Controlled casting of large steel ingots in molds using induction variable power and variable frequency.

JP2023550614A5Active Publication Date: 2024-11-07INDUCTOTHERM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023530324
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-11-20
Filing Date
2021-11-19
Publication Date
2024-11-07
Estimated Expiration
2041-11-19

AI Technical Summary

Technical Problem

Casting large steel ingots is time-consuming and prone to structural defects due to uneven solidification, leading to reduced quality and increased waste from non-metallic inclusions.

Method used

Employ a variable power and frequency induction heating system to control the solidification process from bottom to top, using a pancake-shaped induction coil suspended above the mold, with a variable power supply to maintain the top molten state and electromagnetic stirring to reduce defects.

Benefits of technology

This method significantly reduces casting defects and improves the quality of steel ingots by ensuring gradual solidification and minimizing impurities, resulting in high-quality products.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Large steel ingots are cast using overhead induction heaters powered by variable power and frequency. The overhead induction heaters provide induction heating and stirring, gradually solidifying the metal from bottom to top, with the molten metal above the feeder section compensating for the shrinkage of the solidified metal below the main section. Variable electromagnetic stirring forces selectively remove inclusions from the molten metal, reducing the formation of casting defects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Cross - Reference to Related Applications This application claims the benefit of U.S. Provisional Application No. 63 / 116,455, filed on November 20, 2020, which is hereby incorporated by reference in its entirety.

[0002] The present invention generally relates to the casting of large amounts of metal ingots, and more particularly to the casting of large - volume steel ingots, such as suspending a pancake - type coil or a similar induction heating device above the upper surface of molten metal to supply induction heating power and electromagnetic stirring force to the molten material in the mold. The process of induction heating and electromagnetic stirring delays the solidification of the material at a portion higher than the solidification line of the mold, causing the upper molten metal to cool and solidify more slowly than the lower molten metal. A general objective is to make the solidification of the metal proceed gradually from bottom to top, so that the upper molten metal compensates for the shrinkage of the lower solidified metal, and selective defects move due to the stirring force of variable power and variable frequency supplied to the induction heating device. The advantage of this technology is to reduce casting defects and improve the quality of the final ingot product.

Background Art

[0003] Casting large - scale steel ingots requires a considerable amount of molten material in the mold, thus requiring a relatively long time. Correspondingly, large shrinkage may occur in the ingot during the solidification process, which leads to large structural defects and ultimately reduces the quality of the cast product. Therefore, a casting method appropriately designed mainly to optimize the solidification process is desired.

[0004] A typical casting process for large steel ingots involves pouring molten material into a mold and allowing the molten metal to cool until it is completely solidified. This process periodically requires riser space, which is extra void within the mold filled with molten material to compensate for shrinkage during solidification. As the steel is poured into the ingot mold, solidification begins gradually from the mold walls and base, moving inward towards the thermal center or axis. Liquid steel decreases in volume during and after solidification, and if the molten material in the riser solidifies faster or at the same pace as the material in the main part of the mold, there will be insufficient solid metal to fill the initially formed shell. This results in a steel body with cavitation, particularly in the areas of the metal that solidify last. Such cavitation is also associated with impurities concentrated by segregation, which creates an undesirable distribution of undesirable elements in the final product.

[0005] Traditionally, various approaches have been applied to maintain the material in the riser in a molten state until the metal in the main part of the ingot mold has completely solidified. This is based on the recognition that gradually solidifying the molten metal from bottom to top is important for the quality of the final product.

[0006] Korean Patent No. 10-2123914 (hereinafter referred to as Korean Patent '914) discloses a steel ingot casting technology that uses a pancake-shaped electric induction heating device in which the internal coils are arranged in a spiral shape and grouted with refractory material attached to and suspended from the top of the mold. The ingot casting procedure using this technology consists of four steps: in the first step, molten steel is poured into the mold, for example from the bottom inlet; in the second step, heating material and insulating material are added to the top surface of the molten steel in the mold; in the third step, the induction heating device is lowered to the required position adjacent to the top surface of the molten metal; and in the fourth step, an alternating current of a specific frequency is passed through the coil to heat the metal until it is completely solidified. The advantage of this technology is that the top of the metal is kept in a molten state and solidification proceeds gradually from bottom to top. Thus, the molten metal at the top compensates for the shrinkage of the solidified metal at the bottom and reduces structural defects.

