Zeolite, method for producing the zeolite, and catalyst including the zeolite

JP2022089155A5Active Publication Date: 2024-10-07JGC CATALYSTS & CHEMICALS LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021167398
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-12-03
Filing Date
2021-10-12
Publication Date
2024-10-07
Estimated Expiration
2041-10-12

AI Technical Summary

Technical Problem

Conventional fluid catalytic cracking catalysts fail to maintain sufficient activity in the presence of increasing vanadium and nickel in residual oil, leading to reduced performance and increased hydrogen, gas, and coke production.

Method used

A fluid catalytic cracking catalyst containing a specific faujasite-type zeolite with a peak area ratio of hexacoordinated Al to tetracoordinated Al in the range of 0.20 to 0.40, and ammonia desorption in the range of 1.0 to 2.5 mmol/g, along with ultra-stable Y-type zeolite having a lattice constant of 24.40 to 24.60 Å, is developed to enhance cracking performance and resistance to metal poisoning.

Benefits of technology

The catalyst exhibits high cracking activity, low hydrogen and coke production, and high yield of gasoline and kerosene fractions, with excellent hydrothermal stability and resistance to metal poisoning, suitable for petroleum refining and petrochemical applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a zeolite suitable for catalysts, for example, a fluid catalytic cracking catalyst.SOLUTION: A zeolite for a fluid catalytic cracking catalyst has following characteristics. (a) It is a faujasite zeolite. (b) As measured for alumina by solid NMR, a peak area ratio between a peak area (P4Al) of spectrum of 4-coordinated Al and a peak area (P6Al) of spectrum of 6-coordinated Al, (P6Al) / (P4Al), is 0.20-0.40. (c) As measured by ammonia temperature-programmed desorption method (NH3-TPD method), the amount of ammonia desorption is 1.0-2.5 mmol / g. There is also provided a catalyst including the zeolite. There is also provided a production method that includes subjecting zeolite to acid treatment in the presence of ammonium salt for solid-liquid separation, to obtain zeolite cake; and obtaining zeolite from the zeolite cake.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a zeolite suitable for use as a component or adsorbent in catalysts used in petroleum refining and petrochemical fields, a method for producing the same, and a catalyst using the zeolite. [Background technology]

[0002] In recent years, the petroleum refining industry has seen an increase in the use of heavy hydrocarbon oils, such as residual oil, as feedstocks for catalytic cracking. In particular, there is a demand for catalysts that can be used in the catalytic cracking of heavy hydrocarbon oils such as residual oil, possess metal resistance to vanadium and nickel, have excellent residual oil decomposition capabilities, produce low levels of hydrogen and coke, and yield high yields of gasoline and kerosene fractions (LCO).

[0003] To some extent, solutions to these problems have been proposed through process improvements and the development of fluid catalytic cracking catalysts (hereinafter also simply referred to as FCC catalysts).

[0004] Patent Document 1 discloses a catalytic cracking catalyst characterized by a faujasite-type zeolite with a silica-to-carbon ratio of 6 or more, a Na2O content of 0.5% by weight or less, and 25 or more aluminum atoms in the framework (4-coordinate). It has been reported that the catalytic cracking catalyst disclosed in Patent Document 1 maintains a stable crystal structure even after high-temperature steam treatment, does not impair the intrinsic catalytic cracking reaction activity of the zeolite, and exhibits excellent hydrothermal resistance.

[0005] Furthermore, Patent Document 2 discloses an ultrastable Y-type zeolite (USY zeolite) in which the pore volume is controlled in the range of pore diameter 3.5 to 5 nm. The ultrastable Y-type zeolite described in Patent Document 2 has a unit cell constant (UD) of 24.55 Å or less, an SiO2 / Al2O3 (molar ratio) of 8 or more, and a specific surface area of ​​400 to 900 m². 2 It has been reported that it has a crystallinity of 95% or higher and can be used for the hydrocracking of hydrocarbon oils such as diesel fuel and residual oil.

[0006] Furthermore, Patent Document 3 discloses a Y-type zeolite in which aluminum is reinserted into the skeletal structure of a dealuminized Y-type zeolite. The Y-type zeolite disclosed in Patent Document 3 is characterized by a unit cell constant (UD) of 24.25 to 24.60 Å, a certain degree of crystallinity, specific surface area, and pore size, and a proportion of 60% or more of aluminum atoms in the framework (4-coordinate), and has been reported to exhibit excellent performance.

