Medical rubber composition, medical rubber part, and package for medical rubber part
Patent Information
- Application Number
- JP2021208610
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2021-12-22
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2041-12-22
AI Technical Summary
Medical rubber parts sterilized with gamma rays experience polymer chain scission and low-molecular-weight component elution, leading to adhesion and reduced elution properties, with antioxidants potentially compromising drug compatibility.
A medical rubber composition comprising halogenated butyl rubber, polyethylene, and a triazine derivative as a cross-linking agent, with specific ratios and additives to prevent chain scission and maintain non-elution properties.
The composition ensures non-elution properties post-sterilization, reducing manufacturing issues and maintaining compatibility with medical supplies.
Smart Images

Figure 00000015_0000 
Figure 00000015_0001 
Figure 00000015_0002
Abstract
Description
[Technical Field]
[0001] The present disclosure relates to a medical rubber composition for gamma ray sterilization, and a gamma ray sterilized medical rubber part and its packaging. [Background technology]
[0002] Medical rubber stoppers, which seal the openings of syringes, vials, etc., are required to have many properties, such as non-elution, high cleanliness, chemical resistance, needle-prick resistance, self-sealing properties, and high sliding properties. The quality characteristics required of medical rubber stoppers should conform to the rubber stopper test for infusions in the 17th revision of the Japanese Pharmacopoeia, given their intended use.
[0003] For example, Patent Document 1 discloses a rubber stopper for pharmaceutical containers, which is obtained by vulcanizing halogenated butyl rubber, in which 5 to 25 parts by weight of ultra-high molecular weight polyethylene fine powder is blended per 100 parts by weight of halogenated butyl rubber, with at least one 2-substituted-4,6-dithiol-s-triazine derivative or an organic peroxide in the absence of a zinc compound.
[0004] There is an increasing demand for ready-to-use (RTU) medical rubber products (such as syringe gaskets and vial stoppers) that are delivered in a sterilized state. Sterilization assurance methods include high-pressure steam sterilization, ethylene oxide gas (EOG) sterilization, and gamma ray sterilization. Gamma ray sterilization allows medical rubber products to be sterilized in their packaging, so it has the advantage of allowing them to be delivered without opening the packaging. Due to environmental concerns, there is a trend towards gamma ray sterilization over EOG sterilization.
[0005] Gamma ray sterilization guarantees sterilization by setting and measuring the absorbed dose. When multiple medical rubber parts are packed into a packaging bag and then gamma ray sterilized, uneven distribution of the medical rubber parts within the packaging bag may occur. Therefore, even if the packaging bag is irradiated with gamma rays at a specified exposure dose, variations in the absorbed dose of gamma rays may occur within the packaging bag, resulting in some with a low absorbed dose and others with a high absorbed dose. However, it is necessary to ensure a minimum absorbed dose that can sterilize each medical rubber part, and therefore the packaging bag must be irradiated with gamma rays that is equal to or greater than the minimum absorbed dose. As a result, some medical rubber parts within the packaging bag will absorb excessive gamma rays during gamma ray sterilization.
[0006] Patent Document 2 discloses a rubber composition or crosslinked product thereof that is used for medical rubber stoppers or medical rubber products, which has an isobutylene copolymer as the main component and a density of 0.95 or less and is easy to treat with radiation.
[0007] Patent Document 3 discloses a method for packaging an elastomer part (1) such as a stopper for a pharmaceutical container, which comprises the steps of packing the part (1) into a primary bag (10) made of a material that is substantially impermeable to air, and applying an atmosphere of at least 80% nitrogen to the primary bag (10), and is characterized in that the primary bag (10) is placed into a secondary bag (20) and a vacuum is created between the primary bag (10) and the secondary bag (20). [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 10-179690 [Patent Document 2] Japanese Patent Application Laid-Open No. 2002-301133 [Patent Document 3] Special Publication No. 2017-531604 Summary of the Invention [Problem to be solved by the invention]
[0009] When medical rubber parts are sterilized by gamma rays, the polymers that make up the medical rubber parts are simultaneously cleaved and crosslinked. Excessive gamma rays accelerate the cleavage of the polymer main chains that make up the medical rubber parts, resulting in the generation of low-molecular-weight components. This results in poor elution performance of the medical rubber parts after gamma ray sterilization. Furthermore, the cleaved low-molecular-weight components bleed out onto the surface of the rubber parts, causing the medical rubber parts to adhere to each other, leading to clogging of part feeders used in the medical supply manufacturing process.
[0010] One option is to incorporate antioxidants into medical rubber parts to prevent excessive gamma ray absorption, but there are concerns that adding antioxidants may reduce elution characteristics and have adverse effects on drugs.