[0007] Korean Patent '914 describes an overhanging induction heating device, along with a provided heating agent (material) and insulating agent (material), which aims to maintain the metal in a molten state at the top of the mold, which is important for eliminating internal defects in the final product. Structural defects in the final product include macrosegregation, shrinkage porosity, and inclusions. In terms of eliminating inclusions, the advantage of induction heating is the control of the solidification direction and the overall solidification time.

[0008] In the case of cast steel, nonmetallic inclusions are classified into intrinsic and extrinsic inclusions depending on their source. Intrinsic inclusions are deoxygenation products or precipitates formed during the cooling and solidification process. For example, nonmetallic substances trapped by the growth of dendrites. Extrinsic inclusions arise from unintended chemical and mechanical reactions between the molten steel and its environment, leading to ingot defects such as pores and pinholes. Some nonmetallic inclusions tend to flow into the upper layers of the molten metal and become trapped in the slag, eventually being disposed of by separating them from the final product. Discarded cutoffs are unusable and typically account for 13-15% of the final product. [Prior art documents] [Patent Documents]

[0009] [Patent Document 1] Korean Registered Patent Publication No. 10-2123914 [Overview of the Initiative] [Problems that the invention aims to solve]

[0010] There is always a demand for clean steel, a defect-free material, for use in challenging applications such as automotive parts and components used in corrosive environments.

[0011] One objective of the present invention is to further reduce defects in ingot products when casting by coordinating the induction power and frequency supplied to an overhanging induction heating device. [Means for solving the problem]

[0012] In one embodiment, the present invention includes a system and method specifically for large ingot mold casting applications. Here, an electric induction heating device is used to induce thermal energy and electromagnetic stirring force in the casting metal through an induction heating coil supplied with alternating current from a power source having variable power and variable frequency output, thereby maintaining the top of the molten metal and gradually advancing the solidification process from bottom to top. The advantage of maintaining the top of the molten casting metal in a molten state and using electromagnetic stirring force is that structural defects are greatly reduced and the quality of the final ingot product is improved.

[0013] In another embodiment, the present invention includes an induction heating device mounted and suspended above a casting mold, and a power supply having variable power and variable frequency output to heat the molten steel in the mold and power the induction heating device for ingot production. The induction heating device includes an induction coil, a refractory that fixes the coil and embeds the induction coil therein to reduce heat dissipation from the molten metal, and a lifting device for raising and lowering the induction coil. The power supply is configured to provide alternating current in a range of frequencies and power rates that best match the requirements of heating energy and stirring force from the solidification process to reduce casting defects.

[0014] In another embodiment, the present invention is a method for manufacturing an ingot using an induction heating device suspended above a mold, wherein a variable power and variable frequency power supply provides power to the induction heating device. The ingot casting process employing this technology consists of four steps: in the first step, molten steel is poured into the mold from a bottom inlet; in the second step, heating and insulating material is added to the top surface of the molten steel in the mold; in the third step, the induction heating device is lowered to a position for preheating the refractory material to the refractory preheating temperature; in the fourth step, in order to heat the casting metal, an alternating current of molten metal heating frequency is applied to the coil from a variable power and variable frequency power supply, and the top of the metal is kept in a molten state as solidification gradually begins from the bottom upward, and the electromagnetic stirring speed is increased and the movement of inclusions is accelerated by controlling the variable frequency output from the variable power and variable frequency power supply.

[0015] In certain applications of this method, the cavity of the ingot mold can be divided into a main section and a riser section. In the fourth step described above, the heating process can be started when the solidification of the main section is completely finished and the metal in the riser is still molten.

[0016] In another embodiment, the present invention includes an upper induction heater mounted and suspended above a casting mold, and a power supply having variable power and variable frequency output to supply power to the induction heater. The upper induction heater and power supply are configured for metal ingot production. The upper induction heater is configured as a pancake-shaped refractory with helically arranged induction coils embedded within it. The induction coils are grouted inside the pancake-shaped refractory, and the grouted coils are covered layer by layer from the inside out using shellac wool, insulating material, and castable cement. These structures form a solid body of an induction heater that can be raised and lowered by a hoisting device.

[0017] The above embodiments of the present invention are particularly applicable to modifying existing ingot molds, as the electric induction heating device is positioned above the molten metal surface. However, the present invention is not limited to modification applications.

