Fluid catalytic cracking catalyst and production method therefor

JP2023053577A5Active Publication Date: 2024-10-01JGC CATALYSTS & CHEMICALS LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021162699
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-10-01
Publication Date
2024-10-01
Estimated Expiration
2041-10-01

AI Technical Summary

Technical Problem

Conventional FCC catalysts have limitations in improving propylene yield in fluidized catalytic cracking processes.

Method used

A fluid catalytic cracking catalyst composition comprising 10-30% silica-based binder, 10-40% rare earth metal ion-exchanged FAU-type zeolite, 10-60% clay minerals, and 5-30% active matrix, produced through a method involving slurry preparation, spray-drying, and rare earth metal ion exchange, optionally with a ZSM-5 co-catalyst.

Benefits of technology

Enhances propylene yield by suppressing hydrogen transfer reactions and maintaining catalyst activity, wear resistance, and fluidity, while improving hydrothermal resistance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a fluid catalytic cracking catalyst enhancing the yield of propylene in fluid catalytic cracking.SOLUTION: The fluid catalytic cracking catalyst includes in mass%: 10-30% of a binder, 10-40% of zeolite ion-exchanged by rare-earth metal, 10-60% of clay minerals and 5-30% of active matrix. The binder is a silica-based binder formed from a binder-forming component having pH of less than 1.6, and the zeolite is an FAU-type one. The content of the rare earth metal is in the range of 0.5 to 1.2 mass% in terms of rare-earth metal oxide (RE2O3).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a fluid catalytic cracking catalyst and a method for producing the same. [Background technology]

[0002] Various research and development efforts have been made regarding catalysts used in the fluid catalytic cracking of hydrocarbon oils (hereinafter also referred to as "FCC catalysts") and their manufacturing methods, with the aim of increasing the yield of gasoline fractions and improving wear resistance.

[0003] For example, Patent Document 1 discloses a method for producing an FCC catalyst with a high gasoline yield, low coke yield, and high abrasion strength. The method involves mixing zeolite (such as ultra-stable Y-type zeolite or rare-earth-exchanged ultra-stable Y-type zeolite), a binder (such as basic aluminum chloride), and an inorganic oxide matrix (such as kaolin), and then spray-drying the resulting slurry, which has been pH-adjusted. It also describes that spherical particles obtained by spray-drying were washed with pure water, then with water containing ammonium sulfate, and dried to produce the FCC catalyst.

[0004] Patent Document 2 describes how the production of ethylene and propylene can be increased by including phosphorus-modified submicron ZSM-5 in the FCC catalyst. Patent Document 3 describes the use of an FCC catalyst containing a superstable Y-type zeolite in which some of the skeletal aluminum atoms are replaced with zirconia and titanium atoms in a fluid catalytic cracking apparatus for producing light olefins and gasoline fuel.

[0005] Patent Document 4 describes how using a Y zeolite containing barium ions at ion exchange site III in an FCC catalyst can increase the yield of butylene. Patent documents 5 and 6 describe how using colloidal silica as a raw material for FCC catalysts can improve the wear resistance of FCC catalysts. [Prior art documents] [Patent Documents]

[0006] [Patent Document 1] Japanese Patent Publication No. 2009-657 [Patent Document 2] Special Publication No. 2015-518782 [Patent Document 3] Special Publication No. 2017-534433 [Patent Document 4] Special Publication No. 2018-536535 [Patent Document 5] Special Publication No. 2019-528163 [Patent Document 6] Special Publication No. 2021-511200 [Overview of the project] [Problems that the invention aims to solve]

[0007] Recently, there has been a demand for improved propylene yield in fluid catalytic cracking, and there is room for further improvement in conventional FCC catalysts. Therefore, the present invention aims to provide an FCC catalyst that improves the propylene yield in a fluid catalytic cracking catalyst, and a method for producing the same. [Means for solving the problem]

[0008] The present invention relates, for example, to the following [1] to [3]. [1] It contains 10-30% by mass of a binder, 10-40% by mass of zeolite ion-exchanged with rare earth metals, 10-60% by mass of clay minerals, and 5-30% by mass of an active matrix. The aforementioned binder is a silica-based binder formed from a silica-based binder-forming component having a pH of less than 1.6. The aforementioned zeolite is a FAU-type zeolite. The rare earth metal content is 0.5 to 1.2 mass%, converted to rare earth metal oxides (RE2O3). Fluid catalytic cracking catalyst.

