Group IIIA nitride growth systems and methods

JP2022105014A5Active Publication Date: 2024-11-06ジョルゲンソンロビー
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2022064068
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2017-02-22
Filing Date
2022-04-07
Publication Date
2024-11-06
Estimated Expiration
2037-05-26

AI Technical Summary

Technical Problem

Conventional methods for growing gallium nitride (GaN) films, such as metal-organic chemical vapor deposition (MOCVD), face challenges with high temperatures leading to wafer bow, cracking, non-uniformity, and the need for thicker substrates, while sputtering techniques are often considered unprofitable due to poor film quality.

Method used

The use of solid gallium targets for epitaxial atomic layer sputtering (EALS) at lower temperatures, which reduces hydrogen and carbon content, enhances growth rate, and results in high-quality GaN films with reduced dislocation densities, avoiding columnar growth and minimizing wafer stress.

Benefits of technology

This approach produces high-quality GaN films with improved uniformity and reduced cracking, enabling larger epitaxial regions and lower misfit dislocation densities, thus overcoming the limitations of MOCVD and enhancing the efficiency and cost-effectiveness of GaN production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A system and method for growing gallium nitride (GaN) structures is provided. The system and method include: providing a mold; and growing at least a first GaN layer on the mold using a first sputtering process, the first sputtering process including: controlling the temperature of a sputtering target; and adjusting between a gallium-rich condition and a gallium-lean condition, the gallium-rich condition including a gallium-to-nitrogen ratio having a first value greater than 1 and the gallium-lean condition including a gallium-to-nitrogen ratio having a second value less than the first value. The system includes a load lock configured to load and remove substrate wafers into and from the system; and multiple deposition chambers, the multiple deposition chambers including GaN deposition chambers configured to grow at least a first GaN layer on the mold containing the substrate wafer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] <Cross-references to related applications> This application is based on U.S. Provisional Patent Application No. 62 / 342,026, filed by Robbie J. Jorgenson on 26 May 2016 under 35 U.S.C §119(e), titled "Low Temperature Gallium Nitride by Magnetron Sputtering / PVD Materials, Process and Equipment," and U.S. Provisional Patent Application No. 62 / 385,089, filed by Robbie J. Jorgenson on 8 September 2016, titled "SYSTEM AND METHOD FOR DOPING GALLIUM NITRIDE DURING GROWTH BY PHYSICAL VAPOR DEPOSITION AND RESULTING MATERIALS AND DEVICES," and filed by Robbie J. Jorgenson on 19 September 2016, titled "SYSTEM AND METHOD FOR DOPING GALLIUM NITRIDE DURING GROWTH BY PHYSICAL VAPOR DEPOSITION AND RESULTING MATERIALS Claiming priority to U.S. Provisional Patent Application No. 62 / 396,646, entitled “GALLIUM NITRIDE GROWTH BY SPUTTERING AND RESULTING MATERIALS AND DEVICES”, U.S. Provisional Patent Application No. 62 / 412,694, entitled “GALLIUM NITRIDE GROWTH BY SPUTTERING AND RESULTING MATERIALS AND DEVICES”, filed by Robbie J. Jorgenson et al. on 25 October 2016, and U.S. Provisional Patent Application No. 62 / 462,169, entitled “GALLIUM NITRIDE GROWTH BY SPUTTERING AND RESULTING MATERIALS AND DEVICES”, each application is incorporated herein by reference in its entirety.

[0002] This application relates to prior applications: - U.S. Patent Application No. 15 / 294,558, filed on 14 October 2016, titled "SYSTEM AND METHOD FOR LIGHT-EMITTING DEVICES ON LATTICE-MATCHED METAL SUBSTRATES," and published on 20 April 2017 as U.S. Patent No. 2017 / 0110626; and - Provisional U.S. Patent Application No. 62 / 242,604, filed on 16 October 2015, titled "METHOD AND HYPER EMISSION GREEN LIGHT-EMITTING DIODE ON LATTICE-MATCHED METAL SUBSTRATES FOR ADVANCED OPTICAL FIBER NETWORKING," which are incorporated herein by reference in their entirety.

[0003] This application also refers to the following prior applications: - U.S. Provisional Patent Application No. 60 / 835,934, filed on August 6, 2006, titled "III-NITRIDE LIGHT-EMITTING DEVICES WITH ONE OR MORE RESONANCE REFLECTORS AND REFLECTIVE ENGINEERED GROWTH TEMPLATES FOR SUCH DEVICES, AND METHODS"; - U.S. Provisional Patent Application No. 60 / 821,588, filed on August 7, 2006, titled "III-NITRIDE LIGHT-EMITTING DEVICES WITH ONE OR MORE RESONANCE REFLECTORS AND REFLECTIVE ENGINEERED GROWTH TEMPLATES FOR SUCH DEVICES, AND METHODS"; - U.S. Provisional Patent Application No. 60 / 821,588, filed on February 25, 2008, titled "CURRENT-INJECTING / TUNNELING LIGHT EMITTING DEVICE AND - U.S. Provisional Patent Application No. 61 / 066,960, titled "METALLO-SEMICONDUCTOR STRUCTURES FOR III-NITRIDE DEVICES", filed on March 14, 2012; - U.S. Provisional Patent Application No. 61 / 610,943, filed on April 13, 2012, titled "STRUCTURES FOR III-NITRIDE DEVICES"; - U.S. Provisional Patent Application No. 61 / 623,885, filed on April 13, 2012, titled "STRUCTURES FOR III-NITRIDE DEVICES"; - U.S. Provisional Patent Application No. 61 / 655,477, filed on June 4, 2012, titled "METAL-BASE TRANSISTORS FOR III-NITRIDE DEVICES"; - Issued on March 29, 2011, titled "III-NITRIDE LIGHT-EMITTING DEVICES WITH ONE OR MORE RESONANCE REFLECTORS AND REFLECTIVE ENGINEERED GROWTH U.S. Patent No. 7,915,624, titled “TEMPLATES FOR SUCH DEVICES, AND METHODS”;-Published on August 28, 2012, U.S. Patent No. 8,253,157 (now a division of the application, U.S. Patent No. 7,915,624), titled "III-NITRIDE LIGHT-EMITTING DEVICES WITH REFLECTIVE ENGINEERED GROWTH TEMPLATES AND METHODS OF MANUFACTURE"; -Published on November 18, 2014, U.S. Patent No. 8,890,183 (now a division of the application, U.S. Patent No. 8,253,157), titled "III-NITRIDE LIGHT-EMITTING DEVICES WITH REFLECTIVE ENGINEERED GROWTH TEMPLATES AND MANUFACTURING METHOD"; -Published on November 30, 2010, titled "CURRENT-INJECTING / TUNNELING LIGHT-EMITTING DEVICE AND In relation to U.S. Patent No. 7,842,939, titled “METHOD”; U.S. Patent No. 8,865,492 (now a division of the application that was U.S. Patent No. 7,842,939), published on 21 October 2014, titled “METHOD OF FORMING CURRENT-INJECTING / TUNNELING LIGHT-EMITTING DEVICE”; and U.S. Patent No. 9,608,145, published on 28 March 2017, titled “MATERIALS, STRUCTURES, AND METHODS FOR OPTICAL AND ELECTRICAL III-NITRIDE SEMICONDUCTOR DEVICES”; these documents are incorporated herein by whole-word reference.

[0004] Numerous embodiments exist as described herein, each of which can be combined with one or more other embodiments described herein and / or incorporated by reference. In some other embodiments, the present invention provides a partial combination encompassing most of the features of various embodiments, but omitting one or more features individually shown and described herein.

[0005] This invention relates to the field of semiconductor devices and methods for manufacturing semiconductor devices, and more specifically to materials, structures, and methods for growing Group III nitride devices. [Background technology]

[0006] Non-patent document 1 is incorporated herein by reference.

[0007] Non-patent document 2 is incorporated herein by reference.

[0008] Non-patent document 3 is incorporated herein by reference.

[0009] Non-patent document 4 is incorporated herein by reference.

[0010] Non-patent document 5 is incorporated herein by reference.

[0011] Non-patent document 6 is incorporated herein by reference.

[0012] Non-patent document 7 is incorporated herein by reference.

[0013] Non-patent document 8 is incorporated herein by reference.

[0014] Non-patent document 9 is incorporated herein by reference.

[0015] Non-patent document 10 is incorporated herein by reference.

[0016] Non-patent document 11 is incorporated herein by reference.

[0017] Non-patent document 12 is incorporated herein by reference.

[0018] Patent Document 1 is incorporated herein by reference.

[0019] Patent Document 2 is incorporated herein by reference.

[0020] Patent Document 3 is incorporated herein by reference.

[0021] U.S. Patent No. 7,879,697 to P.I. Cohen, issued on February 1, 2011, entitled "GROWTH OF LOW DISLOCATION DENSITY GROUP-III NITRIDES AND RELATED THIN-FILM STRUCTURES", is incorporated herein by reference.

Prior Art Documents

Patent Documents

[0022]

Patent Document 1

Patent Document 2

Patent Document 3

Non-Patent Documents

[0023]

Non-Patent Document 1

Non-Patent Document 10

Non-Patent Document 11

Non-Patent Document 12

Summary of the Invention

[0024] In some embodiments, the present invention provides epitaxial atomic layer sputtering (EALS) utilizing a solid gallium target (in some such embodiments, EALS includes magnetron sputtering). In some embodiments, where columnar growth is undesirable, the present invention produces films using two-dimensional (2D) step growth. Such processes enable high-quality gallium nitride (GaN) films with low hydrogen and carbon content. In some embodiments, organometallic compounds are not required, unlike in metal-organic vapor deposition (MOCVD). In some embodiments, the plasma used during the process reduces the required growth temperature (compared to MOCVD) and increases the growth rate (compared to molecular beam epitaxy (MBE)) while still maintaining high-quality films.

[0025] In some embodiments, the present invention provides systems and methods for growing high-quality, cost-effective epitaxial materials that push the envelope of current industrial functionality. In some embodiments, such materials have a larger epitaxial region and misfit dislocations of different densities before coalescence.

[0026] In some embodiments, associated ion interactions cause the density of dislocations to self-annihilate (self-react) within thinner film thicknesses compared to the pure thermal environment of MOCVD.

[0027] Furthermore, due to the difference in thermal expansion between GaN and the substrate (for example, due to different coefficients of thermal expansion (CTE)), in some embodiments, when GaN is grown on sapphire at a lower temperature than that used by MOCVD, the degree of subsequent wafer warping and wafer stress is reduced. This solves many problems related to wafer cracking, epitaxy cracking, non-uniformity, the need for a thicker sapphire substrate, and the need for processed wafer pockets in the MOCVD system for subsequent active region growth. [Brief explanation of the drawing]

[0028] [Figure 1] This is a flowchart of a method (101) for growing gallium nitride (GaN) based devices. [Figure 2] This is a schematic diagram of a system (201) for growing GaN-based devices. [Figure 3] This is a schematic diagram of the GaN structure (301). [Figure 4] This is a schematic diagram of a low-temperature IIIA nitride sputtering system (401). [Figure 5A] The present invention includes schematic diagrams of several growth modes (501) illustrating various epitaxial growth modes of several embodiments of the present invention. [Figure 5B] This is a set of atomic force microscope (AFM) images (502) of GaN growth. [Figure 6A] Table (601) shows the thicknesses (nanometers) of the AlN layer and GaN layer as indicated in the GaN structure (301) in Figure 3. [Figure 6B] This is a continuation of Table (601). [Figure 7A] Table (701) shows the ω-rocking curve full width at half maximum (FWHM) X-ray diffraction (XRD) values ​​(arcsec) for GaN produced according to some embodiments of the present invention. [Figure 7B] This is a continuation of Table (701). [Figure 8A]This is a schematic diagram of a template and device epitaxy system (801) for electronic equipment and solid-state lighting (SSL). [Figure 8B] This is a schematic diagram of a template and device epitaxy system (802) for electronic equipment and SSL. [Figure 9] This is a schematic diagram of a template and device epitaxy process (901) for electronic equipment and SSL. [Figure 10] Graph (1001) shows the ratio of n-type carrier concentration (per cubic centimeter) to adsorbed atom mobility (cm² / V·s) for hafnium-doped gallium nitride produced according to some embodiments of the present invention. [Figure 11] Graph (1101) shows X-ray diffraction (XRD) data for GaN produced according to some embodiments of the present invention. [Figure 12] This is a schematic diagram of the GaN template structure (1201) for subsequent LED epitaxial growth. [Figure 13] This is a schematic diagram of the GEMM / GaN epitaxial stack structure (1301). [Figure 14A] This is a graph (1401) of X-ray diffraction (XRD) data for GaN generated according to some embodiments of the present invention. [Figure 14B] This is a graph (1402) of X-ray diffraction (XRD) data for GaN generated according to some embodiments of the present invention. [Figure 14C] This is a graph (1403) of X-ray diffraction (XRD) data for GaN generated according to some embodiments of the present invention. [Figure 14D] This is a graph (1404) of X-ray diffraction (XRD) data for GaN generated according to some embodiments of the present invention. [Figure 15] Chart (1501) shows atomic force microscopy (AFM) data for GaN on a GEMM generated according to some embodiments of the present invention. [Figure 16]Graph (1601) shows a comparison of the reflectivity of GEMM / GaN (solid line) produced according to some embodiments of the present invention versus a conventional AlN / GaN distributed Bragg reflector (DBR) (dotted line). [Figure 17] This is a graph (1701) of estimated sputtering rate versus gallium target temperature for gallium nitride (GaN). [Figure 18] This is a schematic diagram of the sputtering system (1801). [Modes for carrying out the invention]

[0029] The following details include many sub-details for illustrative purposes, but those skilled in the art will recognize that many variations and changes to the following details are within the scope of the invention. Certain examples are used to illustrate specific embodiments; however, the invention as described in the claims is not intended to be limited only to such examples, but rather encompasses the entire scope of the accompanying claims. Accordingly, the following preferred embodiments of the invention are described without losing the general laws of the subject matter of the invention and without imposing any limitations on the subject matter of the invention. Furthermore, the following detailed descriptions of preferred embodiments refer to accompanying drawings that form part of the invention, which are shown for illustrative purposes to illustrate specific embodiments in which the invention may be carried out. Other embodiments may be used, and it should be understood that structural changes will be made without departing from the scope of the invention. Embodiments shown in the figures and described herein may include features not included in all specific embodiments. They may include only all subsets of the features described in a particular embodiment, or they may include all of the features described in a particular embodiment.

