A heavy oil catalytic cracking catalyst
By using mesoporous rare earth-magnesium-aluminum ternary composite oxide as the catalyst matrix material, combined with zeolite molecular sieve and clay, the shortcomings of the catalyst in heavy oil conversion and heavy metal pollution resistance in heavy oil catalytic cracking are solved, and efficient heavy oil conversion and heavy metal pollution resistance are achieved. Excellent anti-pollution properties.
Patent Information
- Application Number
- CN202210859937.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-20
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-07-20
AI Technical Summary
It is difficult for existing catalytic cracking catalysts to simultaneously improve heavy oil conversion capabilities and heavy metal pollution resistance when treating heavy oil, and cannot meet the needs of heavy oil catalytic cracking.
Mesoporous rare earth-magnesium-aluminum ternary composite oxide is used as the catalyst matrix material, which is prepared through a multi-component inorganic acid template, and combined with zeolite molecular sieves, binders and clay to form a catalyst with high specific surface and pore volume.
The heavy oil conversion capacity and resistance to heavy metal pollution of the catalyst are significantly improved, achieving higher heavy oil conversion rate and better cracking product selectivity.
Smart Images

Figure CN115055203B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of chemical industry, and in particular to a heavy oil catalytic cracking catalyst. Background Art
[0002] Fluid catalytic cracking (FCC) technology has become an important means of secondary processing of heavy oil in the world today because of its low investment, strong adaptability to raw materials and simple operation, and catalytic cracking catalyst plays a key role in this process. With the increasing depletion of high-quality light crude oil resources worldwide and the increase in delayed coking capacity, refineries, in order to increase efficiency, blend a large proportion of low-quality crude oil such as residual oil, coking wax oil and deasphalted oil in catalytic cracking units. These crude oils are not only difficult to crack, but also contain a large amount of heavy metal pollution elements, which has a serious impact on the smooth operation of catalytic cracking units and the distribution of cracking products, and thus puts forward higher requirements on the performance of catalytic cracking catalysts.
[0003] For heavy oil catalytic cracking, how to achieve efficient conversion of heavy crude oil and obtain light oil products to the maximum extent is the goal that people have always pursued, and the development of catalysts is a key issue. Catalytic cracking catalysts are mainly composed of molecular sieves and matrix components. Based on the characteristics of heavy oil catalytic cracking reactions, not only are molecular sieves required to have good activity and stability, but also the matrix components are required to have large specific surface area, large pores and good resistance to heavy metal pollution.
[0004] Patent CN1098130A discloses a method for preparing a catalytic cracking catalyst: clay and deionized water are first mixed and slurried, hydrochloric acid is added for acidification, pseudo-boehmite is added, and the resulting slurry is aged at 50-80°C for 0.5-2 hours, and then aluminum sol and molecular sieve slurry are added, mixed evenly and spray dried.
[0005] Patent CN1690168A discloses a method for preparing a molecular sieve-containing hydrocarbon cracking catalyst, which includes slurrying and mixing aluminum sol, hydrated alumina, clay, acid, molecular sieve and water to make a slurry, and then drying the obtained slurry. The hydrated alumina contains a modified hydrated alumina, and the modified hydrated alumina is a hydrated alumina that has been calcined at 150-400°C for at least 10 minutes. During slurrying, the acid is added after the aluminum sol and the hydrated alumina.
[0006] CN101745416A discloses a method for preparing a catalytic cracking catalyst, which includes slurrying silica sol with molecular sieve and clay matrix, spray drying, washing and exchanging with ammonium salt for the first time under the condition of pH value of 9 to 11, roasting and washing and exchanging with ammonium salt for the second time. The catalyst preparation method can significantly increase the pore volume of the catalyst. The catalyst can be used for heavy oil catalytic cracking to improve the conversion rate, gasoline yield and gasoline octane number.
[0007] CN101733141A firstly prepares alkaline silica sol with pH value of 10-11.5 and SiO2 content of 3-20wt% by contacting water glass with acid, then mixes the alkaline silica sol with active components, slurries them, dries them and roasts them to prepare a catalytic cracking catalyst. The prepared catalyst has a very high pore volume and has a higher heavy oil cracking capacity when used for heavy oil catalyst cracking.
