Coated grain-oriented electrical steel sheet and its manufacturing method
Patent Information
- Application Number
- JP2022576881
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-06-17
- Filing Date
- 2021-06-15
- Publication Date
- 2024-12-09
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing grain-oriented electrical steel sheets with inorganic coatings face issues such as brittleness, flaking, and environmental hazards due to chromium compounds, while organic coatings are decomposed during high-temperature recrystallization annealing, necessitating a solution that maintains organic coatings post-manufacturing.
Applying a coating comprising an organic radiation-curable crosslinker and photoinitiator after recrystallization annealing, followed by irradiation for rapid hardening, to create a grain-oriented electrical steel sheet with an organic coating that remains intact and provides corrosion resistance.
The method ensures that the organic coating adheres and protects the steel sheet during processing, offering superior corrosion resistance and moisture resistance, while avoiding environmental hazards associated with chromium compounds.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Technical Field
[0001] Claim of Priority This application claims priority to U.S. Patent Application No. 16 / 903,675, filed on June 17, 2020, the content of which is hereby incorporated by reference in its entirety.
[0002] The present disclosure generally relates to a grain-oriented electromagnetic steel sheet having a coating and a method for manufacturing the same, and more particularly to a grain-oriented electromagnetic steel sheet having a coating containing an organic component and a method for manufacturing the same.
Background Art
[0003] Electromagnetic steel sheets have certain desirable magnetic properties such as low magnetic hysteresis, high magnetic flux density, excellent iron loss, and high magnetic permeability. Electromagnetic steel sheets are typically used in motors, transformers, and other electrical components, and the desirable magnetic properties result in lower energy losses during use. Electromagnetic steel sheets are typically supplied as thin or thick plates, and some of these thick plates are laminated together to form a desired structure. Each thick plate typically has an insulating coating that provides insulating properties, and the coating exhibits good coating properties such as adhesion, strength, and protection from corrosion. Grain-oriented electromagnetic steel sheets are manufactured with anisotropic properties, so that grain-oriented electromagnetic steel sheets have different properties in one direction compared to another direction. Thus, magnetic permeability, magnetic flux density, and other properties can be maximized in a desired direction, which is particularly beneficial for transformers where the orientation of the steel sheets remains constant within the transformer. Grain-oriented electromagnetic steel sheets have an oriented crystal with suitable magnetic properties in the rolling direction. However, the crystals are oriented in a recrystallization annealing process at a temperature high enough to decompose organic components. Thus, the insulating coating of grain-oriented electromagnetic steel sheets is inorganic and many contain chromium compounds such as chromic anhydride, chromate, or dichromate. Chromium compounds provide desirable moisture absorption resistance to the insulator coating but produce a treatment solution containing hexavalent chromium, which has harmful environmental effects. Inorganic coatings are brittle and have limited flexibility and tend to flake off in thin sheets, particularly during cutting, punching, and stamping operations, forming dust. Therefore, it is desirable to provide grain-oriented electrical steel sheets having an insulating coating containing organic matter, and a method for manufacturing the same. In addition, it is desirable to provide a method for manufacturing such steel, which provides grain-oriented electrical steel sheets and an insulating coating that retains its adhesive and protective properties after cutting, drilling, or punching operations, and in which the coating provides good protection from corrosion and moisture. Furthermore, other desirable features and properties of this embodiment will become apparent from the embodiments for carrying out the invention and the appended claims, in conjunction with the accompanying drawings and the background art. [Overview of the project]