[0030] The first digit of a reference number appearing in a drawing corresponds to the drawing number in which the component is first introduced, so that the same reference number can refer to the same component appearing in multiple drawings. Signals and connections may also be referred to by the same reference number or label, and their actual meaning becomes clear from their use in the context of the description.

[0031] As used in the specification, the term “substrate” means the material on which the process is carried out, and the substrate includes silicon, sapphire, or other suitable materials.

[0032] As used in this specification, the term “template” means one or more layers that form a base suitable for epitaxial growth, and the template includes silicon, sapphire, GaN / silicon, GaN / sapphire, GaN / aluminum nitride (AlN), GaN / hafnium nitride (HfN), GaN / zirconium nitride (ZrN), or any other suitable material, structure, pattern template, or substrate.

[0033] As used in this specification, physical vapor deposition ("PVD") describes a deposition method that can be used to produce thin films and coatings, and PVD includes cathode arc deposition, electron beam PVD, evaporative deposition, pulsed laser deposition, and sputtering.

[0034] In some embodiments, sputtering includes one or more of the following: direct current (DC) sputtering, radio frequency (RF) sputtering, reactive sputtering, and magnetron sputtering.

[0035] It should be noted that many of the processes and methods described herein utilize numbered / lettered steps. While these processes and methods may be carried out in the order specified by the numbers / letters, this specification of the present invention also intends to allow these processes and methods to be carried out in any other suitable order. Furthermore, this specification also intends to allow the corresponding processes and methods to be carried out using one or more of the steps described herein, so that a given step(s) may be omitted and / or an additional step(s) may be added as desired.

[0036] Figure 1 is a flowchart of method (101) for growing a gallium nitride (GaN)-based device. In some embodiments, the method of flowchart (101) is carried out in a single deposition chamber. In other embodiments, method (101) is carried out in multiple separate deposition chambers. In some embodiments, method (101) includes one or more of blocks (105-110) (for example, in some embodiments, blocks (106) and (108) are optional). In some embodiments, in block (105), a substrate (e.g., sapphire or silicon) is placed for subsequent deposition. In some embodiments, substrate preparation is carried out in block (106). In some embodiments, aluminum nitride (AlN) is sputtered onto the substrate in block (107), where X represents the thickness of the sputtered AlN. In some embodiments, AlN preparation is carried out in block (108) (e.g., oxide removal in some embodiments). In some embodiments, GaN is sputtered in block (109), where Y represents the thickness of the sputtered GaN. In some such embodiments, GaN sputtering includes doping (e.g., doping with silicon, magnesium, iron, carbon, or similar) and / or increasing the mobility of adsorbed atoms. In some embodiments, GaN is sputtered in block (110), where Z represents the thickness of the sputtered GaN. In some such embodiments, GaN sputtering includes doping (e.g., doping with silicon, magnesium, iron, carbon, or similar) and / or increasing the mobility of adsorbed atoms (sometimes referred to herein as EALS). In some embodiments, GaN is alloyed with scandium, zirconium, hafnium, indium, aluminum, or any other suitable element.

[0037] Figure 2 is a schematic diagram of a system (201) for growing GaN-based devices. In some embodiments, the system (201) is used to implement the method of the flowchart (101) shown in Figure 1. In some embodiments, the system (201) includes a load lock (205) into which a substrate wafer (298) is loaded and into which a finished wafer (299) is removed from the system (201). In some embodiments, the system (201) includes a substrate preparation module (206) (e.g., a module for implementing block (106) in Figure 1), an AlN deposition module (207) (e.g., a module for implementing block (107) in Figure 1), an AlN preparation module (208) (e.g., a module for implementing block (108) in Figure 1), a GaN deposition module (209) (e.g., a module for implementing block (109) in Figure 1), and a doping module (210) for doped GaN deposition. In some embodiments, the modules (205-210) are housed within a single deposition chamber. In other embodiments, each module (205-210) is a deposition chamber. In some embodiments, the system (201) includes a wafer handling robot (215) for moving wafers between modules within the system (201).

[0038] Figure 3 is a schematic diagram of the GaN structure (301). In some embodiments, the GaN structure (301) is produced using the system (201) in Figure 2 and / or the method (101) in Figure 1. In some embodiments, the GaN structure (301) includes a substrate layer (305), a sputtered aluminum nitride (AlN) layer (306) on the substrate layer (305) (in some such embodiments, the thickness of the AlN layer (306) = X), a sputtered GaN layer (307) on the AlN layer (306) having a GaN layer (307) thickness = Y (in some such embodiments, the GaN layer (307) is doped (e.g., doped with silicon, magnesium, or the like)), and a sputtered GaN layer (308) on the GaN layer (307) having a GaN layer (308) thickness = Z (in some such embodiments, the GaN layer (308) is doped (e.g., doped with silicon, magnesium, or the like).

[0039] Conventional industrial systems use metal-organic vapor deposition (MOCVD) for GaN growth to produce GaN-based devices. In some embodiments, the present invention replaces the conventional MOCVD GaN process using sputtered GaN, thereby enabling: less wafer warping, and therefore better wafer / device homogeneity due to sputtering, lower process temperatures, and lower-cost chemical use of NH3 and Ga(CH3)3, etc. In some embodiments, the sputtering process is easier to utilize due to less complex equipment requirements and is less expensive than the MBE process.

[0040] Figure 4 is a schematic diagram of a low-temperature Group IIIA nitride sputtering system (401). In some embodiments, the sputtering system (401) includes a vacuum chamber (405). In some embodiments, the chamber (405) includes a wafer holder (406) and a sputtering gun (407) (for example, in some embodiments, the sputtering gun (407) is a gallium sputtering gun and includes a gallium target). In some embodiments, the sputtering gun (407) includes a metal gasket and other appropriate components to be suitable for operation at low temperatures (e.g., below 0°C). In some embodiments, the system (401) includes a cooling system (408) for cooling the gallium target of the sputtering gun (407) so that the gallium target remains in a solid state during sputtering. In some embodiments, the cooling system (408) is operably connected to the sputtering gun (407) via a cold input line (409) and a heat output line (410). In some embodiments, a cooling system (408) circulates one or more heat transfer fluids via wires (409) and (410) to maintain the gallium target in a solid state during sputtering (for example, in some such embodiments, the heat transfer fluids are cryogenic liquids such as liquid nitrogen and / or liquid hydrogen (in some embodiments, liquid nitrogen and / or liquid hydrogen are used when the sputtering system (401) is used with a large wafer and / or wafer platter production system), one or more alcohols, or other suitable heat transfer fluids). In some embodiments, the system (401) includes a voltage source (415) connected to the system (401) via wire (499). In some embodiments, the voltage is increased by the voltage source (415) as the wafer size increases. In some embodiments, the system (401) includes an optical path (420) for monitoring closed or open processes in situ (in some such embodiments, the path (420) is operably connected to an optical reflectivity system which is a pyrometer and / or a computer tuned for emissivity).

[0041] In some embodiments, the GaN growth processes / systems described herein are complementary to epitaxial atomic layer sputtering (EALS). In some embodiments, EALS is a process that uses sputtering or reactive sputtering to effectively result in stoichiometric epitaxial growth of a metal nitride composite on a substrate, where the ratio of metal (e.g., gallium) to active nitrogen (N) atoms reaching the surface of the formed metal nitride varies periodically between metal-rich and N-rich conditions, relative to the stoichiometric composition of the metal nitride compound. In some embodiments, this process of switching from metal-rich to metal-lean conditions is achieved by (1) decreasing the metal flux to the surface of the formed metal nitride, or (2) increasing the active nitrogen flux, or (3) increasing the substrate temperature (or exposing the surface of the formed metal nitride) to increase the evaporation rate of metal adsorbed atoms (i.e., decrease the residence time), or any combination of (1)-(3). In some embodiments, metal-rich conditions increase the mobility of adsorbed atoms by reducing the effect of unsatisfactory bonding (or dangling bonds) on the surface and enhancing surface migration, thereby resulting in non-columnar step growth and thus a higher quality, smoother film. Generally, in some embodiments, increased surface migration of adsorbed atoms improves the crystalline quality of the deposited material by promoting the incorporation of adsorbed atoms in low-energy regions on the growth front. Similarly, in some embodiments, increasing the surface temperature or applying low-energy ions can increase surface migration of adsorbed atoms to improve thin film quality. Thus, in some embodiments, the present invention provides EALS. In some embodiments, this process involves using a separate nitrogen plasma source (e.g., a radio frequency (RF) nitrogen source) or even ion beam-assisted deposition.

[0042] Figure 5A is a schematic diagram illustrating several different epitaxial growth modes (501) according to several embodiments of the present invention. In epitaxial film growth, the deposited material(s) ideally forms an orderly crystal using the atomic arrangement and orientation determined by the crystalline structure of the substrate (505). In some embodiments, various growth modes (510, 520, and / or 530) are obtained depending on the surface mobility of the atoms to be reached, as well as the properties of the substrate and the epitaxial film. In some embodiments, depending on the surface mobility of the atoms reaching the substrate surface, as well as other factors such as the average terrace length of the surface step, the crystalline orientation and defect density of the substrate, the energetic properties of the surface and interface, and the lattice mismatch between the film and the substrate, the epitaxial growth process may 1) start and proceed in one of the above modes, 2) be a combination of two or more modes, or 3) start in one mode and then transition to other modes or a combined growth mode.

[0043] In some embodiments, growth mode (510), represented by the progression from (510a) to (510b), is called two-dimensional (2D) island growth. In some embodiments, in mode (510), small islands form nuclei across the surface and grow laterally, coalescing into layers, resulting in numerous grain boundaries. In some embodiments, growth mode (520), represented by the progression from (520a) to (520b), is called three-dimensional (3D) island growth. In some embodiments, in mode (520), small islands form nuclei across the surface and grow, with further islands forming on top of the initial islands before the lower layers are finished, resulting in increased surface roughness (in some embodiments, mode (520) includes columnar growth). In some embodiments, growth mode (530), represented by the progression from (530a) to (530b), is called step-flow growth. In some embodiments, in mode (530), atoms reaching the surface migrate and are incorporated into the step edge, completing the layer in a step flow (in some embodiments, mode (530) occurs when surface diffusion is greater than the average terrace length).

[0044] Figure 5B shows a set of atomic force microscope (AFM) images (502) of GaN growth. Image (540) shows smooth GaN containing Ga droplets, which occurs in some embodiments where Ga-rich growth conditions are appropriate. In some embodiments, epitaxial atomic layer sputtering (EALS) is performed between GaN growths such that there is a change between Ga-rich and nitrogen-rich growth conditions, as shown in image (540). Image (545) shows the atomic step of smooth GaN without Ga droplets, which is present in the final state of the GaN film (after the change between Ga-rich and nitrogen-rich conditions) before subsequent deposition. In some embodiments, the root mean square (RMS) roughness of image (540) is approximately 8 angstroms. In some embodiments, the RMS roughness of image (545) is approximately 2 angstroms.

[0045] In some embodiments, the present invention generates a material containing GaN on a two-dimensional (2D) photonic crystal using one or more of the processes described herein. In some embodiments, the GaN on the 2D photonic crystal includes air / GaN repeating periods, which are located on layers of GaN (optionally) on layers of AlN located on sapphire. In some embodiments, the GaN on the 2D photonic crystal includes air / GaN repeating periods, which are located on layers of GaN (optionally) on layers of AlN located on HfN. In some embodiments, the GaN on the 2D photonic crystal includes air / GaN repeating periods, which are located on layers of GaN (optionally) on layers of AlN located on ZrN. In some embodiments, the GaN on the 2D photonic crystal includes air / GaN repeating periods, which are located on layers of GaN (optionally) on layers of AlN located on other suitable Group IIIA nitrides. In some embodiments, any of the GaN structures are replaced by HfGaN. In some embodiments, any of the GaN structures are replaced by ZrGaN.

[0046] In some embodiments, the material thickness resulting from the air is expressed as follows: thickness of the air gap (T air )=(wavelength) * (1-2M) / 4, where M = integer (0, 1, 2, 3, 4, 5).

[0047] In some embodiments, the resulting material thickness of GaN between air and sapphire (Al2O3) is expressed as follows: Thickness of GaN between air and Al2O3 (T GaN )=(wavelength) * (1-2M) / (4n), where M is an integer (e.g., 0, 1, 2, 3, 4, 5) and n is the refractive index.

[0048] In some embodiments, GaN on a 2D photonic crystal is effectively carbon-free compared to GaN formed by MOCVD. In some embodiments, GaN on a 2D photonic crystal is effectively hydrogen-free compared to GaN formed by MOCVD.

[0049] In some embodiments, GaN on a 2D photonic crystal contains effectively larger epitaxial grains or epi-islands compared to GaN formed by MOCVD and / or MBE. In some embodiments, GaN on a 2D photonic crystal contains an epitaxial film with a substantially non-columnar structure. In some embodiments, GaN on a 2D photonic crystal contains ultra-smooth surfaces due to improved 2D growth. In some embodiments, GaN on a 2D photonic crystal contains smoother quantum wells than GaN formed by conventional processes. In some embodiments, thinner GaN thicknesses compared to conventional methods of GaN growth are required for dislocation self-annihilation and / or dislocation bending. In some embodiments, GaN sputtered at low temperatures on any material, template, or substrate has a significantly different density of misfit dislocations than GaN grown at high temperatures. In some embodiments, GaN on a 2D photonic crystal contains a substantially different point defect density than GaN formed by conventional processes. In some embodiments, 2D photonic crystal GaN exhibits less wafer warping than GaN formed by conventional methods. In some embodiments, 2D photonic crystal GaN exhibits substantially different stress levels in the film compared to GaN formed by conventional methods. In some such embodiments, the stress level of the film is detectable by Raman spectroscopy.

