Semiconductor wafer evaluation method and semiconductor wafer manufacturing method

JP2023041001A5Active Publication Date: 2024-10-08SUMCO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2022118842
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-09-10
Filing Date
2022-07-26
Publication Date
2024-10-08
Estimated Expiration
2042-07-26

AI Technical Summary

Technical Problem

Existing methods for evaluating semiconductor wafer surface roughness are limited in reducing the influence of various types of noise, particularly frequency-independent noise, which affects the accuracy of the measurement results.

Method used

A method that uses the maximum height (Sz) as an index to determine the acceptability of other roughness parameters, with threshold-based evaluations and re-measurements or recalculations to exclude noise influences, employing optical interference microscopes for precise measurements.

Benefits of technology

This approach allows for accurate evaluation of semiconductor wafer surface roughness by minimizing noise effects, ensuring high-quality product wafers are supplied by identifying and correcting abnormal measurement results.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000013_0000
    Figure 00000013_0000
  • Figure 00000013_0001
    Figure 00000013_0001
  • Figure 00000013_0002
    Figure 00000013_0002
Patent Text Reader

Abstract

To provide a new evaluation method capable of accurately evaluating the surface roughness of a semiconductor wafer.SOLUTION: A semiconductor wafer evaluation method includes obtaining the maximum height Sz and roughness parameters other than Sz by measuring with a roughness measuring device in one or more measurement areas on the surface of a semiconductor wafer to be evaluated, and determining whether the values of roughness parameters other than Sz obtained in the measurement area are values that can be adopted for evaluation of the semiconductor wafer to be evaluated for each measurement area using the value of the maximum height Sz as an index.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for evaluating a semiconductor wafer and a method for manufacturing a semiconductor wafer.

Background Art

[0002] In the manufacturing process of a semiconductor wafer (hereinafter, also simply referred to as "wafer"), usually, for quality control of products, inspections for process control and sampling inspections before shipment from a lot are performed. Examples of inspection items for such inspections include surface roughness (see, for example, Patent Document 1).

Prior Art Documents

Patent Documents

[0003]

Patent Document 1

Summary of the Invention

Problems to be Solved by the Invention

[0004] Semiconductor wafers are generally manufactured by cutting wafers from ingots and applying various processes such as surface polishing. By measuring the surface roughness of the semiconductor wafers thus manufactured, it is possible to evaluate, for example, whether the surface polishing process was performed properly based on the measurement results. Then, by controlling the surface polishing process based on the evaluation results, and / or by distinguishing between good and defective lots, it becomes possible to supply high-quality product wafers to the market. However, various noises may be included in the surface roughness measurement results (see paragraph 0006 of Patent Document 1). In order to improve the accuracy of evaluation based on the surface roughness measurement results, it is desirable to obtain surface roughness measurement results in which the influence of noise is reduced. In this regard, Patent Document 1 proposes a method in which the surface shape of a semiconductor wafer is measured under at least two different measurement conditions, the data of each surface shape is converted into a power spectrum, peaks appearing in the power spectrum whose peak spatial frequencies do not match are identified as noise components, and the identified noise components are removed from at least one of the power spectra before evaluation. However, the inventors believe that such a method is limited to noise that is frequency-dependent (specifically, noise caused by equipment), and that noise caused by external disturbances, which is not frequency-dependent, cannot be removed. However, from the viewpoint of more accurately evaluating the surface roughness of semiconductor wafers, it is desirable to reduce the influence of various types of noise.

[0005] In view of the above, one aspect of the present invention aims to provide a novel evaluation method that can accurately evaluate the surface roughness of a semiconductor wafer. [Means for solving the problem]

[0006] One aspect of the present invention is as follows: [1] Obtaining the maximum height Sz and roughness parameters other than Sz by performing measurements using a roughness measuring device in one or more measurement areas on the surface of the semiconductor wafer to be evaluated, and, For each measurement region, the value of the maximum height Sz is used as an indicator to determine whether the values ​​of roughness parameters other than Sz obtained in that measurement region are acceptable for evaluating the semiconductor wafer under evaluation. A method for evaluating semiconductor wafers, including (hereinafter also simply referred to as "evaluation method"). [2] The semiconductor wafer evaluation method according to [1], which includes, if the value of the maximum height Sz is less than or equal to a preset threshold, adopting the values ​​of roughness parameters other than Sz obtained for one or more measurement regions where the maximum height Sz of said value was obtained as evaluation values ​​for the semiconductor wafer to be evaluated. [3] If the value of the maximum height Sz is equal to or exceeds a preset threshold, the values ​​of roughness parameters other than Sz obtained for the measurement area in which the maximum height Sz of said value was obtained are not used as evaluation values ​​for the semiconductor wafer to be evaluated, as described in [1] or [2]. [4] The semiconductor wafer evaluation method according to [3], further comprising: if the value of the maximum height Sz is equal to or exceeds a preset threshold, the measurement of the measurement area where the maximum height Sz of said value was obtained is performed again using a roughness measuring device. [5] The semiconductor wafer evaluation method according to [3] or [4], further comprising: if the value of the maximum height Sz is equal to or exceeds a preset threshold, performing a measurement using a roughness measuring device in a region other than the measurement region where the maximum height Sz of the value was obtained. [6] A semiconductor wafer evaluation method according to any one of [3] to [5], further comprising recalculating the values ​​of one or more roughness parameters obtained for the measurement region where the maximum height Sz was obtained, if the value of the maximum height Sz is equal to or exceeds a preset threshold. [7] The semiconductor wafer evaluation method described in [6], wherein the above recalculation is performed by excluding the portion that is presumed to be the cause of the abnormal value of the maximum height Sz from the calculation of the roughness parameter. [8] A method for evaluating a semiconductor wafer according to any one of [1] to [7], wherein the roughness parameters other than Sz are one or more roughness parameters selected from the group consisting of arithmetic mean height Sa and root mean square height Sq. [9] The roughness measuring device is an optical interference microscope, a method for evaluating a semiconductor wafer as described in any of [1] to [8].