[0011] The present disclosure has been made in view of the above circumstances, and aims to provide a medical rubber part and a package for the medical rubber part that maintain non-elution properties even after gamma ray sterilization and that cause few problems in the manufacturing process of medical supplies, as well as a medical rubber composition for manufacturing the medical rubber part. [Means for solving the problem]
[0012] The medical rubber composition of the present disclosure comprises: (a) a base polymer containing a halogenated butyl rubber; (b) polyethylene; (c) containing a triazine derivative as a crosslinking agent, The content of the triazine derivative is 1 mol % to 15 mol % relative to 100 mol % of halogen in the (a) halogenated butyl rubber. [Effects of the Invention]
[0013] According to the present disclosure, it is possible to provide a medical rubber part and its packaging that maintains its non-elution properties even after gamma ray sterilization and causes few problems in the manufacturing process of medical supplies. According to the present disclosure, it is possible to provide a medical rubber composition suitable for manufacturing the medical rubber part. [Brief explanation of the drawings]
[0014] [Figure 1] FIG. 2 is an explanatory view schematically illustrating an example of a packaging form for the medical rubber part of the present disclosure. [Figure 2] FIG. 10 is an explanatory view schematically showing another example of a packaging form for the medical rubber part of the present disclosure. [Figure 3] FIG. 2 is an explanatory diagram schematically illustrating a method for testing adhesion of a medical rubber part according to the present disclosure. DETAILED DESCRIPTION OF THE INVENTION
[0015] The medical rubber composition of the present disclosure is characterized in that it contains (a) a base polymer containing a halogenated butyl rubber, (b) polyethylene, and (c) a triazine derivative as a crosslinking agent, and the content of the (c) triazine derivative is 1 mol % to 15 mol % relative to 100 mol % of the halogen in the (a) halogenated butyl rubber.
[0016] First, the base polymer containing (a) halogenated butyl rubber used in the present disclosure will be described. Examples of halogenated butyl rubber include chlorinated butyl rubber, brominated butyl rubber, and brominated copolymer rubber of isobutylene and p-methylstyrene (brominated isobutylene-paramethylene-styrene copolymer rubber).
[0017] The halogenated butyl rubber is preferably chlorinated butyl rubber or brominated butyl rubber. The chlorinated butyl rubber or brominated butyl rubber is obtained by, for example, adding or substituting chlorine or bromine to the isoprene structure of butyl rubber, specifically to the double bond and / or the carbon atom adjacent to the double bond. Note that butyl rubber is a copolymer obtained by polymerizing isobutylene and a small amount of isoprene.
[0018] The halogen content in the halogenated butyl rubber is preferably 0.5% by mass or more, preferably 1% by mass or more, more preferably 1.5% by mass or more, and is preferably 5% by mass or less, more preferably 4% by mass or less, and even more preferably 3% by mass or less.
[0019] A specific example of the chlorinated butyl rubber is CHLOROBUTYL 1066 (stabilizer: NS, halogen content: 1.26%, Mooney viscosity: 38ML) manufactured by Japan Butyl Co., Ltd. 1+8 (125°C, specific gravity: 0.92); LANXESS X_BUTYL CB1240 manufactured by LANXESS.
[0020] A specific example of the brominated butyl rubber is BROMOBUTYL 2255 (stabilizer: NS, halogen content: 2.0%, Mooney viscosity: 46ML) manufactured by Nippon Butyl Co., Ltd. 1+8 (125°C, specific gravity: 0.93); LANXESS X_BUTYL BBX2 manufactured by LANXESS.
[0021] The base polymer (a) may contain a rubber component other than halogenated butyl rubber. Examples of other rubber components include butyl rubber, isoprene rubber, butadiene rubber, styrene-butadiene rubber, natural rubber, nitrile rubber such as chloroprene rubber or acrylonitrile-butadiene rubber, hydrogenated nitrile rubber, norbornene rubber, ethylene-propylene rubber, ethylene-propylene-diene rubber, acrylic rubber, ethylene-acrylate rubber, fluororubber, chlorosulfonated polyethylene rubber, epichlorohydrin rubber, silicone rubber, urethane rubber, polysulfide rubber, phosphane rubber, and 1,2-polybutadiene. These may be used alone or in combination of two or more.
[0022] When other rubber components are used, the content of the halogenated butyl rubber in the (a) base polymer is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 98% by mass or more. In a preferred embodiment, the (a) base polymer consists solely of the halogenated butyl rubber.
[0023] The medical rubber composition of the present disclosure contains (b) polyethylene. Polyethylene absorbs gamma rays more easily than the (a) base polymer, and is effective in preventing chain scission of the (a) base polymer due to gamma ray irradiation. In addition, polyethylene with a low degree of crystallinity has branched chains, and it is thought that crosslinking proceeds without scission of the main chain even when irradiated with gamma rays. As a result, it is thought that the elution performance of the medical rubber composition is improved.
[0024] From this perspective, the polyethylene (b) used in the present disclosure may be high-density polyethylene (HDPE) or low-density polyethylene (LDPE). High-density polyethylene (HDPE) and low-density polyethylene (LDPE) may be used alone, or high-density polyethylene (HDPE) and low-density polyethylene (LDPE) may be used in combination.