[0050] In some embodiments, subsequent epitaxial growth of the GaN material of the present invention results in any suitable light-emitting device, photodetector, light-gathering device, or transistor device (including transistors with vertical carrier flow). In some embodiments, the GaN material of the present invention is used in applications such as GaN-based displays (e.g., mobile phones, tablets, etc.), GaN-based solar cells, GaN-based detector arrays, GaN-based ultra-large-scale integrated circuits, GaN coatings for windows, and GaN-based high-temperature indium tin oxide (ITO) replacement. In some embodiments, wafers of the GaN material of the present invention have a diameter of approximately 6 inches or less. In some embodiments, wafers of the GaN material of the present invention have a diameter greater than approximately 6 inches.

[0051] In some embodiments, the present invention provides a magnetron-reactive sputtering system for producing the GaN material of the present invention. In some embodiments, other suitable sputtering techniques, such as direct current (DC) sputtering or radio frequency (RF) sputtering, are used. In some embodiments, the system for producing the GaN material of the present invention includes a nitrogen plasma source or an ion gun. In some embodiments, a solid-state gallium target is used and an EALS process is performed to produce the GaN material of the present invention. In some such embodiments, the solid-state gallium enables a sputter-up configuration, a sputter-down configuration, or a sputter-sideways configuration.

[0052] In some embodiments, the present invention provides a sputter GaN growth process using a solid gallium source located very close to (e.g., less than about 8 inches) the heated substrate. In some embodiments, the solid gallium source is placed further away from the substrate. In some embodiments, the wafer substrate is heated to a range of 1100–1000 degrees Celsius (°C), to a range of 1000–900°C in some embodiments, to a range of 900–800°C in some embodiments, to a range of 800–700°C in some embodiments, to a range of 700–600°C in some embodiments, to a range of 600–500°C in some embodiments, to a range of 500–400°C in some embodiments, and to a range of 400°C to room temperature in some embodiments.

[0053] In some embodiments, the proximity and type of the sputtering gun (e.g., balanced, unbalanced, and partially balanced) allows the process to achieve the desired add-atom energy through plasma interaction with the sputtering gun, while minimizing damage to the GaN film. In some embodiments, ionization caused by the proximity of the sputtering gun source and type enables dislocation bending and / or dislocation self-destruction.

[0054] In some embodiments, the sputtering gun used in the process of the present invention is manufactured using all-metal gasket seals, and / or the temperature of N2 used with the sputtering gun is maintained below the melting point of gallium so that gallium can become solid. In some embodiments, a heat transfer liquid such as various alcohols is used. In some embodiments, the specific dimensions of the sputtering target are larger than the 2-inch diameter of such a cooling system.

[0055] In some embodiments, there is an advantage to incorporating a rotating magnet sputtering gun into the gallium gun. In some embodiments, there is another advantage to using a ring-shaped sputtering target and / or a multi-ring sputtering target for co-deposition of composite materials such as indium gallium nitride (InGaN) and / or aluminum gallium nitride (AlGaN). In some embodiments, hafnium, zirconium, or silicon are listed as sputtering targets. In some embodiments, dilute SiH4 in nitrogen is supplied, and the gas delivery system includes a double dilution system. In some embodiments, the ring-shaped sputtering target allows for reflectance measurement in situ. In some embodiments, both radio frequency and DC methods are applicable. In some embodiments, when EALS is used, variation between gallium-rich and gallium-lean conditions is achieved by variation in temperature, pressure, argon, nitrogen, gallium source power, growth rate, or any other appropriate variable.

[0056] In some embodiments, the present invention provides an epitaxial process for magnetron sputtering comprising one or more of the following steps: (1) providing any combination of substrates, including any number and / or size of wafer substrates or wafer substrate cassettes that enter into a load lock; (2) the substrate being any other suitable template such as silicon, sapphire, GaN / sapphire, AlN / sapphire, GaN / silicon, AlN / silicon, sapphire, or any other Group IIIA nitride on silicon; (3) moving the wafer substrate into an epitaxial chamber by any suitable method or mechanism of manual or robotic movement; (4) placing the wafer substrate into an AlN epitaxial sputtering (or other PVD), MOCVD, or MBE chamber, wherein the AlN is grown on the wafer substrate to any thickness (columnar or non-columnar); (5) moving the AlN / wafer substrate by any suitable method or mechanism of manual or robotic movement; (6) epitaxially sputtering the AlN / substrate wafer with GaN (7) A step of placing the GaN into a sputtering chamber, wherein the GaN is grown to an arbitrary thickness by sputtering on an AlN / wafer substrate (in some embodiments, the gallium is in a solid state during this step, the EALS process is performed, and in some embodiments, optional silicon (Si), hafnium (Hf), and / or zirconium (Zr) doping is included in the process); (8) A step of moving the sputtered GaN / AlN / wafer substrate by any suitable method or mechanism of manual or robotic movement; (9) A step of growing epitaxial metal mirrors (Grown-Epitaxial A process for placing a sputtered GaN / AlN / wafer substrate into a Metal Mirror (GEMM) sputtering chamber, wherein the growth of the GEMM is caused by sputtering on the sputtered GaN / AlN / wafer substrate (in some such embodiments, the growth of the GEMM is carried out in accordance with the description of U.S. Patent Nos. 7,915,624, 8,253,157, and / or 8,890,183, which are introduced above and incorporated herein by reference);In some embodiments, the process may repeat steps 5, 6, and 7 in any order or combination as needed: (9) growing a layer of AlN to any appropriate thickness by sputtering on a GEMM; (10) moving the sputtered GEMM / GaN / AlN / wafer substrate by any appropriate method or mechanism of manual or robotic movement; (11) covering the sputtered GEMM / GaN / AlN / wafer substrate with a final layer of sputtered GaN grown to any appropriate thickness by sputtering; (12) moving the sputtered GaN / GEMM / GaN / AlN / wafer substrate by any appropriate method or mechanism of manual or robotic movement; and (13) positioning the sputtered GaN / GEMM / GaN / AlN / wafer substrate into a MOCVD, MBE, or sputtering (or other PVD) system for the growth of quantum wells (also known as active regions) and p-type layers (also known as p-type layers).

[0057] In some embodiments, the present invention provides a growth process for an epitaxial material comprising one or more of the following steps: (1) providing any combination of substrates, including any number and / or size of wafer substrates or wafer substrate cassettes that enter into a load lock; (2) the substrate being any other suitable template such as silicon, sapphire, GaN / sapphire, AlN / sapphire, GaN / silicon, AlN / silicon, sapphire, or any other Group IIIA nitride on silicon; (3) moving the wafer substrate into an epitaxial chamber by any suitable method or mechanism of manual or robotic movement; (4) placing the wafer substrate into an AlN epitaxial sputtering (or other PVD), MOCVD, or MBE chamber, allowing AlN to grow on the wafer substrate to any thickness (columnar or non-columnar); (5) moving the wafer substrate into an epitaxial chamber by any suitable method or mechanism of manual or robotic movement. (6) The steps of moving the AlN / wafer substrate, and placing the GaN / AlN / substrate wafer into a sputtering chamber for growth of an epitaxial metal mirror (GEMM) (in some such embodiments, the growth of the GEMM is carried out in accordance with the description of U.S. Patent Nos. 7,915,624, 8,253,157, and / or 8,890,183, which are introduced above and incorporated herein by reference);In some embodiments, the process repeats steps 1-6 in any order or combination as needed: (7) growing a layer of AlN to any appropriate thickness by sputtering on the GEMM; (8) moving the sputtered GEMM / AlN / wafer substrate by any appropriate method or mechanism of manual or robotic movement; (9) covering the sputtered GEMM / AlN / wafer substrate with a final layer of sputtered GaN grown to any appropriate thickness by sputtering on the GEMM / AIN wafer substrate (some In such embodiments, the gallium is in a solid state, an EALS process is performed, and in some embodiments, doping with Si, Hf, and Zr occurs; (10) the step of moving the sputtered GaN / GEMM / AlN / wafer substrate by any suitable method or mechanism of manual or robotic movement; and (11) the step of placing the sputtered GaN / GEMM / AlN / wafer substrate into a MOCVD, MBE, or sputtering (or other PVD) system for the growth of quantum wells (or multiple) (also known as active regions) and p-type layers (or multiple).

[0058] In some embodiments, the present invention provides a growth process for an epitaxial material comprising one or more of the following steps: (1) providing any combination of substrates, including any number and / or size of wafer substrates or wafer substrate cassettes that enter into a load lock; (2) the substrates being silicon, sapphire, GaN / sapphire, AlN / sapphire, GaN / silicon, AlN / silicon (1) a suitable template such as sapphire or any other Group IIIA nitride on silicon; (2) moving the wafer substrate into the epitaxial chamber by any suitable method or mechanism of manual or robotic movement; (3) positioning the substrate wafer into the growing epitaxial metal mirror (GEMM) sputtering chamber, where the growth of the GEMM is produced by sputtering on the wafer substrate (in some such embodiments, the growth of the GEMM is carried out in accordance with the description of U.S. Patent Nos. 7,915,624, 8,253,157, and / or 8,890,183, which are introduced above and incorporated herein by reference).(4) (5) Moving the GEMM / wafer substrate into the epitaxial chamber by any suitable method or mechanism of manual or robotic movement; (6) Placing the GEMM / wafer substrate into the AlN epitaxial sputtering chamber, where the AlN is grown to any suitable thickness (columnar or non-columnar); in some embodiments, the process repeats steps 4-5 as needed; (7) Arbitrarily growing a layer of AlN to any suitable thickness by sputtering on the GEMM; (8) Moving the sputtered GEMM / AlN / GEMM / wafer substrate by any suitable method or mechanism of manual or robotic movement; (9) Sputtering on the GEMM / AlN / GEMM / wafer substrate to any suitable thickness (10) a step of covering the sputtered GaN / GEMM / AlN / GEMM / wafer substrate with a final layer of sputtered GaN (in some such embodiments, the gallium target used during sputtering is in a solid state, an EALS process is performed, and in some embodiments, doping with Si, Hf, Zr occurs), (11) a step of moving the sputtered GaN / GEMM / AlN / GEMM / wafer substrate by any suitable method or mechanism of manual or robotic movement, and (12) a step of placing the sputtered GaN / GEMM / AlN / GEMM / wafer substrate into a MOCVD, MBE, or sputtering (or other PVD) system for the growth of quantum wells (or multiple) (also known as active regions) and p-type layers (or multiple).

[0059] In some embodiments, the present invention provides a growth process for an epitaxial material comprising one or more of the following steps: (1) providing any combination of substrates, including any number and / or size of wafer substrates or wafer substrate cassettes that enter into a load lock; (2) the substrate being any other suitable template such as silicon, sapphire, GaN / sapphire, AlN / sapphire, GaN / silicon, AlN / silicon, sapphire, or any other Group IIIA nitride on silicon; (3) moving the wafer substrate into a sputtering epitaxial chamber by any suitable method or mechanism of manual or robotic movement; (4) growing any Group IIIA nitride material (columnar or non-columnar) on the wafer substrate to any suitable thickness; (5) moving the Group IIIA nitride / wafer substrate by any suitable method or mechanism of manual or robotic movement; (6) GEMM growth is achieved by sputtering on a Group IIIA nitride / wafer substrate, a process of placing a Group IIIA nitride / wafer substrate into a GEMM sputtering chamber (in some such embodiments, GEMM growth is carried out in accordance with the description of U.S. Patent Nos. 7,915,624, 8,253,157, and / or 8,890,183, which are introduced above and incorporated herein by reference).); In some embodiments, the process is repeated, if necessary, in any order or combination: (7) growing a layer of AlN or any other IIIA nitride to any appropriate thickness by sputtering on the GEMM; (8) moving the sputtered GEMM / IIIA nitride / wafer substrate by any appropriate method or mechanism of manual or robotic movement; (9) covering the sputtered GEMM / IIIA nitride / wafer substrate with a final layer of sputtered GaN grown to any appropriate thickness by sputtering on the GEMM / IIIA nitride / wafer substrate. (10) a step of moving the sputtered GaN / GEMM / IIIA nitride / wafer substrate by any suitable method or mechanism of manual or robotic movement, and (11) a step of placing the sputtered GaN / GEMM / IIIA nitride / wafer substrate into a MOCVD, MBE, or sputtering (or other PVD) system for the growth of quantum wells (or multiple) (also known as active regions) and p-type layers (or multiple).

[0060] In some embodiments, the Group IIIA nitride is replaced by any other Group IIIA nitride, or any combination of Group IIIA nitride layers and / or compounds. In addition, in some embodiments, these materials include silicon (Si), Hf, Zr, and / or magnesium (Mg). In some embodiments, wafers and / or substrates are inserted, moved, or directly transported by any suitable (manual or robotic) method or mechanism within or between any combination and / or any number of material-specific or process-specific epitaxial sputtering (or other PVD), MOCVD, or MBE chambers or equipment. In some embodiments, the process of the present invention occurs in a material-specific sputtering (or other PVD), MOCVD, or MBE epitaxial chamber, and / or any combination of arbitrary wafer movement(s) within and between material-specific sputtering (or other PVD), MOCVD, or MBE chambers. In some embodiments, the process of the present invention occurs in a material-specific sputtering (or other PVD), MOCVD, or MBE epitaxial chamber without wafer movement(s).