[10] The above optical interference microscope is a white light interference microscope, the semiconductor wafer evaluation method described in [9].

[11] Manufacturing evaluation semiconductor wafers under test manufacturing conditions, The manufactured evaluation semiconductor wafer is evaluated by any of the evaluation methods described in [1] to

[10] . Based on the results of the above evaluation, either the manufacturing conditions modified from the above test manufacturing conditions will be determined as the actual manufacturing conditions, or the above test manufacturing conditions will be determined as the actual manufacturing conditions, and To manufacture semiconductor wafers under the actual manufacturing conditions determined above, A method for manufacturing semiconductor wafers containing (hereinafter referred to as "Manufacturing Method 1").

[12] The manufacturing conditions to which the above modifications are made include surface polishing conditions for the semiconductor wafer, as described in

[11] .

[13] Manufacturing a semiconductor wafer lot containing multiple semiconductor wafers, Extracting one or more semiconductor wafers from the above semiconductor wafer lot, The extracted semiconductor wafers are evaluated according to one of the evaluation methods described in [1] to

[10] , and Based on the above evaluation, semiconductor wafers from the same semiconductor wafer lot as those judged to be good products will be prepared for shipment as products. A method for manufacturing semiconductor wafers containing (hereinafter referred to as "Manufacturing Method 2"). [Effects of the Invention]

[0007] According to one aspect of the present invention, a novel evaluation method is provided that can accurately evaluate the surface roughness of a semiconductor wafer. [Brief explanation of the drawing]

[0008] [Figure 1]This is an explanatory diagram illustrating the measurement principle of a white light interference microscope. [Figure 2] This shows an example of the change in interference light during fringe scanning in measurements using a white light interference microscope. [Figure 3] This is an example of measurement results obtained by white light interference microscopy of the surface of a silicon wafer. Figure 3(a) shows the white light interference microscopy image, and Figure 3(b) shows the height profile. [Figure 4] This is a white-light interference microscope image of the surface of a silicon wafer with foreign matter approximately 200 nm in height within the field of view. Figure 4(a) is the overall image from the white-light interference microscope, Figure 4(b) is a magnified image of the area where the foreign matter is attached, and Figure 4(c) is the height profile of the foreign matter. The table in Figure 4(d) shows the roughness parameters calculated from the overall image shown in Figure 4(a). [Figure 5] The measurement flow in the example is shown. [Figure 6] An example of the evaluation results obtained in the example is shown. [Figure 7] The graph shows the arithmetic mean of the Sq values ​​obtained for each of the 25 silicon wafers evaluated in the example. [Modes for carrying out the invention]

[0009] [Methods for evaluating semiconductor wafers] One aspect of the present invention relates to a semiconductor wafer evaluation method, which includes obtaining a maximum height Sz and roughness parameters other than Sz by performing measurements using a roughness measuring device in one or more measurement areas on the surface of the semiconductor wafer to be evaluated, and for each measurement area, determining whether the values ​​of the roughness parameters other than Sz obtained in that measurement area are acceptable for evaluation of the semiconductor wafer to be evaluated, using the value of the maximum height Sz as an indicator (hereinafter also simply referred to as "determination of acceptableness").

[0010] One of the two surfaces of the semiconductor wafer is the surface (front surface) that becomes the device formation surface side, and the other is the surface (back surface) on the opposite side of the front surface. In the present invention and this specification, the semiconductor wafer surface refers to either one or both of the front surface and the back surface.

[0011] In the present invention and this specification, for various roughness parameters, reference can be made to ISO 25178-2:2012 and the Japanese Industrial Standard JIS B0681-2:2018 corresponding to the above ISO. The maximum height Sz, which is one of the roughness parameters, is expressed as "Sz = Sp + Sv". Sp is the maximum peak height (the maximum value of the height from the average surface), and Sv is the maximum valley depth (the absolute value of the minimum value of the height from the average surface). Sz calculated as the sum of these can be said to be the distance from the highest point to the lowest point of the surface of the measurement object.