[0018] The above and other aspects of the present invention are described in this specification and the appended claims.

[0019] The drawings briefly summarized below are provided for illustrative understanding of the present invention and do not limit the present invention further described in this specification and the appended claims.

Brief Description of the Drawings

[0020] [Figure 1] Figure 1 is a simplified schematic view of an embodiment of a molten steel ingot casting system of the present invention. [Figure 2(a)] Figure 2(a) is a schematic view of a large mold filled with molten steel at the start of directional solidification. [Figure 2(b)] Figure 2(b) is a schematic diagram when half of the main body of the molten steel has solidified. [Figure 2(c)] Figure 2(c) is a graphical representation when all of the molten steel has solidified. [Figure 3(a)] Figure 3(a) is a parametric model of adjustable selectable ranges of voltage, current (power) values, and frequency values as the output from a variable power and variable frequency power supply to an electric induction heating coil in an example of the present invention for manufacturing a 100 metric ton large steel ingot with a nominal 250 kW induction power from the power supply. [Figure 3(b)] Figure 3(b) is a parametric model of adjustable selectable ranges of voltage, current (power) values, and frequency values as the output from a variable power and variable frequency power supply to an electric induction heating coil in an example of the present invention for manufacturing a 100 metric ton large steel ingot with a nominal 250 kW induction power from the power supply. [Figure 4(a)] Figure 4(a) is a parametric model of adjustable selectable ranges of voltage, current (power) values, and frequency values as the output from a variable power and variable frequency power supply to an electric induction heating coil in an example of the present invention for manufacturing a 100 metric ton large steel ingot with a nominal 325 kW induction power from the power supply. [Figure 4(b)]Figure 4(b) is a parametric model of the adjustable selectable range of voltage, current (power) values, and frequency values as the output from a variable power and variable frequency power supply to an electric induction heating coil in an example of the present invention for manufacturing a large steel ingot of 100 metric tons with a nominal induction power of 325 kW from a power supply. [Figure 5(a)] Figure 5(a) is a parametric model of the adjustable selectable range of voltage, current (power) values, and frequency values as the output from a variable power and variable frequency power supply to an electric induction heating coil in an example of the present invention for manufacturing a large steel ingot of 150 metric tons with a nominal induction power of 250 kW from a power supply. [Figure 5(b)] Figure 5(b) is a parametric model of the adjustable selectable range of voltage, current (power) values, and frequency values as the output from a variable power and variable frequency power supply to an electric induction heating coil in an example of the present invention for manufacturing a large steel ingot of 150 metric tons with a nominal induction power of 250 kW from a power supply. [Figure 6(a)] Figure 6(a) is a parametric model of the adjustable selectable range of voltage, current (power) values, and frequency values as the output from a variable power and variable frequency power supply to an electric induction heating coil in an example of the present invention for manufacturing a large steel ingot of 150 metric tons with a nominal induction power of 350 kW from a power supply. [Figure 6(b)] Figure 6(b) is a parametric model of the adjustable selectable range of voltage, current (power) values, and frequency values as the output from a variable power and variable frequency power supply to an electric induction heating coil in an example of the present invention for manufacturing a large steel ingot of 150 metric tons with a nominal induction power of 350 kW from a power supply.

Embodiments for Carrying Out the Invention

[0021] A "large" steel casting ingot is defined in this specification as an ingot having a cross-section with an area of at least 0.10 square meters and being circular, square, rectangular, or of other shapes.

[0022] Figure 1 shows one embodiment of the system 10 of the present invention for manufacturing large steel ingots by solidifying molten steel in a mold. In Figure 1, the mold 80 is filled with molten steel through a bottom mold inlet 80', and an electric induction heating device 14 is positioned above the mold 80. The molten steel (also called "molten metal") is poured from the bottom mold inlet up to a molten metal filling height 78. In other embodiments of the present invention, a top-pore casting mold is used. Once the mold 80 is filled with molten steel up to a molten metal filling height 78, directional solidification of the molten steel begins, forming the final steel ingot product. The molten steel 70 in the mold (from the bottom of the mold 80a to the molten metal filling height 78 is referred to as the main portion 70a and the riser portion 70b. In this schematic diagram, the riser portion begins at the mold height 74 and ends at the molten metal filling height 78. The size of the riser portion 70b can be determined by those skilled in the art, taking into account the size of the large steel ingot for a particular application and the solidification process parameters.

