A stack of layers whose color, in the visible spectrum, changes

The stack design with a phase change material layer between the metal and transparent layers in the lower mirror enhances color differentiation, achieving over 50° shade difference and improved brightness, addressing the limitation of existing stacks.

FR3149231A1Pending Publication Date: 2024-12-06UNIV DAIX MARSEILLE +2
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
FR2023005428
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing stacks with an optical cavity using a phase change material for either the upper mirror or transparent layer do not exhibit a significant difference in color between the amorphous and crystalline phases, limiting the variety of shades achievable.

Method used

A stack design with a lower mirror comprising a metal layer, a transparent layer of dielectric material, and an upper mirror, where the phase change material layer is located between the metal layer and the transparent layer, ensuring a refractive index difference greater than 0.2, and using antimony trisulfide (Sb2S3) with specific thicknesses to enhance color differentiation.

Benefits of technology

The proposed stack achieves a color difference of over 50° between amorphous and crystalline phases, providing a wider range of shades without compromising the number of possible shades, and includes a silver upper mirror for increased brightness and saturation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Stack of layers whose color changes in the visible range. This stack comprises, in order: - a lower mirror (12) having a metallic layer (20), - a transparent layer (14) composed of one or more dielectric materials transparent in the visible range, the thickness of this transparent layer being greater than 10 nm, and - an upper mirror (16; 58). The lower mirror includes a layer (22) made of a phase-change material whose thickness is between 10 nm and 250 nm. The phase-change material layer (22) is located above the metallic layer and forms the face of the lower mirror in contact with the transparent layer. Fig. 1
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Stack of layers whose color, in the visible range, changes

[0001] The invention relates to a stack of layers whose color, in the visible range, changes in response to a heat treatment.

[0002] Such stacks have, for example, been disclosed in the following documents:

[0003] - WO2017215363A1, and

[0004] - Weiling DONG et al. : “Wide Bandgap Phase Change Material Tuned Visible Photonics.” In: Advanced Functional Materials 29(6), 8 / 02 / 2019.

[0005] Hereinafter, Weiling Dong's article is referred to as "Dong2019".

[0006] As explained in the previous documents, such stacks are useful for manufacturing the pixels of a screen or manufacturing electronic paper on which it is possible to print an image and then erase it to print a new one many times.

[0007] For this purpose, known stacks comprise a layer of phase change material whose phase changes between an amorphous phase and a crystalline phase in response to a heat treatment. The phase change modifies the refractive index of the phase change material, which modifies the hue of the stack.

[0008] More specifically, it has already been observed that it is advantageous for the stack to comprise an optical cavity. For this, known stacks, such as those described in application WO2017215363A1 and in article Dong2019, comprise, in order, a lower mirror, a transparent layer and an upper mirror. These stacks with an optical cavity make it possible in particular to obtain a greater variety of shades compared to a stack without an upper mirror and therefore without an optical cavity.

[0009] Until now, in stacks with an optical cavity, the phase change material layer is either used to form the upper mirror, as in application WO2017215363A1, or used to form the transparent layer as in article Dong2019. These known stacks make it possible to obtain a wide variety of shades. On the other hand, the difference between the shade obtained when the phase change material is in its amorphous phase and the shade obtained when the phase change material is in its crystalline phase is not very significant.

[0010] The invention aims to remedy this drawback by proposing a stack which retains the advantages of stacks comprising an optical cavity while making it possible to obtain more differentiated shades between the amorphous and crystalline phase change material.

[0011] The invention therefore relates to a stack of layers whose color, in the visible range, changes in response to a heat treatment, this stack comprising in order:

[0012] - a lower mirror comprising a metallic layer,

[0013] - a transparent layer composed of one or more dielectric materials transparent in the visible range, the thickness of this transparent layer being greater than 10 nm, and

[0014] - an upper mirror,

[0015] at least one of the lower and upper mirrors being partially reflective,

[0016] one of the mirrors and the transparent layer comprising a layer made of a phase change material whose thickness is between 10 nm and 250 nm, and

[0017] the difference between the real parts of the refractive indices of the phase change material and the transparent layer is greater than 0.2,

[0018] wherein the phase change material layer is located in the lower mirror above the metal layer and forms the face of the lower mirror in contact with the transparent layer.