[0012] In the above evaluation method, in one or more measurement regions of the semiconductor wafer surface to be evaluated, by performing measurement with a roughness measuring device, for each measurement region, two or more roughness parameters including the maximum height Sz are obtained. Then, using the value of the maximum height Sz as an index, it is determined whether the values of the roughness parameters other than Sz obtained in each measurement region are values that can be adopted for the evaluation of the semiconductor wafer to be evaluated. In this regard, the present inventor speculates as follows. However, the present invention is not limited to the speculation of the present inventor. Since the maximum height Sz is the sum of the maximum peak height and the maximum valley depth as described above, the inventors consider that it is easily affected by noise due to device factors, and further by noise due to disturbance factors such as foreign matter adhesion. As an example, according to the inventors' study, when foreign matter with a size of 100 nm or more adheres within the measurement field of view, the values of other roughness parameters (for example, Sa and Sq described later) change only by about several to a dozen or so nanometers compared to normal times, while the value of Sz changes greatly to 100 nm or more. Also, when sudden vibrations of the device occur, steps of 200 nm or more that normally do not exist may occur on the wafer surface. In such a case, the value of Sz becomes about 200 nm or 200 nm or more. For example, in the case as described above, a threshold value can be set to, for example, 100 nm for the value of Sz, and based on the threshold value, it is possible to determine the presence or absence of the influence of noise. Specifically, it is possible to determine whether the measurement results of the roughness parameters obtained together with Sz include abnormal values due to noise, or whether the measurement results are normal values that do not include or have little influence of noise. For example, in this way, for each measurement area where measurement is performed by the roughness measuring device, using the value of the maximum height Sz as an index, it is possible to determine whether the values of the roughness parameters other than Sz obtained in each measurement area are values that can be adopted for the evaluation of the semiconductor wafer to be evaluated. As a result, it becomes possible to use the values of the roughness parameters with reduced influence of noise for the evaluation of the semiconductor wafer. Hereinafter, the above evaluation method will be described in more detail.

[0013] <Semiconductor wafer to be evaluated> The semiconductor wafers to be evaluated in the above evaluation method can include various types of semiconductor wafers, such as silicon wafers (e.g., single-crystal silicon wafers). In this invention and specification, unless otherwise specified, a silicon wafer refers to a single-crystal silicon wafer. Another example of a semiconductor wafer to be evaluated is a polished wafer. A polished wafer is a wafer in which one or both surfaces are polished surfaces, i.e., surfaces that have undergone surface polishing treatment. Polished wafers are usually manufactured by sequentially going through processes such as rough polishing, etching, and mirror polishing (i.e., finish polishing), and have a polished surface. The polished surface is usually a mirror surface. The surface polishing treatment can be DSP (double-sided polishing) or SSP (single-sided polishing). Furthermore, the conductivity type of the semiconductor wafer to be evaluated is not limited and may be n-type or p-type. Its dopant concentration (i.e., resistivity), oxygen concentration, etc., are also not limited. The diameter of the semiconductor wafer being evaluated can be, for example, 200 mm, 300 mm, or 450 mm, but is not particularly limited.

[0014] <Measurement using a roughness measuring device> In the above evaluation method, measurements are performed using a roughness measuring device to obtain roughness parameters in one or more measurement areas on the surface of the semiconductor wafer to be evaluated. In one embodiment, the surface of the semiconductor wafer on which the measurement is performed may be only the front or back surface, or in another embodiment, it may be both the front and back surfaces. In the measurement using the roughness measuring device in the above evaluation method, the total number of measurement areas per surface (either the front or back surface) is one or more, may be one in one embodiment, or two or more in another embodiment. Furthermore, the above total number may be, for example, 50 or less, 40 or less, 30 or less, or 20 or less, or may exceed the values ​​exemplified herein.

[0015] Various roughness measuring devices capable of acquiring roughness parameters can be used as roughness measuring devices. Specific examples of roughness measuring devices include optical interference microscopes, atomic force microscopes, laser microscopes, and Fizeau interferometers. As an example, optical interference microscopes will be further explained below. However, the roughness measuring device used in the above evaluation method is not limited to optical interference microscopes.

[0016] An optical interference microscope (OCT) is a surface roughness measuring device that uses the interference of light to measure the surface topography of a sample. There are two measurement methods for OCTs: vertical scanning white light interference and phase-shift interference. An OCT using the vertical scanning white light interference method is called a white light interference microscope. More specifically, a white light interference microscope is a device that uses white light as a light source to perform three-dimensional measurements of a sample surface over a wide area with high vertical resolution.

[0017] Figure 1 is an explanatory diagram illustrating the measurement principle of a white light interference microscope. As shown in Figure 1(a), light from a white light source is split into two by a beam splitter. One beam is directed onto a reference mirror attached to the objective lens, and the other onto the surface of the object to be measured. These two beams of light are reflected and recombined. The objective lens is fitted with a vertical scanning scanner. As shown in Figure 1(b), the objective lens is scanned vertically, and height information can be obtained by measuring the height at which the intensity of the resulting interference fringes is maximized. In the example shown in Figure 1(b), the difference in the peak positions of the interference intensity at point A and point B indicates the height difference. White light interference is the superposition of interference of multiple wavelengths of light, and the peak position of the interference signal is the position where all phases are aligned. Therefore, a white light interference microscope allows for highly accurate height measurement regardless of the observation magnification.