[0023] The first step of the process is to determine the magnitude of the induced power to the molten steel in the mold. In one embodiment of the present invention, the initial value of the induced power is selected as 10 kW per square meter of the upper surface area of ​​the molten steel in the mold.

[0024] In alternative embodiments of the present invention, the electric induction heating device 14 includes an electric induction heating coil; a helically wound flat induction heating coil; or an electric induction heating coil at least partially encased in refractory material. Korean Patent '914 discloses a refractory-encased pancake-shaped heating coil as an example of an electric induction heating device suitable for the present invention. Preferably, one or more coils are configured to be initially positioned adjacent to the upper surface region of the molten steel in the casting mold at a molten metal filling height 78.

[0025] In Figure 1, d osThe offset distance shown as is the distance between the upper surface region of the molten steel and the bottom of the induction heating device 14. The electric induction heating device 14 can be mounted movably over the upper surface region of the molten steel via a suitable lifting device known in the art. Korean Patent '914 discloses a lifting device for raising and lowering a pancake-shaped heating device as an example of a lifting device suitable for the present invention. In some embodiments of the present invention, the distance d os This changes by raising or lowering the induction heating device during the directional solidification of the molten metal forming a large steel ingot. When the bottom of the induction heating device is brought closer to the molten metal surface, the electrical efficiency improves with respect to the predetermined power supplied to the molten metal that generates the total power. Since the Lorentz force is proportional to the melting force, the electromagnetic repulsion force remains the same, but the voltage and current from the output of the variable power variable frequency (VP / VF) power supply PS decrease.

[0026] In some embodiments of the present invention, the casting mold has an upper mold section that covers a bottom mold section containing molten steel to form a completely sealed internal mold volume, and an induction heating device is positioned relative to the upper mold section to supply induction heat during the directional solidification of a large steel ingot.

[0027] The molten steel 70 in the mold 80 is schematically shown at the molten metal filling height 78 in Figure 1 at the start of the directional solidification process. Once the directional solidification of all the molten metal is complete, the final solidified large steel ingot 90 is obtained, as shown in Figure 2(c).

[0028] Variable power and variable frequency are supplied from the VP / VF power supply PS shown in Figure 1. In some embodiments of the present invention, variable power is provided from the VP / VF power supply PS by changing the magnitude of the voltage output from, for example, a variable voltage output controller associated with the VP / VF power supply PS. In other embodiments of the present invention, variable power is provided by changing the combination of voltage magnitude and current magnitude output from the VP / VF power supply PS, for example, a variable voltage and current output controller associated with the VP / VF power supply PS.

[0029] The variable frequency, voltage, and current values ​​of the alternating current supplied from the VP / VF power supply PS to the induction heating device 14 are determined by a specific directional solidification process time, the duration of which is further determined by the size and shape of the ingot and the chemical composition of the casting material. Process control parameters are selected such that the molten metal in the riser portion 70b does not begin to solidify until the directional solidification process of the main portion 70a is completely finished in the formation of the main ingot portion.

[0030] In some embodiments of the present invention, a variable frequency is selected to control the reference depth of the through-current into the molten steel, so that the reference depth of the through-current remains within the riser portion 70b. By limiting the reference current depth to the riser portion, the molten steel is kept in a molten state in the riser portion, the heat generated in the riser portion is transferred to the main portion by conduction and convection, and directional solidification is ensured in the main portion.

[0031] In some embodiments of the present invention, a variable frequency output from a power supply PS is selected to suppress the occurrence of casting defects in the directional solidification of the main portion 70a, and the frequency is selected to form a specific type of electromagnetic stirring pattern and speed depending on the type of casting defect.

[0032] In some embodiments of the present invention, a human-machine interface can be utilized to store variable power output values ​​and variable frequency output values ​​of a power supply for future large ingot casting processes. In some embodiments of the present invention, real-time ingot-directed solidification process control by VP / VF power supply PS to induction coils in an induction heating device 14 for a given mold, and steel alloy casting formulas used to construct parametric models of process power and frequency control for casting future ingots in the same mold using the same alloy casting formulas, can be stored in a memory unit of a human-machine interface (HMI) for casting future ingots.