[0025] When high density polyethylene (HDPE) and low density polyethylene (LDPE) are used in combination, the mass ratio of high density polyethylene (HDPE) to low density polyethylene (LDPE) (HDPE / LDPE) is preferably 0.3 or more, more preferably 0.5 or more, even more preferably 1.0 or more, and preferably 5.0 or less, more preferably 4.0 or less, and even more preferably 3.0 or less. This is because, when the mass ratio of high density polyethylene (HDPE) to low density polyethylene (LDPE) (HDPE / LDPE) is within the above range, the radical absorption effect during gamma ray irradiation and appropriate hardness of the rubber can be ensured.
[0026] (b) The polyethylene preferably contains polyethylene having a crystallinity of 70% or less.
[0027] The crystallinity of high-density polyethylene (HDPE) is preferably 60% to 80%, more preferably 60% to 75%, and even more preferably 60% to 70%. The crystallinity of low-density polyethylene (LDPE) is preferably 30% to 50%, more preferably 30% to 45%, and even more preferably 30% to 40%. This is because, if the crystallinity of polyethylene is within the above range, it effectively absorbs radicals generated by gamma ray irradiation and prevents scission of the polymer main chain.
[0028] (b) The crystallinity of polyethylene is determined by the following formula: Crystallinity (%) = (measured heat of fusion (J / g) / heat of fusion of completely crystalline substance (J / g)) x 100 The heat of fusion (J / g) of a completely crystalline polyethylene is 293 J / g (literature value), which is the heat of fusion of polyethylene when it is 100% crystalline. The method for measuring the heat of fusion of polyethylene will be described later.
[0029] (b) The polyethylene is preferably low-density polyethylene. The density (g / cm 3 ) is preferably 0.930 to 0.960, more preferably 0.930 to 0.950. The density (g / cm 3 ) is not particularly limited, but is preferably 0.910 to 0.925, and more preferably 0.910 to 0.920.
[0030] (b) The polyethylene used is preferably in the form of a fine powder. The volume average particle diameter of the fine powder polyethylene is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more, and is preferably 200 μm or less, more preferably 160 μm or less, and even more preferably 120 μm or less. When the average particle diameter of the fine powder polyethylene is within the above range, it is easy to mix and disperse uniformly in the polymer.
[0031] The blend amount of (b) the polyethylene is preferably 3 parts by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, and is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less, per 100 parts by mass of the (a) base polymer. This is because, when the blend amount of (b) polyethylene is within the above range, radicals generated during gamma ray irradiation can be effectively absorbed and scission of the polymer main chain can be prevented.
[0032] The medical rubber composition of the present disclosure preferably contains a triazine derivative as the (c) crosslinking agent.
[0033] The triazine derivative acts as a cross-linking agent for halogenated butyl rubber. Examples of the triazine derivative include compounds represented by general formula (1). [ka] [Wherein R is -SH, -OR 1 , -SR 2 , -NHR 3 or -NR 4 R 5 (R 1 , R 2 , R 3 , R 4 and R 5 represents an alkyl group, an alkenyl group, an aryl group, an aralkyl group, an alkylaryl group, or a cycloalkyl group. 4 and R 5 may be the same or different. 1 and M 2 is H, Na, Li, K, 1 / 2Mg, 1 / 2Ba, 1 / 2Ca, an aliphatic primary amine, a secondary amine, or a tertiary amine, a quaternary ammonium salt, or a phosphonium salt. 1 and M 2 may be the same or different.]
[0034] In general formula (1), examples of the alkyl group include alkyl groups having 1 to 12 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, tert-pentyl, n-hexyl, 1,1-dimethylpropyl, octyl, isooctyl, 2-ethylhexyl, decyl, and dodecyl. Examples of the alkenyl group include alkenyl groups having 1 to 12 carbon atoms, such as vinyl, allyl, 1-propenyl, isopropenyl, 2-butenyl, 1,3-butadienyl, and 2-pentenyl. Examples of the aryl group include monocyclic or fused polycyclic aromatic hydrocarbon groups, such as aryl groups having 6 to 14 carbon atoms, such as phenyl, naphthyl, anthryl, phenanthryl, and acenaphthylenyl. Examples of aralkyl groups include aralkyl groups having 7 to 19 carbon atoms, such as benzyl, phenethyl, diphenylmethyl, 1-naphthylmethyl, 2-naphthylmethyl, 2,2-diphenylethyl, 3-phenylpropyl, 4-phenylbutyl, 5-phenylpentyl, 2-biphenylylmethyl, 3-biphenylylmethyl, and 4-biphenylylmethyl. Examples of alkylaryl groups include alkylaryl groups having 7 to 19 carbon atoms, such as tolyl, xyl, and octylphenyl. Examples of cycloalkyl groups include cycloalkyl groups having 3 to 9 carbon atoms, such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, and cyclononyl.
[0035] Specific examples of the triazine derivative represented by general formula (1) include 2,4,6-trimercapto-s-triazine, 2-methylamino-4,6-dimercapto-s-triazine, 2-(n-butylamino)-4,6-dimercapto-s-triazine, 2-octylamino-4,6-dimercapto-s-triazine, 2-propylamino-4,6-dimercapto-s-triazine, 2-diallylamino-4,6-dimercapto-s-triazine, 2-dimethylamino-4,6-dimercapto-s-triazine, 2-dibutylamino- Examples include 4,6-dimercapto-s-triazine, 2-di(iso-butylamino)-4,6-dimercapto-s-triazine, 2-dipropylamino-4,6-dimercapto-s-triazine, 2-di(2-ethylhexyl)amino-4,6-dimercapto-s-triazine, 2-dioleylamino-4,6-dimercapto-s-triazine, 2-laurylamino-4,6-dimercapto-s-triazine, and 2-anilino-4,6-dimercapto-s-triazine, or sodium salts or disodium salts thereof.