[0018] Figure 2 shows an example of the change in interference light during fringe scanning in measurements using a white light interference microscope. A vertical scanning scanner is attached to the objective lens of a white light interference microscope, for example, as shown in Figure 1(a). Height information is obtained by fringe scanning, which measures the height at which the intensity of interference fringes (fringes) is maximized by scanning the objective lens vertically, as shown in the example in Figure 1. The number of interference fringes is determined by the inclination angle of the surface being measured, and the height difference between adjacent bright and dark areas of the fringe is approximately 140 nm, which is 1 / 4 of the central wavelength of the white light source. In the interference signal of fringe scanning, the point at which the intensity of the interference light is highest is called the 0th order interference, and the point at which it is second strongest is called the 1st order interference. If there is no noise influence, an interference waveform like the one shown in Figure 2 can be obtained. In Figure 2, A corresponds to point A shown in Figure 1(b), and B corresponds to point B shown in Figure 1(b). In contrast, if, for example, a sudden vibration of the device occurs during fringe scanning, the interference waveform may be distorted, and zero-order interference may not be detectable in locations where it should be obtained. In such cases, the first-order or second-order interference may become the highest interference intensity within that pixel, potentially leading to misinterpretation of height information. Furthermore, if a sudden vibration of the device occurs during measurement, distorting the interference waveform and causing a first-order interference to be misinterpreted as zero-order interference, a step of approximately 280 nm (2 / λ of the central wavelength λ of white light, 560 nm) may be formed at that location. Figure 3 shows an example of measurement results from a white light interference microscope image of the surface of a silicon wafer. Figure 3(a) shows the white light interference microscope image, and Figure 3(b) shows the height profile. In Figure 3, it can be seen that a step of approximately 260 nm exists within the measurement field of view due to a sudden vibration of the device during measurement. By using the maximum roughness Sz as an indicator, it is possible to determine, for example, whether the effects of noise from device factors such as those described above are included in the measurement results obtained by the roughness measuring device. As mentioned earlier, this is because the maximum roughness Sz is the sum of the maximum peak height and the maximum valley depth, and is therefore susceptible to noise from equipment-related factors. Furthermore, the maximum roughness Sz is also susceptible to noise from external disturbances such as foreign matter adhesion. Figure 4 is shown below as an example to further explain this point.

[0019] Figure 4 shows a white light interference microscope image of a silicon wafer surface with foreign matter approximately 200 nm in height within the field of view. Figure 4(a) is the overall image from the white light interference microscope, Figure 4(b) is a magnified image of the area where the foreign matter is attached, and Figure 4(c) is the height profile of the foreign matter. The table in Figure 4(d) shows the roughness parameters calculated from the overall image shown in Figure 4(a). When foreign matter, scratches, defects, etc. are present within the measurement field of the white light interference microscope, the values ​​of the roughness parameters of the semiconductor wafer surface may shift due to these foreign matter, scratches, defects, etc. The values ​​of Sa and Sq shown in the table in Figure 4(d) are only slightly higher than the values ​​of Sa and Sq for a typical silicon wafer. Details regarding Sa and Sq will be described later. In contrast, the value of Sz shown in Figure 4(d) is affected by the foreign matter in the field of view and shows a value of 200 nm or more. Therefore, by using Sz as an index, it is possible to determine that the influence of noise from external disturbances such as foreign matter adhesion is included in the measurement results obtained by the roughness measuring device.

[0020] In the above, a white light interference microscope was used as an example of a roughness measuring device, and a silicon wafer was used as an example of a semiconductor wafer. However, as mentioned earlier, the roughness measuring device used in the above evaluation method may be a roughness measuring device other than a white light interference microscope, and the semiconductor wafer to be evaluated may be a semiconductor wafer other than a silicon wafer.

[0021] <Determination of whether or not to adopt the roughness parameter> In the evaluation method described above, as stated above, the maximum height Sz and roughness parameters other than Sz are obtained by performing measurements using a roughness measuring device in one or more measurement areas. Then, for each measurement area, the value of the maximum height Sz obtained for that measurement area is used as an indicator to determine whether the values ​​of the roughness parameters other than Sz obtained for that measurement area are acceptable for evaluation of the semiconductor wafer under evaluation. The details of the reason for adopting the maximum roughness Sz as such an indicator in the evaluation method described above are as stated earlier. Specific forms of determining whether or not to accept the values ​​can be, for example, the following forms. These various forms can also be combined arbitrarily.

[0022] (1) In one embodiment, if the value of the maximum height Sz is less than or equal to a preset threshold, the values ​​of roughness parameters other than Sz obtained for one or more measurement areas where this maximum height Sz was obtained are adopted as evaluation values ​​for the semiconductor wafer under evaluation. The fact that the value of the maximum height Sz is less than or equal to a preset threshold is also described as "no Sz abnormality". The threshold can be determined by considering, for example, the height of foreign matter that may adhere to the semiconductor wafer, the depth of defects or scratches that may occur on the semiconductor wafer, the magnitude of equipment-related noise that may occur during measurement, and the quality required for the semiconductor wafer under evaluation. Whether to use less than or equal to the threshold as the standard or less than the threshold can be decided as appropriate. In addition, as roughness parameters other than Sz, for example, one or more roughness parameters selected from the group consisting of arithmetic mean height Sa and root mean square height Sq can be listed. Only the arithmetic mean height Sa, only the root mean square height Sq, or both can be adopted as evaluation values. For the arithmetic mean height Sa and the root mean square height Sq, refer to ISO 25178-2:2012 as mentioned earlier. The same points apply to the various forms described later.