[0008] CN1195014A calcined kaolin at 850-920°C and then treated it with inorganic acid to prepare modified kaolin with a pore size of 5-20 nm, which can be used as a matrix to improve the activity of cracking catalysts.
[0009] US4836913 reported that kaolin was calcined at above 1000℃ and then treated with NaOH to prepare alkali-modified kaolin with a surface area of 15-350m2 / g and a pore volume of 0.3-1.0ml / g. The catalytic cracking catalyst prepared with this alkali-modified kaolin as the matrix has improved activity, enhanced heavy metal resistance and improved selectivity.
[0010] CN102744099A uses microporous molecular sieve as the main active component and modified meso-microporous molecular sieve as the active auxiliary agent to prepare a heavy oil catalytic cracking catalyst. The content of the microporous molecular sieve is 10-40wt%, the content of the modified meso-microporous molecular sieve is 1-40wt%, the binder is 1-30wt%, and the clay content is 30-80wt%. Compared with the single microporous molecular sieve catalyst, the heavy oil yield of the prepared catalyst is reduced, the light oil yield is increased, and the coke yield is reduced.
[0011] CN1831090A provides a method for synthesizing a macroporous catalytic cracking catalyst using a particle template, the process comprising mixing, aging, molding and drying the template agent particles, the catalyst matrix and the molecular sieve, and then removing the particle template. The volume fraction of pores larger than 5 nm in the synthesized catalyst can be adjusted independently at will, and the catalyst has the advantages of high cracking activity and good selectivity, and is very suitable as a heavy oil catalytic cracking catalyst.
[0012] US6776899 introduces sucrose into the catalytic cracking catalyst synthesis process to produce medium and large pores in the matrix, so that the cracking activity of the catalyst is greatly improved.
[0013] Bao et al. (Bao X., et al. J. Catal., 2007, 251(1): 69-79.) first synthesized a precursor solution of Y-type molecular sieve, and used hexadecyltrimethylammonium bromide as a template to self-assemble it onto kaolin microspheres. They in situ synthesized a composite material with a macropore-mesopore-micropore gradient pore structure, which was well applied in heavy oil catalytic cracking catalysts.
[0014] CN101332433A discloses a method for preparing a catalytic cracking catalyst, including the steps of mixing and slurrying a carrier containing aluminum oxide or its precursor with a molecular sieve, spray drying, and introducing a pore-enlarging agent during the mixing process, wherein the pore-enlarging agent includes one or more of boric acid, phosphoric acid, and an alkali metal salt. The prepared catalyst has the characteristics of high specific surface area, high pore volume, strong heavy oil cracking ability, and strong anti-carbon deposition ability.
[0015] CN1566267A discloses a catalyst for catalytic cracking to increase the production of ethylene and propylene, the catalyst containing 7-70wt% clay, 3-70wt% mesoporous silicon-aluminum material, 5-80wt% inorganic oxide and 5-60wt% MFI structure zeolite.
[0016] CN1436835A incorporates macroporous alumina (pore size>3nm) into the synthesis process of traditional catalytic cracking catalyst. Compared with traditional catalytic cracking catalyst, the prepared catalyst shows higher activity and better selectivity.
[0017] CN1814705A reports a catalytic cracking catalyst with high heavy oil cracking ability and capable of producing more light oil (gasoline and diesel). The catalyst uses macroporous alumina and clay as matrix, with the content of macroporous alumina being 0.5-50wt%, the content of clay being 0-75wt%, and the content of Y-type molecular sieve being 10-70wt%.
[0018] CN1436835A discloses a catalytic cracking catalyst and its preparation method. The prepared catalyst contains 5-40wt% of medium- and macroporous alumina, 5-60wt% of binder, and 5-85wt% of clay, wherein the average pore diameter of the medium- and macroporous alumina is not less than 3nm. Compared with conventional catalysts, the catalyst has enhanced heavy oil conversion capacity and significantly improved gasoline and coke selectivity.
[0019] US5173174 adds 5-20 wt% of macroporous alumina to the catalytic cracking catalyst, thereby significantly increasing the catalytic cracking reaction activity of the catalyst.
