI is then obtained. The hydrolysis rate of the polymer PI is 100%. The solution obtained after hydrolysis of the base polymer 1 presents an active material of 12.7% by weight, a viscosity of 190 cps. The water-soluble polymer PI has a molecular weight obtained by GPC-Malls of 220,000 g / mol. Polymer 2 (P2)

[0236] Polymer 2 is produced according to a process similar to that described for polymer 1.

[0237] First sequence: Prepolymer PP1 Polymer PP1 is obtained from a process similar to that described for polymer PI applied to a fraction Fl composed of 521.1 g of water, 28.15 g of dimethyldiallyl ammonium chloride (64% by weight in water), 49.6 g of N-vinylformamide (99% by weight in water), 1.47 g of dimethylacrylamide and 0.25 g of sodium methallyl sulfonate. The pH is adjusted between 6.2 and 6.8 with 1.96 g of phosphoric acid (75% by weight in water) and 2.48 g of sodium hydroxide (30% by weight in water). The medium is heated and maintained at a temperature between 78 and 82°C using a water bath. An addition of 2 g of V-50 (13% by weight in water) allows this starter to be initiated and the polymerization of the monomers (PO1) to form a first PPL prepolymer.

[0238] Second sequence: PP2 prepolymer The PP2 polymer is obtained from a process similar to that described for the PI polymer applied to a fraction F2. When the exotherm is complete, the following begins to be cast: an initiator (31.1 g of V-50 at 3.0% by weight in water) for 180 minutes, and simultaneously a second fraction F2 in 60 minutes, F2 being composed of 75.5 g of water, 99.3 g of N-Vinylformamide (99% by weight in water), 9.4 g of dimethyldiallyl ammonium chloride (64% by weight in water), 1.47 g of dimethylacrylamide and 0.16 g of sodium methallyl sulfonate.

[0239] Third sequence: Polymer base 2 The base polymer 2 is obtained from a process similar to that described for the polymer PI applied to a fraction F3. Once the fraction F2 is cast, the prepolymer PP2 is left to age for 10 minutes (the PO2 polymerization to form the prepolymer PP2 takes place during the casting of the fraction F2 and during the aging). Then, a third fraction F3 composed of 75.5 g of water, 49.6 g of N-vinylformamide (99% by weight in water), 0.048 g of sodium methallyl sulfonate begins to be cast in 50 minutes. At the end of the addition of the F3 fraction, the polymer is left to age for 120 minutes (PO3 polymerization to form the polymer takes place during the casting of the F3 fraction and during aging). Once aging is complete, 10g of V-50 (39% by weight in water) are added

[0240] Polymer base 2 The solution comprising the base polymer 2 obtained has a pH of 6.6, a active ingredient of 23.2% by weight, a viscosity of 3,000 cps and a molecular weight obtained by GPC-Malls of 185,000 g / mol.

[0241] Hydrolysis of the base polymer 2 to obtain the polymer 2 according to the invention P2 The hydrolysis of polymer base 2 is carried out according to a protocol similar to that of polymer base 1. The hydrolysis rate of polymer P2 is 100%. Polymer base 2 is heated to 80°C. 11.5g of sodium bisulfite (35% by weight in water) and 23.5g of water are added. After 45 minutes, 147.5g of sodium hydroxide (25% by weight in water) are poured in over 20 minutes. The hydrolysis time is 270 minutes. The polymer is cooled to 35°C. 66.4g of hydrochloric acid (33% by weight in water) is added to adjust the pH to 7, and the water-soluble polymer P2 is then obtained. The hydrolysis rate of polymer P2 is 100%. The solution obtained after hydrolysis of the base polymer 2 has a pH of 7, an active material of 12.7% by weight, a viscosity of 100 cps. The water-soluble polymer P2 has a molecular weight obtained by GPC-Malls of 201,000 g / mol. Polymer 3 (P3)

[0242] First sequence: Prepolymer PP1 Polymer PP1 is obtained from a process similar to that described for polymer PI applied to a fraction Fl composed of 431.3 g of water, 68.7 g of dimethyldiallyl ammonium chloride (64% by weight in water), 97.6 g of N-Vinylformamide (99% by weight in water), 2.175 g of dimethylacrylamide and 0.12 g of sodium methallyl sulfonate. The pH is adjusted between 6.2 and 6.8 with 1.96 g of phosphoric acid (75% by weight in water) and 2.48 g of sodium hydroxide (30% by weight in water). The medium is heated and maintained at a temperature between 78 and 82°C using a water bath. An addition of 10.9 g of V-50 (13% by weight in water) allows this starter to be initiated and the polymerization of the monomers (PO1) to form a first PPL prepolymer.