[0061] Growing gallium nitride (GaN) films using conventional sputtering techniques is typically considered unprofitable due to the low film quality (for example, GaN films grown using conventional sputtering techniques usually have a characteristic X-ray diffraction (XRD) rocking curve full width at half maximum of 620 arcsec and / or higher). Because these sputtered epitaxially grown films are considered to be of lower quality than those that can be produced by MOCVD or MBE methods, conventional sputtered epitaxial growth techniques are not designed with intended doping in mind.

[0062] In some embodiments, the present invention provides n-type doped GaN (which is also known to be sometimes unintentionally doped) intentionally doped with doping elements such as silicon (or titanium (Ti), zirconium (Zr), hafnium (Hf), oxygen (O), sulfur (S), selenium (Se), and / or tellurium (Te)), having a background electron concentration of about 5x10 16 / cm 3 and achieving an electron concentration higher than 5x10 18 / cm 3 such as 1x10 20 / cm 3 to 5x10 16 / cm 3 or more. In some embodiments, the electron concentrations of these intentionally doped materials are used to make ohmic contacts and are used as conductive materials.

[0063] In some embodiments, the present invention provides a method for growing high-quality GaN by sputtering with optional n-type doping comprising one or more of the following: (1) degassing a wafer, chamber, and wafer holder; (2) GaN nucleation, wherein GaN nucleation comprises (a) setting a temperature to impart energy to adsorbed atoms so that adsorbed atoms can find energetically favorable positions on the surface of a template for initial epitaxial growth; (b) setting a vacuum pressure in the chamber to allow plasma formation; (c) supplying plasma gas to the chamber; (d) supplying nitrogen gas to the chamber; and (e) supplying power to a gun of a solid gallium (Ga) target to provide gallium, which is a template for adsorbed atoms to induce initial epitaxial growth. The method further comprises (3) stopping the plasma gas source once nucleation has reached a minimum thickness, and (4) growing GaN on the GaN layer with appropriate temperature and gas flow and Ga gun target power to enable best GaN growth, wherein GaN sputtering comprises doping, which comprises (a) simultaneous sputtering of a dopant, (b) thermal evaporation of a dopant, (c) e-beam evaporation of a dopant, (d) Ga mixing with the dopant in a sputtering gun, and (e) dilute SiH4, Si2H6, tetraethylsilane, and / or other reactants that retain the dopant (Si) in a carrier gas (H2, N2, Ar, Xe, He, Kr, Rn, etc.). The method includes (f) gas injection of a dopant reactant, including an example thereof, and silicon ion implantation doping, wherein the method further includes (5) raising the temperature to a temperature high enough to remove any potential gallium droplets and letting it sit until the gallium droplets are gone, and (6) turning off any of the above variables as necessary and removing the wafer.

[0064] The GaN industry is interested in the full width at half maximum (FWHM) value of the ω-rocking curve for measuring the quality of the resulting devices, for both the X-ray diffraction (XRD) 002 (symmetric) peak and 102 (asymmetric) peak. In some embodiments, the present invention provides a sputtering GaN process that enables the FWHM values ​​for both the 002 and 102 peaks to be less than 1000 arcsec, less than 600 arcsec in some embodiments, less than 300 arcsec in some embodiments, less than 200 arcsec in some embodiments, and less than 100 arcsec in some embodiments. In some embodiments of the present invention, the FWHM for the 002 peak is less than 500 arcsec and the FWHM for the 102 peak is less than 1000 arcsec.

[0065] In some embodiments of the present invention, the FWHM of the 002 peak is less than 400 arcsecs and the FWHM of the 102 peak is less than 800 arcsecs. In some embodiments, the FWHM of the 002 peak is less than 300 arcsecs and the FWHM of the 102 peak is less than 600 arcsecs. In some embodiments, the FWHM of the 002 peak is less than 300 arcsecs and the FWHM of the 102 peak is less than 500 arcsecs. In some embodiments, the FWHM of the 002 peak is less than 300 arcsecs and the FWHM of the 102 peak is less than 400 arcsecs. In some embodiments, the FWHM of the 002 peak is less than 250 arcsecs and the FWHM of the 102 peak is less than 350 arcsecs.

[0066] In some embodiments, the present invention provides a method comprising the step of growing gallium nitride (GaN) by physical vapor deposition (PVD) (e.g., by sputtering) such that the grown GaN has ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurements of both the 002 peak and 102 peak with less than 1000 arcsec.

[0067] In some embodiments, the present invention includes: (1) the step of simultaneously sputtering one of Si, Ti, Zr, Hf, O, S, Se, and / or Te while growing GaN by sputtering; (2) the step of thermally evaporating Si, Ti, Zr, Hf, O, S, Se, and / or Te while growing GaN by sputtering; and (3) the step of simultaneously sputtering Si, Ti, Zr, Hf, O, The present invention provides a step of e-beam evaporation of S, Se, and / or Te; (4) growing n-type GaN by mixing Ga with Si, Ti, Zr, Hf, O, S, Se, and / or Te; (5) gas injection of dilute SiH4, GeH4, Si2H6, tetraethylsilane, and / or other reactants containing the previously mentioned elements in a carrier gas (H2, N2, Ar, Xe, He, Kr, Rn...); and (6) ion implantation doping of Si, Ti, Zr, Hf, O, S, Se, and / or Te while growing GaN by sputtering. In some embodiments, the present invention further includes (7) doping with other group IV elements (e.g., Ge or Sn in some embodiments), (8) co-doping with any combination of the above elements, (9) n-doping enhanced with a surfactant (e.g., In), (10) doping tuned to produce a specific doping profile or internal electric field, and / or (11) delta doping with any of the above elements. In some embodiments, the present invention includes the application of surfactants to modify or enhance growth.

[0068] In some embodiments, GaN grown using the method described herein is FWHM for 0-5 arcsec; in some embodiments, 5-10 arcsec; in some embodiments, 10-15 arcsec; in some embodiments, 15-20 arcsec; in some embodiments, 20-25 arcsec; in some embodiments, 25-30 arcsec; in some embodiments, 30-40 arcsec; in some embodiments, 40-50 arcsec WHM; in some embodiments, FWHM of 50-100 arcsecs; in some embodiments, FWHM of 100-150 arcsecs; in some embodiments, FWHM of 150-200 arcsecs; in some embodiments, FWHM of 200-250 arcsecs; in some embodiments, FWHM of 250-300 arcsecs; in some embodiments, FWHM of 300-400 arcsecs; in some embodiments, FWHM of 400-500 arcsecs; in some embodiments, FWHM of 500-600 arcsecs The ω-rocking curve has a full width at half maximum (FWHM) X-ray diffraction measurement of M; FWHM less than 620 arcsec in some embodiments; FWHM less than 600 arcsec in some embodiments; FWHM less than 500 arcsec in some embodiments; FWHM less than 400 arcsec in some embodiments; FWHM less than 300 arcsec in some embodiments; FWHM less than 240 arcsec in some embodiments; FWHM less than 200 arcsec in some embodiments; FWHM less than 100 arcsec in some embodiments; FWHM less than 50 arcsec in some embodiments; FWHM less than 40 arcsec in some embodiments; FWHM less than 30 arcsec in some embodiments; FWHM less than 27 arcsec in some embodiments; FWHM less than 25 arcsec in some embodiments; FWHM less than 20 arcsec in some embodiments; FWHM less than 10 arcsec in some embodiments; and FWHM less than 5 arcsec in some embodiments.

[0069] In some embodiments, the present invention provides a method comprising the step of growing gallium nitride (GaN) by physical vapor deposition (PVD) (e.g., by sputtering) such that the grown GaN has an ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurement of less than 620 arcsec. In some embodiments, the grown GaN has an ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurement of less than 1000 arcsec. In some embodiments, the method further comprises the step of doping the GaN by co-sputtering at least one dopant selected from the group consisting of silicon (Si), titanium (Ti), zirconium (Zr), hafnium (Hf), oxygen (O), sulfur (S), selenium (Se), and tellurium (Te) during the PVD of the GaN. In some embodiments, the method further comprises the step of doping the GaN by thermally evaporating at least one selected from the group consisting of Si, Ti, Zr, Hf, O, S, Se, and Te during the PVD of the GaN. In some embodiments, the method further includes the step of doping the GaN by e-beam evaporation with at least one selected from the group consisting of Si, Ti, Zr, Hf, O, S, Se, and Te to sustain the PVD of the GaN.

[0070] In some embodiments of the method, GaN growth includes the step of doping GaN to form n-type GaN using a mixture of Ga and at least one selected from the group consisting of Si, Ti, Zr, Hf, O, S, Se, and Te. In some embodiments, the method further includes the step of sustaining PVD of GaN by gas injection of dilute SiH4, GeH4, Si2H6, tetraethylsilane, and / or other reactants; and gas injection of at least one selected from the group consisting of Si, Ti, Zr, Hf, O, S, Se, and Te while holding a carrier gas (H2, N2, Ar, Xe, He, Kr, Rn, or similar). In some embodiments, the method further includes the step of sustaining PVD of GaN by ion implantation doping of GaN with at least one selected from the group consisting of Si, Ti, Zr, Hf, O, S, Se, and Te.

[0071] In some embodiments of the method, GaN doping uses at least one dopant selected from the group consisting of germanium (Ge) and tin (Sn), in place of or in addition to the elements described previously. In some embodiments, GaN doping includes (e.g., In)n-doping enhanced with a surfactant. In some embodiments, GaN doping includes doping tuned to produce a specific doping profile or internal electric field. In some embodiments, GaN doping includes delta doping with any of the elements described previously.

[0072] In some embodiments, the present invention provides a method comprising the step of growing gallium nitride (GaN) by physical vapor deposition (PVD) (for example, by sputtering in some embodiments) such that the grown GaN has an ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurement of less than 25 arcsec (in the 002 plane and / or 102 plane).

[0073] In some embodiments, the present invention provides a method comprising the step of growing gallium nitride (GaN) by physical vapor deposition (PVD) (for example, by sputtering in some embodiments) such that the grown GaN has ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurements of both the 002 peak and 102 peak with a duration of less than 1000 arcsec.

[0074] In some embodiments, the present invention provides a method comprising the steps of sputtering epitaxial GaN; and, between sputtering, intended n-type doping. In some embodiments of the method, the doping includes the step of co-sputtering silicon (Si). In some embodiments, the doping includes thermal evaporation of Si. In some embodiments, the doping includes e-beam evaporation of Si. In some embodiments, the sputtering includes using a target material comprising a mixture of Ga and Si. In some embodiments, the doping includes gas injection of SiH4, Si2H6, tetraethylsilane, and / or other reactants (dilute portions in some embodiments) with a carrier gas that holds Si (e.g., H2, N2, Ar, Xe, He, Kr, Rn, etc.).

[0075] In some embodiments, doping includes ion implantation doping of Si. In some embodiments, doping includes sputtering at least one selected from the group consisting of silicon (Si), titanium (Ti), zirconium (Zr), hafnium (Hf), oxygen (O), sulfur (S), selenium (Se), and tellurium (Te). In some embodiments, doping includes thermal evaporation of at least one selected from the group consisting of Si, Ti, Zr, Hf, O, S, Se, and Te. In some embodiments, doping includes e-beam evaporation of at least one selected from the group consisting of Si, Ti, Zr, Hf, O, S, Se, and Te. In some embodiments, sputtering includes using a target material containing a mixture of Ga and at least one selected from the group consisting of Si, Ti, Zr, Hf, O, S, Se, and Te. In some embodiments, doping involves gas injection of SiH4, 2H6, tetraethylsilane, and / or other reactants with a carrier gas (e.g., H2, N2, Ar, Xe, He, Kr, Rn, etc.) that holds at least one selected from the group consisting of Si, Ti, Zr, Hf, O, S, Se, and Te.

[0076] In some embodiments, doping includes ion implantation doping of at least one dopant selected from the group consisting of Si, Ti, Zr, Hf, O, S, Se, and Te. In some embodiments, doping includes doping tuned with at least one dopant selected from the group consisting of Si, Ti, Zr, Hf, O, S, Se, and Te to induce a specific doping profile or internal electric field. In some embodiments, doping includes delta doping with at least one dopant selected from the group consisting of Si, Ti, Zr, Hf, O, S, Se, and Te. In some embodiments, doping includes co-doping with at least one dopant selected from the group consisting of Si, Ti, Zr, Hf, O, S, Se, and Te. In some embodiments, doping includes n-doping enhanced with a surfactant (e.g., In). In some embodiments, the method further includes doping with other group IV elements (e.g., Ge or Sn in some embodiments) instead of or in addition to the aforementioned elements.

[0077] Figure 6A is Table (601) of the thicknesses (nanometers) of the AlN layer and GaN layer as shown in the GaN structure (301) of Figure 3. In some embodiments, each row in Table (601) refers to a range of thickness for the AlN layer (e.g., layer 306 in Figure 3) and a corresponding range of thickness for at least one of the GaN layers (e.g., layer (307) and / or layer 308 in Figure 3). In some embodiments, the thickness of the AlN layer is in the range of approximately the thickness of a monolayer up to 210 nanometers (nm), and the thickness of the GaN layer is in the range of approximately 10 to 20,000 nm.

[0078] Figure 6B is a continuation of Table (601).

[0079] Figure 7A is Table (701), showing the ω-rocking curve full width at half maximum (FWHM) X-ray diffraction (XRD) values ​​(arcsec) for GaN produced according to some embodiments of the present invention. Table (701) includes rocking curve values ​​for both 002 (symmetric) and 102 (asymmetric) peaks. In some embodiments, the rocking curve values ​​typically decrease as the AlN thickness decreases. In some embodiments, smaller rocking curve values ​​are generally preferred.