[0019] The embodiments of this stack may comprise one or more of the following characteristics:

[0020] 1) The phase change material is a material selected from the group consisting of of the following materials and their alloy: Sb2S3, GeTe, Ge2Sb2Te5, GeSe2, Sb2Te3, Bi2 Te3, Sb2Se3, VO2.

[0021] 2) The phase change material is antimony trisulfide of formula chemical Sb2S3.

[0022] 3) The thickness of the phase change material layer is between 10 nm and 50 nm.

[0023] 4) The upper mirror has a silver metallic layer.

[0024] 5) The upper mirror has a titanium metal layer.

[0025] 6) The thickness of the metal layer of the upper mirror is between 3 nm and 40 nm.

[0026] 7) The thickness of the metal layer of the lower mirror is greater than 50 nm.

[0027] 8) The difference between the shades of the stack when the layer of material to phase change is entirely in an amorphous phase and when the layer of phase change material is entirely in a crystalline phase, is greater, in absolute value, than 50° when this deviation is measured using a color wheel where primary red is at 0°, primary green is at 120°, primary blue is at 240°, and mixtures, at intermediate angles, in proportion to the two primary elements that compose them.

[0028] 9) The stack comprises a transparent surface layer deposited on the upper mirror on the side opposite the transparent layer interposed between the lower and upper mirrors.

[0029] The invention also relates to a method for manufacturing the above stack, in which the different layers of the stack are deposited, on a substrate, one on top of the other, by an electron gun evaporation method.

[0030] The invention will be better understood on reading the description which follows, given solely by way of non-limiting example and made with reference to the drawings in which:

[0031] - [Fig.l] is a schematic illustration, in perspective, of the architecture of a first embodiment of a stack capable of changing color in response to heat treatment,

[0032] - Figures 2 and 3 are schematic illustrations, in perspective, respec tively, of a second and a third embodiment of the stack of [Fig.l].

[0033] In these figures, the same references are used to designate the same elements. In the remainder of this description, the characteristics and functions well known to those skilled in the art are not described in detail.

[0034] In this description, in a chapter I, the definitions and terminology used in this text are presented. Then, in a chapter II, detailed examples of embodiments are described with reference to the figures. In a chapter III, variants of these embodiments are introduced. Finally, the advantages of the different embodiments are specified in a chapter IV.

[0035] Chapter I: Definitions and terminology

[0036] The expression “element made of material A” or “element of material A” designates an element in which material A represents at least 70%, by mass, of this element and preferably, at least 90% or 95% by mass of this element.

[0037] The term "PCM material" refers to a solid-solid transition phase change material, where the acronym PCM stands for "Phase Change Material".

[0038] In this text, a phase change of a material designates a change from an amorphous solid phase to a crystalline solid phase of this material as well as the change in the opposite direction, that is to say from the crystalline solid phase to the amorphous solid phase.

[0039] The expression “electrical conductor” designates a material whose electrical conductivity, at 20°C, is greater than 106 S / m and, preferably, greater than 107 S / m.

[0040] The expression “room temperature” designates a temperature between 15°C and 35°C and, typically, equal to 25°C.

[0041] The visible spectrum or the visible domain is formed of electromagnetic waves whose wavelengths are between 380 nm and 760 nm.

[0042] "Light" means electromagnetic radiation whose frequency range extends at least over the entire visible spectrum. For example, light can be natural light on Earth.

[0043] A transparent material is a material whose extinction coefficient is less than 103 at the wavelength of interest.

[0044] The symbols "nr" and "k" denote, respectively, the real part and the imaginary part of the refractive index of a material in the visible range. Therefore, the expression "the refractive index nr" denotes only the real part of the refractive index and the expression "extinction coefficient k" denotes only the imaginary part of the refractive index. The refractive index nr and the extinction coefficient k are likely to depend on the wavelength considered.

[0045] In the field of computing, a hue is coded by a direction identified on a color wheel which presents the colors in the purest possible form. On this color wheel, primary red is at 0°, primary green is at 120°, primary blue is at 240°, and the mixtures, at intermediate angles, in proportion to the two primaries which compose them. In this text, the difference between a first and a second hue is expressed in the form of an angle in degrees. This angle is equal to the difference between a first and second angle. The first and second angles are equal to the angles on the color wheel which code, respectively, the first and second hues.

[0046] The figures are oriented relative to an orthogonal XYZ coordinate system, where the X and Y directions are horizontal and the Z direction is vertical. Terms such as "above", "below", "top", "bottom", "upper", "lower" are defined relative to the Z direction.