[0036] Among these, 2,4,6-trimercapto-s-triazine, 2-dialkylamino-4,6-dimercapto-s-triazine, and 2-anilino-4,6-dimercapto-s-triazine are preferred, and 2-dibutylamino-4,6-dimercapto-s-triazine is particularly preferred due to its easy availability.
[0037] Examples of triazine derivatives include one or more of 6-[bis(2-ethylhexyl)amino]-1,3,5-triazine-2,4-dithiol, 6-diisobutylamino-1,3,5-triazine-2,4-dithiol, 6-dibutylamino-1,3,5-triazine-2,4-dithiol, 6-dibutylamino-1,3,5-triazine-2,4-dithiol monosodium, 6-anilino-1,3,5-triazine-2,4-dithiol, and 1,3,5-triazine-2,4,6-trithiol.
[0038] In the present disclosure, one type of triazine derivative may be used alone, or two or more types may be used in combination.
[0039] The content of the triazine derivative in the medical rubber composition of the present disclosure is preferably 1 mol% or more, more preferably 5 mol% or more, even more preferably 8 mol% or more, preferably 10 mol% or more, more preferably 15 mol% or less, and even more preferably 12 mol% or less, relative to 100 mol% of halogen in the (a) halogenated butyl rubber. When the content of the triazine derivative is within the above range, no residual triazine derivative remains in the rubber composition after vulcanization, and the triazine derivative is entirely used for crosslinking, thereby achieving good rubber properties (hardness, tensile strength, Cset) and elution characteristics.
[0040] The content of (c) the triazine derivative in the medical rubber composition of the present disclosure is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and preferably 1.4 parts by mass or less, and more preferably 1.2 parts by mass or less, per 100 parts by mass of the (a) base polymer component, because if the content of (c) the triazine derivative is within the above range, a rubber with good rubber properties (hardness, tensile strength, Cset) and good processability (less discoloration) can be obtained.
[0041] The medical rubber composition of the present disclosure preferably does not contain a vulcanization accelerator. This is because the vulcanization accelerator may remain in the final rubber product and leach into the medicinal solution in the syringe or vial. Examples of the vulcanization accelerator include guanidine-based accelerators (e.g., diphenyl guanidine), thiuram-based accelerators (e.g., tetramethylthiuram disulfide, tetramethylthiuram monosulfide), dithiocarbamate-based accelerators (e.g., zinc dimethyldithiocarbamate), thiazole-based accelerators (e.g., 2-mercaptobenzothiazole, dibenzothiazyl disulfide), and sulfenamide-based accelerators (N-cyclohexyl-2-benzothiazole sulfenamide, Nt-butyl-2-benzothiazole sulfenamide).
[0042] The medical rubber composition of the present disclosure may contain hydrotalcite. Hydrotalcite functions as a scorch inhibitor during crosslinking of halogenated butyl rubber and also functions to prevent the compression set of medical rubber parts from increasing. Furthermore, hydrotalcite functions as an acid acceptor, absorbing chlorine-based gases and bromine-based gases generated during crosslinking of halogenated butyl rubber and preventing crosslinking inhibition caused by these gases. The aforementioned magnesium oxide can also function as an acid acceptor.
[0043] Examples of hydrotalcite include Mg 4.5 Al2(OH) 13 CO3·3.5H2O, Mg 4.5 Al2(OH) 13 CO3, Mg4Al2(OH) 12 CO3·3.5H2O, Mg6Al2(OH) 16 CO3·4H2O, Mg5Al2(OH) 14 CO3·4H2O, Mg3Al2(OH) 10 One or more of Mg-Al hydrotalcites such as CO3·1.7H2O can be used.
[0044] A specific example of hydrotalcite is DHT-4A (registered trademark)-2 manufactured by Kyowa Chemical Industry Co., Ltd.
[0045] When hydrotalcite is used as an acid acceptor in a medical rubber composition, it is preferably used in combination with MgO. In this case, the blending amount of hydrotalcite is preferably considered to be the total amount of acid acceptors (hydrotalcite and MgO). The total content of the acid acceptors (hydrotalcite and MgO) is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and preferably 15 parts by mass or less, and more preferably 10 parts by mass or less, per 100 parts by mass of the (a) base polymer component. This is because, if the total content of the acid acceptors (hydrotalcite and MgO) is within the above range, rust formation on molds and the like can be suppressed, and problems such as the raw materials themselves becoming white spots can be reduced.