[0007] Patent Document 4 discloses a method for producing a high-octane gasoline fraction by contacting a highly aromatic hydrocarbon oil raw material with a hydrocracking catalyst. The hydrocracking catalyst disclosed in Patent Document 4 is a catalyst that uses a refractory support containing a specific ultrastable Y-type zeolite, characterized in that the unit cell constant (UD) of the UYS zeolite is 24.40 Å or less, the SiO2 / Al2O3 (molar ratio) is 25 or more, and the crystallinity is 50% or more. Patent Document 4 reports that UYS zeolite is effective as a hydrocracking catalyst for the production of gasoline fractions.

[0008] Patent Document 5 discloses a faujasite-type zeolite and a hydrocarbon catalytic cracking catalyst containing the faujasite-type zeolite. Patent Document 5 also reports a catalytic cracking catalyst characterized by a faujasite-type zeolite having an SiO2 / Al2O3 (molar ratio) of 4 to 8, a peak area ratio of 0.4 to 1.0 between outer (6-coordinate) aluminum and inner (4-coordinate) aluminum in solid-state NMR, and a lattice constant in the range of 24.40 to 24.65 Å. [Prior art documents] [Patent Documents]

[0009] [Patent Document 1] Japanese Patent Application Publication No. 09-038499 [Patent Document 2] Japanese Patent Publication No. 2003-095643 [Patent Document 3] Japanese Patent Publication No. 2006-150183 [Patent Document 4] Japanese Patent Publication No. 2010-215736 [Patent Document 5] Japanese Patent Publication No. 2012-140287 [Overview of the Initiative] [Problems that the invention aims to solve]

[0010] In the future, the content of vanadium and nickel, which are toxic substances contained in residual oil, is expected to increase further. Under these conditions, there is a need for fluid catalytic cracking catalysts that can maintain their activity in decomposing residual oil. Conventional fluid catalytic cracking catalysts have the problem of not being able to obtain sufficient activity.

[0011] The object of the present invention is to provide a zeolite suitable for use as a component or adsorbent in catalysts used in petroleum refining and petrochemical fields, a method for producing the zeolite, and a catalyst containing the zeolite. In particular, the present invention aims to provide a zeolite suitable for use in fluid catalytic cracking catalysts. [Means for solving the problem]

[0012] Against this technical backdrop, the inventors diligently researched ways to improve fluid catalytic cracking catalysts (hereinafter also simply referred to as "FCC catalysts") that exhibit excellent decomposition properties for heavy fractions (bottoms). As a result, they discovered that fluid catalytic cracking catalysts containing a specific faujasite-type zeolite exhibit significantly superior hydrothermal stability and resistance to metal toxicity in decomposing heavy fractions (bottoms), thus completing the present invention.

[0013] The zeolite according to the present invention is It has the following characteristics (a) to (c). (a) It is a faujasite-type zeolite. (b) Peak area of ​​the spectrum of 4-coordinate Al measured by solid-state NMR of alumina (P 4Al ) and the peak area of ​​the spectrum of 6-coordinate Al (P 6Al ) Peak area ratio (P 6Al ) / (P 4Al ) is in the range of 0.20 to 0.40. (c) The amount of ammonia desorbed measured by the ammonia temperature-programmed desorption method (NH3-TPD method) is in the range of 1.0 to 2.5 mmol / g.

[0014] Regarding the zeolite according to the present invention, (a) The faujasite-type zeolite is ultrastable Y-type zeolite (USY), (i) The faujasite-type zeolite has a lattice constant of the zeolite in the range of 24.40 to 24.60 Å, etc. can be considered as more preferable solution means.

[0015] Further, the method for producing the zeolite according to the present invention is a method for producing any of the above zeolites, and (1) A first step of preparing zeolite, (2) A second step of obtaining a zeolite cake by subjecting the zeolite to acid treatment in the presence of an ammonium salt and then performing solid-liquid separation, <所 (3) A third step of obtaining zeolite from the zeolite cake, and includes the above.

[0016] Further, the catalyst according to the present invention contains any of the above zeolites.

Effects of the Invention

[0017] As described above, according to the zeolite obtained in the present invention and its production method, when used as a catalyst, particularly as a fluid catalytic cracking catalyst, it has excellent decomposability of heavy fractions (bottoms), high decomposition activity, and moreover, less generation of hydrogen, gas and coke, and gasoline and light gas oil fractions can be obtained in high yields, and a fluid catalytic cracking catalyst excellent in hydrothermal stability and metal poisoning resistance can be provided. Further, the zeolite of the present invention can be used, for example, as a constituent component of a catalyst used in the petroleum refining and petrochemical fields, and also as an adsorbent.

Modes for Carrying Out the Invention

[0018] The zeolite of the present invention was first developed for use as a fluid catalytic cracking catalyst.