[0023] In this embodiment, if the total number of measurement areas is 1, the values ​​of roughness parameters other than Sz obtained for this one measurement area are adopted as evaluation values ​​for the semiconductor wafer under evaluation. On the other hand, in this embodiment, if the total number of measurement areas is 2 or more, and the total number of measurement areas where the maximum height Sz value is below or equal to a preset threshold is 2 or more, the values ​​of roughness parameters other than Sz obtained for all of those 2 or more measurement areas can be adopted as evaluation values ​​for the semiconductor wafer under evaluation, or the values ​​of roughness parameters other than Sz obtained for some of the areas can be adopted as evaluation values ​​for the semiconductor wafer under evaluation. When using the values ​​of roughness parameters other than Sz obtained for 2 or more measurement areas as evaluation values, for example, the arithmetic mean, maximum value, minimum value, etc., of the values ​​obtained for multiple measurement areas can be used to determine whether the semiconductor wafer under evaluation is a semiconductor wafer with the desired quality (i.e., a good product) or a semiconductor wafer that does not meet the desired quality (i.e., a defective product). The threshold for determining whether a product is good or defective should be determined considering the quality required for the semiconductor wafer under evaluation. The same points apply to the various forms described later.

[0024] (2) In one embodiment, if the value of the maximum height Sz is equal to or exceeds a preset threshold, the values ​​of roughness parameters other than Sz obtained for the measurement area in which this maximum height Sz was obtained will not be used as evaluation values ​​for the semiconductor wafer under evaluation. The condition that the value of the maximum height Sz is equal to or exceeds a preset threshold will also be described as "Sz abnormality present". Specifically, according to this embodiment, for measurement areas in which the maximum height Sz is equal to or exceeds a preset threshold, it can be determined that the measurement results performed in this measurement area will not be used as evaluation values ​​for the semiconductor wafer under evaluation because they will contain abnormal values ​​affected by noise.

[0025] In this embodiment, in one embodiment, if a measurement area is obtained in which the maximum height Sz value is equal to or exceeds a preset threshold, the roughness measuring device can be used to perform the measurement again (hereinafter also referred to as "remeasurement"). If there are two or more measurement areas in which the maximum height Sz value is equal to or exceeds a preset threshold, remeasurement can be performed on some or all of them. For example, if the reason why the maximum height Sz value in a certain measurement area is equal to or exceeds a preset threshold is due to equipment factors such as vibration of the device that occurred during measurement, the measurement results obtained by remeasurement for this measurement area may not contain any abnormal values. Whether or not the measurement results of remeasurement contain abnormal values ​​can also be determined using the maximum roughness Sz as an indicator, in the same way as above. If the maximum height Sz value obtained by remeasurement is equal to or less than a preset threshold, the values ​​of roughness parameters other than Sz obtained by remeasurement can be used as evaluation values ​​for the semiconductor wafer under evaluation. On the other hand, if the remeasurement also yields a maximum height Sz value that is equal to or exceeds a predetermined threshold, the values ​​of roughness parameters other than Sz obtained for that measurement area can be definitively decided not to be used as evaluation values ​​for the semiconductor wafer being evaluated.

[0026] Furthermore, in one configuration, if a maximum height Sz value equal to or exceeding a preset threshold is obtained, further measurements using the roughness measuring device can be performed in areas other than the measurement area where this maximum height Sz value was obtained. For example, if the measurement area in the first measurement includes a measurement area in which a maximum height Sz value equal to or exceeding a preset threshold was obtained, then as a second measurement, measurements can be performed using the roughness measuring device on one or more areas that were not measured in the first measurement. If the reason why the maximum height Sz obtained in the first measurement for a certain measurement area equals or exceeds the threshold is due to foreign matter, scratches, defects, etc., present in that measurement area, then by changing the measurement area, it may be possible to obtain measurement results that do not include these influences. In such a case, if the maximum height Sz value obtained by the measurement performed in the changed measurement area is equal to or less than the preset threshold, the values ​​of roughness parameters other than Sz obtained by this measurement can be adopted as evaluation values ​​for the semiconductor wafer under evaluation. On the other hand, if the measurement results obtained by changing the measurement area are equal to or exceed a preset threshold for the maximum height Sz, the values ​​of roughness parameters other than Sz obtained for that measurement area can be determined not to be used as evaluation values ​​for the semiconductor wafer being evaluated, or the measurement area can be remeasured. For the determination of the measurement results obtained by remeasurement, please refer to the above description.

