Magnetic wedge, stator for rotating electric machine, and rotating electric machine

JP2023093437A5Inactive Publication Date: 2024-10-23PROTERIAL LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023043086
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-02-18
Filing Date
2023-03-17
Publication Date
2024-10-23
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional magnetic wedges in rotating electrical machines face issues with bending strength, particularly under high temperatures, and are prone to weight loss and strength reduction due to resin-based bonding, which affects their reliability and ability to fit complex shapes.

Method used

A manufacturing method involving Fe-based soft magnetic particles with an oxidizable element like Al, Si, Cr, or Hf, where the particles are mixed with a binder, molded, machined, and heat-treated to form a surface oxide phase, enhancing bonding and strength.

Benefits of technology

The resulting magnetic wedge exhibits high strength stability at elevated temperatures, supports complex shapes, and reduces eddy current loss, improving the efficiency and reliability of rotating electrical machines.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a magnetic wedge having high strength stability against temperature rise and capable of coping with complex shapes, a stator for a rotating electrical machine, a rotating electrical machine, and a manufacturing method of the magnetic wedge.SOLUTION: A manufacturing method of a magnetic wedge includes a first step of mixing a powder of Fe-based soft magnetic particles containing an element M that is more easily oxidized than Fe with a binder to obtain a mixture, a second step of molding the mixture to obtain a molded body, a third step of machining the molded body, and a fourth step of applying heat treatment to the molded body that has undergone the third step to form a surface oxide phase of the Fe-based soft magnetic particles that binds the Fe-based soft magnetic particles between the particles of the Fe-based soft magnetic particles.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a magnetic wedge used in the magnetic circuit of a rotating electric machine, a stator and a rotating electric machine using the magnetic wedge, and a method for manufacturing such a magnetic wedge. [Background technology]

[0002] In a typical radial gap rotating electric machine, the stator and rotor are arranged coaxially, and multiple teeth with coils wound around them are arranged at equal intervals in the circumferential direction around the stator. In addition, magnetic wedges may be placed at the rotor-side tips of the teeth to connect the tips of adjacent teeth. In this case, unlike coil components, the magnetic wedge itself is not wound with a coil.

[0003] By incorporating such magnetic wedges, the magnetic flux reaching the coils from the rotor can be magnetically shielded, thereby suppressing eddy current losses in the coils. Furthermore, the magnetic wedges smooth the magnetic flux distribution within the gap between the stator and rotor (especially the circumferential magnetic flux distribution), resulting in smoother rotor rotation. Thus, the incorporation of magnetic wedges makes it possible to create highly efficient and high-performance rotating electric machines.

[0004] Furthermore, a conventional method for manufacturing magnetic wedges is known, for example, as described in Patent Document 1, which involves preparing a magnetic sheet obtained by impregnating a glass cloth with a mixture of magnetic iron powder and epoxy resin, and a non-magnetic sheet obtained by impregnating a glass cloth with epoxy resin, and then laminating them in a sandwich-like manner so that the ratio of the thickness of the magnetic layer to the non-magnetic layer is 1:20:1, and then heat-molding. The magnetic wedge obtained by this method has a three-point bending strength of 25 kg / mm². 2 It is high, with a permeability of 13 and a volume resistivity of 10. 3 It is known to exhibit good characteristics in Ωcm.

[0005] Furthermore, as a method for manufacturing magnetic wedges with high relative permeability, for example, as described in Patent Document 2, a liquid mixture of Fe-3wt%Si alloy powder and a room-temperature curing silicone resin is filled into desired positions in the slot openings of the stator core, and the resin is allowed to harden. Magnetic wedges obtained by this method are known to have a very high relative permeability, up to about 35. [Prior art documents] [Patent Documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 62-77030 [Patent Document 2] WO2018 / 008738 publication [Overview of the project] [Problems that the invention aims to solve]

[0007] Magnetic wedges placed in rotating electric machines are subjected to bending stress by alternating magnetic fields, so high bending strength is desired. For example, Patent Document 1 specifies a three-point bending strength of 25 kgf / mm². 2 While some magnetic wedges have been disclosed, further increases in strength were desired to meet requirements such as high reliability. Furthermore, the magnetic wedge in Patent Document 2 is simply made by solidifying alloy powder with resin, so there were issues with reliability such as bending strength. In addition, rotating electric machines inevitably have losses, so they generate heat and their temperature rises during use. In contrast, conventional magnetic wedges disclosed in Patent Documents 1 and 2, etc., are solidified with resin, so they suffer from weight loss and strength reduction when exposed to high temperatures.

[0008] Furthermore, due to its function, the magnetic wedge needs to have a shape suitable for mating with the stator. For example, recesses are formed in the teeth of the stator for fitting the magnetic wedge, and both ends of the magnetic wedge that contact the teeth are formed to conform to these recesses, allowing them to be fitted into the recesses. Therefore, in addition to being able to achieve and maintain the high strength described above, the magnetic wedge is also required to be easy to form into complex shapes.

[0009] Therefore, the present invention aims to provide a magnetic wedge with high strength stability against temperature rise and capable of handling complex shapes, a stator for a rotating electric machine, a rotating electric machine, and a method for manufacturing such a magnetic wedge. [Means for solving the problem]

[0010] The present invention provides a method for manufacturing a magnetic wedge, comprising: a first step of mixing powder of Fe-based soft magnetic particles containing an element M that oxidizes more easily than Fe with a binder to obtain a mixture; a second step of molding the mixture to obtain a molded body; a third step of machining the molded body; and a fourth step of heat-treating the molded body obtained in the third step to form a surface oxide phase of the Fe-based soft magnetic particles that binds the Fe-based soft magnetic particles together between the particles.

[0011] Furthermore, in the method for manufacturing the magnetic wedge, it is preferable that the element M is at least one selected from the group consisting of Al, Si, Cr, Zr, and Hf. Furthermore, in the method for manufacturing the magnetic wedge, it is preferable that the Fe-based soft magnetic particles are Fe-Al-Cr alloy particles.

[0012] Furthermore, in the method for manufacturing the magnetic wedge, it is preferable that the molded body is a prismatic shape obtained by stretching a line-symmetric figure drawn on an arbitrary plane in the direction normal to the plane, and that the machining is performed on a pair of faces obtained by stretching a pair of sides in symmetric positions in the line-symmetric figure in the direction normal to the plane. Furthermore, in the method for manufacturing the magnetic wedge, it is preferable to form non-parallel surfaces on the molded body by performing the machining described above, and to further increase the surface roughness. Furthermore, in the second or third step of the method for manufacturing the magnetic wedge, it is preferable to round off at least one pair of opposing sides of either one or both end faces of the molded body.

[0013] The magnetic wedge of the present invention has a plurality of Fe-based soft magnetic particles. The plurality of Fe-based soft magnetic particles contain an element M that is more easily oxidized than Fe, and are bonded with an oxide phase containing the element M, and at least a part of the surface is a machined surface.

[0014] In addition, in the magnetic wedge, the element M is preferably at least one selected from the group consisting of Al, Si, Cr, Zr, and Hf. Further, in the magnetic wedge, the Fe-based soft magnetic particles are preferably Fe-Al-Cr alloy particles.

[0015] Furthermore, the magnetic wedge is prismatic, obtained by extending a line-symmetric figure drawn on an arbitrary plane in the normal direction of the plane, and at least a pair of surfaces obtained by extending at least a pair of sides at contrasting positions in the line-symmetric figure in the normal direction are preferably machined surfaces. In addition, in the magnetic wedge, at least a pair of surfaces obtained by extending at least a pair of sides at symmetric positions in the line-symmetric figure in the normal direction are preferably non-parallel. In addition, in the magnetic wedge, it is preferable that at least a pair of opposing sides on one or both end faces are rounded.

[0016] The stator for a rotating electric machine of the present invention has a plurality of teeth and a plurality of slots formed by the plurality of teeth, and any one of the magnetic wedges is fitted between the tips of adjacent teeth. In addition, in the stator for a rotating electric machine, the magnetic wedge preferably contacts the teeth at at least a part of the machined surface. In addition, the rotating electric machine of the present invention has any one of the above-mentioned stators for a rotating electric machine and a rotor disposed inside the stator for a rotating electric machine.