[0020] In summary, the use of new matrix materials or modification of existing matrix components is a common approach to improve the performance of catalytic cracking catalyst matrix. However, most of the existing matrix technologies simply increase the specific surface area and pore volume of catalytic cracking catalysts to improve the catalytic cracking performance of catalysts. It is still unable to organically combine the increase in the specific surface area and pore volume of the catalyst matrix with the improvement in the anti-heavy metal pollution performance of the catalyst, thus making it difficult to fully meet the needs of heavy oil catalytic cracking. Summary of the invention
[0021] The object of the present invention is to provide a heavy oil catalytic cracking catalyst, so as to provide a catalytic cracking catalyst with strong heavy oil conversion ability and good resistance to heavy metal pollution.
[0022] To achieve the above object, the present invention provides the following technical solutions:
[0023] A heavy oil catalytic cracking catalyst comprises, by weight, 10 to 40 parts of zeolite molecular sieve, 5 to 30 parts of binder, 1 to 10 parts of mesoporous rare earth-magnesium-aluminum ternary composite oxide, and 20 to 80 parts of clay.
[0024] Preferably, the preparation method of the mesoporous rare earth-magnesium-aluminum ternary composite oxide comprises: uniformly mixing a mixed rare earth solution, a magnesium salt, an aluminum salt, a polybasic organic acid and deionized water according to a weight ratio of Re2O3:MgO:Al2O3:polybasic organic acid:water = 0.005-0.05:0.001-0.01:1:0.01-0.1:5-10, drying and calcining the obtained solid at a temperature of 400-700°C for 1-4 hours to obtain a mesoporous rare earth-magnesium-aluminum ternary composite oxide.
[0025] Preferably, the magnesium salt can be selected from water-soluble inorganic magnesium salts such as magnesium chloride, magnesium nitrate, magnesium sulfate, and magnesium hydroxychloride, preferably magnesium chloride.
[0026] Preferably, the aluminum salt can be selected from one or more water-soluble inorganic aluminum salts such as aluminum chloride, aluminum hydroxychloride, aluminum nitrate, and aluminum sulfate, preferably aluminum nitrate.
[0027] Preferably, the polybasic organic acid is selected from one or more of acetic acid, oxalic acid, citric acid, tartaric acid, citric acid and ascorbic acid, preferably citric acid.
[0028] Preferably, the zeolite molecular sieve is one or more of zeolite molecular sieves selected from HY, REY, REHY, USY, REUSY, etc., which can be used as active components of catalytic cracking catalysts.
[0029] Preferably, the binder is selected from silica sol, alumina sol, acidified pseudo-boehmite, silica-alumina gel, silica-alumina composite sol, aluminum phosphate sol, aluminum phosphate gel, etc., which can be used as one or more of the catalytic cracking catalyst binders, preferably aluminum sol.
[0030] Preferably, the clay can be selected from one or more of the clays that can be used for preparing catalytic cracking catalysts, such as kaolin, halloysite, montmorillonite, diatomaceous earth, saponite, rectorite, sepiolite, attapulgite, bentonite, etc., preferably kaolin.
[0031] Preferably, the preparation method of the heavy oil catalytic cracking catalyst comprises: mixing zeolite molecular sieve, binder, mesoporous rare earth-magnesium-aluminum ternary composite oxide, and clay with deionized water at a solid content of 10 to 30 weight percent, and then spraying and molding to obtain the catalytic cracking catalyst.
[0032] Compared with the prior art, the present invention can produce at least one of the following beneficial effects:
[0033] The present invention uses a polybasic inorganic acid as a template to prepare a mesoporous rare earth-magnesium-aluminum ternary composite oxide matrix material. Compared with the existing catalytic cracking catalyst matrix material, the mesoporous rare earth-magnesium-aluminum ternary composite oxide has a significantly higher specific surface area and pore volume, and can effectively improve the heavy oil conversion capacity of the catalytic cracking catalyst; at the same time, because it contains rare earth and magnesium elements, it can improve the anti-heavy metal pollution performance of the catalytic cracking catalyst as a matrix material. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a nitrogen adsorption-desorption curve diagram of the mesoporous rare earth-magnesium-aluminum ternary composite oxide material C1 prepared in Example 1 of the present invention.
[0035] Figure 2 This is a nitrogen adsorption-desorption curve diagram of the mesoporous rare earth-magnesium-aluminum ternary composite oxide material C3 prepared in Example 3 of the present invention.