[0243] Second sequence: Prepolymer PP2 The PP2 polymer is obtained from a process similar to that described for the PI polymer applied to a fraction F2. When the exotherm is complete, the following begins to be cast: an initiator (58.6 g of V-50 at 2.7% by weight in water) for 180 minutes, and simultaneously a second fraction F2, in 60 minutes, composed of 106.9 g of water, 19.8 g of N-vinylformamide (99% by weight in water), 29.44 g of dimethyldiallyl ammonium chloride (64% by weight in water), 1.45 g of dimethylacrylamide and 0.18 g of sodium methallyl sulfonate.

[0244] Third sequence: Polymer base 3 The base polymer 3 is obtained from a process similar to that described for the PI polymer applied to a fraction F3. Once the fraction F2 is cast, the PP2 prepolymer is left to age for 10 minutes (the PO2 polymerization to form the prepolymer PP2 takes place during the casting of fraction F2 and during aging). Then a third fraction F3 begins to be cast, in 50 minutes, composed of 99.8 g of water, 62.9 g N-vinylformamide (99% by weight in water), 0.18 g of sodium methallyl sulfonate. At the end of the addition of the F3 fraction, the polymer is left to age for 120 minutes (PO3 polymerization to form the polymer takes place during the casting of the F3 fraction and during aging). Once aging is complete, 10g of water are added as well as 0.1g of V-50.

[0245] Polymer base 3 The obtained base polymer 3 has a pH of 6.6, an active material of 24.2% by weight, a viscosity of 3,000 cps and a molecular weight obtained by GPC-Malls of 279,000 g / mol.

[0246] Hydrolysis of the base polymer 3 to obtain the polymer 3 according to the invention P3 The hydrolysis of the base polymer 3 is carried out according to a protocol similar to that of the base polymer 1. The solution obtained after hydrolysis of the base polymer 3 has a pH of 7, an active material of 16% by weight, a viscosity of 310 cps and a molecular weight obtained by GPC-Malls of 299,000 g / mol. The hydrolysis rate of the polymer P3 is 100%.

[0247] Preparation of polymers 4 to 6 counterexamples (CEI to CE3) Polymer 4 (IEC)

[0248] This is a commercial PVAm polymer Xelorex RS 1300 with a hydrolysis rate of 100%. Polymer 5 (CE2)

[0249] Preparation of a base polymer 5 in one sequence In a 1 liter reactor equipped with a mechanical stirrer, a thermometer, a condenser and a nitrogen gas dipstick, 238 g of water and 90 g of dimethyldiallyl ammonium chloride (64% by weight in water) are introduced at the bottom of the tank. The pH is adjusted between 6.2 and 6.8 with 1.96 g of phosphoric acid (75% by weight in water) and 2.48 g of sodium hydroxide (30% by weight in water). The medium is heated and maintained at a temperature of 75 °C using a water bath. The following are poured in: 80.2 g of V-50 (2.9% by weight in water) for 240 minutes, and simultaneously a fraction composed of 169 g of N-vinylformamide (99% by weight in water), in 120 minutes. At the end of the initiator addition, the polymer is left to age for 120 minutes. The obtained base polymer 5 has a pH of 6.4, an active material of 22.6% by weight, a viscosity of 25,000 cps and a molecular weight obtained by GPC-Malls of 250,000 g / mol.

[0250] Hydrolysis of polymer base 5 to obtain polymer 5 counter-example CE2 The hydrolysis of polymer base 5 is carried out according to a protocol similar to that of polymer base 1. The hydrolysis rate of polymer P5 is 100%. In a 1 liter reactor equipped with a mechanical stirrer, a thermometer, and a condenser, 250g of base 5 polymer is introduced to carry out the hydrolysis. The polymer is heated to 80°C. 7.26g of sodium bisulfite (35% by weight in water) is added. After 45 minutes, 96g of sodium hydroxide (25% by weight in water) is poured in over 20 minutes. The hydrolysis time is 270 minutes. The polymer is cooled to 35°C. 42g of hydrochloric acid (33% by weight in water) is added to adjust the pH to 7. The obtained CE2 polymer has a pH of 7, an active material of 15.6% by weight, a viscosity of 1120 cps and a molecular weight obtained by GPC-Malls of 270,000 g / mol. Polymer 6 (CE3)

[0251] The polymer CE3 is prepared according to a protocol similar to that of the polymer PI, with the difference that there is no casting of fraction F3, the compositions of the castings F1 and F2 are adjusted according to the values ​​summarized in table 1. The hydrolysis rate of the polymer P6 is 100%.