[0004] A coated grain-oriented electrical steel sheet and a method for manufacturing the same are provided. In an exemplary embodiment, the method includes producing molten steel having about 2.5 to about 4 mass% silicon, about 0.005 to about 0.1 mass% carbon, and about 90 to about 97.5 mass% iron. The molten steel is cast into slabs and then cold-rolled into plates having a surface. The plates are decarbonized using decarbonization annealing and then recrystallized using recrystallization annealing to produce grain-oriented electrical steel sheets. The coating is applied to the surface and includes an organic photoinitiator and a radiation-curable crosslinking agent. The coating is cured by exposing it to a radiation source. Another method for manufacturing grain-oriented electrical steel sheets is also provided. The method involves manufacturing a thick sheet of electrical steel and then recrystallizing the sheet by recrystallization annealing to produce a grain-oriented electrical steel sheet. The sheet is recrystallized on a production line that includes transfer rollers. A coating containing organic components is applied to the surface of the sheet while it is on the production line. The coating is cured on the surface of the sheet by exposing the coating to a radiation source, and the sheet is cured while it is on the production line. Grain-oriented electrical steel sheets are also provided in other embodiments. The steel sheet has a surface having a forsterite layer on its surface. The coating covers the surface and contains about 10 to about 99% by mass of organic components. The organic components include polymers formed from radiation-curable crosslinking agents. The steel contains about 0.01 to about 0.03% by mass of carbon and about 2.5 to about 4.0% by mass of silicon. The thick plate is a grain-oriented electrical steel sheet having anisotropic magnetic properties, wherein the permeability of the thick plate in the rolling direction is greater than the permeability of the thick plate in the width direction perpendicular to the rolling direction. This embodiment will be described hereafter in conjunction with the following drawings. In the drawings, similar numbers represent similar elements. [Brief explanation of the drawing]
[0005] [Figure 1] This flowchart shows the steps of a method for manufacturing a coated grain-oriented electrical steel sheet according to an exemplary embodiment. [Figure 2] This is a perspective cross-sectional view of a grain-oriented electrical steel sheet according to an exemplary embodiment. [Figure 3] This is a schematic diagram showing a portion of a production line for coated grain-oriented electrical steel sheets according to an exemplary embodiment. [Modes for carrying out the invention]
[0006] The following detailed description is illustrative and not intended to limit the application or use of the described embodiments. Furthermore, it is not intended to be bound by any of the theories presented in the aforementioned technical field, background art, summary of the invention, or the detailed description below. Grain-oriented electrical steel sheets require high-temperature recrystallization annealing to grow crystals with the desired orientation, and this high-temperature annealing decomposes any organic components that may be present in the coating. However, it is desirable to coat grain-oriented electrical steel sheets with organic materials because organic coatings offer superior corrosion resistance, moisture resistance, and processing capabilities (e.g., remaining intact and adhered to the plate during cutting, punching, or drilling steps) compared to coatings without organic components. Introducing long heat-setting treatments into the grain-oriented electrical steel sheet manufacturing process is undesirable. To overcome these limitations, an exemplary embodiment provides a method for manufacturing grain-grain electrical steel sheets, wherein a coating containing organic components is applied after recrystallization annealing, and the coating contains an organic radiation-curable crosslinking agent and a photoinitiator. In this case, the grain-grain electrical steel sheet manufacturing process is modified so that the coating is applied to the surface of the steel and then irradiated for rapid hardening. This procedure produces grain-grain electrical steel sheets having a coating containing organic components.
[0007] Referring to Figure 1, a method for manufacturing grain-oriented electrical steel sheets may include several steps, such as: a step 10 for producing molten steel; a step 20 for casting molten steel into a slab; a step 30 for hot rolling the slab to a desired thickness; optionally, a step 40 for winding the hot-rolled slab; optionally, a step 50 for unwinding the hot-rolled slab; a step 60 for cold rolling the slab to form a plate of a desired thickness; a step 70 for removing carbon from the plate by decarbonization annealing; a step 80 for forming grain-oriented electrical steel sheets by recrystallization annealing to orient the crystal grains in the decarbonized plate; a step 90 for coating the grain-oriented electrical steel sheets; and a step 100 for irradiating the coating for hardening.
