Low Resistivity Contacts and Interconnects
Patent Information
- Application Number
- JP2023528357
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-11-19
- Filing Date
- 2021-11-04
- Publication Date
- 2024-11-07
AI Technical Summary
Depositing low resistivity metal films becomes challenging as semiconductor devices become smaller and more complex, particularly in filling features of varying sizes with conventional deposition methods.
The method involves using atomic layer deposition (ALD) of molybdenum (Mo) to fill smaller features, followed by chemical vapor deposition (CVD) or physical vapor deposition (PVD) of tungsten (W) to fill larger features, optionally with a nucleation layer and treatment with metal halides to enhance conductivity.
This approach results in low resistivity metallization stacks with efficient and scalable deposition, allowing for complete filling of features of varying sizes with minimal resistivity and improved conductivity.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Background technology]
[0001] Related Applications A PCT application has been filed contemporaneously herewith as a part of this application. Each application identified in the contemporaneously filed PCT application to which this application claims benefit or priority is incorporated herein by reference in its entirety for all purposes.
[0002] The background art description provided herein is intended to provide a general context for the present disclosure. Work by the presently named inventors, to the extent described in this background art section, as well as aspects of the description that may not otherwise be considered prior art at the time of filing, are not admitted, expressly or impliedly, as prior art against the present disclosure.
[0003] Metal deposition is an essential part of many semiconductor manufacturing processes. These materials may be used for horizontal interconnects, vias between adjacent metal layers, and contacts between metal layers and devices. However, as devices shrink and more complex patterning schemes are utilized in industry, the deposition of low-resistivity metal films becomes a challenge. Summary of the Invention
[0004] One aspect of the present disclosure relates to a method in a structure including a plurality of features, including depositing a bulk layer of molybdenum (Mo) by atomic layer deposition (ALD) to at least partially fill the plurality of features with Mo, and depositing a bulk layer of tungsten (W) on the bulk layer of Mo by chemical vapor deposition (CVD) or physical vapor deposition (PVD).
[0005] In some embodiments, the plurality of features includes a first set of one or more features having a first critical dimension and a second set of one or more features having a second critical dimension, the first critical dimension being smaller than the second critical dimension, and filling of the first set of features is completed by depositing a bulk layer of Mo, and filling of the second set of features is completed by depositing a bulk layer of W. In some embodiments, at least a portion of the filling of the plurality of features is completed with the bulk layer of W. In some embodiments, the bulk layer of W is deposited only on top surfaces of the plurality of features and not within the plurality of features. In some embodiments, the method further includes removing all of the bulk layer of W. In some embodiments, the plurality of features includes an oxide surface prior to any Mo deposition in the features. In some such embodiments, Mo is formed in the plurality of features, and no barrier layer is disposed between the formed Mo and the oxide surface.
[0006] In some embodiments, the method further comprises depositing a nucleation layer prior to depositing the bulk layer of Mo. In some such embodiments, depositing the nucleation layer comprises forming a layer of molybdenum nitride or molybdenum oxynitride. In some such embodiments, the method further comprises converting the layer of molybdenum nitride or molybdenum oxynitride to molybdenum.
[0007] In some embodiments, the Mo bulk layer and the W bulk layer are deposited in the same chamber. In some embodiments, the Mo bulk layer and the W bulk layer are deposited in different stations in the same chamber. In some embodiments, the Mo bulk layer and the W bulk layer are deposited in different chambers. In some such embodiments, the different chambers are connected to a common vacuum environment, and in other such embodiments, the different chambers are not connected to a common vacuum environment.
[0008] In some embodiments, the method further comprises treating the surface of the deposited bulk Mo layer with a metal halide prior to depositing the bulk W layer.
[0009] In some embodiments, depositing a bulk layer of Mo by atomic layer deposition (ALD) includes exposing a structure to alternating pulses of a Mo precursor and a co-reactant. In some such embodiments, the Mo precursor is a molybdenum halide or a molybdenum oxyhalide. In some such embodiments, the Mo precursor is molybdenum hexafluoride (MoF), molybdenum hexachloride (MoCl), molybdenum dioxide dichloride (MoOCl), molybdenum oxide tetrachloride (MoOCl), molybdenum hexacarbonyl (Mo(CO)), (MoOF), molybdenum dioxide dibromide (MoOBr), MoOI, and MoO. 11 I. In some embodiments, the co-reactant is hydrogen (H). In some embodiments, the Mo precursor is an organometallic precursor.
[0010] Another aspect of the present disclosure relates to a method that includes providing a structure including a first set of features in a chamber, depositing a bulk layer of molybdenum (Mo) by atomic layer deposition (ALD) in the structure including the first set of features to partially fill the features with Mo, and removing the structure including the features partially filled with Mo from the chamber. In some embodiments, depositing the bulk layer of Mo by atomic layer deposition (ALD) includes exposing the structure to alternating pulses of a Mo precursor and a co-reactant. In some such embodiments, the Mo precursor is a molybdenum halide or a molybdenum oxyhalide. In some such embodiments, the Mo precursor is selected from the group consisting of molybdenum hexafluoride (MoF), molybdenum hexachloride (MoCl), molybdenum dioxide dichloride (MoOCl), molybdenum oxide tetrachloride (MoOCl), molybdenum hexacarbonyl (Mo(CO)), (MoOF), molybdenum dioxide dibromide (MoOBr), MoOI, and MoO. 11I. In some embodiments, the co-reactant is hydrogen (H). In some embodiments, the Mo precursor is an organometallic precursor.
[0011] In some embodiments, the method further comprises depositing a nucleation layer prior to depositing the bulk layer of Mo. In some such embodiments, depositing the nucleation layer comprises forming a layer of molybdenum nitride or molybdenum oxynitride. In some such embodiments, the method further comprises converting the layer of molybdenum nitride or molybdenum oxynitride to molybdenum.
[0012] Yet another aspect of the present disclosure relates to a method that includes providing a structure in a chamber that includes a first set of features, the first set of features being at least partially filled with molybdenum (Mo), and depositing a bulk layer of tungsten (W) on the Mo.
[0013] In some embodiments, the structure includes a plurality of features including a first set of one or more features having a first critical dimension and a second set of one or more features having a second critical dimension, the first critical dimension being smaller than the second critical dimension, the first set of features being completely filled with Mo, and the filling of the second set of features is completed by depositing a bulk layer of W.
[0014] In some embodiments, at least a partial fill of the first set of features is completed by a bulk layer of W. In some embodiments, the bulk layer of W is deposited only on top surfaces of the first set of features and not within the first set of features.
[0015] In some embodiments, the method further includes removing all of the bulk layer of W. In some embodiments, Mo is formed in a plurality of features, and no barrier layer is disposed between the formed Mo and the oxide surface.
[0016] These and other aspects of the present disclosure are further described below with reference to the drawings. [Brief explanation of the drawings]
[0017] [Figure 1A] FIG. 1A is a schematic example of a cross section of a structure having features of different sizes filled with a conductive material.
[0018] [Figure 1B] FIG. 1B is a schematic example showing the structure of FIG. 1A after atomic layer deposition (ALD) of a molybdenum (Mo) film.
[0019] [Figure 1C] FIG. 1C is a schematic example showing the structure of FIG. 1B after chemical vapor deposition (CVD) of a tungsten (W) film.
[0020] [Figure 1D] FIG. 1D is a schematic example showing the structure of FIG. 1C after chemical mechanical planarization (CMP).
[0021] [Figure 2] FIG. 2 is a schematic example of a structure where an ALD Mo film completely fills the smaller feature and partially fills the larger feature, and a CVD Mo film fills the remaining portion of the larger feature.
[0022] [Figure 3A] FIG. 3A is a schematic example of the structure of FIG. 1A after ALD of a Mo film completely fills the features of the structure.
[0023] [Figure 3B] FIG. 3B is a schematic example of the structure of FIG. 1B after CVD of a W coating.
[0024] [Figure 3C] FIG. 3C is a schematic example showing the structure of FIG. 3B after chemical mechanical planarization (CMP).
[0025] [Figure 4] FIG. 4 is a flow diagram illustrating certain operations in an example ALD method for forming a Mo film.
[0026] [Figure 5] FIG. 5 is a flow diagram illustrating certain operations in an example method for depositing Mo. [Figure 6] FIG. 6 is a flow diagram illustrating certain operations in an example method for depositing Mo.