[0027] Furthermore, in one configuration, if a maximum height Sz value equal to or exceeding a preset threshold is obtained, the values ​​of one or more roughness parameters obtained for the measurement area where this maximum height Sz value was obtained can be recalculated. The recalculation can be performed by excluding from the calculation of roughness parameters the portion that is estimated to be the cause of the abnormal maximum height Sz value, i.e., the reason why the maximum roughness Sz equals or exceeds the threshold. For example, if the reason why the maximum height Sz obtained for a certain measurement area equals or exceeds the threshold is due to foreign matter, the portion containing the foreign matter can be removed by image processing (e.g., masking), or the measurement results of the portion containing the foreign matter can be removed by data processing, and then the measurement results can be recalculated to obtain measurement results that do not include the influence of foreign matter or whose influence of foreign matter is reduced. The target of the recalculation can be one or more roughness parameters, which can be one or more surface parameters other than the maximum roughness Sz. For example, the recalculation results obtained in this way can be adopted as evaluation values ​​for the semiconductor wafer under evaluation. Alternatively, the maximum roughness Sz may also be recalculated, and if the recalculated maximum roughness Sz is below or equal to the threshold, then the surface parameter values ​​other than the maximum roughness Sz obtained by this recalculation can be determined to be acceptable for evaluating the semiconductor wafer under evaluation.

[0028] In the evaluation method described above, the semiconductor wafer to be evaluated can be evaluated based on the values ​​of roughness parameters other than Sz that were determined to be acceptable, as explained above. This evaluation can be performed based on one or more values ​​of surface parameters other than Sz obtained for one measurement area, or it can be performed based on the arithmetic mean, maximum value, minimum value, etc., of values ​​obtained for multiple measurement areas. In either case, if the value of the surface parameter is below or equal to a preset threshold, the semiconductor wafer to be evaluated can be determined to be a semiconductor wafer with the desired quality (i.e., a good product), and if it is above or equal to a preset threshold, the semiconductor wafer to be evaluated can be determined to be a semiconductor wafer that does not meet the desired quality (i.e., a defective product). As mentioned earlier, the threshold for determining whether a product is good or defective should be determined by considering the quality required for the semiconductor wafer to be evaluated. In one embodiment, the value of the maximum roughness Sz can also be used to determine whether the semiconductor wafer to be evaluated is good or bad. The maximum roughness Sz allows for the determination of the presence or absence of localized defects on the semiconductor wafer surface (front or back side), evaluation of surface irregularities, and other related functions.

[0029] [Manufacturing method 1] Manufacturing method 1 is, To manufacture evaluation semiconductor wafers under test manufacturing conditions, The evaluation semiconductor wafer manufactured as described above is evaluated using the evaluation method described above. Based on the results of the above evaluation, either the manufacturing conditions modified from the above test manufacturing conditions will be determined as the actual manufacturing conditions, or the above test manufacturing conditions will be determined as the actual manufacturing conditions, and To manufacture semiconductor wafers under the actual manufacturing conditions determined above, A method for manufacturing semiconductor wafers, including That is the case.

[0030] In manufacturing method 1, test manufacturing conditions are set as a preliminary step to determining the actual manufacturing conditions, and evaluation semiconductor wafers are manufactured under these test manufacturing conditions. "Actual manufacturing conditions" refers to the manufacturing conditions for product semiconductor wafers. The evaluation semiconductor wafers manufactured under the test manufacturing conditions are subjected to evaluation according to the evaluation method detailed above. There is at least one evaluation semiconductor wafer, and there may be two or more; the number is not particularly limited. If the evaluation results of the surface parameters obtained for the evaluation semiconductor wafer (for example, the arithmetic mean height Sa and / or root mean square height Sq described above) are the values ​​desired for the product semiconductor wafer, then product semiconductor wafers with the desired surface properties can be stably supplied to the market by manufacturing and shipping product semiconductor wafers under these test manufacturing conditions as the actual manufacturing conditions. On the other hand, if the evaluation results show that the evaluation results of the surface parameters obtained for the evaluation semiconductor wafer differ from the values ​​desired for the product semiconductor wafer, then the manufacturing conditions modified from the test manufacturing conditions are determined as the actual manufacturing conditions. As an example of a semiconductor wafer manufacturing process, a polished wafer, which is a form of silicon wafer, can be manufactured by a manufacturing process that includes cutting (slicing), chamfering, rough polishing (e.g., lapping), etching, mirror polishing (finish polishing), and cleaning performed between or after the above processing steps, from a silicon single crystal ingot grown by the Czochralski method (CZ method), etc. For silicon wafers or semiconductor wafers other than silicon wafers, the manufacturing conditions to which the above modifications are made are preferably manufacturing conditions that are considered to affect the surface parameters. An example of such manufacturing conditions is the polishing treatment conditions for the surface (front and / or back) of the semiconductor wafer. Specific examples of such surface polishing treatment conditions include rough polishing conditions and mirror polishing conditions, and more specifically, the type of polishing liquid, the concentration of abrasive particles in the polishing liquid, the type of polishing pad (e.g., hardness, etc.), etc. By modifying the test manufacturing conditions in this way and determining the actual manufacturing conditions, and then manufacturing and shipping product semiconductor wafers under these actual manufacturing conditions, it becomes possible to stably supply the market with product semiconductor wafers that have the desired surface properties.Furthermore, it is possible to manufacture evaluation semiconductor wafers again under manufacturing conditions modified from the test manufacturing conditions, evaluate these evaluation semiconductor wafers using the evaluation method described above, and repeat the process of determining whether to adopt these manufacturing conditions as actual manufacturing conditions or to make further modifications, once or twice or more times. The threshold for determining whether the surface parameter evaluation results obtained for the evaluation semiconductor wafers are the values ​​desired for the product semiconductor wafers can be set appropriately according to market quality requirements, etc.