[0008] In an exemplary embodiment, the method begins with the production of molten steel having a desired composition 10. In the exemplary embodiment, the molten steel contains silicon in an amount of about 2.5 to about 4.0 mass% based on the total mass of the molten steel. The molten steel further contains carbon in an amount of about 0.005 to about 0.1 mass% based on the total mass of the molten steel. The molten steel may optionally contain several elements: aluminum in amounts of about 250 to about 450 parts per million (ppm) (i.e., about 0.025 to about 0.045 mass%) based on the total mass of the molten steel; copper in amounts of about 300 to about 500 ppm; tin in amounts of about 500 to about 1,500 ppm; nitrogen in amounts of 0 to about 150 ppm; manganese in amounts of 0 to about 1,500 ppm; sulfur in amounts of 0 to about 600 ppm; phosphorus in amounts of 0 to about 1,000 ppm; and other impurities in amounts of 0 to about 2,000 ppm. The molten steel also contains iron in amounts of about 90 to about 97.5 mass%, based on the total mass of the molten steel. The molten steel is cast into slabs for further processing 20. In some embodiments, the slabs undergo an intermediate heating process at a temperature of about 1,200 to about 1,320 degrees Celsius (°C), after which the slabs are cooled to below the melting point of the steel. The slabs are then hot-rolled to a desired thickness 30, and the hot-rolled slabs may optionally be coiled 40. If the hot-rolled slabs are coiled, they are coiled at a temperature of about 550 to 700°C, but other temperatures are also possible. The hot-rolled and optionally coiled slabs may be stored or transported in coil form. If the hot-rolled slabs are coiled, the hot-rolled slabs are then uncoiled for further processing 50. Next, the slab is cold-rolled to form a plate of a desired thickness.60 The desired thickness may be about 0.1 to about 0.6 millimeters in exemplary embodiments, but other thicknesses are also possible. The plate is then annealed in a decarbonization annealing to remove carbon from the plate.70 The decarbonization annealing is performed in a humid nitrogen and hydrogen atmosphere at a temperature of about 850°C to about 1,050°C for about 20 to about 150 seconds, which may be followed by nitriding annealing in another humid nitrogen and hydrogen atmosphere containing ammonia at a temperature of about 900°C to about 1,050°C. In some embodiments, decarbonization may include additional annealing at other temperatures or times. After decarbonization annealing, the plate may contain about 100 to about 300 ppm of carbon (i.e., about 0.01 to about 0.03 mass%) based on the total mass of the plate. The thick plates may optionally contain approximately 300–350 ppm of aluminum and approximately 60–90 ppm of nitrogen. Decarbonizing the thick plates may help reduce or minimize their magnetic aging.
[0009] After decarbonization treatment of the thick plate, it is recrystallized by recrystallization annealing to orient the crystal grains and form a grain-oriented electrical steel sheet. In exemplary embodiments, recrystallization annealing is carried out at a temperature of about 700 to 1,300°C, and recrystallization annealing may involve several separate annealings at different temperatures and specific times. Precise orientation of crystal grains in the thick plate can be obtained during recrystallization annealing, during which the growth of crystals with the desired orientation becomes faster than that of crystal grains with different orientations. Although not bound by theory, there is a theory that the grain growth process is activated by heat, and certain crystals are "excited" more than other crystals for kinetic or energetic reasons. Crystals that grow faster tend to have the desired orientation and begin growing at a lower temperature than the temperature at which crystals with the originally undesirable orientation are activated, at the expense of adjacent crystals. This facilitates the crystals with the desired orientation to reach a critical size so that they become dominant in the crystal growth process. The processing of grain-oriented electrical steel sheets involves one, two, or more high-temperature heating cycles, all of which are referred to herein as recrystallization annealing. The exact temperature, timing, and atmosphere during one or more recrystallization annealing thermal cycles depend on the thickness of the plate, the composition of the plate, and / or other factors. This recrystallization annealing produces a forsterite layer on the surface of the steel.
[0010] In some embodiments, the plates may be coated or further treated (not shown), and the general process outlined above may be modified in other embodiments. Coating can be optionally applied before, after, or during recrystallization annealing. Inorganic coatings include, but are not limited to, a wide variety of materials including silica and chromium(VI). These inorganic coatings, in combination with the forsterite layer, can provide protection such as electrical insulation, corrosion resistance, and durability in humid environments. The inorganic layer and forsterite layer can also provide tensile stress that is useful for the performance of grain-oriented electrical steel sheets. However, inorganic layers may contain harmful chemicals such as chromium(VI) and may have drawbacks such as brittleness that produces dust and flakes.