[0047] Chapter II: Examples of embodiments

[0048] [Fig. 1] represents a stack 2 of layers comprising a tinted face 4 whose shade, in the visible range, changes in response to a heat treatment. This change in shade is reversible.

[0049] Stack 2 comprises, stacked on top of each other from bottom to top:

[0050] - a substrate 10,

[0051] - a lower mirror 12,

[0052] - a transparent layer 14,

[0053] - an upper mirror 16, and

[0054] - a transparent surface layer 18.

[0055] The transparent layer 14 forms an optical cavity and more precisely a cavity of Fabry-Perot. For this purpose, layer 14 is made of one or more dielectric materials transparent in the visible range. For example, here, transparent layer 14 is made of silicon dioxide.

[0056] The thickness eM of the transparent layer 14 is between 10 nm and 500 nm or between 50 nm and 500 nm or between 100 nm and 500 nm. The thickness eM is the first parameter which determines the tint of the face 4. By way of illustration, the thickness eu is here equal to 350 nm.

[0057] The mirror 16 is a partially reflecting mirror. A partially reflecting mirror is a mirror through which a portion of the incident light passes. For this purpose, the transmission coefficient of the mirror 16 is greater than 5%. Conversely, the mirror 16 reflects at least 10% of the incident light and, preferably, between 20% and 80% of the incident light. For this purpose, the mirror 16 is formed from a metal layer of thickness ei6. The thickness ei6 depends on the optical properties of the metal used to make the layer 16. However, the thickness ei6 is generally between 5 nm and 100 nm. In the case where the metal used is titanium or silver, the thickness ei6 is for example between 5 nm and 30 nm. For example, in this embodiment, the metal layer is made of titanium and its thickness is equal to 10 nm.

[0058] The surface layer 18 isolates the mirror 16 from the external environment in order to protect it, in particular, against oxidation. The layer 18 can also slightly modify the hues of the face 4. The upper face of the layer 18 forms the tinted face 4 of the stack 2. The layer 18 is made of transparent material. For example, this surface layer 18 is made of a material chosen from those usable for making the layer 14. By way of example, here, the layer 18 is made of silicon dioxide and its thickness ei8 is 25 nm.

[0059] The mirror 12 reflects more than 50% and, preferably, more than 80% or more than 95% of the incident light in the visible range. For this purpose, it comprises, stacked on top of each other in the Z direction and going from bottom to top, a metal layer 20 and a layer 22 of PCM material.

[0060] The thickness e20 of the metal layer 20 is greater than 30 nm and, preferably, greater than or equal to 100 nm to guarantee that the light does not pass through the metal layer and therefore overcome the nature of the substrate 10.

[0061] Here, layer 20 is made of silver.

[0062] The layer 22 is made of a solid-solid transition phase change material. Such a PCM material can switch, reversibly, between an amorphous solid phase and a crystalline solid phase. Such a PCM material has a temperature Te and a temperature Tm which are specific to it. The temperature Te is the temperature above which the PCM material switches from its amorphous phase to its crystalline phase. The temperature Tm is the melting temperature of the PCM material. temperature Te is lower, often by at least 100°C, than temperature Tm.

[0063] Here, the PCM material has a temperature Te which is higher than room temperature. Thus, each of the phases of the PCM material is stable at room temperature. Therefore, the phase in which the PCM material is located remains unchanged in the absence of external energy input and, in particular, in the absence of heat treatment. Preferably, the temperature Te is higher than 100°C or 150°C.

[0064] Typically, the transition from the amorphous phase to the crystalline phase is caused by using a first heat treatment. The first heat treatment is an electrical pulse or a laser pulse that raises the temperature of the PCM material above its temperature Te and below its temperature Tm and then maintains the temperature of the PCM material between the temperatures Te and Tm for a duration ATc before returning to below the temperature Te. The duration ATc is chosen to be long enough, for example, to allow enough time for the PCM material to crystallize completely. Conversely, if the duration ATc is chosen to be too short, only partial crystallization of the PCM material occurs.

[0065] The transition from the crystalline phase to the amorphous phase is caused by using a second heat treatment different from the first heat treatment. Here, the second heat treatment is an electrical pulse or a laser pulse that raises the temperature of the PCM material above its temperature Tm and then maintains it above the temperature Tm for a duration ATm before dropping back below the temperature Tm. The duration ATm is chosen to be long enough to make the PCM material completely amorphous. Generally, the duration ATm is much shorter than the duration ATc. At the end of the duration ATm, the temperature of the PCM material quickly drops back below the temperature Te. This drop in temperature is fast enough so that the PCM material does not re-crystallize upon cooling. For example, the temperature drop is 1°C / ns.