Advantages of the Invention

[0017] According to the present invention, it is possible to provide a magnetic wedge with high strength stability against temperature rise and capable of handling complex shapes, a stator for a rotating electric machine, a rotating electric machine, and a method for manufacturing such a magnetic wedge. [Brief explanation of the drawing]

[0018] [Figure 1] This is a process flow chart for a method of manufacturing a magnetic wedge, which is a first embodiment of the present invention. [Figure 2] These are examples of molded articles or magnetic wedges that are first and second embodiments of the present invention. [Figure 3] These are modified examples of the cross-sectional shape of the molded body according to the first and second embodiments of the present invention. [Figure 4] This is a perspective view showing modified examples of molded articles according to the first and second embodiments of the present invention. [Figure 5] These are enlarged schematic diagrams of magnetic wedges, which are first and second embodiments of the present invention. [Figure 6] This is a schematic diagram of a rotating electric machine, which is a third embodiment of the present invention. [Figure 7] This is a schematic diagram of a rotating electric machine, which is another example of a third embodiment of the present invention. [Figure 8] This is a schematic diagram of a rotating electric machine, which is yet another example of a third embodiment of the present invention. [Figure 9] This is an SEM image showing the cross-sectional structure of the example. [Figure 10] This graph shows the DC magnetization curves of the examples and comparative examples. [Figure 11] This graph shows the iron loss in the example. [Figure 12] This is a model diagram of the rotating electric machine used for electromagnetic field analysis. [Figure 13] This graph shows the results of the electromagnetic field analysis of a rotating electric machine. [Figure 14] This graph shows the temperature dependence of the three-point bending strength in the examples and comparative examples. [Figure 15] This graph shows the weight loss at 220°C for the examples and comparative examples. [Figure 16]This graph shows the weight loss at 290°C for the examples and comparative examples. [Modes for carrying out the invention]

[0019] The method for manufacturing a magnetic wedge according to the present invention will be described below as the first embodiment, the magnetic wedge as the second embodiment, and the stator for a rotating electric machine and the rotating electric machine using the magnetic wedge as the third embodiment, with reference to the drawings. However, the present invention is not limited to these embodiments. Also, in order to clarify the explanation, the following description and drawings have been simplified as appropriate.

[0020] (First Embodiment) <Method for Manufacturing Magnetic Wedges> A method for manufacturing a magnetic wedge, which is the first embodiment of the present invention, will be explained using the flowchart in Figure 1. This embodiment consists of a first step S11 in which Fe-based soft magnetic particle powder and a binder are mixed to obtain a mixture, a second step S12 in which the obtained mixture is molded to obtain a molded body, a third step S13 in which the molded body is machined, and a fourth step S14 in which the molded body that has gone through the third step S13 is heat-treated to form an oxide phase on the surface of the Fe-based soft magnetic particles.

[0021] In the first step S11, a mixture is obtained by mixing a binder with a powder of Fe-based soft magnetic particles containing element M, which is more easily oxidized than Fe. Fe-based soft magnetic powder is a soft magnetic alloy powder mainly composed of Fe (Fe is the most abundant element by mass ratio compared to other elements). In addition to Fe, Co and Ni may also be included, as long as they do not exceed the Fe content.

[0022] The average particle size (median diameter d50 in the volume integrated distribution) of the Fe-based soft magnetic powder is preferably 1 μm or more and 100 μm or less, and more preferably 5 μm or more and 30 μm or less. By setting the particle size in this way, the average particle size of the Fe-based soft magnetic particles of the magnetic wedge obtained by this embodiment can be controlled to a preferred range.

[0023] Element M, which is more easily oxidized than Fe, refers to an element whose standard Gibbs free energy of formation for its oxide is lower than that of Fe2O3. From among the elements that satisfy this condition, element M can be selected from the group consisting of Al, Si, Cr, Zr, and Hf, one or more types, from the viewpoint of having low excessive reactivity and toxicity and being easy to manufacture magnetic wedges. In particular, Fe-Al-Cr alloy particles are preferred for the Fe-based soft magnetic particles. By including such element M, a good surface oxide phase can be formed on the Fe-based soft magnetic particles later. Specifically, by oxidizing the Fe-based soft magnetic powder after molding, a surface oxide phase with a higher element M content than the interior of the Fe-based soft magnetic particles can be easily formed.

[0024] Fe-based soft magnetic powder can be made from granular powder with good moldability produced by atomization methods (e.g., gas atomization or water atomization). Alternatively, powder produced by grinding can be used as flattened powder to take advantage of its anisotropic shape. Powders containing particles surface-treated by chemical methods or heat treatment may also be used. For purposes such as adjusting relative permeability, non-magnetic powder may be mixed with Fe-based soft magnetic powder containing element M, which is more easily oxidized than Fe.

[0025] In the second step S12, described later, the binder is used to temporarily bond the particles together and impart a certain degree of strength to the molded body. The binder also plays a role in providing appropriate spacing between the particles. The type of binder used can be an organic binder such as polyvinyl alcohol or acrylic resin. The organic binder decomposes due to thermal treatment after molding. It is preferable to add the binder in an amount that is sufficiently distributed throughout the mixture, ensuring sufficient strength of the molded body, and that is sufficiently thermally decomposed in the third step S13 described later. For example, if the second step S12 described later is pressure molding, it is preferable to add 0.5 to 3.0 parts by mass of binder per 100 parts by mass of Fe-based soft magnetic powder in order to withstand the machining performed in the third step S13 described later.

[0026] The mixing method in the first step S11 can be any known mixing method or mixer. The mixing form can be selected according to the molding method applied. The following explanation will mainly use pressure molding with a granulation process as an example.

[0027] To obtain a spherical mixture (granulated powder) with uniform particle size, it is preferable to apply a spray drying method using a spray dryer to a slurry-like mixture containing Fe-based soft magnetic powder, a binder, and a solvent such as water. In addition, a lubricant such as stearic acid or stearate may be added to the mixture to reduce friction between the powder and the mold in the second step S12. In that case, the amount added is preferably 0.1 to 2.0 parts by mass per 100 parts by mass of the mixed powder (granulated powder). Note that the lubricant may not be added to the mixture in the first step S11, but rather applied to the mold in the second step S12. Spray drying yields granulated powder with a sharp particle size distribution and a small average particle size. To obtain an even sharper particle size distribution, the granulated powder may be passed through a sieve, for example, using a vibrating sieve, to obtain granulated powder with a desired secondary particle size before being applied to the second step S12. From the viewpoint of improving powder feeding (powder fluidity) during molding, the average particle size (median diameter d50) of the granulated powder is preferably 40 to 150 μm, and more preferably 60 to 100 μm.

[0028] In the second step S12, the mixture obtained in the first step S11 is molded to obtain a molded body. Various known methods (e.g., sheet molding, pressure molding, extrusion molding, etc.) can be applied as the molding method. For example, when sheet molding is applied, green sheets manufactured to a certain thickness using a molding machine such as a doctor blade are laminated and pressed together to obtain a molded body of a predetermined thickness. When pressure molding is applied, the mixture obtained in the first step is filled into a molding die and pressurized with a press machine to obtain a predetermined shape such as a cylindrical shape or a rectangular parallelepiped shape. In this case, molding may be done at room temperature, or warm molding may be performed by heating to a degree that the binder does not disappear.

[0029] As described above, several molding methods are possible, but pressure molding using a press machine and molding die is preferred. Furthermore, since the dimensions, shape, surface roughness, etc. are adjusted by machining in the third step S13, which will be described later, it is not necessarily required to obtain a near-net-shape or final-shape molded body in the second step S12.

[0030] During pressure molding, the packing density of the resulting molded body can be adjusted to a desired range by adjusting the pressurizing conditions such as press pressure and temperature. In the third step S13 described later, increasing the packing density of the molded body is effective in preventing chipping during machining and improving dimensional accuracy. On the other hand, excessively increasing the packing density is undesirable because it reduces mass productivity. Therefore, the packing density of the molded body used in the third step is preferably 78-90%, more preferably 79-88%, and even more preferably 81-86%.

[0031] Furthermore, by using Fe-Cr-Al based Fe-based soft magnetic powder, which has excellent moldability, it is possible to increase the packing density of the molded body subjected to the third step S13 to 82% or more even at low molding pressures. In the second step S12, the packing density of the molded body can be adjusted to this range by adjusting the molding pressure, etc. The packing density (relative density) of the molded body subjected to the third step S13 is calculated by dividing the density of the molded body by the true density of the Fe-based soft magnetic powder. In this case, the mass of the binder and lubricant contained in the molded body is subtracted from the mass of the molded body based on the amount added. The true density of the Fe-based soft magnetic powder can be the density of an ingot made by melting the same composition.

[0032] In the third step S13, the molded body obtained in the second step S12 is machined to achieve the desired shape, dimensions, and surface roughness. In the third step, machining refers to any of the following processing methods, such as cutting, slicing, and grinding, or a combination of these methods. Grinding can be performed using a rotary grinding wheel, cutting using a cutting tool, and slicing using a cutting blade. Furthermore, this includes not only the surface state as it is after machining, but also surfaces whose properties have been changed by heat treatment, coating treatment, etc., after machining. A surface that has been machined in this way is called a machined surface. More preferably, the machined surface is a surface that has undergone heat treatment to form a surface oxide phase. Since the strength of the magnetic wedge becomes very high after the heat treatment in the fourth step described later, the series of manufacturing processes can be simplified by completing the machining before that.

[0033] Here, as an example of the shape of a molded body, we will describe the rectangular parallelepiped shown in Figure 2. Figure 2 shows a state in which the face with the smallest surface area (end face) of the molded body is placed on the xy plane, and the face with the largest surface area (plane) of the molded body is placed on the yz plane, with the depth direction of the paper being the x direction, the left-right direction of the paper being the y direction, and the up-down direction of the paper being the z direction. In this case, the face parallel to the xz plane is called the side face. Also, the cross-section obtained when the molded body is cut by a plane parallel to the xy plane is simply called the cross-section.