[0036] Figure 3 This is a nitrogen adsorption-desorption curve diagram of the mesoporous rare earth-magnesium-aluminum ternary composite oxide material C5 prepared in Example 5 of the present invention. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Several embodiments are listed below.
[0038] Raw material sources and specifications:
[0039] REUSY molecular sieve: ignition loss 6.5 wt%;
[0040] Alumina sol: Al2O3 content 19.40 wt%;
[0041] Kaolin: loss on ignition 15.5% by weight;
[0042] Mixed rare earth solution: Re2O3 content 301.5 g / L; conventional alumina matrix materials (pseudo-boehmite, ignition loss 19.7 wt%) are all qualified industrial products provided by qualified manufacturers.
[0043] Magnesium chloride hexahydrate, aluminum nitrate nonahydrate, and citric acid are all commercially available reagents of analytical grade.
[0044] Material characterization and catalyst heavy oil catalytic cracking reaction performance evaluation:
[0045] The specific surface area and pore volume of the materials were analyzed using a nitrogen adsorption-desorption instrument (Micromeritics ASAP 2010);
[0046] The heavy oil catalytic cracking reaction performance of the catalyst was evaluated on an ACE (Advanced cracking evaluation, R+MultiMode, origin: the United States) device. The device reaction temperature was 530°C, the catalyst / feedstock mass ratio was 5, and the feedstock properties were shown in Table 1.
[0047] Table 1 Raw oil properties
[0048]
[0049]
[0050] Embodiment 1:
[0051] This example is the preparation of the mesoporous rare earth-magnesium-aluminum ternary composite oxide material. 3.3 ml of mixed rare earth solution, 1.5 g of magnesium chloride hexahydrate, 1470 g of aluminum nitrate nonahydrate, 3 g of citric acid and 1000 g of deionized water were fully mixed and dried, and the resulting solid was calcined at 450°C for 4 hours to obtain the mesoporous rare earth-magnesium-aluminum ternary composite oxide C1. The nitrogen adsorption-desorption curve of the mesoporous rare earth-magnesium-aluminum ternary composite oxide C1 (see Appendix) Figure 1 ) It can be seen that the nitrogen adsorption-desorption curve of the sample shows the typical adsorption-desorption curve characteristics of mesoporous materials, indicating that the sample has a rich mesoporous structure.
[0052] Embodiment 2:
[0053] This example is the preparation of the mesoporous rare earth-magnesium-aluminum ternary composite oxide material. 8.3 ml of mixed rare earth solution, 2.5 g of magnesium chloride hexahydrate, 1838 g of aluminum nitrate nonahydrate, 7.5 g of citric acid and 1500 g of deionized water were fully mixed, and the obtained solid was calcined at 500° C. for 3 hours after drying to obtain the mesoporous rare earth-magnesium-aluminum ternary composite oxide C2.
[0054] Embodiment 3:
[0055] This embodiment is the preparation of the mesoporous rare earth-magnesium-aluminum ternary composite oxide material.
[0056] 19.9 ml of mixed rare earth solution, 6.1 g of magnesium chloride hexahydrate, 2205 g of aluminum nitrate nonahydrate, 15 g of citric acid and 2100 g of deionized water were fully mixed, dried and then the obtained solid was calcined at 550°C for 2.5 hours to obtain the mesoporous rare earth magnesium-aluminum ternary composite oxide C3.
[0057] Nitrogen adsorption-desorption curve of mesoporous rare earth-magnesium-aluminum ternary composite oxide C3 (attached Figure 2 ) It can be seen that the nitrogen adsorption-desorption curve of the sample shows the typical adsorption-desorption curve characteristics of mesoporous materials, indicating that the sample has a rich mesoporous structure.
[0058] Embodiment 4:
[0059] This embodiment is the preparation of the mesoporous rare earth-magnesium-aluminum ternary composite oxide material.
[0060] 34.8 ml of mixed rare earth solution, 10.6 g of magnesium chloride hexahydrate, 2573 g of aluminum nitrate nonahydrate, 24.5 g of citric acid and 2800 g of deionized water were fully mixed, dried and then the obtained solid was calcined at 600°C for 2 hours to obtain the mesoporous rare earth-magnesium-aluminum ternary composite oxide C4.