[0046] The medical rubber composition of the present disclosure may contain a co-crosslinking agent. The co-crosslinking agent is preferably a polyfunctional (meth)acrylate compound. The polyfunctional (meth)acrylate compound is more preferably a difunctional or higher (meth)acrylate compound, even more preferably a trifunctional or higher (meth)acrylate compound, preferably an octafunctional or lower (meth)acrylate compound, and preferably a hexafunctional or lower (meth)acrylate compound. Examples of difunctional or higher (meth)acrylate compounds include compounds having at least two acryloyl groups and / or methacryloyl groups. Note that "(meth)acrylate" means "acrylate" and / or "methacrylate."
[0047] Examples of the difunctional or higher functional (meth)acrylate compounds include polyethylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and glycerin tri(meth)acrylate. (meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol tetra(meth)acrylate, tripentaerythritol penta(meth)acrylate, tripentaerythritol hexa(meth)acrylate, tripentaerythritol hepta(meth)acrylate, etc. The co-crosslinking agent may be used alone or in combination of two or more thereof.
[0048] The medical rubber composition of the present disclosure may contain (d) a filler. Examples of the (d) filler include inorganic fillers such as silica, clay, and talc. Clay or talc is more preferred as the filler. The filler functions to adjust the rubber hardness of the medical rubber part and also functions as an extender to reduce the production cost of the medical rubber part.
[0049] Examples of the clay include calcined clay and kaolin clay. Specific examples of the clay include SILLITIN (registered trademark) Z manufactured by HOFFMANN MINERAL, SATINTONE (registered trademark) W manufactured by ENGELHARD, NN kaolin clay manufactured by Tsuchiya Kaolin Kogyo Co., Ltd., and PoleStar 200R manufactured by Imerys Specialties Japan.
[0050] Specific examples of the talc include Hitron A manufactured by Takehara Chemical Industry Co., Ltd., MICRO ACE (registered trademark) K-1 manufactured by Nippon Talc Co., Ltd., and Mistron (registered trademark) Vapor manufactured by Imerys Specialties Japan.
[0051] The medical rubber composition of the present disclosure may further contain colorants such as titanium oxide and carbon black, processing aids, polyethylene glycol as a crosslinking activator, plasticizers (e.g., paraffin oil), etc. in appropriate proportions.
[0052] The present disclosure includes medical rubber parts molded from the medical rubber composition of the present disclosure. Examples of the medical rubber parts of the present disclosure include rubber stoppers and sealing members for containers (e.g., vials) for various drugs such as liquids, powders, and freeze-dried preparations, rubber stoppers for vacuum blood collection tubes, plunger stoppers for pre-filled syringes, and sliding or sealing parts such as nozzle caps.
[0053] The medical rubber composition of the present disclosure can be obtained by kneading (a) a base polymer containing a halogenated butyl rubber, (b) polyethylene, (c) a triazine derivative as a crosslinking agent, and other compounding materials added as needed. Kneading can be performed using, for example, an open roll or an internal kneader. The kneaded product is preferably formed into a ribbon, sheet, pellet, or other shape, and more preferably formed into a sheet.
[0054] A medical rubber part of the desired shape can be obtained by press-molding the kneaded material in ribbon, sheet, or pellet form. The crosslinking reaction of the medical rubber composition progresses during pressing. The molding temperature is, for example, preferably 130°C or higher, more preferably 140°C or higher, and preferably 200°C or lower, more preferably 190°C or lower. The molding time is preferably 2 minutes or longer, more preferably 3 minutes or longer, and preferably 60 minutes or shorter, more preferably 30 minutes or shorter. The molding pressure is preferably 0.1 MPa or higher, more preferably 0.2 MPa or higher, and preferably 10 MPa or lower, more preferably 8 MPa or lower.
[0055] After press molding, unnecessary parts are cut and removed to form the desired shape. The resulting molded product is then washed, dried, and packaged to produce medical rubber parts.
[0056] Medical rubber parts may also be integrated with a resin film laminated thereon, such as films of inactive resins such as polytetrafluoroethylene (PTFE), tetrafluoroethylene-ethylene copolymer (ETFE), modified versions of these, and ultra-high density polyethylene (UHMWPE).
[0057] The resin film may be press-molded, for example, in a state where it is superimposed on a sheet-shaped rubber composition, so that it is integrated with the medical rubber part formed after press-molding.
[0058] The present disclosure includes a medical rubber part package comprising a plurality of medical rubber parts of the present disclosure housed in a package, the medical rubber part package being characterized in that it has been subjected to gamma ray sterilization.
[0059] Examples of gamma rays include gamma rays emitted from cobalt 60 and cesium 137, with gamma rays emitted from cobalt 60 being preferred.
[0060] The gamma ray absorbed dose of medical rubber parts is established through actual sterilization validation procedures. For typical medical devices, 15 kGy is often used as the minimum absorbed dose. The gamma ray exposure dose required to ensure that all medical rubber parts in a package receive an absorbed dose of 15 kGy or more varies depending on the number and arrangement of the medical rubber parts in the package, but is generally 1.4 to 2.0 times 15 kGy. Similarly, if the minimum absorbed dose is 20 kGy, the exposure dose should be 1.4 to 2.0 times 20 kGy, and if the minimum absorbed dose is 25 kGy, the exposure dose should be 1.4 to 2.0 times 25 kGy. The gamma ray absorbed dose can be confirmed by attaching a dosimeter to the irradiated object.