[0009] [2] (a) At least a binder-forming component, zeolite, clay minerals, and an active matrix-forming component are mixed to prepare a raw material slurry; (b) The raw material slurry is spray-dried to obtain particles; (c) The particles are contacted with an aqueous solution containing a rare earth metal to ion-exchange the zeolite with the rare earth metal. comprising The binder-forming component is a silica-based binder-forming component having a pH of less than 1.6; The zeolite is a FAU-type zeolite A method for producing a fluid catalytic cracking catalyst.

[0010] [3] A fluid catalytic cracking catalyst composition comprising the fluid catalytic cracking catalyst of [1] and an auxiliary catalyst containing ZSM-5.

Effects of the Invention

[0011] According to the present invention, when fluid catalytic cracking is carried out using a fluid catalytic cracking catalyst composition obtained by adding a ZSM-5 additive to a fluid catalytic cracking catalyst, the propylene yield can be improved.

Modes for Carrying Out the Invention

[0012] Hereinafter, the present invention will be described in more detail. [Fluid catalytic cracking catalyst] The fluid catalytic cracking catalyst (FCC catalyst) according to the present invention includes a binder, a zeolite ion-exchanged with a rare earth metal, clay minerals, and an active matrix.

[0013] 〈Binder〉 As the binder (hereinafter also referred to as "binder"), a silica-based binder formed from a silica-based binder-forming component having a pH of less than 1.6 is used.

[0014] Details of the silica-based binder-forming component will be described later. The FCC catalyst of the present invention contains the binder in an amount of SiO2 equivalent to, for example, 10 to 30% by mass, preferably 12 to 26% by mass, and more preferably 14 to 24% by mass.

[0015] Although the components and raw materials constituting the FCC catalyst of the present invention may contain water, in this invention, the content of each component or the amount of each raw material used is expressed as the amount excluding water (sometimes referred to as "solid content concentration").

[0016] <Zeolite ion-exchanged with rare earth metals> Details about the zeolite in zeolites that have undergone ion exchange with rare earth metals, i.e., the zeolite before ion exchange, will be described later.

[0017] Examples of the rare earth metals include cerium (Ce), lanthanum (La), praseodymium (Pr), and neodymium (Nd). These may be present individually or in combination of two or more.

[0018] The FCC catalyst of the present invention contains, for example, 10 to 40% by mass, preferably 12 to 38% by mass, and more preferably 14 to 36% by mass of the zeolite. When the content is above the lower limit, the FCC catalyst exhibits sufficient reaction activity. On the other hand, when the content is below the upper limit, it is possible to prevent over-decomposition, decreased selectivity, and deterioration of the catalyst's wear resistance and fluidity, which may result from excessively high activity.

[0019] Although the components and raw materials constituting the FCC catalyst of the present invention may contain water, the content of each component or the amount of each raw material used in this specification is indicated in terms of the amount excluding water or the solid content concentration.

[0020] <Clay Minerals> The clay minerals that serve as fillers are clay and / or clay minerals, examples of which include kaolin, bentonite, kaolinite, halloysite, montmorillonite, etc., with kaolin being particularly preferred.

[0021] The FCC catalyst of the present invention contains, for example, 10 to 60% by mass, preferably 14 to 56% by mass, and more preferably 18 to 52% by mass of the clay minerals. When the content is above the lower limit, the maintenance of the pore structure of the FCC catalyst, the maintenance of the catalyst shape, wear resistance, fluidity, etc., are good. On the other hand, when the content is below the upper limit, the ratio of the zeolite component and the active matrix in the FCC catalyst is high, resulting in good activity of the FCC catalyst.

[0022] <Activated Matrix> Examples of the active matrix include substances containing solid acids such as activated alumina (boehmite, gibbsite, etc.), alumina-silica, silica-magnesia, alumina-magnesia, and alumina-magnesia-silica. A solid acid is a substance that exhibits solid acidity within the reaction temperature range of the catalyst. The solid acid can be measured by a temperature-controlled desorption method using ammonia or by an in situ FTIR (Fourier transform infrared absorption spectrum) method using ammonia or pyridine.