[0080] Figure 7B is a continuation of Table (701). In some embodiments, the FWHM value for the GaN 002 peak is in the range of approximately 14.4 to 619 arcsecs, and the FWHM value for the GaN 102 peak is in the range of approximately 0 to 2515 arcsecs. In some embodiments, the present invention provides combinations of 002 peak values ​​of less than 250 arcsecs and 102 peak values ​​of less than 550 arcsecs for AlN thicknesses shown in Table (1201) and the sputtering process (see Table (1301) for some embodiments of FWHM provided by the present invention; each row in Table (1301) refers to a range of FWHM values ​​for the 002 and 102 peaks of GaN).

[0081] In some embodiments, the present invention provides a method for producing a gallium nitride (GaN)-based device, the method comprising: providing a substrate; sputtering aluminum nitride (AlN) onto the substrate; and sputtering at least a first layer of GaN onto the AlN such that the first layer of GaN has an ω-rocking curve full width at half maximum (FWHM) X-ray diffraction (XRD) measurement of less than 250 arcsec with a 002 peak and an FWHM XRD measurement of less than 550 arcsec with a 102 peak.

[0082] In some embodiments of the method, the first layer of GaN has a thickness in the range of approximately 10 to 20,000 nanometers (nm), where AlN has a thickness in the range of approximately 5 to 210 nm.

[0083] In some embodiments, the present invention provides a gallium nitride (GaN)-based device comprising: a substrate; a first layer of aluminum nitride (AlN) on the substrate; and at least a second layer of GaN on the first layer of AlN, wherein the second layer of GaN has an ω-rocking curve full width at half maximum (FWHM) X-ray diffraction (XRD) measurement of less than 250 arcsec with a 002 peak and an FWHM XRD measurement of less than 550 arcsec with a 102 peak.

[0084] In some embodiments of the apparatus, the first layer of GaN has a thickness in the range of approximately 10 to 20,000 nanometers (nm), where AlN has a thickness in the range of approximately 1 monolayer to 210 nm.

[0085] In some embodiments, the present invention provides a method for growing gallium electrode (Ga electrode) gallium nitride (GaN) on sapphire (in some such embodiments, the sapphire is substantially c-plane oriented; in some embodiments, substantially r-plane oriented; in some embodiments, substantially m-plane oriented; in some embodiments, substantially a-plane oriented). In some embodiments, the method comprises one or more of the following: (1) preparation of a substrate (in some embodiments, step 1 is optional), wherein the preparation of the substrate comprises (a) chemical cleaning (epilled and / or degreased, and / or chemical etching) and (b) pressure lower than air and high temperature (e.g., in some embodiments, 1e -6(1) Preparation of the substrate, including vacuum degassing in Torr (substrate temperature less than 800-900°C); (2) Surface nitriding, wherein the surface nitriding comprises (a) providing an N2 radio frequency (RF) plasma at a certain RF power, N2 flow rate, and substrate temperature for a duration (for example, in some embodiments, RF power: 300-500 watts (W), N2 flow: 2-9 standard cubic centimeters per minute (SCCM), substrate temperature: 300-900°C, duration: 10-60 minutes), and (b) optionally monitoring reflected fast electron diffraction (RHEED) during nitriding;A step of forming an AlN buffer (in some embodiments, step 3 is optional), wherein the step of forming the AlN buffer is to (a) deposit a layer of AlN (e.g., in some embodiments, AlN (or AlGaN) of 5 nanometers (nm) to 50 nm) with RF power on a magnetron gun, nitrogen flow, increasing substrate temperature, and an Al / N flux ratio (e.g., in some embodiments, Rf power: 300-800 W, N2 flow: 2-5 SCCM, substrate temperature: 700-850 °C, Al / N flux is slightly greater than 1:1) A step of forming an AlN buffer, comprising: (b) in some embodiments, depositing Al for 5 seconds, then providing RF activated nitrogen plasma for 10 seconds (once or more times), then depositing AlN for 1 minute, then annealing for 30 seconds (once or more times), then a final N2 anneal (just enough to use up the excess Al on the surface); (c) optionally monitoring changes in the RHEED pattern from sapphire to diffused AlN to streaky AlN; and (d) optionally using optical reflectivity measurements to monitor the number of extra metal anneals. In some embodiments, if the mold is AlN as described in steps (1) to (3) above, gallium is deposited and subsequently evaporated to remove oxygen from the AlN surface. In some embodiments, the method further comprises (4) GaN nucleation, where the GaN nucleation (a) provides high-temperature N-rich GaN of 10-100 nm (e.g., in some embodiments, RF power supply: 300-500 W, N2 flow: 2-5 SCCM, substrate temperature: 700-850 °C, Ga / N flux ratio less than 1:1), (b) optionally monitoring the RHEED pattern from streaky chevrons to extended chevrons (from two-dimensional (2D) diffraction to three-dimensional (3D) diffraction), and (c) optionally monitoring the reflectivity measurement intensity corresponding to the intended surface roughening;(5) Forming a GaN smooth layer, wherein the step of forming the GaN smooth layer is to (a) provide high-temperature Ga-rich GaN of 100-500 nm (for example, in some embodiments, RF power supply: 300-500 W, N2 flow: 2-5 SCCM, substrate temperature: 700-850 °C, Ga / N flux ratio greater than 1:1), (b) remove excess Ga under N2 (RF plasma off) and by increasing the substrate temperature (for example, in some embodiments, 700-800 °C), and (c) optionally monitor the RHEED pattern from elongated vertex to streaky vertex (from 3D to 2D diffraction); (6) The method involves forming a thick GaN defect reduction layer, where forming the GaN defect reduction layer involves (a) providing 1-5 μm of slightly Ga-rich GaN (e.g., in some embodiments, RF power supply: 300-500 W, N2 flow: 2-5 SCCM, substrate temperature: 400-800°C, Ga / N flux ratio greater than approximately 1:1, and growth rate faster than 0.1 μm / hour), (b) removing excess Ga approximately every 15-30 minutes under N2 (RF plasma off) and increasing the substrate temperature (e.g., in some embodiments, 700-800°C), and (c) increasing the GaN thickness and exhibiting a more distinct RHEED pattern. The process includes: (d) optionally monitoring the growth rate, changes in growth mode, and the number of extra Ga annealings using optical reflectivity measurements; (e) optionally using defect reduction techniques such as epitaxial atomic layer sputtering (EALS), plasma-assisted epitaxy, irradiance-angle ion-assisted growth, thin AlN interlayers, and AlN / GaN short-period superlattices, or any other suitable defect reduction techniques; and (f) optionally using doping methods such as those described above (for example, in some embodiments, dilute concentrations of SiH4 in nitrogen are injected into the chamber).

[0086] In some embodiments, the present invention provides Group IIIA nitride AlN / GaN and AlN / AlGaN superlattice (SL) structures used for through-dislocation (TD) density reduction (i.e., TD filtering) and / or for strain control and fabrication in GaN and AlGaN layers and structures grown on sapphire and silicon substrates. In some such embodiments, the sputtering techniques described herein (including epitaxial atomic layer sputtering (EALS) in some embodiments) are used to form high-quality TD-filtered and strain-controlled structures at much lower growth temperatures than conventional methods. In some embodiments, the Group IIIA nitride SL structures include 3 nm to 5 nm AlN with 50 to 100 periodicities, GaN or AlGaN with 10 nm to 30 nm, grown under conditions that promote smooth interfaces. In some embodiments, the present invention provides SL structures comprising periodic lattice-matched III nitride / metal nitride layers, such as GaN / HfN and GaN / ZrN SL (in some such embodiments, the SL structure additionally has higher out-of-plane electrical conductivity compared to AlN / GaN SL due to the very high resistivity of AlN).

[0087] In some embodiments, the present invention provides a method for producing a gallium nitride (GaN)-based device, the method comprising: providing a substrate mold comprising aluminum nitride; depositing one or more gallium nitride (GaN) nucleation layers on the substrate mold; depositing GaN smoothing layers on one or more GaN nucleation layers; and depositing a thick GaN defect reduction layer on the GaN smoothing layers.

[0088] In some embodiments, sputter epitaxy offers several advantages, including (1) no organometallic precursors, (2) lower process temperatures (compared to conventional epitaxy techniques), (3) larger wafers, and (4) a superior thermal budget that enables integration.

[0089] In some embodiments, the present invention provides systems and methods including: PVD of AlN nucleated layers (e.g., sputtering in some embodiments) (in some embodiments, 5 minutes of PVD can be replaced with MOCVD for up to about 1.5 hours); PVD of GaN:Hf templates (in some embodiments, GaN:Hf of about 500 nm can be replaced with MOCVD GaN of up to about 5 μm due to the very high conductivity of GaN:Hf); and PVD of HfN / GaN:Hf distributed Bragg reflector (DBR) templates (in some embodiments, PVD of HfN / GaN:Hf DBR templates enables optical microcavity devices that are lattice-matched to GaN and have 99.99% reflectivity and high conductivity).

[0090] Figure 8A is a schematic diagram of a template and device epitaxy system (801) for electronic devices and solid-state lighting (SSL). In some embodiments, the system (801) performs processing on a bare wafer (850) to produce a metal mirror device (860). In some embodiments, the system (801) includes a plurality of modules (805–810) (in some such embodiments, one of each of the plurality of modules (805–810) is a separate deposition chamber; in other embodiments, the plurality of modules (805–810) are contained within a single deposition chamber). In some embodiments, the system (801) includes an aluminum nitride (AlN) nucleation module (805) configured to produce an AlN nucleation layer using one or more of the PVD processes described herein (in some such embodiments, the thickness of the AlN nucleation layer is approximately 25 nanometers (nm)). In some embodiments, the system (801) further includes a grown epitaxial metal mirror (GEMM) module (806) configured to produce one or more GEMM layers (in some such embodiments, the GEMM layer(s) are produced in accordance with the description of U.S. Patent Nos. 7,915,624, 8,253,157, and / or 8,890,183, which are introduced above and incorporated herein by reference). In some embodiments, the system (801) further includes GaN modules (807, 808, 809, and 810) configured to produce one or more GaN layers using one or more PVD processes described herein (for example, in some embodiments, one or more layers of Hf:GaN are produced in the GaN modules (807, 808, 809, and / or 810)).

[0091] Figure 8B is a schematic diagram of a template and device epitaxy system (802) for electronic devices and SSLs. In some embodiments, the system (802) performs processing on a bare wafer (850) to produce an LED-ready device (870). In some embodiments, the system (802) includes multiple modules (805-808 and 820-821) (in some such embodiments, one of each of the multiple modules (805-808 and 820-821) is a separate deposition chamber; in other embodiments, the multiple modules (805-808 and 820-821) are contained within a single deposition chamber). In some embodiments, instead of GaN modules (809 and 810), the system (802) includes MOCVD modules (821 and 822), which are configured to provide MOCVD processing.

[0092] Figure 9 is a schematic diagram of a template and device epitaxy process (901) for electronic devices and SSL. In some embodiments, process (901) comprises steps (A), (B), and (C). In some embodiments, step (A) comprises generating a nucleation layer of AlN (906) on a sapphire substrate (905) using one or more PVD processes described herein (e.g., sputtering in some embodiments), where the AlN nucleation layer (906) has a thickness of approximately 25 nm (in some such embodiments, step (A) is carried out on module (805) in Figure 8A). In some embodiments, step (B) comprises generating a layer of Hf:GaN (907) on the AlN nucleation layer (906) using one or more PVD processes described herein (e.g., sputtering in some embodiments). In some embodiments, step (B) is carried out in modules (807, 808, 809, and / or 810) of Figure 8A. In some embodiments, step (C) includes the step of generating an N-period alternating layer (e.g., a distributed Bragg reflector) (908) of Hf:GaN and HfN on layer (907), based on the GEMM description of U.S. Patent No. 7,915,624, 8,253,157, and / or 8,890,183 introduced above and incorporated herein by reference (in some such embodiments, step (C) is carried out in GEMM module (806) of Figure 8A). In some embodiments, one or more steps (A), (B), and (C) include producing an n-type GaN layer (920) and a p-type GaN / multiple quantum well (MQW) layer (921) using a MOCVD process (in some such embodiments, the thickness of layer (920) is approximately 5 micrometers (μm); in other such embodiments, the thickness of layer (920) is less than approximately 1 μm). In some embodiments, the layers (920 and 921) are produced in the module (920 and / or 921) of Figure 8B.

[0093] Figure 10 shows the n-type carrier concentration (per cubic centimeter) versus adsorbed atom mobility (cm²) for hafnium-doped gallium nitride produced according to some embodiments of the present invention. 2 This is graph (1001) showing / V·s).

[0094] Figure 11 is a graph (1101) showing X-ray diffraction (XRD) data for GaN produced according to some embodiments of the present invention. In some embodiments, the full width at half maximum (FWHM) of the ω-rocking curve of the 002 peak is 300 arcsec.

[0095] Figure 12 is a schematic diagram of a GaN template structure (1201) for subsequent LED epitaxial growth. In some embodiments, structure (1201) includes one or more indium tin oxide (ITO) substituted layers for use with thin films and standard light-emitting device apparatus. In some embodiments, the ITO substituted layers include transition metal element-doped GaN so as to be patterned (e.g., pyramidal, dome, 2D photonic crystal, etc.) and form patterned, transition metal-doped GaN such as Hf:GaN, Hf:AlGaN, Hf:InGaN, Hf:InGaAlN or similar. In some embodiments, for p-side-up devices, the ITO substitution layer includes a layer of Hf:GaN (1205) directly positioned on top of the p-type GaN / MQW layer (921) and a layer of Si:GaN (1206) directly positioned below the p-type GaN / MQW layer (921) (in some such embodiments, having a thickness of less than 1 μm). In some embodiments, for p-side-down devices, the ITO substitution layer includes a layer of Hf:GaN (1207) directly positioned on top of the AlN nucleation layer (906). In some embodiments, the PVD process (e.g., sputtering) used to produce the Hf:GaN described herein has a low processing temperature, which makes the ITO layer usable both pre-epitaxy and post-epitaxy (and therefore, in some such embodiments, tetrakisdimethylaminohafnium, commonly used in MOCVD systems, is not required).