[0033] In some embodiments of the present invention, control parameters for a given mold and steel alloy type directional solidification process can be stored for future use in a suitable electronic device, such as a solid-state memory component of a human-machine interface (HMI) shown in Figure 1. The power rate and frequency, and the established control parameters, are fixed as a formula by casting process software running on the HMI's system processor and stored in the HMI's solid-state memory component for further use.

[0034] Figures 3(a) to 6(b) show parametric models of four examples of the present invention for controlled casting by in-mold large steel ingot casting using inductive variable power and variable frequency applied to the upper surface region of molten metal in the model.

[0035] The upper half of each of Figures 3(a) to 6(a) plots the typical parametric relationship between the magnitude of the variable output voltage of the power supply (value on the right vertical axis) and the magnitude of the variable current (value on the left vertical axis) (the variable frequency value is referenced on the horizontal axis).

[0036] The lower half of each figure plots the typical parametric relationship between electromagnetic repulsion (values ​​on the right vertical axis) and melting rate (values ​​on the left vertical axis) (variable frequency values ​​are referenced on the horizontal axis).

[0037] In the graph, the term "pre-solidification" refers to the parameters applied from the point when the mold is filled with molten metal and all the steel in the mold is molten, as schematically shown in Figure 2(a), until half of the molten metal has solidified (90'), as shown in Figure 2(b). In the graph, the term "partially solidified" refers to the parameters applied after the formation of the half-solidified main ingot portion 90', until the formation of the complete main ingot portion and the riser ingot portion. [Examples]

[0038] Example 1 Example 1, for the casting of a 100 metric ton (mt) steel ingot, is graphically shown in Figures 3(a) and 3(b). Here, the magnitude of the power induced from the energized induction coil of the electric induction heating device 14 to the upper surface of the molten riser portion 70b is maintained at a nominal 250 kW from the start of directional solidification of the main portion 70a after the molten steel has filled the mold until the main portion 70a and the riser portion 70b have directional solidified to form the final product ingot.

[0039] Graphs G1.1 (power parameters) and G1.2 (electromagnetic stirring parameters) in Figure 3(a) are applied to the ingot solidification process of Example 1 from the start of directional solidification of the main portion 70a after the molten steel has filled the mold until the lower half 90' of the main portion 70a has solidified, as shown in Figure 2(b).

[0040] Graphs G1.3 (power parameters) and G1.4 (electromagnetic stirring parameters) (semi-solidification process curve) in Figure 3(b) are applied to the ingot solidification process of Example 1 from when half of the main portion 70a has solidified until the entire ingot has solidified.

[0041] In Example 1, in Figure 3(a), the dashed solidification process line A1 was selected to vary the output and stirring parameters from the start of directional solidification of the main portion 70a until half of the main portion had solidified. From the dashed process line A1 in Figure 3(a), the VP / VF power supply PS outputs 7,001 amperes at a frequency of 1 kHz and 976 volts, resulting in electromagnetic stirring characteristics of a typical molten steel velocity of 0.192 meters per second (m / s) and a Lorentz repulsion force of 59.3 kilograms (kg).

[0042] In Example 1, in Figure 3(b) (semi-solidification process curve), the dashed solidification process line A2 was selected for variable power and stirring parameters from the time half of the main portion 70a solidified until the remaining portion of the main portion 70a and the riser portion 70b solidified. From the dashed process line A2 in Figure 3(b), the output of the VP / VF power supply PS was adjusted to 6164.1 amperes at a frequency increased to 1.5 kHz and 1.2792 kilovolts (kV), resulting in electromagnetic stirring characteristics where a typical molten steel velocity is 0.142 meters per second (m / s) and the Lorentz repulsion force is 46 kilograms (kg).

[0043] Example 2 Example 2, concerning the casting of a 100mt steel ingot, is graphically shown in Figures 4(a) and 4(b). Here, the magnitude of the power induced from the energized induction coil of the electric induction heating device 14 to the upper surface of the riser portion 70b is maintained at a nominal 325kW from the start of directional solidification of the main portion 70a after the molten steel has filled the mold until the main portion 70a and the riser portion 70b have directional solidified to form the final product ingot.

[0044] Graphs G2.1 (power parameters) and G2.2 (electromagnetic stirring parameters) in Figure 4(a) are applied to the ingot solidification process of Example 2 from the start of directional solidification of the main portion 70a after the molten steel has filled the mold until the lower half 90' of the main portion 70a has solidified, as shown in Figure 2(b).