[0066] The refractive index of the PCM material changes substantially, in the visible range, when this PCM material changes phase. Here, a change in the refractive index is considered substantial if, for at least one wavelength in the visible range, the change in the refractive index nr or the extinction coefficient k is greater than 10% or 20%. In other words, there is a wavelength in the visible range, for which the value of the index nr or the coefficient k increases or decreases by 10% or 20% in response to the phase change.

[0067] The index nr of the layer 22 is different from the index nr of the transparent layer 14. For this purpose, the difference, in absolute value, between the indices nr of the layers 14 and 22 is greater than 0.2 or 0.3.

[0068] Preferably, to have, at the same time, a wide range of possible shades while by obtaining very different shades for the amorphous and crystalline phases of the PCM material, the PCM material is antimony trisulfide with the chemical formula Sb2 S3. The temperatures Te and Tm of this PCM material are approximately equal, respectively, to 270°C and 550°C.

[0069] The thickness e22 of the layer 22 is typically between 10 nm and 250 nm or between 10 nm and 200 nm. In the case of the Sb2S3 material, preferably, the thickness e22 is between 10 nm and 200 nm and, even more advantageously, between 10 nm and 50 nm. The thickness e22 is the second parameter which, in combination with the thickness eM, determines the colors of the face 4. Here, the thickness e22 is equal to 24 nm.

[0070] Preferably, the mirror 12 also comprises a diffusion barrier 24 between the layers 20 and 22. This barrier 24 prevents the layers 20 and 22 from mixing during the manufacture of the stack 2. This barrier 24 has no effect on the colors of the face 4. For this purpose, the thickness of this barrier 24 is very thin, i.e. less than 5 nm. For example, the barrier 24 is made of silicon dioxide and its thickness is between 1 nm and 2.5 nm.

[0071] The substrate 10 serves as a support and has no impact on the colors of the face 4 since the layer 20 cannot be crossed by light. For example, the substrate 10 is made of silicon. The thickness of the substrate 10 is typically greater than 500 μm or 700 μm or 1 mm. A thin adhesion layer is generally provided between the substrate 10 and the layer 20 to increase the adhesion of the layer 20 on the substrate 10. For example, this adhesion layer is made of chromium and its thickness is equal to 5 nm.

[0072] To manufacture the stack 2, the different layers are deposited, on the substrate 10, one on top of the other, by an electron beam deposition process. For example, a deposition machine marketed under the name “SYRUSpro 710” from the company Buhler-Leybold Optics® is used. During deposition, a vacuum of approximately 5x107 mbar is created. The deposition rate used for the metal layers is 0.1 nm / s and the deposition rate for the other layers is 0.2 nm / s.

[0073] After the stack is manufactured, the PCM material is entirely in its amorphous phase. When the thicknesses eM, ei6, ei8 and e22 are equal to, respectively, 350 nm, 10 nm, 25 nm and 24 nm, the hue of face 4 is then bright magenta. Here, the hues of face 4 are all observed in visible light in an observation direction perpendicular to face 4. It is emphasized that the hue of face 4 varies depending on the angle between the direction normal to face 4 and the observation direction.

[0074] Then, to obtain different crystallization states of the layer 22, the manufactured stack 2 is heated to a temperature T between the temperatures Te and Tm for a duration ATc before being cooled. Here, to heat the stack 2, the latter is deposited on a plate heated to 300°C. To cool stack 2, it is simply removed from the heating plate and allowed to cool to room temperature. Under these conditions, for an ATc duration of 2 min, layer 22 is completely crystallized. The color of face 4 is then pale green. For an ATc duration of 30 s, layer 22 is only partially crystallized. The color of face 4 is then blue.

[0075] This embodiment makes it possible to achieve a difference between the shades of face 4 obtained when layer 22 is entirely in amorphous phase and when layer 22 is entirely in crystalline phase, greater than 50° or 60°. Here, the maximum difference achieved is approximately 65°.