[0011] Here, following the reference to Figure 1, we refer to Figure 2. The plate 200 formed from grain-oriented electrical steel sheet has anisotropic magnetic properties, and thereafter, the magnetic properties differ in one direction, the "rolling direction 210," from the other, the width direction 220, which is perpendicular to the rolling direction 210. The rolling direction 210 is the direction in which the slab is cold-rolled to form the plate 200. Both the rolling direction 210 and the width direction 220 are along the surface 230 of the plate 200, and the thickness 240 of the plate 200 is perpendicular to the surface 230 of the plate 200. The thickness 240 is measured along the minimum dimension of the plate 200. For use in transformers, the magnetic properties are usually preferred in the rolling direction 210 rather than in the width direction 220. For example, the permeability of the plate in the rolling direction 210 is higher than in the width direction. In an exemplary embodiment, the permeability of the thick plate is about 20% or more higher than the permeability of the thick plate in the width direction 220. In another embodiment, the permeability of the thick plate in the rolling direction 210 is about 30% or more, or about 50% or more, higher than the permeability of the thick plate in the width direction 220.
[0012] During recrystallization annealing, a microstructure is formed by selective grain growth, and a forsterite layer 250 may be formed on the main body 260 of the plate 200, which is located on the surface 230 of the plate 200. The forsterite layer 250 is sometimes called a "glass coating," but the forsterite layer 250 is not composed of glass. The forsterite layer 250 contains magnesium silicate.
[0013] Referring again to Figure 1, the surface 230 of the grain-oriented electrical steel sheet 200 is covered with a coating 270, which is shown in Figure 2. The coating 270 can be applied by spraying, rolling, dipping, brushing, or any other suitable application technique. In various embodiments, the coating 270 can be applied to one surface 230 of the plate 200, or to two or more different surfaces 230. In the description of Figure 2, the coating 270 is shown covering the top and bottom surfaces 230 of the plate 200, but not the sides 230 of the plate 200. However, in various embodiments, any other combination of surfaces 230 can be covered. The coating 270 can be applied such that the cured coating 270 has a thickness of about 1 to about 50 micrometers. The coating 270 contains organic components, and may also optionally contain inorganic components. Unless otherwise specified, the components of the coating 270 listed and described herein refer to the coating 270 before curing, as applied to the plate 200. It will be understood that chemical reactions occur during the curing process, and as a result, some components may react or evaporate during curing, so the components or concentrations are no longer the same as before curing. After curing, the coating 270 contains organic components in an amount of about 10 to about 99% by mass, based on the total mass of the cured coating 270, and the organic components include polymers formed from radiation-curable crosslinking agents. Coating 270 (before curing, as described above) contains at least one radiation-curable crosslinking agent, which is an organic substance. The radiation-curable crosslinking agent has at least one reactive polymerizable moiety, such as an unsaturated double bond. The radiation-curable crosslinking agent may be selected from the group consisting of epoxy compounds, isocyanate compounds, polyurethane compounds, acrylic compounds, polyamide compounds, polyester compounds, silicone compounds, alkenes, and combinations thereof. However, in other embodiments, other types of radiation-curable crosslinking agents may be used. Coating 270 contains about 10 to about 90% by mass of the radiation-curable crosslinking agent based on the total mass of the coating.
[0014] Radiation-curable crosslinking agents may contain one component, but in some embodiments, two or more components are present. For example, one type of radiation-curable crosslinking agent may be a resin, which may be used in combination with a reactive diluent. Resins tend to increase the viscosity of the coating 270, while reactive diluents decrease the viscosity, thereby balancing the two and providing a coating of the desired viscosity. Reaction rate, polymer strength, and many other factors are also balanced and cured by the selection of the radiation-curable crosslinking agent. Usable reactive diluents (which are radiation-curable crosslinking agents) are radical polymerizable compounds having one or more unsaturated structures. Examples of reactive diluents include, but are not limited to, styrene, vinyltoluene, p-methylstyrene, t-butylstyrene, divinylbenzene, N-vinylpyrrolidone, hydroxybutyl vinyl ether, butanediol, vinyl ether, triethylene glycol divinyl ether, diallyl phthalate, diallyl fumarate, triallyl phosphate, triallyl isocyanurate, diallylbenzene, diallylbisphenol A, pentaerythritol, and tetraallyl ether. Other possible reactive diluents that may be optionally present include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, phenoxyethyl (meth)acrylate, dicyclopentadiene (meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, dipropylene glycol di(meth)acrylate, trimethylolpropane di and tri(meth)acrylate, pentaerythritol di and tri(meth)acrylate, epoxy resin (meth)acrylate, (meth)acrylate of the reaction product of polyaddition of ethylene or propylene oxide with polyols such as trimethylolpropane or pentaerythritol, and acrylic or methacrylic esters such as oligo(ethylene glycol) or oligo(propylene glycol) (meth)acrylate acrylic.