[0034] In other words, the molded body shown in Figure 2 can be described as a shape obtained by stretching a rectangular cross-section on the xy-plane in the z-direction to form a column. More precisely, the molded body can be described as a column obtained by stretching a line-symmetric figure drawn on an arbitrary plane in the direction of the normal to that plane. In this case, the end faces can be described as faces parallel to the figure drawn on the arbitrary plane. Also, the plane and side faces can be described as a pair of faces obtained by stretching a pair of symmetrical edges in a figure drawn on an arbitrary plane in the direction of the normal.

[0035] Figure 3 shows modified cross-sectional shapes of molded bodies. These cross-sections are symmetrical figures. Symmetrical figures include, for example, rectangles, isosceles trapezoids, symmetrical polygons, as well as stepped shapes and figures with a circular arc in part.

[0036] Further explanation is given using Figure 3. (a) is an example with a rectangular cross-section. Reference numeral 301 indicates a pair of opposing sides. (b) to (h) are shapes obtained by machining the sides 301. (b) is a modified example with a T-shaped cross-section, where a pair of parallel sides 302 are present. (c) is a modified example with a trapezoidal cross-section, where a pair of non-parallel sides 303 are present. Furthermore, (d) is a combination of (a) and (c), with a pair of non-parallel sides 304 and a parallel side 305 on both ends. Furthermore, (e) is a modified example with a pair of non-parallel sides 306 and 307 on both ends, where both ends form an acute triangular shape. Furthermore, (f) is a modified example of (e) with parallel sides provided on parts of both sides, with a pair of non-parallel sides 308 and 310 on both sides, and a parallel side 309. Furthermore, (g) is a modified example where both sides are composed of curved surfaces 311. Furthermore, (h) is a modified example in which a pair of parallel sides are provided with recesses, thereby dividing the parallel sides into parallel sides 312 and 313.

[0037] Machining may be performed, for example, on at least one plane on the surface of a prismatic molded body. Alternatively, a pair of sides that are symmetrically positioned when viewed from the axial direction (longitudinal direction) can be formed by machining on a prismatic molded body having a line-symmetrical cross-section. For example, machining may be performed on a pair of opposing planes of a rectangular parallelepiped molded body. Furthermore, a pair of opposing planes of a rectangular parallelepiped molded body may be machined at an angle, i.e., by cutting off the corners (edges) of the rectangular parallelepiped, so that the pair of sides are asymmetrical. By such machining, a magnetic wedge with a trapezoidal cross-section can be easily manufactured. This means that a non-parallel surface with relatively large surface roughness can be used as the fitting surface (contact surface) to the teeth. The machining direction, such as grinding or cutting, is preferably in the longitudinal direction of the prismatic molded body because it is easier to obtain flatness.

[0038] When molding using a mold, the surface roughness of the molded body directly reflects the surface roughness of the mold, resulting in a very smooth surface. However, when fitting a magnetic wedge into the teeth of a stator for a rotating electric machine, a rougher surface is preferable to ensure a strong fixing action. Furthermore, when forming a coating on the surface of the magnetic wedge or later applying an adhesive, a rougher surface can be expected to improve adhesion strength due to the anchoring effect. Therefore, it is preferable that the contact surface during fitting, or the surface when coating or adhesive layers are applied, be a surface that has been roughened (with fine irregularities) by machining, rather than the surface as it is when removed from the mold.

[0039] Machining the molded body allows for the acquisition of a desired shape and a surface roughness greater than that achieved after press molding using a die. While machining can be applied to the entire surface of the molded body, this process is unnecessarily time-consuming and complicated, so it is preferable to machine only the necessary parts. After the heat treatment described in the fourth step, the strength of the molded body becomes very high, making machining difficult; therefore, it is preferable to perform machining before the heat treatment.

[0040] By machining, the average R of the arithmetic mean roughness Ra of the unmachined surface is AS The average R of the arithmetic mean roughness Ra of the machined surface. MD Ratio R MD / R AS This can be reduced to approximately 2-5. This value is the measurement taken after the fourth step S14, which will be described later. The arithmetic mean roughness is 1.0 mm per location, measured using a laser microscope. 2 The above area is evaluated at multiple locations, and the average value is used.

[0041] The planar surface (yz plane) of the molded body shown in Figure 2 is rectangular, but the corners of this rectangle may be rounded. Figure 4 is a perspective view of the molded body with rounded corners. (a) is an example where the cross-section is rectangular (shape of Figure 3(a)), and (b) is an example where the cross-section is a deformed trapezoid (shape of Figure 3(d)). By adopting such a shape, in the third embodiment described later, it becomes easier to insert the magnetic wedge into the tip of the teeth.

[0042] Furthermore, this effect of the radius can be obtained regardless of the composition of the Fe-based soft magnetic particle powder or the binder. That is, the manufacturing method of this embodiment comprises a first step of mixing the soft magnetic particle powder and the binder to obtain a mixture, a second step of molding the mixture to obtain a molded body, a third step of machining the molded body, and a fourth step of heat-treating the molded body that has undergone the third step, wherein the molded body is a prismatic shape obtained by stretching a line-symmetric figure drawn on an arbitrary plane in the direction normal to the plane, and at least a pair of faces obtained by stretching at least a pair of sides in symmetric positions in the line-symmetric figure in the direction normal to the plane are machined faces, and it is preferable to apply a radius to at least one pair of opposing sides of either one or both end faces of the molded body in the second or third step.

[0043] Furthermore, while the effect of this radius is more easily obtained with a larger radius, if the radius is too large, a large gap will be created between the magnetic wedge and the tip of the tooth in this area. This weakens the force that fixes the magnetic wedge, and the distribution of magnetic flux around the gap is disturbed, thus impairing the motor efficiency improvement effect of the magnetic wedge.

[0044] From this viewpoint, the size of the radius is preferably less than 1 / 2 of the width (length in the y-direction) of the magnetic wedge, more preferably 1 / 3 or less, and even more preferably 1 / 4 or less. On the other hand, if the radius is too small, the above-mentioned effects become difficult to obtain, so the size of the radius is preferably 1 / 20 or more of the width (length in the y-direction) of the magnetic wedge, more preferably 1 / 10 or more, and even more preferably 1 / 5 or more. The shape of the radius is not limited to a circular arc, but may also be an elliptical arc or other curve, and it is even better if it is pointed in the longitudinal direction (z-direction). Such a shape makes it easier to insert the magnetic wedge into the tip of the tooth.

[0045] This radius (or any curved portion) may be formed when machining the side surface in the third step S13, or it may be formed in the second step S12 described above by press molding using a die with a radius (or any curved portion) at the corner. From a manufacturing standpoint, if possible, it is preferable to manufacture a molded body with a radius during molding, as this reduces the number of machining steps and is advantageous for improving productivity and reducing costs.

[0046] In the fourth step S14, the molded body obtained through the third step S13 is heat-treated to form a compacted body (magnetic wedge). Figure 5 shows an enlarged schematic diagram of the cross-section of the magnetic wedge. During the heat treatment, the binder present between the Fe soft magnetic particles 1 in the molded body is thermally decomposed and disappears, forming voids 2 between the particles. Further heat treatment oxidizes the Fe-based soft magnetic particles 1, forming a surface oxide phase 3 between the Fe-based soft magnetic particles 1 that binds the Fe-based soft magnetic particles 1 together.

[0047] This oxide phase constitutes the grain boundary phase between Fe-based soft magnetic particles, improving the insulation and corrosion resistance of the Fe-based soft magnetic particles. Furthermore, since this oxide phase is formed after the molded body (bulk body) is constructed, rather than in a powder state, it also contributes to the bonding of Fe-based soft magnetic particles through the oxide phase, resulting in a compacted body (magnetic wedge) with significantly higher strength compared to the molded body state. In the spaces between Fe-based soft magnetic particles 1 that cannot be completely filled with this surface oxide phase, voids 2 are formed.

[0048] For example, when using an Fe-Cr-M' (where M' is at least one of Al and Si) powder as the Fe-based soft magnetic powder, the following configuration is obtained. When M' is Si, i.e., when Al is not actively added, Cr is particularly concentrated in the oxide phase, and an oxide phase is formed on the surface of the Fe-based soft magnetic particles where the ratio of Cr to the sum of Fe, Cr, and M'(Si) is higher than that of the internal alloy phase. On the other hand, when M' contains Al, Al is particularly concentrated in the oxide phase, and an oxide phase is formed on the surface of the Fe-based soft magnetic particles where the ratio of Al to the sum of Fe, Cr, and M' is higher than that of the internal alloy phase.

[0049] The heat treatment can be carried out in an atmosphere where oxygen is present, such as in the air or in a mixture of oxygen and an inert gas. It can also be carried out in an atmosphere where water vapor is present, such as in a mixture of water vapor and an inert gas. Of these, heat treatment in the air is simpler and therefore preferred. While there are no particular limitations on the pressure of the heat treatment atmosphere, atmospheric pressure, which does not require pressure control, is preferred.