[0045] Graphs G2.3 (power parameters) and G2.4 (electromagnetic stirring parameters) (semi-solidification process curve) in Figure 4(b) are applied to the ingot solidification process of Example 2 from when half of the main portion 70a has solidified until the entire ingot has solidified.

[0046] In Example 2, in Figure 4(a), the dashed solidification process line B1 was selected to vary the output and stirring parameters from the start of directional solidification of the main portion 70a until half of the main portion had solidified. From the dashed process line B1 in Figure 4(a), the output of the VP / VF power supply PS was adjusted to 6,460 amperes at a frequency of 2 kHz and 1.779 kV, resulting in electromagnetic stirring characteristics of a typical molten steel velocity of 0.16 meters per second (m / s) and a Lorentz repulsion force of 50.44 kilograms (kg).

[0047] In Example 2, in Figure 4(b) (semi-solidification process curve), the dashed solidification process line B2 was selected until the remainder of the main portion 70a and the riser portion 70b solidified. From the dashed process line B2 in Figure 4(b), the output of the VP / VF power supply PS was adjusted to 6,093 amperes at a frequency of 2.5 kHz and 2.091 kV, resulting in electromagnetic stirring characteristics where the typical molten steel velocity is 0.131 meters per second (m / s) and the Lorentz repulsion force is 44.88 kilograms (kg).

[0048] Example 3 Example 3, concerning the casting of a 150mt steel ingot, is graphically shown in Figures 5(a) and 5(b). Here, the magnitude of the power induced from the energized induction coil of the electric induction heating device 14 to the upper surface of the riser portion 70b is maintained at a nominal 250kW from the start of directional solidification of the main portion 70a after the molten steel has filled the mold until the main portion 70a and the riser portion 70b have directional solidified to form the final product ingot.

[0049] Graphs G3.1 (power parameters) and G3.2 (electromagnetic stirring parameters) in Figure 5(a) are applied to the ingot solidification process of Example 3 from the start of directional solidification of the main portion 70a after the molten steel has filled the mold until the lower half 90' of the main portion 70a has solidified, as shown in Figure 2(b).

[0050] Graphs G3.3 (power parameters) and G3.4 (electromagnetic stirring parameters) (semi-solidification process curve) in Figure 5(b) are applied to the ingot solidification process of Example 3 from when half of the main portion 70a has solidified until the entire ingot has solidified.

[0051] In Example 3, in Figure 5(a), the dashed solidification process line C1 was selected for variable power and stirring parameters from the start of directional solidification of the main portion 70a until the main portion 70a solidified. From the process dashed line C1 in Figure 5(a), the VP / VF power supply PS output 7,834.7 amperes at a frequency of 1 kHz and 1.1296 kV, resulting in electromagnetic stirring characteristics where a typical molten steel velocity is 0.216 meters per second (m / s) and the Lorentz repulsion force is 86.2 kilograms (kg).

[0052] In Example 3, in Figure 5(b) (semi-solidification process curve), the dashed solidification process line C2 was selected for variable power and stirring parameters from after half of the main portion 70a had solidified until the remaining portion of the main portion 70a and the riser portion 70b had solidified. From the dashed process line C2 in Figure 5(b), the output of the VP / VF power supply PS was adjusted to 7,022.1 amperes at a frequency of 1.5 kHz and 1.5135 kV, resulting in electromagnetic stirring characteristics where a typical molten steel rate is 0.16 m / s and the Lorentz repulsion force is 70 kilograms (kg).

[0053] Example 4 Example 4, concerning the casting of a 150mt steel ingot, is graphically shown in Figures 6(a) and 6(b). Here, the magnitude of the power induced from the energized induction coil of the electric induction heating device 14 to the upper surface of the riser portion 70b is maintained at a nominal 325kW from the start of directional solidification of the main portion 70a after the molten steel has filled the mold until the main portion 70a and the riser portion 70b have directional solidified to form the final product ingot.

[0054] Graphs G4.1 (power parameters) and G4.2 (electromagnetic stirring parameters) in Figure 6(a) are applied to the ingot solidification process of Example 4 from the start of directional solidification of the main portion 70a after the molten steel has filled the mold until half of the lower half 90' of the main portion 70a has solidified, as shown in Figure 2(c).