[0252] The compositions of the different fractions of the process for preparing polymers 1 to 6 are summarized in Table 1.

[0253] In Table 1, the monomer content represents the mass percentage of the NVF or DADMAC monomer relative to the total weight of the corresponding monomer in the three fractions. Thus the sum of the percentages of NVF or DADMAC monomer in the three fractions is equal to 100%.

[0254] The contents of compounds I (SMS) and II (DMAM) are expressed in ppm by mass relative to the total weight of monomer(s) in the three fractions.

[0255] [Tables 1] Polymer Quantity of Fl compounds (by weight) Quantity of F2 compounds (by weight) Quantity of F3 compounds (by weight) PI NVF: 25% DMAM: 7085 ppm SMS: 1499 ppm NVF: 50% DMAM: 7085 ppm SMS: 908 ppm WF: 25% SMS: 581 ppm P2 NVF: 25% DADMAC: 75% DMAM: 7480 ppm SMS: 1272 ppm NVF: 50% DADMAC: 25% DMAM: 7480 ppm SMS: 814 ppm NVF: 25% SMS: 244 ppm P3 NVF: 54% DADMAC: 70% DMAM: 12187 ppm SMS: 672 ppm NVF: 11% DADMAC: 30% DMAM: 8124 ppm SMS: 1008 ppm NVF: 35% SMS: 1008 ppm IEC - NVF: 100% - CE2 DADMAC: 100% NVF: 100% - CE3 NVF: 50% DMAM: 7085 ppm SMS: 1499 ppm NVF: 50% DMAM: 7085 ppm SMS: 1489 ppm

[0256] Table 1: Compositions of the fractions of the polymerization process to obtain polymers PI to P3 and CEI to CE3.

[0257] The physicochemical properties of the polymers obtained are described in Table 2 below:

[0258] [Tables2] Polymer Monomer molar ratio Viscosity before hydrolysis (cps) Molecular weight (g / mol) before hydrolysis Viscosity after hydrolysis (cps) Molecular weight (g / mol) after hydrolysis PI NVF (100) 11,000 215,000 190 236,000 P2 NVF / DADMAC (95 / 5) 3,000 205,000 100 225,000 P3 NVF / DADMAC (87 / 13) 3,000 279,000 310 299,000 CEI NVF (100) 55,500 330,000 1200 340,000 CE2 NVF / DADMAC (87 / 13) 25,000 250,000 1120 270,000 CE3 NVF (100) 41,000 240,000 1050 260,000

[0259] Table 2: Physicochemical properties of polymers PI to P3 according to the invention and CEI to CE3.

[0260] The differences and advantages provided by the invention compared to the art are observed. prior art, in particular with regard to the lower viscosity for the polymer solutions according to the invention for a close molecular weight. Application testing

[0261] The wet pulp used in all application examples is obtained by disintegration of dry pulp in order to obtain a final aqueous concentration of 1% by mass. It is a neutral pH pulp composed of 100% recycled cardboard fibers.

[0262] Vacuum Drainage Performance Evaluation (DDA)

[0263] The DDA (Dynamic Drainage Analyzer) makes it possible to automatically determine the time (in seconds) required to drain a fibrous suspension under vacuum on a fabric. The polymers are added to the wet paste (0.6 liters of paste at 1.0% by mass) in the DDA cylinder with stirring at 1000 rpm: T= 0 s: stirring of the paste T= 10 s: addition of the polymer(s) T= 30 s: stop stirring and drain under vacuum at 200 mBar for 60 s.

[0264] The pressure under the fabric is recorded as a function of time. When all the water is evacuated from the fibrous mat, the air passes through it, causing a break in slope to appear on the curve representing the pressure under the fabric as a function of time. The time, expressed in seconds, recorded at this break in slope corresponds to the draining time. The shorter the time, the better the vacuum draining.

[0265] Performance in dry resistance application, weight at 80g.m2

[0266] The necessary quantity of pulp is taken so as to finally obtain a sheet with a weight of 80 g.m2.

[0267] The wet paste is introduced into the vat of the dynamic form and is kept stirring. The various components of the system are injected into this paste according to the predefined sequence. A contact time of 30 to 45 seconds is generally observed between each addition of polymer.