[0061] Embodiment 5:
[0062] This embodiment is the preparation of the mesoporous rare earth-magnesium-aluminum ternary composite oxide material.
[0063] 53.1 ml of mixed rare earth solution, 16.1 g of magnesium chloride hexahydrate, 2940 g of aluminum nitrate nonahydrate, 36 g of citric acid and 3600 g of deionized water were fully mixed and dried, and the resulting solid was calcined at 650°C for 1.5 hours to obtain the mesoporous rare earth-magnesium-aluminum ternary composite oxide C5.
[0064] Nitrogen adsorption-desorption curve of mesoporous rare earth-magnesium-aluminum ternary composite oxide C5 (attached Figure 3) It can be seen that the nitrogen adsorption-desorption curve of the sample shows the typical adsorption-desorption curve characteristics of mesoporous materials, indicating that the sample has a rich mesoporous structure.
[0065] Embodiment 6:
[0066] This example is the preparation of the mesoporous rare earth-magnesium-aluminum ternary composite oxide material. 74.6 ml of mixed rare earth solution, 22.7 g of magnesium chloride hexahydrate, 3308 g of aluminum nitrate nonahydrate, 45 g of citric acid and 4500 g of deionized water were fully mixed, and the obtained solid was calcined at 700°C for 1 hour after drying to obtain the mesoporous rare earth-magnesium-aluminum ternary composite oxide C6.
[0067] Embodiment 7:
[0068] This embodiment is the preparation of the catalytic cracking catalyst containing the mesoporous rare earth-magnesium-aluminum ternary composite oxide matrix material.
[0069] 630 g of REUSY molecular sieve (dry basis), 1298 g of aluminum sol, 27 g of mesoporous rare earth-magnesium-aluminum ternary composite oxide C1 (dry basis), 891 g of kaolin (dry basis) and 12154 g of deionized water were mixed and slurried, and then spray-formed to obtain catalytic cracking catalyst C7.
[0070] Embodiment 8:
[0071] This embodiment is the preparation of the catalytic cracking catalyst containing the mesoporous rare earth-magnesium-aluminum ternary composite oxide matrix material.
[0072] 640 g of REUSY molecular sieve (dry basis), 1340 g of aluminum sol, 40 g of mesoporous rare earth-magnesium-aluminum ternary composite oxide C2 (dry basis), 1060 g of kaolin (dry basis) and 10253 g of deionized water were mixed and slurried, and then spray-formed to obtain catalytic cracking catalyst C8.
[0073] Embodiment 9:
[0074] This embodiment is the preparation of the catalytic cracking catalyst containing the mesoporous rare earth-magnesium-aluminum ternary composite oxide matrix material.
[0075] 616 g of REUSY molecular sieve (dry basis), 1247 g of aluminum sol, 88 g of mesoporous rare earth-magnesium-aluminum ternary composite oxide C3 (dry basis), 1254 g of kaolin (dry basis) and 9017 g of deionized water were mixed and slurried, and then spray-formed to obtain catalytic cracking catalyst C9.
[0076] Embodiment 10:
[0077] This embodiment is the preparation of the catalytic cracking catalyst containing the mesoporous rare earth-magnesium-aluminum ternary composite oxide matrix material.
[0078] 750 g REUSY molecular sieve (dry basis), 1546 g aluminum sol, 150 g mesoporous rare earth-magnesium-aluminum ternary composite oxide C4 (dry basis), 1300 g kaolin (dry basis) and 7124 g deionized water were mixed and slurried, and then spray-formed to obtain catalytic cracking catalyst C10.
[0079] Embodiment 11:
[0080] This embodiment is the preparation of the catalytic cracking catalyst containing the mesoporous rare earth-magnesium-aluminum ternary composite oxide matrix material.
[0081] 672 g of REUSY molecular sieve (dry basis), 1155 g of aluminum sol, 224 g of mesoporous rare earth-magnesium-aluminum ternary composite oxide C5 (dry basis), 1680 g of kaolin (dry basis) and 6439 g of deionized water were mixed and slurried, and then spray-formed to obtain catalytic cracking catalyst C11.
[0082] Embodiment 12:
[0083] This embodiment is the preparation of the catalytic cracking catalyst containing the mesoporous rare earth-magnesium-aluminum ternary composite oxide matrix material.