[0055] Graphs G4.3 (power parameters) and G4.4 (electromagnetic stirring parameters) (semi-solidification process curve) in Figure 6(b) are applied to the ingot solidification process of Example 4 from the time half of the main portion 70a has solidified until the entire ingot has solidified.

[0056] In Example 4, in Figure 6(a), the dashed solidification process line D1 was selected for variable power and stirring parameters from the start of directional solidification of the main portion 90a until half of the main portion had solidified. From the process dashed line D1 in Figure 6(a), the VP / VF power supply PS output 7,428.2 amperes at a frequency of 2 kHz and 2.1229 kV, resulting in electromagnetic stirring characteristics where a typical molten steel velocity is 0.185 meters per second (m / s) and the Lorentz repulsion force is 78.3 kilograms (kg).

[0057] In Example 4, in Figure 6(b) (semi-solidification process curve), the dashed solidification process line D2 was selected for variable power and stirring parameters from after half of the main portion 70a had solidified until the remaining portion of the main portion 70a and the riser portion 70b had solidified. From the process dashed line D2 in Figure 6(b), the output of the VP / VF power supply PS was adjusted to 7,010.0 amperes at a frequency of 2.5 kHz and 2.5041 kV, resulting in electromagnetic stirring characteristics where a typical molten steel rate is 0.15 m / s and the Lorentz repulsion force is 70.3 kilograms (kg).

[0058] As shown in the example above, a 150mt ingot has a larger molten metal top surface area than a 100mt ingot and utilizes a larger induction coil in the electric induction heating device. However, the total power requirements for casting the larger 150mt ingot are less than those for casting the 100mt ingot. This is because, beyond the top surface area, power efficiency increases.

[0059] In some embodiments of the present invention, for example, when less agitation is preferred due to concerns about the migration of nonmetallic inclusions to the main portion, a higher frequency is selected by adjusting the voltage and current output from the VP / VF power supply PS. For a given dissolving force, the melt flow rate is inversely proportional to the square root of the frequency. As the frequency increases from 1000 Hz to 3000 Hz, the rate decreases by 1.732 times.

[0060] As shown in the example above, in some embodiments of the present invention, the variable frequency supplied by the VP / VF power supply PS increases in conjunction with an increase in voltage and a decrease in current.

[0061] Induction power and electromagnetic stirring force are concentrated near the surface. They are not affected by the depth of the molten metal. However, the flow velocity and size of each vortex are affected by the depth of the molten metal.

[0062] Most of the induced thermal output and electromagnetic stirring force are generated within twice the reference depth, a value determined by the frequency of the alternating current. The molten metal depth does not affect the solidification line until it reaches twice the reference depth. However, the velocity of the molten metal flow and the size of each vortex are significantly affected by the molten metal depth.

[0063] By applying this invention, the cooling of the lower end of the mold is accelerated and the cooling of the upper end of the mold is slowed, resulting in the production of high-quality steel ingot products with fewer solidification defects. Furthermore, by coordinating the applied variable power and variable frequency, precise temperature control can be achieved without introducing impurities into the ingot, thereby producing high-quality ingot products.

[0064] While preferred embodiments of the present invention have been disclosed for illustrative purposes, the present invention is not limited to the configuration and operation of those embodiments. Furthermore, those skilled in the art will understand that various changes and modifications can be made without departing from the subject matter of the disclosure. Thus, such changes and modifications are within the spirit and scope of this disclosure.

Claims

1. 1. A system for producing large steel ingots by solidifying molten steel in a mold, comprising: a cast ingot for containing the molten steel, the molten steel forming, within the mould, a feeder portion of the molten steel and a main portion of the molten steel located below the feeder portion; an electric induction heating coil disposed within the mold parallel to and adjacent to a top surface region of the molten steel within the mold, the electric induction heating coil being suspended entirely at an offset distance from the top surface region of the molten steel; a power supply configured for continuously supplying a variable power output and a variable frequency output to the electric induction heating coil, the variable power output and the variable frequency output being simultaneously adjustable over a range of powers and frequencies to provide induction heating energy and stirring power to maintain the molten steel in the feeder portion in a molten state until the molten steel in the main portion solidifies, and the induction heating energy supplied by the power supply to the electric induction heating coil is consistently maintained at a nominal induction power; Including, the system.