[0027] [Figure 7] FIG. 7 is a flow diagram illustrating certain operations in an exemplary method for treating Mo with a metal halide prior to CVD deposition of W.
[0028] [Figure 8] FIG. 8 shows a schematic diagram of one example of a process station that can be used for ALD and / or CVD.
[0029] [Figure 9] FIG. 9 shows an example of a processing system including multiple chambers. DETAILED DESCRIPTION OF THE INVENTION
[0030] Provided herein are low-resistivity metallization stack structures for logic and memory applications, and related fabrication methods. The methods include atomic layer deposition (ALD) of molybdenum (Mo), and in some embodiments, ALD of Mo in barrier-layer-free features. In some embodiments, deposition of an ALD Mo film may be followed by chemical vapor deposition (CVD) or physical vapor deposition (PVD) of a Mo film. In some embodiments, the CVD or PVD Mo film is part of the metallization stack. In other embodiments, the CVD or PVD Mo film is deposited as a sacrificial overlayer. In some embodiments, deposition of an ALD Mo film may be followed by CVD or PVD of another metal, such as tungsten (W). In some embodiments, a CVD or PVD W film is part of the metallization stack. In other embodiments, the CVD or PVD W film is deposited as a sacrificial overlayer. The metallization may be performed in any suitable context, including middle-of-line (MOL) and back-end-of-line (BEOL) metallization.
[0031] According to various embodiments, one or more advantages may be realized. In some embodiments, a low resistivity film may be deposited directly onto the etched dielectric without a diffusion barrier or other intervening film, thereby achieving low resistivity. In some embodiments, the process is efficient and highly scalable, using relatively fast CVD or PVD processes to fill large features and / or overlay layers.
[0032] One aspect of the present disclosure relates to filling features on a substrate with a conductive material. In some embodiments, the structure includes features of different sizes. Figure 1A shows an example of such a structure, which includes a small feature 102 and larger features 104, 106, and 108 etched into a dielectric layer 109. Each feature 102, 104, 106, and 108 has a bottom surface and a sidewall surface.
[0033] In some embodiments, the bottom surface of the feature may be a metal surface, such as cobalt (Co), ruthenium (Ru), copper (Cu), W, Mo, nickel (Ni), iridium (Ir), rhodium (Rh), tantalum (Ta), and titanium (Ti). In some embodiments, the bottom surface is an elemental metal surface. In some embodiments, the bottom surface is a titanium nitride (TiN) surface, molybdenum nitride (MoN x ), tungsten nitride (WN), tungsten carbonitride (WC x N y ), tungsten carbide (WC x ), titanium aluminum carbide (TiAl x C y The bottom surface may be a metal compound such as a tantalum nitride (TaN) surface. The bottom surface may be part of an underlying metal contact, electrode, or other conductive component (not shown). The bottom surface may be part of the main conductor of the underlying layer, rather than a thin layer such as a barrier layer or adhesion layer.
[0034] In some embodiments, the sidewall surfaces may be dielectric surfaces. Such surfaces include alkoxides such as poly(2-ethyl-2-oxazoline) (PEOX), silicon-based oxides such as tetraethyl orthosilicate (TEOS) oxide, flowable silicon-based oxides, and carbon-doped silicon-based oxides. In some embodiments, these surfaces are part of the main dielectric layer 109 surrounding the feature. In some embodiments, the sidewall surfaces are not oxides but nitrides (e.g., Si x N y ) The nitride may be a silicon-based nitride or a silicon-based oxynitride. The surfaces of features 102, 104, 106, and 108 may be the same or different between features.
[0035] 1B shows the structure after ALD deposition of Mo film 111. Smaller feature 102 is completely filled by ALD Mo film 111, while larger features 104, 106, and 108 are partially filled by ALD Mo film 111. ALD of molybdenum is described further below.
[0036] Figure 1C shows the structure after CVD deposition of the W film 113. The W film 113 completes the feature filling of the larger features 104, 106, and 108. Figure 1D shows the structure after chemical mechanical polishing (CMP). As can be seen, the W film 113 forms a part of the conductive component (e.g., contact, interconnect, line, etc.) in each of the larger features 104, 106, and 108. The smaller feature 102 is filled only with the Mo film.
[0037] The metallization scheme obtained as the method and result illustrated in FIGS. 1A-1D has various advantages, including that the ALD Mo film 111 is a low resistivity film on which can be directly deposited on the dielectric, and that the CVD of W is a fast and scalable process. As a result, the entire stack can have a low resistivity and can be manufactured efficiently. In an alternative embodiment, instead of CVD, sputtering or other PVD processes may be used to deposit W.
[0038] Figure 2 shows an example of a structure according to another embodiment. In FIG. 2, the ALD Mo film 111 completely fills the smaller feature 102 and partially fills the larger features 104, 106, and 108. The CVD Mo film 215 fills the remaining portions of the larger features 104, 106, and 108. The Mo film 215 forms a part of the conductive component in each of the larger features 104, 106, and 108. In an alternative embodiment, instead of CVD, sputtering or other PVD processes may be used to deposit Mo.
[0039] In the examples of FIGS. 1A-1D and FIG. 2, the structure includes smaller features that are completely filled by ALD Mo. The methods described herein may also be implemented in structures that include only features that are partially filled with ALD Mo. Thereafter, the feature filling is completed with CVD or PVD W, or CVD or PVD Mo as described above.
[0040] Another aspect of the present disclosure relates to a method that includes filling features with ALD Mo and depositing a sacrificial overlayer. FIGS. 3A-3C illustrate an example structure during such a method. First, in FIG. 3A, the structure shown in FIG. 1A is filled with an ALD Mo film 111. In the example of FIG. 3A, all features are completely filled with the ALD Mo film 111. After the ALD fill process, some amount of ALD Mo film is deposited on features 102, 104, 106, and 108. An ALD Mo film may also be deposited on structures between the features. In FIG. 3B, a W film 113 is deposited by CVD on the filled features. Unlike the W film in FIG. 1D, the W film 113 in FIG. 3B is a purely sacrificial film. Thus, after CMP, only the ALD Mo film 111 is present in features 102, 104, 106, and 108, as shown in FIG. 3C. In alternative embodiments, instead of CVD W, PVD W, CVD Mo, or PVD Mo may be used in the sacrificial film.
[0041] In the context of this description, CVD refers to a process in which the reactants are present in the gas phase simultaneously in a reactor and are generally introduced simultaneously, while ALD refers to a process in which the reactants are introduced in successive pulses, usually separated by purging. Examples of reactants and reaction conditions that can be used for ALD and / or CVD reactions to fill features with conductive material are provided below.
[0042] In some embodiments, ALD relies on the adsorption of one or more reactants to the surface of the substrate, followed by chemical conversion of the adsorbed layer to the desired material. Because ALD employs sequential reactions that occur at the surface of the substrate, are separated in time, and are typically limited by the amount of adsorbed reactants, it provides thin conformal layers with excellent step coverage. In the following description, the molybdenum-containing reactant is referred to as the Mo precursor and is reacted with a co-reactant.
[0043] As further described below, in some embodiments, a Mo precursor is reacted with a reducing agent co-reactant to form a pure Mo film. According to various embodiments, each ALD cycle may begin with the pulse and adsorption of either the Mo precursor or the co-reactant on the surface, followed by a pulse of the other. In other embodiments, a Mo precursor (e.g., an organometallic Mo precursor) may be reacted sequentially with several reactants. And, in other embodiments, the ALD process may include decomposition of the Mo precursor without the co-reactant.
[0044] FIG. 4 illustrates an example of an ALD method for forming a Mo film. First, in operation 405, a Mo precursor is pulsed into a chamber containing a substrate having features to be filled. Examples of Mo precursors are provided below. The precursor can be introduced in a vaporized state in a flow of an inert gas, such as argon (Ar), helium (He), or nitrogen (N). After the Mo precursor is pulsed, an optional purge 415 can occur. Argon or any inert gas can be used to purge any Mo precursor remaining in the vapor phase from the chamber. The purge can be performed by flowing an inert gas at a constant pressure, thereby reducing the chamber pressure, and repressurizing the chamber before beginning another gas exposure. The purge can be performed for a duration of between about 0.25 seconds and about 30 seconds, about 0.25 seconds and about 20 seconds, about 0.25 seconds and about 5 seconds, or about 0.5 seconds and about 3 seconds.