[0096] Figure 13 is a schematic diagram of a GEMM / GaN epitaxial stack structure (1301). In some embodiments, structure (1301) includes a sapphire (Al2O3) substrate layer (1305) and five-period alternating layers of GEMM and GaN (1306). In some embodiments, structure (1301) is lattice-matched for epi-ready growth, has high conductivity (low resistance), and higher reflectivity than an AlN / GaN distributed Bragg reflector (DBR). In some embodiments, GEMM growth is carried out in accordance with the description in U.S. Patents 7,915,624, 8,253,157, and / or 8,890,183, which are introduced above and incorporated herein by reference.

[0097] Figure 14A is a graph (1401) of X-ray diffraction (XRD) data for GaN generated according to some embodiments of the present invention. In some embodiments, GaN is lattice-matched with a low rocking curve full width at half maximum (FWHM) value (e.g., a mismatch of 0.35% in some embodiments).

[0098] Figure 14B is a graph (1402) of X-ray diffraction (XRD) data for GaN generated according to some embodiments of the present invention.

[0099] Figure 14C is a graph (1403) of X-ray diffraction (XRD) data for GaN generated according to some embodiments of the present invention.

[0100] Figure 14D is a graph (1404) of X-ray diffraction (XRD) data for GaN generated according to some embodiments of the present invention.

[0101] Figure 15 is a chart (1501) of atomic force microscopy (AFM) data for GaN on a GEMM produced according to some embodiments of the present invention. In some embodiments, the GaN on the GEMM has an ultrasmooth atomic step surface that allows for the uniform growth of thin quantum wells.

[0102] Figure 16 is a graph (1601) showing a comparison of the reflectivity of GEMM / GaN (solid line) versus conventional AlN / GaN distributed Bragg reflectors (DBR) (dashed line) produced according to several embodiments of the present invention. In some embodiments, the center wavelength λ0 is between 400 nanometers (nm) and 700 nm, depending on the material selection and its thickness.

[0103] Figure 17 is a graph (1701) of estimated sputtering rate versus gallium target temperature for gallium nitride (GaN). Graph (1701) shows that in some embodiments, the estimated sputtering rate is temperature-sensitive when the gallium target temperature is in region (1705) (i.e., above approximately 14 degrees Celsius (°C)). Graph (1701) shows that in some embodiments, the estimated sputtering rate is insensitive when the gallium target temperature is in region (1706) (i.e., below approximately 14°C). Graph (1701) further shows that in some embodiments, the melting point of gallium (1799) (approximately 29°C) falls within the temperature-sensitive region (1705). In some embodiments, the present invention cools the gallium target so that it is within the insensitive region (1706). In some embodiments, cooling the gallium target involves creating a temperature gradient across the depth of the gallium target such that a first depth of the gallium target is at a first temperature and a second depth is at a second temperature.

[0104] In some embodiments, the temperature of the gallium target is kept low for reliable and repeatable manufacturing and high-quality films. In some embodiments, if the gallium is liquid, gallium spitting on the wafer may interfere with manufacturing. In some embodiments, if the target is kept at a temperature close to the melting point of gallium (1799) (e.g., above + / - 20°C above the melting point (1799)), the yield of emitted atoms will be highly dependent on slight changes in process parameters, and the energy of the emitted atoms will have a wide distribution.

[0105] In some embodiments, lowering the temperature of the gallium sputtering target to below 28 degrees Celsius (°C) improves the repeatability and quality of the resulting gallium nitride (GaN) film. In some embodiments, the quality of the resulting GaN film improves down to -40°C, and in some embodiments, further lowering the temperature (e.g., -200°C) results in further improvement of GaN crystal quality. In some embodiments, the reason for the improved film quality is the refinement of gallium purity during the sputtering process, where impurities have a lower sputtering rate at lower target temperatures. Furthermore, in some embodiments, the improvement is due to a reduction in "gallium spitting," where the plasma gas (e.g., noble gases and possibly reactive gases) has shallower penetration into the gallium target. In some embodiments, the present invention includes noble gases and ion sources for sputtering (e.g., in some embodiments, helium (He), neon (Ne), argon (Ar), krypton (Kr), xenon (Xe), radon (Rn), and / or oganesson (Og)).

[0106] In some embodiments of the epitaxial atomic layer sputtering (EALS) provided by the present invention, the gallium sputtering target is kept solid and colder than its melting point at at least 15 degrees Celsius (°C). In some embodiments, the temperature of the gallium sputtering target is comprehensively equal to or between 0°C and 15°C; in some embodiments, the target temperature is comprehensively between -15°C and 0°C; in some embodiments, the target temperature is comprehensively equal to or between -40°C and -15°C; in some embodiments, the target temperature is comprehensively equal to or between -100°C and -40°C; in some embodiments, the target temperature is comprehensively equal to or between -200°C and -100°C; and in some embodiments, the target temperature is less than -200°C. In some embodiments, the target temperature for gallium sputtering is between 14°C and -273°C.

[0107] In some embodiments, the present invention provides a method for producing a gallium nitride (GaN)-based device, the method comprising the steps of: providing a substrate mold containing aluminum nitride; and depositing a patterned transition metal-doped GaN layer onto the substrate mold.

[0108] Conventional techniques avoid gallium deposition by sputtering, particularly when wafer temperatures are several hundred degrees higher than in most applications, and when the wafer-to-target distance is only a few centimeters, due to gallium's low melting point (approximately 29°C).

[0109] In some embodiments, the present invention provides GaN growth by sputtering from a gallium target (solid or liquid) having an XRD 102 peak with an FWHM of less than approximately 3000 arcsecs. In some embodiments, the present invention provides GaN for use with high electron mobility transistors, where the GaN has an XRD 102 peak with an FWHM of less than 1500 arcsecs. In some embodiments, the present invention provides GaN for use with light-emitting devices, where the GaN has an XRD 102 peak with an FWHM of less than 600 arcsecs (e.g., 300 arcsecs). In some embodiments, the present invention provides smooth, non-columnar step growth of GaN by PVD (e.g., sputtering). In some such embodiments, the gallium target is maintained below 14°C (in some embodiments, the gallium target is maintained at sub-zero Celsius temperatures, and a non-aqueous heat transfer fluid such as alcohols is used). In some embodiments, the present invention provides an EALS process to achieve commercial atomic force microscopy (AFM), optical diffraction, and X-ray diffraction (XRD) results.

[0110] In some embodiments, the present invention provides an epitaxial atomic layer sputtering (EALS) process (e.g., GaN, AlN, nucleation layer (described below), or GaN growth on a similar template) comprising one or more of the following: (1) high-temperature annealing; (2) growing Ga:N at a higher-than-standard temperature (e.g., 20°C to 50°C higher) for 5 to 20 minutes in a ratio of 1 or more; (3) growing Ga:N at a standard growth mode (e.g., 700°C) for 20 to 40 minutes in a ratio of 1 or more; (4a) stopping the growth and annealing at 750°C (e.g., annealing for 5 to 10 minutes) until all excess gallium has evaporated and the film is smooth; or (4b) continuing the growth so that the Ga:N ratio is less than 1 (in some such embodiments, the gallium may be blocked or a shutter may be closed); and (5) repeating steps 1 to 4. In some embodiments, RF nitrogen is used instead of N2 or NH3 gas while argon is supplied directly to the gallium target at any time during the above steps, and in some embodiments, an ion source from the gallium target or a separate ion source is used. In some embodiments, doping with hafnium (Hf), zirconium (Zr), silicon (Si), germanium (Ge), magnesium (Mg), copper (Cu), or other transition metals is performed during the above steps. In some embodiments, alloying GaN with aluminum (Al), indium (In), or other transition metals including Hf, Zr, or scandium (Sc) is performed during the above steps.

[0111] In some embodiments, the present invention provides a process for generating a nucleated layer on a mold of a different kind (e.g., Si, sapphire, hafnium nitride (HfN), zirconium nitride (ZrN), zinc oxide (ZnO), glass, or the like), wherein the process comprises one or more of the following: (1) chemically accelerated thermal cleaning, thermal texturing; (2) high-temperature nitriding by exposure to a nitrogen source including N2, nitrogen ions, NH3, or the like; and (3) deposition of AlN (optionally GaN) to a thickness in the range of about 5 nanometers (nm) to 100 nm by sputtering. In some embodiments, RF nitrogen is used instead of N2 gas or NH3 gas while argon is supplied directly to the gallium target at any time during the above steps, and in some embodiments, an ion source from the gallium target or a separate ion source is used. In some embodiments, doping with any of Hf, Zr, Si, Ge, Mg, Cu, or other transition metals is performed during the above steps. In some embodiments, GaN is alloyed with Al, In, or any other transition metal, such as Hf, Zr, or Sc, during the above process.

[0112] Figure 18 is a schematic diagram of a sputtering system (1801). In some embodiments, the system (1801) includes a plurality of Ga guns, including a gallium (Ga) gun (1810) (located at zero degrees from the mold (1805)), a Ga gun (1811) (located at 45 degrees from the mold (1805)), and a Ga gun (1812) (located at 90 degrees from the mold (1805)). In some embodiments, the system (1801) further includes a plurality of ion sources (1(820) and / or 1821), in which the mold (1805) rotates between the Ga guns (1810-1812) and the ion sources (1820 and / or 1821). In some embodiments, for manufacturing stability and quality of the Group IIIA nitride film, it is important to adequately supply ions to the surface by either a sputtering gun or an ion gun. In some embodiments, the ion gun is replaced with a photon source (e.g., ultraviolet light) or an electron source. The ion source (e.g., ion source (1820) and / or ion source (1821)) is best provided at an angle between shallow and 90 degrees to the surface of the mold (1805), whether it is from a dedicated ion source or from the sputtering target. In some embodiments, argon is supplied to the sputtering gun while these components are in place, and the process is performed in a nitrogen toxicity reduction regime to minimize the amount of nitrogen interaction with the gallium target.

[0113] In some embodiments, the present invention provides a method for growing a gallium nitride (GaN) structure by epitaxy, the method comprising the steps of: providing a substrate; and growing at least a first GaN layer on the surface of the substrate using a first physical vapor deposition (PVD) process (e.g., sputtering in some embodiments), wherein the first PVD process comprises: providing a solid gallium target; and maintaining the solid gallium target at a first temperature of less than approximately 29 degrees Celsius.

[0114] In some embodiments of the method, the step of providing a substrate includes growing an aluminum nitride (AlN) layer on a substrate base using a second PVD process (e.g., sputtering in some embodiments) such that the AlN layer forms the surface of the substrate. In some embodiments, the first PVD process further includes epitaxial atomic layer sputtering (EALS). In some embodiments, the first PVD process further includes EALS, where EALS includes heating the substrate. In some embodiments, the first PVD process further includes magnetron sputtering. In some embodiments, the first temperature is less than approximately 15 degrees Celsius. In some embodiments, maintaining a solid gallium target at the first temperature includes fluid convection cooling of the solid gallium target using an alcohol-based liquid. In some embodiments, the first GaN layer has ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurements of both 002 and 102 peaks less than approximately 1000 arcsecs.

[0115] In some embodiments, the present invention provides a method for growing a gallium nitride (GaN) structure, the method comprising: providing a substrate; growing at least a first GaN layer on the surface of the substrate using a first physical vapor deposition (PVD) process (e.g., a first sputtering process in some embodiments); wherein the first PVD process includes: providing a solid gallium target, wherein providing the solid gallium target includes maintaining the solid gallium target at a first temperature; and carrying out epitaxial atomic layer sputtering (EALS) of at least the first GaN layer such that the growth of the at least first GaN layer includes the growth of the at least first GaN layer in non-columnar steps.

[0116] In some embodiments, the present invention provides a system for growing gallium nitride (GaN) structures, the system comprising: a load lock configured to load a substrate wafer into the system and remove a GaN structure from the system; a plurality of deposition modules, wherein the plurality of deposition modules include a GaN deposition module configured to grow at least a first GaN layer on the surface of a substrate wafer via a first physical vapor deposition (PVD) process (e.g., a first sputtering process in some embodiments), wherein the GaN deposition module includes a solid gallium target maintained at a first temperature, and wherein the first PVD process includes epitaxial atomic layer sputtering (EALS) of at least the first GaN layer such that non-columnar step growth of at least the first GaN layer occurs.

[0117] In some embodiments, the present invention provides a method for growing a gallium nitride (GaN) structure, the method comprising the steps of: providing a substrate; and growing at least one first GaN layer on the surface of the substrate using a first sputtering process, wherein the first sputtering process comprises: providing a gallium target; and performing epitaxial atomic layer sputtering (EALS) such that the growth of at least the first GaN layer includes the growth of at least one non-columnar step of the GaN layer.

[0118] In some embodiments, the implementation of MEE includes controlling the nitrogen-to-gallium ratio to be greater than 1:1 for at least a first time of the first sputtering process. In some embodiments of the method, the implementation of MEE includes introducing nitrogen via a radio frequency (RF) nitrogen source.

[0119] In some embodiments of the method, the first sputtering process further includes doping at least a first GaN layer with silicon (Si). In some embodiments, the first sputtering process further includes doping at least a first GaN layer by gas injection of reactants using a carrier gas that retains silicon (Si).

[0120] In some embodiments of the method, the gallium target is a solid gallium target, wherein the first sputtering process further includes maintaining the solid gallium target at a first temperature of approximately less than 15 degrees Celsius.