[0023] Furthermore, examples of active matrices that also function as metal scavengers include alumina, phosphorus-alumina, crystalline calcium aluminate, sepiolite, barium titanate, calcium tin oxide, strontium titanate, manganese oxide, magnesia, and magnesia-alumina. As raw materials for metal scavenging agents, precursor substances such as aluminum hydroxide (gibbsite) and boehmite, which are converted to alumina, can also be used by firing them in an oxidizing atmosphere.

[0024] The FCC catalyst of the present invention contains, for example, 5 to 30% by mass, preferably 8 to 29% by mass, and more preferably 10 to 28% by mass of the active matrix. When the content is above the lower limit, effects such as accelerated decomposition of substances with large molecular weights and suppression of poisoning of the active component by metal capture are observed. On the other hand, when the content is below the upper limit, deterioration of the wear resistance and fluidity of the FCC catalyst can be prevented.

[0025] <Optional ingredients> The FCC catalyst according to the present invention may optionally contain additives in addition to a binder, zeolite ion-exchanged with rare earth metals, clay minerals, and an active matrix. Examples of the aforementioned additives include CO combustion promoting components (Pt, Pd) and desulfurization oxide components (CeO2, MgO).

[0026] (Rare earth metal content) The FCC catalyst of the present invention contains rare earth metals. The content of rare earth metals in the FCC catalyst of the present invention is 0.5 to 1.2% by mass, more preferably 0.6 to 1.1% by mass, when converted to rare earth oxides (RE2O3). When the rare earth metal content is within the above range, the FCC catalyst of the present invention exhibits excellent hydrothermal resistance and excellent propylene yield.

[0027] [Method for producing a fluid catalytic cracking catalyst] The method for producing a fluid catalytic cracking catalyst (FCC catalyst) according to the present invention is: (a) A step of preparing a raw material slurry by mixing at least a binder-forming component, zeolite, clay minerals, and an active matrix-forming component, (b) A step of spray-drying the raw material slurry to obtain particles, (c) A step of bringing the particles into contact with an aqueous solution containing a rare earth metal and performing ion exchange of the zeolite with the rare earth metal, Includes.

[0028] 《Process (a)》 In step (a) above, a raw material slurry containing at least a binder-forming component, zeolite, clay minerals, and an active matrix-forming component is prepared by mixing these.

[0029] One embodiment of step (a) is, for example, preparing a raw material slurry by mixing a binder-forming component with zeolite, clay minerals, an active matrix-forming component, and optionally an additive. Each component may be added in powder form or as a slurry. Furthermore, the order in which the components are added does not matter, as long as the slurry can be prepared without causing gelation.

[0030] (Binding agent forming component) The aforementioned binder-forming component is a component for forming a binder in a fluid catalytic cracking catalyst. A silica-based binder-forming component is used as the binder-forming component. The silica-based binder-forming component is usually prepared by mixing a silica source with an acid. Examples of the silica source include silica, silica gel (including silica hydrogel), silica sol (including silica hydrosol), and aqueous solutions of silicic acid (salt) (including orthosilicic acid (salt) and metasilicic acid (salt)) (for example, water glass). For silica sol and silicate, colloidal silica of sodium type, potassium type, lithium type, acid type, etc. can be used. Of these, silica sol and aqueous solutions of silicic acid (salt) are preferred.

[0031] Examples of the aforementioned acid include inorganic acids. Examples of inorganic acids include sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid, of which sulfuric acid, hydrochloric acid, and nitric acid are preferred, and sulfuric acid is particularly preferred.

[0032] When preparing the silica-based binder forming component by mixing a silica source and an acid, these are determined by the molar ratio (H) between hydrogen ions in the acid and silicon atoms in the silica source. + It is also written as ] / [SiO2]). The mixture is preferably 0.70 or more, more preferably 0.75 or more. The upper limit of the molar ratio is, for example, 2.0.

[0033] Furthermore, the pH of the binder-forming component is less than 1.6, preferably less than 1.5, and more preferably less than 1.3. By setting the pH of the binder-forming component within the above range, the propylene yield can be improved in fluid catalytic cracking. The lower limit of the pH is, for example, 0.1 or higher, and may be 0.2 or higher, or 0.3 or higher. The temperature during pH measurement is 35 to 37°C (for example, 36°C).