[0268] Paper forms are made with an automatic dynamic form: a blotter and the forming fabric are placed in the bowl of the dynamic form before starting the rotation of the bowl at 1000 rpm 1 and building the water wall. The treated pulp is distributed on the water wall to form the fibrous mat on the forming fabric.

[0269] Once the water is drained, the fibrous mat is recovered, pressed under a press delivering 4 bars, then dried at 117 °C. The resulting sheet is conditioned overnight in a room with controlled humidity and temperature (50% relative humidity and 23 °C). The dry strength properties of all the sheets obtained by this procedure are then measured.

[0270] The burst is measured with a Messmer Buchel M 405 burst tester according to the standard TAPPI T403 om-02. The results are expressed in Table 3 as a percentage improvement over a blank.

[0271] The dry breaking length is measured in the machine direction with a Testometric AX tensile tester according to TAPPI T494 om-01. The results are expressed in Table 3 as a percentage improvement compared to a blank.

[0272] The amount of polymer added is expressed in kg of active polymer per tonne of dry fibre. Tests at 1.5 kg / t were carried out and summarised in Table 3.

[0273] [Tables3] Percentage increase Burst (%) Percentage increase DBL (%) Percentage increase DDA (%) White 0 0 0 PI (L5kg / t) 32 19 61 P2 (1.5 kg / t) 29 21 56 P3 (1.5 kg / t) 28 22 55 CEI (1.5 kg / t) 26 15 53 CE2 (1.5 kg / t) 25 14 49 CE3 (1.5 kg / t) 24 15 52

[0274] Table 3: Drainage and dry strength results of polymers 1 to 3 according to the invention and counter-example polymers CEI to CE3.

[0275] The polymers of the invention have superior drainage performance (DDA) and mechanical characteristics (Burst: bursting; DBL: rupture in the dry state) compared to polymers obtained from a single fraction or from 2 fractions, while having a lower viscosity, thus allowing ease of use and a reduction in environmental impact during their use.

Claims

Claims

1. A water-soluble polymer comprising: - at least one monomer A obtained by partial or total hydrolysis of the -N(R2)-CO-R* group of a monomer of formula (AP): [Chem.l] CIb CO (AP) where R1 and R2 are, independently, a hydrogen atom or an alkyl chain of 1 to 6 carbons, - at least one structuring system comprising: (i) at least one compound I chosen from: allylsulfonic acid, methallylsulfonic acid, allyl disulfonic acid, methallyl disulfonic acid, their salts and their mixtures; (ii) at least one compound II and of formula (II): [Chem. 2] R3 and R4 being, independently of each other, a hydrogen atom, a methyl group, an ethyl group, an isopropyl group or a CH2-OH group; R3 and R4 not both being hydrogen (R3^H when R4 =H; R^H when R3=H), - optionally at least one hydrophilic cationic monomer B distinct from monomer A; - optionally at least one monomer C chosen from hydrophilic anionic monomers distinct from compound I, hydrophilic non-ionic monomers distinct from the monomer of formula AP and from compound II, hydrophilic zwitterionic monomers and hydrophobic monomers; said polymer being free of anionic monomer other than compound I; said water-soluble polymer being obtained according to the following steps: a) formation of a solution (SI) comprising at least a first fraction (Fl) containing (1) at least one monomer of formula (AP) and / or at least one of the optional monomers B and C and (2) at least one compound chosen from compounds I and II; b) polymerization 1 (PO1) of fraction F1 to form a solution of a first prepolymer (PP1); c) addition, to the solution comprising PP1, of a second fraction (F2) containing (1) at least one monomer of formula (AP) and / or at least one of the optional monomers B and C and (2) at least one compound chosen from compounds I and II; d) polymerization 2 (PO2) of fraction F2 on PP1 to form a second prepolymer (PP2);e) adding, to the solution comprising PP2, a third fraction (F3) containing (1) at least one monomer of formula (AP) and / or at least one of the optional monomers B and C and (2) at least one compound chosen from compounds I and II; f) polymerization 3 (PO3) of fraction F3 on PP2 to form a solution comprising a base polymer; g) partial or total hydrolysis of the -N(R2)-CO-R* group of the monomer of formula (AP) of the base polymer in order to obtain the water-soluble polymer; at least one of fractions F1, F2 or F3 contains at least one monomer of formula (AP), at least one of fractions F1, F2 or F3 contains at least one compound I and at least one of fractions F1, F2 or F3 contains at least one compound II.;

2. Water-soluble polymer according to claim 1, characterized in that the monomer(s) of formula (AP) may be chosen, in particular, from N-vinylformamide, N-vinyl-N-methylformamide, N-vinylacetamide, N-vinyl-N-methylacetamide, N-vinyl-N-ethylacetamide, N-vinyl-propianamide, N-vinyl-N-methylpropianamide and N-vinylbutyramide. Preferably, it is N-vinylformamide.