[0076] Further tests were performed using a laser pulse directed at face 4 to heat the PCM material. For illustration purposes, the laser pulse used is a laser pulse generated using a femtosecond laser. The pulse duration is 150 fs and its wavelength is 515 nm. The energy of each pulse was adjusted to avoid damaging the stack. The laser pulses were repeated for 10 s at a frequency of approximately 1 MHz. At the point of impact of the laser pulse, the color of face 4 is pale green. Immediately around this point of impact, the color is blue. Finally, the areas of face 4 far from the point of impact remained magenta.

[0077] [Fig. 2] represents a stack 32 identical to stack 2 except that the titanium mirror 16 is replaced by a silver mirror 36 to amplify the difference in shades between the completely amorphous phase and the completely crystalline phase of layer 22. For example, the thickness of the silver metal layer is identical to the thickness of the titanium metal layer of stack 2. This embodiment makes it possible to achieve a difference between the shades of face 4 when layer 22 is entirely in the amorphous phase and when layer 22 is entirely in the crystalline phase, greater than 70° or 80°. For example, here, the maximum difference achieved is approximately 93°.

[0078] [Fig.3] represents a stack 52 identical to stack 2 except that:

[0079] - the substrate 10 is replaced by a substrate 54 made of transparent material,

[0080] - the lower reflecting mirror 12 is replaced by a lower mirror 56 by highly reflective, and

[0081] - the partially reflecting upper mirror 16 is replaced by a reflected mirror chissant 58.

[0082] The substrate 54 is, for example, made of glass such as the glass known as “B270® glass”.

[0083] Mirror 56 is identical to mirror 12 except that metal layer 20 is replaced by a thinner metal layer 60 so that mirror 56 is by partially reflective. For example, metal layer 60 is identical to metal layer 16 or 36.

[0084] Mirror 58 is identical to mirror 16 or 36 except that the metal layer is thicker. For example, the thickness of the metal layer of mirror 58 is greater than 50 nm or 100 nm.

[0085] In the case of stack 52, the light enters the optical cavity by passing through substrate 54 and mirror 56. The tinted face 4 is then the lower face of substrate 54. In this case, substrate 54 is used both as a substrate and to protect mirror 56.

[0086] Chapter III: Variants:

[0087] Lower mirror variant:

[0088] Alternatively, the lower and upper mirrors are both partially reflective and therefore allow at least 5% or 10% of the incident light to pass through.

[0089] The metal layer 20 can be made of one of the following metals or of an alloy of these metals: Au, Pt, Al, Cu, Ti and Ag.

[0090] The layer 22 of PCM material can be made using phase change materials other than Sb2S3. For example, the phase change material is chosen from the group consisting of the following phase change materials and their alloys: Sb2S3, GeTe, Ge2Sb2Te5, GeSe2, Sb2Te3, Bi2Te3, Sb2Se3, VO2. The phase change material can also be doped.

[0091] The layer of PCM material may be formed from a superposition of several sub-layers each made from a respective phase change material. For example, the layer of phase change material may be formed from a sub-layer of GeTe or Sb2Te3 and a sub-layer of Sb2S3. By applying an appropriate heat treatment, the phase of each of these sub-layers may be controlled independently of the phase of the other sub-layers. This makes it possible to further increase the number of possible shades for face 4 obtained in response to a heat treatment.

[0092] Other materials can be used to form the diffusion barrier 24. For example, the barrier 24 is made of Si3N4 and its thickness is 5 nm.

[0093] Other variants:

[0094] The substrate 10 may be made of other materials such as glass (silica) or polymer. In the case of a polymer substrate, the substrate may then be flexible.

[0095] The adhesion layer between the substrate 10 and the layer 20 may be made of another material or omitted.

[0096] Other materials are possible for the transparent layer 14. For example, as a variant, the transparent layer is made of Nb2O5, TiO2, HfO2, Ta2O5 or even ITO (Indium Tin Oxide). LTTO is a material that is both transparent in the visible and electrically conductive domain. Thus, in this case, the transparent layer can also be used as an electrode for conducting an electrical pulse used to heat the PCM material. In such a case, the metal layer 20 or 60 is, for example, used to form the other electrode. Under these conditions, the stack described here can be used to form the pixels of a screen. For example, the arrangement of these pixels is identical to one of those described in application WO2017215363.

[0097] The transparent layer 14 can also be formed by a stack of several sub-layers each in a respective transparent material.

[0098] The metal layer of the upper mirror 16 or 36 or 58 can be made of one of the following metals or an alloy of these metals: Au, Pt, Al, Cu, Ti and Ag.

[0099] In a simplified variant, the surface layer 18 is omitted.