[0121] In some embodiments of the method, the step of providing a substrate includes growing an aluminum nitride (AlN) layer on the base of the substrate using a second sputtering process such that the AlN layer forms the surface of the substrate. In some embodiments, the method further includes growing a grown epitaxial metal mirror (GEMM) on at least a first GaN layer. In some embodiments, the method further includes growing a grown epitaxial metal mirror (GEMM) on at least a first GaN layer, wherein the GEMM comprises alternating layers of hafnium (Hf):GaN and hafnium nitride (HfN). In some embodiments, the method further includes growing a grown epitaxial metal mirror (GEMM) on at least a first GaN layer, wherein the GEMM comprises alternating layers of hafnium (Hf):GaN and hafnium nitride (HfN); and growing at least a first quantum well on the surface of the GEMM using a metal-organic vapor deposition (MOCVD) process. In some embodiments, the first sputtering process further includes magnetron sputtering. In some embodiments, at least the first GaN layer has ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurements of both the 002 peak and the 102 peak for less than approximately 1000 arcsec. In some embodiments, at least the first GaN layer has ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurements of the 002 peak in the range of about 10 arcsec to about 2500 arcsec.

[0122] In some embodiments, the present invention provides a system for growing a gallium nitride (GaN) structure, the method comprising: a load lock configured to load a substrate wafer into the system and remove a GaN structure from the system; a plurality of deposition chambers, wherein the plurality of deposition chambers comprises a GaN deposition chamber configured to grow at least a first GaN layer on the surface of a substrate wafer by a first sputtering process, wherein the first sputtering process comprises epitaxial atomic layer sputtering (EALS) of at least the first GaN layer such that non-columnar step growth of at least the first GaN layer occurs.

[0123] In some embodiments, the system further includes a wafer handling mechanism configured to automatically move a substrate wafer between a plurality of deposition chambers. In some embodiments, the plurality of deposition chambers include an aluminum nitride (AlN) deposition chamber configured to grow an AlN layer on the base of a substrate wafer by a second sputtering process such that the AlN layer forms the surface of the substrate wafer. In some embodiments, the plurality of deposition chambers include a grown epitaxial metal mirror (GEMM) deposition chamber configured to grow a GEMM on at least a first GaN layer. In some embodiments, the GaN deposition chamber includes a solid gallium target maintained at a first temperature, where the first temperature is approximately less than 15 degrees Celsius. In some embodiments, the GaN deposition chamber further includes; a solid gallium target maintained at the first temperature; and a fluid convection cooling device configured to cool the solid gallium target with an alcohol-based liquid.

[0124] In some embodiments, the GaN deposition chamber is further configured to dopage at least a first GaN layer with silicon (Si). In some embodiments, the GaN deposition chamber is further configured to grow at least a first GaN layer such that at least a first GaN layer has ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurements of both the 002 peak and the 102 peak in the range of approximately 1000 arcsec. In some embodiments, the GaN deposition chamber is further configured to grow at least a first GaN layer such that at least a first GaN layer has ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurements of the 002 peak in the range of approximately 10 arcsec to approximately 2500 arcsec.

[0125] In some embodiments, the deposition chambers further include: an aluminum nitride (AlN) deposition chamber configured to grow an AlN layer on a substrate wafer by a second sputtering process such that the AlN layer forms the surface of the substrate wafer; a grown epitaxial metal mirror (GEMM) deposition chamber configured to grow a GEMM on at least a first GaN layer, wherein the GEMM comprises alternating layers of hafnium (Hf):GaN and hafnium nitride (HfN); and a metal-organic vapor deposition (MOCVD) chamber configured to grow at least a first quantum well on the surface of the GEMM.

[0126] In some embodiments, the present invention provides a gallium nitride structure comprising: a substrate; and at least a first gallium nitride (GaN) layer grown on the surface of the substrate, wherein the at least first GaN layer has ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurements of both 002 and 102 peaks in the range of about 1000 arcsec (in some embodiments, the at least first GaN layer has ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurements of 002 peaks in the range of about 10 arcsec to about 2500 arcsec).

[0127] In some embodiments, the structure further includes an AlN layer grown on a base of the substrate such that the aluminum nitride (AlN) layer forms the surface of the substrate. In some embodiments, the structure further includes a grown epitaxial metal mirror (GEMM) grown on the surface of at least a first GaN layer. In some embodiments, the substrate includes sapphire, and the structure further includes: an aluminum nitride (AlN) layer on a base of the substrate such that the AlN layer forms the surface of the substrate; a grown epitaxial metal mirror (GEMM) grown on the surface of at least a first GaN layer; where the GEMM includes alternating layers of hafnium (Hf):GaN and hafnium nitride (HfN); a layer of n-type GaN grown on the surface of the GEMM; and a layer of p-type GaN / multiple quantum wells (MQW) grown on the layer of n-type GaN.

[0128] In some embodiments, the present invention provides a system for growing gallium nitride (GaN) structures, the system comprising: means for loading a substrate wafer into the system; and means for sputtering at least a first GaN layer on the surface of the substrate wafer, wherein the means for sputtering at least a first GaN layer includes means for performing epitaxial atomic layer sputtering (EALS) such that non-columnar step growth of at least a first GaN layer occurs.

[0129] In some embodiments of the system, means for sputtering include means for doping at least a first GaN layer with silicon (Si). In some embodiments, the system further includes means for growing an AlN layer on a substrate base such that an aluminum nitride (AlN) layer forms the surface of the substrate. In some embodiments, the system further includes means for growing a grown epitaxial metal mirror (GEMM) on at least a first GaN layer, wherein the GEMM comprises alternating layers of hafnium (Hf):GaN and hafnium nitride (HfN); and means for growing at least a first quantum well on the surface of the GEMM.

[0130] In some embodiments, the present invention provides a method for growing a gallium nitride (GaN) structure, the method comprising the steps of: providing a mold; and growing at least one first GaN layer on the mold using a first sputtering process, wherein the first sputtering process comprises: controlling the temperature of a sputtering target; and repeatedly adjusting between gallium-rich and gallium-lean conditions, wherein the gallium-rich condition comprises a gallium-to-nitrogen ratio having a first value greater than 1, and wherein the gallium-lean condition comprises a gallium-to-nitrogen ratio having a second value less than 1.

[0131] In some embodiments, the first sputtering process includes introducing nitrogen via a radio frequency (RF) nitrogen source. In some embodiments, the first sputtering process further includes doping at least a first GaN layer with silicon (Si). In some embodiments, the first sputtering process further includes doping at least a first GaN layer by gas injection of reactants using a carrier gas that retains silicon (Si). In some embodiments, the sputtering target is a solid gallium target, where controlling the temperature of the solid gallium target includes maintaining its temperature at a first temperature value which is approximately less than 14°C. In some embodiments, the sputtering target is a solid gallium target, where maintaining the temperature of the solid gallium target includes fluid convection cooling of the solid gallium target using alcohol as a heat transfer fluid.

[0132] In some embodiments, the step of providing a mold includes growing an aluminum nitride (AlN) layer on the mold. In some embodiments, the step of providing a mold includes growing an aluminum nitride (AlN) layer on the mold using a second sputtering process. In some embodiments, the step of providing a mold includes growing a first aluminum nitride (AlN) layer on the mold using a second sputtering process, wherein the method further includes the steps of growing a second aluminum nitride (AlN) layer on at least a first GaN layer using a second sputtering process; and growing a second GaN layer on the second AlN layer using a first sputtering process.

[0133] In some embodiments, the method further comprises the step of growing a grown epitaxial metal mirror (GEMM) on at least a first GaN layer, wherein the GEMM comprises alternating layers of hafnium (Hf):GaN and hafnium nitride (HfN). In some embodiments, the method further comprises the steps of: growing a grown epitaxial metal mirror (GEMM) on at least a first GaN layer, wherein the GEMM comprises alternating layers of hafnium (Hf):GaN and hafnium nitride (HfN); and growing at least a first quantum well on the surface of the GEMM using a metal-organic vapor deposition (MOCVD) process. In some embodiments, the first sputtering process further comprises magnetron sputtering. In some embodiments, the at least first GaN layer has ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurements with a 002 peak in the range of about 10 arcsec to about 2500 arcsec.

[0134] In some embodiments, the present invention provides a system for growing a gallium nitride (GaN) structure, the method comprising: a load lock configured to load a substrate wafer into the system and remove a GaN structure from the system; a plurality of deposition chambers, wherein the plurality of deposition chambers comprises a GaN deposition chamber configured to grow at least a first GaN layer on a mold comprising a substrate wafer by a first sputtering process, wherein the first sputtering process comprises repeated adjustments between gallium-rich and gallium-lean conditions, wherein the gallium-rich condition comprises a gallium-to-nitrogen ratio having a first value greater than 1, and the gallium-lean condition comprises a gallium-to-nitrogen ratio having a second value less than 1.

[0135] In some embodiments, the system further includes a wafer handling mechanism configured to automatically move the mold between a plurality of deposition chambers. In some embodiments, the plurality of deposition chambers include an aluminum nitride (AlN) deposition chamber configured to grow an AlN layer on a substrate wafer by a second sputtering process to form a mold. In some embodiments, the plurality of deposition chambers include a grown epitaxial metal mirror (GEMM) deposition chamber configured to grow a GEMM on at least a first GaN layer. In some embodiments, the GaN deposition chamber includes a solid gallium target maintained at a first temperature, where the first temperature is approximately less than 14 degrees Celsius. In some embodiments, the GaN deposition chamber further includes; a solid gallium target maintained at the first temperature; and a fluid convection cooling device configured to cool the solid gallium target by an alcohol heat transfer fluid. In some embodiments, the GaN deposition chamber is further configured to dopage at least a first GaN layer with silicon (Si). In some embodiments, the GaN deposition chamber is further configured to grow at least a first GaN layer, such that the at least first GaN layer has an ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurement of 002 peaks in the range of about 10 arcsec to about 2500 arcsec. In some embodiments, the deposition chambers further include: an aluminum nitride (AlN) deposition chamber configured to grow an AlN layer on a substrate wafer for forming a template by a second sputtering process; a grown epitaxial metal mirror (GEMM) deposition chamber configured to grow a GEMM on at least a first GaN layer, where the GEMM comprises alternating layers of hafnium (Hf):GaN and hafnium nitride (HfN); and a metal-organic vapor deposition (MOCVD) chamber configured to grow at least a first quantum well on the surface of the GEMM.

[0136] In some embodiments, the present invention provides a gallium nitride structure comprising: a mold; and at least a first gallium nitride (GaN) layer grown on the mold, wherein the at least first GaN layer has an ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurement of a 002 peak in the range of about 10 arcsec to about 2500 arcsec.

[0137] In some embodiments, the template includes an aluminum nitride (AlN) layer grown on a substrate. In some embodiments, the structure further includes a grown epitaxial metal mirror (GEMM) grown on the surface of at least a first GaN layer. In some embodiments, the template is a gallium nitride structure including an aluminum nitride (AlN) layer grown on a sapphire substrate, the structure further includes a grown epitaxial metal mirror (GEMM) on the surface of at least a first GaN layer, where the GEMM includes alternating layers of hafnium (Hf):GaN and hafnium nitride (HfN); a layer of n-type GaN grown on the surface of the GEMM; and a layer of p-type GaN / multiple quantum wells (MQW) grown on the layer of n-type GaN.

[0138] In some embodiments, the present invention provides a system for growing a gallium nitride (GaN) structure, the system comprising: means for loading a substrate wafer into the system; and means for sputtering at least a first GaN layer on a mold containing the substrate wafer, wherein the means for sputtering at least a first GaN layer comprises means for repeatedly adjusting between gallium-rich and gallium-lean conditions, wherein the gallium-rich condition comprises a gallium-to-nitrogen ratio having a first value greater than 1, and wherein the gallium-lean condition comprises a gallium-to-nitrogen ratio having a second value less than 1.

[0139] In some embodiments of the system, means for sputtering include means for doping at least a first GaN layer with silicon (Si). In some embodiments, the system further includes means for growing an aluminum nitride (AlN) layer on a substrate wafer for forming a template. In some embodiments, the system further includes means for growing a grown epitaxial metal mirror (GEMM) on at least a first GaN layer, wherein the GEMM comprises alternating layers of hafnium (Hf):GaN and hafnium nitride (HfN); and means for growing at least a first quantum well on the surface of the GEMM.

[0140] In some embodiments, the present invention provides a method for growing a gallium nitride (GaN) structure, the method comprising the steps of: providing a mold; and growing at least one first GaN layer on the mold using a first sputtering process, wherein the first sputtering process comprises: providing a gallium sputtering target, wherein the gallium sputtering target has depth; and maintaining the temperature of the gallium sputtering target at a first temperature value which is less than approximately 14°C. In some embodiments, the step of maintaining the temperature of the gallium sputtering target comprises the step of creating a temperature gradient across the depth of the gallium sputtering target.

[0141] In some embodiments, the present invention provides a method for growing a gallium nitride (GaN) structure, the method comprising: providing a mold having a surface; and growing at least one first GaN layer on the mold using a first sputtering process, wherein the first sputtering process comprises: repeatedly adjusting a gallium-rich condition and a gallium-lean condition on the surface of the mold for at least a first amplitude (oscillation), wherein the gallium-rich condition comprises a gallium-to-nitrogen ratio having a first value greater than 1, and wherein the gallium-lean condition comprises a gallium-to-nitrogen ratio having a second value less than the first value. In some embodiments, the repeated adjustment comprises repeatedly adjusting for a plurality of amplitudes, including the first amplitude. In some embodiments, at least the first GaN layer has a 10² peak ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurement in the range of about 10 arcsec to about 2500 arcsec.

[0142] In some embodiments, the present invention provides a method for growing a gallium nitride (GaN) structure, the method comprising the steps of: providing a mold; and growing at least one first GaN layer on the mold using a first sputtering process, wherein the first sputtering process comprises: providing a gallium sputtering target, wherein the gallium sputtering target has depth; and maintaining the temperature of the gallium sputtering target at a first temperature value which is less than approximately 14°C. In some embodiments, at least the first GaN layer has 10² peak ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurements in the range of about 10 arcsec to about 2500 arcsec. In some embodiments, the step of maintaining the temperature of the gallium sputtering target includes the step of providing a temperature gradient over the depth of the gallium sputtering target.