[0034] (Zeolite) As the zeolite mentioned above, FAU-type zeolite is used. Examples of FAU-type zeolites include ultra-stable Y-type zeolite (USY) and rare-earth metal-exchange ultra-stable Y-type zeolite (hereinafter also referred to as "REUSY"), which is obtained by introducing rare-earth metals into USY by ion exchange or the like.

[0035] The lattice constant of the zeolite, as measured by the method used in the later-described examples, is preferably in the range of 2.438 to 2.460 nm, and more preferably in the range of 2.440 to 2.458 nm. The lattice constant is determined by X-ray diffraction using anatase-type TiO2 as the standard material, based on the interplanar spacing of the diffraction planes (553) and (642) of the zeolite.

[0036] (Clay minerals) Specific examples of the clay minerals and preferred embodiments are as described above.

[0037] (Active matrix forming component) Examples of the active matrix-forming components include, in addition to the specific examples of active matrices described above, components that form an active matrix upon heating, such as aluminum hydroxide (gibbsite) and alumina hydrate (boehmite).

[0038] A preferred embodiment of step (a) is to add clay minerals and an active matrix forming component to the binder forming component, and then add the zeolite in the form of a slurry with a pH adjusted to 2.8 to 4.5. This suppresses pH fluctuations in the zeolite slurry when added to the raw material slurry, making it less likely for the zeolite to aggregate. The slurry can be prepared, for example, by adding the zeolite and an acid to water. Examples of the acid include sulfuric acid, hydrochloric acid, nitric acid, phosphoric acid, and organic acids (e.g., citric acid, formic acid, acetic acid, etc.).

[0039] Specific examples of each raw material listed as a component of the raw material slurry, preferred embodiments, etc., are as described above. The raw material slurry may be prepared by optionally adding additives and water in addition to these components.

[0040] The raw material slurry contains, for example, 10 to 30% by mass, preferably 12 to 26% by mass, and more preferably 14 to 24% by mass of the binder-forming component, calculated in terms of SiO2 amount (provided that the amount of solids in the raw material slurry (the same applies to components other than the dispersion medium in the raw material slurry) is 100% by mass).

[0041] The raw material slurry contains the zeolite in an amount of, for example, 10 to 40% by mass, preferably 12 to 38% by mass, and more preferably 14 to 36% by mass (provided that the solid content in the raw material slurry is 100% by mass).

[0042] The raw material slurry contains, for example, 10 to 60% by mass, preferably 14 to 56% by mass, and more preferably 18 to 52% by mass of the clay minerals (provided that the solid content in the raw material slurry is 100% by mass).

[0043] The raw material slurry contains the active matrix in an amount of, for example, 5 to 30% by mass, preferably 8 to 29% by mass, and more preferably 10 to 28% by mass (provided that the solid content in the raw material slurry is 100% by mass).

[0044] The raw material slurry contains water as a dispersion medium. The raw material slurry may contain small amounts of components other than water as a dispersion medium, such as methanol, ethanol, and acetone. The solid content concentration of the raw material slurry is, for example, 10 to 50% by mass, preferably 20 to 40% by mass, in order to facilitate spray drying of the raw material slurry.

[0045] 《Process (b)》 In step (b) above, the raw material slurry is spray-dried to obtain particles (hereinafter also referred to as "spray-dried particles").

[0046] The spray drying conditions may be appropriately changed depending on the solid content concentration, viscosity, etc., of the raw material slurry, and are not particularly limited as long as the average particle size of the resulting spray-dried particles is in the range of 50 to 90 μm, similar to general FCC catalyst particles.

[0047] For example, the raw material slurry is placed in the slurry storage tank of a spray dryer, and the raw material slurry is sprayed into a drying chamber through which an airflow (e.g., an airflow) set to a temperature range of, for example, 120 to 450°C flows, thereby obtaining particles (spray-dried particles). Although the temperature of the airflow decreases due to the spraying of the raw material slurry, the temperature at the outlet of the drying chamber is maintained in a range of, for example, 50 to 300°C by using a heater or the like.

[0048] The particle size of the spray-dried particles can be controlled by adjusting the concentration, viscosity, spray volume, and spray pressure of the raw material slurry, as well as the nozzle diameter and hot air temperature of the spray dryer. Alternatively, the spray-dried particles may be washed (for example, with water) and dried.