[0031] [Manufacturing method 2] Manufacturing method 2 is, Manufacturing a semiconductor wafer lot containing multiple semiconductor wafers, Extracting one or more semiconductor wafers from the above semiconductor wafer lot, The extracted semiconductor wafers are evaluated using the evaluation method described above, and Based on the above evaluation, semiconductor wafers from the same semiconductor wafer lot as those judged to be good products will be prepared for shipment as products. A method for manufacturing semiconductor wafers, including That is the case.

[0032] In manufacturing method 2, a so-called sampling inspection is performed, and semiconductor wafers from the same lot as those determined to be good products are prepared for shipment as finished semiconductor wafers. The manufacturing of semiconductor wafer lots in manufacturing method 2 can be carried out using a general semiconductor wafer manufacturing process. For example, the manufacturing process for polished wafers can be described in the previous section.

[0033] The number of semiconductor wafers extracted from a manufactured semiconductor wafer lot and subjected to so-called sampling inspection is at least one, but may be two or more, and the number is not particularly limited. The semiconductor wafers extracted from the semiconductor wafer lot are subjected to evaluation according to the evaluation method detailed above. As a result of the evaluation, semiconductor wafers from the same semiconductor wafer lot as those judged to be good products are prepared for shipment as product semiconductor wafers. The criteria for judging a product as good, specifically the threshold values ​​for surface parameters (for example, the arithmetic mean height Sa and / or root mean square height Sq described above), can be determined according to the quality required for the product semiconductor wafers. Preparation for shipment as product semiconductor wafers can include, for example, packaging. Thus, according to manufacturing method 2, product semiconductor wafers with the desired surface properties can be stably supplied to the market. [Examples]

[0034] The present invention will be further described below based on examples. However, the present invention is not limited to the embodiments shown in the examples.

[0035] [Semiconductor wafers to be evaluated] Twenty-five silicon wafers with a diameter of 300 mm were prepared as semiconductor wafers to be evaluated. These silicon wafers were polished wafers that had been polished on both sides (DSP).

[0036] [Measurement using a roughness measuring device] Measurements were performed on the back surface of each of the above silicon wafers under the following measurement conditions.

[0037] <Measurement conditions> Roughness measuring device: White light interference microscope Measurement magnification: 10x (field of view: 1.6mm x 1.6mm) Filter: Hi-pass Filter 80μm (Removes undulations in spatial wavelengths greater than 80μm) Measurement area: For each silicon wafer, nine areas within the wafer surface as shown in Table 1.

[0038] [Table 1]

[0039] <Measurement Flow> Figure 5 shows the measurement flow in this embodiment. The details of the measurement flow are described below. The surface of the silicon wafer to be measured was subjected to a white-light interference microscope (WAS) and the resulting microscope image was processed with image processing such as planarization. The analysis unit of the WAS was used to analyze the processed microscope image, and roughness parameters Sa, Sq, and Sz were output for each of the nine in-plane points on each silicon wafer. Regarding the Sz threshold, in this embodiment, we assumed that the height of foreign matter causing noise or the depth of defects or scratches is 50 nm or more, and set the Sz threshold to 50 nm. However, the threshold should be a value that does not remove the surface shape of the wafer. For example, if the wafer surface is smooth, it would be appropriate to use a threshold value of 10 nm or 20 nm. In this example, an Sz abnormality was determined by whether the Sz value was 50 nm or greater ("Sz abnormality present") or less than 50 nm ("Sz abnormality not present"). For each of the nine measurement regions of the silicon wafer, if there was no Sz abnormality, it was determined that the Sa and Sq values ​​in that measurement region could be used for wafer evaluation. On the other hand, if an abnormality is detected in Sz, it is determined that further processing is necessary, and one or more processes such as remeasurement, measurement in other measurement areas, and recalculation can be performed. Details of these processes are as described above.

[0040] Figure 6 shows an example of the evaluation results obtained in this embodiment. In Figure 6, Image A is an image where the Sz value is below the threshold, resulting in a determination of "no Sz abnormality." No steps, foreign objects, defects, etc., that could be considered noise in roughness parameter measurement are observed in Image A. In contrast, images B, C, and D are images where the Sz value is above the threshold, resulting in a determination of "Sz abnormality." Image B shows a step that is presumed to be caused by vibration of the device. Image C shows foreign matter adhesion. Image D shows a pit system defect. From the above results, it can be confirmed that by using the Sz value as an indicator, it is possible to determine whether or not noise is affecting the roughness parameter measurement results.