[0050] The heat treatment should be performed by heating to a temperature at which a surface oxide phase 3 can be formed between the Fe-based soft magnetic particles, which binds the Fe-based soft magnetic particles 1 together. However, if the heat treatment temperature is too low, the strain applied to the molded body during molding may not be relieved and may remain, and if it is too high, the Fe-based soft magnetic particles may sinter together, lowering the electrical resistance and potentially resulting in a magnetic wedge with high eddy current loss. Therefore, the heat treatment temperature is preferably in the range of 600°C to 900°C, and more preferably in the range of 700°C to 800°C. The holding time is not particularly limited and is set appropriately depending on the size of the magnetic wedge, the amount to be processed, etc. The holding time is preferably, for example, 0.5 to 3 hours.

[0051] In the third step described above, machining is performed, exposing the internal alloy phase of the Fe-based soft magnetic particles on the machined surface. However, the heat treatment in the fourth step covers the exposed alloy phase with an oxide phase, thus ensuring the insulating properties of the machined surface. The heat treatment in the fourth step serves multiple purposes: removing distortion during molding, bonding the Fe-based soft magnetic particles together, and forming an insulating layer on the machined surface. This enables the efficient production of high-strength, highly insulating magnetic wedges.

[0052] Other steps may be added before or after each of the first to fourth steps. Specifically, a step of forming an insulating film may be added before the first step, a preheating step may be provided between the second and third steps, an additional machining step may be provided after the fourth step to deburr, and a step of forming an electrically insulating film may be added after the fourth step, regardless of whether deburring is performed or not. These steps will be described below.

[0053] Prior to the first step, a preliminary step may be added to form an insulating film on the Fe-based soft magnetic powder by heat treatment, sol-gel method, etc. However, in the method for manufacturing magnetic wedges according to this embodiment, since an oxide phase can be formed on the surface of the Fe-based soft magnetic particles by the fourth step, it is more preferable to omit such a preliminary step and simplify the manufacturing process.

[0054] A preheating step may be provided between the second and third steps. For example, when there is concern about damage to the magnetic wedge in the third step, such as when manufacturing magnetic wedges with complex shapes or magnetic wedges with thin parts, it is preferable to increase the strength of the molded body subjected to the third step compared to its as-molded state. Specifically, it is preferable to have a preheating step between the second and third steps in which the molded body is heated to a temperature lower than the heat treatment temperature in the fourth step. The heat treatment in the fourth step forms an oxide phase containing the elements present in the Fe-based soft magnetic particles on the surface of the Fe-based soft magnetic particles, significantly increasing the strength of the resulting magnetic wedge. However, it is also possible to increase the strength of the molded body by heating to a temperature lower than the heat treatment temperature.

[0055] For optimal heating effectiveness, the heating temperature in the preheating step should be set higher than room temperature. However, if the heating temperature is too high, processing in the third step becomes difficult. Therefore, when performing the above preheating, it should be done at a temperature lower than the heat treatment temperature in the fourth step. For example, in the case of the Fe-Cr-M' system (where M' is at least one of Al and Si), the heating temperature is preferably below the temperature at which elements other than Fe, such as Al and Cr, in the Fe-based soft magnetic powder oxidize and concentrate at the grain boundaries, and more preferably below 300°C. A heating temperature of 300°C or lower is also preferable because it can be applied not only to Fe-Cr-M' system Fe-based soft magnetic powder but also to other soft magnetic material powders. Furthermore, to enhance the strength-improving effect of heating, a heating temperature of 100°C or higher is preferable.

[0056] The heating holding time is preferably between 10 minutes and 4 hours, for example. If it is too short, the effect of increasing the strength of the molded article is small, and if it is too long, productivity decreases. More preferably, it is between 30 minutes and 3 hours. The atmosphere during preheating is not limited to an oxidizing atmosphere. Air is preferred as the atmosphere because it simplifies the process. By going through the above preheating step, the bending strength of the molded article to be subjected to the third step can be made to more than 15 MPa.

[0057] An additional machining step may be added after the fourth step to remove burrs. If the magnetic wedge obtained after the fourth step has burrs, dimensional adjustment may be necessary. In such cases, a fifth step can be added to further machine the magnetic wedge obtained after the fourth step to remove the burrs. Furthermore, a sixth step can be added to heat-treat the magnetic wedge obtained after the fifth step, and this heat treatment can form an oxide phase containing elements of Fe-based soft magnetic particles on the additionally machined surface.

[0058] Regardless of whether deburring is performed or not, additional steps can be added after the fourth step to form an electrically insulating coating on the surface of the compacted body obtained in the fourth step, using it as a base. This further increases the electrical resistance and strength of the magnetic wedge, suppresses the shedding of particles from the surface of the compacted body, and provides a highly reliable magnetic wedge. For the coating, an electrically insulating coating made of resin, oxide, etc., is preferred in order to suppress eddy current loss. For example, powder coating with epoxy resin, sealing treatment coating by impregnation with varnish or silicone resin, or sealing treatment coating of inorganic materials by the sol-gel method using metal alkoxides can be employed. Of these, from the viewpoint of avoiding high-temperature degradation of the resin, a sealing treatment coating of inorganic materials by the sol-gel method that does not contain resin is particularly preferred.

[0059] (Second Embodiment) <Magnetic Wedge> The magnetic wedge of this embodiment has a plurality of Fe-based soft magnetic particles, and the plurality of Fe-based soft magnetic particles contain an element M that is more easily oxidized than Fe, and are bound together by an oxide phase containing the element M, and at least a part of the surface is a machined surface. The shape of the magnetic wedge changes depending on the connection method with the teeth, and steps or tapers may be provided on the longitudinal ridges, or notches may be made, and the cross-section may be a polygon such as a trapezoid or an irregular shape.

[0060] In Figure 2, reference numeral 100 was described as a molded body in the first embodiment described above, but in this embodiment, it can be read as a magnetic wedge. The approximate dimensions of the magnetic wedge are, for example, 10 mm to 300 mm in the longitudinal direction (z direction), 2 mm to 20 mm in the width direction (y direction), and 1 to 5 mm in the thickness direction (x direction).

[0061] Figure 5 is an enlarged schematic diagram of the cross-section of the magnetic wedge of this embodiment. The magnetic wedge is composed of a plurality of Fe-based soft magnetic particles, more specifically, a compacted body of a plurality of Fe-based soft magnetic particles 1 containing element M, which is more easily oxidized than Fe. Between the particles of the compacted body, there are voids 2 and a surface oxide phase 3 of the Fe-based soft magnetic particles that binds the Fe-based soft magnetic particles 1 together. This surface oxide phase is an oxide phase containing element M. By including such element M, a good surface oxide phase 3 that firmly binds the Fe-based soft magnetic particles 1 together can be easily formed. Specifically, by oxidizing multiple Fe-based soft magnetic particles 1 after molding, a surface oxide phase 3 with a higher element M content than the interior of the Fe-based soft magnetic particles 1 can be easily formed. In particular, when Al is selected as element M, a particularly good surface oxide phase 3 can be obtained, which is preferable.

[0062] The surface oxide phase 3 is chemically stable and has high electrical resistance, and adheres strongly to the Fe-based soft magnetic particles 1, forming a robust surface oxide phase. The surface of the Fe-based soft magnetic particles is covered by the layered surface oxide phase. In other words, this surface oxide phase isolates the Fe-based soft magnetic particles 1, resulting in a magnetic wedge with high electrical resistance. Furthermore, the surface oxide phase firmly binds the Fe-based soft magnetic particles 1 together, resulting in a magnetic wedge with high bending strength.

[0063] If the amount of element M contained in the Fe-based soft magnetic particle 1 is too small, it becomes difficult to form a good surface oxide phase in which the element M content is higher than that inside the Fe-based soft magnetic particle, even when the Fe-based soft magnetic particle 1 is oxidized. If the amount is too large, the Fe concentration will be diluted, which may lower the saturation magnetic flux density and Curie temperature of the Fe-based soft magnetic particle. Therefore, it is preferable to set the amount of element M contained in the Fe-based soft magnetic particle to 1.0 mass% or more and 20 mass% or less. By doing so, a good surface oxide phase 3 can be easily formed, and the saturation magnetic flux density and Curie temperature of the Fe-based soft magnetic particle 1 can be maintained at a high level. In other words, a magnetic wedge with high electrical resistance, bending strength, and high magnetic shielding can be realized.

[0064] Furthermore, element M may be not limited to just one type, but may be selected from two or more types, for example, including at least Cr as element M, and in combinations such as Al and Cr, or Si and Cr. It is more preferable to select two types, Al and Cr, so that the Fe-based soft magnetic particles are Fe-Al-Cr alloy particles. In this way, even with a relatively small amount of Al, a good surface oxide phase can be formed in which the total content of element M is higher than that inside the Fe-based soft magnetic particles. That is, a magnetic wedge with high bending strength and adjusted relative permeability can be obtained.

[0065] An Fe-Al-Cr alloy is an alloy in which the elements with the second highest content after Fe are Cr and Al (in any order), and other elements may be present in smaller amounts than Fe, Cr, and Al. The composition of an Fe-Al-Cr alloy is not particularly limited, but for example, the Al content is preferably 2.0 mass% or more, more preferably 5.0 mass% or more. From the viewpoint of obtaining a high saturation magnetic flux density, the Al content is preferably 10.0 mass% or less, more preferably 6.0 mass% or less. Also, the Cr content is preferably 1.0 mass% or more, more preferably 2.5 mass% or more. From the viewpoint of obtaining a high saturation magnetic flux density, the Cr content is preferably 9.0 mass% or less, more preferably 4.5 mass% or less.