[0049] 《Process (c)》 In step (c), the spray-dried particles are brought into contact with an aqueous solution containing a rare earth metal to introduce the rare earth metal into the zeolite in the spray-dried particles. This step (c) yields an FCC catalyst.

[0050] In step (c) above, preferably, the spray-dried particles are suspended in water to prepare a suspension, and this suspension is brought into contact with an aqueous solution containing an ion-exchangeable rare earth metal. The resulting solids (FCC catalyst) may then be separated, washed, and dried. The temperature of the water is preferably 40 to 80°C. Alternatively, the suspension may be filtered, and the filtered solids may be suspended again in water to remove any unwanted soluble substances present in the spray-dried particles.

[0051] The aqueous solution containing the rare earth metal can be prepared, for example, by dissolving a salt of the rare earth metal (e.g., LaCl3) in water. Step (c) is carried out so that the concentration of the rare earth metal in the resulting fluid catalytic cracking catalyst is 0.5 to 1.2% by mass, preferably 0.6 to 1.1% by mass, when converted to rare earth metal oxide (RE2O3). The amount, concentration, etc., of the aqueous solution containing the rare earth metal are adjusted so that the rare earth metal oxide reaches the desired content.

[0052] Even when the zeolite does not contain rare earth metals, or when REUSY is used as the zeolite and some rare earth metal ions are removed from REUSY (replaced by protons) during the preparation of the raw material slurry in step (a) or during the washing of the spray-dried particles obtained in step (b), a fluid catalytic cracking catalyst containing a desired amount of rare earth metal can be produced by performing step (c).

[0053] The above-described fluid catalytic cracking catalyst can be produced by the method for producing a fluid catalytic cracking catalyst according to the present invention, which includes the above-described steps (a) to (c).

[0054] [Fluid catalytic cracking catalyst composition] The fluid catalytic cracking catalyst composition according to the present invention comprises the FCC catalyst according to the present invention and an auxiliary catalyst containing ZSM-5.

[0055] Examples of commercially available additives containing ZSM-5 include the additive (OCTUP-α) manufactured by JGC Catalysts & Chemicals Ltd., and the ZSM-5 additive or ZSM-5-containing additive described in paragraph

[0038] of Japanese Patent Publication No. 2013-522025. The content ratio of the additive in the catalyst composition is preferably 1 to 35% by mass, more preferably 5 to 25% by mass, relative to the FCC catalyst.

[0056] Here, the auxiliary catalyst containing ZSM-5 is not limited to OCTUP-α, but any FCC catalyst containing ZSM-5 available on the market may be used instead. The specific surface area of ​​the FCC catalyst composition according to the present invention, as measured by the method described later, is preferably 200 to 400 m². 2 / g, more preferably 250-350m 2 It is / g.

[0057] When the FCC catalyst composition according to the present invention is used in fluid catalytic cracking, the yield of propylene can be improved. Because the hydrogen transfer reaction in the parent catalyst is suppressed, the yield of the olefin fraction, which is the source of propylene, increases, and the effect of the co-catalyst containing ZSM-5 becomes more apparent. It is presumed that the use of a predetermined binder changes the coating state of the zeolite to a state different from that of the conventional method, thereby suppressing the hydrogen transfer reaction on the acid sites of the zeolite. [Examples]

[0058] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0059] [Methods for measuring or evaluating catalysts, etc.] (composition) The content of each element in the zeolite and catalysts obtained in the examples was measured using an X-ray fluorescence analyzer (Rigaku Corporation, RIX 3000).

[0060] (Lattice constant of zeolite) The lattice constant of the zeolite was determined by the interplanar spacing of the (553) and (642) diffraction planes of the zeolite, using anatase-type TiO2 as the standard material and X-ray diffraction under the following conditions.

[0061] Measurement conditions After crushing and molding the catalysts obtained in the examples, etc., they were set in an X-ray diffractometer (Rigaku Corporation X-RAY DIFFRACT METER (RINT 1400)) and measured under the following conditions: tube voltage 30.0kV, tube current 130.0mA, cathode Cu, measurement range: start angle ~ end angle (2θ) 10.000° ~ 70.000°, scan speed 2.000° / min, divergence slit 1deg, scattering slit 1deg, and receiving slit 0.15mm.