[0015] Coating 270 also contains at least one photoinitiator. A wide variety of photoinitiators can be used, including, but are not limited to, benzoin, benzophenone, dialkoxybenzophenone, 4,4'-bis(dimethylamino)benzophenone (Michler ketone), and diethoxyacetophenone, although other photoinitiators may be used in other embodiments. The photoinitiator must be able to initiate crosslinking of the radiation-curable crosslinking agent. Coating 270 may contain about 0.1 to about 20% by mass of the photoinitiator based on the total mass of the coating.
[0016] The silicon compound is an optional component of coating 270. The silicon compound improves the adhesion of coating 270 to the plate 200, and may be present in coating 270 in an amount of about 0 to about 50% by mass based on the total mass of coating 270, although in another embodiment, the silicon compound may be present in coating 270 in an amount of about 10 to about 50% by mass. The silicon compound in coating 270 may be one or more silanes that have been partially or completely hydrolyzed. The silane may be an acyloxysilane, alkylsilane, alkyltrialkoxysilane, aminosilane, aminoalkylsilane, aminopropyltrialkoxysilane, bissilylsilane, epoxysilane, allylsilane, fluoralkylsilane, glycidoxysilane, isocyanatosilane, mercaptosilane, alkylsilane, monosilylsilane, multisilylsilane, bis(trialkoxysilylpropyl)amine, bis(trialkoxysilyl)ethane, sulfur-containing silane, ureidosilane (e.g., 3-ureidopropyltriethoxysilane and vinylsilane), or other silane compounds. Coating 270 may also include at least one siloxane corresponding to the above silane as a substitute or supplement for the silane, and therefore, in some embodiments, the silicon compound is selected from the group consisting of silanes, siloxanes, and combinations thereof. In some embodiments, the silane and / or siloxane further comprises functional groups having a chain length of 2 to 5 carbon atoms and suitable for reaction with radiation-curable crosslinking agents.
[0017] One or more inorganic components may be present in the coating 270. One or more inorganic components may promote certain aspects of the coating 270 that are beneficial for the grain-oriented electrical steel sheet 200, such as improvements in corrosion resistance, coloration, mechanical stability of the coating, thermal conductivity, electrical properties, and thermal durability. In exemplary embodiments, the inorganic components may be present in the coating 270 in the form of a solution, colloid, dispersion, or other form. Exemplary inorganic components include, but are not limited to, carbonates, oxides, silicates, sulfates, and sulfides. In the case of particulate inorganic particles, the particles may include one or more of aluminum (Al), barium (Ba), cerium (Ce), calcium (Ca), lanthanum (La), silicon (Si), titanium (Ti), yttrium (Y), zinc (Zn), and zirconium (Zr). Particulate inorganic compounds may have an average particle size of about 2 nanometers (nm) to 3,000 nm. Small particles having a particle size of approximately 2 nm to approximately 250 nm may also be included as a stabilized dispersion or in the form of a sol or gel. Coating 270 may optionally contain one or more inorganic compounds in an amount of approximately 0 to approximately 60% by mass, based on the total mass of coating 270. In some embodiments, coating 270 contains very small amounts of inorganic compounds, such as less than approximately 5% by mass, based on the total mass of coating 270.