[0066] Furthermore, if two or more elements are selected for element M, the total content of these elements is preferably 1.0% by mass or more and 20% by mass or less, similar to the case where only one element is selected.

[0067] Fe-based soft magnetic particles may also be particles to which elements other than element M are added. However, it is preferable that these added elements be added in amounts less than element M. Furthermore, Fe-based soft magnetic particles can also be composed of multiple types of Fe-based soft magnetic particles with different compositions.

[0068] The surface oxide phase may contain Fe or other elements in addition to element M, and the elemental concentrations of M, Fe, etc., do not necessarily have to be uniform within the surface oxide phase. In other words, the elemental concentrations may differ at each grain boundary.

[0069] As the thickness of the surface oxide phase increases, the electrical isolation between particles increases, and the resistivity of the magnetic wedge increases. On the other hand, to improve relative permeability and magnetic shielding effect, a thinner surface oxide phase is preferable. From the viewpoint of providing a magnetic wedge with high resistivity and bending strength and controlled relative permeability, the thickness of the surface oxide phase is preferably, for example, 0.01 to 1.0 μm.

[0070] Reducing the particle size of Fe-based soft magnetic particles is advantageous in reducing eddy current losses generated in the magnetic wedge itself. However, if the particle size is small, it may become difficult to manufacture the particles themselves. Therefore, in the cross-sectional observation image of the magnetic wedge, the average of the maximum diameter of each Fe-based soft magnetic particle is preferably 0.5 μm or more and 15 μm or less, and more preferably 0.5 μm or more and 8 μm or less. Furthermore, the ratio of particles with a maximum diameter exceeding 40 μm is preferably less than 1.0%. The average of the maximum diameter of each Fe-based soft magnetic particle referred to here is the average value obtained by polishing the cross-section of the magnetic wedge, observing it under a microscope, and reading the maximum diameters of 30 or more particles present within a certain area of ​​the field of view.

[0071] The presence of voids and surface oxide phases between Fe-based soft magnetic particles widens the average spacing between Fe-based soft magnetic particles, thereby increasing the electrical resistance of the magnetic wedge. In addition, the relative permeability of the magnetic wedge can be adjusted by adjusting the volume ratio of the voids and surface oxide phases relative to the entire magnetic wedge. In other words, since the volume ratio of the voids and surface oxide phases relative to the entire magnetic wedge and the volume ratio of the Fe-based soft magnetic particles (hereinafter referred to as the packing factor) are complementary, the relative permeability of the magnetic wedge can also be adjusted by adjusting the packing factor of the Fe-based soft magnetic particles. The packing factor is defined as the ratio (relative density) of the magnetic wedge density to the true density of the Fe-based soft magnetic particles. The packing factor can be adjusted by the molding pressure of the mixture or the heat treatment temperature of the molded body, as will be described in later embodiments.

[0072] The relative permeability mentioned here is a value μ obtained by dividing the value of the magnetic flux density (unit: T) at an applied magnetic field of 160 kA / m in the DC B-H curve of the magnetic wedge by the value of the magnetic field (i.e., 160 kA / m), and further dividing by the permeability of vacuum (4π×10 -7 H / m). Also, as the relative permeability, the slope of the magnetization curve (so-called minor loop) measured at an excitation level of 1 / 10 or less of the saturation magnetic flux density of the magnetic wedge and at a frequency (including DC) of 1 / 10 or less of the natural resonance frequency of the magnetic wedge is sometimes used as the value μi after dividing by the permeability of vacuum (4π×10 -7 H / m). The natural resonance frequency is the frequency at which the imaginary part of the relative permeability becomes maximum. When multiple maxima appear, the one on the lowest frequency side is adopted.

[0073] The higher the relative permeability of the magnetic wedge, the higher the magnetic shielding effect and the lower the loss. On the other hand, if the relative permeability is too high, the magnetic flux does not flow from the teeth to the rotor but short-circuits between the teeth, and the torque of the rotating electrical machine decreases. Such an effect also depends on the thickness of the magnetic wedge. Even with a magnetic wedge having a high relative permeability, the magnetic resistance can be adjusted by making it thinner, and it is possible to achieve both loss reduction and torque to some extent. Also, if the magnetic wedge is too thick, it will compress the coil installation space, which is not preferable. Since the magnetic wedge of this embodiment has high strength, it is particularly suitable to make it thinner. Therefore, the thickness of the magnetic wedge can be, for example, 3 mm or less.

[0074] In order to maintain the loss reduction effect by magnetic shielding even when the thickness of the magnetic wedge is 3 mm or less, the relative permeability μ of the magnetic wedge is preferably 4 or more (5 or more in terms of μi), and more preferably 7 or more (10 or more in terms of μi). For this purpose, the occupancy rate of Fe-based soft magnetic particles in the magnetic wedge is preferably 50% or more, and more preferably 70% or more.

[0075] On the other hand, if the magnetic wedge is made too thin, the load-bearing capacity may decrease, potentially leading to insufficient strength. From this viewpoint, the thickness of the magnetic wedge is preferably 0.5 mm or more, and more preferably 1 mm or more. Even if the thickness of the magnetic wedge is 1 mm or more, in order to suppress the torque reduction of the rotating electric machine, the relative permeability μ of the magnetic wedge is preferably adjusted to 8.0 or less (μi of 65 or less), and more preferably to 7.5 or less (μi of 50 or less). Furthermore, it is even more preferable that it is adjusted to 7.0 or less (μi of 35 or less). To achieve this, the packing fraction of Fe-based soft magnetic particles in the magnetic wedge is preferably less than 90%, and more preferably 85% or less.

[0076] The magnetic wedge preferably has a high relative permeability to effectively magnetically shield the coil, and preferably has high electrical resistance to suppress eddy current losses due to the alternating magnetic field of the coil and rotor. The volume resistivity of the magnetic wedge is preferably 10 Ω·m or more, more preferably 20 Ω·m or more, and even more preferably 100 Ω·m or more. Furthermore, the volume resistivity of the magnetic wedge is even more preferably 1000 Ω·m or more. The bending strength of the magnetic wedge is also preferably as high as possible, preferably 150 MPa or more in three-point bending strength, and more preferably 200 MPa or more. Furthermore, the three-point bending strength of the magnetic wedge is even more preferably 250 MPa or more.

[0077] The above-described configuration, which includes Fe-based soft magnetic particles and a surface oxide phase, enables the realization of a magnetic wedge with high electrical resistance and bending strength. Furthermore, this configuration, combined with the air gap 2, provides a magnetic wedge with high electrical resistance, bending strength, and a controlled relative permeability.

[0078] For purposes such as adjusting the relative permeability, a compacted body of multiple Fe-based soft magnetic particles containing element M, which is more easily oxidized than Fe, and multiple non-magnetic particles can also be used. In this case as well, the multiple Fe-based soft magnetic particles are bound together by an oxide phase containing element M. "Non-magnetic" here means not ferromagnetic at room temperature. Specifically, it refers to particles that exhibit paramagnetic, diamagnetic, or antiferromagnetic magnetism at room temperature. Furthermore, the non-magnetic particles may be metals or nonmetals such as oxides. The presence of non-magnetic particles between the Fe-based soft magnetic particles widens the average particle spacing of the Fe-based soft magnetic particles, and the relative permeability of the magnetic wedge can be lowered by the demagnetizing effect. In other words, the relative permeability can be adjusted by adjusting the content of non-magnetic particles.

[0079] Conventional magnetic wedges disperse iron powder in epoxy resin and bond the soft magnetic particles together with the epoxy resin. As a result, the resin component decreases with increasing temperature, and in high-temperature environments, the resin may soften, potentially reducing the bonding strength. In other words, when used in high-temperature environments such as rotating electric machines, bending strength may become an issue. In contrast, the magnetic wedge of this embodiment bonds the particles together with a surface oxide phase rather than resin, thus suppressing the decrease in bonding strength between particles at high temperatures and providing a magnetic wedge with high bending strength even at high temperatures. For example, the decrease in three-point bending strength when the temperature is raised from room temperature (25°C) to 150°C can be reduced to less than 5%, more preferably to less than 3%. Furthermore, the decrease in three-point bending strength when the temperature is raised from room temperature (25°C) to 200°C can also be reduced to less than 10%, more preferably to less than 5%.

[0080] As mentioned above, conventional magnetic wedges contain resin as a binder, which leads to the problem that prolonged exposure to high-temperature environments causes the resin to decompose and deteriorate, resulting in irreversible strength reduction and dimensional loss. In contrast, the resin-free magnetic wedge of this embodiment does not suffer from such problems. In this respect as well, a magnetic wedge with excellent heat resistance and long-term reliability can be provided. For example, the mass loss rate after 1000 hours at 180°C can be reduced to less than 0.05%, more preferably less than 0.03%. Furthermore, the mass loss rate after 450 hours at 220°C can be reduced to less than 0.1%, more preferably less than 0.05%. Moreover, the mass loss rate after 240 hours at 290°C can be reduced to less than 1%, more preferably less than 0.5%.