[0019] As a fluid catalytic cracking (FCC) catalyst for hydrocarbons, catalyst compositions are conventionally known in which a porous inorganic oxide, such as silica-alumina, silica-zirconia, silica-magnesia, and further silica-clay, is used as a matrix and fine zeolite is dispersed and contained therein. However, generally, in this type of catalyst composition, there is a risk that the pores of the zeolite are encapsulated by the matrix component, particularly by the silica component in the matrix, and when this encapsulation occurs, the performance as a catalyst may be significantly reduced.

[0020] <Zeolite> The present invention provides a fluid catalytic cracking catalyst excellent in cracking activity, gasoline selectivity, hydrothermal stability, and metal poisoning resistance by a zeolite dispersed in a matrix. That is, the FCC catalyst according to the present invention contains a specific faujasite-type zeolite in a dispersed state.

[0021] The zeolite used in the present invention is a faujasite-type zeolite, and particularly, ultrastable Y-type zeolite (USY) is suitable because of its excellent hydrothermal stability.

[0022] The USY zeolite of the present invention contains 6-coordinate Al atoms in a specific ratio together with 4-coordinate Al atoms in the framework. The present inventors define the ratio of such 4-coordinate Al atoms and 6-coordinate Al atoms by the ratio of the peak areas using solid NMR.

[0023] That is, the peak area (P 4Al ) of the spectrum of 4-coordinate Al measured by solid NMR of alumina in the USY zeolite of the present invention and the peak area (P 6Al ) of the spectrum of 6-coordinate Al, and the peak area ratio (P 6Al ) / (P 4AlThe ratio must be in the range of 0.20 to 0.40. If the peak area ratio is smaller than the lower limit of the ratio, the metal resistance and water and heat resistance may be insufficient, and if the peak area ratio exceeds the upper limit, it means that there is a small amount of 4-coordinate Al (Al atoms in the skeleton), which may result in insufficient activity.

[0024] In this invention, the coordination state of aluminum present in the zeolite was determined using a solid-state high-resolution NMR (Nuclear Magnetic Resonance) spectrometer (Agilent VNS-600). 27 Al MAS (Magic Angle Spinning) NMR spectra were measured at room temperature under the following conditions: resonance frequency 156.29 MHz, spin velocity 20 kHz, waiting time 0.1 sec, and number of integrations 128 times. Prior to measurement, the samples were placed in a desiccator containing saturated NH4Cl water vapor for more than 24 hours to allow sufficient water adsorption. Aluminum nitrate nonahydrate (Al(NO3)3·9H2O) was used as an external standard.

[0025] The composition of the zeolite was analyzed using a glass bead method with an X-ray fluorescence analyzer (PHILIPS MagiX PRO). The lattice constant of the zeolite was measured using a powder X-ray diffractometer (Rigaku Corporation: RINT-2100). Using Cu-Kα rays, the lattice constant was calculated under conditions of a tube voltage of 30kV and a tube current of 14mA. The lattice constant of the USY zeolite of the present invention is preferably in the range of 24.40 to 24.60 Å. A lattice constant within this range results in a large amount of solid acid and high activity. If the lattice constant is too high, the water and metal resistance may be insufficient, and if the lattice constant is too low, the amount of solid acid may be small and the activity may be insufficient.

[0026] Specific surface area was measured by pre-treating sample powders at 500°C for 1 hour under an inert gas atmosphere, and measuring the amount of N2 adsorbed and desorbed using a MacSorb-1220 manufactured by Mountec. The specific surface area was calculated from the amount of N2 desorbed based on the BET one-point method.

[0027] The amount of ammonia desorbed was measured by the ammonia thermal desorption method (NH3-TPD method). Specifically, using a BELCAT-B® manufactured by Microtrac-Bel, 0.2g of the sample was placed in the measurement cell, exhaust treatment was performed at 500°C for 1 hour, then the temperature was reduced to 100°C, and ammonia gas was introduced at 100°C for 0.5 hours for adsorption. Next, exhaust treatment was performed again at 100°C for 0.5 hours, and then, under a flow of 50 ml of He gas per minute, the temperature was increased from 100°C to 700°C at a rate of 10°C per minute, and the amount of ammonia desorbed with increasing temperature was measured. The amount of ammonia desorbed needs to be in the range of 1.0 to 2.5 mmol / g. If the amount of ammonia desorbed is below the lower limit, the decomposition activity is insufficient, while if it exceeds the upper limit, the amount of coke formation increases and gasoline selectivity may decrease.