[0018] Inorganic compounds may be useful for modifying the liquid properties of coating 270, as well as the properties of the curable protective layer. Examples of such inorganic compounds include oxides, phosphoric acids, nitrates, silicates, carbonates, sulfates, and sulfides, but other types of compounds may also be included in coating 270. For example, inorganic or organic compounds containing metals may be present, and such compounds may contain one or more of the following elements: lithium (Li), sodium (Na), potassium (K), magnesium (Mg), aluminum (Al), boron (B), bismuth (Bi), silicon (Si), selenium (Se), germanium (Ge), lanthanum (La), gallium (Ga), lead (Pb), tantalum (Ta), yttrium (Y), cerium (Ce), calcium (Ca), titanium (Ti), vanadium (V), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), zirconium (Zr), manganese (Mn), tin (Sn), molybdenum (Mo), and tungsten (W). Each of the elements listed above may be optionally included in the coating 270 in combination with one or more inorganic or organic parts, and the coating may contain 0, 1, or more of the elements listed above. In this disclosure, unless otherwise specified, a component, part, or element may be considered absent from the coating 270 if it is present in an amount of 0 to about 100 ppm. In exemplary embodiments, the coating 270 does not contain chromium (Cr), and thus Cr is present in the coating 270 in an amount of 0 to about 100 ppm (0 to about 0.01 mass%) based on the total mass of the coating 270.
[0019] It may be beneficial to include a wide variety of additives in the coating 270. Additives may be included to adjust the substrate wetting, surface properties, rheological properties, viscosity, color, or a wide variety of other coating properties, either in the liquid state as applied or in the solid state after curing. Additives that may be included in the coating 270 include, but are not limited to, defoamers, dispersants, wetting agents, matting agents, antimicrobial agents, thickeners, and colorants. The coating 270 may contain 0, 1, or more additives.
[0020] The coating 270 may also contain 0, 1 or two or more non-reactive components, and the non-reactive components may be present in the coating 270 in an amount of about 0 to about 60% by mass based on the total mass of the coating 270. Non-reactive components are those that do not participate in a chemical reaction under normal application conditions or participate in a chemical reaction only to an extent that can be ignored, such as less than 0.1% by mass of the components during the chemical reaction based on the total mass of the component, and mean all components used to adjust the properties of the coating 270. Examples of non-reactive components include, but are not limited to, non-polar diluents, polar aprotic diluents, and polar protic diluents. Some examples of non-reactive non-polar diluents include alkanes, cycloalkanes, heterocyclic compounds, aromatic compounds, ethers, and some halogenated species. Examples of polar aprotic diluents include, but are not limited to, propylene carbonate, acetone, ethyl acetate, tetrahydrofuran; compounds containing heteroatoms such as dimethylformamide, dimethyl sulfoxide, acetonitrile, nitromethane, and many others. Exemplary protic diluents include water, alcohols, polyalcohols, organic acids, and other compounds having one or more hydroxyl groups, etc.
[0021] As shown in Figure 1 and subsequently referenced in Figure 2, after the coating 270 is applied, the coating 270 is irradiated and cured 100. The coating is cured on the plate 200 by irradiation using a radiation source 340, which may be an electron beam or an electromagnetic radiation source. The coating 270 can be cured in a curing unit equipped with a radiation source. Examples of radiation sources that may be used in various embodiments include ultraviolet radiation sources such as light-emitting diodes (LEDs), xenon lamps, mercury lamps, or other arc lamps, which may be partially doped or not. In another embodiment, the radiation source is an electron beam source such as a beta ray generator. In another embodiment, a gamma ray generator may also be available. Combinations of multiple radiation sources are also available. Various atmospheres are available in the curing unit. Air is one possible atmosphere, but in some embodiments, other atmospheres such as nitrogen, argon, xenon, helium, carbon dioxide, hydrogen, other inert gases, or combinations thereof may be preferred.
[0022] In some embodiments, as shown in Figure 3 following references to Figures 1 and 2, the plate 200 is coated and cured in a production line 280. Figure 3 is a diagram showing the general concept of the production line, although specific details have been omitted or simplified for clarity. The production line 280 includes transfer rollers 290 used to facilitate the transfer of the plate 200 from one manufacturing step to the next. In the embodiment of Figure 3, a recrystallization annealing step 80, a coating step 90, and a curing step 100 are shown, as shown in Figure 1. The recrystallization annealing step 80 is carried out in a recrystallization oven 300, which includes a heating element 312. In the embodiment shown in Figure 3, the plate 200 is transferred along the production line 280 from the recrystallization oven 300 to a coating station 310, which includes a coating roller 320. The plate 200 is then transported along the production line 280 from the coating station 310 to the curing station 330, where the coating 270 is cured on the surface 230 of the plate 200 using one or more radiation sources 340. Thus, the curing station 330 includes the radiation sources 340. The plate 200 may be transported from the recrystallization oven 300 to the coating station 310 and from the coating station 310 to the curing station using transport rollers 290, thereby coating the plate 200 in the same production line and process used for recrystallization. Additional embodiments (not shown) are also possible, such as the use of an air curtain for transporting the plate 200 from the coating station 310 to the curing station 330. Vertical transport of the plate 200 from the coating station 310 to the curing station 330 is also possible, as in other embodiments.