[0045] The substrate is exposed to a co-reactant in operation 425. As noted above, the co-reactant can be a reducing agent for reducing the Mo precursor to form elemental Mo. In other embodiments, the co-reactant is any suitable co-reactant or co-reactants that react with the Mo precursor to form elemental Mo. The reactant can be a hydrogen-containing reactant. In some embodiments, the hydrogen-containing reactant can be thermal (non-plasma) hydrogen (H).
[0046] The plasma-based process may use a remote plasma or an in-situ plasma generated from H. An optional purge may be performed at 435, after which operations 405-435 may be repeated in operation 445 until the film is fully grown. According to various embodiments, this may be when the feature is partially or fully filled, as described above with respect to FIGS. 1A-3.
[0047] The substrate temperature during Mo deposition may be between 300°C and 750°C, and in certain embodiments, between 450°C and 550°C. The substrate temperature depends on the thermal budget and deposition chemistry. The thermal budget is application dependent; for memory applications, high deposition temperatures may not be an issue, but for logic applications, the thermal budget may be exceeded.
[0048] The ALD Mo layer deposited in FIG. 4 forms all or part of the bulk conductive material in the feature, as described above with respect to FIGS. 1-3. In some embodiments, it may be deposited on a Mo nucleation layer formed by a separate ALD process. The nucleation layer is a thin conformal layer that can be used to support bulk deposition. In some embodiments, the Mo nucleation layer is deposited using one or more of a boron-containing reducing agent (e.g., B2H6) or a silicon-containing reducing agent (e.g., SiH4) as a co-reactant. For example, the Mo nucleation layer may be deposited using one or more S / Mo cycles or Mo / S cycles. S / Mo refers to a pulse of silane followed by a pulse of a Mo-containing precursor. In another example, one or more B / Mo cycles or Mo / B cycles may be used to deposit a Mo nucleation layer onto which the bulk Mo layer is deposited. Both B / Mo and S / Mo cycles (or Mo / B and / or Mo / S) may be used to deposit a Mo nucleation layer, e.g., x(B / Mo)+y(S / Mo), where x and y are integers. Examples of B- and S-containing reducing agents are provided below. For the deposition of a Mo nucleation layer, in some embodiments, the Mo-containing precursor may be a non-oxygen-containing precursor, e.g., molybdenum hexafluoride (MoF6) or molybdenum hexachloride (MoCl6). Oxygen in the oxygen-containing precursor may react with a silicon- or boron-containing reducing agent to form an impure, high-resistivity film, MoSi x O y or MoB x O y Oxygen-containing precursors may be used with minimal oxygen incorporation. In some embodiments, H2 may be used as the reducing gas for Mo nucleation layer deposition instead of a boron-containing or silicon-containing reducing gas. Example thicknesses for Mo nucleation layer deposition range from 5 Å to 30 Å. Films at the lower end of this range may not be continuous, but the thickness may be sufficient as long as it helps initiate continuous bulk Mo growth.
[0049] In some embodiments, the reducing agent pulse during deposition of the nucleation layer or bulk Mo layer may occur at a lower substrate temperature than the Mo precursor pulse. For example, the B2H6 or SiH4 (or other boron- or silicon-containing reducing agent) pulse may occur at a temperature below 300°C, while the Mo pulse occurs at a temperature above 300°C.
[0050] In some embodiments, the ALD formation of a Mo layer can be initiated by a reducing agent layer. An example of such a process is shown in the flow diagram of FIG. 5. In operation 502, a substrate is exposed to a reducing agent gas to form a reducing agent layer. In some embodiments, the reducing agent gas can be silane, borane, or a mixture of silane and diborane. Further examples of reducing agents are provided below. In some implementations, the reducing agent layer can include silicon or a silicon-containing material, phosphorus or a phosphorus-containing material, germanium or a germanium-containing material, boron or a boron-containing material, and combinations thereof, capable of reducing the Mo precursor. According to various embodiments, hydrogen may or may not be flowed in the background. (Hydrogen can reduce tungsten precursors, but does not function as a reducing agent in gas mixtures with sufficient amounts of stronger reducing agents, such as silane and diborane.) In some embodiments, the reducing agent gas is a mixture containing a small amount of a boron-containing gas, such as diborane, and another reducing agent. The addition of a small amount of a boron-containing gas can significantly affect the decomposition and sticking coefficients of other reducing agents. It should be noted that sequential exposure of the substrate to two reducing agents, for example, silane and diborane, may also be performed. However, flowing a mixture of gases can facilitate the addition of very small amounts of a minority gas, for example, a ratio of silane to diborane of at least 100:1. In some embodiments, a carrier gas may be flowed. In some embodiments, a carrier gas, such as nitrogen (N), argon (Ar), helium (He), or other inert gas, may be flowed during operation 502.
[0051] In some embodiments, the reducing agent layer may include elemental silicon (Si), elemental boron (B), elemental germanium (Ge), or mixtures thereof. For example, the reducing agent layer may include elemental Si and B, which are distinct from adsorbed silane or diborane molecules and may involve decomposition of the compound in the reducing agent gas. The amount of B may be adjusted to achieve low resistivity while achieving a high deposition rate of the reducing agent layer. In some embodiments, the reducing agent layer may have between 5% and 80% B, e.g., between 5% and 50% B, between 5% and 30% B, or between 5% and 20% B, with the remainder consisting essentially of Si and, optionally, H. Hydrogen atoms may be present, e.g., SiH x , B.H. y , GeH z , or mixtures thereof, where x, y, and z may independently be between 0 and a number less than the stoichiometric equivalent of the corresponding reducing agent compound. In some embodiments, the composition may vary through the thickness of the reducing agent layer. For example, the reducing agent layer may be 20% B at the bottom of the reducing agent layer and 0% B at the top of the layer. The total thickness of the reducing agent layer may be between 10 Å and 50 Å, and in some embodiments, between 15 Å and 40 Å, or between 20 Å and 30 Å. The reducing agent layer conformally lines along the features.
[0052] The substrate temperature during operation 502 may be maintained at temperature T1 so that the film is conformal. If the temperature is too high, the film may not conform to the topography of the underlying structure. In some embodiments, step coverage of greater than 90% or 95% is achieved. For silane, diborane, and silane / diborane mixtures, conformance is excellent at 300°C and may deteriorate at temperatures of 400°C or higher. Thus, in some embodiments, the temperature during operation 502 is at most 350°C, or at most 325°C, or at most 315°C, or at most 300°C. In some embodiments, temperatures less than 300°C are used. For example, the temperature may be as low as only 200°C.
[0053] Operation 502 may be performed for any suitable duration, including, in some examples, between about 0.25 seconds and about 30 seconds, between about 0.25 seconds and about 20 seconds, between about 0.25 seconds and about 5 seconds, or between about 0.5 seconds and about 3 seconds.
[0054] In operation 504, the chamber is optionally purged to remove excess reducing agent that has not been adsorbed to the surface of the substrate. Purging may be performed by flowing an inert gas at a constant pressure, thereby reducing the chamber pressure, and repressurizing the chamber before initiating another gas exposure. Examples of inert gases include nitrogen (N), argon (Ar), helium (He), and mixtures thereof. Purging may be performed for a duration of between about 0.25 seconds and about 30 seconds, about 0.25 seconds and about 20 seconds, about 0.25 seconds and about 5 seconds, or about 0.5 seconds and about 3 seconds.
[0055] In operation 506, the substrate is exposed to a Mo precursor at a substrate temperature T2. The use of oxygen-containing precursors can result in impurity incorporation and higher resistivity. However, if oxygen is incorporated, a very thin, possibly discontinuous, reducing agent layer may be used for acceptable resistivity. In some embodiments, a carrier gas such as nitrogen (N2), argon (Ar), helium (He), or other inert gas may be flowed during operation 506. Example temperatures are 500°C to 700°C.