[0041] In this example, 25 silicon wafers were used, and each wafer had 9 measurement areas, resulting in a total of 225 images obtained by white-light interference microscopy. Of the 225 images, Sz abnormality detection was performed, and 216 images were determined to be "no Sz abnormality" and 9 images were determined to be "Sz abnormality present". Table 2 shows the arithmetic mean and standard deviation of the Sq values ​​for the 225 images, as well as the arithmetic mean and standard deviation of the Sq values ​​for the 216 images determined to be "no Sz abnormality".

[0042] [Table 2]

[0043] Figure 7 plots the arithmetic mean of the Sq values ​​obtained for each of the 25 silicon wafers (indicated as "Sq arithmetic mean"). In the double-sided polishing performed on the silicon wafer evaluated in this embodiment, the normal value for the Sq of the polished surface after double-sided polishing is approximately 0.2 nm. In Figure 7, the left side plots the arithmetic mean of Sq obtained for nine in-plane measurement regions for 25 silicon wafers. The plots on the left side of Figure 7 also include plots where the arithmetic mean of Sq values ​​is 1 nm or greater. In Figure 7, the right-hand plot shows the arithmetic mean of Sq obtained after excluding images judged to have an Sz abnormality. In all plots on the right side of Figure 7, the arithmetic mean of Sq is around 0.2 nm.

[0044] The results shown in Table 2 and Figure 7 confirm that the surface roughness of semiconductor wafers can be accurately evaluated by using the Sz value as an indicator. [Industrial applicability]

[0045] One aspect of the present invention is useful in the field of manufacturing various semiconductor wafers, such as silicon wafers.

Claims

1. To obtain the maximum height Sz and roughness parameters other than Sz by performing measurements using a roughness measuring device on one or more measurement areas on the surface of the semiconductor wafer to be evaluated, and, For each measurement region, the value of the maximum height Sz is used as an indicator to determine whether the values ​​of roughness parameters other than Sz obtained in that measurement region are acceptable for evaluating the semiconductor wafer under evaluation. A method for evaluating semiconductor wafers, including those containing [specific components / materials].

2. The semiconductor wafer evaluation method according to claim 1, further comprising: if the value of the maximum height Sz is less than or equal to a preset threshold, adopting the values ​​of roughness parameters other than Sz obtained for one or more measurement regions where the maximum height Sz was obtained as evaluation values ​​for the semiconductor wafer to be evaluated.

3. The semiconductor wafer evaluation method according to claim 1, wherein if the value of the maximum height Sz is equal to or exceeds a preset threshold, the values ​​of roughness parameters other than Sz obtained for the measurement region in which the maximum height Sz was obtained are not used as evaluation values ​​for the semiconductor wafer to be evaluated.

4. The semiconductor wafer evaluation method according to claim 3, further comprising: if the value of the maximum height Sz is equal to or exceeds a preset threshold, repeating the measurement using a roughness measuring device in the measurement area where the maximum height Sz was obtained.

5. The semiconductor wafer evaluation method according to claim 3, further comprising: if the value of the maximum height Sz is equal to or exceeds a preset threshold, performing a measurement using a roughness measuring device in a region other than the measurement region where the maximum height Sz was obtained.

6. The semiconductor wafer evaluation method according to claim 3, further comprising recalculating the values ​​of one or more roughness parameters obtained for the measurement region where the maximum height Sz was obtained, if the value of the maximum height Sz is equal to or exceeds a preset threshold.

7. The semiconductor wafer evaluation method according to claim 6, wherein the recalculation is performed by excluding the portion that is presumed to be the cause of the abnormal value of the maximum height Sz from the calculation target of the roughness parameter.

8. The method for evaluating a semiconductor wafer according to claim 1, wherein the roughness parameter other than Sz is one or more roughness parameters selected from the group consisting of arithmetic mean height Sa and root mean square height Sq.

9. The method for evaluating a semiconductor wafer according to claim 1, wherein the roughness measuring device is an optical interference microscope.

10. The method for evaluating a semiconductor wafer according to claim 9, wherein the optical interference microscope is a white light interference microscope.

11. To manufacture evaluation semiconductor wafers under test manufacturing conditions, The manufactured evaluation semiconductor wafer is evaluated by the evaluation method described in any one of claims 1 to 10. Based on the results of the evaluation, either the manufacturing conditions modified from the test manufacturing conditions are determined as the actual manufacturing conditions, or the test manufacturing conditions are determined as the actual manufacturing conditions, and To manufacture semiconductor wafers under the actual manufacturing conditions determined above, A method for manufacturing semiconductor wafers containing [the specified material].

12. The method for manufacturing a semiconductor wafer according to claim 11, wherein the manufacturing conditions to which the above-mentioned modifications are made include surface polishing treatment conditions for the semiconductor wafer.

13. Manufacturing a semiconductor wafer lot containing multiple semiconductor wafers, Extracting one or more semiconductor wafers from the aforementioned semiconductor wafer lot, The extracted semiconductor wafer is evaluated by the evaluation method described in any one of claims 1 to 10, and Based on the results of the above evaluation, semiconductor wafers from the same semiconductor wafer lot as those judged to be good products will be prepared for shipment as products. A method for manufacturing semiconductor wafers containing [the specified material].