[0100] It is also possible to add barrier layers between the layers described above. Such barrier layers can be used to improve the adhesion of the layers to each other, to avoid diffusion phenomena between materials. On the other hand, these barrier layers do not have a significant impact on the optical properties of the stack. Indeed, their thicknesses are always very low, i.e. less than 5 nm or even less than 1 nm. For example, such barrier layers can be made from one of the following materials: Cr, MgO or others.

[0101] Several of the variants described above can be combined in the same embodiment.

[0102] Chapter IV: Advantages of the described embodiments:

[0103] Placing the layer of PCM material between the metal layer 20 or 60 and the transparent layer 14 makes it possible to obtain greater variations in shades between the amorphous phase and the crystalline phase of the PCM material. In particular, the variations in shades obtained are greater than when the PCM material is used to form the transparent layer or the upper mirror. Furthermore, this increase in the difference between the shades obtained is not achieved at the expense of the possibility of having a very large number of different shades by varying the thicknesses of the layer 22 of PCM material and the transparent layer 14.

[0104] The fact that the PCM material is Sb2S3 makes it possible to obtain an even greater number of different shades than with other PCM materials.

[0105] Choosing the thickness of the Sb2S3 layer between 10 nm and 50 nm makes it possible to further increase the difference between the shades obtained with the amorphous and crystalline phases, respectively.

[0106] Making the upper mirror silver increases the brightness and color saturation. This also further increases the difference between the shades corresponding, respectively, to the amorphous and crystalline phases of the PCM material.

Claims

Claims

1. Stack of layers whose color, in the visible range, changes in response to a heat treatment, this stack comprising in order: - a lower mirror (12; 56) comprising a metallic layer (20; 60), - a transparent layer (14) composed of one or more dielectric materials transparent in the visible range, the thickness of this transparent layer being greater than 10 nm, and - an upper mirror (16;58), at least one of the lower and upper mirrors being partially reflective, one of the mirrors and the transparent layer comprising a layer (22) made of a phase change material whose thickness is between 10 nm and 250 nm, and the difference between the real parts of the refractive indices of the phase change material and the transparent layer is greater than 0.2, characterized in that the layer (22) of phase change material is located in the lower mirror above the metal layer and forms the face of the lower mirror in contact with the transparent layer.;

2. Stack according to claim 1, wherein the phase change material is a material selected from the group consisting of the following materials and their alloy: Sb2S3, GeTe, Ge2Sb2Te5, GeSe2, Sb2Te3, Bi2Te3, Sb2Se3, VO2.

3. Stack according to claim 2, in which the phase change material is antimony trisulfide of chemical formula Sb2S3.

4. Stack according to claim 3, in which the thickness of the layer (22) of phase change material is between 10 nm and 50 nm.

5. A stack according to any preceding claim, wherein the upper mirror (16) comprises a silver metal layer.

6. Stack according to any one of claims 1 to 4, in which the upper mirror (36) comprises a titanium metal layer.

7. Stack according to claim 5 or 6, in which the thickness of the metal layer of the upper mirror (16; 36) is between 3 nm and 40 nm.

8. Stack according to any one of the preceding claims, in which the thickness of the metal layer (20) of the lower mirror (12) is greater than 50 nm.

9. Stack according to any one of the preceding claims, in which the difference between the hues of the stack when the layer (22) of phase change material is entirely in an amorphous phase and when the layer of phase change material is entirely in a crystalline phase, is greater, in absolute value, than 50° when this difference is measured using a color wheel where the primary red is at 0°, the primary green is at 120°, the primary blue is at 240°, and the mixtures, at intermediate angles, in proportion to the two primaries which compose them.

10. Stack according to any one of the preceding claims, in which the stack comprises a transparent surface layer (18) deposited on the upper mirror on the side opposite the transparent layer interposed between the lower and upper mirrors.

11. Method of manufacturing a stack according to any one of the preceding claims, characterized in that the different layers of the stack are deposited, on a substrate (10), one on top of the other, by an electron gun evaporation process.

Citation Information

Patent Citations

  • Display device based on phase change material

    WO2017215363A1

  • A light modulation device with dynamic color display based on phase change materials and its fabrication method

    CN107942540B

  • Double-wave dynamic thermal camouflage structure and optimization method thereof

    CN116088077A

  • An optical device for forming a distribution of a three-dimensional light field

    EP3521912A1

  • display

    US20200409228A1