[0056] Operation 506 may be performed for any suitable duration. In some embodiments, it may include a Mo precursor soak, and in some embodiments, it may include a series of Mo precursor pulses. According to various embodiments, operation 506 may or may not be performed in the presence of H. If H is used, in some embodiments, the H and Mo-containing precursor may be applied in an ALD-type mode, for example: H2 Pulse Argon purge Pulsing of Mo-containing precursors with or without H2 in the background Argon purge repetition
[0057] The substrate temperature T2 is high enough for the Mo-containing precursor to react with the reducing agent layer to form elemental Mo. The entire reducing agent layer is converted to Mo. In some embodiments, the temperature is at least 450°C, and may be at least 550°C to obtain 100% or near-100% conversion. The resulting features are now lined with a conformal Mo film. The conformal Mo film may be between 10 Å and 50 Å, and in some embodiments, between 15 Å and 40 Å, or between 20 Å and 30 Å. It will generally be about the same thickness as the reducing agent layer. In some embodiments, it may be up to 5% thicker than the reducing agent layer due to volume expansion during conversion. The chamber may be purged in operation 508.
[0058] The ALD process described with reference to Figure 4 may then be performed. The process described in Figure 5 may be used to deposit Mo directly onto oxide dielectric surfaces or surfaces that include a barrier layer such as titanium nitride (TiN).
[0059] In some embodiments, ALD Mo films may be deposited directly on oxide or TiN barrier surfaces by first depositing a metal nitride or metal oxynitride film that is converted to a pure metal film during subsequent processing. Figure 6 is a process flow diagram illustrating operations in a method for depositing molybdenum. In operation 602, a conformal nucleation layer is formed on the structure by ALD. As described above, this may include exposing the structure to cycles of successive pulses of Mo precursor and reducing agent, with optional purging between pulses. The cycle may be repeated until a nucleation layer of the desired thickness is formed on the substrate. As described above, the order of precursor and reducing agent may be reversed, such that the sequence may begin with reducing agent addition, followed by metal-containing precursor addition.
[0060] In some embodiments, the reducing agent is ammonia (NH) or other nitrogen-containing reducing agent, such as hydrazine (NH). The chemisorption of NH onto dielectrics is favored over that of hydrogen (H). In some embodiments, the reducing agent and precursor are selected to react without dissociation of the reducing agent. NH reacts with metal oxychlorides and metal chlorides without dissociation. This contrasts with, for example, ALD from metal oxychlorides, which uses H as the reducing agent; H dissociates at the surface to form adsorbed atomic hydrogen, resulting in very low concentrations of reactive species and low surface coverage during the initial nucleation of metal on the dielectric surface. The use of NH and metal oxychloride or metal chloride precursors reduces or eliminates nucleation delays at deposition temperatures up to several hundred degrees lower than those used in the H reduction of the same metal precursor.
[0061] In some embodiments, the reducing agent may be a boron- or silicon-containing reducing agent, such as B2H6 or SiH4. These reducing agents may be used with metal chloride precursors. However, when used with metal oxychlorides, B2H6 and SiH4 react with water, which is formed as a by-product during the ALD process, to form solid B2O3 and SiO2, which are insulating and remain in the film, increasing resistivity. The use of NH3 also improves adhesion over B2H6 and SiH4 ALD processes on certain surfaces, including Al2O3. The resulting nucleation layer is generally a metal nitride or metal oxynitride film rather than a pure elemental film. In some embodiments, residual chlorine or fluorine from the deposition may be present, especially if the deposition is performed at low temperatures. In some embodiments, only trace amounts of residual chlorine or fluorine are present. In some embodiments, the nucleation layer is an amorphous layer. Impurities in the film (e.g., oxygen, NH3, chlorine, or other halogens) promote the growth of an amorphous microstructure. In some embodiments, the deposited nucleation layer is an amorphous metal oxynitride layer or an amorphous metal nitride layer. The amorphous nature templates large grain growth in the subsequently deposited conductor. The surface energy of the nitride or oxynitride relative to an oxide surface is much more favorable than the surface energy of the metal relative to an oxide surface, promoting the formation of a continuous and smooth film on the dielectric. This allows for the formation of a thin, continuous layer. Example thicknesses of the nucleation layer range from 5 to 30 Å as deposited. This may be, for example, about 5 to 50 ALD cycles, depending on the temperature.
[0062] During subsequent processing, as described below, the nucleation layer may be converted to a pure (or low-impurity) elemental metal film of decreasing thickness. The surface on which the nucleation layer is deposited depends on the particular application. In some embodiments, the nucleation layer is deposited directly on a dielectric (e.g., silicon oxide, aluminum oxide, silicon nitride, etc.) surface. In some embodiments, the nucleation layer is deposited directly on a titanium nitride or other surface. By performing operation 602, subsequent elemental metal deposition may be performed on any surface, as discussed further below.
[0063] After deposition of the nucleation layer, optional operation 604 may be performed. In operation 604, a low temperature ALD cycle of pulses of a molybdenum precursor and a reducing agent is performed.
[0064] A "lower" temperature refers to a lower temperature in operation 604 than in subsequent operation 606, if performed. Example temperatures may be less than 500°C, less than 550°C, less than 450°C, less than 400°C, or less than 350°C. In this operation, the reducing agent is different from operation 602 and, in certain examples, may be hydrogen (H). In particular, H may result in the deposition of an elemental film with significantly fewer impurities than the nucleation layer. The temperature may, in some embodiments, be the same temperature as used in operation 602. The Mo precursor may also be the same or a different precursor employed in operation 602. In some embodiments, the same precursor is used, and only the reducing agent is changed. In some embodiments, operation 604 may facilitate the conversion of the Mo nitride or Mo oxynitride nucleation layer to an elemental metal film. According to various embodiments, operation 604 may or may not deposit a significant film of the main conductor.
[0065] In a further optional operation 606, the substrate temperature is increased. In some embodiments in which operation 604 is performed, operation 606 is also performed. In other embodiments, only operation 606 may be performed. For example, if the nucleation layer deposition occurs at a relatively low temperature (e.g., less than 400°C), the temperature may be increased in operation 606 to a higher temperature at which the main conductor deposition occurs. In some embodiments, the temperature may be greater than 500°C, and in some embodiments, greater than 600°C. In some embodiments, a lower temperature (e.g., between 400°C and 500°C, including the endpoint) may be used for bulk deposition. The temperature may or may not be increased depending on the temperature of the previous operation.
[0066] The method may then proceed to operation 608 (from either operation 602, 604, or 606) where a bulk Mo layer is deposited by ALD. As in operation 604 (if performed), H may be used as the reducing agent.
[0067] During one or more of operations 604-608, the nucleation layer is converted to an elemental Mo layer. This may also be characterized as removing impurities, i.e., any non-metallic components. The nucleation layer may have more impurities than the subsequently deposited elemental Mo layer, but the impurities are sufficiently removed so that the resistivity of the stack is the same or comparable to a stack without the nucleation layer. The thickness is also reduced; for example, 30 Å in the as-deposited film may contribute about 10 Å of metal to the stack.
[0068] According to various embodiments, one or more of the following may be employed to facilitate conversion of the nucleation layer to an elemental Mo film: 1) depositing the bulk Mo layer at a higher temperature (e.g., 550°C) than the nucleation layer is deposited at; 2) performing a lower temperature ALD H / metal precursor cycle, as described with reference to operation 604 above; and 3) in-situ deposition of the bulk Mo layer, whereby the nucleation layer is not exposed to air or other oxidation prior to bulk deposition. Mo oxychloride, in particular, is relatively easy to convert to elemental metal. The resulting converted nucleation layer and pure metal layer may each be characterized by atomic impurities of less than 1%.
[0069] In some embodiments, the feature onto which Mo is deposited has a dielectric and a metal surface. For example, the feature may be etched into a dielectric layer to provide contact to an underlying conductor. In such embodiments, Mo may be deposited selectively or non-selectively relative to the metal surface. Selective deposition refers to the preference for deposition onto a metal surface, such as a Co, W, or Cu surface, relative to a dielectric surface. This may be quantified as a ratio of deposition rates or as a ratio of deposition thickness after a certain number of deposition cycles. In a feature with a bottom metal surface, selective deposition results in a bottom-up fill. Non-selective deposition results in a conformal fill. To selectively deposit Mo, Mo x O x Hal z Mo oxyhalides such as may be used, where Hal is a halogen (fluorine (F), chlorine (Cl), bromine (Br), or iodine (I)), and x, y, and z are any numbers greater than 0 that can form a stable molecule. A reducing agent reacts with the molybdenum oxyhalide to form elemental molybdenum. In some embodiments, the reducing agent is thermal or plasma hydrogen (H2). Temperature affects selectivity, grain size, and resistivity. High temperatures can reduce the selectivity of Mo films and result in growth on oxides or nitrides of dielectric surfaces as well as on metal-containing basal surfaces. However, temperatures that are too low can result in high impurity levels and reduced grain size, resulting in high resistivity. The substrate temperature may be between 350°C and 600°C for selective deposition of Mo using chlorine-containing chemistries. Lowering the temperature can improve selectivity. Thus, in some embodiments, the substrate temperature may be between about 350°C and 550°C, or between 350°C and 450°C for chlorine-containing precursors. Substrate temperatures for fluorine-containing chemistries may be lower, for example, 150° C. to 350° C. Higher temperatures may be used for non-selective deposition.