[0061] The oxygen concentration in the package containing the medical rubber part before gamma ray sterilization is preferably 5% or less, more preferably 3% or less, and even more preferably 1% or less. By keeping the oxygen concentration in the package at 5% or less, deterioration of the (a) base polymer due to gamma ray irradiation can be suppressed.
[0062] Methods for reducing the oxygen concentration in the package to 5% or less include replacing the air in the package with an inert gas and placing an oxygen absorber in the package.
[0063] The inert gas may be a rare gas such as helium, neon, or argon, or nitrogen gas.
[0064] The oxygen absorber may include an iron-based oxygen absorber, Ageless (commercially available product).
[0065] The packaging for housing the medical rubber part is not particularly limited as long as it can be irradiated with gamma rays. Examples of the packaging include a bag, a box, and the like.
[0066] Examples of the packaging bag include a packaging bag made of a thermoplastic resin film such as polyethylene, polyamide, or polyester. The packaging bag is preferably airtight. Examples of the box include, but are not limited to, a paper box, a cardboard box, and the like.
[0067] The packaging material may be a breathable packaging material or a non-breathable (gas-tight) packaging material, and it is also preferable to use a combination of these.
[0068] Gamma ray sterilization of medical rubber parts may be performed, for example, by placing multiple medical rubber parts in a primary package (e.g., a packaging bag) and then further placing multiple primary packages in a package (e.g., a cardboard box).
[0069] FIG. 1 is a schematic diagram illustrating an example of a packaging configuration for gamma ray irradiation. In the configuration shown in FIG. 1, a primary package 3 containing multiple medical rubber parts 1 is further housed in a secondary antistatic package 5 and a tertiary antistatic package 7. The primary package 3 is preferably breathable, and the secondary antistatic package 5 and the tertiary antistatic package 7 are preferably gas-tight. The secondary antistatic package 5 and the tertiary antistatic package 7 are preferably sealed with a heat seal 9. If an oxygen absorber 11 is used, it is preferable to place the oxygen absorber 11 between the primary package 3 and the secondary package 5 so that it does not come into direct contact with the medical rubber part 1. By placing the oxygen absorber 11 in the secondary package 5, the oxygen concentration in the secondary package 5 and the primary package 3 can be kept below 5%. Multiple tertiary antistatic packages 7 can be housed in a quaternary package (e.g., a cardboard box) and then irradiated with gamma rays.
[0070] FIG. 2 is an explanatory diagram schematically illustrating another example of a packaging embodiment for gamma ray irradiation. In the embodiment shown in FIG. 2, a primary package 3 containing multiple medical rubber parts 1 is further housed in a secondary antistatic package 5 and a tertiary antistatic package 7. The secondary antistatic package 5 and the tertiary antistatic package 7 are preferably sealed with a heat seal 9. The primary package 3 is preferably breathable, and the secondary antistatic package 5 and the tertiary antistatic package 7 are preferably gas-tight. The secondary package 5 containing the primary package 3 is filled with an inert gas. By filling the secondary package 5 and the primary package 3 with an inert gas, the oxygen concentration in the secondary package 5 and the primary package 3 can be kept below 5%. A plurality of the tertiary antistatic packages 7 can be housed in a quaternary package (e.g., a cardboard box) and then irradiated with gamma rays.
[0071] It is preferable that the package containing the medical rubber parts be irradiated with gamma rays while it is housed in a container made of aluminum alloy, for example. [Example]
[0072] The present disclosure will be described in detail below using examples, but the present disclosure is not limited to the following examples, and all modifications and embodiments that do not deviate from the spirit of the present disclosure are included within the scope of the present disclosure.
[0073] [Preparation of Medical Rubber Composition] The components shown in Table 1, except for the crosslinking component, were blended and kneaded at a filling rate of 75% using a 10 L pressurized closed kneader. After aging at room temperature, the crosslinking component was added and kneaded using an open roll to prepare a rubber composition.
[0074] [Manufacturing medical rubber stoppers] The rubber composition was molded into a sheet, sandwiched between upper and lower molds, and vacuum-pressed at 180°C for 10 minutes to form multiple rubber stoppers for lyophilized injection vials, each with a flange diameter of 19.0 mm, a leg diameter of 13.2 mm, and a flange puncture thickness of 2.5 mm, all on a single sheet. A silicone-based lubricant coating was then applied to both sides of the sheet, followed by visual inspection, punching, washing, sterilization, drying, and packaging to produce the rubber stoppers. The rubber stoppers were used in elution and adhesion tests.