[0023] Any heat source 350 may be included within the curing station 330, and the addition of heat may accelerate the curing process. The heat source 350 may be an infrared radiation source, a thermal heat source, or a device used to capture heat from another part such as the recrystallization oven 300 of the production line. The thick plate 200 may be coated immediately after exiting the recrystallization oven 300, whereby the thick plate 200 may remain hot enough in some embodiments to accelerate the curing process after coating. The thick plate 200 remains on the same production line 280 while being processed within each of (a) the recrystallization oven 300, (b) the coating station 310, and (c) the curing station 330 and while being transferred therebetween. Accordingly, the manufacturing process of the directionally electromagnetic steel sheet 200 includes the coating station 310 and the curing station 330, and thus the final product exiting the production line includes the cured coating 270. The thick plate 200 may optionally be wound up after coating and curing of the coating. The coating 270 containing organic components provides, as described above, excellent corrosion resistance, moisture resistance, and processing ability (e.g., remaining adhered to the thick plate intact during cutting, punching, or perforation steps) compared to coatings without organic components.
[0024] In the foregoing detailed description of the invention, although at least one exemplary embodiment has been presented, it should be understood that there are a vast number of variations. It should also be understood that the exemplary embodiments or exemplary embodiments are merely examples and are not intended to limit the scope, applicability, or configuration of the present application in any way. Rather, the foregoing detailed description provides a convenient guide for those skilled in the art for implementing one or more embodiments, and these embodiments may be variously modified without departing from the scope shown in the appended claims in terms of the functions and arrangements of the elements described in the exemplary embodiments.
Claims
1. 1. A method for manufacturing a steel sheet, comprising the steps of: forming a molten steel comprising, by weight, 2.5-4.0% silicon, 0.005-0.1% carbon, and 90-97.5% iron, based on the total weight of the molten steel (10); casting the molten steel into a slab (20); cold rolling (60) the slab into a plate, the plate including a surface; decarburizing the plate using a decarburizing anneal at a temperature between 850 and 1,050 degrees Celsius (°C) (70); recrystallizing the plate using a recrystallization anneal at 700-1,300°C to form a grain oriented electrical steel plate (80), comprising recrystallizing the plate in a recrystallization oven (300); applying (90) a coating over the surface (230), comprising applying the coating in a coating station (310), the coating (270) comprising a radiation curable crosslinker that is organic, and the coating (270) comprising a photoinitiator; curing (100) the coating on the surface (230) of the plank (200) by exposing (100) the coating to a radiation source; and Transporting said plank (200) from said recrystallization oven (300) to said coating station (310) over transfer rollers (290).
2. The method of claim 1 , wherein curing the coating (100) comprises exposing the coating (270) to an electron beam, an electromagnetic radiation source, or a combination thereof.
3. The method of claim 1, wherein applying the coating (90) comprises applying the coating (90) comprising 0 to 50 weight percent silane, based on a total weight of the coating (270).
4. 10. The method of claim 1, wherein applying the coating (90) comprises applying the coating (90) comprising 0 to 60 weight percent inorganic particles, based on a total weight of the coating (270).
5. 5. The method of claim 4, wherein applying the coating (90) comprises applying the coating wherein the inorganic particles are selected from the group consisting of carbonates, oxides, silicates, sulfates, sulfides, and combinations thereof, and the inorganic particles further comprise one or more of aluminum (Al), barium (Ba), cerium (Ce), calcium (Ca), lanthanum (La), silicon (Si), titanium (Ti), yttrium (Y), zinc (Zn), and zirconium (Zr).