[0070] In some embodiments, ALD filling of a feature with Mo can include one or more suppression and / or etching operations to tailor the fill. Nitrogen-containing chemistries can be used, for example, to suppress molybdenum nucleation. In some embodiments, exposure of the molybdenum surface to N plasma or ammonia gas can be used to selectively suppress further molybdenum nucleation at the top of the feature to promote deposition and bottom-up fill at the bottom of the feature. Halogen-containing chemistries can be used to preferentially etch deposited molybdenum at the top of the feature to promote deposition and bottom-up fill at the bottom of the feature. The suppression and etching operations may be used to prevent voids and / or seams from growing in the filled feature.
[0071] Examples of Mo precursors for the ALD of molybdenum materials include molybdenum halides such as MoF6 and MoCl6, molybdenum oxyhalides such as molybdenum dioxide dichloride (MoO2Cl2) and molybdenum oxide tetrachloride (MoOCl4), and molybdenum hexacarbonyl (Mo(CO)6). x O x Hal z Other Mo oxyhalides, where Hal is a halogen (fluorine (F), chlorine (Cl), bromine (Br), or iodine (I)), and x, y, and z are any numbers greater than 0 that can form a stable molecule. These include molybdenum oxide tetrafluoride (MoOF), molybdenum dioxide dibromide (MoOBr), molybdenum oxyiodide MoOI, and MoO. 11 Includes I.
[0072] In certain embodiments, organometallic precursors may also be used, with examples including Mo precursors with cyclopentadienyl ligands. n wherein each L is independently selected from amidate, amidinate, and guanidinate ligands, and n is 2 to 5. nThe precursor contains multiple molybdenum-molybdenum bonds (e.g., double bonds or any multiple bonds having a bond order of 2 to 5). Further examples include halide-containing heteroleptic molybdenum compounds (i.e., compounds having different types of ligands). Specific examples of such precursors are compounds containing molybdenum, at least one halide that forms a bond with the molybdenum, and at least one organic ligand having any of the elements N, O, and S, where an atom of any of these elements forms a bond with the molybdenum. Examples of suitable organic ligands providing nitrogen or oxygen bonds include amidinates, amidates, iminopyrrolidinates, diazadienes, β-iminoamides, α-iminoalkoxides, β-aminoalkoxides, β-diketiminates, β-ketoiminates, β-diketonates, amines, and pyrazolates. Examples of suitable organic ligands providing sulfur bonds include thioethers, thiolates, dithiolenes, dithiolates, and α-iminothiolenes. These ligands can be substituted or unsubstituted. In some embodiments, these ligands contain one or more substituents independently selected from the group consisting of H, alkyl, fluoroalkyl, alkylsilyl, alkylamino, and alkoxy substituents. The organic ligands can be neutral or anionic (e.g., monoanionic or dianionic), and the molybdenum can be in various oxidation states, such as +1, +2, +3, +4, +5, and +6.
[0073] As mentioned above, many Mo precursors react with reducing agents to form Mo films. Examples of reducing agents include H2, boron-containing reducing agents including diborane (B2H6) and other boranes, silicon-containing reducing agents including silane (SiH4) and other silanes, hydrazine, and germane. An example of a silane is disilane (Si2H6), and an example of a borane is B n H n+4 , B n H n+6 , B n H n+8 , B n H mIn the formula, n is an integer of 1 to 10, and m is an integer different from m. Other boron-containing compounds, such as alkylborane, alkylboron, aminoborane (CH3)2NB(CH2)2, C2B n H n+2 Carboranes such as may be used.
[0074] In some embodiments, a separate reactant may not be used; for example, the metal-containing precursor may undergo thermal or plasma-assisted decomposition. In some embodiments, H2 is used as a reducing agent for bulk layer deposition to deposit high-purity films.
[0075] In some embodiments, ALD of Mo is followed by a CVD process. The Mo precursors and co-reactants described above can be used for CVD of Mo. In such a process, the reactants are in the gas phase simultaneously within the reactor. The reactants are typically (but not necessarily) introduced into the reactor simultaneously. In one example, both MoF6 and H2 are flowed into the reactor for the CVD reaction to form Mo.
[0076] In some embodiments, ALD of Mo is followed by a CVD process to deposit W. Examples of W-containing precursors for CVD of tungsten include tungsten halides, such as tungsten hexacarbonyl (W(CO)), tungsten hexafluoride (WF), tungsten hexachloride (WCl), and tungsten pentachloride (WCl). In some embodiments, tungsten oxyhalides, including WOCl, WOBr, WOCl, and WOF, may also be used. Metalorganic precursors, such as MDNOW (methylcyclopentadienyl-dicarbonylnitrosyl-tungsten) and EDNOW (ethylcyclopentadienyl-dicarbonylnitrosyl-tungsten), may also be used. PVD of Mo or W can be performed by sputter-depositing a target material.
[0077] In some embodiments, CVD Mo deposition is preceded by deposition of a Mo nucleation layer on the ALD Mo layer. In some embodiments, the CVD Mo bulk layer is deposited directly on the ALD Mo bulk layer without an intervening nucleation layer. The nucleation layer, as described above, may be deposited by an ALD process in some embodiments.
[0078] In some embodiments, the CVD W deposition is preceded by the deposition of a W nucleation layer on the ALD Mo layer. In some embodiments, the CVD W bulk layer is deposited directly on the ALD W bulk layer without an intervening nucleation layer. The nucleation layer may be deposited by an ALD process using the W precursor and reducing agent described above.
[0079] In some embodiments, the ALD Mo layer is treated prior to CVD or PVD deposition of Mo or W. FIG. 7 illustrates a process according to certain embodiments in which the ALD Mo film is treated with a metal halide prior to CVD deposition. In FIG. 7, in operation 705, a substrate including an ALD Mo film is provided. As noted above, the feature may be part of a partially fabricated semiconductor device. In some embodiments, the substrate includes Mo and a dielectric surface. For example, referring to FIG. 1B, in some embodiments, the surface of the dielectric layer 109 may be exposed in a larger feature (not shown).
[0080] The surface of the Mo film may include oxides formed due to exposure to air or other oxidizing environments. A substrate may be provided to a processing chamber, as described further below. The Mo film is exposed to a metal halide in operation 715. The metal halide is provided as a gas to the chamber containing the substrate and may be pulsed or continuously flowed into the chamber. The metal halide can effectively reduce any oxides on the underside of features with little or no damage to the dielectric surface on the substrate. This differs from other halide processes, which can damage the dielectric. For example, nitrogen trifluoride etches the dielectric, resulting in an increase in the critical dimension of the feature. Halide compounds are more effective at removing oxidized layers than other reducing agents, such as ammonia or hydrazine.
[0081] The metal halide may be any that is volatile or has a sufficient vapor pressure to be delivered to the substrate at or below the substrate temperature. Example substrate temperatures during operation 715 range from 100°C to 450°C, and in some embodiments, from 350°C to 450°C. For some metal halides, higher temperatures may result in dielectric etching. The metal halide may include any suitable metal, including Mo, W, chromium (Cr), titanium (Ti), tantalum (Ta), and vanadium (V), as well as any halide, including fluorine F, Cl, Br, and I. Examples of tungsten halides that may be used include WF6, WCl6, tungsten pentachloride WCl5, and tungsten hexabromide WBr6. Examples of molybdenum halides that may be used include MoF6 and MoCl6. Examples of niobium halides that may be used include niobium pentachloride (NbCl5), niobium tetraiodide (NbI4), and niobium pentabromide (NbBr5). Examples of tantalum halides that can be used include tantalum pentafluoride (TaF5), tantalum pentaiodide (TaI5), and tantalum pentachloride (TaCl5). Examples of vanadium halides that can be used include vanadium pentafluoride (VF5). Examples of chromium halides that can be used include chromium pentafluoride (CrF5) and chromium diiodide (CrI2). Examples of titanium halides that can be used include titanium tetrachloride (TiCl4).