[0062] (specific surface area) The specific surface area of ​​the catalysts in the examples was measured using BELSORP-mini Ver2.5.6 manufactured by Microtrac-Bell Co., Ltd. Specifically, the catalyst was heat-treated at 500°C for 1 hour under vacuum, nitrogen gas was adsorbed onto it, and the specific surface area (m²) was measured by the BET method. 2 The value per gram ( / g) was calculated.

[0063] [Example 1] ~FCC catalyst-1 preparation~ 2647g of water glass (SiO2 concentration: 17% by mass) and 1598g of sulfuric acid (sulfuric acid concentration: 25% by mass) were added simultaneously and sequentially to prepare 4245g of silica hydrosol (an example of a silica binder) with an SiO2 concentration of 10.6% by mass and a pH of 1.0 (measured at 35-37°C). Molar ratio ([H + The SiO2 ratio was 1.09. To this silica hydrosol, 923 g of kaolin (solid content: 84% by mass), 484 g of activated alumina (solid content: 62% by mass) as an active matrix forming component, and 1731 g of alumina-silica slurry containing 4% silica (solid content: 12% by mass), whose pH was adjusted to 3.0 with sulfuric acid, were added. Furthermore, 2273 g of ultra-stable Y-type zeolite slurry (solid content: 33% by mass), whose pH was adjusted to 3.9 with sulfuric acid, were added and stirred. This mixed slurry was then spray-dried to obtain spherical particles with an average particle size of 70 μm. The obtained spherical particles were washed with hot water (60°C), then subjected to ion exchange with an aqueous ammonium sulfate solution, and finally contacted with an aqueous lanthanum chloride solution. Ion exchange was performed so that the lanthanum content in the FCC catalyst was 1.0% by mass in terms of La2O3. The obtained washed cake was dried in a dryer maintained at an ambient temperature of 150°C for 10 hours to obtain FCC catalyst-1.

[0064] [Example 2] ~FCC catalyst-2 preparation~ During the preparation of the silica hydrosol, 2647g of water glass (SiO2 concentration: 17% by mass) and 2244g of sulfuric acid (sulfuric acid concentration: 25% by mass) were added simultaneously and continuously (molar ratio ([H +FCC Catalyst-2 was obtained in the same manner as in Example 1, except that 4891 g of a silica sol having a molar ratio ([H + ] / [SiO2]) of 1.53, a SiO2 concentration of 9.2% by mass, and a pH of 0.6 was prepared.

[0065] [Example 3] ~Preparation of FCC Catalyst-3~ During the preparation of the silica sol, 2647 g of water glass (SiO2 concentration: 17% by mass) and 2585 g of sulfuric acid (sulfuric acid concentration: 25% by mass) were continuously added simultaneously (molar ratio ([H + / [SiO2]) of 1.76), and FCC Catalyst-3 was obtained in the same manner as in Example 1, except that 5233 g of a silica sol having a SiO2 concentration of 8.6% by mass and a pH of 0.4 was prepared.

[0066] [Example 4] ~Preparation of FCC Catalyst-4~ During the preparation of the silica sol, 2647 g of water glass (SiO2 concentration: 17% by mass) and 1266 g of sulfuric acid (sulfuric acid concentration: 25% by mass) were continuously added simultaneously (molar ratio ([H + / [SiO2]) of 0.86), and FCC Catalyst-4 was obtained in the same manner as in Example 1, except that 3913 g of a silica sol having a SiO2 concentration of 11.5% by mass and a pH of 1.3 was prepared.

[0067] [Comparative Example 1] ~Preparation of FCC Catalyst-R1~ During the preparation of the silica sol, 2647 g of water glass (SiO2 concentration: 17% by mass) and 953 g of sulfuric acid (sulfuric acid concentration: 25% by mass) were continuously added simultaneously (molar ratio ([H + / [SiO2]) of 0.65), and FCC Catalyst-R1 was obtained in the same manner as in Example 1, except that 3600 g of a silica sol having a SiO2 concentration of 12.5% by mass and a pH of 1.6 was prepared.