[0075] [Table 1]
[0076] The details of the ingredients used are as follows: Butylated rubber: ExxonMobil HT-1066 (chlorine content: 1.26 wt%) Polyethylene 1: Mipelon XM-220 (crystallinity 69%) manufactured by Mitsui Chemicals, Inc. Polyethylene 2: Flothane UF20S (crystallinity 35%) manufactured by Sumitomo Seika Chemicals Co., Ltd. Triazine derivative: Jisnet DB manufactured by Sankyo Kasei Co., Ltd. Talc: Mistron Vapor manufactured by Imerys Specialties Silica: Nipsil LP manufactured by Tosoh Silica Corporation, Magnesium oxide: Kyowa Chemical Industry Co., Ltd. Magsarat 150s Carbon black: Mitsubishi Chemical Diablack G Titanium oxide: Titanium Kogyo KR-380 Oil: Idemitsu Kosan PW380
[0077] [Evaluation method] (1) Measurement of the heat of fusion of polyethylene The heat of fusion of polyethylene was obtained from a first temperature rise test by differential scanning calorimetry (DSC). DSC measurement conditions: 20℃ to 200℃, heating rate 10℃ / min
[0078] (2) Extractables test Measurement samples: The rubber stoppers were irradiated with gamma rays so that the absorbed doses were 25 kGy and 50 kGy, respectively, to prepare gamma-irradiated rubber stoppers. The measurement samples were subjected to the "Elution Test" described in the 17th Revised Japanese Pharmacopoeia "7.03 Test Method for Rubber Stoppers for Infusions." The compliance conditions were as follows: Test liquid properties: clear and colorless UV transmittance: With a layer length of 10 mm, transmittance at wavelengths of 430 nm and 650 nm is 99.0% or more. Ultraviolet absorption spectrum: absorbance of 0.20 or less in the wavelength range of 220 nm to 350 nm pH: The difference between the test solution and the blank test solution is 1.0 or less Zinc: The absorbance of the sample solution is equal to or less than that of the standard solution. Potassium permanganate reducing agent: 2.0 mL / 100 mL or less (Pharmacopoeia standard) Evaporation residue: 2.0 mg or less If any item was not satisfied, it was rated as "non-compliant," and if all items were satisfied, it was rated as "compliant."
[0079] (3) TOC test The total organic carbon (TOC) value (NPOC: TOC after acidification and aeration treatment) was measured for the eluate from the eluate test in (2). Measurement and analysis equipment: Shimadzu Total Organic Carbon Analyzer TOC-VCSH (combustion oxidation method) Measurement and analysis conditions: combustion tube temperature 680 degrees, high-sensitivity catalyst used, Carrier gas: High-purity air 150 mL / min, Injection volume 200μL, Acid concentration 1.5%, Ventilation time: 90 seconds
[0080] The elution characteristics were evaluated before and after gamma irradiation. The TOC before gamma irradiation was set at 100%, and the TOC after gamma irradiation was evaluated using a relative index. The larger the number, the worse the elution performance compared to before gamma irradiation. Evaluation criteria ◎: Less than 100% (improved from before irradiation) 〇: Over 100%, 120% or less (same as before irradiation) △: Over 120%, under 150% (slightly worse than before irradiation) ×: Over 150% (greater deterioration than before irradiation)
[0081] (4) Adhesion test The measurement was performed using a Shimadzu EZ-SX benchtop testing machine as follows. As shown in Figure 3, the sample 13 was fixed to the lower fixture 15, and the upper metal probe 17 was pressed onto the sample 13. After the set pressure was reached, the pressure was maintained for 10 seconds. The metal probe 17 was then raised, and the peak value of the adhesion force generated between the metal probe 17 and the sample 13 was taken as the tack value. Measurements were performed five times for each sample, and the average of the three measurements, excluding the maximum and minimum values, was calculated. The adhesion force of the sample before gamma irradiation was set to 100, and the adhesion force of the sample after gamma irradiation was indexed. The smaller the index, the lower the adhesion and the better the result. Measurement conditions: Pressing speed: 0.5 mm / s Pressing load: 1000g Pressing time: 10 seconds Pulling speed: 10 mm / s Final pull distance: 3mm Probe diameter: 10mm Evaluation criteria: ◎: Less than 100% (improved from before irradiation) 〇: Over 100%, 120% or less (same as before irradiation) △: Over 120%, under 150% (slightly worse than before irradiation) ×: Over 150% (greater deterioration than before irradiation)
[0082] The results of the extractables test, TOC test, and adhesion test are shown in Table 1.
[0083] The suitability of READY TO USE was judged as follows: If the extractables test results were pass, the TOC test results were rated fair or better, and the adhesion test results were rated fair or better, the product was deemed to be in compliance with READY TO USE. If any one of the evaluation results was not met, the product was deemed to be non-compliant.
[0084] The results in Table 1 show that medical rubber parts formed from a medical rubber composition containing (a) a base polymer containing halogenated butyl rubber, (b) polyethylene, and (c) a triazine derivative as a crosslinking agent, in which the content of the triazine derivative is 1 mol % to 15 mol % relative to 100 mol % of the halogen in (a) the halogenated butyl rubber, maintain their non-elution properties even after gamma ray sterilization. [Industrial Applicability]
[0085] According to the present disclosure, it is possible to provide a medical rubber part and its packaging that maintains its non-elution properties even after gamma ray sterilization and causes few problems in the manufacturing process of medical supplies. According to the present disclosure, it is possible to provide a medical rubber composition suitable for manufacturing the medical rubber part. [Explanation of symbols]
[0086] 1: Medical rubber parts, 3: Primary packaging, 5: Secondary packaging, 7: Tertiary packaging, 9: Heat seal, 11: Oxygen absorber, 13: Sample, 15: Fixture, 17: Metal probe
[0087] The medical rubber composition of the present disclosure (1) (a) a base polymer containing a halogenated butyl rubber; (b) polyethylene; (c) containing a triazine derivative as a crosslinking agent, The content of the triazine derivative is 1 mol % to 15 mol % relative to 100 mol % of halogen in the (a) halogenated butyl rubber.