[0082] The metal halide may be mixed with an inert gas, such as argon (Ar) or helium (He). The inert gas may be used to dilute the metal halide and control the reduction rate. An example chamber pressure during operation 315 is in the range of 1 to 30 Torr. The processing time may range from 2 seconds to 4 minutes, or from 2 seconds to 60 seconds. In some embodiments, the processing time may be on the order of 2 to 3 minutes.
[0083] It is understood that exposure to a particular metal halide may include exposure to other halides formed in the gas source, gas inlet, and / or chamber. For example, WBr6 may decompose into tungsten pentabromide (WBr5) and tungsten tetrabromide (WBr4), and WF6 may decompose into tungsten pentafluoride (WF5) and tungsten tetrafluoride (WF4). Metal halides may also take various forms, including dimers and other oligomers, e.g., MoCl5 may decompose into the dimer Mo2Cl 10 The metal halide may be oxygen-free. (Some metal oxyhalides, such as molybdenum tetrachloride (MoOCl4), can etch / reduce metal oxides, but are generally less effective than metal halides. Other metal oxyhalides are described above in connection with ALD or CVD deposition.) The choice of a particular metal halide depends on the etch selectivity of the metal oxide relative to silicon oxide or other dielectric material. In 725, W is deposited on the Mo film. This can be done without a nucleation layer. Operation 725 may include a CVD or PVD process.
[0084] Although FIG. 7 shows an example of depositing W on Mo, the metal halide treatment of the ALD Mo layer may be performed prior to the deposition of any conductive material according to the integration scheme.
[0085] Operations 715 and 725 may occur in the same chamber or in different chambers, which may or may not be integrated under a common vacuum, and in some embodiments, these operations are performed in different stations of a multi-station chamber.
[0086] In some embodiments, the feature surface may be susceptible to incorporation of halogens from the metal halide during operation 715. Operation 725 may use relatively high temperatures to aid in desorption or other removal of the incorporat- ed halogens. In some embodiments, exposure to a reducing gas, such as H2, at relatively high temperatures may be used to remove residual halogens. Such operations may be performed between operations 715 and 725.
[0087] According to various embodiments, the ALD Mo film and the subsequently deposited CVD film may be deposited in the same or different chambers. Further description of apparatus for depositing ALD Mo and / or CVD Mo or CVD W is provided below. PVD deposition typically occurs in a separate chamber from the ALD Mo. In embodiments where the ALD Mo film and CVD Mo or CVD W film are deposited in the same or different chambers under a common vacuum, the CVD Mo or W deposition may occur after the ALD Mo deposition without an intervening metal halide treatment.
[0088] Device As noted above, ALD and CVD operations may be performed in the same or different chambers and in the same or different stations. FIG. 8 shows a schematic diagram of one example of a process station 800 that can be used for ALD and / or CVD. The process station 800 is in fluid communication with a reactant delivery system 801 a for delivering process gases to a distribution showerhead 806. The reactant delivery system 801 a includes a mixing vessel 804 for combining and / or conditioning process gases (such as a metal precursor-containing gas and a hydrogen-containing gas for deposition) for delivery to the showerhead 806. One or more mixing vessel inlet valves 820 may control the introduction of process gases into the mixing vessel 804.
[0089] The embodiment of Figure 8 includes a vaporization point 805 for the process solids fed into the mixing vessel 804. In another scenario, the vaporized process solids may be fed directly into the showerhead 806. Vaporization can be by sublimation or vaporization from solid to liquid to gas. With the exception of WF6 and MoF6, metal halides are generally solids at room temperature.
[0090] As an example, the embodiment of FIG. 8 includes a vaporization point 803 for vaporizing a liquid reactant supplied to the mixing vessel 804. In some embodiments, the vaporization point 803 may be a heated vaporizer. In some embodiments, the liquid precursor or liquid reactant may be vaporized in a liquid injector (not shown). For example, the liquid injector may inject a pulse of the liquid reactant into a carrier gas stream upstream of the mixing vessel 804. In one embodiment, the liquid injector may vaporize the reactant by rapidly depressurizing the liquid from a higher pressure to a lower pressure. In another example, the liquid injector may atomize the liquid into dispersed microdroplets that are then vaporized in a heated delivery tube. Smaller droplets may vaporize faster than larger droplets, reducing the delay between liquid injection and complete vaporization. Faster vaporization may reduce the length of tubing downstream from the vaporization point 803. In some scenarios, the liquid injector may be attached directly to the mixing vessel 804. In another scenario, the liquid injectors may be attached directly to the showerhead 606.
[0091] In some embodiments, a liquid flow controller (LFC) upstream of the vaporization point 803 may be provided to control the mass flow rate of the liquid for vaporization and delivery to the process chamber 802. For example, the LFC may include a thermal mass flow meter (MFM) located downstream of the LFC. The plunger valve of the LFC may then be adjusted in response to a feedback control signal provided by a proportional-integral-derivative (PID) controller in electrical communication with the MFM. However, stabilizing the liquid flow using feedback control may take one second or more, which may extend the time for adding the liquid reactant. Therefore, in some embodiments, the LFC may be dynamically switched between feedback control mode and direct control mode. In some embodiments, this may be accomplished by disabling the sense tubes of the LFC and the PID controller.
[0092] 8, the substrate 812 is located below the showerhead 806 and is shown resting on a pedestal 808. The showerhead 806 may have any suitable shape and any suitable number and arrangement of ports for delivering process gases to the substrate 812.
[0093] In some embodiments, the pedestal 808 may be raised or lowered to expose the substrate 812 to a volume between the substrate 812 and the showerhead 806. In some embodiments, the pedestal 808 may be temperature controlled via a heater 810. The pedestal 808 may be set to any suitable temperature, such as between about 150° C. and about 600° C., during operation to perform various disclosed embodiments. It will be appreciated that in some embodiments, the height of the pedestal may be programmatically adjusted by a suitable computer controller 850. At the end of a process stage, the pedestal 808 may be lowered during another substrate transfer stage to allow removal of the substrate 812 from the pedestal 808.
[0094] In some embodiments, the position of the showerhead 806 may be adjusted relative to the pedestal 808 to change the volume between the substrate 812 and the showerhead 806. Furthermore, it will be understood that the vertical position of the pedestal 808 and / or the showerhead 806 may be changed by any suitable mechanism within the scope of the present disclosure. In some embodiments, the pedestal 808 may include a rotation axis for rotating the orientation of the substrate 812. It will be understood that in some embodiments, one or more of these adjustments may be performed programmatically by one or more suitable computer controllers 850.
[0095] In some embodiments where the plasma may be used for PECVD or PEALD, the showerhead 806 and pedestal 808 are in electrical communication with a radio frequency (RF) power source 814 and matching network 816 to power the plasma. In some embodiments, the plasma energy may be controlled by controlling one or more of the process station pressure, gas concentration, RF source power, RF source frequency, and plasma power pulse timing. For example, the RF power source 814 and matching network 816 may be operated at any suitable power to form a plasma having a desired composition of radical species. Similarly, the RF power source 814 may provide RF power at any suitable frequency. In some embodiments, the RF power source 814 may be configured to control high-frequency and low-frequency RF power sources independently of each other. Examples of low-frequency RF frequencies may include, but are not limited to, frequencies between 0 kHz and 900 kHz. Examples of high frequency RF frequencies may include, but are not limited to, frequencies between 1.8 MHz and 2.45 GHz, or frequencies greater than about 13.56 MHz, or greater than 27 MHz, or greater than 80 MHz, or greater than 60 MHz. It will be appreciated that any suitable parameters may be adjusted, either discretely or continuously, to provide plasma energy for surface reactions.
[0096] In some embodiments, the plasma may be monitored in situ by one or more plasma monitors. In one scenario, plasma power may be monitored by one or more voltage and current sensors (e.g., VI probes). In another scenario, plasma density and / or process gas concentration may be measured by one or more optical emission spectroscopy (OES) sensors. In some embodiments, one or more plasma parameters may be programmatically adjusted based on measurements from such in situ plasma monitors. For example, OES sensors may be used in a feedback loop to provide programmatic control of plasma power. It will be understood that in some embodiments, other monitors may be used to monitor the plasma and other process characteristics. Such monitors may include, but are not limited to, infrared (IR) monitors, acoustic monitors, and pressure transducers.