[0068] [Comparative Example 2] ~Preparation of FCC Catalyst-R2~ During the preparation of the silica hydrosol, 2647g of water glass (SiO2 concentration: 17% by mass) and 762g of sulfuric acid (sulfuric acid concentration: 25% by mass) were added simultaneously and continuously (molar ratio ([H + FCC catalyst-R2 was obtained in the same manner as in Example 1, except that 3409 g of silica hydrosol was prepared with a ratio of 0.52 ([SiO2]), an SiO2 concentration of 13.1% by mass, and a pH of 1.8.

[0069] [Comparative Example 3] ~FCC catalyst-R3 preparation~ FCC catalyst-R3 was obtained in the same manner as in Example 1, except that 1596 g of an aqueous solution of basic aluminum chloride (solid content concentration: 23.5% by mass) prepared by the method described in the Examples of Japanese Patent Application Publication No. 2021-121420 was used instead of silica hydrosol, and the amount of kaolin (solid content concentration: 84% by mass) used was changed to 1012 g.

[0070] The composition and properties of the FCC catalyst are summarized in Tables 1-1 and 1-2.

[0071] [Table 1-1]

[0072] [Table 1-2]

[0073] In Table 1-2, "fresh catalyst" refers to the catalyst obtained in the examples or comparative examples, and "steam-treated catalyst" refers to the fresh catalyst that has been steam-treated under conditions of being held at 810°C under 100% water vapor conditions for 12 hours. The retention rate (%) is expressed as a percentage of the specific surface area of ​​the steam-treated catalyst divided by the specific surface area of ​​the fresh catalyst. A higher retention rate indicates higher water and heat resistance.

[0074] <Method for producing a fluid catalytic cracking catalyst composition> A fluid catalytic cracking catalyst composition was obtained by mixing 15% by mass of an additive (OCTUP-α) manufactured by JGC Catalysts & Chemicals Co., Ltd. as an auxiliary catalyst containing ZSM-5 with the FCC catalyst obtained in the examples or comparative examples.

[0075] The obtained fluid catalytic cracking catalyst compositions were subjected to performance evaluation tests using ACE-MAT (Advanced Cracking Evaluation-Micro Activity Test) under the same crude oil and reaction conditions. The results of the performance evaluation tests for each catalyst composition are shown in Table 2.

[0076] However, prior to conducting these performance evaluation tests, a steam treatment at 810°C for 12 hours was performed to simulate the conditions under which the catalyst regeneration tower would undergo hydrothermal degradation. The operating conditions for the performance evaluation test are as follows:

[0077] Raw material oil: Desulfurized vacuum diesel fuel (DSVGO) 100% by mass Catalyst / oil flow rate by weight ratio (hereinafter referred to as "C / O"): 5.0 (mass% / mass%) Catalyst mass-based space velocity (WHSV): 8h -1 Reaction temperature: 580℃ 1) Conversion rate=100-(LCO+HCO+CLO) (mass%) 2) Yield: The weight of each product when C / O = 5.0 was expressed as mass %. 3) Boiling point range of gasoline: 30~216℃ (Gasoline) 4) Boiling point range of LCO: 216~343℃ (LCO: Light Cycle Oil) 5) Boiling point range of HCO+CLO: 343°C+ (HCO: Heavy Cycle Oil, CLO: Clarified Oil) 6) LPG (Liquid Petroleum Gas) 7) Dry Gas: Methane, ethane, and ethylene 8) Propylene: Included in LPG.

[0078] The reaction results are summarized in Table 2.

[0079] Table 2

Claims

1. (a) preparing a raw material slurry by mixing a silica-based binder-forming component having a pH of less than 1.6, an FAU-type zeolite, clay minerals, and an active matrix-forming component; (b) spray-drying the raw slurry to obtain particles; (c) contacting the particles with an aqueous solution containing a rare earth metal to ion-exchange the zeolite with the rare earth metal; Equipped A method for producing a fluid catalytic cracking catalyst.

2. A process for preparing a raw material slurry by mixing a silica-based binder-forming component having a pH of less than 1.6, an FAU-type zeolite, clay minerals, and an active matrix-forming component; spray-drying the raw slurry to obtain particles; contacting the particles with an aqueous solution containing a rare earth metal to ion-exchange the zeolite with the rare earth metal to obtain a fluid catalytic cracking catalyst; mixing the fluid catalytic cracking catalyst with a co-catalyst comprising ZSM-5. A method for producing a fluid catalytic cracking catalyst composition.