[0084] 832 g of REUSY molecular sieve (dry basis), 1649 g of aluminum sol, 320 g of mesoporous rare earth-magnesium-aluminum ternary composite oxide C6 (dry basis), 1728 g of kaolin (dry basis) and 6135 g of deionized water were mixed and slurried, and then spray-formed to obtain catalytic cracking catalyst C12.
[0085] Comparative Example 1:
[0086] This comparative example is the preparation of a catalytic cracking catalyst containing a conventional alumina matrix material (pseudo-boehmite).
[0087] 693 g of REUSY molecular sieve (dry basis), 1428 g of aluminum sol, 30 g of pseudo-boehmite (dry basis), 980 g of kaolin (dry basis) and 13369 g of deionized water were mixed and slurried, and then spray-formed to obtain catalytic cracking catalyst D1.
[0088] Comparative Example 2:
[0089] This comparative example is the preparation of a catalytic cracking catalyst containing a conventional alumina matrix material (pseudo-boehmite).
[0090] 704 g of REUSY molecular sieve (dry basis), 1474 g of aluminum sol, 44 g of pseudo-boehmite (dry basis), 1166 g of kaolin (dry basis) and 11278 g of deionized water were mixed and slurried, and then spray-formed to obtain catalytic cracking catalyst D2.
[0091] Comparative Example 3:
[0092] This comparative example is the preparation of a catalytic cracking catalyst containing a conventional alumina matrix material (pseudo-boehmite).
[0093] 678 g of REUSY molecular sieve (dry basis), 1372 g of aluminum sol, 97 g of pseudo-boehmite (dry basis), 1379 g of kaolin (dry basis) and 9919 g of deionized water were mixed and slurried, and then spray-formed to obtain catalytic cracking catalyst D3.
[0094] Comparative Example 4:
[0095] This comparative example is the preparation of a catalytic cracking catalyst containing a conventional alumina matrix material (pseudo-boehmite).
[0096] 713 g of REUSY molecular sieve (dry basis), 1469 g of aluminum sol, 143 g of pseudo-boehmite (dry basis), 1235 g of kaolin (dry basis) and 6768 g of deionized water were mixed and slurried, and then spray-formed to obtain catalytic cracking catalyst D4.
[0097] Comparative Example 5:
[0098] This comparative example is the preparation of a catalytic cracking catalyst containing a conventional alumina matrix material (pseudo-boehmite).
[0099] 638 g of REUSY molecular sieve (dry basis), 1097 g of aluminum sol, 213 g of pseudo-boehmite (dry basis), 1596 g of kaolin (dry basis) and 6117 g of deionized water were mixed and slurried, and then spray-formed to obtain catalytic cracking catalyst D5.
[0100] Comparative Example 6:
[0101] This comparative example is the preparation of a catalytic cracking catalyst containing a conventional alumina matrix material (pseudo-boehmite).
[0102] 790 g of REUSY molecular sieve (dry basis), 1566 g of aluminum sol, 304 g of pseudo-boehmite (dry basis), 1642 g of kaolin (dry basis) and 5828 g of deionized water were mixed and slurried, and then spray-formed to obtain catalytic cracking catalyst D6.
[0103] Table 2 Structural parameters of different matrix materials
[0104]
[0105] Table 2 lists the structural parameters of different matrix materials. It can be seen that compared with the conventional alumina matrix material pseudo-boehmite, the mesoporous rare earth-magnesium-aluminum ternary composite oxide matrix material prepared in the embodiment of the present invention has a significantly higher specific surface area and pore volume, and as a catalyst matrix material, it will be very beneficial to the catalytic cracking reaction of heavy oil molecules.
[0106] Table 3 Heavy oil catalytic cracking reaction performance of different catalytic cracking catalysts
[0107]
[0108]
[0109] Table 3 lists the heavy oil catalytic cracking reaction performance of different catalytic cracking catalysts. It can be seen that compared with the catalyst prepared in the comparative example using the conventional alumina matrix material, the catalyst prepared in the embodiment of the present invention containing the mesoporous rare earth-magnesium-aluminum ternary composite oxide matrix material shows a more excellent heavy oil catalytic cracking reaction performance, not only showing a stronger heavy oil conversion ability, but also having a better cracking product selectivity.