[0097] In some embodiments, instructions to the controller 850 may be provided via input / output control (IOC) sequencing instructions. In one example, instructions for setting conditions for a process step may be included in a corresponding recipe step of a process recipe. In some cases, process recipe steps may be sequentially arranged such that all instructions for a process step are executed simultaneously with that process step. In some embodiments, instructions for setting one or more reactor parameters may be included in a recipe step.
[0098] For example, in the case of ALD deposition, a first recipe step may include instructions for adjusting the flow rate of a first reactant gas (e.g., Mo precursor gas), instructions for adjusting the flow rate of a carrier gas or purge gas, and a time delay instruction for the first recipe step. A second, subsequent recipe step may include instructions for adjusting or stopping the flow rate of a reactant gas (e.g., H), instructions for adjusting the flow rate of a carrier gas or purge gas, and a time delay instruction for the second recipe step. It will be understood that these recipe steps may be further subdivided and / or repeated in any suitable manner within the scope of the present disclosure.
[0099] Additionally, in some embodiments, pressure control of the process station 800 may be provided by a butterfly valve 818. As shown in the embodiment of Figure 8, the butterfly valve 818 throttles the vacuum provided by a downstream vacuum pump (not shown). However, in some embodiments, pressure control of the process station 800 may also be adjusted by varying the flow rate of one or more gases introduced to the process station 800.
[0100] As described above, the ALD Mo and subsequent CVD operations may be performed in a single station of a single or multi-station chamber, in different stations of a multi-station chamber, or in different chambers. If performed in different chambers, the chambers may be integrated under a common vacuum environment to prevent oxidation of the ALD Mo deposition. Similarly, the metal halide treatment (if performed) may be performed in the same or a different chamber as the subsequent CVD treatment. Also, the chambers may be under a common vacuum to prevent oxidation after the metal halide treatment and metal oxide removal. In some embodiments, the metal halide treatment may not be integrated, at least for a relatively short time, providing a passivation effect to prevent oxidation.
[0101] 9 illustrates an example of a processing system including multiple chambers. System 900 includes a transfer module 903. Transfer module 903 provides a clean vacuum environment to minimize the risk of contamination as the substrate being processed moves between various reactor modules. Attached to transfer module 903 is a multi-station reactor 909 capable of performing ALD and CVD according to embodiments. In some embodiments, reactor 909 also performs a metal halide exposure prior to CVD. Nucleation layer deposition (if performed) may be performed in the same or a different station or chamber as the subsequent bulk layer deposition.
[0102] Reactor 909 may include multiple stations 911, 913, 915, and 917 that may sequentially perform operations according to disclosed embodiments. For example, reactor 909 may be configured such that station 911 performs ALD Mo deposition, station 913 performs a metal halide reduction process as described with respect to Figure 7, and stations 915 and 917 perform bulk layer deposition CVD. In another example, reactor 909 may be configured such that station 911 performs ALD nucleation layer deposition as described with respect to Figure 6, station 913 performs ALD deposition of bulk Mo, and stations 915 and 917 perform CVD.
[0103] Two or more stations, e.g., two to six stations, may be included in a multi-station reactor, with appropriate distribution of operations. For example, a two-station reactor may be configured to expose a substrate to a metal halide in a first station, followed by CVD deposition in a second station. As described above with respect to FIG. 8, a station may include a heated pedestal or substrate support, one or more gas inlets, a showerhead, or a distribution plate.
[0104] Transfer module 903 may also be fitted with one or more single or multi-station modules 907. In some embodiments, ALD may be performed in module 907, after which the substrate is transferred under vacuum to another module (e.g., another module 907 or reactor 909) for CVD or PVD deposition.
[0105] The system 900 also includes one or more wafer source modules 901 where wafers are stored before and after processing. An atmospheric robot (not shown) in an atmospheric transfer chamber 919 may initially remove wafers from the source modules 901 to a load lock 921. A wafer transfer device (typically a robot arm unit) in a transfer module 903 moves wafers from the load lock 921 to and between modules mounted on the transfer module 903.
[0106] In some embodiments, ALD deposition of Mo occurs in a first chamber, which may be part of a system such as system 900, and CVD or PVD deposition of W or other conductive material occurs in a separate chamber, which may not be connected to a common transfer module but is part of a separate system. In such cases, the substrate may be delivered to a source module of the separate system for optional metal halide processing and CVD or PVD deposition.
[0107] In various embodiments, a system controller 929 is employed to control process conditions during deposition. The controller 929 typically includes one or more memory devices and one or more processors. The processor may include a CPU or computer, analog and / or digital input / output connections, stepper motor controller boards, etc.
[0108] A controller 929 may control all activity of the apparatus. The system controller 929 executes system control software, which includes sets of instructions for controlling the timing, mixture of gases, chamber pressure, chamber temperature, wafer temperature, radio frequency (RF) power levels, wafer chuck or pedestal position, and other parameters of a particular process. Other computer programs stored in memory devices associated with the controller 929 may be employed in some embodiments.
[0109] Typically, there is a user interface associated with the controller 929. The user interface may include a display screen, a graphical software display of equipment and / or process conditions, and user input devices such as a pointing device, keyboard, touch screen, microphone, etc.
[0110] The system control logic may be configured in any suitable manner. In general, logic can be designed or configured in hardware and / or software. Instructions for controlling the drive circuitry may be hard-coded or provided as software. The instructions may be provided by "programming." Such programming is understood to include any form of logic, including hard-coded logic in digital signal processors, application-specific integrated circuits, and other devices that implement specific algorithms as hardware. Programming is also understood to include software or firmware instructions that may be executed on a general-purpose processor. The system control software may be coded in any suitable computer-readable programming language.
[0111] The computer program code for controlling the germanium-containing reducing agent pulses, hydrogen flow, and tungsten-containing precursor pulses, as well as other processes in the process sequence, can be written in any conventional computer-readable programming language, such as assembly language, C, C++, Pascal, Fortran, etc. The compiled object code or script is executed by a processor to perform the tasks specified in the program. Also, as shown, the program code may be hard-coded.
[0112] The controller parameters relate to process conditions such as, for example, process gas composition and flow rates, temperature, pressure, cooling gas pressure, substrate temperature, and chamber wall temperature, etc. These parameters may be provided to the user in the form of a recipe and entered using a user interface.
[0113] Signals for monitoring the process may be provided by analog and / or digital input connections of the system controller 929. Signals for controlling the process are output at analog and digital output connections of the deposition tool.
[0114] The system software may be designed or configured in many ways. For example, various chamber component subroutines or control objects may be written to control the operation of the chamber components necessary to perform a deposition process in accordance with the disclosed embodiments. Examples of programs or sections of programs for this purpose include substrate positioning code, process gas control code, pressure control code, and heater control code.
[0115] In some embodiments, the controller 929 is part of a system, which may be part of the examples described above. Such a system may include semiconductor processing equipment, including one or more processing tools, one or more chambers, one or more processing platforms, and / or specific processing components (such as a wafer pedestal, gas flow system, etc.). These systems may be integrated with electronics for controlling their operation before, during, and after processing of semiconductor wafers or substrates. The electronics, sometimes referred to as a "controller," may control various components or subparts of one or more systems. Depending on the processing requirements and / or type of system, the controller 929 may be programmed to control any of the processes disclosed herein, including delivery of process gases, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, radio frequency (RF) generator settings in some systems, RF matching circuit settings, frequency settings, flow rate settings, liquid delivery settings, position and motion settings, wafer transfer into and out of the tool, and wafer transfer into and out of other transport tools and / or load locks connected or interfaced with the particular system.
[0116] Broadly speaking, a controller may be defined as an electronic device having various integrated circuits, logic, memory, and / or software that receive instructions, issue instructions, control operations, enable cleaning operations, enable endpoint measurements, etc. Integrated circuits may include chips in the form of firmware that store program instructions, digital signal processors (DSPs), chips defined as application-specific integrated circuits (ASICs), and / or one or more microprocessors or microcontrollers that execute program instructions (e.g., software). Program instructions may be instructions communicated to the controller in the form of various individual settings (or program files) that define operational parameters for performing a particular process on or for a semiconductor wafer or for a system. The operational parameters, in some embodiments, may be part of a recipe defined by a process engineer to accomplish one or more processing steps during the manufacture of one or more layers, materials, metals, oxides, silicon, silicon dioxide, surfaces, circuits, and / or dies of a wafer.