[0028] In addition to the above-mentioned fluid catalytic cracking applications, the zeolite of the present invention can be used, for example, as a component of catalysts used in catalytic cracking and hydrogenation treatments in petroleum refining and petrochemical fields, and as an adsorbent for separating organic substances in molecular sieves, gas phases, or liquid phases.

[0029] <Method for manufacturing zeolite> (1) The first step of preparing the zeolite Conventional NaY-type zeolites can be used as the NaY-type zeolite. The SiO2 / Al2O3 molar ratio of the NaY-type zeolite used in this invention is preferably in the range of 3 to 6, and more preferably in the range of 4 to 6.

[0030] Ammonium ion exchange involves dispersing NaY-type zeolite in an aqueous ammonium salt solution to obtain NH4Y-type zeolite. This can be done using conventionally known methods. Preferably, the amount of ammonium salt used is 0.6 to 3 moles, and more preferably 1 to 2 moles, per mole of NaY-type zeolite (Na2O·Al2O3·nSiO2: n is the SiO2 / Al2O3 molar ratio). If the amount of ammonium salt used is too small, the predetermined ion exchange rate cannot be achieved, and a large amount of Na remains, which may significantly reduce the crystallinity of the NH4Y-type zeolite in subsequent steps. There are no particular restrictions on the temperature during ion exchange, but it is preferably in the range of room temperature to 100°C, and more preferably 50 to 95°C.

[0031] NH4Y type zeolite can be heat-treated at 550-750°C using conventionally known methods. For example, a muffle furnace or rotary kiln can be used. Steam may also be supplied during heating, or NH4Y type zeolite containing moisture may be used beforehand. The lattice constant can be adjusted by heat treatment in the presence of steam.

[0032] (2) Second step: To obtain a zeolite cake, the zeolite is acid-treated in the presence of an ammonium salt, followed by solid-liquid separation. Heat-treated zeolite can be treated with an acid solution at a temperature of 40-100°C to remove extraskeletal aluminum. The acid solution used in this process is an acid-containing solution, including conventionally known inorganic acids such as sulfuric acid, hydrochloric acid, and nitric acid. Alternatively, any acid capable of removing extraskeletal aluminum, such as organic acids like citric acid or acetic acid, may be used.

[0033] In this process, a salt containing ammonium ions may be added to the acid solution. When acid treatment is performed using an acid solution containing ammonium ions in this way, the countercation of aluminum, Na, is formed. + It becomes easier to remove.

[0034] After acid treatment, the acid solution and zeolite can be separated into solid and liquid components by methods such as filtration to obtain a zeolite cake. Since components derived from the acid solution may remain in the separated zeolite, it is preferable to perform a washing treatment such as resuspending the separated zeolite in water or pouring warm water over it on a filter cloth.

[0035] Furthermore, since the filtrate contains dissolved aluminosilicate, the solid components may be flocculated and recovered from the viewpoint of yield and performance. A flocculant is added to the filtrate to obtain a precipitate containing dissolved aluminosilicate. The recovered dissolved aluminosilicate is separated into solid and liquid components by methods such as filtration, and then washed by methods such as suspending it in water again or pouring warm water over a filter cloth to obtain a dissolved aluminosilicate cake. Alternatively, when obtaining the dissolved aluminosilicate cake, a device that concentrates and settles the slurry, such as a thickener, may be used. For example, a thickener can be used as a practical device to concentrate and settle the filtrate with a flocculant added, and then mix it directly into a filtration device such as an Oliver filter for washing.

[0036] The flocculant is preferably an inorganic flocculant such as polyaluminum chloride or polyferric sulfate, or an organic polymer flocculant such as polyacrylic acid ester or polyacrylamide, and both may be used in combination. At least one of the following types of organic polymer flocculants can be used: cationic, anionic, nonionic, or amphoteric.

[0037] (3) Third step of obtaining zeolite from the zeolite cake The zeolite cake can be dried at a temperature of 80°C to 400°C to obtain zeolite. Furthermore, if necessary, this zeolite may be baked in an air atmosphere at a temperature of 400°C to 900°C.

[0038] The catalyst containing the zeolite of the present invention will be explained using a fluid catalytic cracking catalyst as an example. - Fluid catalytic cracking catalyst - The fluid catalytic cracking catalyst according to the present invention comprises a matrix containing a binder component containing silica or alumina and the zeolite prepared above (hereinafter also simply referred to as zeolite), and an additive containing at least one selected from activated alumina and a metal scavenger, and may further contain rare earth metal oxides. These zeolites are used in a form that has been ion-exchanged with cations selected from hydrogen, ammonium, and polyvalent metals, as is the case when used in ordinary catalytic cracking catalysts.