[0110] Table 4 Heavy metal pollution resistance of different catalytic cracking catalysts
[0111] catalytic D4 D5 D6 C10 C11 C12 Dry gas 2.93 2.96 2.94 3.15 3.20 3.31 liquefaction 19.67 19.76 19.88 19.64 19.73 20.83 gasoline 48.91 49.54 49.35 52.26 52.68 51.68 diesel fuel 1343 1282 1288 1065 1031 975 heavy oil 6.01 5.55 5.71 4.29 4.06 3.71 Coke 9.05 9.37 9.24 10.00 10.01 10.73 Conversion 80.57 81.63 81.41 85.06 85.62 86.55 Total fluid 82.01 82.12 82.11 82.56 82.73 82.25
[0112] Table 4 lists the heavy metal pollution resistance of different catalysts. Under the same heavy metal pollution conditions (V: 5000ppm, Ni: 3000ppm), compared with the comparative catalyst, the catalyst of the embodiment of the present invention shows significantly better heavy oil catalytic cracking reaction performance, with significantly lower heavy oil yield and higher gasoline yield, total liquid recovery and conversion rate, which fully demonstrates that the catalyst provided by the present invention has excellent heavy metal pollution resistance.
Claims
1. Use of a heavy oil catalytic cracking catalyst in heavy oil catalytic cracking, characterized in that: Calculated by weight, the catalyst comprises: 10-40 parts of zeolite molecular sieve, 5-30 parts of binder, 1-10 parts of mesoporous rare earth-magnesium-aluminum ternary composite oxide, and 20-80 parts of clay; the preparation method of the mesoporous rare earth-magnesium-aluminum ternary composite oxide comprises: uniformly mixing a mixed rare earth solution, a magnesium salt, an aluminum salt, a polybasic organic acid and deionized water according to a weight ratio of Re2O3:MgO:Al2O3:polybasic organic acid:water=0.005-0.05:0.001-0.01:1:0.01-0.1:5-10, drying and calcining the obtained solid at a temperature of 400-700°C for 1-4 hours to obtain the mesoporous rare earth-magnesium-aluminum ternary composite oxide; the aluminum salt is selected from one or more of aluminum chloride, hydroxyaluminum chloride, aluminum nitrate and aluminum sulfate.
2. The use according to claim 1, characterized in that: The magnesium salt is selected from one or more of magnesium chloride, magnesium nitrate, magnesium sulfate and hydroxymagnesium chloride.
3. The use according to claim 2, characterized in that: The polybasic organic acid is selected from one or more of acetic acid, oxalic acid, citric acid, tartaric acid, citric acid and ascorbic acid.
4. The use according to claim 1, characterized in that: The zeolite molecular sieve is one or more selected from HY, REY, REHY, USY, and REUSY zeolite molecular sieves.
5. The use according to claim 1, characterized in that: The binder is selected from one or more of silica sol, alumina sol, acidified pseudo-boehmite, silica-alumina gel, silica-alumina composite sol, aluminum phosphate sol, and aluminum phosphate gel.
6. The use according to claim 1, characterized in that: The clay is selected from one or more of kaolin, halloysite, montmorillonite, diatomaceous earth, saponite, rectorite, sepiolite, attapulgite and bentonite.
7. The use according to claim 1, characterized in that: The preparation method of the heavy oil catalytic cracking catalyst comprises: mixing zeolite molecular sieve, binder, mesoporous rare earth-magnesium-aluminum ternary composite oxide, and clay with deionized water at a solid content of 10-30%, and then spraying and molding to obtain the catalytic cracking catalyst.
Citation Information
Patent Citations
Catalytic cracking catalyst, preparation method and use thereof
CN101332433A
Catalytic cracking catalyst and preparation method thereof
CN101733141A
Catalytic cracking catalyst and preparation method thereof
CN101745416A
Heavy oil catalytic cracking catalyst and preparation method thereof
CN102744099A
Cracking catalyst and preparing process thereof
CN1098130A
Cited By
Catalytic cracking catalyst, preparation method and application thereof, and wax oil processing method
CN118079993A
Catalytic cracking catalyst, process for its preparation and use, and process for processing a gas oil
CN118079993B