[0088] The medical rubber composition of the present disclosure (2) is the medical rubber composition of the present disclosure (1), wherein the halogenated butyl rubber is at least one selected from the group consisting of chlorinated butyl rubber, brominated butyl rubber, and brominated isobutylene-paramethylstyrene copolymer rubber.
[0089] The medical rubber composition of the present disclosure (3) is the medical rubber composition according to the present disclosure (1) or (2), wherein (b) the polyethylene contains polyethylene having a crystallinity of 70% or less.
[0090] The medical rubber composition of the present disclosure (4) is a medical rubber composition according to any one of the present disclosures (1) to (3), in which (b) the amount of the polyethylene blended is 3 to 30 parts by mass per 100 parts by mass of the (a) base polymer.
[0091] The medical rubber composition of the present disclosure (5) is a medical rubber composition according to any one of the present disclosures (1) to (4), in which (c) the content of the triazine derivative is 0.1 parts by mass or more and 1.4 parts by mass or less per 100 parts by mass of the (a) base polymer component.
[0092] A medical rubber part according to the present disclosure (6) is a medical rubber part obtained by molding the medical rubber composition according to any one of the present disclosures (1) to (5).
[0093] The medical rubber part packaging body of the present disclosure (7) is a medical rubber part packaging body that contains a plurality of the medical rubber parts described in the present disclosure (6) in a packaging body, and is characterized by having been subjected to gamma ray sterilization treatment.
[0094] The packaging of medical rubber parts of the present disclosure (8) is the packaging of medical rubber parts according to the present disclosure (7) that has been subjected to gamma ray sterilization treatment so that the absorbed dose of gamma rays is 15 kGy or more.
[0095] The packaging of medical rubber parts of the present disclosure (9) is the packaging of medical rubber parts according to the present disclosure (7) or (8) that has been subjected to gamma ray sterilization treatment so that the absorbed dose of gamma rays is 25 kGy or more.
[0096] The package for medical rubber parts of the present disclosure (10) is the package for medical rubber parts according to any one of the present disclosures (7) to (9), in which the oxygen concentration of the package before gamma ray sterilization is 5% or less.
[0097] The medical rubber part packaging body of the present disclosure (11) is the medical rubber part packaging body according to any one of the present disclosures (7) to (10), in which the medical rubber part is a rubber stopper for a vial, a cap for a syringe, a plunger stopper, or a rubber stopper for a vacuum blood collection tube.
Claims
1. (a) a base polymer containing a halogenated butyl rubber; (b) As polyethylene, high density polyethylene and low density polyethylene (c) containing a triazine derivative as a crosslinking agent, A medical rubber composition comprising the triazine derivative in an amount of 1 mol % to 15 mol % relative to 100 mol % of halogen in the halogenated butyl rubber (a).
2. 2. The medical rubber composition according to claim 1, wherein the halogenated butyl rubber is at least one selected from the group consisting of chlorinated butyl rubber, brominated butyl rubber, and brominated isobutylene-paramethylstyrene copolymer rubber.
3. 3. The medical rubber composition according to claim 1, wherein the polyethylene (b) has a crystallinity of 70% or less.
4. The medical rubber composition according to any one of claims 1 to 3, wherein the blending amount of (b) said polyethylene is 3 to 30 parts by mass per 100 parts by mass of (a) the base polymer.
5. The medical rubber composition according to any one of claims 1 to 4, wherein the content of the triazine derivative (c) is 0.1 parts by mass or more and 1.4 parts by mass or less per 100 parts by mass of the base polymer component (a).
6. A medical rubber part obtained by molding the medical rubber composition according to any one of claims 1 to 5.
7. 7. A medical rubber part package comprising a plurality of the medical rubber parts according to claim 6 housed in a package, the medical rubber part package being sterilized by gamma radiation.
8. 8. The medical rubber part packaging body according to claim 7, which has been subjected to gamma ray sterilization so that the gamma ray absorbed dose is 15 kGy or more.
9. 9. The medical rubber part packaging body according to claim 7 or 8, which has been subjected to gamma ray sterilization so that the gamma ray absorbed dose is 25 kGy or more.
10. The package for medical rubber parts according to any one of claims 7 to 9, wherein the oxygen concentration of the package before gamma ray sterilization is 5% or less.
11. 11. The package of medical rubber parts according to claim 7, wherein the medical rubber parts are rubber stoppers for vials, caps for syringes, plunger stoppers, or rubber stoppers for vacuum blood collection tubes.