6. 2. The method of claim 1, wherein applying the coating (90) comprises applying the coating (270) comprising one or more of the elements lithium (Li), sodium (Na), potassium (K), magnesium (Mg), aluminum (Al), boron (B), bismuth (Bi), silicon (Si), selenium (Se), germanium (Ge), lanthanum (La), gallium (Ga), lead (Pb), tantalum (Ta), yttrium (Y), cerium (Ce), calcium (Ca), titanium (Ti), vanadium (V), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), zirconium (Zr), manganese (Mn), tin (Sn), molybdenum (Mo), and tungsten (W).
7. 2. The method of claim 1, wherein applying the coating comprises applying the coating comprising the radiation curable crosslinker in an amount of 10 to 90 weight percent, based on the total weight of the coating, and the photoinitiator in an amount of 0.1 to 20 weight percent, based on the total weight of the coating.
8. 10. The method of claim 1, wherein applying the coating (90) comprises applying the coating (90) wherein the radiation curable crosslinking agent is selected from the group consisting of an epoxy compound, an isocyanate compound, a polyurethane compound, an acrylic compound, a polyamide compound, a polyester compound, a silicone compound, and combinations thereof.
9. 2. The method of claim 1, wherein applying the coating (90) comprises applying the coating (270) to be substantially free of chromium, whereby a concentration of chromium in the coating (270) is 0.01% by weight or less, based on a total weight of the coating (270).
10. Recrystallizing the plank (80) comprises recrystallizing the plank (80) on a production line (280), the production line (280) comprising a transport roller (290) configured to move the plank (200); and The method of claim 1 , wherein applying the coating (80) comprises applying the coating (80) on the production line (280).
11. The method of claim 10, further comprising moving the plank (200) on the production line (280) from a recrystallization oven (300) to a coating station (310).
12. The method of claim 1, wherein the coating (270) comprises water in an amount of 20 to 80 weight percent, based on the total weight of the coating (270).
13. A method for producing a grain oriented electrical steel sheet (200) comprising the steps of: manufacturing a plate comprising electrical steel sheet; A step (80) of manufacturing a grain-oriented electrical steel sheet by recrystallization annealing the thick plate at a temperature of 700 to 1,300 degrees Celsius, in which the thick plate (200) is recrystallized on a production line (280) including a transfer roller (290); applying (90) a coating to a surface (230) of the plank (200) while the plank (200) is on the production line (280), the coating (270) comprising an organic component and a reactive diluent, the reactive diluent being selected from the group consisting of vinyl toluene; divinyl benzene; hydroxybutyl vinyl ether; butanediol vinyl ether; triethylene glycol divinyl ether; phthalic acid diallyl ester; fumaric acid diallyl ester; triallyl phosphate; triallyl isocyanurate; diallyl benzene; diallyl bisphenol A; pentaerythritol and tetraallyl ether; and combinations thereof; and Curing (100) the coating (270) on the surface (230) of the plank (200) by exposing the coating (270) to a radiation source (340), wherein the plank (200) is cured while in the production line (280).
14. A grain-oriented electromagnetic steel sheet (200) having no laser marks, A surface (230) of a grain-oriented electrical steel sheet (200); a forsterite layer (250) on the surface (230) of the grain-oriented electrical steel sheet (200); a coating (270) overlying said surface (230), said coating (270) comprising 10-99% by weight of an organic component and 5% by weight or less of an inorganic compound, based on the total weight of said coating (270), said organic component comprising a polymer formed from a radiation curable crosslinker; Including, The grain-oriented electrical steel sheet contains 0.01 to 0.03 mass% carbon, based on the total mass of the grain-oriented electrical steel sheet, and 2.5 to 4.0 mass% silicon, based on the total mass of the grain-oriented electrical steel sheet; and The grain-oriented electrical steel sheet (200) comprises a grain-oriented electrical steel sheet having anisotropic magnetic properties, whereby the thick plate permeability in the rolling direction (210) is greater than the thick plate permeability in the width direction (220), and the width direction (220) is perpendicular to the rolling direction (210). Grain-oriented electrical steel sheet (200).