[0117] In some embodiments, the controller 929 may be part of or connected to a computer that is integrated into the system, connected to the system, otherwise networked to the system, or a combination thereof. For example, the controller 929 may be all or part of a “cloud,” i.e., fab host computer system, enabling remote access to wafer processing. The computer may enable remote access to the system to monitor the current progress of a manufacturing operation, examine the history of past manufacturing operations, examine trends or performance criteria from multiple manufacturing operations, modify parameters of a current process, configure processing steps to track a current process, or initiate a new process. In some examples, a remote computer (e.g., a server) can provide process recipes to the system over a network, which may include a local network or the Internet. The remote computer may include a user interface that allows entry or programming of parameters and / or settings, which are then communicated from the remote computer to the system. In some examples, the controller receives instructions in the form of data specifying parameters for each of the processing steps to be performed during one or more operations. The parameters may be specific to the type of process being performed and the type of tool the controller is configured to interface with or control. Thus, as described above, the controller may be distributed, such as by including one or more individual controllers networked together and operating toward a common purpose, such as the processes and controls described herein. One example of a distributed controller for such purposes is one or more integrated circuits on the chamber that are located remotely (e.g., at the platform level or as part of a remote computer) and communicate with one or more integrated circuits that cooperatively control the processes in the chamber.
[0118] Examples of systems may include, but are not limited to, a plasma etch chamber or module, a deposition chamber or module, a spin rinse chamber or module, a metal plating chamber or module, a cleaning chamber or module, a bevel edge etch chamber or module, a PVD chamber or module, a CVD chamber or module, an ALD chamber or module, an atomic layer etch (ALE) chamber or module, an ion implantation chamber or module, a track chamber or module, and any other semiconductor processing system that may be associated with or used in the fabrication and / or manufacturing of semiconductor wafers.
[0119] As described above, depending on the process step or steps being performed by the tool, the controller may communicate with one or more of other tool circuits or modules, other tool components, cluster tools, other tool interfaces, adjacent tools, nearby tools, tools located throughout the factory, a main computer, another controller, or tools used to transport materials to and from tool locations and / or load ports of wafers within a semiconductor fabrication factory.
[0120] The controller 929 may include a variety of programs. A substrate positioning program may include program code for controlling chamber components used to load the substrate onto the pedestal or chuck and control spacing between the substrate and other parts of the chamber, such as the gas inlets and / or target. A process gas control program may include code for controlling gas composition, flow rates, and pulse times, as well as code for optionally flowing gas into the chamber before deposition to stabilize the pressure in the chamber. A pressure control program may include code for controlling the pressure in the chamber, for example, by adjusting a throttle valve in the chamber's exhaust system. A heater control program may include code for controlling current to a heating unit used to heat the substrate. Alternatively, the heater control program may control the delivery of a heat transfer gas, such as helium, to the wafer chuck.
[0121] Examples of chamber sensors that may be monitored during deposition include mass flow controllers, pressure sensors such as manometers, and thermocouples located on the pedestal or chuck. Appropriately programmed feedback and control algorithms may be used with data from these sensors to maintain desired process conditions.
[0122] The above describes the implementation of the disclosed embodiments in single-chamber or multi-chamber semiconductor processing tools. The apparatus and processes described herein may be used in conjunction with lithographic patterning tools or processes, for example, for the manufacture or production of semiconductor devices, displays, LEDs, solar panels, etc. Typically, although not necessarily, such tools / processes are used or performed together in a common manufacturing facility. Lithographic patterning of films typically involves some or all of the following steps, with each step providing several possible tools: (1) applying photoresist onto a workpiece, i.e., substrate, using a spin-on or spray-on tool; (2) curing the photoresist using a hotplate, furnace, or UV curing tool; (3) exposing the photoresist to visible, UV, or X-ray light using a tool such as a wafer stepper; (4) developing the resist to selectively remove and thereby pattern the resist using a tool such as a wet bench; (5) transferring the resist pattern into the underlying film or workpiece using a dry etching or plasma-assisted etching tool; and (6) removing the resist using a tool such as an RF or microwave plasma resist stripper.
[0123] conclusion Although the foregoing embodiments have been described in some detail for purposes of clarity of understanding, it will be apparent that certain changes and modifications may be practiced within the scope of the appended claims. It should be noted that there are many alternative ways of implementing the processes, systems, and apparatus of the present embodiments. Accordingly, the present embodiments are to be considered as illustrative and not restrictive, and the present embodiments are not to be limited to the details given herein.
Claims
1. 1. A method comprising: depositing a bulk layer of molybdenum (Mo) by atomic layer deposition (ALD) in a structure including a plurality of features to at least partially fill the plurality of features with Mo; depositing a bulk layer of tungsten (W) on said bulk layer of Mo by chemical vapor deposition (CVD) or physical vapor deposition (PVD); A method comprising:
2. 2. The method of claim 1 , wherein the plurality of features includes a first set of one or more features having a first critical dimension and a second set of one or more features having a second critical dimension, the first critical dimension being smaller than the second critical dimension, and wherein filling of the first set of features is completed by depositing a bulk layer of Mo and filling of the second set of features is completed by depositing a bulk layer of W.
3. The method of claim 1 , wherein the filling of at least a portion of the plurality of features is completed with a bulk layer of W.
4. 2. The method of claim 1, wherein the bulk layer of W is deposited only over top surfaces of the plurality of features and not within the plurality of features.
5. The method of claim 4 further comprising removing all of the W bulk layer.
6. 10. The method of claim 1, wherein the features include an oxide surface prior to any Mo deposition in the features.
7. 7. The method of claim 6, wherein the Mo is formed in the plurality of features, and no barrier layer is disposed between the formed Mo and the oxide surface.
8. 10. The method of claim 1 further comprising depositing a nucleation layer prior to depositing the bulk layer of Mo.
9. 9. The method of claim 8, wherein depositing the nucleation layer comprises forming a layer of molybdenum nitride or molybdenum oxynitride.
10. 10. The method of claim 9, further comprising converting the layer of molybdenum nitride or molybdenum oxynitride to molybdenum.
11. 2. The method of claim 1, wherein the bulk layer of Mo and the bulk layer of W are deposited in the same chamber.
12. 12. The method of claim 11, wherein the bulk layer of Mo and the bulk layer of W are deposited at different stations in the same chamber.
13. 10. The method of claim 1, wherein the bulk Mo layer and the bulk W layer are deposited in different chambers.
14. The method of claim 13 , wherein the different chambers are connected to a common vacuum environment.
15. The method of claim 14 , wherein the different chambers are not connected to a common vacuum environment.
16. 2. The method of claim 1, further comprising treating a surface of the deposited bulk Mo layer with a metal halide prior to depositing the bulk W layer.
17. 10. The method of claim 1, wherein the depositing a bulk layer of Mo by atomic layer deposition (ALD) comprises exposing the structure to alternating pulses of a Mo precursor and a co-reactant.
18. 18. The method of claim 17, wherein the Mo precursor is a molybdenum halide or a molybdenum oxyhalide.
19. 19. The method of claim 18, wherein the Mo precursor is molybdenum hexafluoride (MoF 6 ), molybdenum pentachloride (MoCl 5 ), molybdenum dioxide dichloride (MoO 2 C 2 ), molybdenum oxide tetrachloride (MoOCl 4 ), molybdenum hexacarbonyl (Mo(CO) 6 ), (MoOF 4 ), molybdenum dioxide dibromide (MoO 2 B 2 ), MoO 2 I, and Mo 4 O 11 The method is one of I.
20. 18. The method of claim 17, wherein the Mo precursor is an organometallic precursor.
21. 1. A method comprising: providing a structure in a chamber, the structure including a first set of features; depositing a bulk layer of molybdenum (Mo) by atomic layer deposition (ALD) in a structure including a first set of features to partially fill the features with Mo; removing the structure including the feature partially filled with Mo from the chamber; A method comprising:
22. 1. A method comprising: providing a structure in a chamber including a first set of features, the first set of features being at least partially filled with molybdenum (Mo); depositing a bulk layer of tungsten (W) on the Mo; A method comprising: