Nonwoven fabric containing filament layers
Patent Information
- Application Number
- JP2023526295
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-11-02
- Filing Date
- 2021-10-29
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2041-10-29
AI Technical Summary
Existing nonwoven fabrics face challenges in achieving a balance between softness, bulkiness, and abrasion resistance, with insufficient bonding between fibers leading to inferior quality and inadequate abrasion resistance.
A nonwoven fabric design featuring multiple filament layers with varying densities and interfilament bonding levels, including a first layer with high density forming the outer surface, a second layer with low density in the middle, and a hierarchical structure that promotes uniform fiber-to-fiber adhesion through controlled heat application during the manufacturing process.
The fabric achieves a combination of high abrasion resistance, bulkiness, and softness by ensuring uniform fiber bonding throughout the thickness, enhancing its durability and comfort.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical Field]
[0001] This invention relates to a nonwoven fabric including a filament layer. [Background technology]
[0002] Nonwoven fabrics used in various fields must meet various requirements depending on their intended use. For example, in fields such as disposable hygiene products, disposable cleaning supplies, and medical applications, softness, high loft, and good resilience are important characteristics.
[0003] Carded materials have traditionally been and continue to be used for many such applications. However, manufacturing nonwoven products from carded fibers is complex, and the adhesion between fibers in such nonwovens is either significantly low in pile length or softness, or the adhesion between fibers is insufficient, resulting in poor quality nonwovens, i.e., insufficient abrasion resistance.
[0004] Air-through adhesive spunlay technology is a viable solution that meets industry requirements, primarily because its longer fiber length overcomes some of the drawbacks of carded materials. Various approaches are known within the industry.
[0005] For example, the desired bulkiness and softness can be achieved as disclosed in patent application WO2018059610, which describes the use of crimped filaments having a so-called crimped cross-section (e.g., eccentric core / sheath), or as disclosed in patent application WO2020103964 of PF Nonwovens, which describes the use of filaments with a non-crimped cross-section (e.g., concentric core-sheath).
[0006] Nonwoven fabrics with good abrasion resistance as demonstrated by the Martindale abrasion test are described, for example, in WO2020112705.
[0007] WO2020107421 discloses an air-through bonding method for nonwoven fabrics aimed at producing soft loft fabrics. A continuous fiber fabric is guided between a porous rotating member and a porous belt, and heated air is flowed into the fabric first from one side and then from the other side. However, the description of this method is very vague, and no data on the resulting product is provided.
[0008] Nonwoven fabrics that combine both requirements—namely, soft loft (compressibility, drape, flexibility, non-rigidity, pleasant feel, etc.) and three-dimensional stability (abrasion resistance, pilling resistance, etc.)—are considered the ideal fabric in the industry. Softness and three-dimensional stability are not simple values that can be easily measured, quantified, and compared; rather, they are complex characteristics that encompass a variety of fabric properties, and in fact, a single term encompasses a variety of fabrics. Many patents and applications claim fabrics with softness, loft (high thickness at low basis weight), and several types of resistance. It is readily apparent to those skilled in the art that many of these patents or applications understand the terms "softness" and "resistance" as very different things. For example, the aforementioned application WO2020103964 understands softness as "soft loft" and defines the softness of the fabric based on a special coefficient. Conversely, the aforementioned WO2020112705 also defines softness based on compression rebound force testing. Even if both fabrics are defined as soft, their behavior and the feel experienced by the end user may differ significantly, making direct comparison difficult.
[0009] The objective of the present invention is to provide a nonwoven fabric that is soft and bulky, yet does not easily fray during use.
[0010] The object of the present invention is achieved by a nonwoven fabric, the nonwoven fabric comprising a plurality of filament layers as defined in claim 1: - A first layer (A) forming the first outer surface of the nonwoven fabric, comprising continuous multi-component filaments made of the component, - Extending along the longitudinal direction of the filament, - Forming at least 20% of the surface of the filament, - Form filament-to-filament adhesion within the first layer (A), - A component having a melting point at least 5°C lower than the melting point of the other components of the filament in the first layer (A); - A second layer (B) comprising a continuous multi-component filament consisting of the following components, - Extending along the longitudinal direction of the filament, - Forming at least 20% of the surface of the filament, - Form filament-to-filament adhesion within the second layer (B), - A component having a melting point at least 5°C lower than the melting points of the other components of the filament in the second layer (B); including, - The bulk density of the fibers is 60 kg / m³. 3 Less than It is characterized by the following:
[0011] Further embodiments of the present invention are defined in the dependent claims.
[0012] definition In this specification, the term "filament" is generally defined as an endless filament, while the term "staple fiber" refers to a fiber cut to a defined length. The terms "fiber" and "filament" are used interchangeably in this specification. In the case of cut fibers, only the term "staple fiber" is used.
[0013] The term "filament bonding" refers to all possible interactions between individual filaments or between individual parts of a filament, including adhesion, partial adhesion, non-adhesive contact, crossing, interconnection, and parallel contact. While filament bonding can form adhesion between filaments, it can also allow two independent filaments to come into contact with each other without any restriction on their relative movement.
[0014] The term "filament bonding" or "bonding point" typically refers to the bonding of two filaments at points where they intersect, touch, or are adjacent to each other. Bonding / consolidation bonding can connect more than two filaments or two points on the same filament. Therefore, as used herein, the term "bonding point" refers to the connection of two or more fibers / filaments at a contact point due to the interconnection of low-melting-point components. At bonding points, the high-melting-point components formed in the filament are generally less affected than the low-melting-point components formed in the filament; that is, the sheath melts slightly, but the core remains essentially unchanged. Conversely, the term "bonding indentation" refers to the surface affected by the ridges of the calendar roller. Bonding indentations have a region defined by the size of the ridges on the bonding roller and are usually smaller in thickness than adjacent regions. During the bonding process, the bonding indentation region is usually subjected to high mechanical pressure, and this pressure, along with temperature, may affect the shape of all filament components within the bonding indentation region.
[0015] The term "single-component filament" or "single-component fiber" refers to a filament formed from a single polymer or a single polymer blend, and is therefore distinguished from two-component filaments or multi-component filaments.
[0016] The term "multicomponent fiber" or "multicomponent filament" refers to a fiber or filament that incorporates two or more individual partial components in its cross-section, each of which consists of a different polymer compound or a different blend of polymer compounds. Therefore, the term "multicomponent fiber / multicomponent filament" is a broader term that includes, but is not limited to, "two-component fiber / two-component filament." The various components of a multicomponent filament are basically arranged in clearly defined regions along the cross-section of the filament and extend continuously along the length of the filament. The cross-section of a multicomponent filament may be divided into several partial cross-sections consisting of various components of any shape or arrangement, such as any arrangement of partial components of the cross-section in forms such as coaxial arrangement, core / sheath, radial, or so-called lands-in-the-sea configuration.
[0017] The terms "two-component" and "two-component" used to describe filaments are interchangeable in this specification.
[0018] The design of multicomponent filaments has a decisive influence on the crimpability of these filaments. A good way to recognize the design of multicomponent filaments is to check and evaluate a cross-section that visualizes the positions of the different components of the filament. Frequently, the different components are formed from different polymer formulations that are selected and characterized by different melting points and / or different shrinkage properties, for example, after spinning, heat setting, drawing, and final fiber consolidation. Usually, a rotationally symmetric position (e.g., concentric core / shell) of the filament components in the cross-section results in a non-crimped filament, while an asymmetric position (e.g., parallel, or eccentric core / shell) of the filament components results in a differential potential crimping force for achieving either a self-crimping and / or a heat-activated crimping filament. For the sake of simplicity of the terms of this application, instead of the terms "filament with a cross-section corresponding to crimp" and "filament with a cross-section not corresponding to crimp", the terms "crimpable cross-section" and "non-crimpable cross-section" are used. As used herein, the term "crimpable cross-section" refers to a multicomponent fiber in which components with different shrinkage properties are arranged in the cross-section, whereby these filaments self-crimp during the drawing and consolidation of the filament, or when slowly cooled after heating above the activation temperature, the fibers crimp, and the fibers come to follow the vector of the contraction force. Thus, when the fiber is unraveled, a so-called helical crimp is formed, but when the fiber is within the fiber layer, an ideal helix cannot be formed due to the mutual adhesion of the fibers. In the case of multicomponent fibers, the center of mass of each individual component in the fiber cross-section can be determined (taking into account the area / position of each component in the cross-section). Without being bound by theory, as explained for a rotationally symmetric concentric core / shell, when the center of gravity of the total area of each component is at approximately the same point, the fiber is considered to be "non-crimpable". For example, in the case of a round two-component fiber having a symmetric or centered core-shell cross-sectional structure, the center of mass is at the center of the cross-section (see Figure 1).
[0019] The measured value "filament diameter" is expressed in the unit of μm. Since the term "gram number of filaments per 9000 m" (also called denier or den) or "gram number of filaments per 10000 m" (also called dTex) correlates with the value obtained by multiplying the density of the material(s) used by the filamental diameter (assuming a circular cross-section of the filament), it is used to represent the degree of fineness or coarseness of the filament.
[0020] "Machine direction" (MD) - Regarding the production of non-woven fiber materials and the actual non-woven fiber materials themselves, the term "machine direction" (MD) basically represents the direction corresponding to the forward movement direction of the non-woven fiber material on the production line for manufacturing this material.
[0021] "Cross direction" (CD) - Regarding the production of non-woven fiber materials and the actual non-woven fiber materials themselves, the term "cross direction" (CD) basically represents the direction that is transverse to the forward movement direction of the non-woven fiber material on the production line while being located on the plane of the non-woven fiber material. [[ID=B]]
[0022] The "z-direction" - In relation to the production of non-woven fabric fiber materials, it is perpendicular to the planar machine direction × width direction (MD × CD). The elongation direction in the z-direction represents the thickness of the non-woven fabric material.
[0023] "Nonwoven material" or "nonwoven fabric" refers to a belt-like or fibrous material made from directionally or randomly oriented filaments, which are initially formed during the formation of a filament layer, then joined together by friction or the induction of binding or adhesive forces, and finally joined together by the formation of mutual adhesion. This integration is achieved thermally (e.g., by ventilation, calendering, ultrasonic effect, etc.), chemically (e.g., by the use of adhesives, etc.), mechanically (e.g., by water entanglement, etc.), or a combination of these methods. This term does not refer to fabrics formed by weaving or knitting, or fabrics using twisted yarns or fibers to form adhesive seams. The fibers may be of natural or synthetic origin, and may be stapled yarns, continuous fibers, or fibers manufactured directly at the processing site. Commercially available fibers range in diameter from approximately less than 0.001 mm to approximately 0.2 mm and are available in various forms: short fibers (known as staple fibers or cut fibers), continuous individual fibers (filaments or monofilament fibers), untwisted bundles of filaments (comb fibers), and twisted bundles of filaments (twisted yarn). Nonwoven fabrics can be manufactured using many methods, including meltblown, spunbond, spunmelt, solvent spinning, electrospinning, carding, film fibrillation, fibrillation, air-lay treatment, dry-lay treatment, wet-lay treatment, and various combinations of these processes known in the art. The basis weight of nonwoven fabrics is usually expressed in grams per square meter (g / m²). 2 It is represented as ).
[0024] The "spunbond" or "spunlaid" process is a nonwoven fabric manufacturing process that directly converts a polymer into filaments and immediately deposits these filaments to form a layer of nonwoven filaments with randomly arranged filaments. This nonwoven filament layer then integrates with the nonwoven fabric by forming adhesive zones between the filaments. This integration process can be carried out using various methods, such as ventilation or calendering.
[0025] The term "butt" refers to a filamentous material in its pre-bonding state, which can be achieved through various methods, such as air-through bonding or calendering. A "butt" consists of individual filaments that are not yet interbonded, even if they have been pre-bonded / pre-consolidated in a specific way. Here, this pre-consolidation may occur during or immediately after filament lamination in the spunlay process. However, in this pre-consolidation, many filaments are still free to move and can be rearranged. The aforementioned "butt" may consist of several layers formed by the accumulation of filaments from several spinning beams in the spunlay process.
[0026] In the sense used herein, the term “layer” refers to a partial component or element of a fabric. A “layer” may be in the form of multiple filaments produced on a single spinning beam or on two or more consecutively arranged spinning beams that form essentially the same filaments. For example, two consecutively arranged spinning beams intended to carry out the spunbond method can be combined to produce a single layer by setting them up in essentially the same way and processing polymers of essentially the same composition. Conversely, if one of two spunbond-type spinning beams produces, for example, a single-component filament and the other produces, for example, a two-component filament, two different layers will be formed. The composition of a layer can be determined based on the individual settings and component knowledge that determine the resin (polymer) composition used to form the layer, or by analysis of the nonwoven fabric itself, for example, by analysis using an electron microscope, or by analysis of the composition used to produce the filaments contained in the layer by DSC or NMR. Layers of filaments adjacent to each other do not necessarily need to be strictly separated, and layers in the boundary region may mix as a result of filaments from later deposited layers falling into the gaps between filaments in earlier deposited layers. In nonwoven fabrics, layers may form typical structures independent of the hierarchical structure (e.g., spunbond + meltblown + spunbond (SMS)). A single layer can contain one, two, or more layers.
[0027] As used herein, the term “stratum” (plural “strata”) refers to a filamentous region of a nonwoven fabric that extends substantially along the MD and CD planes, has a specific thickness in the z-direction of the fabric, and has a substantially uniform filament density (i.e., mass of filaments per unit volume). The filament density of a stratum within a nonwoven fabric cannot be precisely measured, but may be visually assessed in a cross-section of the nonwoven fabric. A stratum may also be characterized by substantially uniform filament adhesion density and / or substantially uniform content of strong and weak filament adhesion (although there may be a slight gradient in density from the outer surface of the outer stratum toward the intermediate region). Thus, it is understood that filament stratums within a nonwoven fabric are never perfectly uniform; because the filaments of the nonwoven fabric are randomly arranged and oriented, filaments may enter one stratum into another, and furthermore, certain regions of a stratum may locally expand or extend from the plane in which the majority of that stratum exists, and some of the filaments of that stratum may enter adjacent stratums or exit the surface of the nonwoven fabric. The hierarchical structure can be observed by analyzing the nonwoven fabric itself, for example, by using an electron microscope (especially from cross-sectional views), or by tomography or micro-CT measurement.
[0028] In this specification, the term "compressibility" refers to the distance in millimeters over which a nonwoven fabric is compressed due to the effect of a defined load during the measurement of "elasticity."
[0029] In this specification, the term "recovery" refers to the ability of a fabric to return to its initial shape after compression. This is primarily related to the bulkiness recovery (recovery) ability of the fabric, which is based on the ratio of the fabric's thickness after the release of the applied load to its initial thickness.
[0030] In this specification, the term "drawdown ratio" or "draw ratio" refers to the value calculated by dividing the capillary cross-sectional area by the filament cross-sectional area. To calculate the filament cross-sectional area, the fineness of the fiber, measured based on its apparent diameter, is used. Since this method cannot be used to calculate other non-circular cross-sections, analysis of SEM images showing the actual cross-section is required in such cases.
[0031] Preferred embodiments of the present invention will be described in more detail below with reference to the attached schematic diagrams, photographs, and three-dimensional models. [Brief explanation of the drawing]
[0032] [Figure 1] This is an example of a crimped cross-section. [Figure 2] This is a scanning electron microscope (SEM) image showing a cross-section of one embodiment of the present invention. [Figure 3] This is a schematic diagram showing a cross-section of one embodiment of the present invention. [Figure 4] This is a schematic diagram showing a cross-section of another embodiment of the present invention. [Figure 5A] This is a schematic plan view showing a non-adhesive type filament joint. [Figure 5B] Figure 5A is a schematic cross-sectional view showing the filament junction. [Figure 6A] This is a schematic plan view showing a weakly adhesive type filament joint. [Figure 6B] Figure 6A is a schematic cross-sectional view showing the filament junction. [Figure 7A] This is a schematic plan view showing a fully bonded filament joint. [Figure 7B] Figure 7A is a schematic cross-sectional view showing the filament junction. [Figure 8A] This is a schematic plan view showing the filamentous junctions of a tree trunk type. [Figure 8B] Figure 8A is a schematic cross-sectional view showing the filament junction. [Figure 9] This is a photograph showing a cross-section of one embodiment of the present invention when fixed in resin. [Figure 10] This is an SEM microscope image showing a cross-section of one embodiment of the present invention. [Figure 11] This is a schematic diagram showing a cross-section of a fabric with a very low inter-filament bonding density and a relatively large void volume. [Figure 12] This is a schematic diagram showing a cross-section of a fabric with a uniformly low density of inter-filament bonding. [Figure 13] This is a schematic diagram showing a cross-section of a fabric with a uniformly high level of inter-filament bonding density and a relatively small void volume. [Figure 14] This is a schematic diagram showing a cross-section of a fabric with a very high inter-filament bonding density and a small void volume. [Figure 15] This is an SEM microscope image showing a nonwoven fabric according to the present invention after delamination, where traces of adhesive failure can be seen. [Figure 16] This is an SEM microscope image showing a nonwoven fabric according to the present invention after delamination, where traces of adhesive failure can be seen. [Figure 17] This is an SEM microscope image showing a nonwoven fabric according to the present invention after delamination, where traces of adhesive failure can be seen. [Figure 18] This is an SEM microscope image showing a nonwoven fabric according to the present invention after delamination, where traces of adhesive failure can be seen. [Figure 20A] This is an SEM micrograph showing a cross-section of one embodiment of the present invention, which includes a non-crimped filament. [Figure 20B] This is an SEM microscope image showing a cross-section of one embodiment of the present invention, which includes a non-curved filament. [Figure 21] This is a schematic diagram showing a cross-section of yet another embodiment of the present invention. [Figure 22] This is an SEM microscope image showing a cross-section of one embodiment of the present invention. [Figure 23] This is a schematic diagram showing the process line for manufacturing the nonwoven fabric of the present invention. [Figure 24] This is an SEM microscope image showing a cross-section of Example 1. [Figure 25]This is an SEM microscope image showing a cross-section of Example 2. [Figure 26] This is a photograph showing a cross-section of Example 2, which is fixed in resin. [Figure 27] This is a three-dimensional model showing the X-ray tomography of Example 1. [Figure 28] This is a digital cross-section of the 3D model shown in Figure 27. [Figure 29] This is an SEM micrograph showing a cross-section of Example 3. [Figure 30] This is an SEM micrograph showing a cross-section of Example 4. [Figure 31] This is an SEM micrograph showing a cross-section of Example 5. [Figure 32] This is an SEM microscope image showing a cross-section of Example 6. [Figure 33] This is an SEM microscope image showing a cross-section of Example 7. [Figure 34] This is an SEM microscope image showing a cross-section of Example 8. [Figure 35] This is an SEM micrograph showing a cross-section of Example 9. [Figure 36] none [Figure 37] This is an SEM microscope image showing a cross-section of Example 11. [Figure 38] This is a perspective view showing the apparatus used for the Martindale mean abrasion resistance grade test. [Figure 39] This is a grade index used for evaluating fuzziness in the Martindale mean abrasion resistance grade test. [Figure 40] This is a schematic diagram illustrating a delamination test. [Figure 41] This is a schematic diagram illustrating a delamination test. [Figure 42A] This is a photograph showing a holder for samples used for SEM (Scanning Electron Microscope) observation. [Figure 42B] This is a photograph showing a holder for samples used for SEM (Scanning Electron Microscope) observation. [Figure 43A] This is a photograph showing a holder used for 3D tomography. [Figure 43B] This is a photograph showing a holder used for 3D tomography. [Figure 43C] This is a photograph showing a holder used for 3D tomography. [Figure 44] This is a three-dimensional model of a micro-CT analysis of a sample according to the present invention. [Figure 45] This is a three-dimensional model of a micro-CT analysis of a sample according to the present invention. [Figure 46] This is a three-dimensional model of a micro-CT analysis of a sample according to the present invention.
[0033] Detailed explanation Spunbond and / or spunmelt nonwovens are well known in the industry. Endless filaments produced using a spinning beam are laid on a manufacturing belt to form a vat, which is then pre-compacted and bonded to form a fabric. The bonding process can be one of several known options, e.g.: - Mechanical entanglement, for example, caused by a needle or a stream of water; - Chemical bonding performed using adhesives or other additives added for bonding purposes; - Thermal bonding is performed by exposing the bat to heat, which melts and compacts at least a portion of the polymer composition to form bonding points. You may choose from the following: Heat can be provided, for example, by a pair of calender rolls, radiant heat, or a hot fluid passing through a vat.
[0034] Each of the listed methods has specific advantages and disadvantages, giving the fabric a typical appearance and characteristics, which can be controlled by setting the process within a given range. The examples listed above are for illustrative purposes only, and it will be understood by those skilled in the art that other bonding methods or various combinations thereof can be used to achieve the desired characteristics of the fabric.
[0035] Fabrics compacted by thermal fluid flow are well known in the industry, and in particular, carding techniques using short fibers to produce soft, heat-bonded fabrics are well known. The main advantage of thermal fluid bonding is that the bonding extends throughout the entire fabric, and each individual fiber intersection can form a bonding zone. Each bonding zone is small and forms between two or more fibers in contact with each other. Short fiber techniques take advantage of the ability to mix multiple fibers to create a homogeneous fiber blend and to precisely control the amount of fiber containing low-melting-point polymers (adhesive polymers). For example, if a very soft, lofty fabric is desired, only a small amount of fiber containing adhesive polymers may be included in the fiber premix, and vice versa.
[0036] Conversely, spunmelt nonwovens are typically manufactured from a single type of filament, and the amount of adhesive polymer can only be controlled by the content of the adhesive polymer in each fiber (polymer ratio in the two-component filament). Spunmelt manufacturing lines are equipped with multiple spinning beams, and by combining each beam in various ratios, layered fabrics with different adhesive polymers can be produced. Multiple layers with different adhesive polymer ratios result in different properties, and the fabric can utilize the synergistic effect of strongly bonded and moderately bonded layers. The ratio of adhesive polymer in the filament composition is illustrative in this specification, and more technical features can be combined, for example, as described in Reifenhauser's application EP19189238.9 (unpublished) from 2018. This application describes a fabric consisting of at least two layers, one layer providing high abrasion resistance and the other layer providing softness and bulkiness.
[0037] While the above solution provides a fabric with a desirable combination of properties, it hides one disadvantage for fabric manufacturers from a process perspective. The best abrasion resistance and softness (in terms of flexibility or drape) are achieved only when the first layer forms a thin surface on top of the second layer. This means that the basis weight of the first layer is low, and therefore, in a two-beam production line, the first beam cannot be used to optimize its processing rate.
[0038] The solution of the present invention provides a spunmelt material in which the "soft and bulky" portion of the "skin" can be formed by setting up a high-temperature fluid flow bonding process, and the thickness of the "skin" can be controlled according to the desired final properties of the fabric.
[0039] A fabric according to the present invention can be manufactured from a vat containing a multi-component filament with a low-melting-point adhesive polymer on at least a portion of its surface. The vat on a moving belt is subjected to heat treatment. Heat can be transferred to the vat by a high-temperature fluid, such as hot air. In general, heat can be transferred to the vat at different stages of the manufacturing process, for example, immediately after laying the filaments on the belt and pre-compacting the structure, during the thermal activation process, during the bonding process, etc.
[0040] The high-temperature fluid penetrates the surface of the filament vat and flows around the filaments, transferring some of the heat carried by the high-temperature fluid to the cooler filaments. When some of the heat is transferred to the filaments on the surface of the vat, the temperature of the high-temperature fluid decreases somewhat, as does the temperature difference between the filaments and the high-temperature fluid. As those skilled in the art will know, when the surface filaments acquire this heat, the temperature of the filaments increases, while the temperature difference between the high-temperature fluid and the filaments decreases. With sufficient time and heat, it is possible to heat all the filaments in the fabric to a uniform temperature, resulting in uniform adhesion between fibers throughout the entire thickness of the fabric. Thus, the fabric can be said to be uniformly, completely, or sufficiently bonded.
[0041] Surprisingly, it has been found that fabrics with non-uniform adhesion point density across their entire thickness can offer significant advantages. Fabrics according to the present invention, when viewed in cross-section, include regions of strong filament bonding (where more filaments are in contact with each other, thus forming more filament bonding and / or stronger bonding) and regions of weak filament bonding; here, bonding is defined as all possible interactions between individual filaments, i.e., contact, crossing, interconnection, parallel contact, etc., i.e., bonding, partial bonding, or non-bonding (more detailed definitions below). Such distinctions between these regions correlate with filament density (number of filaments in a given region) for a single type of filament (based on fiber surface characteristics). Regions with a higher degree of bonding are usually formed on the outer surface of the filament battens, where high-temperature fluids flow into the fabric. Although high-filament density and low-filament density regions (layers) are generally well visible, there is usually no strict boundary between them. Fabrics according to the present invention include at least two different filament layers in the thickness direction. A hierarchy is generally defined as a three-dimensional region oriented in a planar MD-CD direction where the level of filament adhesion and / or filament density is typically uniform. The formation of such a hierarchy is influenced by various factors, and it can be recognized in several ways.
[0042] For example, layers with a high level of inter-filament bonding also have high filament density or fiber density. Although the filaments are formed from the same vat, they are closer together than filaments in layers with a lower degree of fiber bonding. Fiber density levels can be estimated, for example, by observing SEM microscope cross-sections as shown in Figure 2, or by analyzing and calculating them from tomography or micro-CT measurements. In this case, a two-dimensional digital cross-sectional view can be created and used for accurate determination of filament density.
[0043] For example (see Figure 3), a fabric according to the present invention may include at least two different filament layers (A, B) having different filament densities in the thickness direction. Preferably, the ratio of the filament density of layer A to the filament density of layer B is at least 1.5; more preferably at least 2.0; more preferably at least 2.5; more preferably at least 3, and even more preferably at least 5.
[0044] For example, a fabric according to the present invention may include at least two different filament layers. In this case, a first layer (A) with a high filament density forms one surface of the nonwoven fabric, and a second layer (B) with a low filament density forms an intermediate region or a second surface of the nonwoven fabric.
[0045] For example (see Figure 4), a fabric according to the present invention may include at least three different layers. In this case, there is a first layer (A) forming the first outer surface of the fabric, a second layer (B), and a third layer (C) forming the second outer surface of the fabric. Here, the second layer (B) is positioned between the first layer (A) and the third layer (C). The filament density of the second layer (B) forming the intermediate region is lower than that of the first layer (A) and the third layer (C). Note that the outer layers (A,C) may have the same properties, but do not need to be the same as long as their filament density is higher than that of the (inner) second layer (B). Preferably, the ratio of the filament density of the first layer (A) to the filament density of the second layer (B) is at least 1.5; more preferably at least 2.0; more preferably at least 2.5; more preferably at least 3, and even more preferably at least 5. Preferably, the ratio of the filament density of the third layer (C) to the filament density of the second layer (B) is at least 1.5; more preferably at least 2.0; more preferably at least 2.5; more preferably at least 3, and even more preferably at least 5.
[0046] For example, the interfilamental bonding density can be measured directly and estimated using, for instance, an optical microscope or a scanning electron microscope (SEM). Both methods are applicable only to the surface analysis of fabric samples. For a perfect sample analysis, the "Method for Determining Fiber Shape Statistics of Nonwoven Fabrics" is publicly known in the industry, which converts 3D micro-CT images into a fabric model. This method uses a machine learning approach to identify individual fibers in the sample, then performs shape analysis of these fibers to obtain statistical values suitable for material characterization. As a result, the fiber orientation and density distribution can be determined. This analytical workflow was developed by Math2Market and is part of GeoDict The Digital Material Laboratory.
[0047] For example, a fabric according to the present invention may include at least two different filament layers (A, B) having different filament bonding densities in the thickness direction. Preferably, the ratio of the filament bonding density of the first layer (A) to the filament bonding density of the second layer (B) is at least 2; more preferably at least 3; more preferably at least 4; more preferably at least 5; even more preferably at least 7.
[0048] For example, a fabric according to the present invention may include at least three different layers: a first layer (A) forming the first outer surface of the nonwoven fabric; a second layer (B); and a third layer (C) forming the second outer surface of the fabric, with the second layer (B) positioned between the first layer (A) and the third layer (C). The filament bonding densities of the first layer (A) and the third layer (C) are higher than those of layer (B) forming the intermediate region of the fabric. Both outer layers (A, C) may have the same properties, but it should be noted that they do not need to be the same, as long as their filament bonding densities are higher than those of the (inner) second layer (B), which has the lowest filament bonding density. Preferably, the ratio of the filament bonding density of layer (A) (or the third layer (C)) to the filament bonding density of layer (B) is at least 2; more preferably at least 3.0; more preferably at least 4; more preferably at least 5; even more preferably at least 7.
[0049] Filament bonding The density of inter-filament bonds correlates with the adhesive density in the fabric, or in other words, with the length of a portion of the filaments between adhesive points. It should be noted here that not all inter-filament bonds form adhesives; if so, different types of adhesives will appear depending on the filament composition and surrounding conditions. Without being bound by theory, the inventors believe there are four typical examples: 1) No adhesion - Even if two filaments come into contact, no adhesion occurs (see Figures 5A and 5B). For example, in the case of parallel fiber types where the polymer adheres only to a portion of the filament surface, the filaments may face each other in areas where the adhesive polymer is not available. Therefore, the filaments can come into contact with each other, but they are not connected or adhered. Also, for example, if a fabric is bonded and then filament crimping is resumed using a technique that does not heat the adhesive polymer to its melting point, the filaments may intertwine and form more filament contact points, but no new / additional filament adhesion will be formed. 2) Weak or tangential adhesion - Two filaments may be in "tangential" contact with each other, and the adhesive polymer may form a "neck" between them (see Figures 6A, 6B). This can occur, for example, when the fibers are in only slight contact with each other, or when there is a small amount of adhesive polymer available. 3) Complete bonding – The two filaments are in contact with each other, and the adhesive polymer covers the filaments with a bonding sheath (see Figures 7A and 7B). This can occur, for example, when the fibers are slightly pressed against each other, or, for example, when there is a large amount of adhesive polymer available to form the coating. 4) "Tree trunk" - Two filaments are in contact with each other longitudinally, and an adhesive polymer forms a neck or bonding film on both fibers along a specific length, for example, a length greater than the sum of the diameters of the two bonded filaments (see Figures 8A, 8B).
[0050] It should be noted that more than two fibers can form bonding points, and it is possible to combine different types of bonding points. For example, a tree trunk with weak / tangential bonding can be bonded to a third fiber, etc. The classification presented above is a typical example for illustrative purposes, and in reality, various types of bonding can be seen in fabrics, particularly transient bonding between weak and complete bonding, and tree trunks can form bonding ranging from very short to very long.
[0051] For example, layers with a large number of filamentary bonds may have a higher density of adhesion 3 (complete adhesion) and 4 (tree trunk) than layers with a small number of filamentary bonds.
[0052] For example, a fabric according to the present invention may include at least two different filament layers (A, B) with different levels of complete adhesion and trunk-type adhesion density along its thickness. Preferably, the ratio of complete adhesion density to trunk-type adhesion density in the first layer (A) and the second layer (B) is at least 1.5; more preferably at least 2.0; more preferably at least 3.0; more preferably at least 4.0, and even more preferably at least 5.
[0053] For example, a fabric according to the present invention may include at least three different layers: a first layer (A) forming the first outer surface of the nonwoven fabric; a second layer (B); and a third layer (C) forming the second outer surface of the fabric, where the second layer (B) is positioned between the first layer (A) and the third layer (C). The total density of complete adhesion and stem-type adhesion in the first layer (A) and the total density of complete adhesion and stem-type adhesion in the third layer (C) are higher than the total density of complete adhesion and stem-type adhesion in the second layer (B). The outer layers (A,C) may have the same properties, but it should be noted that they do not need to be the same as long as the total density of complete adhesion and stem-type adhesion is higher than that of the (inner) second layer (B). Preferably, the ratio of the total density of complete adhesion to trunk-type adhesion of the first layer (A) (or third layer (C)) to the second layer (B) is at least 1.5; more preferably at least 2.0; more preferably at least 3.0; more preferably at least 4.0, and even more preferably at least 5.0.
[0054] It is possible to observe all four types of adhesion in a single fabric sample. The strength of the adhesion increases from the initial option (no adhesion) to weak adhesion / tangential adhesion, then to full adhesion, and finally to trunk adhesion. The number and ratio of the various types of adhesion present in the fabric can affect the final fabric properties. For example, a greater number of high-strength adhesions can promote the fabric's durability and tensile strength, but it may also make the fabric stiffer. In particular, a large number of trunk adhesions with large void volumes may form undesirable hard inner areas that can be negatively evaluated as rough or uncomfortable to wear.
[0055] For example, when examining a cross-section, multiple void volumes can be observed in the nonwoven fabric. Large void volumes, called "cavities," can be seen in the cross-section of the nonwoven fabric and are three-dimensional. Generally, in regions with a high level of inter-filament bonding, the void volume between filaments is small, and the total void volume of the entire region is generally small. Conversely, in regions with less inter-filament bonding, the void volume is large, and the total void volume of a given region is also large. Large voids, called cavities, can also be observed in the cross-section of the fabric. In a cross-section along the long axis (MD) of the nonwoven fabric, the length of the cavity is considerably larger than the height of the cavity.
[0056] For example, the nonwoven fabric according to the present invention may include a layer B containing cavities, where the ratio of the length to the height of the cavities, L:H, is at least 3:1, preferably 5:1, and most preferably 10:1. See, for example, Figures 9 and 10.
[0057] While nonwoven fabrics themselves can be analyzed using different types of microscopes or other visualization techniques to explain differences in their fiber structure, from the end-user's perspective, fabric properties are a significant advantage. Without being bound by theory, and assuming that the level of inter-filament bonding is proportional to the adhesion density when nonwoven fabrics are manufactured from a uniform filament vat consisting of the same filaments, it becomes possible to predict the final properties based on the level of inter-filament bonding density.
[0058] For example, a single-layer vat for a spunbond air-through bonding process is pre-consolidated on a belt. Here, a high-temperature fluid flows into the fabric from above, and then the vat is transferred to an air-through bonding unit for bonding on a belt or drum. Here, the high-temperature fluid flows into the vat from the same side as the pre-consolidated air. Based on the correct techniques and process conditions, various structures with various properties can be formed.
[0059] If the heat supplied to the bat filaments is insufficient, the adhesive polymer will not soften or melt sufficiently, and the resulting bond will generally be weak. The resulting fabric typically has a very low inter-filament adhesion density and relatively large void volumes. Such fabrics are sometimes referred to as "underbonded." It is usually easy to break the filaments or to remove parts of them, and their resistance (to both surface and interlayer delamination / disintegration) is very low. This fabric can also be described as unstable. On the other hand, such fabrics are considered very soft in terms of compressibility, flexibility, and drape. See Figure 11.
[0060] When heat (preferably at the lower limit of a suitable temperature range) flows into the vat filaments, especially when there is sufficient time for the heat to be distributed as uniformly as possible throughout the vat and into the filaments, or when the vat allows heat to pass through easily, for example, with the same temperature gradient at all locations (a person skilled in the art can easily determine a suitable process setting), the adhesive polymer softens or melts sufficiently (at the lower limit of a suitable bonding temperature range), and filament bonding is formed. The formed fabric typically exhibits a homogeneous low level of filament bonding density, and the void volume remains relatively large. Such fabrics are sometimes called "low-bonding" fabrics. Typically, these fabrics are bulky (long pile) and soft in terms of compressibility, flexibility, and drape, but maintain a certain (low) level of surface resistance and delamination resistance. See Figure 12.
[0061] When heat flows into the bat filaments and is distributed unevenly (viewed from the direction of heat inflow), more heat is absorbed by the outer fibers and less by the fibers inside the fabric, a layered structure may be formed.
[0062] The hierarchical structure requires a high filament bonding density level on the outer surface and a low filament bonding density level within the fabric. See Figure 3.
[0063] Heat can flow into the filament vat from one side or both sides simultaneously (e.g., one side and a hot airflow from a high-temperature surface, such as a belt, table, or drum; a hot airflow from the other side), or from both sides in separate processes (from one side, then from the other side). Under these circumstances, a first layer (A) with a high filament bonding density may be formed on the first outer surface, a third layer (C) with a high filament bonding density may be formed on the second outer surface, and a second layer (B) with the lowest filament bonding density may constitute an intermediate region. See Figure 4.
[0064] Without being bound by theory, the inventors believe that a hierarchical structure can be formed if there are many cooperating process elements and parameters. For example, a small compressive force under heat (e.g., tension of fabric on the cylindrical surface of a drum or roll) may promote the formation of an outer layer with a higher level of inter-filament bonding density. For example, heat flowing into the filaments may soften or partially soften non-adhesive polymers in the polymer composition, and the partial softening of the filament closest to the heat source may help in the formation of the outer layer. For example, filaments having a crimpable cross-section or containing a shrinkable polymer may attempt to transition from a semi-stable state to a more stable state under heat. Even if the process is not strong enough to form crimp, the forces of the inner filaments can promote layer formation. Patent application WO2020103964 describes the theory of inner shrinkage force and fiber / filament resistance threshold, explaining the formation of bulky structures with a non-crimpable cross-section. Without being bound by theory, the inventors believe that a similar principle could be used in an oven to explain the force that moves a portion of the filament in the z-direction to form a hierarchical structure. For example, cooling immediately after removing from the oven helps to form a hierarchical structure, or at least fix the formed hierarchical structure.
[0065] Fabrics formed according to the present invention, which combine layers with high and low filament bonding density levels within their structure, exhibit a very good combination of properties. Here, good resistance (both surface resistance of the layers with high filament bonding density levels and the strong force required against delamination occurring at the weakest layer B with low filament bonding density levels) is combined with good bulkiness and softness (in terms of compressibility, flexibility, and drape) promoted by the bulky layers with low filament bonding density levels.
[0066] Without being bound by theory, the inventors believe that the balance between softness / bulkness and resistance / tensile strength properties can also be achieved by utilizing the synergistic effects resulting from the lack of clear boundaries between adjacent layers. For example, a particular filament can have a portion extending into a first or third layer (A,C) with a high filament bonding density, and another portion extending into a second layer (B) with a low filament bonding density. For example, a layered structure formed within one layer of a filament vat improves internal complexity compared to a similar structure formed from different fiber layers. When heat (preferably at an intermediate to high level within a suitable heat range) flows into the vat filaments, especially when there is sufficient time for the heat to flow into the filaments as uniformly as possible at all locations in the fabric, or when the vat allows heat to pass through easily so that it passes through with the same thermal gradient at all locations (a person skilled in the art can easily determine a suitable process setting), the adhesive polymer softens or melts sufficiently (up to the upper limit of a suitable bonding temperature range), and filament bonding is formed. The resulting fabric typically exhibits a homogeneous, high interfilament bonding density level and relatively small void volume. Such fabrics are sometimes referred to as "fully bonded." They typically have low bulk, high rigidity, and maintain a high level of surface resistance, particularly delamination resistance. See Figure 13.
[0067] If too much heat flows into the butt filaments, the adhesive polymer completely melts, mainly forming full adhesion and trunk-type adhesion. Furthermore, other polymers may be affected by the filament composition, for example, becoming more flexible, and the filament butts may collapse into the filament composition itself. Typically, the resulting fabric has a very high inter-filament bonding density and a small void volume. Such fabrics are sometimes called "over-bonded." These fabrics are usually highly rigid and durable. They may also have low bulk and an insufficient soft feel. See Figure 14.
[0068] Furthermore, the aforementioned hypothesis that the thickness of the fabric decreases with increasing heat absorption is based on the assumption that the filaments are not subjected to significant changes during bonding that induce internal forces that alter their shape (e.g., crimp activation, controlled shrinkage, etc.). Under these circumstances, the thickness curve of the fabric in response to heat absorption may differ; that is, there may be one or more peaks at the optimal crimp / shrinkage value, and the thickness decreases in fabrics with weak or excessive bonding. The principle of bonding is generally the same, and a hierarchical structure with all the advantages can be formed.
[0069] It is well known in this industry that so-called crimping is produced by a specific combination of multiple polymers with different shrinkage levels arranged in a so-called crimpable cross-section. This crimping can be either immediate self-crimping or latent crimping, where the fiber must be activated (e.g., by thermal activation) to exhibit crimping. When a fiber has a crimpable cross-section, it results in regular crimping that forms so-called helical crimping. Simply put, a fiber with a crimpable cross-section tends to bend in the direction toward the component with the higher shrinkage rate, which results in nearly uniform helical crimping. In other words, the crimpable cross-section causes the internal force vectors of the first and second components to shift regularly toward each other. Without being bound by theory, the inventors believe that the regularity of this shift is the main reason why the crimping of a free single fiber is regular. In contrast, according to the present invention, and without being bound by theory, the inventors believe that in fibers having a non-crimped cross-section, the shift between the internal contraction force vectors of the first and second components is not regular, and therefore the fiber forms an irregular bow or wave in any direction. In very simple terms, the fiber does not have a uniform tendency to bend toward its cross-section or any particular part of its periphery, resulting in an irregular final shape. After activation, the fiber cross-section remains almost non-crimped.
[0070] For example, a fabric according to the present invention may include a multi-component filament having an adhesive polymer on at least a portion of its surface. The adhesive polymer can be selected from the group consisting of polyolefins (i.e., polypropylene or polyethylene), low-melting-point polymers including low-melting-point polyester grades (i.e., aliphatic such as polylactic acid, or aromatic such as polyethylene terephthalate), copolymers, or blends of suitable polymers. It is within the scope of the present invention that the adhesive polymer consists of, or is basically composed of, plastics from the group of polyesters, such as polyester copolymer (coPET) or polylactic acid copolymer (COPLA).
[0071] For example, a fabric according to the present invention may include a multi-component filament containing a first polymer having a melting point higher than the melting point of the adhesive polymer, preferably with a melting point difference of at least 5°C. The first polymer can be selected from the group consisting of polyolefins (i.e., polypropylene or polyethylene), polyesters (i.e., aliphatic such as polylactic acid, or aromatic such as polyethylene terephthalate), copolymers, or blends of suitable polymers. It is within the scope of the present invention that the first polymer consists of, or is basically composed of, plastics from the group of polyesters, such as polyester copolymers (coPET) or polylactic acid copolymers (COPLA).
[0072] Preferred combinations of components for the two-component filament according to the present invention include polypropylene (PP) / polyethylene (PE), polyethylene terephthalate (PET) / PE, PET / PP, PET / copolyethylene terephthalate (CoPET), polylactic acid (PLA) / copolylactic acid (COPLA), PLA / PE, and PLA / PP.
[0073] For example, a fabric according to the present invention may contain multi-component filaments, preferably two-component filaments.
[0074] Fabrics according to the present invention can be formed from bulky vats, preferably from vats containing crimped filaments or filaments having potential crimp that can self-crimp under appropriate activation.
[0075] For example, a fabric according to the present invention may include multi-component filaments having a crimpable cross-section, preferably two-component filaments having a crimpable cross-section, and more preferably filaments having an eccentric core / sheath (eC / S) or sheath / sheath (S / S) cross-section. For example, some preferred combinations of eC / S cross-sections include: PP / PE, PET / PE, PLA / PE, PET / PP, PLA / PP, PP / coPP, PET / coPET, and PLA / coPLA, where the specified polymer forms at least 75% of the filament component.
[0076] For example, a fabric according to the present invention may contain, in its composition preferably, a multi-component filament having a non-crimped cross-section containing a shrinkable polymer, or a two-component filament having a core / sheath (C / S) cross-section containing polyester, preferably in the core. For example, some preferred combinations of C / S cross-sections include: PET / PE, PET / PP, PET / coPET, PLA / PE, PLA / PP, and PLA / coPLA, where the specified polymer forms at least 75% of the filament component.
[0077] While a hierarchical structure can be formed in certain cases without being bound by theory, the inventors believe that if the amount of adhesive polymer available on the surface of the filament is small, the formed adhesion will be too weak to hold in place and obtain the desired structure. On the other hand, if the filament contains too much adhesive polymer that melts during the bonding process, the remaining solid portion of the filament that does not melt will become too weak to maintain its structure and obtain the desired structure again when subjected to a heat flow.
[0078] For example, a fabric according to the present invention may contain at least 15% by weight of an adhesive polymer, preferably at least 18% by weight of an adhesive polymer.
[0079] For example, a fabric according to the present invention may contain up to 75% by weight of an adhesive polymer, preferably up to 80% by weight of an adhesive polymer.
[0080] Various amounts can be used for various polymer combinations. For example, a fabric according to the present invention having PP / PE filaments may contain at least 25% by weight of adhesive polymer, preferably at least 30% by weight of adhesive polymer, and more preferably at least 35% by weight of adhesive polymer. For example, a fabric according to the present invention containing PP / PE filaments may contain up to 75% by weight of adhesive polymer, preferably up to 70% by weight of adhesive polymer, and more preferably up to 65% by weight of adhesive polymer.
[0081] Furthermore, it should be noted that the adhesive polymer must be present on the filament surface. In the case of a core-sheath or eccentric core-sheath, the adhesive polymer must be part of the sheath, or preferably form part of the sheath.
[0082] For example, a fabric according to the present invention may contain an adhesive polymer that forms at least 20%, preferably at least 35%, and more preferably at least 50% of the filament surface area. The layered structure according to the present invention provides a balance between fabric resistance and softness / bulkiness.
[0083] For example, fabric durability is always necessary. Fabrics need sufficient durability to withstand the conversion process to the final product without being damaged, and further to withstand the use of the final product. Two very important aspects of durability are the surface stability of the fabric (resistance to fibers unraveling from the surface) and the delamination stability of the fabric (resistance to the top of the fabric tearing from the bottom). These two types of durability are often evaluated along with other durability such as abrasion resistance, and are assessed using the Martindale test method a set number of times, followed by a human evaluation of the results on a scale of 1 to 5. While this test is very suitable for setting a threshold with a binary pass / fail evaluation for a particular product, its scale is coarse, and the lack of additional information to compare the pass sample with the best result means it is not the best option for distinguishing in sufficient detail to explain the advantages of the present invention.
[0084] In other words, the tensile strength in the z-direction of a fabric is lower in layers with lower levels of inter-filament bonding. The tensile strength in the z-direction of a fabric can be measured, for example, in a delamination strength test. The fabric will tear at the weakest layer. If the delamination strength is too low, the fabric will not be stable enough, and under the load of conversion or normal operation, the fabric will delaminate and tear in layers, or delamination will occur only in specific areas where the delaminated parts are partially connected, leading to the formation of undesirable pilling. Similarly, even if the abrasion resistance of the fabric surface is very high, delamination can result in pilling or a so-called spiderweb effect appearing during the Martindale abrasion test, impairing the results.
[0085] Without being bound by theory, the inventors believe that in fabrics with a layered structure, the important numerical value representing resistance is peel strength. Fully bonded fabrics with no or low layered structure have good surface stability and high interlayer peel strength. Fabrics with a well-formed layered structure are characterized by good surface stability and moderate interlayer peel strength. Fabrics with a weak or non-existent layered structure and weak adhesion are characterized by being prone to surface collapse and having low interlayer peel / collapse strength.
[0086] For example, a fabric according to the present invention may include at least two different layers. In this case, the delamination strength is 0.5 N or more, preferably greater than 0.6 N, preferably greater than 0.7 N, and preferably greater than 0.8 N.
[0087] For example, the fabric according to the present invention may include at least two different layers, in which case the interlayer peel strength is 2.0 N or less.
[0088] The delamination force is the force required to separate the outer portion / outer layer of a nonwoven fabric along the weakest region within the fabric. When a fabric has a layered structure, delamination is said to occur at the layer with the lowest interlayer bonding density. In this specification, in typical nonwoven fabric compositions, the tensile strength of the adhesive polymer is lower than that of other polymers, meaning that the weakest point is usually the adhesive area, not the filament itself. This property is also very often influenced by the fiber cross-section. For example, the tensile strength of polyethylene as an adhesive polymer is lower than that of polypropylene or polyester. For instance, since the sheath is usually a relatively thin coating on the inner core, the adhesion between filaments in a core / sheath structure using polyethylene for the sheath is relatively weak. As a result, generally, cutting the adhesion between filaments is easier than cutting the filaments themselves. See Figures 15-19.
[0089] For example, bulkiness is one of the important characteristics. As mentioned above, the filament butt should be sufficiently bulky to allow the high-temperature fluid to flow properly during bonding, for example, during the air-through bonding process. Bulkiness is very important to human perception, and since fabrics often feel softer the bulkier they are, the final fabric should also be bulky. Layered structures provide bulkiness; for example, layer B is typically very bulky, increasing the overall bulkiness of the structure. On the other hand, the higher the filament bonding density level of one or more layers, the lower the overall bulkiness of the structure, and in extremely bulky structures, one or more outer layers may not be formed at all.
[0090] For example, the bulk density of the fabric according to the present invention is 60 kg / m². 3 Less than 58 kg / m 3 Less than 56 kg / m², more preferably 56 kg / m² 3 Less than, more preferably 54 kg / m 3 It is acceptable to be less than [a certain value].
[0091] For example, the bulk density of the fabric according to the present invention is 15 kg / m². 3 More preferably 20 kg / m 3Ultra, more preferably 25 kg / m 3 Ultra, most preferably 30 kg / m 3 It may even be more than that.
[0092] Bulkiness / bulk density represents the number of kilograms per cubic meter, so the smaller the value, the bulkier the material; at the same time, in order to represent the volume of 1 kilogram of fabric in liters, dm 3 It is possible to use the "thickness ratio to basis weight" of dm / kg or l / kg. The higher this value, the higher the bulkiness / bulk density.
[0093] For example, the thickness ratio to basis weight of the fabric according to the present invention may be at least 16.5 l / kg, preferably at least 17.0 l / kg, preferably at least 18.0 l / kg, more preferably at least 18.5 l / kg.
[0094] For example, the bulk density of the fabric according to the present invention may be at most 66 l / kg, preferably 50 l / kg or less, preferably 40 l / kg or less, more preferably 33 l / kg or less.
[0095] For example, the basis weight of the fabric according to the present invention may be at least 5 grams per square meter (gsm), preferably at least 10 gsm, more preferably at least 15 gsm.
[0096] For example, the basis weight of the fabric according to the present invention may be 200 gsm or less, preferably 150 gsm or less, more preferably 100 gsm or less.
[0097] For example, the recovery rate of the fabric according to the present invention may be at least 0.5 (which corresponds to a 50% recovery rate of the original thickness), preferably at least 0.6, more preferably at least 0.7, more preferably at least 0.8, most preferably at least 0.9.
[0098] For example, the resilience of the fabric according to the present invention may be at least 5%, preferably at least 10%, more preferably at least 13%, more preferably at least 15%, and more preferably at least 18%.
[0099] The above explanation of the hierarchical structure, as illustrated in the diagram, assumes that all filaments within the vat are uniformly laid out in three dimensions. Such uniformity is desirable for most nonwoven fabric applications. Non-uniformity is usually directly visible to the human eye. The fabric may appear denser / thicker in some areas and less dense / thinner / weaker in others. In extreme cases, the fabric may appear as dense islands separated from each other, connected by sparse filaments. However, even fabrics that a human observer perceives as uniform may have small areas of high and low density non-uniformity throughout the fabric's entire three-dimensional structure.
[0100] Crimped fibers typically arise from self-crimping, activated crimping, or completely controlled shrinkage, and tend to form characteristic structures with high-density and low-density regions. Specifically, certain regions form micro-aglomerates, while other regions retain relatively hollow microspaces. Microscale inspection of a fabric cross-section reveals that high-density regions can partially obscure layers with fewer filament bonds, and vice versa. See Figures 20A and 20B.
[0101] The object of the present invention is to explain the advantages of a hierarchical structure compared to a layer formation approach. As described above, a hierarchical structure can be formed with a single layer of nonwoven fabric; in other words, a hierarchical structure can be formed independently of the fabric layer.
[0102] The hierarchical structure can also be advantageously combined with layer formation. For example, a fabric according to the present invention consists of two or more filament layers, in which at least one outer layer of filaments can be constructed into at least one outer layer having a high level of inter-filament bonding density and at least one other layer having a low level of inter-filament bonding density.
[0103] As detailed above, a single layer can contain one, two, or more layers. Generally, one layer can form part of another layer, be equal to one layer, or contain even more layers. Within the scope of the present invention, a layered fabric can be considered that includes at least one layer having at least two layers.
[0104] For example, a fabric according to the present invention includes at least one layer of endless filaments, each having at least two layers.
[0105] For example, by combining multiple layers with different filament thicknesses and amounts of adhesive polymer, it is possible to achieve a fabric having a single surface with excellent abrasion resistance (provided by layers with finer fibers and more adhesive polymer) and overall bulkiness (provided by layers with coarser fibers and less adhesive polymer). This is illustrated, for example, in the patent application of Reifenhauser, European Patent Application No. 19189238.9 (unpublished).
[0106] For example, by combining multiple layers with different amounts of adhesive polymer on the filament surface, such as combining S / S filaments with C / S or eC / S filaments, it is possible to produce a fabric in which the soft loft properties provided by the filament layer with a low amount of adhesive polymer are improved, and the surface abrasion resistance of the filament with a high amount of adhesive polymer is extremely good.
[0107] Those skilled in the art may recognize various combinations of layers that take advantage of the hierarchical structure formed in part or in whole. The hierarchical filament layers can also be advantageously combined with one or more short fiber layers, films, etc.
[0108] Layer formation can also achieve specific hierarchical structures by exposing the vat to various heat sources. For example, a bulky fabric formed from two layers manufactured using two spinning beams, pre-compacted with hot air, and then bonded in a hot air oven can form a visible structure of five layers with alternating layers of high and low filament bonding density. See Figures 21 and 22.
[0109] Without being bound by theory, the inventors believe that an internal layer located between two layers with low inter-filament bonding density levels, and having a specific inter-filament bonding density level, can, in certain cases, be supported by pre-consolidation of the butt. Here, for example, a high-temperature fluid source (such as a hot air knife) located behind one, several, or each of the manufacturing beams and / or (depending on manufacturing needs) a second or any further high-temperature fluid source, along with a vacuum section installed below the belt, is installed to promote the formation of nuclei of high inter-filament bonding density, thereby increasing the probability of the formation of an internal layer structure with high inter-filament bonding density levels in the fabric.
[0110] Similar structures can also be manufactured by combining specific layers, for example. For instance, a two-layer fabric formed from crimpable fibers with different levels of inner filament crimping force (e.g., different filament cross-sections, different component ratios, different process settings that produce different potential crimping levels) allows the filaments to move independently in both layers, forming layers with high filament bonding density levels at the boundary regions between the layers on the surface of the layers, i.e., the surfaces of both fabrics.
[0111] A fabric according to the present invention can be manufactured from a vat containing a multi-component filament with a low-melting-point adhesive polymer on at least a portion of its surface. The vat on a moving belt is subjected to heat treatment. Heat can be transferred to the vat by a high-temperature fluid, such as hot air. In general, heat can be transferred into the vat at different stages of the manufacturing process, for example, immediately after laying the filaments on the belt and pre-compacting the structure, during the thermal activation process, during the bonding process, etc.
[0112] The high-temperature fluid enters the surface of the filament butt and flows around the filaments, transferring some of the heat it carries to the cooler filaments. Because some heat is transferred to the filaments on the butt surface, the temperature of the high-temperature fluid decreases slightly, and the temperature difference between the filaments and the high-temperature fluid also decreases. Those skilled in the art will notice that as the surface filaments gain heat, their temperature increases, and the temperature difference between the high-temperature fluid and the filaments decreases. With sufficient time and heat, all filaments within the fabric can be heated to a uniform temperature, resulting in uniform adhesion between fibers throughout the entire thickness of the fabric. The fabric can then be said to be uniformly, completely, or well-bonded.
[0113] Adhesion between filaments also depends on the local fluid resistance pressure strength; that is, the filaments may be in contact with each other or intersecting each other, and while some filaments may not form any adhesion or only weak adhesion, it should be noted that filaments in stronger contact will have stronger adhesion due to the molten low-melting-point polymer. The dynamic fluid resistance of the fabric, along the mainly vertical path of the high-temperature fluid flowing through the fabric, creates pressure as the high-temperature air flows through the fabric, which reduces the subsequent ability of the fluid to transfer temperature and energy, gradually decreasing from the initial point of impact with the exposed fabric surface toward the opposite side of the fabric. Here, as the fluid flows out of the fabric, the temperature and fluid velocity decrease, creating a difference in adhesion density in the cross-section of the fabric, and this difference becomes apparent in the formation of layers within the fabric layers.
[0114] Products according to the present invention are required to have non-uniform inter-filament bonding density across their entire thickness. The process setup and machinery used to produce such products from filament nonwoven vats must be able to supply the necessary hot air at a constant rate and temperature in both the CD and MD, which also means that the rate and temperature remain constant over time. This requirement applies to all hot air supply devices, such as hot air knives, hot air fields, hot bonding ovens with drums, flat belt ovens, or combinations of drum bonding and flat belt bonding.
[0115] A recommended configuration according to the present invention is a multi-component filament, or preferably a two-component filament, produced by spinning on a spinning machine or using a spinneret, and then preferably passed through a cooler. Inside the cooler, the filament is usually cooled by a fluid flow, mainly cold air. It is within the scope of the present invention to then pass the spun filament through a drawing mechanism, where it is processed by drawing. The drawn (stretched) filament is then accumulated on a moving belt, where a filament butt is formed. In one advantageous configuration, it is possible to create a butt-shaped filament with a controlled degree of potential shrinkage by adjusting specific parameters that determine the draw ratio. In other advantageous combinations, it is possible to set a crimpable filament cross section and then, by adjusting specific parameters that determine the draw ratio and cooling, create a butt-shaped filament that either self-crimps or has a desired level of potential crimp.
[0116] According to a preferred embodiment of the machinery and process configuration of the present invention, an integrated dispensing device is used as a magazine mechanism. This device controls the accumulation of filaments and is installed between the stretching mechanism and the filament accumulation position. It is within the scope of the present invention to use at least one dispensing device, the opposing side walls of which branch off from each other with respect to the direction of filament passage. A highly recommended embodiment of the configuration of the present invention is characterized in that the drive units of the cooling mechanism and the stretching mechanism are designed as a sealed system. Within this sealed system, no additional air source is added to supplement the supply of an external cooling medium or cold air to the cooling mechanism. Such a sealed system has been found to be particularly suitable for the manufacture of nonwoven fabrics.
[0117] In an example of manufacturing a nonwoven fabric according to the present invention using shrinkage, it was found that the technical solution according to the present invention, which resolves the problems associated with filament shrinkage, can be functionally reliable and effectively implemented by using the aforementioned unit, and in particular by using a dispensing device placed between the stretching mechanism and the filament accumulation position, in addition to a particularly preferred configuration. As already mentioned, the shrinkage of nonwoven vats manufactured by the spunbond method can be very clearly adapted or adjusted by parameters such as the draw ratio, cooling air / polymer ratio, and filament speed.
[0118] In an example of manufacturing a nonwoven fabric according to the present invention using self-crimping filaments, these filaments are released from aerodynamic stretching forces when they move away from a diffusion device located at the end of the stretching chamber, and are subsequently laid in a vacuum-supported fabric-forming region. Here, as soon as the vacuum force becomes the lowest at the end of the suction region—to MD—the filaments crimp, and such crimped filaments can increase the thickness of the resulting fabric.
[0119] To compact the filament orientation and three-dimensional structure, thereby giving the fabric vat thickness / bulk, a subsequent process is performed in which hot air is passed through the vat in one direction. The parameters for high-temperature fluid / hot air temperature, penetration rate, and volume are mainly as follows: - Total processing volume of spanmelt beams; - Fiber dimensions and polymer combinations - Line speed - Bat thickness - Fabric basis weight g / m 2 It depends on this and maintains the desired thickness without affecting the final parameter settings of the bonded fabric.
[0120] Since the above process steps can be reused multiple times by adding further spun melt beams with similar or different polymer combinations, fiber dimensions, and basis weights, it is preferable to also utilize a high-temperature fluid-assisted consolidation step on a common conveyor belt to obtain preliminary product characteristics prior to the final bonding step.
[0121] From the definition already stated, it is clear that manufacturing using the spunbond method consists of the direct conversion of polymers into filaments, which are then randomly spread at an accumulation site for the purpose of creating a nonwoven vat containing these filaments. The spunbond process determines the properties of both the individual filaments and the final nonwoven. The final manufactured nonwoven is not necessarily usable to determine the various properties and states of the individual filaments, such as the rheological properties, polymer structural properties, activated crimp, self-crimping level, and shrinkage that occur in the individual manufacturing steps of this nonwoven. The potential crimp or shrinkage of the nonwoven generally determines its ability to create bulky nonwovens. This ability is achieved by utilizing the crimp or shrinkage of individual filaments to increase the thickness of the filament vat, but nevertheless, the crimp or shrinkage occurs without the fabric structure collapsing and / or without significant changes in the length and width of the filament vat. The crimping / shrinkage of a filament is defined by using various raw materials in the composition of the filament, and / or by setting different material processing conditions during the manufacture of filaments for nonwoven fabrics, and / or by utilizing different filament cross-sectional shapes / arrangements, and / or by adjusting the mass ratios between various input materials, and / or by setting different filament orientations, which is within the scope of the present invention.
[0122] The recommended configuration of the present invention does not distinguish between filaments having a crimpable cross-section and filaments having a non-crimpable cross-section. Both types can be advantageously used for specific applications. Similarly, suitable combinations can be created by using crimped filament layers and non-crimped filament layers. It will be obvious to those with technical expertise that there are technical advantages to using filaments with a non-crimpable cross-section, in contrast to crimped filaments, in achieving bulky, flexible, and pliable materials.
[0123] The process according to the present invention may include one or more different bonding steps. See Figure 23. For example, one butt of filaments can be laid on a moving belt and bonded from one or both sides in a bonding unit located immediately behind the filament laying from the spinning beam.
[0124] For various reasons, increasing the distance between the filament spinning beam and the bonding unit can be advantageous. Multiple spinning beams are very often used for process reasons, such as forming layered structures or requiring filament butts to pass through gaps between the moving belt and the bonding unit. In such situations, common to spunmelt production lines, the butts need to be pre-compacted to increase their stability and withstand the manufacturing process prior to bonding. Additionally, thermal activation of latent crimp may be required before bonding, for example. Pre-compacting and / or activation can be performed using rolls (e.g., compression rolls), hot air (e.g., hot air knife (HAK), hot air field (HAF) units), thermal radiation (e.g., infrared pre-compacting), etc. To further illustrate, an example involving three different bonding steps will be selected to describe the process. It should be noted that the hierarchical structure of the present invention can also be formed by different manufacturing processes with different combinations of pre-compacting / activation and bonding units.
[0125] For example, one configuration of the present invention may include thermal pre-compacting of the filament bat, i.e., pre-compacting the filament bat and thermally forming adhesion. Another advantageous configuration of the present invention is thermal activation of the resulting nonwoven fabric for the purpose of controlling filament shrinkage and / or crimping in at least one layer. Preferably, compaction and, optionally, thermal activation are performed by at least one of the effects of contact with a high-temperature medium flow (e.g., by hot air or infrared irradiation) and / or contact with a high-temperature surface. Examples of such high-temperature surfaces mainly include parts of rollers. Thermal activation is preferably performed under conditions in which the action occurs uniformly across the entire surface of the fiber layer.
[0126] Thermal activation can be performed in a chamber supplied with hot air, or by passing a layer of filament through an oven. Thermal activation and compaction can also be performed by infrared, ultraviolet, transmission microwave, and / or laser irradiation. Within the scope of this described procedure performed "on the production line," it is important to emphasize that thermal compaction may be performed immediately after the completion of both the thermal activation and compaction procedures, either preceding the manufacturing procedure or, separately from the manufacturing procedure, "off the production line." Therefore, thermal activation can essentially be performed "off the production line," that is, at different times and locations.
[0127] In the solution according to the present invention, it is advantageous that a high-temperature medium flow passes through the fabric, and as a result, heat is transferred throughout the entire volume of the nonwoven fabric.
[0128] The required pre-consolidation of a filament fiber vat depends to a considerable extent on the conditions of the manufacturing process. A key prerequisite is to correctly set the level of filament binding between filaments within the filament vat, and therefore to be able to control the level of filament binding based on the requirements of subsequent steps in the manufacturing process. When the manufacturing process is carried out on a production line and activation is performed on the belt itself, the desired binding is relatively low, as it is only necessary to prevent collapse or thinning caused by highly undesirable movements during the activation process. In certain cases, for example, when the filaments bind very well on their own when in contact with each other or with the substrate, and this binding is made possible by, for example, the shape / arrangement of the cross-section, the rate of entanglement, or the material composition, the binding characteristics of the filament vat can be sufficiently good even without thermal pre-consolidation. In other examples, for example, when the manufacturing process is divided into two stages, or when the filament vat is pre-consolidated before being fully activated and transported, for example, in the form of a roll, a considerably high level of binding is required, and consequently, a considerably high level of pre-consolidation is also required. Anyone with specialized qualifications in this technical field and a thorough understanding of the manufacturing process conditions will be able to easily determine the required level of pre-consolidation in a particular case.
[0129] For example, when controlling shrinkage, the activation temperature should be within the range between the glass transition temperature and softening temperature (Vicat softening temperature according to ISO DIN 306) of one or more components A. A person with the necessary expertise in this art should be able to determine the optimal activation temperature for a given component composition.
[0130] Inside a convection cooling system, the filament is typically cooled by a flowing fluid, mainly cold air. As described above, the potential shrinkage or crimping of the filament needs to be uniformly distributed across the entire length, width, and thickness of the butt exhibiting shrinkage. While the properties related to the filament can be modified by adjusting the draw ratio, cooling air / polymer ratio, and filament speed, according to the present invention, these parameters are substantially the same for each individual filament.
[0131] The nonwoven fabric created is preferably made using a spinning beam. 1 The above is within the scope of the invention as it is produced by the spunbond method. At the same time, multiple layers may be stacked and piled up, and then these layers together into at least one forming belt 2 The mechanism for final consolidation is shown above. 3 It is clear that they will be transported to [location].
[0132] Spinner head 5 By spinning in this way, filaments 4 The filaments are prepared. The arrangement of the filaments may be optimized by alternating them, thereby achieving a state in which the weight of each individual filament is very similar and a supply of cold air at a very similar temperature is achieved. The spinneret has a variety of capillaries, and similarly, the diameter (d) and length (l) of these capillaries also vary. The length (l) is, in principle, calculated as a multiple of the capillary diameter, and in this application area, the length (l) is selected so that l / d is in the range of 2 to 10. The number of capillaries should be selected based on the desired final diameter of the filament, the desired or planned total amount of polymer processed, and the desired spinning rate of the filament. The number of capillaries may be varied in the range of 800 to 7000 per meter, and this number yields filaments with diameters in the range of 8 to 45 μm. The capillary diameter and filament rate are selected so that the potential shrinkage of the final filament is at the correct level. The filament speed should be in the range of 1000 to 10000 m / min, and for filaments with a cross-section that does not shrink and does not correspond to crimping, it should be in the range of 3000 to 5500 m / min. The diameter of the capillary tube should be selected in the range of 200 to 1000 μm, which allows for a suitable process draw ratio in the range of 200 to 1300 for circular capillaries. On the other hand, for these circular capillaries, a draw ratio in the range of 300 to 800 is most advantageous to achieve the desired level of productivity of the manufacturing line. Non-circular capillaries generally have a higher draw ratio, which largely depends on the shape of the capillary tube and the relative ratio of surface to volume.
[0133] The volume and temperature of the cold air are set in such a way that the draw ratio and cooling conditions are correct. In relation to the present invention, it has been found that a ratio of cold air volume to spun polymer in the range of 20:1 to 45:1 is useful. The volume and temperature of the cold air are controlled in the cooler (6). This temperature can be set in the range of 10°C to 90°C, preferably in the range of 15°C to 80°C, so as to use the cooling conditions in specific cases to control the shrinkage process. The cooling conditions determine how quickly the filament cools from its melting point to its glass transition point during the spinning process. For example, setting a higher cold air temperature slows down the cooling of the filament. In fact, for the purposes of the present invention, achieving the necessary and usable cold air temperature range is facilitated by dividing the cooler into two regions in which the temperature range can be controlled separately. The first region is located near the spinneret. 6a The temperature can be set in the range of 10°C to 90°C, preferably in the range of 15°C to 80°C, and most preferably in the range of 15°C to 70°C. In the second region (6b) located immediately adjacent to the first region, the temperature can be set in the range of 10°C to 80°C, preferably in the range of 15°C to 70°C, and most preferably in the range of 15°C to 45°C.
[0134] Then, the filament is stretched in the region 7 This section describes how the filament is stretched using the tensile force generated by the cold air velocity effect. A specific air velocity is obtained by adjusting the cold air volume and the adjustable shape of the stretching area, and this velocity is transmitted to the filament velocity. This filament velocity then determines the filament diameter along with the amount of polymer processed. Potential shrinkage / reduction is controlled by the filament velocity, draw ratio, and cooling air / polymer ratio.
[0135] In the next step, the filament is diffused in a diffusion device. 8 Send to. Diffusion device 8 The opposing walls of the structure branch off from each other with respect to the direction of filament movement. The positions of these walls can be adjusted in a manner that allows for the acquisition of a nonwoven fabric with a uniform composition in which individual integrated filaments are arranged in all directions on the MD / CD plane.
[0136] At the same time, it is clear that the accumulating filament vat is affected by air due to its effect of sending these filaments to the diffusion device. The airflow can be adapted in such a way that it forms various arrangements, from obviously zigzag filament accumulations to circular loops, and even elliptical structures oriented in the CD direction. The filaments accumulate on the forming belt and at least one mechanism for pre-consolidation. 9 The filaments are transported to the processing area. Cold air flows through the filament accumulation vat, through the forming belt, and then away from the processing area. The volume of the suctioned air can be adjusted in a manner that facilitates filament accumulation and ensures effective contact between the filament vat and the forming belt. The pre-consolidation mechanism is located near the diffusion device. The formation of the filament vat is controlled by the suctioned air throughout the entire path between the diffusion device and the pre-consolidation mechanism. Pre-consolidation of the filament vat is performed with hot air.
[0137] The amount of energy transferred to the filament butt is controlled by process parameters that only soften or pre-melt the filaments to a certain extent. This ensures good bonding between individual filaments. After the required bonding between filaments is achieved, the fiber butt can be transported on the forming belt without the need for additional auxiliary mechanisms and without the risk of breakage / damage due to the forces generated during transport. This pre-consolidation procedure is also sufficient to move filament butts to different accumulation areas on a production line consisting of multiple spinning beams. The energy transferred to the filaments may not be sufficient to activate the shrinkage of these filaments.
[0138] The method according to the present invention includes determining the balance between pre-consolidation parameters: pre-consolidation temperature, pre-consolidation air velocity, and pre-consolidation time. It is understood that the pre-consolidation time is the time for modifying the filament vat with pre-consolidated air.
[0139] The pre-consolidation time for the filament vat is recommended to be in the range of 1 to 10,000 ms, preferably 2 to 1,000 ms, and most preferably 4 to 200 ms.
[0140] The velocity of the pre-consolidated air used in this pre-consolidation unit is set to a range of 0.1 to 10 m / s, preferably 0.8 to 4 m / s. The consolidation temperature during pre-consolidation is recommended to be in the range of 80°C to 200°C, preferably 100°C to 180°C. In one configuration, this pre-consolidation temperature is in the range of 90°C to 150°C, mainly 110°C to 140°C.
[0141] One advantageous configuration in the area of the manufacturing line where the diffusion device is located is a filament vat with at least one activation unit. 10 The filaments are transported to a location where they are activated by hot air. It is understood that the actual crimping or shrinkage of the shrinkable component of the filaments is a function of temperature, and similarly, a function of the duration of the temperature-affected period. Furthermore, it is clear that the rate of the crimping / shrinkage process also depends on temperature. As a result of this control of the process, a bundled, uniform structure of the nonwoven fabric with reduced filament density is achieved, which similarly leads to an increase in the thickness of this nonwoven fabric.
[0142] According to one embodiment of the present invention, the execution of the pre-consolidation and activation method, the pre-consolidation and / or activation time during the process, the wind speed required for pre-consolidation and / or activation, and the temperature for pre-consolidation and activation are controlled by a combined method in a combined mechanism for pre-consolidation and activation.
[0143] One advantageous method according to the present invention involves determining the balance between activation parameters: activation temperature, activation air velocity, and activation time. It is understood that activation time is the time for which the filament vat is modified with activated air. It is clear that these parameters may be modified within a specific range depending on the potential shrinkage level of the filament, and similarly, for the purpose of setting an ideal combination of activation time, activation temperature, and activation air velocity.
[0144] The activation time of the filament bat is recommended to be in the range of 20 to 5000 ms, preferably in the range of 30 to 3000 ms, and most preferably in the range of 50 to 1000 ms.
[0145] The velocity of the activated air used in this activation unit is set to a range of 0.1 to 2.5 m / s, preferably 0.3 to 1.5 m / s. The activation temperature during thermal activation is recommended to be in the range of 80°C to 200°C, preferably 100°C to 160°C. In one configuration, this activation temperature is in the range of 90°C to 140°C, mainly 110°C to 130°C.
[0146] One embodiment of the present invention may include one or more gaps between a plurality of manufacturing units or a plurality of processing units. When releasing a spare fabric or vat from a conveyor belt along an MD fabric path, it is advantageous to perform this release by minimizing the possible pre-speed difference between the conveyor belt and the first friction point downstream in order to maintain the overall shape and dimensions, in particular the original thickness, and the original tactile properties, such as the soft surface of the fabric or vat, without altering them.
[0147] The characteristics of the final product may also depend on the tension that needs to be applied to release the pre-consolidated butt from the conveyor belt and from each active moving surface in the machine direction, also known as a friction point.
[0148] In particular, the tension released from the conveyor belt can sometimes be important.
[0149] While controlled tension is typically described as force per linear fabric dimension and its elongation in the width direction, a method of "interpreting" tension by the velocity difference between two downstream adjacent friction points is accepted from the perspective of the process of defining and controlling parameter settings.
[0150] Since this primarily depends on the fabric weight, line speed, and surface friction between the fabric and the support surface, setting the speed difference is a direct way to adjust the active drive surface speed.
[0151] For example, in a process according to the present invention, the speed difference between the conveyor belt and the suction drum of the air-through bonding unit may be less than 1.0%; more preferably less than 0.5%, and even more preferably less than 0.3%. A speed difference of less than 1.0% means that the speed of the second device may be in the range of +1.0% to -1.0%.
[0152] One embodiment according to the present invention includes a conveyor belt (2), and this embodiment is carried out under conditions that the fabric strength of the nonwoven fabric bat in the mechanical direction (MD) is 0.5 to 5 N / 5 cm, preferably 0.7 to 3.5 N / 5 cm, and more preferably 0.8 to 3.5 N / 5 cm, before the nonwoven fabric bat is transferred from the pre-consolidation process to the consolidation unit (3).
[0153] One embodiment according to the present invention includes a conveyor belt (2), and this embodiment is carried out under conditions that the fabric strength of the nonwoven fabric bat in the mechanical direction (MD) is greater than 6 N / 5 cm, preferably greater than 8 N / 5 cm, and more preferably greater than 10 N / 5 cm, before the nonwoven fabric bat is transferred from the pre-consolidation process to the consolidation unit (3).
[0154] One embodiment of the present invention includes an intermediate cooling between the pre-consolidation step and the final consolidation step. For example, the nonwoven vats in between the steps can be exposed to a cooling medium, preferably air at a temperature of 70°C or lower, preferably 60°C or lower, and most preferably 55°C or lower. For example, intermediate cooling may be carried out by exposing the pre-consolidated vats to ambient air. Without being bound by theory, the inventors believe that intermediate cooling, in particular by heating at least one surface of the nonwoven fabric during pre-consolidation, exposing it to a low temperature, and then heating it during the consolidation step, is advantageous for forming a denser outer layer.
[0155] An advantageous configuration according to the present invention includes a final compaction procedure, which consists of modifying the filament vat using hot air in a compaction mechanism (3). In this compaction mechanism, the filament vat is compacted into a cloth in which filament adhesion is formed. This compaction can be achieved by various devices, such as a compaction mechanism equipped with a bell-shaped drum, a compaction mechanism equipped with a flat belt, or a compaction mechanism equipped with multiple drums. Thermoplastic polymers and their blends are characterized by the phenomenon that, when exposed to heat, they exhibit a gradual increase in plastic softening (viscosity reduction) between the glass transition point (where all amorphous parts begin to soften) and the melting point (where all crystalline parts melt). The melting point is usually in a very narrow temperature range (maximum 2.0°C) and is defined by the homopolymer or copolymer used. In the case of polymer blends, the narrow temperature range can be determined when the polymer blend becomes tacky and can form filament adhesion.
[0156] An advantageous configuration according to the present invention includes a final consolidation procedure performed using at least three different consolidation sections. Essentially, the airflow is nearly perpendicular to the fabric and maintains a uniform flow with minimal temperature and volume fluctuations.
[0157] The first compaction section preheats the fabric to a temperature close to, but below, the melting point of the adhesive polymer. Preferably, the temperature is set to 5 to 20°C lower than the melting point of the adhesive polymer. More preferably, the temperature is set to 5 to 15°C lower than the melting point of the adhesive polymer; advantageously, the temperature is set to 5 to 10°C lower than the melting point of the adhesive polymer. Advantageously, in the first compaction section, the direction of heat flow is alternately changed from the first outer surface and the second outer surface of the fabric.
[0158] In the second consolidation section, the melting point range of the low-temperature molten polymer composition is narrowed to enable fusion formation. On the other hand, the temperature set considering the basis weight of the fabric, fiber dimensions, and cross-sectional ratio between constituent polymers is in a range of up to 5.0°C lower and up to 3.0°C higher than the melting point of the adhesive polymer. For example, if the melting point is 130°C, the set temperature is preferably in the range of 125°C (130-5) to 133°C (130+3). Preferably, the temperature is set in a range from 5°C lower than the melting point of the adhesive polymer to the same temperature as the melting point of the adhesive polymer. More preferably, the temperature is set in a range of 4°C to 1°C lower than the melting point of the adhesive polymer. Advantageously, in the second consolidation section, heat flows alternately from the direction of the first and second outer surfaces of the fabric.
[0159] The third compaction section is a cooling section, which significantly cools the air to a temperature of preferably 10-40°C, more preferably 20-30°C. Ambient air can also be used. The cooling section helps to solidify the filaments or at least the filaments on the fabric surface, fixing the layered structure formed in the fabric. It is advantageous not to apply excessive tension immediately before and during the cooling process. It is advantageous to be able to perform another cooling process behind the compaction unit. This further cooling can be performed by an additional airflow, cooling rolls, etc. It is advantageous to perform further cooling when the temperature of the fabric that has left the third compaction section has not yet reached the ambient temperature. It is advantageous for the fabric to reach the ambient temperature, preferably 40-10°C, more preferably 20-30°C. The described process produces bulky, soft, and low-linting nonwoven fabrics at high processing volume and high production speed for economic reasons.
[0160] For example, in one embodiment according to the present invention, a high-temperature air-through consolidation apparatus equipped with four drums can be used. This apparatus enables a process that fully exposes the fabric to the desired hot air flow and volume along the maximum fabric path in order to achieve a low-viscosity molten flow necessary to form a fusion within a defined narrow parameter range, as well as high speed and short residence time. With the drums oriented in the mechanical direction, the contact angle is at least 100°, preferably at least 130°, more preferably at least 150°, and advantageously at least 160°.
[0161] The precise parameter setting range of the selected device depends on the selected adhesive polymer, filament dimensions, filament cross-section, and the mass ratio between the polymer component formulations.
[0162] The aforementioned four-drum apparatus also allows for the rapid flow of alternating, nearly vertical, strong hot air onto the substrate. The first pair of drums is positioned to preheat the fabric structure to a temperature just below the softening and melting points of the low-melting-point polymer composition. The second pair of drums is positioned so that the melting point range of the low-melting-point polymer composition allows for the formation of fusion. To maintain the fabric structure and preserve the fusion, the final drum is equipped with a high-temperature section and a cooling section along the circumference in the machine direction. It is advantageous to solidify the fabric structure, or at least the surface of the fabric structure, before releasing the fabric from the consolidator. A separate additional cooling roll with a high-flow cold air passing through the fabric is positioned as close as possible to the last roll of the air-through adhesive consolidator. This air-through adhesive consolidator completes the fabric solidification with immediate cooling.
[0163] The compacted nonwoven fabric is wound onto a spool (11) in the final stage. If it is necessary to modify the surface properties of the nonwoven fabric, for example, to improve fluid permeability or fluid discharge capacity, a spray mechanism or dip roll is placed either between the moving belt and the final compaction mechanism, or between the final compaction mechanism and the spool.
[0164] One embodiment of the present invention consists of a combination of activation and consolidation steps, in which the activation time and / or consolidation time, the air velocity required for activation and / or consolidation, and the activation and / or consolidation temperature are controlled within the consolidation mechanism.
[0165] Consolidation parameters: Determining the balance between consolidation temperature, consolidation air velocity, and consolidation time is a crucial factor. Consolidation time is understood to mean the time it takes for the filament vat to be modified by the consolidation air. It is clear that these parameters may be modified within specified ranges, in relation to the potential consolidation level of the filament vat, as well as to achieve an ideal combination of consolidation time, consolidation temperature, and consolidation air velocity.
[0166] The compaction time for the filament vat is recommended to be in the range of 200 to 20,000 ms, preferably in the range of 200 to 15,000 ms, and most preferably in the range of 200 to 10,000 ms.
[0167] The velocity of the consolidated air used in this consolidation unit is set to a range of 0.2 to 4.0 m / s, preferably 0.4 to 1.8 m / s. The consolidation temperature during hot consolidation is recommended to be in the range of 100°C to 250°C, preferably 120°C to 220°C. In one configuration, this consolidation temperature is in the range of 90°C to 140°C, mainly 110°C to 130°C.
[0168] Examples Further details and specific features of the present invention will be described below based on examples. These examples illustrate the practical application of the present invention, but are not intended to be limiting. It will be apparent to those skilled in the art that additional embodiments and modifications fall within the claimed scope of the present invention. Accordingly, the scope of the present invention is defined by the appended claims.
[0169] The examples were manufactured using the R5 spunmelt production line manufactured by Reifenhauser Reicofil GmbH & Co. KG. This production line is equipped with two spunbond beams (A and D), each adapted to produce two-component filaments. In Example 1, only one of the spunbond beams was used, but in Examples 2 to 13, both beams were used. The first layer was formed by laying filaments from the first beam onto a moving belt, and the second layer of the vat was formed by laying filaments from the second beam on top of it. The vat was pre-consolidated with hot air behind each beam. Thus, one layer was pre-consolidated behind the first beam, and both layers were pre-consolidated together behind the second beam. The resulting two-layer vat was transferred to an air-through bonding unit equipped with four drums. The vat was air-through bonded from the first side by the first drum, then from the second side by the second drum, then again from the first side by the third drum, and again from the second side by the fourth drum. The first two drums constitute the first compaction section, while the third drum and part of the fourth drum constitute the second compaction section. Cooling of the nonwoven fabric begins in the fourth drum (third compaction section), where most of its contact surface is used for the final stage of hot air-through bonding (second compaction section), and the final portion—corresponding to the 30° contact surface of the drum—is used for the first stage of fabric cooling, i.e., the air-through cooling stage (i.e., the last surface in contact with the nonwoven fabric just before it leaves the air-through bonding unit is used for initial fabric cooling). The resulting nonwoven fabric is further cooled by air immediately after leaving the air-through bonding unit. Specific features of the manufacturing example are defined below, and the obtained features of the manufacturing example are specified in the table below.
[0170] Example 1 - Invention The first beam produced a filament butt, in which each filament had a core / sheath structure (non-curved cross-section). The core formed 70% by weight of the filament and contained polyethylene terephthalate (type 5520, manufactured by Invista), while the sheath formed 30% by weight of the filament and contained polyethylene (Aspun 6834, manufactured by Dow Chemicals).
[0171] The second beam had its power turned off.
[0172] The processing rate of the first beam was 220 kg / h per meter of beam width.
[0173] The air-through bonding unit was set to 121°C for the first and second drums, 127°C for the third drum and most of the fourth drum, and the remaining portion of the fourth drum (the remaining portion corresponding to the 30° contact surface of the drum) was set to 24°C using ambient air.
[0174] The resulting nonwoven fabric is 75 gsm thick, and its cross-section clearly shows a layered structure (as shown in the figure). The denser layers A and C form the outer surface of the fabric, while the hollow, very bulky intermediate layer B provides the fabric with bulk. The layers may or may not be uniformly formed. For example, in this specification, layer A is much thicker than layer C. See Figure 24.
[0175] TIFF2023547228000002.tif182136
[0176] Example 2 - Invention The first beam produced the first layer of a filament having an eccentric core / sheath structure, in which the core formed 40% by weight of the filament and contained a polypropylene blend (Exxonmobil 3155 type, Borealis HG475FB type, white colorant TiO2, and erucamide), and the sheath formed 60% by weight of the filament and contained polyethylene (Aspun 6850, Dow Chemicals).
[0177] The second beam produced a second layer of filaments with a parallel structure, where each parallel section formed 50% by weight of the filament. One parallel section contained a polypropylene blend (Exxonmobil 3155 type, Borealis HG475FB type, white colorant TiO2, and erucamide), while the second parallel section contained polyethylene (Aspun 6850, Dow Chemicals).
[0178] The processing rate of the first beam was 160 kg / h per meter of beam width, and the processing rate of the second beam was 240 kg / h per meter of beam width.
[0179] The air-through bonding unit was set to 125°C for the first and second drums, 129°C for the third drum and most of the fourth drum, and the remaining portion of the fourth drum (the remaining portion corresponding to the 30° contact surface of the drum) was set to 24°C using ambient air, and a cooling unit was placed behind the consolidation unit in the MD.
[0180] The resulting nonwoven fabric was 25 gsm thick, and its layered structure was clearly visible.
[0181] The hierarchical structure was determined using three different methods: 1) Cross-sectional observations were performed using SEM microscopy. Recognizing the outer layers A and C, and the inner layer B, was easy. However, because SEM microscopy views the "inside" of the fabric, determining inter-filament bonding and adhesion, and measuring cavities, can be very complex in some cases (Figure 25). 2) The nonwoven fabric was fixed in the resin and a cross-section was prepared. When only the cross-section is viewed, the filaments are visible as black dots (because they are randomly oriented at this microscale). It is clear that the filaments (dots) are quite dense in layers A and C, and that cavities are formed in the inner layer B (Figure 26). 3) The nonwoven fabric was analyzed by X-ray tomography to improve the spatial resolution of the fabric / filament in the X-ray images. The sample was metallized using the same method as with SEM microscopy. A 3D model of the fabric was created on a computer (Figure 27), and it was digitally cut into 2D cross-sections of the fabric (Figure 28). Metallized filaments are shown as white dots (the size of the white area may be influenced by the amount of metal on the filament surface). Areas where filaments are close to each other (high-density areas) may also be represented by white areas. Here, layers A and C, as well as the inner layer B, are very clearly visible.
[0182] All three methods described above clearly demonstrated the formation of a layered structure within the sample. Furthermore, the different appearances in different parts of the fabric sample revealed that the inner layer B may be formed near one fabric surface, in the center, or near another fabric surface. (Especially in the SEM images) it is clear that the inner layer is not necessarily formed at layer / layer boundaries. In addition, the fabric properties shown in the table demonstrate a good combination of the sample's durability and softness.
[0183] Examples 3-5 - Inventive Step Examples 3, 4, and 5 are almost identical to Example 2. Examples 3, 4, and 5 differ in basis weight and filament thickness (due to different settings before filament laying). The bonding process settings were also the same as in Example 2. The layered structure was clearly visible (see fabric cross-section diagram in the figure). The fabric characteristics are shown in the table.
[0184] TIFF2023547228000003.tif209141
[0185] Example 6 - Inventive Step The first beam produced the first layer of a filament having an eccentric core / sheath structure, in which the core formed 40% by weight of the filament and contained a polypropylene blend (Exxonmobil 3155 type, Borealis HG475FB type, white colorant TiO2, and erucamide), and the sheath formed 60% by weight of the filament and contained polyethylene (Aspun 6850, Dow Chemicals).
[0186] The second beam produced a second layer of filaments having a parallel structure, in which each parallel section formed 50% by weight of the filament. One parallel section contained a polypropylene blend (Exxonmobil 3155 type, Borealis HG475FB type, and the white coloring agent TiO2), while the second parallel section contained polyethylene (Aspun 6850, Dow Chemicals).
[0187] The processing rate of the first beam was 120 kg / h per meter of beam width, and the processing rate of the second beam was 240 kg / h per meter of beam width.
[0188] The air-through bonding unit was set to 124°C for the first and second drums, 128°C for the third drum and most of the fourth drum, and the remaining portion of the fourth drum (the remaining portion corresponding to the 30° contact surface of the drum) was set to 24°C using ambient air, and a cooling unit was placed behind the consolidation unit in the MD.
[0189] The resulting nonwoven fabric was 25 gsm thick, and its layered structure was clearly visible.
[0190] Example 7 - Inventive Step The first beam produced the first layer of a filament having an eccentric core / sheath structure, in which the core formed 40% by weight of the filament and contained a polypropylene blend (Exxonmobil 3155 type, Borealis HG475FB type, white colorant TiO2, and erucamide), and the sheath formed 60% by weight of the filament and contained polyethylene (Aspun 6850, Dow Chemicals).
[0191] The second beam produced a second layer of filament having a parallel structure, in which the first parallel section formed 75% by weight of the filament. The first parallel section contained a polypropylene blend (Exxonmobil 3155 type, Borealis HG475FB type, white colorant TiO2, and erucamide), while the second parallel section formed 25% by weight of the filament and contained polyethylene (Aspun 6834, Dow Chemicals).
[0192] The processing rate for the first beam was 220 kg / hour per meter of beam width, and the processing rate for the second beam was 240 kg / hour per meter of beam width.
[0193] The air-through bonding unit was set to 117°C for the first and second drums, 123°C for the third drum and most of the fourth drum, and the remaining portion of the fourth drum (the remaining portion corresponding to the 30° contact surface of the drum) was set to 24°C using ambient air, with a cooling unit positioned behind the consolidation unit in the MD.
[0194] The resulting nonwoven fabric had a thickness of 55 gsm, and its layered structure was clearly visible.
[0195] Example 8 - Inventive Step The first beam produced the first layer of a filament having an eccentric core / sheath structure, in which the core formed 40% by weight of the filament and contained a polypropylene blend (Exxonmobil 3155 type, Borealis HG475FB type, white colorant TiO2, and erucamide), and the sheath formed 60% by weight of the filament and contained polyethylene (Aspun 6850, Dow Chemicals).
[0196] The second beam produced a second layer of filament having a parallel structure, in which the first parallel section formed 50% by weight of the filament. The first parallel section contained a polypropylene blend (Exxonmobil type 3155, Borealis type HG475FB, white colorant TiO2, and erucamide), while the second parallel section, which formed 50% by weight of the filament, contained polyethylene (Aspun 6834, Dow Chemicals).
[0197] The processing rate for the first beam was 120 kg / hour per meter of beam width, and the processing rate for the second beam was 240 kg / hour per meter of beam width.
[0198] The air-through bonding unit was set to 125°C for the first and second drums, 129°C for the third drum and most of the fourth drum, and the remaining portion of the fourth drum (the remaining portion corresponding to the 30° contact surface of the drum) was set to 24°C using ambient air, and a cooling unit was placed behind the consolidation unit in the MD.
[0199] The resulting nonwoven fabric was 25 gsm thick, and its layered structure was clearly visible.
[0200] Example 9 - Inventive Step The first beam produced the first layer of a filament having an eccentric core / sheath structure, in which the core formed 50% by weight of the filament and contained a polypropylene blend (Exxonmobil 3155 type, Borealis HG475FB type, white colorant TiO2, and erucamide), and the sheath formed 50% by weight of the filament and contained polyethylene (Aspun 6850, Dow Chemicals).
[0201] The second beam produced a second layer of filament having a parallel structure, in which the first parallel section formed 50% by weight of the filament. The first parallel section contained a polypropylene blend (Exxonmobil type 3155, Borealis type HG475FB, white colorant TiO2, and erucamide), while the second parallel section, which formed 50% by weight of the filament, contained polyethylene (Aspun 6834, Dow Chemicals).
[0202] The processing rate of the first beam was 160 kg / h per meter of beam width, and the processing rate of the second beam was 240 kg / h per meter of beam width.
[0203] The air-through bonding unit was set to 124°C for the first and second drums, 129°C for the third drum and most of the fourth drum, and the remaining portion of the fourth drum (corresponding to the remaining 30° contact surface of the drum) was set to 24°C using ambient air. A cooling unit was also placed behind the consolidation unit in the MD.
[0204] The resulting nonwoven fabric was 22 gsm thick, and its layered structure was clearly visible.
[0205] Example 10 - Inventive Step The first beam produced the first layer of a filament having an eccentric core / sheath structure, in which the core formed 50% by weight of the filament and contained a polypropylene blend (Exxonmobil 3155 type, Borealis HG475FB type, white colorant TiO2, and erucamide), and the sheath formed 50% by weight of the filament and contained polyethylene (Aspun 6850, Dow Chemicals).
[0206] The second beam produced a second layer of filament having a parallel structure, in which the first parallel section formed 50% by weight of the filament. The first parallel section contained a polypropylene blend (Exxonmobil type 3155, Borealis type HG475FB, white colorant TiO2, and erucamide), while the second parallel section, which formed 50% by weight of the filament, contained polyethylene (Aspun 6834, Dow Chemicals).
[0207] The processing rate of the first beam was 200 kg / h per meter of beam width, and the processing rate of the second beam was 240 kg / h per meter of beam width.
[0208] The air-through bonding unit was set to 124°C for the first and second drums, 131°C for the third drum and most of the fourth drum, and the remaining portion of the fourth drum (the remaining portion corresponding to the 30° contact surface of the drum) was set to 24°C using ambient air, and a cooling unit was placed next to the consolidation unit in the MD.
[0209] The resulting nonwoven fabric had a thickness of 65 gsm, and its layered structure was clearly visible.
[0210] TIFF2023547228000004.tif244151
[0211] It should be noted that Examples 9 and 10 exhibit low tensile and adhesive strengths, and therefore may be considered to have weak adhesion in many applications. However, even in these cases, a highly durable layered structure is formed on the outer fabric surface.
[0212] In the multilayer examples above, a combination of eC / S and S / S filaments is used, but it should be noted that this combination is not important to the present invention, even if it may offer advantages. Example 11 below shows a two-layer fabric in which both layers are formed from filaments having an eC / S cross-section.
[0213] Example 11 - Inventive Step The first beam produced the first layer of a filament having an eccentric core / sheath structure, in which the core formed 60% by weight of the filament and contained a polypropylene blend (Exxonmobil 3155 type, Borealis HG475FB type, white colorant TiO2, and erucamide), and the sheath formed 40% by weight of the filament and contained polyethylene (Aspun 6850, Dow Chemicals).
[0214] The second beam produced a second layer of filament with an eccentric core / sheath structure, in which the core formed 50% by weight of the filament. The core contained a polypropylene blend (Exxonmobil 3155 type, Borealis HG475FB type, white colorant TiO2, and erucamide), and the sheath formed 50% by weight of the filament and contained polyethylene (Aspun 6834, Dow Chemicals).
[0215] The processing rate of the first beam was 120 kg / h per meter of beam width, and the processing rate of the second beam was 240 kg / h per meter of beam width.
[0216] The air-through bonding unit was set to 124°C for the first and second drums, 129°C for the third drum and most of the fourth drum, and the remaining portion of the fourth drum (corresponding to the remaining 30° contact surface of the drum) was set to 24°C using ambient air. A cooling unit was also placed behind the consolidation unit in the MD.
[0217] The resulting nonwoven fabric was 25 gsm thick, and its layered structure was clearly visible.
[0218] TIFF2023547228000005.tif163124
[0219] Example 12 - Inventive Step The first beam produced the first layer of a filament having an eccentric core / sheath structure, in which the core formed 50% by weight of the filament and contained a polypropylene blend (Exxonmobil 3155 type, Borealis HG712FB type, white colorant TiO2, and erucamide), and the sheath formed 50% by weight of the filament and contained polyethylene (Aspun 6834, Dow Chemicals).
[0220] The second beam produced a second layer of filament having a parallel structure, in which the first parallel section formed 50% by weight of the filament. The first parallel section contained a polypropylene blend (Exxonmobil type 3155, Borealis type HG712FB, white colorant TiO2, and erucamide), while the second parallel section, which formed 50% by weight of the filament, contained polyethylene (Aspun 6834, Dow Chemicals).
[0221] The processing rate of the first beam was 160 kg / h per meter of beam width, and the processing rate of the second beam was 240 kg / h per meter of beam width.
[0222] The air-through bonding unit was set to 120°C for the first and second drums, 128°C for the third drum and most of the fourth drum, and the remaining portion of the fourth drum (corresponding to the remaining 30° contact surface of the drum) was set to 24°C using ambient air, and a cooling area was placed behind the consolidation unit in the MD.
[0223] The resulting nonwoven fabric was 35 gsm thick, and its layered structure was clearly visible.
[0224] Example 13 - Inventive Step The first beam produced the first layer of a filament having an eccentric core / sheath structure, in which the core formed 40% by weight of the filament and contained a polypropylene blend (Exxonmobil 3155 type, Borealis HG712FB type, white colorant TiO2, and erucamide), and the sheath formed 60% by weight of the filament and contained polyethylene (Aspun 6850, Dow Chemicals).
[0225] The second beam produced a second layer of filament having a parallel structure, in which the first parallel section formed 50% by weight of the filament. The first parallel section contained a polypropylene blend (Exxonmobil type 3155, Borealis type HG712FB, white colorant TiO2, and erucamide), while the second parallel section, which formed 50% by weight of the filament, contained polyethylene (Aspun 6834, Dow Chemicals).
[0226] The processing rate of the first beam was 120 kg / h per meter of beam width, and the processing rate of the second beam was 240 kg / h per meter of beam width.
[0227] The air-through bonding unit was set to 123°C for the first and second drums, 128°C for the third drum and most of the fourth drum, and the remaining portion of the fourth drum (the remaining portion corresponding to the 30° contact surface of the drum) was set to 19°C using ambient air, and a cooling area was placed behind the consolidation unit in the MD.
[0228] The resulting nonwoven fabric was 25 gsm thick, and its layered structure was clearly visible.
[0229] Example 14 - Inventive Step The first beam produced the first layer of a filament having an eccentric core / sheath structure, in which the core formed 50% by weight of the filament and contained a polypropylene blend (Exxonmobil 3155 type, Borealis HG712FB type, white colorant TiO2, and erucamide), and the sheath formed 50% by weight of the filament and contained polyethylene (Aspun 6850, Dow Chemicals).
[0230] The second beam produced a second layer of filament having a parallel structure, in which the first parallel section formed 50% by weight of the filament. The first parallel section contained a polypropylene blend (Exxonmobil type 3155, Borealis type HG712FB, white colorant TiO2, and erucamide), while the second parallel section, which formed 50% by weight of the filament, contained polyethylene (Aspun 6834, Dow Chemicals).
[0231] The processing rate of the first beam was 140 kg / h per meter of beam width, and the processing rate of the second beam was 240 kg / h per meter of beam width.
[0232] The air-through bonding unit was set at 124°C for the first and second drums, 129°C for the third drum and most of the fourth drum, and the remaining part of the fourth drum (the remaining part corresponding to the 30° contact surface of the drum) was set at a temperature of 21°C using ambient air, and a cooling area was arranged behind the consolidation unit in the MD direction.
[0233] The obtained non-woven fabric was 20 gsm and had a well-visible layered structure.
[0234] Example 15 - Inventive Step The first beam produced the first layer of filaments with an eccentric core / shell structure. In this first layer, the core formed 50% by weight of the filaments and contained a polypropylene blend (type 3155 from Exxonmobil, type HG712FB from Borealis, white colorant TiO2, and erucamide), and the shell formed 50% by weight of the filaments and contained polyethylene (Aspun 6850, from Dow Chemicals).
[0235] The second beam produced the second layer of filaments with a parallel structure. In this second layer, the first parallel part formed 50% by weight of the filaments. The first parallel part contained a polypropylene blend (type 3155 from Exxonmobil, type HG712FB from Borealis, white colorant TiO2, and erucamide), and the second parallel part formed 50% by weight of the filaments and contained polyethylene (Aspun 6834, from Dow Chemicals).
[0236] The throughput of the first beam was 140 kg / h per meter of the width of the first beam, and the throughput of the second beam was 240 kg / h per meter of the width of the second beam.
[0237] The air-through bonding unit was set to 124°C for the first and second drums, 129°C for the third drum and most of the fourth drum, and the remaining portion of the fourth drum (the remaining portion corresponding to the 30° contact surface of the drum) was set to 18°C using ambient air, and a cooling area was placed behind the consolidation unit in the MD.
[0238] The resulting nonwoven fabric was 18gsm, and its layered structure was clearly visible.
[0239] TIFF2023547228000006.tif202151
[0240] I. Test Method The basis weight of nonwoven fabrics is measured using a test method compliant with European standard (EN ISO) 9073-1:1989 (corresponding to the method of Worldwide Strategic Partners (WSP) 130.1). Ten layers of nonwoven fabric are used for measurement. Sample dimensions are 10 × 10 cm. 2 That is the case.
[0241] The tensile strength and elongation of nonwoven fabrics shall be measured using a test method compliant with the WSP110.4.R4 (12) standard.
[0242] The "thickness" or "measured height" of the nonwoven fabric shall be measured according to the test measurement method in accordance with the European standard EN ISO9073-2:1995 (corresponding to the method of WSP120.6), and corrected in the following manner: 1. The material is to be measured using a sample taken from the manufacturing process without being subjected to high deformation forces or pressure for more than one day (e.g., pressure from rollers in the manufacturing equipment), but otherwise it must be left free on some surface for at least 24 hours. 2. The total weight of the upper arm of the measuring machine, including additional ballast, is 130g.
[0243] The "bulkness," "bulk height," or "bulk density" of nonwoven fabrics is expressed in kg / m³. 3 Expressed as g / m 2The calculation is performed by dividing the "basis weight" (unit) by the "thickness" (unit) in millimeters.
[0244] The "thickness ratio to basis weight" of nonwoven fabrics is dm 3 Expressed in units of / kg or l (liters) / kg, the "thickness" in mm multiplied by 1000 is calculated as g / m². 2 The calculation is performed by dividing by the unit "basis weight".
[0245] The "rigidity" of nonwoven fabrics is expressed by the "handle ometer (HOM)" measurement value and determined in accordance with the international standard WSP90.3. Unless otherwise specified, the sample dimensions are 100 x 100 mm. HOM is measured separately in the MD direction and the CD direction. Unless the MD or CD direction is specified, the arithmetic mean of these two values is taken.
[0246] In this specification, the terms "regeneration rate" or "recovery rate" in relation to bulkiness refer to the ratio of the thickness of the fabric after the applied load is released to the initial thickness of the fabric. The thickness of the fabric is measured according to standard EN ISO 9073-2:1995 using a preliminary load force equivalent to a pressure of 0.5 kPa. The measurement procedure for regeneration consists of the following steps: 1. Prepare a fabric sample measuring 10 x 10 cm; 2.1 Measure the thickness of the fabric; 3. Measure the thickness (Ts) of five overlapping fabrics using a preliminary load force equivalent to a pressure of 0.5 kPa; 4. In the thickness measuring device, apply a load (pressure of 2.5 kPa) to five stacked pieces of fabric for 5 minutes; 5. Remove from the device and wait for 5 minutes; The thickness (Tr) of the five overlapping fabrics is measured using a preliminary load force equivalent to a pressure of 6.0.5 kPa; 7. Calculate the reproduction rate according to the following formula: Regeneration rate = Tr / Ts (unitless) Ts = Thickness of the new sample Tr = Thickness of the regenerated sample
[0247] As used herein, the term "compressibility" refers to the distance in millimeters by which the nonwoven fabric is compressed under the influence of the load defined when measuring "flexibility". Compressibility can also be calculated as the product of the resilience (unitless) × thickness (mm). The "elasticity" or "resilience" of the nonwoven fabric is measured using the test method according to Standard EN ISO 964-1 and corrected by the following method: 1. Measure the thickness of one layer of the fabric; 2. Prepare several fabric samples and stack them so that the total thickness after stacking is at least 4 mm, ideally 5 mm. The stacked fabric group includes at least one layer of fabric; 3. Measure the thickness of these stacked fabric samples; 4. Apply a force of 5 N to this group of laminated fabric samples at a loading rate of 5 mm / min; 5. Measure the distance the clamp element has moved; 6. Calculate the resilience according to the following formula: R (unitless) = T1 (mm) / T0 (mm) Or, R (%) = T1 (mm) / T0 (mm) × 100% T1 = the distance the clamp element has moved under a load of 5 N [mm] = the degree of compression of the laminated fabric T0 = thickness (compliant with Standard EN ISO 9073-2:1995 with a preloading force of 1.06 N applied) [mm].
[0248] "Martindale average abrasion resistance grade test" or "Martindale" Figure 38 is a perspective view of the apparatus for the Martindale average abrasion resistance grade test. Figure 39 is the grade index for evaluating hairiness in the Martindale average abrasion resistance grade test of this specification, as described in U.S. Patent Application Publication No. 20200170853A1 filed by Procter & Gamble.
[0249] The Martindale average abrasion resistance grade of the nonwoven fabric is measured using a Martindale abrasion tester. The test is conducted in a dry state. - Condition the nonwoven fabric sample at a temperature of 23 ± 2 °C and a relative humidity of 50 ± 2% for 24 hours. - Cut out 10 circular samples with a diameter of 162 mm (6.375 inches) from each nonwoven fabric sample. Cut out one standard felt circle with a diameter of 140 mm. - First, place the cut felt, then the cut nonwoven fabric, and secure each sample to its respective position on the Martindale abrasion test bench. Next, secure the clamp ring to prevent wrinkles from forming on the nonwoven fabric sample. - Assemble the polisher holder. The polisher is made of 38mm diameter, 1 / 32 inch thick silicone rubber (part number 86045K21-50A, manufactured by McMaster-Carr), compliant with the U.S. Food and Drug Administration (FDA). Place the desired weights in the polisher holder so that a pressure of 9kPa is applied to the sample. Install the assembled polisher holder in Model #864 so that the polisher is in contact with the NW sample, as instructed in the operator's guide. - Perform Martindale wear under the following conditions: • Mode: Abrasion test • Speed: 47.5 cycles / minute • Cycle: 16 cycles - After the test is complete, the polished nonwoven fabric is placed on a smooth, matte black surface, and the level of fuzziness is graded using the index shown in the figure. Each sample is evaluated by observing both the dimensions and number of defects from above and the height of the defect protrusions from the side. A number from 1 to 5 is assigned to the sample that best matches this grading index. Next, the Martindale mean abrasion resistance grade is calculated as the average evaluation of all samples, and the closest grade on a 10-point scale is reported.
[0250] "Delamination strength" or "adhesion" can be determined by the following method (see Figures 40 and 41): 1) Cut out a test specimen that is 120 mm long (in the MD direction) and at least 30 mm wide. 2) Cut two strips of tape, each 145 mm long, and fold 25 mm from one end of each strip. Reinforce the sample with 25.4 mm wide tape and adhere it by rolling it once in one direction with a 7 kg hand roller. Cut the sample along the tape so that it is 25 mm wide on a CD. Separate the free ends of the tape strips. 3) The tensile strength testing machine shall feature: two jaws with clamping surfaces on the same plane parallel to the direction of stress application; these two jaws shall be aligned to hold the specimen on that plane without slipping or damaging the specimen throughout the test. The four faces of the jaws shall be padded with thin strips of soft gasket rubber to prevent slipping and damage to the specimen. In accordance with the American Society for Testing and Materials (ASTM) D76-99, Twing Albert, Instron, Zwick, or equivalent machines may be used as constant-speed lateral-movement tensile testing machines. 4) Set the parameters as follows: a) Gauge length ......................50mm b) Crosshead speed ..............305 mm / min c) Preliminary tensile length ..................10mm d) Measurement length ......................152mm e) Sample scanning frequency .................50Hz 5) Place the test specimen in the testing machine by clamping the free end of the tape, which is properly positioned on the upper grip (Figure 41). Fold the free end of the tape back and secure it with the lower grip. Align the free ends of the test specimen symmetrically within the grips to ensure uniform tension. Adjust the load range as needed so that the reading is between 30% and 80% of the full load range. 6) Start the tensile testing machine. 7) Measure 10 samples and calculate the average value. 8) Report the average peeling force in increments of 0.01 N.
[0251] The "type of fiber cross-section" can be determined from the process conditions defined for the fiber molding die. If the process conditions are unknown, the following estimation method can be used: A fabric sample is taken, and photographs of the cross-sections of at least 20 fibers are taken. Measurements are taken at the free portion of the fiber, and not at joints or contact points with other fibers where deformation is expected. For each cross-section, each component is marked separately on the image surface. The center of mass for each component is determined based on the determination of the centroid or shape center of the planar object, and its position is recorded using a Cartesian coordinate system with center [0;0] at the shape center of the fiber cross-section. The deflection (D) of the center of mass of each component in each fiber cross-section is calculated according to the following formula: D = the absolute value of the product (x × y), where x and y are the coordinates of the center of mass. If one of the values x or y is 0 and not equal to the other, the sample is excluded from evaluation.
[0252] Calculate the mean and standard deviation for each component.
[0253] If the ratio of ((mean deflection) + (standard deviation)) to the total fiber cross-section is less than 5%, the fiber is considered non-crimped.
[0254] If the ratio of ((mean deflection) - (standard deviation)) to the total fiber cross-section is less than 10%, the fiber is presumed to be non-crimped.
[0255] The "interfilament bonding density," "filament density," "cavity length and height," and "percentage of cavities relative to the thickness of the nonwoven fabric" can be determined from the cross-section of the fabric.
[0256] At least 10 samples are collected using MD and at least 10 samples using CD. The fabric is judged to have a layered structure if a layered structure is observed in at least 50% of the samples.
[0257] The material is to be measured using a sample taken directly from the manufacturing process, without being subjected to high deformation forces or pressure for more than a day (e.g., pressure from rollers in the manufacturing equipment). Otherwise, it must be freely laid out on some surface and left for at least 24 hours.
[0258] Cross-sections can be created and analyzed in several ways: How to create a cross-section of fabric 1) Simple cross-section: Place the fabric on a suitable surface and cut it with a sharp razor blade. Ensure the cut edge is approximately the same thickness as the fabric (for example, that the filament is not compressed or "cut and glued"). 2) Resin cross-section: The fabric sample is placed in a container, and liquid resin is poured in and allowed to solidify. The resin should be selected such that, in its liquid state, it easily fills the total void volume of the fabric, and in its solid state, it is easily distinguishable from the fabric polymer. A block of solid resin is cut in half to create a cross-section of the fabric sample. 3) Digital section: The sample is scanned (e.g., tomography, micro-CT), and digital cross-sections are created on a computer.
[0259] Method for analyzing the cross-section of the sample: 1) SEM microscopy observation a) If necessary, place the filament sample in a suitable holder (see, for example, Figures 42A and 42B) and analyze it. b) Metallize the sample with gold (for example, using an Au / Pd metallization apparatus SC 7640 Sputter Coater). c) Analyze the sample using an electron microscope (e.g., using a Tescan backscatter electron (BSE) detector) at 30kV and an appropriate magnification (30x to 1000x). 2) 3D tomography a) If necessary, a thin layer of contrast agent is applied to the sample. For example, when using 3D X-ray tomography (Skyscan), polyolefins are not fully visualized. For example, the sample can be metallized with gold (e.g., using an Au / Pd metallization device SC 7640 Sputter Coater). b) Place the sample in the analysis chamber and scan it. 3) 3D μCT – See "Method for determining the shape and fiber statistics of nonwoven fabrics."
[0260] The above methods and analyses (excluding 3D μCT) could potentially be carried out, for example, at the Faculty of Engineering, Tomas Bata in Zlin University (Czech Republic).
[0261] Next, we analyze the obtained cross-sectional images: 1) "Interfilament bonding density", "filament density" a) Divide the fabric cross-section into regular segments. Each segment has a maximum thickness of 0.05 mm (for example, divide a 0.45 mm thick fabric into nine sections of 0.05 mm thickness). b) The length of each segment is at least 0.5 mm, and it is preferable that this length is visible in the cross-sectional photograph. c) Set the density i) Calculate the number of interfilamental bonds for each segment and express it as the density of interfilamental bonds (number of bonds / segment area); or ii) Calculate the area occupied by the filament in each segment and express it as filament density (area occupied by filament / segment area). d) A hierarchy may be formed by joining adjacent segments that have the same or very similar density. e) Name hierarchies A, B, and possibly C, and calculate their average value. f) Calculate the ratio value. 2) "Length and height of the cavity" and "Percentage of cavities in the thickness direction of the nonwoven fabric" a) Adopt the hierarchical structure determined above and further investigate the area of hierarchy B. b) Highlight the void volume region. c) Mark any cavities (a region is considered a cavity if it is within the fabric thickness, is more than three times larger than the average filament thickness (in the z-direction of the fabric), and is more than five times longer than the average filament thickness in the MD × CD plane direction of the fabric). d) Calculate the total area of the void and express it as a percentage of the area of layer B. e) Measure the height of each cavity in the direction of the fabric thickness, measure its length in the direction of the fabric's MD × CD plane, and calculate the L:H ratio using the maximum values of these measurements.
[0262] "Method for determining the shape and fiber statistics of nonwoven fabrics" The following describes a software-based method for analyzing nonwoven fabric samples and characterizing their morphological properties. This method utilizes a machine learning approach to identify individual fibers within the sample, followed by morphological analysis of these fibers to obtain statistical values suitable for material characterization. The results include fiber orientation and density distributions. This analysis workflow was developed by Math2Market and is part of GeoDict, a digital materials laboratory software.
[0263] Step 1: Acquisition of a 3D μCT image of the sample First, a three-dimensional image is obtained by digitizing the nonwoven fabric sample using a μCT scanner. This three-dimensional image consists of a uniform Cartesian grid, and each cell (volume element: voxel) of the grid stores the X-ray irradiation attenuation value of the sample at the corresponding position. The pore space usually has the lowest attenuation value (lowest grayscale value), while the material phase shows a high attenuation value, and the attenuation value depends on the material and the configuration of the μCT device.
[0264] Step 2: Micro-CT image segmentation to separate material from pore space. For further analysis, the grayscale images are subjected to noise filtering using a non-local approach [1]. The images are then binarized using a global threshold derived by the Otsu algorithm [2]. This binarization classifies each voxel in the image as either containing pore space or fibrous material. Voxels with a gray value below the threshold are classified as pore space. All other voxels are classified as fibrous material. The ImportGeo module of the GeoDict software is used for both noise filtering and threshold setting.
[0265] Step 3: Analysis of material density distribution Furthermore, the material density distribution in the Z direction is calculated electronically. For each image cross-section (with a given depth in the Z direction), the material density is calculated electronically as the number of voxels of the white material divided by the total number of voxels in the cross-section. This analysis is performed using the MatDict module of the GeoDict program.
[0266] Step 4: Use of a neural network to identify the fiber centerline The main challenge in identifying individual fibers in μCT images is failing to spatially separate the fibers at their contact points after binarization. This leads to undersegmentation, where multiple objects (fibers) are mistakenly classified as a single fiber.
[0267] To separate fibers, Math2Market developed an approach to identify the fiber's center curve. These center lines are displayed on a binary voxel image of the same dimensions as the original image. In this image, voxels located approximately 1-2 voxels away from the fiber's center are marked.
[0268] For this purpose, a semantic partitioning approach using a neural network was employed [3]. The image is analyzed considering a sliding 3D input window that moves across the image. For each input window, a small output window is defined at the center of the input window. The neural network analyzes the binary voxel values of the input window and predicts each voxel in the output window. Based on the predictions, it is determined whether the voxel in the output window is part of the center line. By combining the results of all these output windows, a binary image is obtained in which each voxel of the material contained in the original image is classified. This image transformation is performed by the FiberFind-AI module in the GeoDict program using the Tensorflow software library [4].
[0269] Step 5: Creating training data for the neural network To train the neural network required for the aforementioned transformation, Math2Market used the probabilistic FiberGeo structure generation module of the GeoDict software program to create several artificial 3D images of nonwoven materials. This module depicts the analytical shape of the fibers as a series of line segments. Simultaneously, the module outputs a binary image of the fiber structure, which is compared with the result of the binarization in step 2.
[0270] By changing the fiber diameter by approximately 2-3 voxels within the analysis, a similar image of the centerline corresponding to the artificial fiber structure can be obtained.
[0271] Next, these pairs of images (fibers and centerlines) are used to train a neural network that converts fiber images into centerline images. This network effectively learns to "collapse" the fibers into centerlines.
[0272] Step 6: Tracing the fiber centerline to depict the shape of the fiber. After the fibers are contracted towards their centerlines, it is assumed that the centerlines are not in contact with each other. Then, the individual centerlines are separated by analyzing the connected components of the centerline image. In this process, it is assumed that each component corresponds to the centerline of one fiber. The connected components are defined as a subset of material voxels, and all voxels are the same color, and they cannot be expanded by adding voxels of the same color that are in contact with each other.
[0273] At each centerline, a curve is traced through a set of voxels, depicting the shape of the corresponding fiber in the form of a series of connected line segments (polylines). This process is also part of the FiberFind-AI in the GeoDict program.
[0274] As a result, a digital 3D model of the fabric was obtained, and examples of fabrics with a hierarchical structure can be seen in Figures 44-46.
[0275] Step 7: Computer analysis of the sample To determine the "interfilament bonding density," "filament density," "cavity length and height," and "cavity percentage relative to the nonwoven fabric thickness," the filament segments of each cross-section were projected onto a plane and divided into subsegments (each with a maximum thickness of 0.05 mm) for analysis. Values were compared between segments, and if possible, several adjacent segments with identical or similar results may be joined to the same hierarchical level. Hierarchical levels A, B, and possibly C were named, and the values for each level were averaged from the segment data.
[0276] [1] Buades, Antoni, Bartomeu Coll, and JM.Morel. "A non-local algorithm for image denoising", Computer Vision and Pattern Recognition, 2005, CVPR 2005, IEEE Computer Society Conference, Volume 2, IEEE, 2005. [2] Nobuyuki Otsu, "A method for selecting a threshold from a gray-level histogram," IEEE Transactions on Systems, Man, and Cybernetics 9.1 (1979): pp. 62-66 [3] Noh, Hyeonwoo, Seunghoon Hong, and Bohyung Han, "Learning deconvolution network for semantic segmentation," Proceedings of the IEEE International Conference on Computer Vision, 2015. [4] Martin Abadi, Ashish Agarwal, Paul Barham, Eugene Brevdo, Zhifeng Chen, Craig Citro, Greg S. Corrado, Andy Davis, Jeffrey Dean, Matthew Devin, Sanjay Ghemawat, Ian Goodfellow, Andrew Harp, Geoffrey Irving, Michael Isard, Rafal Jozefowicz, Yangqing Jia, Lukasz Kaiser, Manjunath Kudlur, Josh Levenberg, Dan Mane, Mike Schuster, Rajat Monga, Sherry Moore, Derek Murray, Chris Olah, Jonathan Shlens, Benoit Steiner, Ilya Sutskever, Kunal Talwar, Paul Tucker, Vincent Vanhoucke, Vijay Vasudevan, Fernanda Viegas, Oriol Vinyals, Pete Warden, Martin Wattenberg, Martin Wicke, Yuan Yu, and Xiaoqiang Zheng, TensorFlow: Large-scale machine learning on heterogeneous systems, 2015, Available from tensorflow.org.
[0277] The snowflake of the snowflake The present invention is useful when a bulky nonwoven fabric with a balanced softness / resistance is required—for example, as a component of various absorbent hygiene products (e.g., baby diapers, incontinence products, feminine hygiene products, replacement pads, etc.) in the hygiene industry manufacturing sector, or in the healthcare sector, for example, as part of wound sponges and / or protective clothing, surgical cover sheets, underlays, and other barrier material products. Furthermore, it can also be used in industrial applications, such as parts of protective clothing, filtration, heat insulation, packaging, sound absorption, the footwear industry, automobiles, furniture, etc. The present invention is particularly advantageous in applications that combine the requirements for improving the bulkiness, compressibility, and resilience of fabrics with the requirement for endless fibers.
Claims
1. 1. A nonwoven fabric comprising a plurality of filament strata: a first layer (A) forming a first outer surface of the nonwoven fabric and comprising continuous multicomponent filaments of a first component, the first component comprising: - extending along the longitudinal direction of said filament, - forming at least 20% of the area of the surface of said filaments, - forming interfilament bonds within said first level (A), a first layer (A), which is a component having a melting point at least 5° C. lower than the melting point of said component of said filaments of said first layer (A); a second layer (B) comprising continuous multicomponent filaments of a first component, said first component comprising: - extending along the longitudinal direction of said filament, - forming at least 20% of the area of the surface of said filaments, - forming interfilament bonds within said second layer (B), - a component having a melting point at least 5° C. lower than the melting points of the other components of the filaments of the second layer (B), A second layer (B); - The bulk density of the fibre is 60 kg / m 3 is less than A nonwoven fabric characterized by:
2. The nonwoven fabric includes a third layer (C) that forms the second outer surface of the nonwoven fabric such that the second layer (B) is disposed between the first layer (A) that forms the first outer surface and the third layer (C) that forms the second outer surface of the nonwoven fabric, the third layer (C) including continuous multicomponent filaments of a first component, the first component being - extending along the longitudinal direction of said filament, - forming at least 20% of the surface of said filaments, - forming interfilament bonds within said third level (C), - have a melting point at least 5°C lower than the melting points of the other components of the filaments of said third layer (C); 2. The nonwoven fabric according to claim 1.
3. 3. The nonwoven fabric according to claim 1 or 2, characterized in that the ratio of the filament density of the first layer (A) to the filament density of the second layer (B) is at least 1.5; more preferably at least 2.0; more preferably at least 2.5; more preferably at least 3, even more preferably at least 5.
4. The nonwoven fabric according to any one of claims 1 to 3, characterized in that the ratio of the interfilament bond density of the first layer (A) to the interfilament bond density of the second layer (B) is at least 2; more preferably at least 3.0; more preferably at least 4; more preferably at least 5, and even more preferably at least 7.
5. The nonwoven fabric of any one of claims 1 to 4, wherein the first component of the first layer (A) and / or the first component of the second layer (B) comprises an adhesive polymer selected from the group consisting of polyolefins, aliphatic polyesters, aromatic polyesters, or copolymers thereof.
6. A nonwoven fabric described in any one of claims 1 to 5, characterized in that the fabric layer peel strength is 0.5 N or more, preferably greater than 0.6 N, more preferably greater than 0.7 N, and most preferably greater than 0.8 N.
7. 7. The nonwoven fabric according to any one of the preceding claims, characterized in that the textile layer peel strength is at most 10.0N, preferably at most 8.0N, more preferably at most 6.0N and advantageously at most 4.0N.
8. 8. The nonwoven fabric according to any one of claims 1 to 7, characterized in that the nonwoven fabric comprises at least a first layer (i) and a second layer (ii) of filaments.
9. An absorbent sanitary article comprising the nonwoven fabric according to any one of claims 1 to 8.
10. A method for producing the nonwoven fabric of claim 1, comprising the steps of: a) melting a. at least a first polymeric material forming a first component; b. a second polymeric material forming at least one other component; b) feeding a molten polymeric material to a nozzle of a spinning beam and extruding said molten polymeric material through the nozzle, said step comprising: a. forming an endless filament from the molten polymeric material exiting the nozzle; b. said first polymeric material is oriented longitudinally of said filaments and forms at least a portion of a surface of said filaments, said first polymeric material having a melting point at least 5° C. lower than the melting points of other components of said filaments; c) cooling the formed filaments with a fluid medium having a temperature between 10 and 90° C. and drawing the filaments at a drawdown ratio between 200 and 1300 to achieve at least a semi-stable crystalline state of the second polymeric material; d) randomly laying the filaments on a forming belt to form a nonwoven filament batt; e) pre-consolidating the nonwoven filament batt with a heat flow for 1-10,000 ms; f) preheating the filament batt with a heat flow at a temperature between 5 and 20° C. below the melting point of the first polymeric material, preferably between 5 and 15° C. below the melting point of the first polymeric material, more preferably between 5 and 10° C. below the melting point of the first polymeric material; and g) consolidating said filament batt by a heat flow having a temperature at most 5° C. below the melting point of said first polymeric material and at most 3° C. above the melting point of said first polymeric material, and cooling said filament batt thus consolidated by an air flow having a temperature between 10 and 40° C., preferably between 20 and 30° C. The method according to claim 1, further comprising:
11. 11. The method of claim 10, further comprising the step of: between the pre-consolidation step e) and the pre-heating step f), intermediate cooling is performed by exposing the pre-consolidated batt to air.
12. 12. The method for producing a nonwoven fabric according to claim 11, characterized in that the intermediate cooling is carried out with air at a temperature of not more than 70°C, preferably not more than 60°C, most preferably not more than 55°C.
13. 13. The method for producing a nonwoven fabric according to claim 10, wherein during the consolidation of the batt in step g), the heat flow is applied in alternating directions, entering first from one side of the batt and then from the other side of the batt.
14. The method for producing a nonwoven fabric according to any one of claims 10 to 13, characterized in that at least a part of the steps f) and / or h) is carried out by aligning the batt with a drum of an air-through consolidation device.
15. 15. The method of claim 10, wherein at least a portion of steps f) and / or h) are performed by passing the batt through a flat oven consolidation device.