[0039] As precursors for rare earth metal oxides in the present invention, commercially available rare earth metal carbonates, hydrochlorides, nitrates, oxalates, etc., can be used.

[0040] The fluid catalytic cracking catalyst according to the present invention uses a porous inorganic oxide matrix, similar to conventional catalytic cracking catalysts. The porous inorganic oxide matrix can be silicates such as sodium silicate, silica-based binders such as silica sol, or alumina-based binders such as basic aluminum chloride, alumina sol, or alumina gel. Furthermore, additives such as clay minerals like kaolin, halloysite, and montmorillonite, solid acid-containing matrices such as activated alumina, silica-alumina, silica-magnesia, alumina-magnesia, and silica-magnesia-alumina, and metal scavengers such as manganese dioxide, calcium aluminate, aluminum hydroxide, and rare earth metal oxides (e.g., lanthanum carbonate) can be used in combination.

[0041] The fluid catalytic cracking catalyst of the present invention is characterized in that the zeolite and preferably the rare earth metal oxide are dispersed in the porous inorganic oxide matrix. In the fluid catalytic cracking catalyst, the zeolite is preferably contained in an amount of 5 to 50% by mass, more preferably 10 to 40% by mass, based on the catalyst. Furthermore, if the rare earth metal oxide is included, it is preferably contained in an amount of 0.5% by mass or more, preferably 0.8% by mass or more, more preferably 1.0% by mass or more, on an oxide basis (RE2O3) based on the catalyst, with a maximum of 20% by mass or less, preferably 18% by mass or less, and more preferably 15% by mass or less, and is uniformly dispersed in the porous inorganic oxide matrix.

[0042] If the zeolite content is less than 5% by mass, the decomposition activity of the resulting catalyst may be low. On the other hand, if it is more than 50% by mass, the decomposition activity may be too high, increasing the production of hydrogen, gas, and coke, which may result in a low gasoline yield. Furthermore, if the content of the rare earth metal oxide precursor is less than 0.5% by mass as RE2O3, the desired effect cannot be obtained. On the other hand, if it is more than 20% by mass, the wear resistance (Attr.Res.) of the catalyst composition may decrease. In addition, it is desirable that the fluid catalytic cracking catalyst contains the aforementioned porous inorganic oxide matrix in the range of 30 to 90% by mass, preferably 30 to 85% by mass. The content of each component of the catalyst composition is determined within its respective range so that the total is 100% by mass.

[0043] — Method for producing fluid catalytic cracking catalysts — The aforementioned fluid catalytic cracking catalyst will be explained using, as an example, a method of production in which a mixture slurry obtained by uniformly dispersing the aforementioned porous inorganic oxide matrix precursor, basic aluminum chloride, with the zeolite, is spray-dried and washed in the following steps. If a silica-based binder is used, the conditions may differ; in such cases, this will be indicated in parentheses.

[0044] <Mixed Slurry Acquisition Process> The mixed slurry acquisition step involves obtaining a mixed slurry containing a matrix comprising a binder component and zeolite, and an additive comprising at least one selected from activated alumina and a metal scavenger. The resulting mixed slurry is preferably adjusted to a solid content concentration of 25 to 50% by mass in order to be suitable for the subsequent spray drying process. If the solid content concentration is less than 25% by mass, the bulk density of the catalyst decreases and its wear resistance deteriorates, and if it exceeds 50% by mass, the viscosity of the mixed slurry increases, which may make spray drying difficult.

[0045] <Precursor acquisition process> The precursor acquisition step involves obtaining a precursor for a fluid catalytic cracking catalyst by spray-drying the mixed slurry obtained in the mixed slurry acquisition step. In this process, the spray drying conditions are preferably such that the spray outlet temperature is in the range of 200 to 250°C (155 to 215°C when using a silica-based binder). If the outlet temperature is below 200°C, it becomes difficult to maintain the particle shape after washing the catalyst, and the abrasion resistance deteriorates. On the other hand, if the temperature exceeds 250°C, although the particle shape can be maintained after washing, the drying rate becomes faster, making the catalyst particles more prone to cracking, which may actually worsen the abrasion resistance.

[0046] <Process for obtaining washed cake 1> The precursor of the fluid catalytic cracking catalyst obtained in the precursor acquisition step is suspended in an aqueous solution with a pH in the range of 5.5 to 7.5 (2.5 to 3.5 when a silica-based binder is used) at 40 to 70°C, filtered, and if necessary, further washed with hot water and filtered to obtain washed cake 1. This step is called the washed cake 1 acquisition step. In this process, the aqueous solution used for suspension is preferably an aqueous solution containing sodium carbonate, sodium bicarbonate, and sodium hydroxide salts, and it is preferable to adjust the pH of the aqueous solution to be within a desired range. In the case of sodium hydroxide, it is preferable to use ammonium sulfate at the same time.