2. 10. The system of claim 1, wherein the electric induction heating coil comprises a flat spiral wound induction coil, the turns of the flat spiral wound induction coil being coplanar forming a pancake shaped heating coil.

3. The system of claim 2 , wherein the flat spirally wound induction coil is at least partially encased in refractory.

4. 3. The system of claim 2, wherein said flat spirally wound induction coil is completely encased in refractory material.

5. The system of claim 1 , wherein the variable power output is provided by a variable voltage controller.

6. The system of claim 1 , wherein the variable power output is provided by a variable voltage and variable current controller.

7. 10. The system of claim 1, further comprising a lifting device configured to raise or lower the electric induction heating coil above the upper surface region of the molten steel to selectively increase or decrease, respectively, the offset distance.

8. 10. The system of claim 1, further comprising a human machine interface for storing variable power output values ​​and variable frequency output values ​​of said power supply for future large ingot casting processes.

9. The system of claim 1, wherein the variable frequency output increases in conjunction with an increase in voltage and a decrease in current.

10. The system of claim 1, wherein the mold includes an upper mold section and a lower mold section, the upper mold section covering the lower mold section containing the molten steel and forming a completely enclosed mold interior volume.

11. 1. A method for producing a large steel ingot by solidifying molten steel delivered to a mold, the molten steel forming a riser portion of the molten steel above a main portion of the molten steel, the method comprising: positioning an electric induction heating coil within the mold above a top surface region of the molten steel; continuously supplying a variable amount of power and a variable frequency to the electric induction heating coil; selecting a directional solidification process according to each of the size of the large steel ingot, the shape of the large steel ingot, and the chemical composition of the molten steel, wherein the directional solidification process includes a range of parameters of solidification power magnitude and solidification frequency over a process time; and Coordinately and simultaneously adjusting the amount of variable power and the variable frequency supplied to the electric induction heating coil over the process time to match the solidification power magnitude and the solidification frequency parameters of the selected directional solidification process. Including, wherein the solidification power magnitude and solidification frequency parameters are configured to maintain induction power from the electric induction heating coil at a nominal induction power level from the time the molten steel in the main portion is in a molten state until at least the main portion has solidified, and to maintain the molten steel in the feeder portion in a molten state until the main portion below has solidified.

12. 12. The method of claim 11, further comprising adjusting a variable frequency supplied to the electric induction heating coil to move one or more inclusions from the main portion to the feeder portion.

13. 12. The method of claim 11 , wherein the variable frequency is adjusted to limit a defined depth of current penetration into the feeder portion.

14. The method of claim 11 , wherein the variable amount of power is controlled by adjusting the height of the electric induction heating coil above the top surface area of ​​the molten steel.

15. 12. The method of claim 11, wherein adjusting the amount of variable power comprises adjusting a supply voltage and a supply current to the electric induction heating coil on a scale of multiples of 10 kilowatts per square meter of the top surface area of ​​the molten steel.

16. The method of claim 11 , wherein adjusting the variable frequency comprises controlling an electromagnetic stirring force for a stirring pattern and rate of molten metal flow in the molten steel.

17. The method of claim 11 , further comprising adding heat generating and insulating materials to the top surface region prior to placing the electric induction heating coil on the top surface region.

18. 1. A method for producing a large steel ingot by solidifying molten steel delivered to a mold, the molten steel forming an upper riser portion of the molten steel above a lower main portion of the molten steel, the method comprising: Positioning an electric induction heating coil above a top surface region of the molten steel; continuously supplying a variable amount of power and a variable frequency to the electric induction heating coil; First, adjusting the supply voltage and supply current to the electric induction heating coil on a scale of multiples of 10 kilowatts per square meter of the top surface area of ​​the molten steel; and co-ordinately simultaneously adjusting the variable power amount and variable frequency supplied to the electric induction heating coil to maintain induction power from the electric induction heating coil at a nominal induction power level from the time the molten steel in the main portion is in a molten state until at least the main portion has solidified, and to maintain the molten steel in the feeder portion in the molten state until the main portion below has solidified. A method comprising:

19. 20. The method of claim 18, further comprising controlling the amount of variable power by adjusting a height of the electric induction heating coil above the top surface area of ​​the molten steel.

20. The method of claim 18, further comprising constructing and storing a parametric model of the magnitude and variable frequency of the variable power from the start of solidification to the end of solidification, the parametric model being associated with a particular alloy of the mold and the molten steel.