[0081] The heat resistance temperature of rotating electrical machines varies depending on the application and specifications, but some are set at 155°C or 180°C according to standards. In addition, some rotating electrical machines can reach temperatures of up to 200°C. The magnetic wedge of this embodiment can maintain excellent bending strength even at high temperatures, so it can be suitably used in rotating electrical machines where magnetic wedges could not be installed before, such as those with a maximum temperature exceeding 180°C, and even those exceeding 200°C.

[0082] The compacted body constituting the magnetic wedge of this embodiment is resin-free and therefore has high thermal conductivity. By placing this embodiment, which has high thermal conductivity and excellent heat dissipation, as a magnetic wedge near the gap, which is a heat source of the rotating electric machine, heat can be effectively dissipated, and an effect of improving the cooling efficiency of the rotating electric machine can be expected. Such a cooling effect is preferable as the thermal conductivity of the magnetic wedge increases. For example, a thermal conductivity of 2.0 W / (m·K) or higher is preferable, 5.0 W / (m·K) or higher is more preferable, and 8.0 W / (m·K) or higher is even more preferable. Furthermore, since the thermal conductivity of the electromagnetic steel sheet constituting the stator of the rotating electric machine is generally high, around 20 W / (m·K), it can be expected that the closer the thermal conductivity of the magnetic wedge is to this value, the higher the cooling effect will be. Therefore, the thermal conductivity of the magnetic wedge is preferably 1 / 10 or more of that of the magnetic material (electromagnetic steel sheet) constituting the stator, more preferably 1 / 5 or more, and even more preferably 1 / 3 or more.

[0083] The magnetic wedge of this embodiment has at least a portion of its surface that is machined. It should be noted that the term "machined surface" here does not mean a surface that has undergone machining such as cutting, grinding, or slicing, but rather a surface that has undergone machining. In other words, it includes surfaces whose properties have changed after machining, such as through heat treatment or coating.

[0084] The machined surface is more preferably a heat-treated surface that forms a surface oxide phase, as described later. Conventionally, magnetic wedges are formed using molds, so the surface of the magnetic wedge is the surface in contact with the mold. The magnetic wedge of this embodiment can also be manufactured by forming using a mold, but a machined surface is formed on at least a part of the surface by machining (surface processing). The machined surface has a greater surface roughness than the smooth surface in contact with the mold. If a surface with a large surface roughness is used, for example, as a surface in contact with the teeth of a stator for a rotating electric machine, the contact resistance between the surface and the irregularities on the teeth side will increase, and the fixing of the magnetic wedge can be expected to be strengthened. Also, if a surface with a large surface roughness is used as a surface to which a coating or adhesive is applied, the adhesion strength of the coating or adhesive can be expected to be improved due to the anchoring effect. The entire surface may be a machined surface, but since the processing becomes complicated, it is preferable that only a part of the surface is machined as needed.

[0085] The magnetic wedge of this embodiment can be described as having a shape obtained by stretching a rectangular cross-section on the xy-plane in the z-direction to form a columnar shape. More precisely, the molded body can be described as a columnar shape obtained by stretching a line-symmetric figure drawn on an arbitrary plane in the direction normal to that plane. In this case, the end face can be described as a face parallel to the figure drawn on the arbitrary plane. Also, the plane and side face can be described as a pair of faces obtained by stretching a pair of sides in symmetrical positions in a figure drawn on an arbitrary plane in the direction normal to that plane.

[0086] Furthermore, as shown in Figure 4, the corners of the plane may be rounded. This effect of the rounded edges can be obtained regardless of the composition of the Fe-based soft magnetic particle powder or the binder. That is, the magnetic wedge of this embodiment consists of a plurality of soft magnetic particles and is a prismatic shape obtained by stretching a line-symmetric figure drawn on an arbitrary plane in the direction normal to the plane, and at least a pair of faces obtained by stretching at least a pair of sides in symmetrical positions in the line-symmetric figure in the direction normal are machined surfaces, and it is preferable that at least one pair of opposing sides of either one or both end faces are rounded.

[0087] In the first embodiment described above, Figures 3 and 4 were explained as modified examples of the molded body, but in this embodiment, they may be interpreted as modified examples of the magnetic wedge. The embodiments shown in Figures 3 and 4 have already been described in detail, so they will be omitted here.

[0088] If the side surface of the molded body in Figure 2 is a machined surface, then such a surface can be used as the surface that contacts the teeth in the third embodiment described later, that is, the surface on which the magnetic wedge is fitted and fixed between the teeth. Since such a magnetic wedge can be clamped by the teeth from both sides via a pair of side surfaces on which machined surfaces are formed, a stronger fixation is possible. It is preferable that such a pair of side surfaces are non-parallel. This is because it enables a stronger fixation when the magnetic wedge is fitted into the teeth, and also has the effect of improving manufacturability.

[0089] The magnetic wedge of this embodiment may also be provided with an electrically insulating coating on its surface, using the above-mentioned compacted body as a base. By doing so, the electrical resistance and strength of the magnetic wedge can be further increased, and the shedding of particles from the surface of the compacted body can be suppressed, thereby providing a highly reliable magnetic wedge. For the coating, an electrically insulating coating made of resin, oxide, etc. is preferred in order to suppress eddy current loss. For example, powder coating with epoxy resin, sealing treatment coating by impregnation with varnish or silicone resin, or sealing treatment coating of inorganic materials by the sol-gel method using metal alkoxides can be employed. Of these, from the viewpoint of avoiding high-temperature degradation of the resin, sealing treatment coating of inorganic materials by the sol-gel method is particularly preferred.

[0090] (Third Embodiment) <Stator for Rotating Electric Machine and Rotating Electric Machine> Next, a rotating electric machine 300, which is a third embodiment of the present invention, will be described together with a stator for the rotating electric machine, which is one of its components. Figure 5 is a schematic diagram of the rotating electric machine 300, showing the cross-sectional structure perpendicular to the rotation axis of the rotating electric machine 300. The rotating electric machine 300 is a radial gap type rotating electric machine and has a stator 31 and a rotor 32 located inside the stator 31, which are arranged coaxially. The stator 31 has a plurality of teeth 34 and a plurality of slots formed by the plurality of teeth 34, and the plurality of teeth 34 around which the coil 33 is wound are arranged at equal intervals in the circumferential direction.

[0091] In the rotating electric machine of this embodiment, the magnetic wedge 100 of the second embodiment is fitted to the rotor 32 side of the slot, that is, to the rotor 32 side tip of the tooth 34, so as to connect the tips of adjacent teeth 34.

[0092] Here, the relative permeability and saturation magnetic flux density of the teeth 34 are typically designed to be higher than those of the magnetic wedge 100. This allows the magnetic flux from the rotor 32 that reaches the magnetic wedge 100 to flow into the teeth 34 via the magnetic wedge 100, suppressing the magnetic flux reaching the coil and reducing eddy current losses in the coil.

[0093] Furthermore, when a rotating electric machine is driven, most of the magnetic flux in the teeth 34 generated by the coil current flows into the rotor 32 across the gap, but some is attracted to the magnetic wedge 100 and spreads out in the circumferential direction. As a result, the magnetic flux distribution in the gap between the stator 31 and the rotor 32 becomes smoother, and in a rotating electric machine where permanent magnets are arranged on the rotor 32, for example, cogging can be suppressed and eddy current losses generated in the rotor 32 can be reduced. Also, in an induction type rotating electric machine where a squirrel-cage conductor is arranged on the rotor 32, for example, secondary copper losses can be reduced. As described above, by arranging the magnetic wedge 100 in a rotating electric machine, losses can be reduced and a highly efficient and high-performance rotating electric machine can be made.

[0094] The cross-sectional shape of the magnetic wedge 100 is not limited to a rectangle; as described above, it can have various shapes. For example, as shown in Figure 7, if the tip of the teeth 34 has a projection in the circumferential direction, the cross-sectional shape of the magnetic wedge 100 can be convex, and it can be arranged as shown in the figure. Furthermore, it is possible to change the thickness of the magnetic wedge 100 (the radial dimension of the rotating electric machine) in the width direction of the magnetic wedge. For example, as shown in Figure 8, a shape in which the area near the center in the width direction is relatively thinner is preferable because it is possible to suppress excessive short circuits of magnetic flux between the teeth 34 in the thin-walled area near the center of the magnetic wedge, while effectively smoothing the spatial distribution of magnetic flux in the thicker areas at both ends. This makes it possible to achieve a high level of both torque and efficiency. In addition to the linear shape shown in Figure 8, various other variations of the thickness of the magnetic wedge 100 can be applied, such as curvilinear or stepped changes.

[0095] When the magnetic wedge 100 is positioned to connect the tips of adjacent teeth 34, it is preferable that the magnetic wedge 100 is in contact with the teeth 34 at least a portion of the machined surface described above. That is, it is preferable to position the machined surface at the portion where the magnetic wedge 100 and the teeth 34 are in contact. At least a portion of the machined surface of the magnetic wedge 100 and the teeth 34 may be in direct contact, or they may be in contact via an adhesive layer or the like. As described above, this configuration can be expected to strengthen the fixing of the magnetic wedge 100.