[0047] If the aqueous solution temperature is below 40°C, the amount of residual chlorine derived from the binder components increases, which is likely to corrode the fluid catalytic cracking apparatus. On the other hand, if the temperature is above 70°C, hydrolysis of the binder components is more likely to occur, which may worsen wear resistance. (When using silica-based binders, there is no particular need to limit the temperature of the aqueous solution during cleaning, but it is preferable to do so in the range of 50 to 70°C.)

[0048] Furthermore, from the viewpoint of soluble impurities and filterability, the ratio of solid content to aqueous solution of the precursor during washing is preferably in the range of solid content / aqueous solution = 1 / 3 to 1 / 15 by mass ratio.

[0049] <Process for obtaining washed cake 2> The process of obtaining washing cake 2 involves drying the washing cake 1 obtained in the washing cake 1 acquisition process to obtain washing cake 2. Before drying, it is preferable to suspend the cake in water, and if necessary, add and stir an aqueous solution containing a rare earth element RE2O3 precursor, filter it, and then wash it with hot water.

[0050] <Heat drying process> The heating and drying step involves heating the washed cake 2 obtained in the washing cake 2 acquisition step in a general manner, such as in a dryer, muffle furnace, or rotary kiln, in a temperature range of 80 to 600°C to obtain the fluid catalytic cracking catalyst of the present invention. This step may also be carried out under any conditions, such as air or steam. Below 80°C, drying may be insufficient, potentially degrading the physical properties and performance of the catalyst during use. On the other hand, above 600°C, performance may decrease due to aggregation of the active components.

[0051] The fluid catalytic cracking catalyst of the present invention can be used in conventional hydrocarbon oil fluid catalytic cracking methods, and conventional fluid catalytic cracking conditions can be employed. Furthermore, the catalyst composition of the present invention can be used in the fluid catalytic cracking of any conventional hydrocarbon oil feedstock, but it has excellent hydrothermal resistance and is particularly suitable for the fluid catalytic cracking of heavy hydrocarbon oils containing nickel, vanadium, etc.

[0052] In addition to being a fluid catalytic cracking catalyst as described above, the zeolite of the present invention can also be suitably used as a catalyst for petroleum refining, such as for hydrocracking and isomerization, as a catalyst for petrochemical synthesis of xylene, ethylbenzene, cumene, etc., and as a catalyst for fine chemical synthesis. [Examples]

[0053] The present invention will be explained in detail below with reference to examples, but the present invention is not limited to these examples. (Example 1) Preparation of ultra-stabilized Y-type zeolite No. 1 As a NaY-type zeolite, it has a molar ratio of 5.2 for SiO2 / Al2O3, a lattice constant of 2.466 nm, and a specific surface area of ​​720 m². 2 A NaY-type zeolite with a Na content of 13.0% by mass (calculated as Na2O) was used. 50.0 kg of NaY-type zeolite was added to 500 L of 60°C hot water, and then 14.0 kg of ammonium sulfate was added to obtain a suspension. This suspension was stirred at 70°C for 1 hour and filtered. The solid obtained by filtration was washed with 60°C hot water. Next, this solid was washed with an ammonium sulfate solution prepared by dissolving 14.0 kg of ammonium sulfate in 500 L of 60°C hot water, and then washed again with 500 L of 60°C water to obtain a washed cake. The obtained washed cake was dried at 130°C for 20 hours, and approximately 65% ​​by mass of the Na contained in the NaY-type zeolite was converted into ammonium ions (NH4). + Y-type zeolite (NH4Y) was obtained by ion exchange using ). The Na content of this NH4Y-type zeolite was 4.5% by mass in terms of Na2O (first step).

[0054] 40 kg of this NH4Y type zeolite was calcined at 670°C for 1 hour in a saturated steam atmosphere. The resulting calcined powder was added to 400 L of 60°C hot water, the pH was adjusted to 2.5-4.5 with 25% sulfuric acid, then 49.0 kg of ammonium sulfate was added, and the mixture was stirred at 90°C for 1 hour. The resulting slurry was filtered and then washed with 200 L of 60°C hot water to obtain a washed cake (1) (second step). The obtained washed cake (1) was added to 400 L of 60°C hot water and stirred at 60°C for 10 minutes. The obtained slurry was filtered and then washed with 200 L of 60°C hot water to obtain washed cake (2). Next, washed cake (2) was dried at 130°C for 20 hours to obtain super-stabilized Y-type (hereinafter referred to as "USY") zeolite No. 1 (third step). The properties of USY zeolite No. 1 are shown in Table 1. In this example, the process was carried out using a flocculant with the intention of improving the yield. However, when the flocculant was not used, although a decrease in yield was observed, it was confirmed that there was almost no difference in the physical properties of the resulting zeolite.