3. Water-soluble polymer according to one of the preceding claims, characterized in that it comprises between 500 and 50,000 ppm of compound I, relative to the total weight of the monomers of formula (AP) (+ option-

4.

5.

6.

7. clearly monomers B and C). Water-soluble polymer according to one of the preceding claims, characterized in that it comprises between 500 and 50,000 ppm of compound II, relative to the total weight of the monomers of formula (AP) (+ optionally monomers B and C). Water-soluble polymer according to one of the preceding claims, characterized in that compound II is chosen from: N,N-dimethylacrylamide, N,N-diethylacrylamide, N,N-isopropylacrylamide, N-methylolacrylamide and mixtures thereof. Water-soluble polymer according to one of the preceding claims, characterized in that the mass ratio between compound I and compound II is between 0.01 and 100. A process for the sequential preparation of a water-soluble polymer, comprising the following steps: a) formation of a solution (SI) comprising at least a first fraction (Fl) containing (1) at least one monomer of formula (AP) and / or at least one of the optional monomers B and C and (2) at least one compound chosen from compounds I and II; b) polymerization 1 (PO1) of the fraction Fl to form a solution of a first prepolymer (PP1); c) adding, to the solution comprising PP1, a second fraction (F2) containing (1) at least one monomer of formula (AP) and / or at least one of the optional monomers B and C and (2) at least one compound chosen from compounds I and II; d) polymerization 2 (PO2) of fraction F2 on PP1 to form a second prepolymer (PP2); e) adding, to the solution comprising PP2, a third fraction (F3) containing (1) at least one monomer of formula (AP) and / or at least one of the optional monomers B and C and (2) at least one compound chosen from compounds I and II; f) polymerization 3 (PO3) of fraction F3 on PP2 to form a solution comprising a base polymer; g) partial or total hydrolysis of the amide group -N(R2)-CO-R* of the monomer of formula (AP) of the base polymer in order to obtain the water-soluble polymer; at least one of the fractions F1, F2 or F3 contains at least one monomer of formula (AP), at least one of the fractions F1, F2 or F3 contains at least one compound I and at least one of the fractions F1, F2 or F3 contains at least one compound II.

8. A method according to claim 7, characterized in that an initiator is added continuously throughout the polymerization process.

9. Method according to claim 7 or 8, characterized in that, after step f) of polymerization (PO3) and prior to step g), the method comprises an aging step of 10 minutes to 180 minutes.

10. Method according to one of claims 7 to 9, characterized in that the hydrolysis is a basic hydrolysis.

11. Process according to one of claims 7 to 10, characterized in that between 1 and 100 mol% of monomer of formula (AP) are hydrolyzed.

12. A method of manufacturing paper or cardboard comprising the addition of a water-soluble polymer according to one of claims 1 to 6, in an aqueous suspension of fibers and the formation of a sheet of paper or cardboard.

13. Use of the water-soluble polymer according to one of claims 1 to 6, in the recovery of hydrocarbons; in the drilling or cementing of wells; in the stimulation of hydrocarbon wells; in the treatment of water in an open, closed or semi-closed circuit; in the treatment of fermentation musts; in the treatment of sludge; in construction; in the treatment of wood; in the treatment of hydraulic composition; in the mining industry; in the formulation of cosmetic products; in the formulation of detergents; in the manufacture of textiles; in geothermal energy; in the manufacture of hygienic diapers; or in agriculture.

14. Use of the water-soluble polymer according to one of claims 1 to 6, as flocculant, coagulant, binding agent, fixing agent, viscosity reducing agent, thickening agent, absorbent agent, friction reducing agent, drainage agent, charge retention agent, dehydrating agent, conditioning agent, stabilizing agent, fixing agent, film-forming agent, sizing agent, superplasticizing agent, clay inhibitor or dispersant.

Citation Information

Patent Citations

  • Hydrated crystalline form of 2-acrylamido-2-methylpropane sulfonic acid

    US10759746B2

  • Inverse suspension polymerization of water soluble unsaturated monomers

    US2982749A

  • Water-soluble polymers and copolymers

    US3278506A

  • Water-in-oil emulsion polymerization process for polymerizing watersoluble monomers

    US3284393A

  • Process of production of water-soluble linear polymers of very high molecular weight

    US3957739A