[0143] In some embodiments, the present invention provides a method for growing a gallium nitride (GaN) structure, the method comprising: providing a mold; growing a first aluminum nitride (AlN) layer on the mold using a first sputtering process; and growing a first GaN layer on the first AlN layer using a second sputtering process. In some embodiments, the method further comprises: growing a second AlN layer on the first GaN layer using a first sputtering process; and growing a second GaN layer on the second AlN layer using a second sputtering process. In some embodiments, the first GaN layer has 10² peak ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurements in the range of about 10 arcsec to about 2500 arcsec.

[0144] In some embodiments, the present invention provides a method for growing a gallium nitride (GaN) structure, the method comprising: providing a mold having a surface; growing at least one first GaN layer on the mold using a first sputtering process; wherein the first sputtering process: growing at least the first GaN layer under at least two conditions, wherein the two conditions include a gallium-rich condition and a gallium-lean condition, wherein the gallium-rich condition includes a gallium-to-nitrogen ratio having a first value greater than 1, and wherein the gallium-lean condition includes a gallium-to-nitrogen ratio having a second value less than the first value; and alternating between the two conditions for at least a first growth under the first of the two conditions, a second growth under the second of the two conditions after the first growth, and a third growth under the first of the two conditions after the second growth. In some embodiments, the step of alternating between two conditions further includes a fourth growth under the second of two conditions after the third growth, and a fifth growth under the first of two conditions after the fourth growth. In some embodiments, the first value of the gallium-to-nitrogen ratio is at least 10 percent greater than the second value of the gallium-to-nitrogen ratio. In some embodiments, the first value of the gallium-to-nitrogen ratio is at least 50 percent greater than the second value of the gallium-to-nitrogen ratio. In some embodiments, the first value of the gallium-to-nitrogen ratio is at least twice as great as the second value of the gallium-to-nitrogen ratio.

[0145] In some embodiments, the present invention provides a method for growing a gallium nitride (GaN) structure, the method comprising: providing a mold; growing a first aluminum nitride (AlN) layer on the mold using a first sputtering process; and growing a first GaN layer on the first AlN layer using a second sputtering process. In some embodiments, the method further comprises: growing a second AlN layer on the first GaN layer using a first sputtering process; and growing a second GaN layer on the second AlN layer using a second sputtering process. In some embodiments, the first GaN layer has 10² peak ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurements in the range of about 10 arcsec to about 2500 arcsec. In some embodiments, the method further comprises: growing a second AlN layer on a first GaN layer using a first sputtering process; growing a second GaN layer on a second AlN layer using a second sputtering process; and growing an Al on the second GaN layer. x Ga (1-x) A step of growing one or more layers of N, wherein x comprehensively includes 0 and 1; and a step of growing a second AlN layer on a first GaN layer using a first sputtering process; a step of growing a second GaN layer on a second AlN layer using a second sputtering process; and an Al on a second GaN layer x Ga (1-x)A step of growing one or more layers of N, where x varies with depth and comprehensively includes 0 and 1; In some embodiments, the method further includes a step of growing a second AlN layer on a first GaN layer using a first sputtering process; a step of growing a second GaN layer on a second AlN layer using a second sputtering process; and a step of growing one or more layers of a compound on the second GaN layer, wherein the compound comprises one or more selected from the group consisting of hafnium nitride (HfN), zirconium nitride (ZrN), aluminum nitride (AlN), gallium nitride (GaN), and scandium nitride (ScN). In some embodiments, the method further includes Al on a first GaN layer x Ga (1-x) The method includes the step of growing one or more layers of N, where x is comprehensively between 0 and 1. In some embodiments, the first sputtering process further includes doping at least the first GaN layer with silicon (Si). In some embodiments, the method further includes doping Al on the first GaN layer. x Ga (1-x) The method includes the step of growing one or more layers of N, where x is comprehensively between 0 and 1. In some embodiments, the method further includes Al on the first GaN layer. x Ga (1-x) The method includes the step of growing one or more layers of N, where x varies with depth and is comprehensively between 0 and 1. In some embodiments, the method further includes the step of growing one or more layers of a compound on a first GaN layer, wherein the compound comprises one or more selected from the group consisting of hafnium nitride (HfN), zirconium nitride (ZrN), aluminum nitride (AlN), gallium nitride (GaN), and scandium nitride (ScN).

[0146] In some embodiments, the present invention provides a system for growing a gallium nitride (GaN) structure, the system comprising: a load lock configured to load a substrate wafer into the system and remove a GaN structure from the system; a plurality of deposition chambers, wherein the plurality of deposition chambers include a first GaN deposition chamber configured to grow at least a first GaN layer on a mold comprising a substrate wafer by a first sputtering process, wherein the first GaN deposition chamber comprises a gallium sputtering target, wherein the gallium sputtering target has depth, and wherein the GaN deposition chamber is further configured to maintain the temperature of the gallium sputtering target at a first temperature value which is less than approximately 14°C.

[0147] In some embodiments, the system further includes a wafer handling mechanism configured to automatically move a mold between a plurality of deposition chambers. In some embodiments, the plurality of deposition chambers include an aluminum nitride (AlN) deposition chamber configured to grow an AlN layer on a substrate wafer for forming a mold by a second sputtering process. In some embodiments, the plurality of deposition chambers include a grown epitaxial metal mirror (GEMM) deposition chamber configured to grow a GEMM on at least a first GaN layer. In some embodiments, the system further includes a fluid convection cooling device configured to cool a gallium sputtering target with an alcohol heat transfer fluid. In some embodiments, the GaN deposition chamber is further configured to maintain a temperature gradient over the depth of the gallium sputtering target. In some embodiments, the plurality of deposition chambers include a metal-organic vapor deposition (MOCVD) chamber. In some embodiments, the GaN deposition chamber is further configured to dopage at least a first GaN layer with silicon (Si).

[0148] In some embodiments, the present invention provides a gallium nitride structure comprising: a template; and at least a first gallium nitride (GaN) layer grown on the template, wherein the at least first GaN layer has 10² peak ω-rocking curve full width at half maximum (FWHM) X-ray diffraction measurements in the range of about 10 arcsec to about 2500 arcsec. In some embodiments, the template comprises an aluminum nitride (AlN) layer grown on a sapphire substrate, the structure further comprising a growable epitaxial metal mirror (GEMM) grown on the surface of at least the first GaN layer, wherein the GEMM comprises: alternating layers of hafnium (Hf):GaN and hafnium nitride (HfN); a layer of n-type GaN grown on the surface of the GEMM; and a layer of p-type GaN / multiple quantum wells (MQW) grown on the n-type GaN layer.

[0149] It is explicitly intended that the present invention includes embodiments having combinations and partial combinations of the various embodiments and features described herein (i.e., rather than describing all combinations of elements, this specification includes descriptions of representative embodiments and includes embodiments that include some features from one embodiment combined with some features from another embodiment). Furthermore, some embodiments include fewer components than all components described as part of any one of the embodiments described herein. Moreover, it is explicitly intended that the present invention includes combinations and partial combinations of the various embodiments described herein and embodiments described in related applications and publications incorporated by reference in the paragraphs of this application.

[0150] It should be understood that the features described above are illustrative and not limiting. While many features and benefits of various embodiments as described herein have been shown in the preceding description, many other embodiments and variations to the details, in addition to structural and functional details of various embodiments, will become apparent to those skilled in the art in considering the above description. Therefore, the scope of the invention should be determined by referring to the appended claims in addition to the entire scope, which is equivalent to the rights granted by the patent claims. In the appended claims, the terms “including” and “in which” are used as plain English synonyms for the terms “comprising” and “wherein,” respectively. Terms such as “first,” “second,” and “third” are used merely as indicators and are not intended to impose any numerical requirements on their objects.

Claims

1. 1. A method for growing a nitride compound structure comprising one or more Group IIIA metals, the Group IIIA metal-containing nitride compound comprising a nitride compound selected from gallium (Ga)-containing GaN, AlGaN, and InGaN, the method comprising: (a) providing a template; (b) growing a first layer of a nitride compound comprising at least said Group IIIA metal on the template using a first sputtering process; wherein the first sputtering process comprises: (i) providing a gallium sputtering target, wherein the gallium sputtering target has a depth; (ii) heating the substrate to less than 800 degrees Celsius; and (iii) maintaining the gallium sputtering target in a frozen state substantially throughout its depth by maintaining the temperature of the gallium sputtering target at a first temperature value that is equal to or less than −40 degrees Celsius; A method comprising:

2. 2. The method of claim 1, wherein the first layer of nitride compound containing at least the Group IIIA metal has an omega rocking curve full width at half maximum (FWHM) x-ray diffraction measurement of 102 peaks in the range of 10 arcsec to 2500 arcsec.

3. 10. The method of claim 1, wherein the first sputtering process further comprises doping the first layer of nitride compound containing at least the Group IIIA metal with silicon (Si).

4. 10. The method of claim 1, wherein maintaining the temperature of the gallium sputtering target comprises fluid convection cooling of a solid gallium target using a cryogenic heat transfer fluid comprised of liquid nitrogen or liquid hydrogen.

5. 1. A method for growing a nitride compound structure comprising one or more Group IIIA metals, the Group IIIA metal-containing nitride compound comprising a nitride compound selected from gallium (Ga)-containing GaN, AlGaN, and InGaN, the method comprising: (a) providing a template; (b) growing a first aluminum nitride (AlN) layer on the mold using a first sputtering process; (c) growing a first layer of a nitride compound containing said Group IIIA metal on the first AlN layer using a second sputtering process; Including, (d) the method, wherein the first layer of Group IIIA metal containing nitride compound has an omega rocking curve full width at half maximum (FWHM) x-ray diffraction measurement of 102 peaks in the range of 10 arcsec to 2500 arcsec.

6. (e) growing a second AlN layer on the first layer of nitride compound containing a Group IIIA metal using the first sputtering process; (f) growing a second layer of a nitride compound containing the Group IIIA metal on the second AlN layer using the second sputtering process; The method of claim 5 further comprising:

7. (e) growing a second AlN layer on the first layer of nitride compound containing a Group IIIA metal using the first sputtering process; (f) growing a second layer of a nitride compound containing the Group IIIA metal on the second AlN layer using the second sputtering process; (g) depositing Al on the second layer of the nitride compound containing a Group IIIA metal. x G (1-x) growing one or more layers of N; 6. The method of claim 5, further comprising:

8. (e) growing a second AlN layer on the first layer of nitride compound containing a Group IIIA metal using the first sputtering process; (f) growing a second layer of a nitride compound containing the Group IIIA metal on the second AlN layer using the second sputtering process; (g) depositing Al on the second layer of the nitride compound containing a Group IIIA metal. x G (1-x) growing one or more layers of N; 6. The method of claim 5, further comprising:

9. (e) growing a second AlN layer on the first layer of nitride compound containing a Group IIIA metal using the first sputtering process; (f) growing a second layer of a nitride compound containing the Group IIIA metal on the second AlN layer using the second sputtering process; (g) growing one or more layers of a compound on said second layer of nitride compound containing a Group IIIA metal; 6. The method of claim 5, further comprising: wherein the compound comprises one or more compounds selected from the group consisting of indium nitride (InN), hafnium nitride (HfN), zirconium nitride (ZrN), aluminum nitride (AlN), gallium nitride (GaN), and scandium nitride (ScN).

10. (e) depositing Al on the first layer of the nitride compound containing a Group IIIA metal. x G (1-x) The method of claim 5 , further comprising growing one or more layers of N, where x is 0 to 1, inclusive.

11. 10. The method of claim 1, wherein the first sputtering process further comprises: (e) doping the first layer of nitride compound containing at least the Group IIIA metal with silicon (Si).

12. 2. The method of claim 1, wherein the first sputtering process further comprises doping a first layer of nitride compound containing at least the Group IIIA metal with germanium (Ge).

13. 2. The method of claim 1, wherein the first sputtering process further comprises doping a first layer of nitride compound containing at least the Group IIIA metal with hafnium (Hf).

14. 2. The method of claim 1, wherein the first sputtering process further comprises doping the first layer of nitride compound containing at least the Group IIIA metal with magnesium (Mg).

15. 6. The method of claim 5, wherein the second sputtering process further comprises doping the first layer of nitride compound containing at least the Group IIIA metal with germanium (Ge).

16. 6. The method of claim 5, wherein the second sputtering process further comprises doping the first layer of nitride compound containing at least the Group IIIA metal with hafnium (Hf).

17. 6. The method of claim 5, wherein the second sputtering process further comprises doping the first layer of nitride compound containing at least the Group IIIA metal with magnesium (Mg).

18. The method of claim 1 , wherein growing the first layer of a nitride compound containing at least the Group IIIA metal comprises step-flow growth.

19. 10. The method of claim 1, wherein growing the first layer of a nitride compound comprising at least the Group IIIA metal comprises two-dimensional (2D) island growth.

20. 1. A method for growing a nitride compound structure comprising one or more Group IIIA metals, the Group IIIA metal-containing nitride compound comprising a nitride compound selected from gallium (Ga)-containing GaN, AlGaN, and InGaN, the method comprising: (a) providing a template; (b) growing a first layer of a nitride compound comprising at least said Group IIIA metal on the template using a first sputtering process; Including, The first sputtering process comprises: (i) providing a gallium sputtering target, the gallium sputtering target having a depth; (ii) heating the substrate to less than 800 degrees Celsius; (iii) maintaining the gallium sputtering target in a frozen state substantially throughout its depth by maintaining the temperature of the gallium sputtering target at a first temperature value equal to or less than 0 degrees Celsius; Including, (iv) a method for growing one or more Group IIIA metal containing nitride compound structures, wherein at least a first layer of said Group IIIA metal containing nitride compound has a ω rocking curve full width at half maximum (FWHM) x-ray diffraction measurement of a 102 peak in the range of 10 arcsec to 2500 arcsec.