[0055] Preparation of fluid catalytic cracking catalyst No. 1 For the fluid catalytic cracking catalyst, USY's zeolite No. 1 was further calcined at 830°C for 30 minutes. To this, water glass (No. 3 water glass adjusted to 17.5% by mass in terms of SiO2) and sulfuric acid (adjusted to a concentration of 25% by mass) were added simultaneously and continuously to prepare a silica hydrosol containing 12.5% ​​by mass of SiO2. To 4000 g of this silica hydrosol, 891.4 g of kaolin (solid content concentration: 85.54% by mass), 580.3 g of activated alumina powder (solid content concentration: 84% by mass), and 2272.7 g of USY zeolite slurry (solid content concentration: 33% by mass), whose pH was adjusted to 3.9 with sulfuric acid, were added to prepare a mixed slurry. This mixed slurry was spray-dried as droplets in a spray dryer with an inlet temperature of 250°C and an outlet temperature of 150°C to obtain dried particles with an average particle size of 70 μm. The obtained spray-dried particles were suspended in 10 times their mass volume of hot water (60°C) and dehydrated by filtration. Next, 10 times their mass volume of hot water (60°C) was poured over them, and they were suspended again and brought into contact with an aqueous solution of rare earth metal chlorides (including cerium and lanthanum chlorides) for ion exchange treatment to achieve 2.0 mass% as RE2O3. The cake was then recovered and dried in a dryer maintained at an ambient temperature of 150°C for 10 hours to obtain fluid catalytic cracking catalyst No. 1. The catalyst composition and catalytic properties of fluid catalytic cracking catalyst No. 1 are shown in Table 2.

[0056] (Example 2) Preparation of ultra-stabilized Y-type zeolite No. 2 USY zeolite No. 2 was obtained in the same manner as in Example 1, except that 40 kg of NH4Y type zeolite obtained in Example 1 was calcined at 590°C for 1 hour in a saturated water vapor atmosphere. The properties of USY zeolite No. 2 are shown in Table 1. Preparation of fluid catalytic cracking catalyst No. 2 Fluid catalytic cracking catalyst No. 2 was obtained in the same manner as in Example 1, except that USY zeolite No. 2 was used as the USY zeolite. The catalyst composition and catalytic properties of fluid catalytic cracking catalyst No. 2 are shown in Table 2.

[0057] (Example 3) Preparation of ultra-stabilized Y-type zeolite No. 3 USY zeolite No. 3 was obtained in the same manner as in Example 1, except that 40 kg of NH4Y type zeolite obtained in Example 1 was calcined at 695°C for 1 hour in a saturated water vapor atmosphere. The properties of USY zeolite No. 3 are shown in Table 1. Preparation of fluid catalytic cracking catalyst No. 3 Fluid catalytic cracking catalyst No. 3 was obtained in the same manner as in Example 1, except that USY zeolite No. 3 was used as the USY zeolite. The catalyst composition and catalytic properties of fluid catalytic cracking catalyst No. 3 are shown in Table 2.

[0058] (Comparative Example 1) Preparation of ultra-stable Y-type zeolite No. R1 The washed cake (1) obtained in Example 1 was dried at 130°C for 20 hours to obtain USY zeolite No. R1. The properties of USY zeolite No. R1 are shown in Table 1. Preparation of fluid catalytic cracking catalyst No. R1 Fluid catalytic cracking catalyst No. R1 was obtained in the same manner as in Example 1, except that USY zeolite No. R1 was used as the USY zeolite. The catalyst composition and catalytic properties of fluid catalytic cracking catalyst No. R1 are shown in Table 2.

[0059] (Comparative Example 2) Preparation of super-stabilized Y-type zeolite No. R2 40 kg of NH4Y-type zeolite obtained in Example 1 was calcined at 500°C for 1 hour in a saturated steam atmosphere. The resulting calcined powder was added to 400 L of 60°C hot water, the pH was adjusted to 2.5-4.5 with 25% sulfuric acid, and then 49.0 kg of ammonium sulfate was added and the mixture was stirred at 90°C for 1 hour. The resulting slurry was filtered and then washed with 200 L of 60°C hot water to obtain a washed cake (4). The washed cake (4) was then dried at 130°C for 20 hours to obtain USY zeolite No. R2. The properties of USY zeolite No. R2 are shown in Table 1. Preparation of fluid catalytic cracking catalyst No. R2 Fluid catalytic cracking catalyst No. R2 was obtained in the same manner as in Example 1, except that USY zeolite No. R2 was used as the USY zeolite. The catalyst composition and catalytic properties of fluid catalytic cracking catalyst No. R2 are shown in Table 2.