[0096] Furthermore, a magnetic wedge 100, which is columnar in shape with a line-symmetrical cross-section and has a pair of machined surfaces located symmetrically in the axial direction, can be used with these surfaces in contact with the teeth 34, i.e., the surfaces to which the magnetic wedge 100 is fitted and fixed between the teeth 34. For example, the sides of the teeth 34, which are constructed by laminating plate-shaped magnetic materials such as electromagnetic steel sheets and amorphous alloy strips, i.e., the slot-side surfaces, have large irregularities. Therefore, by adopting an arrangement in which these surfaces are in contact with the machined surfaces of the magnetic wedge 100, a stator 31 for a rotating electric machine and a rotating electric machine in which the magnetic wedge is more firmly fixed can be expected.

[0097] As mentioned above, the thickness of the magnetic wedge 100 can be appropriately set in consideration of the relative permeability, but if it is too thin, the strength will decrease and the effect of the magnetic wedge 100 will also weaken, so a thickness of 1 mm or more is preferable. On the other hand, if it is too thick, it will compress the space of the coil 33 and contribute to increased copper loss, and the volume of the magnetic wedge 100 will increase, so the loss (iron loss) that occurs in the magnetic wedge 100 itself will also increase. Therefore, a thickness of 5 mm or less is preferable, 3 mm or less is more preferable, and 2 mm or less is even more preferable.

[0098] The width of the magnetic wedge 100 (the circumferential dimension of the rotating electric machine) is set appropriately to match the spacing between adjacent teeth 34, but is preferably in the range of 2 mm to 20 mm.

[0099] The length of the magnetic wedge 100 (the axial dimension of the rotating electric machine) is basically set appropriately to match the thickness (axial length) of the stator 31. However, if it is too long, it becomes difficult to manufacture and is prone to breaking when attached to the rotating electric machine, resulting in poor workability. Therefore, the length is preferably 300 mm or less, more preferably 200 mm or less, and even more preferably 100 mm or less. On the other hand, if it is too short, it is undesirable as it complicates the work when attaching it to the rotating electric machine. From this viewpoint, the length is preferably 10 mm or more, more preferably 25 mm or more, and even more preferably 50 mm or more. [Examples]

[0100] An example using an Fe-Al-Cr alloy as the Fe-based soft magnetic particles is shown below.

[0101] (Preparation of compacted bodies) Fe-5%Al-4%Cr (mass%) alloy powder (Fe-based soft magnetic powder) was prepared by high-pressure water atomization. The raw materials were dissolved and the molten metal was extracted under an Ar atmosphere. The average particle size (median diameter) of the prepared powder was 12 μm, and the specific surface area of ​​the powder was 0.4 m². 2 The true density of the powder is 7.3 g / cm³. 3 The oxygen content of the powder was 0.3%. A slurry was prepared by adding polyvinyl alcohol (PVA) and deionized water to this alloy powder, and granulated powder was obtained by spray drying with a spray dryer. The amount of PVA added was 0.75 parts by mass when the raw material powder was 100 parts by mass. Zinc stearate was added to the obtained granulated powder at a ratio of 0.4 parts by mass and mixed. The resulting mixture was filled into a mold and press-molded at room temperature under a molding pressure of 0.9 GPa. The molded body was subjected to heat treatment at 750°C for 1 hour in air. The heating rate during this treatment was 250°C / h. The oxygen content in the compacted body after heat treatment was 2%.

[0102] The dimensions of the sample prepared for characterization are as follows: Sample for evaluating bending strength and heat loss: Width 2.0 mm x Length 25.5 mm x Thickness 1.0 mm Sample for DC magnetization curve evaluation: 10mm square x 1.0mm thick Sample for evaluating magnetic core loss and electrical resistance: Outer diameter 13.4 mm x Inner diameter 7.7 mm x Thickness 2.0 mm (ring shape)

[0103] (Cross-sectional structure of the example) The examples prepared as described above were observed in cross-section using a scanning electron microscope (SEM / EDX), and the distribution of each constituent element was simultaneously investigated. The results are shown in Figure 9. Figure 9(a) is an SEM image, and Figures 9(b) to (e) are mapping images showing the distribution of Fe (iron), Al (aluminum), Cr (chromium), and O (oxygen), respectively. Brighter colors indicate a higher concentration of the target element. From Figure 9, it can be seen that there is a high concentration of aluminum and oxygen at the grain boundaries between Fe-based soft magnetic particles, and that an oxide phase is formed. Furthermore, it can be seen that the soft magnetic particles are bonded to each other via this oxide phase.

[0104] (Comparative example) As a comparative example, a commercially available magnetic wedge material, a magnetic laminate, was used. This magnetic wedge consists of iron powder dispersed in a glass epoxy substrate, and was cut from a 3.2 mm thick plate to the size required for various measurements.

[0105] (Density / Electrical Resistance) The density of the sample in the above example is 6.4 g / cm³. 3 The packing fraction (relative density), which is the value obtained by dividing the density of the sample by the true powder density mentioned above, was 88%. On the other hand, the density of the comparative example was 3.7 g / cm³. 3 That was the case. Furthermore, the electrical resistivity of the example measured using the ring-shaped sample described above was 3 × 10⁻⁶ 4 The value was Ω·m. The electrical resistivity was calculated using the following formula, with the resistance value R(Ω) measured with an Advantest R8340 digital ultra-high resistance meter, after forming electrodes by applying conductive adhesive to two opposing planes of the ring sample. ρ(Ω·m) = R × A / t Here, A is the area of ​​the plane of the ring sample (m²). 2 ), where t is the thickness of the sample (m). On the other hand, the electrical resistance of the comparative example was too low to be measured with the above-mentioned ultra-high electrical resistance meter, so it was measured using a HIOKI RM3545 resistance meter. The sample used for measurement was a 10 mm square plate with electrodes formed on both sides. The electrical resistance value in the thickness direction of the plate was measured by pressing the probe of the resistance meter against the electrodes, and the electrical resistivity of the comparative example was calculated from the above formula, yielding 9 × 10⁻⁶. -3 It was Ω·m.

[0106] (DC magnetization curve) The DC magnetization curve (BH curve) of the sample was measured using a DC recording magnetometer (TRF-5AH, manufactured by Toei Kogyo) with the 10 mm square sample sandwiched between the magnetic poles of an electromagnet, at a maximum applied magnetic field of 500 kA / m. The measurement results at room temperature are shown in Figure 10. The BH curve for the comparative example is also shown in the same figure. The magnetic flux density values ​​at an applied magnetic field of 160 kA / m were 1.60 T for the example and 0.76 T for the comparative example. Therefore, the relative permeability μ was 8.0 for the example and 3.8 for the comparative example. Furthermore, the relative permeability μi of the sample, determined from the AC magnetization curve (minor loop) measured at f=1kHz and Bm=0.07T, was 59. The natural resonance frequency of the example was 150MHz. An attempt was made to measure the core loss of the comparative example using a similar method, but the permeability was too low to measure effectively.

[0107] (Magnetic core loss) Primary and secondary windings were applied to the ring sample of the above embodiment using polyurethane-coated copper wire. The number of turns was set to 50 for both the primary and secondary windings. This sample was connected to a BH loop analyzer (IF-BH550, IFG Corporation) equipped with a high-current bipolar power supply (BP4660, NF Circuit Design Block Co., Ltd.) to measure the iron loss Pcv. The measurement conditions were a frequency f = 50 Hz to 1 kHz and a maximum magnetic flux density Bm = 0.05 to 1.55 T. In order to prevent the sample temperature from rising due to Joule heating of the primary winding, the sample was immersed in a cooling tank (Julabo high / low temperature circulator FP50-HE) with the refrigerant temperature maintained at 23°C to measure the iron loss. Silicone oil (KF96-20cs, Shin-Etsu Chemical Co., Ltd.) was used as the refrigerant.