[0060] (Comparative Example 3) Preparation of super-stabilized Y-type zeolite No. R3 Similar to Example 1, 40 kg of NH4Y type zeolite was calcined at 670°C for 1 hour in a saturated steam atmosphere. The resulting calcined powder was added to 400 L of 60°C hot water, and then 49.0 kg of ammonium sulfate was added to obtain a suspension. This suspension was stirred at 90°C for 1 hour and filtered. The solid obtained by filtration was washed with 200 L of 60°C hot water. Then, this solid was dried at 130°C for 20 hours. The resulting dried powder was calcined in a saturated steam atmosphere at 750°C for 2 hours to obtain USY zeolite No. R3. The properties of USY zeolite No. R3 are shown in Table 1. Preparation of fluid catalytic cracking catalyst No. R3 Fluid catalytic cracking catalyst No. R3 was obtained in the same manner as in Example 1, except that USY zeolite No. R3 was used as the USY zeolite. However, the additional calcination at 830°C for 30 minutes was omitted. The catalyst composition and catalytic properties of fluid catalytic cracking catalyst No. R3 are shown in Table 2.

[0061] [Catalytic activity evaluation test] For each example of the invention and comparative example, the catalysts were subjected to performance evaluation tests using ACE-MAT (Advanced Cracking Evaluation Micro Activity Test). However, prior to these performance evaluation tests, the catalysts obtained as described above were pre-calcined at an ambient temperature of 600°C for 2 hours. Subsequently, predetermined amounts of nickel octylate and vanadium octylate were deposited onto the calcined catalyst particles. Next, the catalysts were dried at an ambient temperature of 110°C, calcined at an ambient temperature of 600°C for 1.5 hours, and then subjected to heat treatment under various steam atmospheres to simulate equilibrate the catalysts. The pretreatment conditions are shown in Table 3. Condition No. S1 was used as the standard, and conditions No. S2, in which nickel and vanadium were deposited, and condition No. S3, in which the steaming calcination temperature was high, were also used.

[0062] The operating conditions for the activity evaluation test are as follows: Raw materials: Desulfurized atmospheric residue oil (DSAR) + Desulfurized vacuum diesel oil (DSVGO) (50+50) Catalyst / oil flow rate mass ratio (C / O): 5.00 Reaction temperature: 520℃ 1) Conversion rate = 100 - (LCO + HCO) 2) Boiling point range of gasoline: 30~216℃ 3) Boiling point range of LCO: 216~343℃ (LCO: Light Cycle Oil) 4) Boiling point range of HCO: 343°C+ (HCO: Heavy Cycle Oil)

[0063] Table 4 shows the results of metal resistance tests on the catalyst against nickel and vanadium. In all examples, the conversion rate and gasoline yield after metal treatment were higher than in the comparative example, and the retention rate of the conversion rate was also high, so the catalyst can be evaluated as having excellent metal resistance.

[0064] Table 5 shows the results of the water and heat resistance test on the catalysts. In all of the invention examples, the conversion rate was maintained at a higher level than the comparative example even when the steaming firing temperature was increased, and they can be evaluated as catalysts with excellent water and heat resistance.

[0065] Table 1

[0066] Table 2

[0067] Table 3

[0068] Table 4

[0069] Table 5

Claims

1. The peak area (P 4Al ) and the peak area of ​​the spectrum of 6-coordinated Al (P 6Al ) and the peak area ratio (P 6Al ) / (P 4Al ) is in the range of 0.20 to 0.40, Ammonia temperature programmed desorption (NH 3 A faujasite-type zeolite having an ammonia desorption amount measured by a TPD method in the range of 1.0 to 2.5 mmol / g.

2. The faujasite-type zeolite according to claim 1, having a lattice constant in the range of 24.40 to 24.60 Å.

3. A method comprising the steps of: preparing a zeolite; a step of treating the zeolite with an acid in the presence of an ammonium salt, followed by solid-liquid separation to obtain a first zeolite cake; suspending the first zeolite cake in water to obtain a suspension; subjecting the suspension to solid-liquid separation to obtain a second zeolite cake; and drying the second zeolite cake at 80 to 400°C.

4. A catalyst comprising the faujasite-type zeolite described in claim 1.