[0108] The measurement results are shown in Figure 11. The white circles in the figure represent the measured values. As shown in the figure, in the region of high Bm, Pcv tends to gradually saturate as it approaches magnetic saturation. In the motor characteristic simulation in the next section, these measured values ​​were used as the iron loss for the example. Although the measurement could only be performed up to Bm = 1.55T, the magnetic wedge inside the motor may be magnetized to about 2T, which corresponds to the saturation magnetic flux density of the electromagnetic steel sheet. Therefore, for Pcv values ​​on the high Bm side exceeding 1.55T, the measurement results were applied to the following equation using the least squares method, and the extrapolated value of this equation was used. Example: Pcv = 6.9f / (1 + (1.28 / Bm) 2 ) Here, the unit Pcv is kW / m 3 The unit of Bm is T, and the unit of f is Hz. The solid line in Figure 11 represents the calculated value using this formula. The iron loss of the comparative example was also measured using the same method as described above. The sample used for measurement was a ring shape with an outer diameter of 20 mm, an inner diameter of 14 mm, and a thickness of 3.2 mm, and both the primary and secondary windings were wound with 85 turns. Because the permeability of the comparative example was lower than that of the example, the maximum magnetic flux density Bm that could be measured was 0.6 T, but the measured value was approximately twice that of the example's Pcv. In the motor characteristic simulation in the next section, this measured value was used as the iron loss of the comparative example. For the Pcv value when Bm > 0.6 T, the measurement results were applied to the following formula, as in the example, and the extrapolated value of this formula was used. Comparison example: Pcv=6.7f / (1+(1.1 / Bm) 1.58 )

[0109] (Evaluation of the processed surface of the compacted material) A molded body, similar to the molded body in the example, was manufactured by press molding and then ground using a rotary grinding wheel. The processed molded body was then heat-treated at 750°C for 1 hour in air to obtain a compacted body. The surface roughness of the processed surface (the surface that underwent the grinding process) and the unprocessed surface (the forming punch surface) of the obtained compacted body was measured using an OLYMPUS OLS5100 laser microscope. Measurements were taken at 5 locations on both the processed and unprocessed surfaces. The evaluation area per location was 1.12 mm². 2The arithmetic mean roughness Ra of the unprocessed surface (forming punch surface) was in the range of 2.00 to 3.06 μm, and its average R AS The surface roughness was 2.37 μm. In contrast, the arithmetic mean roughness Ra of the machined surface ranged from 4.92 to 11.13 μm, with an average R MD It was 7.93 μm. From this result, R MD and R AS Ratio R MD / R AS The coefficient was approximately 3.3, and it was confirmed that a relatively rough surface could be formed by machining.

[0110] (Simulation of rotating electric machine characteristics) The characteristics (efficiency and torque) of an induction-type rotating electric machine with a magnetic wedge from an example or comparative example were calculated using electromagnetic field simulation with the finite element method. In this calculation, the magnetization curve shown in Figure 11 and the aforementioned iron loss value were incorporated as the magnetic properties of the magnetic wedge. The specifications of the induction-type rotating electric machine used in the electromagnetic field simulation are as follows: Stator: Diameter 450mm x Height 162mm Number of poles: 4 Number of slots: 36 Rotor and stator material: Electromagnetic steel sheet (50A1000) Rotating electric motor output: 150kW, rotational speed: 1425rpm Figure 12 shows the placement of the magnetic wedge 100 used in this simulation. The width of the magnetic wedge (circumferential length of the rotating electric machine) was 7.0 mm, and the thickness (radial length of the rotating electric machine) was varied to 0.0 mm (without magnetic wedge), 1.5 mm, and 3.0 mm for the calculations.

[0111] (Simulation results of rotating electric machine characteristics) Figure 13 shows the electromagnetic field simulation results. This figure plots the calculation results with the efficiency of the rotating electric machine on the horizontal axis and the torque of the rotating electric machine on the vertical axis. The torque on the vertical axis is a value normalized to the torque value without a magnetic wedge. When comparing the 3mm thick example with the comparative example, the example obtained high efficiency, but the torque was lower than that of the comparative example. This is thought to be because the example, with its high relative permeability, experienced more magnetic flux short circuits between the teeth than the comparative example. Therefore, when the thickness of the example was reduced to 1.5mm with the aim of suppressing magnetic flux short circuits, efficiency and torque equivalent to that of the comparative example were obtained.

[0112] As described above, by using a magnetic wedge with high magnetic permeability and adjusting the thickness of the magnetic wedge to be thin, it is possible to improve efficiency while suppressing torque reduction. Moreover, although not included in this electromagnetic field simulation, since a thinner magnetic wedge increases the space for the coil, it is possible to lower the electrical resistance of the coil by increasing the coil wire diameter, and further improvements in efficiency can be expected.

[0113] (Temperature dependence of bending strength) Using the aforementioned rod-shaped samples, the three-point bending strength was measured from room temperature to 200°C using a universal testing machine (Instron Model 5969). The measurement conditions were: load cell capacity 500N, support diameter 4mm, indenter diameter 10mm, support distance 16mm, and test speed 0.5mm / min. The three-point bending strength σ was calculated from the load W(N) at fracture using the following formula. σ = 3LW / (2bh) 2 ) Here, L is the distance between the support points, b is the width of the sample, and h is the thickness of the sample.

[0114] Figure 14 shows the three-point bending strength of the embodiment obtained as described above. The figure also shows the three-point bending strength of the comparative example. As shown in the figure, the three-point bending strength of the comparative example containing resin decreases significantly with increasing temperature, whereas the resin-free embodiment of this embodiment does not experience any decrease in strength even at a high temperature of 200°C, maintaining high strength equivalent to that at room temperature.

[0115] (Heating loss) When a motor is in operation, its internal temperature rises, so magnetic wedges are required to have durability that prevents performance degradation even when exposed to high-temperature environments for extended periods. To evaluate this durability, the mass change due to aging (heating loss) was measured using the aforementioned rod-shaped samples. Aging was performed in air at 220°C and 290°C, and the samples were removed and cooled at regular intervals, and the mass was measured at room temperature. The reasons for setting the heating temperatures to 220°C and 290°C are as follows: 220°C is the highest temperature that the motor's internal temperature can reach, and 290°C is used to perform an accelerated test of heating loss. An electronic balance with a minimum display of 0.01 mg (Shimadzu AUW220D) was used for mass measurement. Since the rod-shaped samples in the examples had a small mass of about 0.3 g, five samples were used to ensure the reliability of the measurement.

[0116] The measurement results at 220°C are shown in Figure 15, and the measurement results at 290°C are shown in Figure 16. In both figures, the data for the example are the average values ​​of five samples. The figures also show the measurement results for the comparative example. At 220°C, the mass of the comparative example decreased by 0.56% after 456 hours, while the mass change of the example remained below 0.05%. At 290°C, the difference in mass change became more pronounced, with the mass decrease of the comparative example exceeding 10% after 240 hours, while the mass change of the example remained below 0.05%. Furthermore, when the three-point bending strength was measured after the 290°C aging process described above, no change in bending strength was observed in the example compared to before aging, whereas the comparative example's strength had decreased to the point where it broke just by being held in the hand. As described above, this embodiment exhibits superior durability against high-temperature and long-term aging compared to the comparative example, and can be said to be a more practical material for use as a magnetic wedge.

[0117] (Thermal diffusivity) The thermal diffusivity of the example and comparative example at room temperature was measured using a thermal diffusivity measuring device (Netzsch LFA467). The example showed a thermal diffusivity of 3.4 mm. 2 / s, comparative example is 0.8mm 2The value was / s. Furthermore, when the specific heat at room temperature of the example and comparative example was measured using a differential scanning calorimeter (Netzsch DSC404F1), the example was 0.4 J / (g·K) and the comparative example was 0.5 J / (g·K). When the thermal conductivity was determined by multiplying the thermal diffusivity, specific heat, and the density mentioned above, the example was 8.7 W / (m·K) and the comparative example was 1.5 W / (m·K), showing that the example had a thermal conductivity approximately six times higher than the comparative example. Generally, the thermal conductivity of resins is low, less than 1 / 10 of that of metals, so the high thermal conductivity of this example is thought to be due to its resin-free characteristic. By placing this example, which has high thermal conductivity and excellent heat dissipation, as a magnetic wedge near the gap, which is a heat source, heat can be effectively dissipated, and it is expected to have the effect of improving the cooling efficiency of rotating electric machines.

[0118] As described above, according to the present invention, the particles constituting the magnetic wedge are bound together by a surface oxide phase, thus providing a magnetic wedge with high electrical resistance and bending strength. Furthermore, since the magnetic wedge of the present invention is made without resin, it can be made into a magnetic wedge with excellent heat resistance, heat dissipation, and long-term reliability.

[0119] Although the present invention has been described above using the above embodiments, the technical scope of the present invention is not limited to the above embodiments. The content can be modified within the technical scope described in the claims. [Explanation of Symbols]

[0120] 1:Fe-based soft magnetic particles 2:Void 3: Surface oxide phase 31: Status 32: Rotor 33: Coil 34: Teeth 100: Molded object (magnetic wedge) 301~313: Side view 304, 306, 307, 308, 310: Non-parallel sides 305, 309, 312, 313: Parallel sides 311: Curved surface

Claims

1. A prism shape obtained by stretching a line-symmetric figure drawn on an arbitrary plane in the normal direction of the plane, At least a pair of surfaces obtained by extending at least a pair of sides located symmetrically in the line-symmetric figure in the normal direction are machined surfaces, A magnetic wedge in which at least one pair of opposing sides of one or both end faces of the prismatic shape are rounded.

2. A magnetic wedge as described in claim 1, wherein at least a pair of faces obtained by extending at least a pair of edges located symmetrically in the line-symmetric figure in the normal direction are non-parallel.

3. A rotor having a plurality of teeth and a plurality of slots formed by the plurality of teeth, 3. A stator for a rotating electric machine, comprising the magnetic wedge according to claim 1 or 2 fitted between tips of adjacent teeth.

4. A stator for a rotating electric machine as described in Claim 3, wherein the magnetic wedge is in contact with the tooth on at least a portion of the machined surface.

5. A rotating electric machine having a stator for a rotating electric machine as described in claim 3 or 4, and a rotor arranged inside the stator for the rotating electric machine.